Electrode manufacturing method
The method addresses electrode manufacturing by using elastic rolls to apply compressive and deformation forces on the uncoated area, preventing breakage and wrinkles, thus enhancing the manufacturing process efficiency.
Patent Information
- Application Number
- JP2021142874
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-02
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-09-02
AI Technical Summary
Existing methods for manufacturing electrodes with coated and uncoated areas face issues of breakage at the uncoated portion due to elongation differences, leading to wrinkles and potential fractures.
A method involving a precursor sheet with a coated and uncoated part, where the uncoated part is pressed using a pair of elastic rolls with a shaft and elastic body, applying both compressive and deformation forces to stretch the uncoated area without breakage.
The method effectively stretches the uncoated portion while suppressing breakage and wrinkles, reducing the need for separate tensioning devices and allowing for downsized manufacturing equipment.
Smart Images

Figure 0007559714000004 
Figure 0007559714000005 
Figure 0007559714000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing an electrode. [Background technology]
[0002] As a method for manufacturing an electrode, a method in which a sheet in which an electrode mixture is applied onto a long metal foil is rolled is known.
[0003] For example, Patent Document 1 discloses a method for pressing a battery electrode having a coated portion coated with an electrode active material and an uncoated portion not coated with the electrode active material. Patent Document 2 discloses a method for stretching only the uncoated portion of an electrode material to which a tensile force is applied between guide rolls using a pressing roll, and then roll-pressing the electrode material. Patent Document 3 discloses a roll-pressing method using a roll press machine equipped with a wrinkle prevention device that suppresses the occurrence of wrinkles caused by the roll-pressing operation in the coated and uncoated portions of an electrode plate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5760366 [Patent Document 2] JP 2014-220113 A [Patent Document 3] JP 2019-102172 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, when a sheet having a coated portion and an uncoated portion is pressed, the coated portion and the uncoated portion may be pressed separately to adjust the difference in elongation so as to prevent wrinkles from occurring. In this case, breakage may occur in the uncoated portion located at the edge of the sheet.
[0006] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide a method for manufacturing an electrode that can stretch an uncoated portion while suppressing breakage. [Means for solving the problem]
[0007] In order to solve the above problems, the present disclosure provides a method for manufacturing an electrode, comprising: a preparation step of preparing a precursor sheet having a metal foil and a coated portion and an uncoated portion arranged on the metal foil; a coated portion pressing step of pressing the coated portion in a thickness direction; and an uncoated portion pressing step of pressing the uncoated portion in the thickness direction before or after the coated portion pressing step, wherein the coated portion contains an electrode material including at least an active material, and the uncoated portion does not contain the electrode material and is arranged at an end of the coated portion, and in the uncoated portion pressing step, the uncoated portion is roll-pressed while being pressed in the thickness direction using a pair of elastic rolls having a shaft and an elastic body covering the shaft.
[0008] According to the present disclosure, the uncoated portion is roll pressed using a specified elastic roll, so that the uncoated portion can be stretched while preventing breakage.
[0009] In the above disclosure, the elastic body may have a compressive Young's modulus of 11.1 MPa or more and 86.1 MPa or less.
[0010] In the above disclosure, the elastic body may have a compressive Young's modulus of 20 MPa or more.
[0011] In the above disclosure, when the thickness of the elastic body is T1 and the thickness of the applied electrode mixture is T2, T1 / T2 may be 4 or more.
[0012] In the above disclosure, the uncoated portion pressing step may be performed while applying a tensile force of 100 N or less. Effect of the Invention
[0013] The present disclosure has the effect of enabling the uncoated portion to be stretched while suppressing breakage. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a flow diagram showing an example of a method for producing an electrode according to the present disclosure. [Diagram 2] FIG. 1 is a diagram illustrating the mechanism in the present disclosure. [Diagram 3] FIG. 1 is a diagram illustrating the mechanism in the present disclosure. [Figure 4] FIG. 2 is a schematic plan view illustrating an example of a precursor sheet in the present disclosure. [Diagram 5] FIG. 2 is a diagram illustrating an uncoated portion pressing step in the present disclosure. [Figure 6] FIG. 2 is a diagram illustrating a method for measuring elongation in the examples and comparative examples. [Figure 7] FIG. 2 is a diagram illustrating the breaking limit elongation in the examples and comparative examples. [Figure 8] 1 is a graph showing the relationship between compressive Young's modulus and breaking limit elongation in Examples. [Figure 9] FIG. 13 is a diagram illustrating a reference example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the manufacturing method of an electrode according to the present disclosure will be described in detail. In this specification, when expressing an aspect in which another member is disposed on a certain member, the term "on" includes both a case in which another member is disposed directly on a certain member so as to be in contact with the certain member, and a case in which another member is disposed above a certain member via another member, unless otherwise specified.
[0016] FIG. 1 is a flow diagram showing an example of a method for producing an electrode according to the present disclosure. In FIG. 1, first, a precursor sheet having a metal foil and a coated portion and an uncoated portion arranged on the metal foil is prepared (preparation step). The coated portion contains an electrode material including at least an active material. The uncoated portion does not contain an electrode material and is arranged at an end of the coated portion. Next, the coated portion is pressed in the thickness direction (coated portion pressing step). Then, the uncoated portion is pressed in the thickness direction (uncoated portion pressing step). In FIG. 1, the uncoated portion pressing step is performed after the coated portion pressing step, but it may be performed before the coated portion pressing step. In the uncoated portion pressing step, a pair of elastic rolls having a shaft body and an elastic body covering the shaft body are used to roll press the uncoated portion while pressing it in the thickness direction.
[0017] According to the present disclosure, the uncoated portion is roll pressed using a specified elastic roll, so that the uncoated portion can be stretched while preventing breakage.
[0018] In Patent Document 2, a stepped roll is pressed against one side of the uncoated portion to stretch it, and only a tensile force for stretching is applied to the uncoated portion. Although this method can stretch the uncoated portion, there is a risk of it breaking (see FIG. 2(b)). In Patent Document 3, the uncoated portion of the electrode mixture is stretched by a rolling mechanism. As shown in Comparative Example 2 described later, the method of applying only a press pressure (compressive force) does not allow the uncoated portion to be stretched effectively.
[0019] On the other hand, in the manufacturing method of an electrode according to the present disclosure, a predetermined elastic roll is used to roll-press the uncoated portion, so that the compressive force and the deformation force caused by the deformation of the elastic body can be applied to the same location of the uncoated portion, thereby suppressing the generation of voids and enabling stretching while suppressing breakage of the uncoated portion.
[0020] The mechanism in the present disclosure will be explained using the figures. FIG. 2(a) is a schematic diagram showing a general metal foil. As shown in FIG. 2(a), the metal foil generally contains a hard tissue harder than the material of the metal foil as an inclusion. By including the hard tissue, for example, the strength of the metal foil can be increased. When a tensile force (a force in the left-right direction of the paper) is applied to stretch the metal foil, the hard tissue does not deform, but the surrounding metal foil, which is softer than the hard tissue, deforms. As a result, as shown in FIG. 2(b), voids are formed around the hard tissue. Then, a plurality of voids are connected to each other, causing breakage. On the other hand, in the manufacturing method of the electrode in the present disclosure, as shown in FIG. 2(c), a compressive force and a deformation force of an elastic body can be locally applied to the metal foil. As a result, it is considered that the generation of voids around the hard tissue can be suppressed. In addition, even if voids are generated, it is considered that the expansion of the voids due to the compressive force can be suppressed. Here, the deformation force of the elastic body acts in the same direction as the tensile force (the left-right direction on the paper in FIG. 2) and is a force that stretches the metal foil like the tensile force. On the other hand, since the deformation force is applied to the point where the elastic body and the metal foil (uncoated portion) are in contact as described below, it is considered that the force can be applied more locally than, for example, the tensile force applied by a tension applying device.
[0021] Next, the mechanism in the present disclosure will be described using a schematic diagram of the elastic roll in the present disclosure. As shown in FIG. 3, the uncoated portion 3 (metal foil 1) and the elastic body 22 in the pair of elastic rolls 20 (A, B) come into contact with each other during roll pressing. By pressing the pair of elastic rolls 20 (A, B) from the thickness direction of the precursor sheet, a compressive force (a force from the vertical direction of the paper surface) can be applied to the uncoated portion. In addition, since the elastic body 22 of the elastic rolls 20 (A, B) has elasticity, the elastic body 22 is deformed by the compressive force, and a deformation force (a force in the horizontal direction of the paper surface) is applied to the uncoated portion 3 in contact with the elastic body 22. In this way, by using the elastic roll of the present disclosure, both the compressive force and the deformation force of the elastic body can be applied to the same location of the uncoated portion. This allows the uncoated portion to be stretched while suppressing breakage. Furthermore, with the electrode manufacturing method disclosed herein, the force required to stretch the uncoated portion can be provided by the deformation force of the elastic body, so that the uncoated portion can be stretched without the need for a separate tensioning device or the like, and it is also possible to miniaturize the manufacturing equipment.
[0022] 1. Preparation process The preparing step in the present disclosure is a step of preparing a precursor sheet having a metal foil and a coated portion and an uncoated portion disposed on the metal foil.
[0023] The precursor sheet prepared in the preparation step has a metal foil, a coated portion, and an uncoated portion.
[0024] The material of the metal foil can be a metal used as a material of a battery current collector. Details will be described in "4. Electrodes". The thickness of the metal foil is, for example, 1 μm or more, and may be 10 μm or more. On the other hand, the thickness of the metal foil is, for example, 100 μm or less.
[0025] The coated portion of the precursor sheet contains an electrode material including at least an active material. The coated portion is disposed on the metal foil. The coated portion becomes an electrode layer through a coated portion pressing process described below.
[0026] The electrode material contains at least an active material. The electrode material may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary. The active material, the conductive material, and the binder are described in "4. Electrodes."
[0027] The coated portion may be disposed only on the first surface of the metal foil in the thickness direction, or may be disposed on both the first surface and the second surface opposite to the first surface.
[0028] The coated parts are preferably arranged in the longitudinal direction (transport direction) of the metal foil.
[0029] The thickness of the coated portion is not particularly limited and can be appropriately adjusted according to the desired electrode size. The thickness of the coated portion is, for example, 0.2 mm or more, may be 0.3 mm or more, or may be 0.5 mm or more. On the other hand, the thickness of the coated portion is, for example, 1.5 mm or less, may be 1.0 mm or less, or may be 0.6 mm or less.
[0030] The width of the coated portion (the length in the direction perpendicular to the longitudinal direction of the metal foil) is not particularly limited and can be adjusted appropriately according to the desired electrode size. The ratio of the width of the coated portion to the width of the metal foil is, for example, 30% or more, or may be 50% or more, or may be 70% or more. Moreover, the ratio is, for example, 90% or less, or may be 80% or less.
[0031] The uncoated portion does not contain the electrode material and is disposed at an end of the coated portion. The uncoated portion may be disposed at only one end of the coated portion, or at both ends of the coated portion. The uncoated portion may be disposed at only one end of the metal foil in a direction perpendicular to the longitudinal direction of the metal foil, or at both ends.
[0032] The uncoated portion is disposed on the metal foil. The uncoated portion is usually disposed on the same side of the metal foil as the coated portion. The uncoated portion is, for example, a portion where the metal foil is exposed.
[0033] The width of the uncoated portion (the length in the direction perpendicular to the longitudinal direction of the metal foil) is not particularly limited and can be appropriately adjusted according to the desired electrode size. The ratio of the width of the uncoated portion to the width of the metal foil is, for example, 3% or more, and may be 5% or more. On the other hand, the ratio is, for example, 20% or less, and may be 10% or less.
[0034] The ratio of the width of the uncoated portion to the width of the coated portion is, for example, 20% or more, and may be 30% or more, whereas the ratio is, for example, 50% or less.
[0035] The precursor sheet can be prepared, for example, by applying an electrode material containing a dispersion medium to a metal foil and drying it. Examples of the dispersion medium include organic solvents such as butyl butyrate, dibutyl ether, and heptane. The method for applying the electrode material is not particularly limited, and a general application method can be used. The drying temperature is not particularly limited as long as it is a temperature at which the dispersion medium volatilizes.
[0036] The precursor sheet prepared in the preparation step may be, for example, a precursor sheet 10 having, in a plan view, one row of coated sections 2 and two rows of uncoated sections 3 arranged in a striped pattern at both ends of the coated sections 2, as shown in Fig. 4. Although not shown, the precursor sheet may also be a sheet having, in a plan view, N rows (N is an integer of 2 or more) of coated sections and uncoated sections arranged at both ends of each of the N rows of coated sections. In this case, the number of rows of uncoated sections is N+1.
[0037] 2. Coating press process The coated portion pressing step is a step of pressing the coated portion in the thickness direction. The coated portion pressing step may be performed before or after the uncoated portion pressing step described below.
[0038] The method and conditions of the coating part pressing step are not particularly limited as long as the coating part can be pressed and stretched. For example, a roll pressing method in which the coating part is roll-pressed can be mentioned as a pressing method. For example, the coating part can be pressed by passing the precursor sheet between a pair of press rolls and pressing the press rolls against both sides of the precursor sheet in the thickness direction.
[0039] The compressive force in the coated portion pressing step is not particularly limited, but is preferably greater than the compressive force in the uncoated portion pressing step described below. This is because wrinkles may occur in the coated portion of the precursor sheet when it is wetted with the electrode material (slurry) containing a dispersion medium, and a large stretching force is required to remove the wrinkles.
[0040] 3. Pressing process for uncoated parts The uncoated portion pressing step is a step of pressing the uncoated portion in the thickness direction before or after the coated portion pressing step, and in the uncoated portion pressing step, the uncoated portion is roll-pressed while being pressed in the thickness direction using a pair of elastic rolls having a shaft body and an elastic body covering the shaft body.
[0041] By pressing the uncoated portion, the uncoated portion can be stretched to adjust the difference in elongation with the coated portion. This makes it possible to prevent wrinkles from forming in the electrode. The amount of elongation of the uncoated portion is appropriately adjusted according to the conditions of the coated portion pressing process.
[0042] Here, the uncoated portion pressing step will be described with reference to the drawings. Fig. 5(a) is a schematic side view of the uncoated portion pressing step as seen from the width direction of the metal foil. Fig. 5(b) is a schematic plan view of Fig. 5(a) as seen from the thickness direction of the precursor sheet (the vertical direction of the paper). Fig. 5(c) is a schematic front view of Fig. 5(a) as seen from the conveying direction of the precursor sheet (the horizontal direction of the paper).
[0043] As shown in Figures 5(a) and (c), in the uncoated portion pressing process, the precursor sheet is passed between a predetermined pair of elastic rolls 20A and 20B, while the elastic rolls 20A and 20B are pressed against both sides of the precursor sheet in the thickness direction, thereby roll-pressing the uncoated portion 3 (metal foil 1).
[0044] The elastic roll 20 usually has a roll shape in which an elastic body 22 is arranged around a shaft body 21. As shown in FIG. 5(c), the elastic roll is a so-called stepped roll, and can press only the uncoated parts. In the case of a roll shape, the shaft body of the elastic roll and the elastic body are bonded to each other, so that deformation of the elastic body in the conveying direction of the precursor sheet is suppressed compared to a sheet shape, and the compressive force can be made stronger. In addition, the deformation direction of the elastic body is stable, and the occurrence of wrinkles can be further suppressed.
[0045] The material of the shaft body is not particularly limited, but is preferably a material having a compressive Young's modulus greater than that of the elastic body. Examples of the material of the shaft body include metal.
[0046] The elastic body is not particularly limited as long as it is a material having elasticity, and examples thereof include rubber and resins such as urethane.
[0047] The elastic body preferably has a predetermined compression Young's modulus. The compression Young's modulus is, for example, 10 MPa or more, may be 11.1 MPa or more, may be 15 MPa or more, or may be 20 MPa or more. On the other hand, the compression Young's modulus is, for example, 90 MPa or less, may be 86.1 MPa or less, may be 60 MPa or less, may be 40 MPa or less, or may be 35 MPa or less. If the compression Young's modulus is too low, the deformation of the elastic body becomes too large, and excessive deformation force is applied to the uncoated part. As a result, there is a risk that breakage cannot be sufficiently suppressed. On the other hand, if the compression Young's modulus is too high, the elastic body is difficult to deform, and there is a risk that sufficient deformation force cannot be applied to the uncoated part.
[0048] 5(b), the width W1 of the elastic body may be wider than the width W2 of the uncoated portion. W1 / W2 is, for example, 1.1 or more, or may be 1.2 or more, or may be 1.3 or more.
[0049] As shown in Figures 5(a) and 5(c), when the thickness of the elastic body is T1 and the thickness of the coated portion is T2, T1 / T2 is, for example, 4 or more, and may be 5 or more, 10 or more, or 15 or more. On the other hand, T1 / T2 is, for example, 40 or less, and may be 33.3 or less, 30 or less, 25 or less, or 20 or less. The thickness of the elastic body (T1) is typically determined as the radius of the elastic roll minus the radius of the shaft body.
[0050] In the present disclosure, the compression force in the uncoated portion pressing step is not particularly limited, but is preferably adjusted appropriately based on the material of the elastic body used, the material of the metal foil, and the required elongation. The compression load is, for example, 2 kgf / cm or more, may be 2.1 kgf / cm or more, may be 5 kgf / cm or more, or may be 10 kgf / cm or more. On the other hand, the linear pressure is, for example, 40 kgf / cm or less, may be 36 kgf / cm or less, may be 30 kgf / cm or less, or may be 20 kgf / cm or less. The method of determining the compression force (linear pressure) will be described in the examples.
[0051] The uncoated portion can be stretched by applying a deformation force by the elastic roll to the uncoated portion. Therefore, in the uncoated portion pressing step of the present disclosure, the tensile force can be reduced compared to when an elastic roll is not used (for example, when a metal roll is used). The tensile force applied in the uncoated portion pressing step is, for example, 100 N or less, may be 70 N or less, or may be 50 N or less. On the other hand, the tensile force is, for example, 30 N or more. The tensile force can be applied, for example, by a tension applying device.
[0052] The uncoated section pressing step is performed before or after the coated section pressing step. That is, the uncoated section pressing step may be (i) performed before the coated section pressing step and not necessarily after the coated section pressing step, (ii) performed after the coated section pressing step and not before the coated section pressing step, or (iii) performed before the coated section pressing step and further after the coated section pressing step.
[0053] 4. Electrode In the electrode manufactured by the method of the present disclosure, an electrode layer is formed on at least one surface of the metal foil. The electrode layer is a layer obtained by pressing the coated portion. The electrode manufactured by the method of the present disclosure may be a positive electrode or a negative electrode.
[0054] The metal foil typically functions as a current collector (current collector). That is, the metal foil may be a positive electrode current collector or a negative electrode current collector. When the metal foil is a positive electrode current collector, examples of the material of the metal foil include Al, SUS, and Ni. When the metal foil is a negative electrode current collector, examples of the material of the metal foil include Cu, SUS, and Ni.
[0055] The electrode layer contains at least an active material. When the electrode layer is a positive electrode layer, the active material is a positive electrode active material. A typical example of the positive electrode active material is an oxide active material. For example, LiCoO 2 , LiMnO 2 , LiNiO 2 , LiVO 2 , LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Rock salt layered active materials such as LiMn 2 O 4 , Li(Ni 0.5 Mn 1.5 )O 4 Spinel-type active materials such as LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCuPO 4 Examples of the olivine type active material include those mentioned above.
[0056] When the electrode layer is a negative electrode layer, the active material is a negative electrode active material. Examples of the negative electrode active material include carbon active material, oxide active material, and metal active material. Examples of the carbon active material include mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. Examples of the oxide active material include Nb 2 O 5 , Li 4 Ti 5 O 12 and SiO. Metal active materials include, for example, In, Al, Si, and Sn.
[0057] Furthermore, the electrode layer may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary.
[0058] The solid electrolyte may be, for example, an inorganic solid electrolyte. The inorganic solid electrolyte may be, for example, a sulfide solid electrolyte, an oxide solid electrolyte, a nitride solid electrolyte, or a halide solid electrolyte. In addition, the inorganic solid electrolyte may preferably have, for example, Li ion conductivity.
[0059] Examples of conductive materials include carbon materials, metal particles, and conductive polymers. Examples of carbon materials include particulate carbon materials such as acetylene black (AB) and ketjen black (KB); and fibrous carbon materials such as carbon fiber, carbon nanotubes (CNT), and carbon nanofibers (CNF). Examples of binders include fluorine-containing binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE), rubber-based binders such as butadiene rubber, and acrylic binders.
[0060] Examples of applications of the electrodes in the present disclosure include Li-ion batteries. The battery in the present disclosure may be an all-solid-state battery in which the electrolyte layer contains an inorganic solid electrolyte. Applications of the batteries in the present disclosure are not particularly limited, and examples include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicles (BEVs), gasoline-powered vehicles, and diesel-powered vehicles. In particular, the batteries are preferably used as driving power sources for hybrid electric vehicles or electric vehicles. The batteries in the present disclosure may be used as power sources for moving objects other than vehicles (for example, railways, ships, and aircraft), and may be used as power sources for electrical products such as information processing devices.
[0061] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0062] [Example 1] An electrode mixture containing a dispersion medium was applied to one side of an aluminum foil (1N30) having a thickness of 12 μm to a thickness of 500 μm and then dried, thereby preparing a precursor sheet 10 having a coated portion 2 and an uncoated portion 3 as shown in FIG.
[0063] Additionally, an elastic roll (stepped roll) was prepared in which an elastic body was placed on the surface of a shaft (diameter 50 mm). The thickness of the elastic body was 10 mm. The compression Young's modulus of the elastic body used was measured as follows. First, the elastic body was adjusted to a size of 10 mm x 10 mm x 10 mm. This elastic body was operated on an autograph so that the compression deformation rate (deformation rate) was 0% → 25% → 0% (first cycle) and 0% → 25% (second cycle), and the relationship between the deformation rate and stress was measured. The stress (σ 10 ) was used to calculate the compressive Young's modulus from the following formula. The results are shown in Table 1. Compressive Young's modulus = σ10 / 0.1
[0064] Using the prepared precursor sheet and elastic roll, the maximum elongation of the uncoated portion was calculated as follows. First, as shown in FIG. 6(a), two lines were drawn at any positions in the longitudinal direction on the uncoated portion 3 (metal foil 1) of the precursor sheet 10, and the length between the lines before pressing (L 0 ) was measured. Next, as shown in FIG. 5, a pair of elastic rolls was used to roll press the uncoated portion while pressing it in the thickness direction. Then, as shown in FIG. 6(b) and FIG. 6(c), the uncoated portion was cut out from the pressed precursor sheet, and the length (L 1 ) was measured. The elongation percentage (%) was calculated from the following formula. The uncoated portion was pressed while applying a tensile force of 50 N to the precursor sheet. Elongation rate = (L 1 -L 0 ) / L 0 ×100 The load applied to the elastic roll was increased, and the maximum elongation at which no break occurred was taken as the breaking limit elongation. The results are shown in Table 1. The load (linear pressure) at break was calculated from the following formula, and is also shown in Table 1. Linear pressure = load (P) / (elastic body width (W1) x 2)
[0065] [Examples 2 to 7] For Examples 2 to 4 and 6, precursor sheets and elastic rolls were prepared in the same manner as in Example 1, except that an elastic body having a compressive Young's modulus of the value shown in Table 1 was used. For Examples 5 and 7, precursor sheets and elastic rolls were prepared in the same manner as in Example 1, except that an elastic body having a compressive Young's modulus of the value shown in Table 1 was used and the thickness of the elastic body was changed to 1 mm. Using the prepared precursor sheets and elastic rolls, the breaking limit elongation and the breaking load were calculated in the same manner as in Example 1. The results are shown in Table 1.
[0066] [Comparative Example 1] A precursor sheet was prepared in the same manner as in Example 1. The breaking limit elongation percentage when only a tensile force was applied to the uncoated portion of this precursor sheet was determined as follows. The results are shown in Table 2. An uncoated portion (aluminum foil) was punched out from the precursor sheet and subjected to a tensile test using an autograph. The breaking limit elongation ε of the aluminum foil was calculated using the following formula: max asked for. Breaking limit elongation ε max = (elongation at break ε A )-(Springback amount at 1.0% strain ε B ) As shown in Fig. 7(a) and Fig. 7(b), ε A is the strain at which fracture occurs (%), and ε B is the amount of springback (%) from 1.0% strain.
[0067] [Comparative Example 2] Except for using a metal roll instead of the elastic roll, the breaking limit elongation and the breaking load were calculated in the same manner as in Example 1. The results are shown in Table 2.
[0068] [Table 1]
[0069] [Table 2]
[0070] As shown in Tables 1 and 2, the breaking limit elongation of Examples 1 to 7 was improved compared to Comparative Example 1. This confirmed that when both deformation force and compression force were applied to the uncoated part using an elastic roll, the breakage of the uncoated part was suppressed more than when only tensile force was applied. In addition, from Examples 1 to 7 and FIG. 8, it was confirmed that the greater the compressive Young's modulus of the elastic roll, the greater the breaking limit elongation, and the greater the effect of suppressing breakage of the uncoated part. On the other hand, from Comparative Example 2, when a metal roll with a large compressive Young's modulus was used, the uncoated part broke with almost no elongation. This is thought to be because the metal roll was hardly deformed and sufficient deformation force was not applied to the uncoated part. In addition, from Examples 4 and 5, there was no change in the breaking limit elongation even when the thickness of the elastic body was changed.
[0071] [Reference examples 1~11] An elastic roll was prepared with the thickness of the elastic body adjusted to the value shown in Table 3. A precursor sheet was prepared with the thickness of the coated portion adjusted to the value shown in Table 3. Using this elastic roll and precursor sheet, roll pressing was performed with the elastic roll riding on the coated portion as shown in FIG. 9. After pressing, the electrode sheet was checked for the presence or absence of breakage (breakage due to riding on the elastic body). The results are shown in Table 3. The roll pressing was performed by applying a compressive force such that the stretch amount of the uncoated portion was 2%. An elastic body with a compression Young's modulus of 19.6 MPa was used for the elastic roll.
[0072] [Table 3]
[0073] In pressing the uncoated portion, a certain compressive force is applied to the elastic roll and a load is applied to the elastic body in order to stretch the uncoated portion by the deformation force of the elastic body. If the elastic roll rides up on the coated portion in this state, an additional load is applied to the elastic body at the ride-up portion, and the deformation force of the elastic body increases. As a result, ride-up breakage occurs. On the other hand, if the thickness of the elastic body is sufficiently large compared to the thickness of the coated portion, the effect of the load applied when it rides up on the coated portion can be reduced, and the effect on the deformation force of the elastic body can be reduced. As a result, ride-up breakage can be prevented.
[0074] As shown in Table 3, when the thickness of the elastic body was less than four times the thickness of the coated part, run-up fracture occurred. The results of the Reference Example suggest that, taking into consideration the case where the elastic roll runs up onto the coated part due to meandering or the like, it is preferable that the thickness of the elastic body is four or more times the thickness of the coated part. [Explanation of symbols]
[0075] 1...Metal foil 2 … Coating section 3 … Uncoated area 10 ... Precursor sheet 21 ... Shaft body 22...Elastic body 20... Elastic roll
Claims
1. A preparation step of preparing a precursor sheet having a metal foil and a coated portion and an uncoated portion disposed on the metal foil; a coating portion pressing step of pressing the coating portion in a thickness direction; an uncoated portion pressing step of pressing the uncoated portion in the thickness direction before or after the coated portion pressing step; having The coated portion contains an electrode material including at least an active material, The uncoated portion does not contain the electrode material and is disposed at an end of the coated portion, In the uncoated portion pressing step, the uncoated portion is roll-pressed while being pressed in the thickness direction using a pair of elastic rolls having a shaft body and an elastic body covering the shaft body, The elastic body has a compressive Young's modulus of 10 MPa or more and 86.1 MPa or less, as measured and calculated by the <Method for measuring compressive Young's modulus of elastic body> described below; and In the uncoated portion pressing step, a tensile force of 30 N or more and 100 N or less is applied. A method for manufacturing an electrode. <Method for measuring compressive Young's modulus of elastic body> An elastic body having a size of 10 mm x 10 mm x 10 mm is subjected to an autograph so that the compression deformation rate (deformation rate) is 0% → 25% → 0% (first cycle) and 0% → 25% (second cycle), and the relationship between the deformation rate and the stress is measured. The compressive Young's modulus is calculated from the following formula using the stress (σ 10 ) when the deformation rate in the second cycle is 10%. Compressive Young's modulus = σ 10 / 0.1
2. The method for manufacturing an electrode according to claim 1 , wherein the elastic body has a compressive Young's modulus of 11.1 MPa or more and 86.1 MPa or less.
3. The method for manufacturing an electrode according to claim 2 , wherein the elastic body has a compressive Young's modulus of 20 MPa or more.
4. 4. The method for manufacturing an electrode according to claim 1, wherein, when the thickness of the elastic body is T1 and the thickness of the coated portion is T2, T1 / T2 is 4 or more.
Citation Information
Patent Citations
Language teaching device
JP1982060366A
Press device for electrode material and press-processing method
JP2014103068A
Electrode manufacturing apparatus
JP2014120273A
Roll press method and roll press facility of electrode material
JP2014220113A
Roll press machine and roll press method
JP2017084545A