Steel plate and its manufacturing method

A steel plate with controlled composition and manufacturing process addresses brittle fracture issues in high-Ni steel, ensuring high cryogenic toughness and safety in cryogenic environments by limiting Mn enrichment and stabilizing austenite.

JP7559733B2Active Publication Date: 2024-10-02JFE STEEL CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021167660
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-12
Publication Date
2024-10-02
Estimated Expiration
2041-10-12

AI Technical Summary

Technical Problem

Existing high-Ni steel plates manufactured through direct quenching and tempering exhibit decreased absorbed energy and increased risk of brittle fracture due to Mn-enriched regions and unstable austenite formation, which conventional technologies do not adequately address.

Method used

A steel plate composition with controlled amounts of C, Si, Mn, Ni, Cr, Mo, P, S, N, Al, and optional additions of Cu, Nb, V, Ti, B, Ca, REM, and Mg, along with a manufacturing process involving direct quenching and tempering, limits Mn enrichment and stabilizes austenite to suppress brittle cracks, ensuring high cryogenic toughness.

Benefits of technology

The solution provides a high-strength steel plate with excellent cryogenic toughness and reduced brittle crack generation, suitable for cryogenic environments, enhancing safety in structures like LNG tanks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559733000001
    Figure 0007559733000001
  • Figure 0007559733000002
    Figure 0007559733000002
Patent Text Reader

Abstract

To provide a high-strength steel plate that excels in cryogenic toughness and brittle crack inhibiting ability, in the case where it is produced in a simplified process using direct quenching and tempering.SOLUTION: A steel plate comprises, in mass%, C: 0.01% or more and 0.15% or less, Si: 0.01% or more and 0.50% or less, Mn: 0.05% or more and less than 0.20%, Ni: 6.0% or more and 7.5% or less, Cr: 0.01% or more and 1.00% or less, Mo: 0.01% or more and 0.50% or less, P: 0.03% or less, S: 0.005% or less, N: 0.0010% or more and 0.0080% or less, and Al: 0.008% or more and 0.100% or less, with the balance being Fe and inevitable impurities. The amount of retained austenite at a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness direction is less than 1.7%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel plate, in particular to a thick steel plate suitable for use at cryogenic temperatures, capable of stably ensuring excellent cryogenic toughness over a wide range of plate thicknesses, and a method for manufacturing the same. The steel plate of the present invention can be suitably used for structures used in cryogenic environments, such as liquefied gas storage tanks for ships and land use. [Background technology]

[0002] When hot-rolled steel plates are used in structures such as liquefied gas storage tanks, the environment in which they are used is extremely low, and so the steel plates are required to have not only excellent strength but also excellent toughness at extremely low temperatures (cryogenic toughness). For example, when hot-rolled steel plates are used in liquefied natural gas storage tanks, they need to ensure excellent toughness at extremely low temperatures of -164°C or lower, which is the boiling point of liquefied natural gas. If the cryogenic toughness of steel materials is poor, there is a risk that the safety of the cryogenic storage structures cannot be maintained, and therefore there is a strong demand for improved cryogenic toughness of the steel plates used. To meet this demand, 7%Ni or 9%Ni steel plates have been used conventionally.

[0003] A 7% Ni steel sheet is proposed in, for example, Patent Document 1. Patent Document 1 discloses a steel plate for cryogenic use containing Ni: more than 5.0% to less than 10.0% and predetermined amounts of C, Si, Mn, and Al. The steel plate disclosed in Patent Document 1 has an average absorbed energy per unit area vE-196 of 1.25 J / mm across a plate thickness of 6 to 50 mm. 2 That's all. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-219848 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors conducted extensive research into high Ni steel plate (hereinafter also referred to as 7% Ni steel plate) containing about 6.0 to 7.5% Ni, and found that when the plate is quenched and tempered directly after rolling for the purpose of improving productivity, the absorbed energy in a Charpy test or the like decreases and the risk of brittle fracture increases. However, Patent Document 1 does not consider these problems, particularly the occurrence of brittle fracture.

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a high-strength steel plate that is excellent in cryogenic temperature toughness and brittle crack initiation suppression performance, on the premise that it is produced by a reduced process using direct quenching and tempering. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors have conducted extensive research into the chemical composition and structure of 7% Ni steel sheet and have obtained the following findings. (a) The above-mentioned decrease in absorbed energy is due to the formation of Mn-enriched and Mn-depleted regions, which causes cracks (herein also referred to as separation) that are perpendicular to the fracture surface and parallel to the rolled surface. (b) The brittle crack initiation described above originates in Mn-enriched regions, particularly in unstable austenite (hereinafter also referred to as γ) which is likely to form there. (c) In order to steadily increase absorbed energy, Mn should be limited to less than 0.20%, thereby lowering the concentration of the band-like Mn-enriched regions and reducing the occurrence of separation caused by Mn segregation bands. (d) In order to reduce the occurrence of brittle cracks, in addition to ensuring the Charpy absorbed energy in the low temperature range, it is necessary to limit the amount of Mn, lower the concentration of the band-like Mn-enriched zone, and suppress the formation of γ, which is the cause of the cracks.

[0008] The present invention has been completed based on the above findings, and the gist of the present invention is as follows. [1] In mass percent, C: 0.01% or more and 0.15% or less, Si: 0.01% or more and 0.50% or less, Mn: 0.05% or more and less than 0.20% Ni: 6.0% or more and 7.5% or less, Cr: 0.01% or more and 1.00% or less, Mo: 0.01% or more and 0.50% or less, P: 0.03% or less, S: 0.005% or less, N: 0.0010% to 0.0080% and Al: 0.008% or more and 0.100% or less The remainder of the composition is Fe and unavoidable impurities. A steel plate in which the amount of retained austenite at a depth of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness direction is less than 1.7%.

[0009] [2] The composition further includes, in mass%, Cu: 0.40% or less, Nb: 0.05% or less, V: 0.05% or less, Ti: 0.03% or less and B: 0.0030% or less The steel sheet according to the above [1], containing one or more selected from the following:

[0010] [3] The composition further comprises, in mass%, Ca: 0.007% or less, REM: 0.010% or less and Mg: 0.070% or less The steel sheet according to the above [1] or [2], comprising one or more selected from the following:

[0011] [4] A method for producing a steel plate, comprising the steps of: hot rolling a steel material having a chemical composition according to any one of [1] to [3] above, with a cumulative reduction of 15 to 75% at 870°C or less and a final rolling end temperature of 830 to 700°C at the surface of the steel plate to form a steel plate; directly quenching the steel plate at a temperature from the surface of the steel plate to a depth position of 1 / 4 of the plate thickness in the plate thickness direction, with an average cooling rate of 3°C / s or more in a temperature range of 600°C or less and 300°C or more and a cooling end temperature of 300°C or less, and tempering the steel plate at 550°C or more and less than Ac1 point; and the amount of retained austenite at a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness direction is less than 1.7%. Effect of the Invention

[0012] According to the present invention, a steel plate having excellent cryogenic toughness and brittle crack suppression ability can be provided with high productivity. By using the steel plate of the present invention for steel structures used in low temperature and cryogenic environments, such as tanks for storing liquefied gas, for example, LNG tanks and liquefied CO2 tanks, the safety of the steel structures can be improved, which is an industrially significant advantage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments of the present invention will be described in detail. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited thereto.

[0014] [Component composition] The steel plate of the present invention has a predetermined composition. In addition, it is preferable that the steel material used for manufacturing the steel plate of the present invention also has the above-mentioned predetermined composition. Each element contained in this composition will be explained below. In addition, unless otherwise specified, in this specification, "%" as a unit of the content of each element means "mass%".

[0015] C: 0.01% or more and 0.15% or less C is an element that has the effect of improving the strength of a steel plate. To obtain this effect, the C content is set to 0.01% or more, and preferably 0.03% or more. On the other hand, if the C content exceeds 0.15%, the cryogenic toughness of the steel plate decreases. Therefore, the C content is set to 0.15% or less, and preferably 0.12% or less.

[0016] Si: 0.01% or more and 0.50% or less Silicon is an element that contributes to improving the strength of steel sheets and also acts as a deoxidizer. To achieve these effects, the silicon content is set to 0.01% or more, and preferably 0.03% or more. On the other hand, if the silicon content is excessively high, the toughness decreases. Therefore, the silicon content is set to 0.50% or less, and preferably 0.30% or less.

[0017] Mn: 0.05% or more and less than 0.20% Mn is an element that improves the hardenability of steel and is effective in increasing the strength of steel sheets. To obtain this effect, Mn is added at 0.05% or more. Preferably, it is added at 0.10% or more. On the other hand, if Mn is added at 0.20% or more, the probability of austenite forming locally increases, which may reduce absorbed energy, etc., so the Mn content is limited to less than 0.20%.

[0018] Ni: 6.0% or more and 7.5% or less Ni is an element that is extremely effective in improving the cryogenic toughness of steel plate. To achieve this, the Ni content is set to 6.0% or more. Preferably, it is set to 6.5% or more. More preferably, it is set to 7.0% or more. On the other hand, since Ni is an expensive element, the higher the Ni content, the higher the steel plate cost. Therefore, in the present invention, the Ni content is set to 7.5% or less.

[0019] Cr: 0.01% or more and 1.00% or less Cr is an element that can improve the strength of steel plate without significantly impairing cryogenic toughness. To obtain the above effect, the Cr content is set to 0.01% or more, and preferably 0.30% or more. However, if the Cr content exceeds 1.00%, the cryogenic toughness of the steel plate decreases. Therefore, the Cr content is set to 1.00% or less, and preferably 0.80% or less.

[0020] Mo: 0.01% or more and 0.50% or less Like Cr, Mo is an element that can improve the strength of steel plate without significantly impairing cryogenic toughness. To achieve this, the Mo content is set to 0.01% or more. Preferably, it is more than 0.10%. On the other hand, if the Mo content exceeds 0.50%, the cryogenic toughness is rather reduced. Therefore, the Mo content is set to 0.50% or less. Preferably, it is 0.30% or less. More preferably, it is 0.25% or less.

[0021] P:0.03% or less P is an inevitable impurity and a harmful element that adversely affects the cryogenic toughness of steel plates. For example, in order to obtain a sound base material and welded joint when steel plates are welded to form a welded structure, it is preferable to reduce the P content as much as possible. Therefore, the P content is suppressed to 0.03% or less. From the viewpoint of cryogenic toughness, the lower the P content, the better, so the lower limit is not particularly limited and may be 0%, but even in that case, it is acceptable to contain P as an inevitable impurity. On the other hand, excessive reduction causes an increase in cost, so from the viewpoint of cost, it is preferable to set the lower limit of the P content to 0.001%.

[0022] S: 0.005% or less Since S forms MnS in steel and significantly deteriorates cryogenic toughness, it is desirable to reduce the S content as much as possible, with an upper limit of 0.005%. The S content is preferably 0.002% or less. On the other hand, since the lower the S content, the better, there is no particular lower limit, and it may be 0%, but even in that case, it is permitted to contain S as an unavoidable impurity.

[0023] N: 0.0010% or more and 0.0080% or less N forms precipitates in steel, and if its content exceeds 0.0080%, it causes a decrease in the toughness of the base material. However, N is also an element that contributes to the refinement of the base material by forming AlN, and such an effect can be obtained by making the N content 0.0010% or more. Therefore, the N content is set to 0.0010% or more and 0.0080% or less. The N content is preferably 0.0020% or more. It is preferably 0.0060% or less.

[0024] Al: 0.008% or more and 0.100% or less Al is an element contained in the deoxidizer. If the Al content is less than 0.008%, the effect as a deoxidizer is poor. Furthermore, Al is also an element that contributes to the refinement of the base material by forming AlN. Therefore, the Al content is set to 0.008% or more. Preferably, it is set to 0.020% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the steel is impaired, and the toughness, particularly the Charpy absorbed energy at extremely low temperatures, decreases. Therefore, the Al content is set to 0.100% or less. Preferably, it is set to 0.050% or less.

[0025] The component composition in one embodiment of the present invention may be such that, in addition to the above-mentioned predetermined amounts of elements, the balance is Fe and unavoidable impurities.

[0026] In another embodiment of the present invention, the above-mentioned composition may further contain, optionally, one or more elements selected from Cu, Nb, V, Ti and B, preferably in the amounts described below.

[0027] Cu:0.40% or less Cu is an element that has the effect of increasing the strength of steel sheet by improving hardenability. However, if the Cu content exceeds 0.40%, the cryogenic toughness of the steel sheet decreases, and the surface properties of the steel (slab) after casting deteriorate. Therefore, when Cu is added, the Cu content is preferably 0.40% or less, and more preferably 0.30% or less. On the other hand, although there is no particular lower limit for the Cu content, in order to obtain the above effect, the Cu content is preferably 0.10% or more.

[0028] Nb: 0.05% or less Nb is an effective element for increasing the strength of steel plate by precipitation strengthening. However, if the Nb content is excessively high, the cryogenic toughness of the steel plate decreases. Therefore, when Nb is added, the Nb content is preferably 0.05% or less, and more preferably 0.03% or less. On the other hand, the lower limit of the Nb content is not particularly limited, but in order to obtain the above effect, the Nb content is preferably 0.010% or more.

[0029] V: 0.05% or less Like Nb, V is an effective element for increasing the strength of steel sheet by precipitation strengthening. However, if the V content is excessively high, the cryogenic toughness of the steel sheet decreases. Therefore, when V is added, the V content is preferably 0.05% or less, and more preferably 0.04% or less. On the other hand, although there is no particular lower limit for the V content, in order to obtain the above-mentioned effect, the V content is preferably 0.010% or more.

[0030] Ti: 0.03% or less Ti is an element that has the effect of increasing the toughness of the weld without degrading the mechanical properties of the base material when steel plates are welded to form a welded structure. For this purpose, it is preferable to add 0.003% or more. On the other hand, if the content exceeds 0.03%, the toughness is rather decreased, so it is preferable to add Ti in a range of 0.03% or less.

[0031] B: 0.0030% or less B is an element that improves hardenability when added in small amounts. To effectively exert this effect, it is preferable to contain 0.0003% or more of B. On the other hand, if the B content exceeds 0.0030%, toughness deteriorates. Therefore, when B is contained, the content is preferably 0.0030% or less.

[0032] In another embodiment of the present invention, the above-mentioned composition may further contain, optionally, one or more elements selected from Ca, REM and Mg, preferably in the amounts described below.

[0033] Ca: 0.007% or less Ca is an element that has the effect of improving the cryogenic toughness of steel plate by controlling the morphology of inclusions in steel. However, excessive Ca impairs the cleanliness of the steel and reduces the Charpy absorbed energy (hereinafter also referred to as Charpy toughness) at cryogenic temperatures. Therefore, when Ca is added, the Ca content is preferably 0.007% or less, and more preferably 0.004% or less. On the other hand, the lower limit of the Ca content is not particularly limited, but in order to obtain the above effect, it is preferably 0.001% or more.

[0034] REM: 0.010% or less Like Ca, REM (rare earth metal) is an element that has the effect of improving the cryogenic toughness of steel plate by controlling the morphology of inclusions in steel. However, if REM is excessive, the cleanliness of steel is impaired and the Charpy toughness is reduced. Therefore, when REM is added, the REM content is preferably 0.010% or less, and more preferably 0.008% or less. On the other hand, although there is no particular lower limit for the REM content, in order to obtain the above effect, the REM content is preferably 0.001% or more. Here, REM is a collective term for 17 elements, including 15 lanthanoid elements, Y, and Sc, and these elements can be contained alone or in combination. The content of REM means the total content of these elements.

[0035] Mg: 0.070% or less Like Ca and REM, Mg is an element that has the effect of improving the cryogenic toughness of steel plate by controlling the morphology of inclusions in steel. However, excessive Mg impairs the cleanliness of steel and reduces Charpy toughness. Therefore, when Mg is added, the Mg content is preferably 0.070% or less, and more preferably 0.004% or less. On the other hand, although there is no particular lower limit for the Mg content, it is preferable that the Mg content be 0.001% or more to obtain the above effect.

[0036] [Microstructure] The steel sheet of the present invention has a structure in which the amount of retained austenite (hereinafter also referred to as γ) at a depth position of 1 / 4 of the sheet thickness t (hereinafter also referred to as 1 / 4t) from the surface of the steel sheet in the sheet thickness direction is less than 1.7%. In other words, if the amount of retained γ is 1.7% or more, brittle cracks are likely to occur.

[0037] In addition, the structure of the steel plate is preferably a structure mainly composed of martensite and bainite, specifically, the total area ratio of bainite and martensite is preferably 98.3% or more. As described above, a structure mainly composed of bainite + martensite can easily obtain sufficient strength while ensuring excellent cryogenic toughness. The ratio of bainite to martensite can be any ratio.

[0038] The thickness of the steel plate is not particularly limited and may be any thickness, for example, preferably from 6 mm to 50 mm.

[0039] [Mechanical properties] (Tensile strength) The lower limit of the tensile strength of the steel sheet does not need to be particularly limited, but it is preferable that the lower limit is 690 MPa, and more preferably, 720 MPa or more. On the other hand, the upper limit of the tensile strength does not need to be particularly limited, but it is preferable that the upper limit is 930 MPa, and more preferably, 900 MPa or less. The tensile strength can be measured by the method described in the Examples section below.

[0040] (Cryogenic toughness) The toughness value of the steel plate is not particularly limited, but the Charpy absorbed energy (vE -196℃ In the full-size Charpy impact test, vE is preferably 200 J or more. On the other hand, it is preferably 350 J or less. More preferably, it is 280 J or less. In the half-size Charpy impact test, vE -196℃ is preferably 100 J or more. On the other hand, the upper limit is less than 200 J. More preferably, it is 150 J or less.

[0041] (Brittle crack suppression performance) As for the brittle crack initiation suppression performance of a steel plate, it is preferable that in a CTOD test, the maximum load point is reached without a sudden drop in load.

[0042] [Manufacturing method] Next, a method for producing a steel sheet of the present invention will be described. In the following description, unless otherwise specified, the temperature refers to the temperature at the center of the sheet thickness. The temperature at the center of the sheet thickness can be calculated by heat transfer calculation from the surface temperature of the steel sheet measured by a radiation thermometer, for example. That is, the steel sheet of the present invention can be suitably produced by sequentially carrying out the following steps (1) to (4). (1) Heating of steel material (2) Hot rolling (3) Quenching (accelerated cooling) (4) Tempering

[0043] (1) Heating of steel material First, it is preferable to heat a steel material having the above-mentioned composition to a temperature of 900°C or more and 1200°C or less. The method for producing the steel material is not particularly limited, but for example, the steel material can be produced by melting molten steel having the above-mentioned composition by a normal method and casting it. Melting can be carried out by any method, such as a converter, an electric furnace, or an induction furnace. Furthermore, from the viewpoint of productivity, casting is preferably carried out by a continuous casting method, but it can also be carried out by an ingot casting-breakdown rolling method. For example, a steel slab can be used as the steel material. Here, the heating of the steel material may be carried out after the steel material obtained by a method such as casting is once cooled, or the obtained steel material may be directly subjected to heating without being cooled.

[0044] If the heating temperature of the steel material is less than 900°C, the deformation resistance of the steel material is high, which may increase the load on the rolling mill in the subsequent hot rolling, making it difficult to perform the hot rolling. Therefore, it is preferable to heat the steel material to 900°C or higher. On the other hand, if the heating temperature of the steel material is higher than 1200°C, oxidation of the steel becomes significant, and the loss caused by removing the oxide film due to oxidation increases, which may result in a decrease in yield. Therefore, it is preferable to heat the steel material to 1200°C or lower.

[0045] (2) Hot rolling [Rolling reduction: Cumulative rolling reduction below 870℃ is 15-75%] In hot rolling, if the cumulative reduction is less than 15% in the austenite non-recrystallization temperature range of 870°C or less, the structure is not sufficiently refined, and toughness is reduced. On the other hand, if the cumulative reduction exceeds 75%, rolling at the following finishing temperatures becomes difficult. Therefore, the cumulative reduction at 870°C or less is set to 15 to 75%, and preferably 30 to 70%. [Final rolling temperature: 700~830℃] In hot rolling, if the final rolling end temperature is less than 700°C, separation due to texture is likely to occur, and toughness is reduced. On the other hand, if the final rolling end temperature exceeds 830°C, sufficient rolling reduction in the non-recrystallized region becomes difficult, a fine texture cannot be obtained, and strength is reduced. The final thickness of the hot-rolled steel sheet is not particularly limited, but as described above, it is preferably 6 mm or more and 50 mm or less.

[0046] (3) Quenching (accelerated cooling) The hot-rolled steel sheet after the hot rolling is directly quenched. In this direct quenching, it is essential that the average cooling rate in the temperature range of 600°C or less and 300°C or more at the 1 / 4t position of the steel sheet is 3°C / s or more.

[0047] That is, in the direct quenching, if the average cooling rate is less than 3°C / s, it is difficult to obtain the desired transformed structure, and it is difficult to obtain sufficient strength and toughness. On the other hand, although there is no particular upper limit to the average cooling rate, if the average cooling rate is higher than 200°C / s, it becomes difficult to control the temperature at each position in the steel plate, and the material tends to vary in the plate width direction and rolling direction. As a result, the material properties such as tensile properties and toughness tend to vary. Therefore, it is preferable that the average cooling rate is 200°C / s or less.

[0048] In addition, in direct quenching, if the cooling end temperature is higher than 300°C at (1 / 4)t, unstable residual γ is likely to be generated. Therefore, the cooling end temperature is set to 300°C or less at (1 / 4)t. By performing accelerated cooling under these conditions, the hot-rolled steel sheet is well quenched.

[0049] The cooling process in the direct quenching is not particularly limited and can be performed by any method. For example, air cooling and / or water cooling can be used. As for water cooling, any cooling method using water (for example, spray cooling, mist cooling, laminar cooling, etc.) can be used.

[0050] (4) Tempering Next, the quenched hot-rolled steel sheet is tempered. The tempering temperature is 550°C or higher and lower than the Ac1 point. If the tempering temperature is lower than 550°C, the tempering is insufficient and the Charpy toughness decreases. If the tempering temperature is higher than the Ac1 point, the strength decreases and unstable γ is generated, which reduces the ability to suppress the occurrence of brittle cracks.

[0051] The Ac1 point can be determined by the following formula (1). A C1 Point (℃)=750.8-26.6×C+17.6×Si-11.6×Mn-22.9×Cu-23×Ni+24.1×Cr+22.5×Mo-39.7×V-5.7×Ti +232.4×Nb-169.4×Al...(1) In the above formula (1), the element symbols represent the content (mass%) of each element, and if the element is not contained, the value is set to 0.

[0052] Any heating method can be used for the heating in the tempering process as long as the heating temperature can be controlled as described above. One example of the heating method is furnace heating. The furnace heating is not particularly limited, and a general heat treatment furnace can be used.

[0053] After the tempering temperature is reached, the material may be held at the tempering temperature for an arbitrary period of time, and then any cooling may be started. When holding at the tempering temperature, the holding time is not particularly limited, but is preferably 5 minutes or more. EXAMPLES

[0054] Steel plates were manufactured according to the procedure described below, and their properties were evaluated. First, molten steel having the composition shown in Table 1 was melted in a converter and a steel slab (thickness: 200 mm) was produced as a steel material by a continuous casting method. C1 The points (°C) are also shown in Table 1.

[0055] [Table 1]

[0056] Next, according to the conditions shown in Table 2, the obtained steel slabs were heated and hot-rolled to obtain hot-rolled steel sheets having each plate thickness (final plate thickness), which were then quenched and tempered to obtain product steel sheets.

[0057] The microstructure, residual γ content, tensile strength (TS), and Charpy absorbed energy (vE -196℃ The brittle crack initiation inhibition ability (CTOD test) was evaluated according to the following methods. The evaluation results are shown in Table 2.

[0058] [Microstructure] A test piece for microstructure observation was taken from each steel plate so that the 1 / 4t position was the observation position. The test piece was embedded in resin so that the cross section perpendicular to the rolling direction was the observation surface, and was mirror-polished. Next, after performing nital etching, the specimen was observed with a scanning electron microscope at magnifications of 2000 and 10,000 times, and images of the structure were taken. The obtained images were analyzed to identify the microstructure.

[0059] [Residual gamma content after deep-freezing treatment] Five test pieces for X-ray diffraction were taken parallel to the plate surface from the 1 / 4t position of each steel plate, and after immersion in liquid nitrogen for 30 minutes, the test pieces were ground and chemically polished so that the 1 / 4t position became the measurement surface, and then subjected to X-ray diffraction. The diffraction intensities of the (200), (211) planes of α-Fe and the (200), (220), and (311) planes of γ-Fe, which appear in the symmetric reflection X-ray diffraction pattern, were obtained, and the volume fraction of γ-Fe was calculated. The average value of the five test pieces was obtained, and this was taken as the amount of residual γ (volume fraction).

[0060] (Tensile strength) A JIS No. 4 tensile test piece was taken from the 1 / 4t position of the steel plate. Using this tensile test piece, a tensile test was carried out in accordance with the provisions of JIS Z 2241 to evaluate the tensile strength (TS) of the steel plate. If the tensile strength was 690 MPa or more, the steel plate was deemed to have high strength and passed the test.

[0061] (Cryogenic toughness) A V-notch test piece was taken from the 1 / 4t position of the steel plate in accordance with the provisions of JIS Z 2202. Using this V-notch test piece, a Charpy impact test was carried out in accordance with the provisions of JIS Z 2242, and the Charpy absorbed energy (vE -196℃ ) was obtained. The Charpy absorbed energy can be regarded as an index of the cryogenic toughness of the steel plate. For the Charpy impact test, three test pieces were taken along the rolling direction from the leading edge, trailing edge and near the center of each steel plate in the rolling direction, and measurements were performed on each test piece. The individual measurement results and average values ​​are shown in Table 2. In this full-size Charpy impact test, the vE -196℃ If the Charpy toughness was 200 J or more, it was evaluated as having excellent Charpy toughness and was considered to have passed the test.

[0062] (Ability to suppress brittle fracture) For steel plates with a thickness of 15 mm, test pieces of 10 x 10 x 55 mm were taken from a depth position of 1 / 2 the plate thickness (t) (1 / 2t), and for other steel plates, from a position of 1 / 4t, and tests were conducted in accordance with ISO 12135. The test temperature was -165°C. Those that did not experience unstable fracture (brittle fracture) in the test were deemed to have passed.

[0063] [Table 2]

Claims

1. In mass percent, C: 0.01% or more and 0.15% or less, Si: 0.01% or more and 0.50% or less, Mn: 0.05% or more and less than 0.20%; Ni: 7.0% or more and 7.5% or less, Cr: 0.01% or more and 1.00% or less, Mo: 0.01% or more and 0.50% or less, P: 0.03% or less, S: 0.005% or less, N: 0.0010% or more and 0.0080% or less; Al: 0.008% or more and 0.100% or less The balance is Fe and unavoidable impurities, A steel plate in which the amount of retained austenite at a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness direction is less than 1.7%.

2. The composition further includes, in mass%, Cu: 0.40% or less, Nb: 0.05% or less, V: 0.05% or less, Ti: 0.03% or less; B: 0.0030% or less The steel sheet according to claim 1 , comprising one or more selected from the following:

3. The composition further comprises, in mass%, Ca: 0.007% or less, REM: 0.010% or less; Mg: 0.070% or less The steel sheet according to claim 1 or 2, comprising one or more selected from the following:

4. A steel material having the composition according to any one of claims 1 to 3 is hot-rolled at a cumulative rolling reduction rate of 15 to 75% at 870°C or less and a final rolling end temperature of 830 to 700°C at the surface temperature of the steel plate to obtain a steel plate. The steel plate is then quenched at a temperature at a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness direction, with an average cooling rate of 3°C / s or more in a temperature range of 600°C to 300°C or more and a cooling end temperature of 300°C or less, and then cooled to 550°C or more. 1 The method for producing a steel plate, comprising tempering the steel plate to a temperature range below the tempering point, and the amount of retained austenite at a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness direction is less than 1.7%.

Citation Information

Patent Citations

  • Nickel saving type 7Ni steel for ultralow temperature environment and heat treatment technology of nickel saving type 7Ni steel

    CN107937824A

  • Thick steel plate for ultra-low temperature and method for producing the same

    JP2011219848A

  • JPP7396507B

  • Nickel-containing steel sheet

    WO2020136829A1