Laminate, manufacturing method thereof, and airless tire
By directly bonding a vulcanized rubber layer with a surface treatment layer to a thermosetting resin layer, the laminate manufacturing process is simplified, and the heat resistance of the resin layer is enhanced, addressing the challenges of complex bonding methods and property deterioration in existing technologies.
Patent Information
- Application Number
- JP2020161745
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-28
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-28
AI Technical Summary
The existing methods for bonding vulcanized rubber and resin materials in laminates, such as those used in airless tires, require the application of adhesive and heat, which can deteriorate the physical properties of the rubber and necessitate complex manufacturing processes and equipment.
A laminate is created by directly joining a vulcanized rubber layer with a surface treatment layer to a thermosetting resin layer, eliminating the need for adhesive and heat application, using a surface treatment layer such as a chlorinated layer to enhance bonding.
This method simplifies the manufacturing process, prevents deterioration of rubber properties, and improves the heat resistance of the resin layer, resulting in a durable laminate suitable for airless tire applications.
Smart Images

Figure 0007559470000004 
Figure 0007559470000005 
Figure 0007559470000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate in which a rubber layer and a resin layer are laminated, a method for producing the same, and an airless tire. [Background technology]
[0002] 2. Description of the Related Art Laminates in which rubber and resin are bonded together have been used in a variety of applications. In recent years, such laminates have been used in the development of airless tires.
[0003] An airless tire includes a hub portion fixed to an axle, a tread ring that contacts the ground, and a number of spokes that connect the hub portion and the tread ring. The tread ring is made of vulcanized rubber. Meanwhile, the spokes are made of a resin material. They are joined together with an adhesive. Therefore, the laminated portion of the spokes and the tread ring corresponds to the above-mentioned laminate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-165154 A Summary of the Invention [Problem to be solved by the invention]
[0005] When vulcanized rubber and a resin material are bonded, the bonding surface of the resin material is first degreased, and then pre-processed by applying a primer, buffing, etc. Next, an adhesive is applied to the bonding surface, and the resin material and the vulcanized rubber are bonded via the adhesive. At this time, the adhesive is usually heated to cause a reaction.
[0006] As described above, in order to prepare the laminate as described above, it is necessary to apply the adhesive, heat it, and further to have environmental facilities for carrying out these steps.
[0007] In addition, when the adhesive is heated, the vulcanized rubber is also indirectly heated, and there is a risk that the physical properties of the vulcanized rubber may deteriorate if it is heated again after vulcanization. Furthermore, from the viewpoint of improving the durability of the laminate, it has been desired to improve the heat resistance of the resin material.
[0008] The present invention has been devised in view of the above-mentioned circumstances, and a main object of the present invention is to provide a laminate that can simplify the manufacturing steps and equipment and that can suppress deterioration of the physical properties of the vulcanized rubber and improve the heat resistance of the resin layer, as well as a manufacturing method thereof and an airless tire. [Means for solving the problem]
[0009] The present invention is a laminate of a rubber layer and a resin layer, wherein the rubber layer is made of vulcanized rubber, the vulcanized rubber includes a surface treatment layer, the surface treatment layer is directly bonded to the resin layer without an intervening adhesive layer, and the resin layer is made of a thermosetting resin.
[0010] In the laminate according to the present invention, the thermosetting resin may be a urethane resin.
[0011] In the laminate according to the present invention, the decomposition temperature of the thermosetting resin may be 180 to 220 (°C).
[0012] In the laminate according to the present invention, the surface treatment layer may be a chlorinated layer.
[0013] In the laminate according to the present invention, the surface treatment layer may have a thickness of 1 to 15 (μm).
[0014] The present invention is a method for manufacturing a laminate as described in any one of claims 1 to 5, characterized in that it includes a step of preparing a vulcanized rubber member for forming the rubber layer, a step of forming the surface treatment layer on at least a portion of the vulcanized rubber member, a step of bringing a liquid resin into contact with the surface treatment layer of the vulcanized rubber member without applying the adhesive to the vulcanized rubber member, and a step of hardening the resin to bond the resin layer and the rubber layer.
[0015] The present invention is an airless tire comprising the laminate according to any one of claims 1 to 6. Effect of the Invention
[0016] By adopting the above-described configurations, the laminate, the manufacturing method thereof, and the airless tire of the present invention, it is possible to simplify the manufacturing process and equipment, and also to suppress deterioration of the physical properties of the vulcanized rubber and improve the heat resistance of the resin layer. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a partial cross-sectional view showing an example of a laminate. [Diagram 2] 5(A) to 5(D) are cross-sectional views illustrating a method for producing a laminate according to the present embodiment. [Diagram 3] FIG. 1 is a partial front view showing an example of an airless tire. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. It should be understood that the drawings include exaggerated expressions and expressions different from the dimensional ratio of the actual structure in order to help understand the contents of the invention. Furthermore, the same or common elements are given the same reference numerals throughout the embodiments, and duplicated explanations are omitted. Furthermore, the specific configurations shown in the embodiments and drawings are for understanding the contents of the present invention, and the present invention is not limited to the specific configurations shown in the drawings.
[0019] [Overall structure of the laminate] Fig. 1 shows a partial cross-sectional view of a laminate 1 of this embodiment. As shown in Fig. 1, the laminate 1 of this embodiment has a rubber layer 2 and a resin layer 3 laminated together. The rubber layer 2 is made of vulcanized rubber 2G. The vulcanized rubber 2G includes a surface treatment layer 4, and this surface treatment layer 4 is directly bonded to the resin layer 3 without an adhesive layer therebetween. In Fig. 1, the symbol B indicates the interface between the rubber layer 2 and the resin layer 3.
[0020] [Surface treatment layer] The surface treatment layer 4 is formed locally on the resin layer 3 side in the rubber layer 2 (vulcanized rubber 2G). The surface treatment layer 4 of this embodiment is formed as, for example, a chlorinated layer. Such a surface treatment layer 4 can be specified as a region in the rubber layer 2 where chlorine is present.
[0021] The surface treatment layer 4 can be easily formed, for example, by applying a chlorine-based primer to the surface of the rubber layer 2 (vulcanized rubber 2G) before it is joined to the resin layer 3. Such a primer is not particularly limited, but an example is a product called "Chemlock 7701" (manufactured by Lord Far East Corporation) that uses trichloroisocyanuric acid. Note that the surface of the rubber layer 2 may be degreased prior to applying the primer.
[0022] It is presumed that the surface treatment layer 4 creates some kind of chemical bonding element in the bonding between the rubber layer 2 and the resin layer 3. The inventors analyzed various laminates 1 using a focused ion beam (FIB-SEM). As a result, they found that the surface treatment layer 4 creates unevenness on the surface (interface B) of the rubber layer 2, and the unevenness creates an anchor effect, improving the bonding between the rubber layer 2 and the resin layer 3.
[0023] Furthermore, the inventors analyzed the laminate 1 (surface treatment layer 4) with an atomic force microscope (AFM) and found that the surface treatment layer 4 was relatively hardened in the rubber layer 2. Such hardening of the surface treatment layer 4 occurs due to a reaction between the rubber layer 2 and the primer, and is considered to be useful for improving the bonding between the rubber layer 2 and the resin layer 3.
[0024] In order to further strengthen the bond between the rubber layer 2 and the resin layer 3, it is desirable that the thickness of the surface treatment layer 4 (the thickness measured from the interface B) be 1 μm or more.
[0025] If the thickness of the surface treatment layer 4 is too small, the unevenness of the surface (interface B) of the rubber layer 2 will be reduced, and the reaction factors required for adhesion will be reduced, so that there is a risk that the bonding strength with the resin layer 3 will not be sufficient. Surprisingly, if the thickness of the surface treatment layer 4 is too large, there is a risk that the bonding strength with the resin layer 3 will not be sufficient. This is presumably because the strength of the rubber layer 2 will be reduced, causing the rubber layer 2 to break, resulting in a reduced bonding strength. From this perspective, it is desirable that the thickness of the surface treatment layer 4 be 15 μm or less. The thickness of the surface treatment layer 4 is positively correlated with, for example, the number of times a primer is repeatedly applied, and can be adjusted by changing the number of applications.
[0026] Although there is no clear interface between the surface treatment layer 4 and other parts in the rubber layer 2, by identifying the positions of the chlorine in the rubber layer 2 that are farthest from the interface B and connecting them together, it is possible to essentially identify the thickness of the surface treatment layer 4.
[0027] Furthermore, the analysis of the laminate 1 above has revealed that in order to strengthen the bond between the rubber layer 2 and the resin layer 3, the surface free energy of the surface treatment layer 4 needs to be within a range of 30 to 50 (mJ / m 2 ) was found to be desirable.
[0028] Surface free energy is 30 (mJ / m 2 ), the surface free energy of the surface treatment layer 4 can be made larger than the surface free energy of the rubber layer 2 (vulcanized rubber 2G). This makes it possible to bring the surface free energy of the surface treatment layer 4 closer to the surface free energy of the resin layer 3. As a result, the laminate 1 of this embodiment makes it possible to firmly bond the rubber layer 2 and the resin layer 3 via the surface treatment layer 4.
[0029] On the other hand, the surface free energy is 50 mJ / m 2 By setting the surface free energy at or below 38 (mJ / m), it is possible to prevent the surface free energy of the surface treatment layer 4 from becoming unnecessarily large, which would cause the surface free energy of the surface treatment layer 4 to deviate from the surface free energy of the resin layer 3. This maintains a strong bond between the rubber layer 2 and the resin layer 3. From this viewpoint, the surface free energy is preferably set to 38 (mJ / m 2 ) or more, and preferably 45 (mJ / m 2 ) or less.
[0030] In this specification, the surface free energy (mJ / m 2 ) is obtained by dropping the following liquid reagents onto the surface treatment layer 4 under the following conditions, measuring the contact angles of each of the liquid reagents, and using the following software according to the Owens-Wendt method. Contact angle meter: "DM-501H1" manufactured by Kyowa Interface Science Co., Ltd. Software: Multi-functional integrated analysis software "FAMAS (interFAce Measurement and Analysis System)" Temperature: 23℃ Humidity: 55%RH Liquid reagent: water, diiodomethane (drop volume: 1.0 microliters) Contact angle: Average value of 10 measured contact angles
[0031] As described above, the laminate 1 of the present embodiment has the advantage that the step of applying an adhesive and the step of reacting the adhesive by applying heat are not required because no adhesive is used to bond the rubber layer 2 and the resin layer 3. This makes it possible to simplify the steps and equipment required to manufacture the laminate 1.
[0032] In addition, since the above steps are not necessary, the rubber layer 2 (vulcanized rubber 2G) is not indirectly heated by heating the adhesive as in the conventional case. Therefore, the laminate 1 of this embodiment can suppress deterioration of the physical properties of the vulcanized rubber 2G. Each part will be described in detail below.
[0033] [Rubber component of rubber layer (vulcanized rubber)] The rubber layer 2 (vulcanized rubber 2G) contains a rubber component. Examples of the rubber component include diene rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber, acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and styrene-isoprene-butadiene copolymer rubber (SIBR). The rubber component may be composed of one type of rubber, or may be a blend of two or more types.
[0034] [Adhesive agent in rubber layer (vulcanized rubber)] In a preferred embodiment, the rubber layer 2 (vulcanized rubber 2G) may contain a tackifier in addition to the rubber component. Such a tackifier is useful for further improving the adhesion between the rubber layer 2 and the resin layer 3. Examples of the tackifier include natural resins and synthetic resins, and preferably, synthetic resins are used. Suitable examples of this synthetic resin include petroleum-based resins and alkylphenol resins.
[0035] Examples of the petroleum-based hydrocarbon resin include aliphatic petroleum resins, aromatic petroleum resins, and aliphatic / aromatic copolymer petroleum resins. The aliphatic petroleum resins are resins obtained by cationic polymerization of unsaturated monomers such as isoprene and cyclopentadiene, which are petroleum fractions having 4 to 5 carbon atoms (C5 fractions) (also referred to as C5 petroleum resins), and may be hydrogenated. The aromatic petroleum resins are resins obtained by cationic polymerization of monomers such as vinyl toluene and alkylstyrene, which are petroleum fractions having 8 to 10 carbon atoms (C9 fractions) (also referred to as C9 petroleum resins), and may be hydrogenated. The aliphatic / aromatic copolymer petroleum resins are resins obtained by copolymerizing the above C5 fraction and C9 fraction (also referred to as C5 / C9 petroleum resins), and may be hydrogenated.
[0036] Examples of alkylphenol-based resins include alkylphenol acetylene-based resins, which are polycondensates of alkylphenols (e.g., pt-butylphenol) and acetylene, and alkylphenol formaldehyde-based resins, which are polycondensates of alkylphenols (e.g., pt-butylphenol, pt-octylphenol, pt-dodecylphenol) and formaldehyde, with alkylphenol formaldehyde-based resins being particularly preferred.
[0037] If the softening point of the tackifier is high, it may not be sufficiently dispersed in the rubber component in the rubber kneading process. From this viewpoint, the softening point of the tackifier is preferably 150 (°C) or less, more preferably 100 (°C) or less. On the other hand, if the softening point of the tackifier is too low, it may be sticky when mixed with rubber and difficult to mix, and the heat resistance of the joint may be reduced. From this viewpoint, the softening point of the tackifier is preferably 60 (°C) or more, more preferably 70 (°C) or more. In this specification, the softening point of the resin is defined as the temperature at which the ball drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring and ball softening point measuring device.
[0038] The amount of the tackifier is, for example, 1 to 15 parts by weight, more preferably 1 to 10 parts by weight, based on 100 parts by weight of the rubber component. If the amount of the tackifier is less than 1 part by weight, the effect of improving the adhesion to the resin due to the addition of the tackifier cannot be expected to be significant. On the other hand, if the amount of the tackifier is more than 15 parts by weight, the scorch resistance of the rubber material may deteriorate, and the moldability may decrease.
[0039] The acid value of the tackifier is desirably, for example, 120 or less. If the acid value of the tackifier is large, it is easily oxidized, resulting in poor viscosity stability, and also tends to have poor adhesion to the resin layer 3. On the other hand, since the acid value of the tackifier is better as it is smaller, there is no need to set a lower limit. In this specification, the acid value of a resin is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of the resin, and is defined as a value measured by potentiometric titration (JIS K 0070:1992).
[0040] [Thermoplastic elastomer in rubber layer (vulcanized rubber)] The rubber layer 2 (vulcanized rubber 2G) may further contain a thermoplastic elastomer in addition to the rubber component. When a thermoplastic elastomer is added to the rubber layer 2 in this manner, high adhesion durability is imparted to the rubber layer 2. The thermoplastic elastomer is preferably at least one selected from the group consisting of polyester-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers.
[0041] The thermoplastic elastomer is added before vulcanization of the rubber layer 2 (vulcanized rubber 2G). Therefore, since the thermoplastic elastomer needs to be compatible with the rubber component during vulcanization, it is preferable that the thermoplastic elastomer has a melting point lower than the vulcanization temperature. On the other hand, if the melting point of the thermoplastic elastomer is too low, there is a risk of it volatilizing during vulcanization. From this viewpoint, it is preferable that the melting point of the thermoplastic elastomer is in the range of 100 to 150 (°C).
[0042] As the thermoplastic elastomer, polyester-based thermoplastic elastomers are particularly preferred. Among them, taking into consideration the affinity with polyester-based resins described below, crystalline resins having ester bonds are suitable in that they impart higher adhesion durability to the rubber layer 2 (vulcanized rubber 2G). It is presumed that such crystalline resins form a discontinuous phase (island regions in a sea-island structure) and exist in a particulate state like fillers. Therefore, it is presumed that the particulate crystalline resin enhances the elasticity and rigidity of the rubber layer 2, and thus improves its strength.
[0043] Examples of the crystalline resin having an ester bond include crystalline polyester thermoplastic resin, crystalline polycarbonate thermoplastic resin, and crystalline polyurethane thermoplastic resin. In particular, crystalline polyester thermoplastic resin or crystalline polycarbonate thermoplastic resin is preferable. Examples of commercially available crystalline resins include the crystalline polyester resin "Vylon" series by Toyobo Co., Ltd. and the "Hytrel" series by Toray Industries, Inc.
[0044] As described above, the rubber layer 2 (vulcanized rubber 2G) to which the thermoplastic elastomer is added has improved strength itself, and when a load is applied to the rubber layer 2, not only does it reinforce the surface treatment layer 4, but it also suppresses the occurrence of misalignment at the interface B with the resin layer 3. Therefore, it is presumed that high adhesion durability is obtained between the rubber layer 2 and the resin layer 3.
[0045] In the rubber layer 2 (vulcanized rubber 2G), the amount of thermoplastic elastomer added is not particularly limited, but if it is too much, the vulcanization time will be faster and the viscosity of the rubber will be lowered, which may deteriorate the processability. From this viewpoint, the amount of thermoplastic elastomer added is preferably, for example, about 10 parts by weight or less per 100 parts by weight of the rubber component.
[0046] In addition to the above-mentioned components, the rubber composition constituting the rubber layer 2 (vulcanized rubber 2G) of this embodiment may contain, as appropriate, compounding agents generally used in the production of rubber materials, such as zinc oxide, stearic acid, various antioxidants, plasticizers such as oil and wax, tackifiers, vulcanizing agents (sulfur, organic peroxides, etc.), vulcanization accelerators, etc.
[0047] [Resin layer] The resin layer 3 of this embodiment is made of a thermosetting resin. The thermosetting resin is molded by polymerization (crosslinking reaction) caused by heating. Compared to, for example, a thermoplastic resin, such a thermosetting resin is less likely to deform even when heat is applied after molding, and has the property of being able to suppress a temperature rise when a load is applied. Therefore, the resin layer 3 made of a thermosetting resin can improve the heat resistance, and therefore the durability of the laminate 1 can be improved. Furthermore, when the resin layer 3 is used in the spoke portion 13 (shown in FIG. 3) of the airless tire 10, it is possible to improve the durability (including heat resistance during high-speed driving) of the spoke portion 13.
[0048] The thermosetting resin is not particularly limited, but is preferably one that can be molded by a casting method. Examples of such resins include 、 Polyimide 、 Examples of the resin include urea resin, phenol resin, polyester, polyurethane, epoxy resin, melamine resin, and silicone resin.
[0049] From the viewpoints of moldability and processability and freedom of material design, the thermosetting resin is preferably a polyurethane resin, a polyamide resin, a polyester resin, etc., and more preferably a polyurethane resin. Such a polyurethane resin can exhibit high elasticity properties compared to other resins.
[0050] The decomposition temperature of the thermosetting resin is preferably 180 to 220°C. Here, the decomposition temperature is the temperature at which the thermosetting resin thermally decomposes. By setting the decomposition temperature to 180°C or higher, the heat resistance of the resin layer 3 can be improved. Furthermore, when the laminate 1 is used in the spoke portion 13 (shown in FIG. 3) of an airless tire 10, it is possible to improve the durability (including heat resistance during high-speed driving) of the spoke portion 13.
[0051] On the other hand, by setting the decomposition temperature of the thermosetting resin to 220 (°C) or less, it is possible to suppress an increase in the degree of crosslinking of the thermosetting resin, and to prevent the resin layer 3 from becoming harder than necessary. Therefore, when the laminate 1 is used in the spoke portion 13 (shown in FIG. 3) of the airless tire 10, it is possible to suppress a decrease in ride comfort.
[0052] In order to effectively exert such an effect, the decomposition temperature of the thermosetting resin is preferably 190° C. or higher and preferably 210° C. or lower. The "decomposition temperature" can be measured based on DSC (Differential Scanning Calorimetry).
[0053] [Manufacturing method] Next, a method for producing the laminate 1 of this embodiment will be described with reference to Figures 2(A) to (D). The production method of this embodiment includes a step of preparing a vulcanized rubber member 2a (vulcanized rubber 2G) for forming the rubber layer 2, and a step of forming a surface treatment layer 4 on at least a part of the vulcanized rubber member 2a. Furthermore, the production method of this embodiment includes a step of bringing a liquid resin 3a into contact with the surface treatment layer 4 of the vulcanized rubber member 2a without applying an adhesive to the vulcanized rubber member 2a, and a step of curing the resin 3a to bond the resin layer 3 and the rubber layer 2. The resin 3a of this embodiment is the above-mentioned thermosetting resin.
[0054] As shown in FIG. 2(A), the vulcanized rubber member 2a is previously vulcanized and molded into a predetermined shape in a separate process.
[0055] 2(B), the surface treatment layer 4 is formed, for example, by chlorinating at least a part of the prepared vulcanized rubber member 2a (specifically, the surface to be bonded to the resin layer 3 (shown in FIG. 1)). More specifically, chlorine is introduced into the surface of the vulcanized rubber member 2a.
[0056] 2(C), the surface-treated vulcanized rubber member 2a is set, for example, in a cavity 5 of a mold M. At this time, an empty space 6 is left in the cavity 5 so that the resin 3a can be supplied. In addition, the surface treatment layer 4 of the vulcanized rubber member 2a is positioned so as to face the empty space 6 of the cavity 5.
[0057] 2(D), liquid resin (thermosetting resin) 3a is supplied (injected) into the empty space 6 of the cavity 5. As a result, the liquid resin 3a comes into contact with the surface treatment layer 4 of the vulcanized rubber member 2a.
[0058] By hardening the resin 3a supplied to the empty space 6 of the cavity 5, it is possible to obtain the laminate 1 in which the rubber layer 2 (vulcanized rubber 2G) and the resin layer 3 are directly bonded without an adhesive layer, as shown in Fig. 1. Note that a heating process is employed to heat the resin 3a (thermosetting resin) for hardening the resin 3a.
[0059] [Airless tires] Next, an airless tire using the laminate 1 of the present embodiment will be described. Fig. 3 is a partial front view of an airless tire as seen from the axle direction, and Fig. 4 is a cross-sectional view taken along line IV-IV of Fig. 3. As shown in Fig. 3 and Fig. 4, an airless tire 10 includes a hub portion 11 fixed to an axle, an annular tread ring 12 for contacting the ground, and spoke portions 13 connecting the hub portion 11 and the tread ring 12.
[0060] The hub portion 11 is made of, for example, a metal material.
[0061] The tread ring 12 is formed of vulcanized rubber 2G. The tread ring 12 may have, for example, a reinforcing cord layer 20 therein in order to increase its circumferential rigidity, etc. The tread ring 12 has a surface treatment layer 4 formed on the inner circumferential surface side in the tire radial direction. The surface treatment layer 4 is formed by chlorination treatment.
[0062] The spoke portion 13 is formed of a resin layer 3 made of a thermosetting resin. The spoke portion 13 in this embodiment integrally includes, for example, an outer portion 14 on the outer side in the tire radial direction, an inner portion 15 on the inner side in the tire radial direction, and a plurality of spoke elements 16.
[0063] The outer portion 14 is an annular body joined to the inner circumferential surface of the tread ring 12 (i.e., the surface treatment layer 4). The thickness of the outer portion 14 is not particularly limited, but is, for example, about 0.5 to 10.0 mm, and more preferably about 1.0 to 5.0 mm. The inner portion 15 is an annular body joined to the outer circumferential surface of the hub portion 11. Each spoke element 16 extends in the tire radial direction between the outer portion 14 and the inner portion 15, and connects them to each other.
[0064] The surface treatment layer 4 of the tread ring 12 and the outer portion 14 are directly bonded to each other without an adhesive layer as shown in Fig. 4. Therefore, in the airless tire 10 of the present embodiment, the tread ring 12 and the outer portion 14 correspond to the rubber layer 2 and the resin layer 3, respectively, and are manufactured using the laminate 1 of the present invention.
[0065] As described above, in the airless tire 10 of this embodiment, the spoke portions 13 are formed using the resin layer 3 made of a thermosetting resin, which makes it possible to improve the durability (including heat resistance during high-speed driving) of the spoke portions 13. Furthermore, since the surface treatment layer 4 and the outer portion 14 of the tread ring 12 are directly bonded together without an adhesive layer therebetween, it is possible to prevent a decrease in bonding strength due to softening of the adhesive or the like during high-speed driving when the temperature of these portions becomes high. Therefore, the airless tire 10 can improve its durability (heat resistance) during high-speed driving.
[0066] The method for manufacturing the airless tire 10 of the present embodiment is as follows. First, an annular tread ring 12 (rubber layer 2) is prepared by vulcanization molding. Next, a surface treatment layer 4 is formed on the inner circumferential surface of the tread ring 12. The surface treatment layer 4 is formed, for example, by chlorination treatment. Next, the tread ring 12 and the hub portion 11 are set in a mold cavity (both not shown). After these members are set, the mold cavity leaves an empty space for molding the spoke portion 13. A liquid resin (thermosetting resin in this example) is supplied to this empty space. By hardening this resin, an airless tire 10 is obtained in which the surface treatment layer 4 of the tread ring 12 and the resin are directly bonded without an adhesive layer. As described above, in the manufacturing method of this embodiment, the tread ring (vulcanized rubber) 12 is not indirectly heated by heating the adhesive, so that deterioration of the physical properties of the tread ring 12 can be suppressed.
[0067] Although a particularly preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the illustrated embodiment and can be modified and carried out in various forms. EXAMPLES
[0068] [Example A] More specific, non-limiting examples of the present invention will now be described. Several types of rubber compositions were prepared based on the rubber compounding in Table 1. These were each subjected to compression at a temperature of 170°C and a pressure of 50 kg / cm 2 The rubber was press-vulcanized for 12 minutes under the conditions of 4 mm x 120 mm x 150 mm to obtain a sheet of vulcanized rubber. This vulcanized rubber was degreased with isopropanol to obtain a sample of the rubber layer.
[0069] Next, to form a surface treatment layer, a surface treatment agent containing a chlorinating agent, "Chemlock 7701" (product name of Lord Far East Corporation), was applied to the sample surface of the rubber layer (vulcanized rubber). After the solvent of the surface treatment agent evaporated, the same operation was repeated three times. The thickness of the surface treatment layer was set to 5 μm.
[0070] A sample of the rubber layer was placed in a mold cavity, and a thermosetting resin or a thermoplastic resin was supplied into the empty space of the cavity to form a resin layer. The thickness of the resin layer was adjusted to 3 mm.
[0071] After the resin layer was cured, the laminate consisting of the resin layer and the rubber layer was removed from the mold, and a rectangular specimen having a width of 25 mm and a length of 100 mm was cut out as a sample of the laminate.
[0072] A peel test (T-peel) was conducted to evaluate the adhesive strength at the interface between the rubber layer and the resin layer in the laminate. The peel test was conducted in accordance with JIS K 6854 at room temperature (23°C and 55% humidity) and at a high temperature (150°C). The results of the tests are shown in Table 1.
[0073] [Table 1]
[0074] As a result of the test, in the laminates of Examples 1 and 2, in the peel test (at room temperature and 150°C), material failure occurred in the rubber layer, but no peeling occurred at the interface between the rubber layer and the resin layer. On the other hand, in Comparative Examples 1 and 4, interfacial peeling occurred between the resin layer and the rubber layer in a high temperature environment. In Comparative Example 2, interfacial peeling occurred between the resin layer and the rubber layer, and in Comparative Example 3, interfacial peeling occurred in the adhesive layer between the resin layer and the rubber layer.
[0075] In this way, it was confirmed that the laminate of the example had high adhesive strength over a long period of time even without an adhesive between the rubber layer and the resin layer, and that the process and equipment for manufacturing the laminate could be simplified. In addition, in the example, the rubber layer was not heated again, so deterioration of physical properties could be suppressed. Furthermore, it was confirmed that the laminate of the example could have improved heat resistance because the resin layer was made of a thermosetting resin.
[0076] Next, airless tires were prototyped using the rubber layer and resin layer with the composition shown in Table 1, and the high-speed durability of the tires was evaluated. In the evaluation of high-speed durability, a drum testing machine was used to apply a load of 2.6 kN to the airless tire, and the tire was started to roll at an initial speed of 100 km / h, and then the speed was increased by 10 km / h every 10 minutes. The maximum speed at which the airless tire was not damaged was expressed as an index, with Comparative Example 1 being set at 100. The higher the value, the better the high-speed durability.
[0077] As a result of the test, it was confirmed that the airless tires of the Examples exhibited superior high-speed durability compared to the airless tires of the Comparative Examples. Therefore, it was confirmed that the Examples can suppress the deterioration of the physical properties of the vulcanized rubber and improve the heat resistance of the resin layer.
[0078] [Example B] Based on the rubber compounding etc. of Example 1 in Table 1, a number of airless tires with different decomposition temperatures of the thermosetting resin (urethane type) were prototyped, and high-speed durability tests were carried out on them, and the ride comfort performance was evaluated (Examples 3 to 8). The evaluation procedure for high-speed durability was as described in Example A, and is shown with an index of Example 4 being 100.
[0079] Meanwhile, the ride comfort performance was evaluated by mounting the airless tires to be evaluated on all four wheels of a vehicle (small EV: product name COMS), driving the vehicle with one passenger on a tire test course with a dry asphalt road surface, and evaluating the ride comfort performance through the driver's sensory evaluation. The results are shown as an index, with the higher the value, the better the performance. The test results are shown in Table 2.
[0080] [Table 2]
[0081] As a result of the tests, it was found that the examples in which the decomposition temperature of the thermosetting resin (urethane type) was within the preferred range were able to improve ride comfort while exhibiting superior high-speed durability compared to the other examples.
[0082] [Example C] Based on the rubber compounding etc. of Example 1 in Table 1, a number of laminates were formed (Examples 9 to 14) differing only in the thickness of the surface treatment layer. Then, a peel test (T-peel) was conducted to evaluate the adhesive strength at the interface between the rubber layer and the resin layer in the laminate. Details of the test method etc. are as described in Example A. The test results are shown in Table 3.
[0083] [Table 3]
[0084] As a result of the test, the laminates of Examples 9 and 14, in which the thickness of the surface treatment layer was outside the preferred range, were able to increase the bonding strength compared to Comparative Examples 1 to 4 shown in Table 1 of Example A, but interfacial peeling occurred between the resin layer and the rubber layer. On the other hand, in Examples 10 to 13, in which the thickness of the surface treatment layer was within the preferred range, it was confirmed that no peeling occurred at the interface between the rubber layer and the resin layer and high adhesive strength was obtained. [Explanation of symbols]
[0085] 1. Laminate 2 Rubber layers 2G Vulcanized rubber 3 Resin layer 4 Surface treatment layer
Claims
1. An airless tire including a laminate of a rubber layer and a resin layer, The rubber layer is made of vulcanized rubber, The vulcanized rubber includes a surface treatment layer, the surface treatment layer is directly bonded to the resin layer without an adhesive layer; The resin layer is made of a thermosetting resin, The surface treatment layer is a chlorinated layer. Airless tires.
2. The airless tire according to claim 1 , wherein the thermosetting resin is a urethane resin.
3. An airless tire as described in claim 1 or 2, wherein the thickness of the surface treatment layer is 1 to 15 (μm).
4. A method for producing an airless tire according to any one of claims 1 to 3, preparing a vulcanized rubber member for forming the rubber layer; forming the surface treatment layer on at least a portion of the vulcanized rubber member; a step of bringing a liquid resin into contact with the surface treatment layer of the vulcanized rubber member without applying the adhesive to the vulcanized rubber member; and curing the resin to bond the resin layer and the rubber layer. A method for manufacturing airless tires.
Citation Information
Patent Citations
One-surface metal lined laminated board
JP1985032651A
Plant controller
JP1987058301A
Boot made of rubber
JP1993043724A
Method for multicolor molding thermoplastic resin on rubber
JP1996294933A
Composite and manufacturing method therefor
JP2003320618A