Synthetic fiber cord for rubber reinforcement
The synthetic fiber cord with a specific adhesive resin composition and RFL coating addresses adhesive deterioration and durability issues in rubber products, ensuring robust performance under heat and stress.
Patent Information
- Application Number
- JP2021029604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing rubber products face issues with adhesive deterioration and insufficient durability due to heat and repeated stretching/compression, especially in applications like tires, belts, and hoses, as current treatments do not provide adequate heat-resistant adhesive strength and fatigue resistance.
A rubber-reinforcing synthetic fiber cord coated with an adhesive resin containing guaiacol (m/z 124) and vanillin (m/z 152) detected by pyrolysis GC-MS, exhibiting a peak at 1510-1550 cm^-1 in IR analysis, with Gurley cord hardness of 70 mN/% or less and a 90%-230% hardness change rate, using resorcinol-formalin-rubber latex (RFL) for improved adhesion.
The synthetic fiber cord maintains high initial adhesion and heat-resistant adhesive strength, offering enhanced durability and fatigue resistance in high-temperature conditions, extending the lifespan of rubber products.
Smart Images

Figure 0007559610000003 
Figure 0007559610000001 
Figure 0007559610000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a synthetic fiber cord for reinforcing rubber, and a rubber product including the synthetic fiber cord for reinforcing rubber. [Background technology]
[0002] Synthetic fibers such as nylon fibers, polyester fibers, and aromatic polyamide fibers have been widely used as reinforcing materials in rubber products such as tires, hoses, and belts. However, the heat generated during processing to embed the synthetic fibers in rubber products as reinforcing materials and the heat generated by the rubber when used in rubber products cause a decrease in adhesion between the rubber and the synthetic fibers, which leads to failure of the rubber products. In recent years, there has been an increasing need to improve the durability of rubber products in order to reduce the frequency of replacement of rubber products due to breakdowns from the perspective of environmental protection.
[0003] Techniques disclosed to address the above problem include the prior art techniques disclosed in Patent Documents 1 to 4, for example.
[0004] Patent Document 1 discloses a polyester fiber cord for reinforcing rubber, which is coated with a first treating agent containing three types of compounds: a compound containing an oxazoline group, an epoxy compound, and rubber latex, and is further coated with a second treating agent containing resorcinol-formaldehyde-rubber latex (RFL).
[0005] Patent Document 2 discloses a method for producing a polyester fiber cord for rubber reinforcement, which is coated with a first treating agent containing three types of compounds, namely, an aliphatic epoxide compound, a blocked polyisocyanate compound, and a vinylpyridine-styrene-butadiene rubber latex having a glass transition point of -30 to 0°C, and is further coated with a second treating agent containing resorcin-formaldehyde-rubber latex (RFL) as an outer layer, and which is treated with a first bath hot stretch tension of 0.05 to 0.40 cN / dtex.
[0006] Patent Document 3 discloses a cord that includes an aramid ply / twist yarn and an adhesive applied to the outer surface of the aramid ply / twist yarn, and the penetration rate of the adhesive into the aramid ply / twist yarn is set to 3.5% to 9%.
[0007] Patent Document 4 discloses an organic fiber cord having a first twist and a second twist, the first twist having a twist multiplier of 1000 to 2500 and the second twist having a twist multiplier of 1500 to 3600, the ply-twisted cord being covered with an adhesive containing resorcinol-formaldehyde-rubber latex (RFL), the cord compression ratio being 83 to 97%, and the degree of RFL impregnation into the cord being 10 to 50%. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2009-203594 A [Patent Document 2] Special Publication No. 2014-530302 [Patent Document 3] JP 2013-76186 A [Patent Document 4] JP 2017-150105 A Summary of the Invention [Problem to be solved by the invention]
[0009] However, although the initial adhesive strength is improved according to Patent Document 1, the heat-resistant adhesive strength and durability are not sufficient. According to Patent Document 2, fatigue resistance is improved, but the adhesive strength is not sufficient. According to Patent Documents 3 and 4, the adhesive strength and fatigue resistance are improved compared to the conventional ones, but the durability in the face of increasingly higher demand levels is not sufficient.
[0010] The present invention has been made as a result of studies aimed at solving the problems in the above-mentioned conventional techniques.
[0011] An object of the present invention is to provide a synthetic fiber cord for reinforcing rubber which is less susceptible to adhesion deterioration even when exposed to high temperatures for a long period of time when embedded in rubber such as in tires, belts, hoses, etc., and which inhibits deterioration when subjected to repeated extension and compression in the rubber. [Means for solving the problem]
[0012] In order to solve the above problems, the present invention adopts the following means. (1) A synthetic fiber cord for reinforcing rubber, comprising a synthetic fiber and an adhesive resin adhered to the synthetic fiber, wherein guaiacol having a mass-to-charge ratio (m / z) of 124 is detected in the adhesive resin by pyrolysis GC-MS analysis. (2) The synthetic fiber cord for rubber reinforcement according to (1) above, wherein vanillin having a mass-to-charge ratio (m / z) of 152 is further detected in the adhesive resin by pyrolysis GC-MS analysis. (3) Infrared absorption spectrum analysis (IR) of adhesive resin: Wavenumber 1510-1550 cm -1 The synthetic fiber cord for rubber reinforcement according to the above (1) or (2), characterized in that it exhibits a peak derived from deformation vibration of an NH group in the range. (4) A synthetic fiber cord for rubber reinforcement according to any one of the above (1) to (3), characterized in that the Gurley cord hardness per unit of resin attached to the cord is 70 mN / % or less, and the rate of change in Gurley cord hardness after heating is 90% to 230%. (5) A synthetic fiber cord for reinforcing rubber according to any one of (1) to (4), characterized in that an adhesive treatment agent containing resorcinol-formalin-rubber latex (RFL) is adhered to the synthetic fiber cord. (6) The synthetic fiber cord for reinforcing rubber according to any one of (1) to (5), wherein the synthetic fiber includes at least one selected from the group consisting of nylon fiber, polyester fiber, and aromatic polyamide fiber. (7) A rubber product comprising the synthetic fiber cord for rubber reinforcement according to any one of (1) to (6) above. Effect of the Invention
[0013] In order to solve the above problems, the present invention adopts the following means. (1) A synthetic fiber cord for reinforcing rubber, comprising a synthetic fiber and an adhesive resin adhered to the synthetic fiber, wherein guaiacol having a mass-to-charge ratio (m / z) of 124 is detected in the adhesive resin by pyrolysis GC-MS analysis. (2) The synthetic fiber cord for rubber reinforcement according to (1) above, wherein vanillin having a mass-to-charge ratio (m / z) of 152 is further detected in the adhesive resin by pyrolysis GC-MS analysis. (3) The synthetic fiber cord for rubber reinforcement according to (1) or (2) above, characterized in that, in infrared absorption spectroscopy (IR) of the adhesive resin, it shows a peak attributable to deformation vibration of an NH group in the wavenumber range of 1510 to 1550 cm-1. (4) A synthetic fiber cord for rubber reinforcement according to any one of the above (1) to (3), characterized in that the Gurley cord hardness per unit of resin attached to the cord is 70 mN / % or less, and the rate of change in Gurley cord hardness after heating is 90% to 230%. (5) Contains resorcinol, formalin and rubber latex (RFL) Adhesive resin The synthetic fiber cord for reinforcing rubber according to any one of (1) to (4), characterized in that (6) The synthetic fiber cord for reinforcing rubber according to any one of (1) to (5), wherein the synthetic fiber includes at least one selected from the group consisting of nylon fiber, polyester fiber, and aromatic polyamide fiber. (7) A rubber product comprising the synthetic fiber cord for rubber reinforcement according to any one of (1) to (6) above. [Brief description of the drawings]
[0014] [Figure 1] This is an oblique view of "Gurley's stiffness tester." DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below.
[0016] The synthetic fiber cord for rubber reinforcement of the present invention is a cord made of synthetic fiber, particularly organic fiber. The synthetic fiber cord for rubber reinforcement of the present invention can be used in various rubber members, such as tires, belts, hoses, etc., for automobiles and the like, to reduce the weight and improve the durability of the rubber members.
[0017] The organic fiber used in the synthetic fiber cord for rubber reinforcement is preferably in the form of a multifilament. The organic fiber is not particularly limited, but preferably contains at least one selected from polyester fibers such as polyethylene terephthalate and polyethylene naphthalate, polyamide fibers such as nylon 6, nylon 66 and nylon 46, polyvinyl alcohol fibers, rayon fibers and aromatic polyamide (aramid) fibers in terms of versatility, durability and industrial productivity. Among them, it is preferable to contain at least one selected from polyethylene terephthalate, nylon 66 and aramid in terms of versatility, durability and industrial productivity.
[0018] The organic fiber used in the present invention may be one to which a polyepoxide compound has been added in advance in the spinning process. The polyepoxide compound that can be used in the present invention is a compound containing at least two epoxy groups in one molecule, in an amount of 0.1 g equivalent or more per 100 g of the compound. Specifically, examples of the polyepoxide include reaction products of polyhydric alcohols such as pentaerythritol, ethylene glycol, polyethylene glycol, propylene glycol, glycerol, and sorbitol with halogen-containing epoxides such as epichlorohydrin, polyepoxide compounds obtained by oxidizing unsaturated compounds with peroxide or hydrogen peroxide, and aromatic polyepoxides such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexenecarboxylate, bis(3,4-epoxy-6-methyl-cyclohexylmethyl)adipate, phenol novolac type, hydroquinone type, biphenyl type, bisphenol S type, brominated novolac type, xylene modified novolac type, phenol glyoxal type, trisoxyphenylmethane type, trisphenol PA type, and bisphenol type polyepoxides. Particularly preferred are sorbitol glycidyl ether type and cresol novolac type polyepoxides.
[0019] These compounds are usually used as an emulsion or solution, that is, the compounds are dissolved in a solvent and used as a solution, or emulsified using a common emulsifier such as sodium alkylbenzenesulfonate, sodium dioctyl sulfosuccinate, or nonylphenol ethylene oxide adduct and used as an emulsion.
[0020] The polyepoxide compound is applied together with a spinning oil in the spinning process of the organic fiber. The amount of the polyepoxide compound attached is preferably in the range of 0.1 to 5% by weight. If the amount of the polyepoxide compound attached is within the above range, the effect of the polyepoxide compound is fully exerted, and a satisfactory adhesion is obtained between the organic fiber and the rubber. In addition, if the amount is within the above range, the fiber does not become too hard, and the strength is not easily reduced when twisting in the next process or later.
[0021] The organic fiber used in the present invention is not restricted by fineness, number of filaments, cross-sectional shape, etc., but usually, a total fineness of 200 to 5000 dtex and 30 to 1000 filaments is preferable, and 250 to 3000 dtex and 50 to 500 filaments are particularly preferable. If the total fineness is less than 200 dtex, the strength of the cord may be insufficient, and if it exceeds 5000 dtex, the cord may become thick and the handling may be deteriorated. In addition, if it is less than 30 filaments, the cord may become hard and the handling may be deteriorated, and if it exceeds 500 filaments, the fluff may increase and the quality may be deteriorated.
[0022] From the viewpoint of improving fatigue resistance, the synthetic fiber cord for rubber reinforcement of the present invention can be obtained by twisting the organic fibers to form a twisted cord, and then dipping and heat-treating the twisted cord as it is or after it has been woven into a blind. For example, a twisted cord for use in a tire cord for a carcass can be obtained by first twisting in the S or Z direction, combining two or three first-twisted cords, and then twisting the same number of cords together in the opposite direction to the first twist to form a multi-twisted twisted cord. The twisted cord is used as the warp, and cotton yarn is used as the weft, or organic fiber is covered with cotton yarn to form the weft, which is woven into a blind to form a green curtain cloth, which is then dipped and heat-treated in an adhesive to obtain a dipped curtain cloth.
[0023] On the other hand, in the case of a hose cord, for example, one strand or two strands that have been fully aligned are first twisted to form a single-twist twisted cord, and in the case of a belt cord, two or three single-twist cords are combined and usually the same number of second twists are applied in the opposite direction to the first twist to form a multi-twist twisted cord, and each of these is dipped in an adhesive treatment agent and heat treated while still in the twisted cord form to obtain a dipped cord.
[0024] The synthetic fiber cord for reinforcing rubber in the present invention refers to both the above-mentioned dipped fabric and dipped cord.
[0025] The adhesive treatment agent is not particularly limited, but examples thereof include a primer treatment agent containing an epoxy compound, an adhesive treatment agent containing resorcinol-formaldehyde-rubber latex (RFL), an adhesive treatment agent containing a compound having a phenolic hydroxyl group, and the like. In the present invention, these can be used alone or in combination.
[0026] The epoxy compound that can be used in the primer treatment agent can be a compound that contains at least two or more epoxy groups in one molecule, and the compound has an equivalent of 0.1 g or more per 100 g.Specific examples include the reaction product of polyhydric alcohols such as pentaerythritol, ethylene glycol, polyethylene glycol, propylene glycol, glycerol, and sorbitol with halogen-containing epoxides such as epichlorohydrin, and polyepoxide compounds obtained by oxidizing unsaturated compounds with peroxide or hydrogen peroxide, such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexenecarboxylate, bis(3,4-epoxy-6-methyl-cyclohexylmethyl)adipate, phenol novolac type, hydroquinone type, biphenyl type, bisphenol S type, brominated novolac type, xylene modified novolac type, phenol glyoxal type, trisoxyphenylmethane type, trisphenol PA type, and aromatic polyepoxides such as bisphenol type polyepoxides. Particularly preferred are sorbitol glycidyl ether type and cresol novolac type polyepoxides.
[0027] These compounds are usually used as an emulsion or solution, that is, the compounds are dissolved in a solvent and used as a solution, or emulsified using a common emulsifier such as sodium alkylbenzenesulfonate, sodium dioctyl sulfosuccinate, or nonylphenol ethylene oxide adduct and used as an emulsion.
[0028] In adhesive treatment agents containing resorcinol-formaldehyde-rubber latex (RFL), RFL is a mixture of resorcinol-formaldehyde precondensate and rubber latex. It is preferable to prepare the resorcinol-formaldehyde precondensate obtained by precondensation under an alkaline catalyst. For example, resorcinol and formaldehyde are added and mixed in an alkaline aqueous solution containing an alkaline compound such as sodium hydroxide, and the mixture is left at room temperature for several hours to allow the resorcinol and formaldehyde to precondense, after which rubber latex is added to form a mixed emulsion.
[0029] The resorcinol-formaldehyde initial condensation product preferably has a molar ratio of resorcinol to formaldehyde in the range of 1:0.3 to 1:5, preferably 1:0.75 to 1:2.0. If the molar ratio of formaldehyde is less than the above range, the dipped cord may become sticky, leading to soiling of the dipping machine, whereas if the molar ratio of formaldehyde is more than this range, the adhesive strength may decrease.
[0030] Examples of rubber latexes used in the preparation of resorcinol-formaldehyde-rubber latex include natural rubber latex, butadiene rubber latex, styrene-butadiene rubber latex, vinylpyridine-styrene-butadiene rubber latex, nitrile rubber latex, hydrogenated nitrile rubber latex, chloroprene rubber latex, chlorosulfonated rubber latex, and ethylene-propylene-diene rubber latex. These can be used alone or in combination.
[0031] In the case of resorcinol-formaldehyde-rubber latex, the compounding ratio of resorcinol-formaldehyde initial condensate to rubber latex is preferably 2 / 1 to 1 / 12 by solid weight. Outside this range, the adhesive strength may decrease.
[0032] Examples of adhesive treatment agents containing a compound having a phenolic hydroxyl group include catechol, hydroquinone, hydroxyquinol, benzenetetraol, tyrosol, hydroxytyrosol, catechin, glucosylrutin, phenylpropanoids, vanillins, etc., and these compounds are at least mixed with latex alone or in combination with a plurality of these compounds.
[0033] In the synthetic fiber cord for reinforcing rubber of the present invention, when the adhesive resin recovered from dissolving the fibers of the cord is analyzed by pyrolysis GC-MS, it is necessary that guaiacol having a mass-to-charge ratio (m / z) of 124 is detected. The adhesive resin is preferably one from which vanillin having a mass-to-charge ratio (m / z) of 152 is further detected. The synthetic fiber cord for reinforcing rubber having the above-mentioned characteristics not only has high initial adhesive strength, but also has good heat resistance as the molecular chains are less likely to be broken by heat, and improves fatigue resistance in rubber products and the like that are repeatedly stretched and compressed.
[0034] The means for satisfying this requirement is not particularly limited, but for example, the synthetic fiber cord for rubber reinforcement may be treated with an adhesive treatment agent containing a compound having a phenolic hydroxyl group, and the compound having a phenolic hydroxyl group may be any compound that generates guaiacol upon thermal decomposition, and preferably also generates vanillin. Examples of the compound having a phenolic hydroxyl group are as described above, but vanillins are preferred as compounds that generate guaiacol upon thermal decomposition, and examples of vanillins include vanillin, vanillic acid, isovanillin, isovanillic acid, ortho-vanillin, vanillyl alcohol, vanillylmandelic acid, etc.
[0035] The rubber reinforcing fiber cord of the present invention preferably has a Gurley cord hardness of 70 mN / % or less per unit of resin attached to the cord, and a rate of change in the Gurley cord hardness after heating of 90% to 230%. More preferably, in a two-ply cord having a first twist and a second twist, the Gurley cord hardness is 30 mN / % to 70 mN / % and a rate of change in the Gurley cord hardness after heating of 90% to 130%. In a single-ply cord having only a first twist, the Gurley cord hardness is preferably 10 mN / % or less and a rate of change in the Gurley cord hardness after heating of 120% to 230%. By setting the range, the rubber-cord composite can improve the rubber-following property of the cord, and good adhesive strength can be obtained. There is no particular limitation on the method for setting the range, but it can be achieved, for example, by setting the heat treatment temperature after application of the adhesive to 200 to 250°C and setting the tension during mechanical softening treatment to 0.5 cN to 5.0 cN / dtex.
[0036] In addition, the synthetic fiber cord for rubber reinforcement of the present invention has an infrared absorption spectrum (IR) of an adhesive resin with a wave number of 1510 to 1550 cm ―1 It is preferable that the peak derived from the deformation vibration of the NH group is in the range. By setting it in this range, a cord having good heat-resistant adhesion and fatigue resistance in a high-temperature atmosphere can be obtained. The absorption in this range is the absorption of polyurethane urea, which is the absorption of the deformation vibration of the NH group of the urethane bond and the urea bond and the absorption of the aromatic ring overlap. There is no particular limitation on the means for obtaining this absorption, but it can be achieved, for example, by blending a compound having a phenolic hydroxyl group in the adhesive component constituting the synthetic fiber cord for rubber reinforcement, and blending a blocked isocyanate compound as another component in the same adhesive in a solid content ratio range of the compound having a phenolic hydroxyl group / blocked isocyanate compound = 20 / 80 to 80 / 20. It is preferable that rubber latex is contained here, and an example of the rubber latex used here is the rubber latex used in the RFL described above. The ratio of the rubber latex is preferably the compound having a phenolic hydroxyl group + blocked isocyanate compound / rubber latex = 5 / 95 to 70 / 30 (solid content ratio).
[0037] A blocked isocyanate compound is one in which a blocking agent is liberated by heating to generate an active isocyanate compound. Specific examples of the blocked isocyanate compound include reaction products of polyisocyanate compounds such as tolylene diisocyanate, metaphenylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and triphenylmethane triisocyanate with blocking agents such as phenols such as phenol, cresol, and resorcin, lactams such as ε-caprolactam and valerolactam, and oximes such as acetoxime, methyl ethyl ketoxime, and cyclohexane oxime.
[0038] Among these blocked polyisocyanate compounds, aromatic polyisocyanate compounds blocked with ε-caprolactam and aromatic compounds blocked with diphenylmethane diisocyanate give particularly good results.
[0039] The synthetic fiber cord for rubber reinforcement of the present invention preferably has a pull-out adhesive strength of 100 N / cm to 250 N / cm as measured by the method described below, and more preferably has a pull-out adhesive strength of 175 N / cm to 250 N / cm for polyester and 140 N / cm to 200 N / cm for para-aramid. By setting the strength within these ranges, the rubber product made into a rubber product can be practically used.
[0040] The synthetic fiber cord for rubber reinforcement of the present invention characterized as above significantly improves the decrease in adhesion during the rubber vulcanization process and during use of the rubber product. The rubber products reinforced with the synthetic fiber cord for rubber reinforcement of the present invention can withstand longer-term and harsher use than ever before when used as tires, belts and hoses, and are therefore extremely useful for rubber reinforcement.
[0041] Next, a method for producing the synthetic fiber cord for reinforcing rubber of the present invention will be described.
[0042] An example of a method for producing the synthetic fiber cord for rubber reinforcement of the present invention is a method in which a twisted organic fiber cord is dipped in an adhesive treatment agent, and then the water is dried preferably at a temperature of 100 to 150°C, and then a heat treatment is performed at 200 to 255°C.
[0043] Here, dipping refers to applying an adhesive treatment agent to a twisted cord by running the twisted cord through a dipping tank equipped with rollers and filled with the adhesive treatment agent. Heat treatment refers to heating the twisted cord by running the twisted cord through an oven equipped with rollers and capable of being set at a predetermined temperature. Dip treatment machines for carrying out such dipping and heat treatment are commercially available, for example, from Ritzler. Note that any other method can be used to attach the adhesive treatment agent to the organic fibers, such as application by spraying the adhesive treatment agent from a nozzle.
[0044] In order to control the amount of solids of the adhesive treatment agent attached to the organic fibers, means such as squeezing with a pressure roller, scraping with a scraper, blowing off with air or suction may be used.
[0045] Furthermore, after the above drying and heat treatment, the synthetic fiber cord can be softened by rubbing it against an edge to obtain a desired cord stiffness.
[0046] The adhesive treatment agent is not particularly limited, but as mentioned above, examples include a primer treatment agent containing an epoxy compound, an adhesive treatment agent containing resorcinol-formaldehyde-rubber latex (RFL), an adhesive treatment agent containing a compound having a phenolic hydroxyl group, etc., and in the present invention, these can be used alone or in combination. For example, a two-bath treatment method in which a dip treatment is performed with a primer treatment agent and then a treatment with an RFL, or a two-bath treatment method in which a dip treatment is performed with a primer treatment agent and then a treatment with an adhesive treatment agent containing a compound having a phenolic hydroxyl group, etc., can be appropriately selected.
[0047] Here, the primer treatment agent containing an epoxy compound preferably has a solids concentration of 1 to 10% by weight, and the resin adhesion amount of the primer treatment agent is preferably in the range of 0.2 to 6 parts by weight per 100 parts by weight of synthetic fiber from the viewpoints of adhesion and fatigue resistance.
[0048] The adhesive treatment agent containing RFL preferably has a solids concentration of 3 to 20% by weight, and the resin adhesion amount of the adhesive treatment agent containing RFL is preferably in the range of 0.5 to 10 parts by weight per 100 parts by weight of synthetic fiber from the viewpoints of adhesion and fatigue resistance. If it exceeds 10 parts by weight, it may cause dirt on the dip treatment machine. The adhesive treatment agent containing a compound having a phenolic hydroxyl group preferably has a solids concentration of 2 to 20% by weight, and the resin adhesion amount of the primer treatment agent is preferably in the range of 0.2 to 20 parts by weight per 100 parts by weight of synthetic fiber from the viewpoints of adhesion and fatigue resistance.
[0049] The synthetic fiber cord for rubber reinforcement of the present invention thus obtained has significantly improved heat-resistant adhesion when exposed to high temperatures for a long time during the rubber vulcanization process or during use as a rubber product. Rubber products reinforced with the synthetic fiber cord for rubber reinforcement of the present invention can withstand longer-term, harsher use than conventional products when used as tires, belts, and hoses, and are therefore extremely useful for rubber reinforcement. EXAMPLES
[0050] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples specifically described below, each measurement value was determined by the following method.
[0051] (1) Adhesive resin Amount of adhesion The weight of the twisted yarn cord per certain length is measured in advance, and the weight of the synthetic fiber cord of the same length after the adhesive is applied is measured. Adhesive resin The amount of adhesion was calculated.
[0052] (2) Pyrolysis GC-MS analysis Synthetic fiber cord for rubber reinforcement was immersed in HFIP (hexafluoroisopropanol) to dissolve the polyester fiber. The remaining solid was dried to obtain a measurement sample for the adhesive resin.
[0053] Approximately 0.3 mg of the measurement sample was placed in the pyrolyzer of a pyrolysis gas chromatograph mass spectrometer (pyrolyzer: PY-2020iD manufactured by Frontier Labs, gas chromatograph: 6890 manufactured by Agilent Technologies, mass spectrometer: JMS-Q1000GC manufactured by JEOL) and pyrolyzed at 600°C. The generated gas (decomposition product) was introduced into the gas chromatograph mass spectrometer, and after holding at 40°C for 3 minutes, the temperature was increased to 320°C at a rate of 20°C / min, and the decomposition product was separated and mass spectrum was measured under the conditions of holding at 320°C for 18 minutes. The metal capillary column for gas chromatography was a dimedyl polysiloxane column (Ultra ALLOY-5 manufactured by Frontier Labs), and the carrier gas was helium. Ionization in mass spectrometry was performed by electron ionization method. From the obtained pyrograms, the presence or absence of detection of a guaiacol peak in the mass chromatogram extracted at m / z=124, and the presence or absence of detection of vanillin in the mass chromatogram extracted at m / z=152 were evaluated.
[0054] (3) Initial adhesive strength and heat-resistant adhesive strength This indicates the adhesive strength between synthetic fiber cord and rubber. In accordance with the 3.1T test (A method) of JIS L-1017 (2002) Appendix 1, the synthetic fiber cord was embedded in unvulcanized rubber and press-vulcanized under pressure (initial adhesive strength: 30 minutes at 150°C, heat-resistant adhesive strength: 70 minutes at 170°C), and after cooling, the synthetic fiber cord was pulled out of the rubber block at a speed of 300 mm / min, and the load required to pull out was displayed in N / cm. The adhesive strength was calculated as the average value of 10 measurements.
[0055] (4) Fatigue resistance in rubber (retention rate) The evaluation was performed in accordance with JIS-L1017 (2002) Appendix 1, 2.2.2 Disk fatigue strength (Goodrich method). Two synthetic fiber cords were embedded in unvulcanized rubber and vulcanized at 150°C for 30 minutes to create a rubber composite. The test piece was subjected to a deformation of 6.3% compression and 12.6% elongation per cycle at 2600 cycles / min in a 100°C atmosphere for 12 hours, after which the synthetic fiber cords were removed from the rubber and the tensile strength after fatigue was measured, and the tensile strength was expressed as the retention rate before and after the fatigue test. The retention rate was the average value of 8 measurements. The tensile strength was measured based on JIS-L1017 (2002) 8.5 Tensile strength and elongation a) Standard time test.
[0056] The composition of the unvulcanized rubber compound used in measuring T-initial adhesive strength, T-heat resistant adhesive strength, and fatigue resistance in rubber is as follows. Natural rubber (RSS#1): 70 (parts by weight) SBR (JSR1501): 30 (weight parts) RF carbon black: 40 (parts by weight) Stearic acid: 2 (parts by weight) Sulfur: 2 (parts by weight) Zinc oxide: 5 (parts by weight) 2,2'-Dithiobenzothiazole: 3 (parts by weight) Naphthenic acid process oil: 3 (parts by weight).
[0057] (5) Gurley cord hardness per unit of resin attached to the cord A synthetic fiber cord was cut to a length of 1 m, a metal hook was tied to one end and a 300 g weight was tied to the other end, and the cord was hung vertically in the air for 24 hours in an environment regulated at a temperature of 25°C and a relative humidity of 40%, to obtain a measurement sample.
[0058] This was cut into test pieces of 38.1 mm (1.5 inches) and the Gurley cord hardness was measured using a "Gurley's stiffness tester" manufactured by Yasuda Seiki Co., Ltd. Figure 1 shows a perspective view of the "Gurley's stiffness tester."
[0059] The method of mounting and measuring the test piece is as follows: (a) Fix the chuck 1 to the set position according to the length of the sample, and mount the test piece 2. (b) The load setting holes are located at 25.4 mm (1 inch) (W1 in Fig. 1), 50.8 mm (2 inches) (W2 in Fig. 1), and 101.6 mm (4 inches) (W3 in Fig. 1) from the shaft at the bottom of the rotating rod 3 (below the bearing), so set the weight of the load and the position of the hole according to the flexibility of the test piece 2. In this case, the load and the position of the hole must be selected so that the needle 5 on the scale plate 4 points to 2 to 4. (c) Once the setting suitable for the test piece 2 is completed, press the drive button to move the drive shaft left and right, and read the value on the scale plate 4 where the needle points to within 0.1 units. (d) For one test piece 2, once left and once right, 10 test pieces, a total of 20 values are obtained, and the average value for one sample is obtained. The calculation method is as follows. The average value of each measurement was calculated using the following formula. Finally, the Gurley cord hardness (mg) was divided by the amount of resin attached (%) to obtain the Gurley cord hardness per unit of resin attached to the cord (mg / %). Gurley cord hardness (mg) = R x {(W1 x 1) + (W2 x 2) + (W3 x 4)} / 5 x (L-12.7) 2 / W×19.8 however, R: Average value of measured values W1: Load applied to the load position (hole) at 25.4 mm (unit: g) W2: Load applied to the load position (hole) at 50.8 mm (unit: g) W3: Load applied to the load position (hole) at 101.6 mm (unit: g) L: Sample length (mm) W: Width of test piece (code gauge) (mm).
[0060] (6) Change in hardness of Gurley cord after heating (change after heating) A synthetic fiber cord was cut to a length of 1 m, a metal hook was tied to one end of the cord, and a 300 g weight was tied to the other end. The synthetic fiber cord was heated by hanging the cord vertically in the air for 2 hours in an environment controlled at a temperature of 160°C. The Gurley cord hardness was then determined in the same manner as in (5) above. The value in (6) was divided by the value in (5) to determine the rate of change (%) in the Gurley cord hardness after heating.
[0061] (7) Infrared absorption spectroscopy (IR) of adhesive resin FT-IR measurements were performed on both the synthetic fiber cord for rubber reinforcement with the adhesive resin attached and the twisted cord before the adhesive resin treatment. The spectrum of the synthetic fiber cord was subtracted from the spectrum of the twisted cord (textile material) to obtain a difference spectrum, and the spectrum of the adhesive resin was obtained. From the obtained spectrum, NH absorption (wavenumber 1510-1550 cm -1 ) was confirmed.
[0062] (Examples 1 to 7) Glycerol polyglycidyl ether ("Denacol" EX313, manufactured by Nagase Chemical Industries, Ltd.) was diluted with water to obtain a primer treatment agent with a total solid content of 6.0% by weight.
[0063] In addition, the compound (A) having a phenolic hydroxyl group, the blocked isocyanate compound (B), and the rubber latex (C) were mixed with water so that the solid contents of each were in the ratios shown in Table 1, to obtain an adhesive treatment agent with a total solid content concentration of 15% by weight.
[0064] Two 1670 dtex circular cross section polyester multifilament yarns ("Tetoron" 1670T-360-705M, manufactured by Toray Industries, Inc.) were twisted with a twist number of 40 turns / 10 cm for the first twist and 40 turns / 10 cm for the second twist to obtain a twisted yarn cord.
[0065] The twisted yarn cord was immersed in the primer treatment agent using a Computreator treatment machine (manufactured by Ritzler Co., Ltd.), then dried at 120° C. for 2 minutes, and subsequently subjected to heat treatment at 245° C. for 1 minute.
[0066] Next, using a Computreator processor (manufactured by Ritzler Co., Ltd.), the cord was immersed in an adhesive treatment agent containing the above-mentioned components (A), (B), and (C), and then dried at 120°C for 2 minutes, followed by heat treatment at 245°C for 1 minute to obtain a synthetic fiber cord.
[0067] The solid adhesive adhesion amount of the obtained synthetic fiber cord was 1.2 parts by weight of the primer treatment agent per 100 parts by weight of the synthetic fiber, and 4.0 parts by weight of the adhesive containing (A), (B) and (C) per 100 parts by weight of the synthetic fiber.
[0068] Example 8 Two 1400 dtex circular cross-section polyamide multifilament yarns ("Amilan" 1400T-204-1783, manufactured by Toray Industries, Inc.) were twisted with a twist number of 40 turns / 10 cm for the first twist and 40 turns / 10 cm for the second twist to obtain a twisted yarn cord. A synthetic fiber cord was obtained by carrying out the same process as in Example 1, except that this was used instead of the polyester multifilament yarn.
[0069] The solid adhesive adhesion amount of the obtained synthetic fiber cord was 1.2 parts by weight of the primer treatment agent per 100 parts by weight of the synthetic fiber, and 4.0 parts by weight of the adhesive containing (A), (B) and (C) per 100 parts by weight of the synthetic fiber.
[0070] Example 9 Two 1670 dtex circular cross-section Kevlar multifilament yarns were twisted with a twist number of 40 times / 10 cm for the first twist and 40 times / 10 cm for the second twist to obtain a twisted yarn cord. This was used instead of the polyester multifilament yarn, and a synthetic fiber cord was obtained by carrying out the same treatment as in Example 1, except that the total solid content of the primer treatment agent was 10% by weight and the total solid content of the adhesive containing (A), (B) and (C) was 15% by weight.
[0071] The solid adhesive adhesion amount of the obtained synthetic fiber cord was 1.8 parts by weight of the primer treatment agent per 100 parts by weight of the synthetic fiber, and 6.0 parts by weight of the adhesive containing (A), (B) and (C) per 100 parts by weight of the synthetic fiber.
[0072] [Table 1]
[0073] (Examples 10 to 12) The compound (A) having a phenolic hydroxyl group, the blocked isocyanate compound (B), and the rubber latex (C) were mixed with water so that the solid contents of each were in the ratios shown in Table 1, to obtain an adhesive treatment agent with a total solid content concentration of 8% by weight.
[0074] In addition, a molar ratio of resorcinol / formalin was 1 / 1.4, mixed in the presence of caustic soda, adjusted to a solid content concentration of 10%, and aged for 2 hours to obtain an initial condensation product of resorcinol and formalin. Next, this initial condensation product (RF) was mixed with rubber latex (Nippol 2518FS, manufactured by Nippon Zeon Co., Ltd.) in a ratio of RF / L = 1 / 5 (solid content weight ratio) and aged for 24 hours. This mixture was diluted with water to obtain an RFL adhesive treatment agent with a solid content weight of 15%.
[0075] Two 1670 dtex circular cross section polyester multifilament yarns ("Tetoron" 1670T-360-705M, manufactured by Toray Industries, Inc.) were twisted with a twist number of 40 turns / 10 cm for the first twist and 40 turns / 10 cm for the second twist to obtain a twisted yarn cord.
[0076] The twisted yarn cord was immersed in an adhesive treatment agent containing the above-mentioned components (A), (B) and (C) using a Computoreater treatment machine (manufactured by Ritzler Co., Ltd.), then dried at 120°C for 2 minutes and subsequently heat-treated at 245°C for 1 minute.
[0077] Next, the cord was immersed in the RFL adhesive treatment agent using a Computreator treatment machine (manufactured by Ritzler Co., Ltd.), dried at 120° C. for 2 minutes, and then heat-treated at 245° C. for 1 minute to obtain a synthetic fiber cord.
[0078] The adhesive solids adhesion amount of the obtained synthetic fiber cord was 3.0 parts by weight of the adhesive containing (A), (B), and (C) per 100 parts by weight of the synthetic fiber, and 4 parts by weight of the adhesive containing RFL per 100 parts by weight of the synthetic fiber.
[0079] Comparative Example 1 A synthetic fiber cord was obtained by carrying out the same treatment as in Example 10, except that the step of immersing the cord in an adhesive treatment agent containing (A), (B) and (C) and then carrying out a dry heat treatment was not carried out. The adhesive solid content of the obtained synthetic fiber cord was 4 parts by weight of the adhesive containing RFL per 100 parts by weight of the synthetic fiber.
[0080] Comparative Example 2 A synthetic fiber cord was obtained in the same manner as in Example 1, except that the solid contents of (A), (B), and (C) were set to the ratios shown in Table 1. The adhesive solid content of the obtained synthetic fiber cord was 1.2 parts by weight for the primer treatment agent per 100 parts by weight of the synthetic fiber, and 4.0 parts by weight for the adhesive containing (A), (B), and (C) per 100 parts by weight of the synthetic fiber.
[0081] Comparative Example 3 Glycerol polyglycidyl ether ("Denacol" EX313, manufactured by Nagase Chemical Industries, Ltd.) was diluted with water to obtain a primer treatment agent with a total solid content of 6.0% by weight.
[0082] In addition, a molar ratio of resorcinol / formalin was 1 / 1.4, mixed in the presence of caustic soda, adjusted to a solid content concentration of 10%, and aged for 2 hours to obtain an initial condensation product of resorcinol and formalin. Next, this initial condensation product (RF) was mixed with rubber latex (Nippol 2518FS, manufactured by Nippon Zeon Co., Ltd.) in a ratio of RF / L = 1 / 5 (solid content weight ratio) and aged for 24 hours. This mixture was diluted with water to obtain an RFL adhesive treatment agent with a solid content weight of 15%.
[0083] Two 1670 dtex circular cross section polyester multifilament yarns ("Tetoron" 1670T-360-705M, manufactured by Toray Industries, Inc.) were twisted with a twist number of 40 turns / 10 cm for the first twist and 40 turns / 10 cm for the second twist to obtain a twisted yarn cord.
[0084] The twisted yarn cord was immersed in the above-mentioned primer treatment agent using a Computreator treatment machine (manufactured by Ritzler Co., Ltd.), then dried at 120°C for 2 minutes, and subsequently heat-treated at 245°C for 1 minute.
[0085] Next, the cord was immersed in the RFL adhesive treatment agent using a Computreator treatment machine (manufactured by Ritzler Co., Ltd.), dried at 120° C. for 2 minutes, and then heat-treated at 245° C. for 1 minute to obtain a synthetic fiber cord.
[0086] The solid adhesive adhesion amounts of the primer treatment agent and the RFL-containing adhesive on the resulting synthetic fiber cord were 1.2 parts by weight per 100 parts by weight of the synthetic fiber, and 4 parts by weight per 100 parts by weight of the synthetic fiber.
[0087] Comparative Example 4 A synthetic fiber cord was obtained by carrying out the same treatment as in Comparative Example 3, except that the primer treatment agent used was a mixture of glycerol polyglycidyl ether ("Denacol" EX313, manufactured by Nagase Chemical Industries, Ltd.), a blocked isocyanate compound ((B)-1) and a rubber latex ((C)-1) in a solids ratio of 15 / 15 / 70, which was then diluted with water to a total solids content of 6.0% by weight. The adhesive solids adhesion amount of the obtained synthetic fiber cord was 1.2 parts by weight per 100 parts by weight of the primer treatment agent and 4.0 parts by weight of the adhesive containing RFL per 100 parts by weight of the synthetic fiber.
[0088] Comparative Example 5 A synthetic fiber cord was obtained by carrying out the same treatment as in Comparative Example 4, except that the RFL treatment agent was changed to the PRFL treatment agent described below. The solid content of the adhesive of the obtained synthetic fiber cord was 1.2 parts by weight of the primer treatment agent per 100 parts by weight of the synthetic fiber, and 4.0 parts by weight of the adhesive containing RFL per 100 parts by weight of the synthetic fiber. The resorcinol / formalin molar ratio was 1 / 1.4, and mixed in the presence of caustic soda, and the solid content concentration was adjusted to 10%, and aged for 2 hours to obtain an initial condensation product of resorcinol and formalin. Next, this initial condensation product (RF) was mixed with rubber latex (Nippol 2518FS, manufactured by Nippon Zeon Co., Ltd.) in a ratio of RF / L = 1 / 5 (solid content weight ratio), and aged for 24 hours. To this, 20 parts of chloro-modified resorcinol-formaldehyde condensate (Denabond-E (Nagase Chemtex Corporation)) was mixed with 100 parts by weight of the solid content of the resorcinol-formalin-latex, and the mixture was further aged for 20 hours. The mixture was diluted with water to a solid content of 15% by weight, and used as a PRFL treatment agent.
[0089] [Table 2]
[0090] The components of the adhesive treatment agents shown in Tables 1 and 2 are as follows: (A)-1: Vanillin (Fujifilm Wako Pure Chemical Industries, Ltd.) (A)-2: Vanillic acid (Fujifilm Wako Pure Chemical Industries, Ltd.) (A)-3: Ortho-vanillin (Tokyo Chemical Industry Co., Ltd.) (B)-1: Blocked isocyanate (Meisei Chemicals, DM-6400) (C)-1: Rubber latex (Pyratex, manufactured by Nippon A&L Co., Ltd.) The synthetic fiber cord thus obtained was embedded in unvulcanized rubber and vulcanized, after which the initial adhesive strength, heat-resistant adhesive strength, and fatigue resistance in rubber were measured. In addition, analysis by pyrolysis GC-MS, IR measurement, Gurley cord hardness, and Gurley cord hardness after heating were measured by the methods described above. The results are shown in Table 1.
[0091] As can be seen from the results in Tables 1 and 2, in the case of Examples 1 to 12 according to the present invention, the adhesion to rubber and heat-resistant adhesion are good, and further, fatigue resistance in a high-temperature atmosphere is remarkably improved. [Explanation of symbols]
[0092] 1 Chuck 2 Test specimens 3 Rotating rod 4 Scale plate 5 needles W1 Load setting hole (25.4mm (1 inch) from shaft) W2 Load setting hole (50.8mm (2 inches) from shaft) W3 Load Setting Hole (101.6mm (4 inches) from shaft)
Claims
1. A synthetic fiber cord for reinforcing rubber, comprising a synthetic fiber and an adhesive resin adhered to the synthetic fiber, wherein guaiacol having a mass-to-charge ratio (m / z) of 124 is detected in the adhesive resin by pyrolysis GC-MS analysis.
2. 2. The synthetic fiber cord for reinforcing rubber according to claim 1, characterized in that vanillin having a mass-to-charge ratio (m / z) of 152 is detected in the adhesive resin by pyrolysis GC-MS analysis.
3. Infrared absorption spectrum analysis (IR) of adhesive resin shows a wave number of 1510 to 1550 cm -1 3. The synthetic fiber cord for reinforcing rubber according to claim 1, which shows a peak due to deformation vibration of an N--H group in the range of
4. 4. The synthetic fiber cord for rubber reinforcement according to any one of claims 1 to 3, characterized in that the Gurley cord hardness per unit of resin attached to the cord is 70 mN / % or less, and the rate of change in Gurley cord hardness after heating is 90% to 230%.
5. 5. The synthetic fiber cord for reinforcing rubber according to claim 1, characterized in that an adhesive resin containing resorcinol-formalin-rubber latex (RFL) is adhered to the synthetic fiber cord.
6. 6. The synthetic fiber cord for reinforcing rubber according to claim 1, wherein the synthetic fiber comprises at least one fiber selected from the group consisting of nylon fiber, polyester fiber, and aromatic polyamide fiber.
7. A rubber product comprising the synthetic fiber cord for rubber reinforcement according to any one of claims 1 to 6.
Citation Information
Patent Citations
Adhesive composition for cloth or cord coating, coating method and coated cloth or cord
JP1984093774A
Aramid fiber / Rubber composite material and its production
JP1995011012A
Polyester fiber cord for reinforcing rubber
JP2009203594A
Manufacturing method of polyester fiber cord for rubber reinforcement and tire
JP2013076186A
Aramid fiber cord and method for manufacturing the same
JP2014530302A