Dispersion

A dispersion of tetrafluoroethylene polymer, inorganic filler, and compound P with a balanced liquid medium stabilizes the mixture, addressing foaming and dispersibility issues, resulting in molded articles with enhanced surface smoothness and properties.

JP7559773B2Active Publication Date: 2024-10-02AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021567381
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-12-18
Publication Date
2024-10-02
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing dispersions of tetrafluoroethylene polymers with inorganic fillers face challenges in achieving sufficient properties and stability, particularly when compounded with additional components, leading to foaming and decreased dispersibility, which hinders the formation of molded articles with excellent surface smoothness.

Method used

A dispersion containing a tetrafluoroethylene polymer, an inorganic filler, a polymer with ester, imide, or amide bonds, and a specific liquid medium, balanced with a second liquid compound, enhances stability and dispersibility, allowing for the formation of molded products with improved surface smoothness and reduced foaming.

Benefits of technology

The dispersion achieves high state stability and enables the production of molded articles with excellent surface smoothness and physical properties, maintaining the integrity of the tetrafluoroethylene polymer, inorganic filler, and compound P components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559773000001
    Figure 0007559773000001
  • Figure 0007559773000002
    Figure 0007559773000002
  • Figure 0007559773000003
    Figure 0007559773000003
Patent Text Reader

Abstract

Provided is a dispersion liquid comprising a tetrafluoroethylene-based polymer, an inorganic filler, and a compound made from a polymer that has a ester bond, an imide bond or an amide bond or made from a precursor of said polymer, wherein said dispersion liquid has excellent state stability, and can form a molded object having, to a high degree, the physical properties of each component therein. The dispersion liquid according to the present invention comprises: a tetrafluoroethylene-based polymer; an inorganic filler; a compound P made from a polymer that has an ester bond, an imide bond, or an amide bond, or made from a precursor of said polymer; a liquid amide; and at least one liquid compound selected from the group consisting of ketones, esters, and aromatic hydrocarbons.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dispersion liquid containing a tetrafluoroethylene-based polymer powder, an inorganic filler, a compound P consisting of a polymer having an ester bond, an imide bond or an amide bond or a precursor of such a polymer, and a specified liquid dispersion medium, a method for producing the same, and a method for producing a laminate having a polymer layer formed from the dispersion liquid. [Background technology]

[0002] Tetrafluoroethylene-based polymers such as polytetrafluoroethylene (PTFE), copolymers of tetrafluoroethylene and perfluoro(alkyl vinyl ether) (PFA), and copolymers of tetrafluoroethylene and hexafluoropropylene (FEP) have excellent physical properties such as mold releasability, electrical properties, water and oil repellency, chemical resistance, weather resistance, and heat resistance, and are used for various industrial applications. As a coating agent for imparting these physical properties to the surface of a substrate, a dispersion containing a powder of a tetrafluoroethylene-based polymer is known. Patent Document 1 describes a non-aqueous dispersion in which, in addition to PTFE powder, an inorganic filler made of at least one ceramic (inorganic compound) selected from the group consisting of Al2O3, SiO2, CaCO3, ZrO2, SiC, Si3N4, and ZnO is blended in order to improve the state stability (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-194017 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the dispersion of a tetrafluoroethylene-based polymer contains an inorganic filler, there is a problem that it is difficult to obtain a molded product having sufficient properties. This problem is remarkable when the dispersion is further blended with other components (such as the various components described in paragraph 0019 of Patent Document 1). According to the study by the present inventors, when a polymer having an ester bond, an imide bond or an amide bond or a compound P consisting of a precursor of such a polymer is blended as another component, the state stability of the dispersion is significantly reduced. Specifically, due to foaming of the dispersion and reduced dispersibility, a molded product having excellent surface smoothness cannot be obtained.

[0005] As a result of intensive research, the present inventors have found that a dispersion containing a tetrafluoroethylene-based polymer, an inorganic filler, the compound P, a liquid amide, and a specific liquid compound has excellent state stability, is less likely to foam, and can form a molded product with excellent surface smoothness. They also found that such a molded product has the physical properties of each component to a high degree. It is an object of the present invention to provide such a dispersion and a method for its preparation, as well as a method for preparing a laminate having a polymer layer formed from such a dispersion. [Means for solving the problem]

[0006] The present invention has the following aspects. [1] A dispersion comprising a powder of a tetrafluoroethylene-based polymer, an inorganic filler, a compound P consisting of a polymer having an ester bond, an imide bond or an amide bond or a precursor of such a polymer, and at least one liquid compound selected from the group consisting of a liquid amide, a ketone, an ester and an aromatic hydrocarbon. [2] The dispersion of [1], wherein the content of the liquid amide is greater than the content of the liquid compound. [3] The dispersion of [1] or [2], wherein the content of the tetrafluoroethylene-based polymer is 5% by mass or more. [4] The dispersion liquid according to any one of [1] to [3], wherein the ratio by mass of the content of the inorganic filler to the content of the tetrafluoroethylene-based polymer is 0.5 to 2.0. [5] The dispersion according to any one of [1] to [4], wherein the ratio by mass of the content of the compound P to the content of the tetrafluoroethylene-based polymer is 0.4 or less.

[0007] [6] The dispersion liquid according to any one of [1] to [5], wherein the inorganic filler is an inorganic filler containing silica. [7] The dispersion liquid according to any one of [1] to [6], wherein the inorganic filler is a hollow inorganic filler. [8] The dispersion liquid according to any one of [1] to [7], wherein the inorganic filler has an average particle size of 1 μm or less. [9] The dispersion liquid according to any one of [1] to [8], wherein the liquid amide is N-methyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylacetamide or dimethylformamide, and the liquid compound is cyclohexanone, cyclopentanone, γ-butyrolactone or toluene.

[10] The dispersion liquid according to any one of [1] to [9], wherein the tetrafluoroethylene-based polymer is a tetrafluoroethylene-based polymer containing a unit based on perfluoro(alkyl vinyl ether) or a unit based on hexafluoropropene, or a polytetrafluoroethylene having a number average molecular weight of 200,000 or less.

[0008]

[11] The dispersion liquid according to any one of [1] to

[10] , wherein the compound P is an aromatic polyester, an aromatic polyimide, an aromatic polyamic acid or a maleimide compound.

[12] The dispersion liquid according to any one of [1] to

[11] , wherein the compound P is a liquid crystalline aromatic polyester, a thermoplastic aromatic polyimide or a thermosetting maleimide compound.

[13] A dispersion liquid according to any one of [1] to

[12] , further comprising a surfactant.

[14] A method for producing the dispersion according to any one of [1] to

[13] , comprising mixing a liquid composition containing the compound P, the inorganic filler, the liquid amide, and the liquid compound with a liquid composition containing a powder of the tetrafluoroethylene-based polymer and the liquid amide to obtain the dispersion.

[15] A method for producing a laminate, comprising applying the dispersion liquid according to any one of [1] to

[13] to a surface of a substrate, heating the substrate, and forming a polymer layer containing the tetrafluoroethylene-based polymer to obtain a laminate having a substrate layer constituted by the substrate and the polymer layer. Effect of the Invention

[0009] According to the present invention, a dispersion liquid containing a tetrafluoroethylene-based polymer powder, an inorganic filler, and the compound P and having excellent state stability can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The following terms have the following meanings. "Average particle size (D50)" is the cumulative 50% volumetric diameter of a target object (powder or filler) determined by laser diffraction / scattering. In other words, the particle size distribution of the target object is measured by laser diffraction / scattering, the total volume of the target particle group is set as 100%, and a cumulative curve is calculated. The average particle size (D50) is the particle size at the point on the cumulative curve where the cumulative volume is 50%. "D90" is the volume-based cumulative 90% diameter of an object, measured in a similar manner. The "specific surface area" is a value determined by analyzing the inorganic filler by gas adsorption method (BET method). The term "melting temperature (melting point)" refers to the temperature corresponding to the maximum value of the melting peak of a polymer as measured by differential scanning calorimetry (DSC). The "glass transition point" is a value measured by analyzing a polymer using a dynamic mechanical analysis (DMA) method. A "unit" in a polymer is an atomic group formed directly from one monomer molecule by a polymerization reaction, and may be an atomic group in which a part of the structure is transformed by treating the polymer obtained by the polymerization reaction in a specific manner. A unit based on monomer A contained in a polymer is also referred to simply as a "monomer A unit."

[0011] The dispersion of the present invention (hereinafter also referred to as "the present dispersion") contains a powder (hereinafter also referred to as "F powder") of a tetrafluoroethylene polymer (hereinafter also referred to as "F polymer"), an inorganic filler, a compound P consisting of a polymer having an ester bond, an imide bond or an amide bond or a precursor of such a polymer, a liquid amide, and at least one liquid compound selected from the group consisting of ketones, esters and aromatic hydrocarbons. Hereinafter, the liquid compound selected from the group consisting of ketones, esters and aromatic hydrocarbons will also be referred to as "liquid compound Q". It should be noted that the F polymer and the compound P are different compounds, and the compound P is a different compound from both the liquid amide and the liquid compound Q. This dispersion is a dispersion in which F powder and inorganic filler are dispersed in a liquid dispersion medium containing a liquid amide and liquid compound Q, and compound P is highly dissolved. This dispersion has excellent state stability. From this dispersion, it is easy to form a molded product that has high physical properties of each of the F polymer, inorganic filler, and compound P (hereinafter, also referred to as "three components"). The reason for this is not necessarily clear, but it is thought to be as follows.

[0012] The liquid amide has high wettability with all three components and functions as a good dispersion medium or solvent for the three components in the dispersion. Due to this function, in a dispersion containing the liquid amide, the liquid amide is highly wetted with the F polymer, which has low surface tension, and it is considered that the apparent concentration of the other two components, especially compound P, is increased. As a result, it is considered that the interaction of compound P is excessively promoted, which induces high viscosity of the dispersion and aggregation and precipitation of the three components, and thus reduces the state stability of the entire dispersion. In addition to the liquid amide, this dispersion further contains a liquid compound Q. This liquid compound Q has a solubility for compound P comparable to that of the liquid amide, but has a lower wettability for inorganic fillers and F polymers, especially F polymers, than the liquid amide. Therefore, if the dispersion further contains liquid compound Q, it is considered that it selectively functions as a solvent for compound P and stabilizes the state.

[0013] In other words, the present dispersion liquid is considered to have excellent homogeneity and state stability such as foaming, because the dispersion liquid contains two liquid dispersion media and the dispersibility or solubility of the three components is balanced. As a result, the present dispersion liquid is considered to easily form a molded product having excellent surface smoothness and high physical properties of the three components.

[0014] The F powder in the present dispersion contains an F polymer. The content of the F polymer in the F powder is preferably 80% by mass or more, more preferably 100% by mass. Other components that may be included in the F powder include polymers different from the F polymer and inorganic substances. Polymers different from the F polymer include aromatic polyesters, polyamideimides, thermoplastic polyimides, polyphenylene ethers, and polyphenylene oxides. Inorganic substances include silicon oxide (silica), metal oxides (beryllium oxide, cerium oxide, alumina, soda alumina, magnesium oxide, zinc oxide, titanium oxide, etc.), boron nitride, and magnesium metasilicate (steatite). The F powder containing the other components preferably has a core-shell structure with an F polymer as the core and the other components as the shell, or has a core-shell structure with an F polymer as the shell and the other components as the core. Such F powder is obtained, for example, by coalescence (collision, aggregation, etc.) of an F polymer powder and a powder of the other components.

[0015] The D50 of the F powder is preferably 10 μm or less, more preferably 6 μm or less, and even more preferably 4 μm or less. The D50 of the F powder is preferably 0.01 μm or more, more preferably 0.1 μm or more, and even more preferably 1 μm or more. The D90 of the F powder is more preferably 10 μm or less. The content of the F polymer in the present dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 25% by mass or more. The content of the F polymer is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. Due to the above-mentioned mechanism of action, the present dispersion is likely to have excellent state stability even when the content of the F polymer is high.

[0016] The F polymer in this dispersion is a polymer containing units based on tetrafluoroethylene (TFE) (TFE units). As the F polymer, polytetrafluoroethylene having a number average molecular weight of 200,000 or less (hereinafter also referred to as "low molecular weight PTFE") and a polymer containing a unit based on perfluoro(alkyl vinyl ether) (PAVE) (PAVE unit) or a unit based on hexafluoropropene (HFP) (HFP unit) are preferred. The latter F polymer may contain both PAVE units and HFP units.

[0017] The number average molecular weight of the low molecular weight PTFE is preferably 100,000 or less, more preferably 50,000 or less. The number average molecular weight of the PTFE is preferably 10,000 or more. The number average molecular weight is a value calculated based on the following formula (1). Mn = 2.1 × 10 10 ×ΔHc -5.16 ... (1) In formula (1), Mn represents the number average molecular weight of the low-molecular-weight PTFE, and ΔHc represents the heat of crystallization (cal / g) of the low-molecular-weight PTFE measured by differential scanning calorimetry. Preferably, PAVE is CF2=CFOCF3, CF2=CFOCF2CF3 or CF2=CFOCF2CF2CF3 (PPVE), more preferably PPVE.

[0018] The melting temperature (melting point) of the F polymer is preferably 200°C or higher, more preferably 260°C or higher, further preferably 280 to 325°C, particularly preferably 285 to 320°C. The glass transition point of the F polymer is preferably from 75 to 125°C, more preferably from 80 to 100°C. The F polymer preferably has a polar functional group. The polar functional group may be contained in a unit in the F polymer, or may be contained in a terminal group of the main chain of the polymer. Examples of the latter embodiment include an F polymer having a polar functional group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and an F polymer having a polar functional group obtained by subjecting an F polymer to plasma treatment or ionizing radiation treatment.

[0019] The polar functional group is preferably a hydroxyl group-containing group or a carbonyl group-containing group, and from the viewpoint of enhancing the state stability of the present dispersion, a carbonyl group-containing group is more preferable. The hydroxyl-containing group is preferably a group containing an alcoholic hydroxyl group, and is preferably -CF2CH2OH or -C(CF3)2OH. The carbonyl group-containing group is a group containing a carbonyl group (>C(O)), and is preferably a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH2), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)-, etc.) or a carbonate group (-OC(O)O-). The number of carbonyl-containing groups in the F polymer is 1 × 10 6 The number of carbonyl-containing groups per unit is preferably 10 to 5000, more preferably 100 to 3000, and further preferably 50 to 1500. The number of carbonyl-containing groups in the F polymer can be quantified by the composition of the polymer or the method described in WO2020 / 145133.

[0020] As the F polymer, a polymer containing TFE units and PAVE units, containing 1.5 to 5.0 mol % of PAVE units based on all units, and having a melting temperature of 285 to 320°C is preferred, and a polymer (1) having a polar functional group, containing TFE units, PAVE units, and units based on a monomer having a polar functional group, and a polymer (2) not having a polar functional group, containing TFE units and PAVE units and containing 2.0 to 5.0 mol % of PAVE units based on all units, are more preferred. These F polymers not only have excellent powder state stability, but also tend to be more densely and uniformly distributed in the molded product formed from the dispersion. Furthermore, they tend to form microspherulites in the molded product, which tends to increase the adhesion with other components. As a result, molded products that have high physical properties of the three components are more likely to be obtained.

[0021] The polymer (1) preferably contains, based on all units, 90 to 98 mol % of TFE units, 1.5 to 9.97 mol % of PAVE units, and 0.01 to 3 mol % of units based on a monomer having a polar functional group. Moreover, as the monomer having a polar functional group, itaconic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride (also called himic anhydride; hereinafter, also referred to as "NAH") are preferable. Specific examples of polymer (1) include the polymers described in WO 2018 / 16644.

[0022] The polymer (2) is preferably composed only of TFE units and PAVE units, and contains 95.0 to 98.0 mol % of TFE units and 2.0 to 5.0 mol % of PAVE units based on the total units. The content of PAVE units in the polymer (2) is preferably 2.1 mol % or more, more preferably 2.2 mol % or more, based on all units. In addition, the polymer (2) having no polar functional group means that the number of carbon atoms constituting the polymer main chain is 1×10 6This means that the number of polar functional groups in the polymer is less than 500 per unit. The number of the polar functional groups is preferably 100 or less, more preferably less than 50. The lower limit of the number of the polar functional groups is usually 0. The polymer (2) may be produced by using a polymerization initiator or a chain transfer agent that does not generate a polar functional group as a terminal group of the polymer chain, or by fluorinating an F polymer having a polar functional group (such as an F polymer having a polar functional group derived from a polymerization initiator at the terminal group of the main chain of the polymer). As a method of fluorination treatment, a method using fluorine gas (see JP 2019-194314 A, etc.) can be mentioned.

[0023] The content of the inorganic filler in the present dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The content of the inorganic filler is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less. The ratio by mass of the inorganic filler content to the F polymer content in the dispersion is preferably 0.5 or more, more preferably 0.8 or more, and even more preferably 1.0 or more. The ratio is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 1.6 or less. Due to the above-mentioned mechanism of action, the present dispersion tends to have excellent state stability even when it contains a high concentration of inorganic filler.

[0024] As the inorganic filler, nitride fillers and inorganic oxide fillers are preferred, and boron nitride fillers, beryllia fillers (beryllium oxide fillers), silicate fillers (silica fillers, wollastonite fillers, talc fillers), and metal oxide fillers (cerium oxide, aluminum oxide, magnesium oxide, zinc oxide, titanium oxide, etc.) are more preferred. Such inorganic fillers tend to balance the interactions between the components, and tend to further improve the state stability of the dispersion. In addition, the physical properties tend to be significantly expressed in the molded product. From the viewpoint of further improving the state stability of the present dispersion, it is preferable that the inorganic filler contains silica. The silica content in the silica-containing inorganic filler is preferably 50% by mass or more, more preferably 75% by mass or more, and even more preferably 99% by mass or more. The upper limit of the silica content is 100% by mass.

[0025] At least a part of the surface of the inorganic filler is preferably surface-treated. Examples of surface treatment agents used for such surface treatment include polyhydric alcohols (trimethylolethane, pentaerythritol, propylene glycol, etc.), saturated fatty acids (stearic acid, lauric acid, etc.), esters thereof, alkanolamines, amines (trimethylamine, triethylamine, etc.), paraffin wax, silane coupling agents, silicones, and polysiloxanes. The silane coupling agent is preferably 3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane or 3-isocyanatopropyltriethoxysilane.

[0026] The average particle size of the inorganic filler is preferably 20 μm or less, more preferably 1 μm or less, even more preferably 0.8 μm or less, and particularly preferably 0.6 μm or less. The average particle size is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more. Even if the present dispersion contains an inorganic filler that has a large specific surface area and is easily wetted, the above-mentioned mechanism of action makes it easy to achieve excellent state stability. In addition, when the inorganic filler is a hollow inorganic filler, the average particle size described below is preferable. Specific examples of such inorganic fillers include silica fillers (such as the "Admafine" series manufactured by Admatechs Co., Ltd.), zinc oxide surface-treated with an ester such as propylene glycol dicaprylate (such as the "FINEX" series manufactured by Sakai Chemical Industry Co., Ltd.), spherical fused silica (such as the "SFP" series manufactured by Denka Company, Ltd.), coated with polyhydric alcohol and inorganic substances (such as the "Tipaque" series manufactured by Ishihara Sangyo Kaisha, Ltd.), rutile-type titanium oxide surface-treated with alkylsilane (such as the "JMT" series manufactured by Teika Corporation), talc fillers (such as the "SG" series manufactured by Nippon Talc Co., Ltd.), steatite fillers (such as the "BST" series manufactured by Nippon Talc Co., Ltd.), and boron nitride fillers (such as the "UHP" series manufactured by Showa Denko KK, and the "Denka Boron Nitride" series ("GP" and "HGP" grades) manufactured by Denka Company, Ltd.).

[0027] The shape of the inorganic filler may be any of granular, needle-like (fibrous) and plate-like. Specific shapes of the inorganic filler include spherical, scale-like, layered, leaf-like, apricot kernel-like, columnar, cockscomb-like, equiaxial, leaf-like, micaceous, block-like, flat, wedge-like, rosette-like, net-like and prismatic shapes. The inorganic filler is preferably hollow in shape. Even when the present dispersion contains such an inorganic filler, which has a large specific surface area and can be said to be easily wetted, the dispersion tends to have excellent state stability due to the above-mentioned mechanism of action.

[0028] The average particle size of the hollow inorganic filler is preferably 0.01 μm or more, more preferably 0.1 μm or more. The average particle size is preferably 100 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. In such a case, in a molded product molded from the present dispersion, the inorganic filler particles are likely to be filled in contact with each other, and the molded product is likely to have excellent electrical insulation properties. The specific surface area of ​​inorganic fillers (BET method) is 10 to 250 m 2 / g is preferable, and 40 to 100m 2 / g is more preferred. Due to the above-mentioned mechanism of action, the present dispersion tends to have excellent state stability even when it contains an inorganic filler having a large average particle size and a large specific surface area.

[0029] The average pore size of the hollow inorganic filler is preferably 10 to 1000 nm, more preferably 50 to 100 nm. The average pore size is determined by directly observing a plurality of pores (100 pores) using a scanning electron microscope (SEM) or the like, and the average value is taken as the average pore size. In the case of irregular pores, the maximum diameter of the pores is taken as the pore size. The apparent specific gravity of the hollow inorganic filler is preferably 100 g / L or less, more preferably 30 to 60 g / L, from the viewpoint of sufficiently increasing the porosity. The apparent specific gravity of the hollow inorganic filler is determined from the mass and volume of the inorganic filler placed in a measuring cylinder (capacity 250 mL). The bulk density of the hollow inorganic filler is 5 g / cm 3 Less than 1g / cm is preferable. 3 The lower limit of the bulk density is preferably 0.1 or more. As the hollow inorganic filler, hollow silica filler is preferable. Specific examples of hollow silica filler include hydrophobic AEROSIL series "RX200" (manufactured by Nippon Aerosil Co., Ltd.), E-SPHERES series (manufactured by Taiheiyo Cement Corporation), Silinax series (manufactured by Nippon Steel Mining Co., Ltd.), and Ecocosfire series (manufactured by Emerson & Cumming Co., Ltd.).

[0030] The compound P in the present dispersion is a polymer having an ester bond, an imide bond or an amide bond, or a precursor of such a polymer. A precursor of a polymer refers to an oligomer or a non-polymeric compound that becomes a polymer by polymerization, crosslinking, or the like. The compound P is preferably a compound P having an imide bond or an amide bond, more preferably a polymer having a unit containing an imide bond, a polymer having a unit containing an amide bond, and a precursor having an N-substituted maleimide structure, a succinimide structure, or a phthalimide structure.Furthermore, polyimide, polyamideimide, polyamic acid, and a compound having an N-substituted maleimide structure (maleimide compound) are preferred, and polyimide and maleimide compounds are particularly preferred. The polymeric compound P is a polymer different from the polymer F. When the compound P is a polymer precursor, the dispersion preferably contains a polymerization initiator for polymerizing the polymer precursor and a curing agent for curing the polymer precursor together with the polymer precursor.

[0031] The compound P is preferably aromatic. When the aromatic compound P is used to form a molded product, the aromatic rings having high planarity tend to be stacked together, and therefore the mechanical strength and heat resistance of the molded product tend to be improved. In addition, the aromatic compound has an absorbency for ultraviolet rays having a wavelength of 355 nm, which is common in UV lasers, and therefore the UV processability of the molded product obtained tends to be improved. The polyimide is preferably an aromatic polyimide, more preferably a thermoplastic aromatic polyimide. If the compound P is a thermoplastic aromatic polyimide, the plasticity of the aromatic polyimide improves the uniformity of the aromatic polyimide in the molded product formed from the dispersion, and a dense molded product is easily formed. As a result, the physical properties of the aromatic polyimide are easily expressed in the molded product, and the molded product is also easily excellent in adhesion.

[0032] As the aromatic polyimide, a semi-aromatic polyimide in which one of the tetracarboxylic dianhydride and the diamine has an aromatic ring, or a fully aromatic polyimide in which both of them have aromatic rings, is more preferable. Specific examples of aromatic polyimides include the "Neoprim" series (manufactured by Mitsubishi Gas Chemical Company, Inc.), the "Spiceria" series (manufactured by Somar), the "Q-PILON" series (manufactured by PI Technical Research Institute, Inc.), the "WINGO" series (manufactured by Wingo Technology Co., Ltd.), the "Tomide" series (manufactured by T&K TOKA Corporation), and the "KPI-MX" series (manufactured by Kawamura Sangyo Co., Ltd.).

[0033] If compound P is a maleimide compound, the maleimide compound is likely to be distributed uniformly and densely in a molded product formed from the dispersion, the physical properties of the maleimide compound are likely to be highly expressed, and the electrical properties, flame retardancy, and adhesion of the molded product are likely to be further improved. In this case, it is preferable that the dispersion further contains a component that further promotes the reaction of the maleimide compound (such as a radical polymerization initiator, an imidazole-based curing agent, a cationic curing agent, or another copolymerizable crosslinking monomer). The maleimide compound is preferably a bismaleimide compound. The bismaleimide compound may have an N-substituted maleimide structure only at the terminal group, or may have an N-substituted maleimide structure at both the terminal group and the side chain.

[0034] Examples of the maleimide compound include 4,4'-diphenylmethane bismaleimide, phenylmethane maleimide, m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, and 1,6'-bismaleimide-(2,2,4-trimethyl)hexane. The maleimide compound may be a bismaleimide compound obtained by reacting a polyimide having an amino group as a terminal group with maleic anhydride, which is a reaction product of a diamine such as a dimer diamine or a diamine having an alicyclic structure with a tetracarboxylic dianhydride having an aromatic ring. These maleimide compounds are commercially available as the BMI series manufactured by DESIGNER MOLECULES Inc.

[0035] The compound P having an ester bond is preferably an aromatic polyester, more preferably a liquid crystalline aromatic polyester (liquid crystal polyester). The aromatic polyester also includes aromatic polyesteramides having an amide bond introduced therein, and aromatic polyesters having isocyanate-derived bonds such as imide bonds, carbonate bonds, carbodiimide bonds, and isocyanurate bonds introduced therein. Specific examples of liquid crystal polyesters include polymers of dicarboxylic acids (terephthalic acid, isophthalic acid, diphenyl ether-4,4'-dicarboxylic acid, acetic anhydride, etc.), dihydroxy compounds (4,4'-biphenol, etc.), aromatic hydroxycarboxylic acids (4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 2-hydroxy-6-naphthoic acid, etc.), aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, etc., reaction products of 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, reaction products of 6-hydroxy-2-naphthoic acid, terephthalic acid, and acetaminophen, reaction products of 4-hydroxybenzoic acid, terephthalic acid, and 4,4'-biphenol, and reaction products of 2-hydroxy-6-naphthoic acid, 4,4'-dihydroxybiphenyl, terephthalic acid, and 2,6-naphthalenedicarboxylic acid. The liquid crystal polyester may be either a solvent-soluble type or a solvent-insoluble type. The melting point of the liquid crystal polyester is preferably 280 to 340°C.

[0036] The content of compound P in the present dispersion is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and preferably 5% by mass or less, more preferably 1% by mass or less. The ratio by mass of the content of the compound P to the content of the F polymer in the present dispersion (mass ratio) is preferably 0.001 or more, more preferably 0.01 or more. The above ratio is preferably 0.4 or less, more preferably 0.2 or less. Even when the compound P is contained at such a ratio, the present dispersion has excellent state stability due to the above-mentioned mechanism of action.

[0037] The liquid amide in the present dispersion is a liquid compound that functions as a dispersion medium or solvent for the three components and is inactive at 25° C. The liquid amide is preferably an amide that is compatible with liquid compound Q. The liquid amides may be used in combination of two or more kinds. The boiling point of the liquid amide is preferably 125 to 250° C. In this case, when a molded product is formed from the dispersion, the molded product tends to have excellent homogeneity. As the liquid amide, from the viewpoint of wettability with the three components, N-methyl-2-pyrrolidone (NMP), 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylacetamide and dimethylformamide are preferred, and NMP is more preferred. The liquid amide content in the present dispersion is preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less.

[0038] The liquid compound Q in the present dispersion is a liquid compound selected from the group consisting of ketones, esters, and aromatic hydrocarbons, and is a liquid compound that is inactive at 25° C. The liquid compound Q is preferably a compound that is compatible with the liquid amide. Two or more types of liquid compound Q may be used in combination. From the viewpoint of enhancing the state stability of the present dispersion, the liquid compound Q is preferably 4-methyl-2-pentanone, cyclohexanone, tetrahydrofuran, toluene, xylene, γ-butyrolactone, cyclopentanone, butyl acetate, and methyl isopropyl ketone, and more preferably cyclohexanone, cyclopentanone, γ-butyrolactone, and toluene. When the compound P is a polyimide, the liquid compound Q is more preferably cyclohexanone, cyclopentanone, and γ-butyrolactone, and when the compound P is a maleimide compound, the liquid compound Q is more preferably toluene.

[0039] The content of the liquid compound Q in the present dispersion is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. The content of the liquid compound Q is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less. The content of the liquid amide in the present dispersion is preferably greater than the content of the liquid compound Q. In this case, the above-mentioned mechanism of action makes it easier to balance the affinity between the three components (particularly between the inorganic filler and the compound P) without decreasing the dispersibility of the three components (particularly the F polymer) themselves, thereby further improving the state stability of the present dispersion. The ratio by mass of the content of the liquid compound Q to the content of the liquid amide (mass ratio) is preferably 0.8 or less, more preferably 0.5 or less. The ratio is preferably 0.1 or more, more preferably 0.2 or more. If the ratio of the two is within this range, the above-mentioned mechanism of action makes it easier to balance the affinity between the three components (particularly, between the inorganic filler and the compound P) without reducing the dispersibility of the three components (particularly, the F polymer) themselves, and to further improve the state stability of the dispersion.

[0040] From the viewpoint of improving state stability and handleability, the present dispersion preferably further contains a surfactant. The surfactant is preferably nonionic. The hydrophilic site of the surfactant preferably has an oxyalkylene group or an alcoholic hydroxyl group. The oxyalkylene group may be composed of one type or two or more types. In the latter case, the different types of oxyalkylene groups may be arranged randomly or in a block form. The oxyalkylene group is preferably an oxyethylene group. The hydrophobic portion of the surfactant preferably has an acetylene group, a polysiloxane group, a perfluoroalkyl group, or a perfluoroalkenyl group. In other words, the surfactant is preferably an acetylene-based surfactant, a silicone-based surfactant, or a fluorine-based surfactant, and more preferably a silicone-based surfactant.

[0041] As the fluorosurfactant, a fluorosurfactant having a hydroxyl group (particularly an alcoholic hydroxyl group) or an oxyalkylene group and a perfluoroalkyl group or a perfluoroalkenyl group is preferred. Specific examples of surfactants include the "Ftergent" series (manufactured by Neos), the "Surflon" series (manufactured by AGC Seimi Chemical Co., Ltd.), the "Megafac" series (manufactured by DIC Corporation), the "Unidyne" series (manufactured by Daikin Industries, Ltd.), "BYK-347", "BYK-349", "BYK-378", "BYK-3450", "BYK-3451", "BYK-3455", "BYK-3456" (manufactured by BYK Japan KK), and "KF-6011" and "KF-6043" (manufactured by Shin-Etsu Chemical Co., Ltd.). The content of the surfactant in the present dispersion is preferably 1 to 15% by mass, in which case the affinity between the components is enhanced, and the state stability of the present dispersion is more likely to be improved.

[0042] The viscosity of the present dispersion is preferably 50 mPa·s or more, more preferably 100 mPa·s or more. The viscosity of the present dispersion is preferably 10,000 mPa·s or less, more preferably 1,000 mPa·s or less, and even more preferably 800 mPa·s or less. The thixotropy ratio of the present dispersion is preferably 1.0 or more, more preferably 3.0 or less, and even more preferably 2.0 or less. The present dispersion can be easily adjusted to have a viscosity or thixotropy within the above range, and has excellent handleability.

[0043] The dispersion may further contain a resin (polymer) different from the F polymer and the compound P. The other resin may be a thermosetting resin or a thermoplastic resin. Other resins include epoxy resins, urethane resins, elastomers, polyphenylene ethers, polyphenylene oxides, and fluoropolymers other than F polymers. In addition to the above-mentioned components, the present dispersion may contain additives such as a thixotropic agent, an antifoaming agent, a silane coupling agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a brightening agent, a colorant, a conductive agent, a release agent, a surface treatment agent, a viscosity adjusting agent, and a flame retardant.

[0044] This dispersion is preferably produced by a method (hereinafter also referred to as "Method 1") in which compound P dissolved in liquid compound Q, liquid amide, and inorganic filler are mixed to prepare a liquid composition (hereinafter also referred to as "liquid composition N"), and liquid composition N is mixed with a liquid composition containing F powder and liquid amide (hereinafter also referred to as "liquid composition F"). In the preparation of liquid composition N, liquid compound Q may be further mixed separately to adjust the state stability. The content of the compound P in the liquid composition N is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and is preferably 10% by mass or less. The content of the inorganic filler in the liquid composition N is preferably 5% by mass or more, more preferably 10% by mass or more, and is preferably 50% by mass or less.

[0045] The content of the liquid amide in the liquid composition N is preferably 50% by mass or more, more preferably 60% by mass or more, and is preferably 90% by mass or less. The content of the liquid compound Q in the liquid composition N is preferably 1% by mass or more, more preferably 5% by mass or more, and is preferably 40% by mass or less. It is preferable that Liquid Composition N further contains a dispersant. The embodiment of the dispersant in Liquid Composition N, including the preferred embodiment, is the same as the embodiment of the dispersant in the present dispersion. The liquid composition N may further contain a resin (polymer) different from the F polymer and the compound P, and other components other than the inorganic filler.

[0046] The content of the F polymer in the liquid composition F is preferably 5% by mass or more, more preferably 10% by mass or more, and is preferably 60% by mass or less. The content of the liquid amide in the liquid composition F is preferably 50% by mass or more, more preferably 60% by mass or more, and more preferably 90% by mass or less. It is preferable that Liquid Composition F further contains a dispersant. The embodiment of the dispersant in Liquid Composition F, including the preferred embodiment, is the same as the embodiment of the dispersant in the present dispersion. The liquid composition F may further contain a resin (polymer) different from the F polymer and the compound P, and other components.

[0047] This dispersion can be used to form molded articles that have high physical properties of the three components. A laminate having a substrate layer made of the above substrate and the above polymer layer can be obtained by applying this dispersion onto the surface of a substrate and heating to form a polymer layer containing the F polymer. This polymer layer is a layer containing the F polymer, an inorganic filler, and the compound P or a reaction product thereof, and each component is uniformly and densely distributed in the layer. Examples of the substrate include metal substrates (metal foils of copper, nickel, aluminum, titanium, alloys thereof, etc.), resin films (films of polyimide, polyarylate, polysulfone, polyarylsulfone, polyamide, polyetheramide, polyphenylene sulfide, polyaryletherketone, polyamideimide, liquid crystalline polyester, liquid crystalline polyesteramide, etc.), and prepregs (precursors of fiber-reinforced resin substrates).

[0048] The dispersion can be applied by spraying, roll coating, spin coating, gravure coating, microgravure coating, gravure offset, knife coating, kiss coating, bar coating, die coating, fountain-meyer bar, or slot die coating. Heating after coating is preferably performed by heating to remove the liquid dispersion medium (liquid amide, liquid compound Q) and dry the film, and by heating to melt and sinter the F polymer. The heating temperature for the former is preferably 120°C to 200°C. The heating temperature for the latter is preferably 250°C to 400°C, more preferably 300°C to 380°C. When compound P is a polymer precursor, it usually becomes a polymer by the latter heating. Heating can be carried out by a method using an oven, a method using a ventilated drying furnace, or a method using heat rays such as infrared rays.

[0049] The thickness of the polymer layer formed is preferably 0.1 to 150 μm. Specifically, if the substrate is a metal foil, the thickness of the polymer layer is preferably 1 to 30 μm. If the substrate is a resin film, the thickness of the polymer layer is preferably 1 to 150 μm, and more preferably 10 to 50 μm. The polymer layer may be formed on only one surface of the substrate, or on both surfaces of the substrate. In the former case, a laminate having a substrate layer and a polymer layer on one surface of the substrate layer is obtained, and in the latter case, a laminate having a substrate layer and a polymer layer on both surfaces of the substrate layer is obtained. The latter laminate is less likely to warp, and therefore has excellent handling properties during processing.

[0050] Specific examples of laminates include metal clad laminates having a metal foil layer and a polymer layer on at least one surface of the metal foil layer, and multilayer films having a polyimide film layer and polymer layers on both surfaces of the polyimide film layer. These laminates have high physical properties of the three components, and are particularly excellent in electrical properties, and are therefore suitable as print substrate materials, etc. Specifically, such laminates can be used in the production of flexible print substrates and rigid print substrates. EXAMPLES

[0051] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. 1. Preparation of each ingredient [F Polymer / F Powder] Powder 1: Contains 97.9 mol% TFE units, 0.1 mol% NAH units, and 2.0 mol% PPVE units, in that order, and has a carbonyl group with a main chain carbon number of 1 × 10 6 Powder (D50: 2.1 μm) made of polymer (melting temperature: 300°C, F polymer 1) with 1000 particles per particle Powder 2: Contains 98.7 mol% TFE units and 1.3 mol% PPVE units, in that order, and has a carbonyl group with a main chain carbon number of 1×10 6 Powder (D50: 1.8 μm) made of polymer 2 (melting temperature: 305 °C, F polymer 2) with 40 particles per particle

[0052] [Inorganic filler] Filler 1: Hollow silica filler (D50: 0.5 μm, bulk density: 0.10 g / cm 3 ) Filler 2: Crushed titanium oxide filler (D50: 2-6 μm, bulk density: 0.25-0.75 g / cm 3 ) [Compound P] PI1: Thermoplastic aromatic polyimide BM1: Bismaleimide compound ("BMI-3000" manufactured by DESIGNER MOLECULES). Note that BM1 further contains a heat-sensitive radical polymerization initiator for thermal curing.

[0053] [Liquid dispersion medium] NMP: N-methyl-2-pyrrolidone CHN: Cyclohexanone Tol: Toluene [Surfactants] Surfactant 1: CH2=C(CH3)C(O)OCH2CH2(CF2)6F and CH2=C(CH3)C(O)(OCH2CH2) 23 Copolymer with OH

[0054] 2. Dispersion liquid production example (Example 1) First, the varnish in which PI1 was dissolved in CHN and NMP were added to the pot, then the zirconia balls were added and the pot was rolled at 150 rpm for 1 hour, followed by adding the surfactant 1 and rolling the pot at 150 rpm for 1 hour, and then adding the filler 1 and rolling the pot at 150 rpm for 1 hour to prepare liquid composition N1. Powder 1, surfactant 1, and NMP were placed in a separate pot, and zirconia balls were then placed in. The pot was then rolled at 150 rpm for 1 hour to prepare Liquid Composition F1.

[0055] In addition, both liquid compositions were poured into another pot, and zirconia balls were poured in. The pot was then rolled at 150 rpm for 1 hour to obtain Dispersion 1 (viscosity: 700 mPa s) containing Powder 1 (8 parts by mass), Filler 1 (12 parts by mass), PI1 (0.1 parts by mass), Surfactant 1 (1 part by mass), NMP (49 parts by mass), and CHN (27 parts by mass). The ratio by mass of the content of liquid compound Q to the content of liquid amide in dispersion 1 was 0.6, the ratio by mass of the content of F polymer to the content of PI1 was 0.01, and the ratio by mass of the content of F polymer to the content of inorganic filler was 1.5.

[0056] (Examples 2 to 7) Dispersions 2 to 7 were obtained in the same manner as in Example 1, except that the type and amount of the liquid dispersion medium was changed as shown in Table 1 below. [Table 1]

[0057] 3. Manufacturing example of laminate (copper clad laminate) Dispersion liquid 1 was applied to the surface of a long copper foil (thickness: 18 μm) using a bar coater to form a wet film. The copper foil on which the wet film was formed was then passed through a drying oven at 120° C. for 5 minutes and dried by heating to obtain a dry film. The dry film was then heated at 380° C. for 3 minutes in an oven under a nitrogen gas atmosphere. This produced a laminate 1 having a copper foil and a polymer layer (thickness: 5 μm) containing F polymer 1, PI 1, and filler 1. Laminates 2 to 4 were produced in the same manner as laminate 1, except that dispersion 1 was changed to dispersions 2 to 7, respectively.

[0058] 4. Evaluation 4-1. Dispersion stability The state of each dispersion immediately after preparation and after storage in a container at 25° C. were visually inspected, and the state stability was evaluated according to the following criteria. [Evaluation Criteria] ◯: Little foaming immediately after preparation, and well dispersed even after storage. △: Immediately after preparation, the mixture foams but is dispersed. After storage, aggregates adhere to the wall. ×: The mixture foams immediately after preparation and quickly becomes mousse-like. After storage, a large amount of aggregates settles.

[0059] 4-2. Surface smoothness of laminate The surface smoothness of the polymer layer of each laminate was visually confirmed and evaluated according to the following criteria. [Evaluation Criteria] ◯: The entire surface of the polymer layer is smooth. △: The edges of the polymer layer are raised and the center is recessed. ×: The edges of the polymer layer are raised and the center is depressed, and irregularities due to loss of polymer or inorganic filler are also observed. The evaluation results are summarized in Table 2 below.

[0060] [Table 2]

[0061] 4-3. Electrical properties and dimensional stability of laminates For each of the laminates 1, 3, and 7, the copper foil of the laminate was removed by etching with an aqueous ferric chloride solution to produce a single polymer layer, and the dielectric constant and dielectric tangent (measurement frequency: 10 GHz) of the above polymer layer were measured using the SPDR (split post dielectric resonance) method. Furthermore, for each of the laminates 1, 3 and 7, a square test piece measuring 180 mm square was cut out, and the linear expansion coefficient of the test piece was measured in the range of 25° C. to 260° C. in accordance with the measurement method specified in JIS C 6471:1995. The results are summarized in Table 3 below.

[0062] [Table 3] [Industrial Applicability]

[0063] This dispersion has excellent state stability and can be used to produce molded products (films, impregnated products such as prepregs, laminates, etc.) that have high physical properties based on the F polymer, inorganic filler, and compound P. The molded product of the present invention is useful as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, paints, cosmetics, etc., and specifically, it is useful as electric wire covering materials (aircraft electric wires, etc.), electrical insulating tapes, insulating tapes for oil drilling, materials for printed circuit boards, separation membranes (microfiltration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode binders (for lithium secondary batteries, for fuel cells, etc.), copy rolls, furniture, automobile dashboards, covers for home appliances, etc., sliding members (load bearings, sliding shafts, valves, bearings, gears, cams, belt conveyors, food transport belts, etc.), tools (shovels, files, saws, saws, etc.), boilers, hoppers, pipes, ovens, baking molds, chutes, dies, toilets, and container covering materials. The entire contents of the specification, claims and abstract of Japanese Patent Application No. 2019-234714, filed on December 25, 2019, are hereby incorporated by reference as the disclosure of the specification of the present invention.

Claims

1. A dispersion liquid comprising a powder of a tetrafluoroethylene-based polymer, an inorganic filler, a compound P which is a thermoplastic aromatic polyimide or a thermosetting maleimide compound, a liquid amide which is N-methyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylacetamide or dimethylformamide, and at least one liquid compound selected from the group consisting of ketones, esters and aromatic hydrocarbons.

2. 2. The dispersion of claim 1, wherein the liquid amide content is greater than the liquid compound content.

3. The dispersion according to claim 1 or 2, wherein the content of the tetrafluoroethylene-based polymer is 5% by mass or more.

4. The dispersion according to any one of claims 1 to 3, wherein the ratio by mass of the content of the inorganic filler to the content of the tetrafluoroethylene-based polymer is 0.5 to 2.

0.

5. 5. The dispersion according to claim 1, wherein the ratio by mass of the content of the compound P to the content of the tetrafluoroethylene-based polymer is 0.4 or less.

6. The dispersion according to any one of claims 1 to 5, wherein the inorganic filler is an inorganic filler containing silica.

7. The dispersion according to any one of claims 1 to 6, wherein the inorganic filler is a hollow inorganic filler.

8. The dispersion according to any one of claims 1 to 7, wherein the inorganic filler has an average particle size of 1 µm or less.

9. The dispersion according to claim 1, wherein the liquid compound is cyclohexanone, cyclopentanone, γ-butyrolactone or toluene.

10. The dispersion according to any one of claims 1 to 9, wherein the tetrafluoroethylene-based polymer is a tetrafluoroethylene-based polymer containing a unit based on perfluoro(alkyl vinyl ether) or a unit based on hexafluoropropene, or a polytetrafluoroethylene having a number average molecular weight of 200,000 or less.

11. The dispersion according to any one of claims 1 to 10, further comprising a surfactant.

12. 12. The method for producing the dispersion according to claim 1, comprising mixing a liquid composition containing the compound P, the inorganic filler, the liquid amide, and the liquid compound with a liquid composition containing a powder of the tetrafluoroethylene-based polymer and the liquid amide to obtain the dispersion.

13. A method for producing a laminate, comprising: applying the dispersion according to any one of claims 1 to 11 to a surface of a substrate; heating the coating; and forming a polymer layer containing the tetrafluoroethylene-based polymer to obtain a laminate having a substrate layer constituted by the substrate and the polymer layer.

Citation Information

Patent Citations

  • Non-aqueous dispersion of polytetrafluoroethylene

    JP2016194017A

  • Non-aqueous dispersion of polytetrafluoroethylene micropowder

    JP2017066327A

  • Organosol composition of fluorine-containing polymer

    WO2012002038A1

  • Nonaqueous dispersion containing fluorine-based resin; polyimide precursor solution composition containing fluorine-based resin; polyimide, polyimide film and adhesive composition for circuit boards, each using said polyimide precursor solution composition containing fluorine-based resin; and production methods thereof

    WO2016159102A1

  • Dispersion, metal laminate plate, and production method for printed board

    WO2019131809A1