Polyolefin resin film and laminate using same
A polyolefin resin film with controlled heat shrinkage and plane orientation, using specific copolymers and additives, addresses tearing and transparency issues in packaging bags, providing easy opening and high tear resistance.
Patent Information
- Application Number
- JP2023192993
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-20
- Filing Date
- 2023-11-13
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-05-26
AI Technical Summary
Existing polyolefin resin films used in packaging bags face issues such as difficulty in tearing parallel to one side due to molecular orientation axis distortion, leading to separation and spillage of contents, especially for elderly users, and lack of transparency and tear resistance.
A polyolefin resin film composition comprising specific proportions of propylene-α olefin random copolymer, ethylene-propylene block copolymer, and optional additives like anti-blocking agents, controlled for heat shrinkage and plane orientation, ensuring easy tearing and transparency.
The film achieves excellent transparency, sealability, and tear resistance, allowing easy opening without tearing, while maintaining high puncture strength and low heat shrinkage, suitable for packaging applications.
Smart Images

Figure 0007559908000001 
Figure 0007559908000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyolefin resin film and a laminate thereof with a biaxially oriented film made of at least one polymer selected from the group consisting of a polyamide resin film, a polyester resin film, and a polypropylene resin film. [Background technology]
[0002] Packaging bags are typically produced by heat sealing the peripheral portions of a laminate of a base film, such as a polyamide resin film, polyester resin film, or polypropylene resin film, and a polyolefin resin film, with the polyolefin resin film surfaces in contact with each other at a temperature close to the melting point of the polyolefin resin film. In food packaging bags, heat-sealable films made of polyolefin resins are often used as films for packaging foods that require water vapor barrier properties, such as dried foods and confectioneries. In recent years, the demand for food packaged in films has increased due to social factors such as the advancement of women in the workplace, the trend toward nuclear families, and the aging of the population, and at the same time, there is a demand for further improvement in properties. For example, there is a demand for improvement in ease of opening so that even people with weak strength, such as the elderly, can easily remove the food inside.
[0003] In addition, when removing food contents from a packaging bag, the bag is often torn by hand from a notch, a cut made in the seal around the bag. However, when a conventional laminate is used, the bag cannot be torn parallel to one side, which is usually the horizontal direction, and the bag is opened at an angle, or the tear direction of the laminate on the front and back of the bag is reversed from top to bottom, which is called tearing. This makes it difficult to remove the food contents, and it is difficult to remove food such as furikake. There was a risk of spilling particulate contents.
[0004] The reason why it is difficult to tear a packaging bag parallel to one side of the packaging bag is that the base film used in the laminate is distorted, i.e., the molecular orientation axis direction of the base film is not parallel to one side of the package.
[0005] If the molecular orientation axis direction of the base film could be made the same as the tear direction of the packaging bag, such a problem would not occur. The molecular orientation axis direction of the produced wide-width stretched film in the width direction center coincides with the running direction of the film, and it is possible to tear it parallel to one side of the packaging bag. However, the molecular orientation axis direction is inclined at the width direction end of the film, and the tear direction of the packaging bag is inclined. It is not realistic to procure base film that completely avoids the width direction end of the film, and the degree of distortion tends to become even greater than before as the production speed of the base film increases and the width increases. Furthermore, in food packaging bags for dry foods, sweets, etc., it is preferable that the contents are easily visible.
[0006] Therefore, attempts have been made to solve these problems by improving the polyolefin resin film that is laminated to the base film.
[0007] Patent Document 1 discloses a technique for uniaxially stretching a sheet in which a polyethylene resin such as linear low-density polyethylene or high-pressure low-density polyethylene is added to a polypropylene resin. However, there is a problem with the appearance of the film.
[0008] Also, Patent Document 2 discloses a film obtained by uniaxially stretching a polyolefin resin sheet containing a propylene-ethylene block copolymer and an ethylene-propylene copolymer in a seal layer at 3.0 times its original length. However, there are problems with haze, seal strength, tear strength, and tear separation.
[0009] Furthermore, Patent Document 3 discloses a film obtained by uniaxially stretching a polyolefin resin sheet containing a propylene-ethylene block copolymer, an ethylene-propylene copolymer, and a propylene-butene copolymer. However, there was a problem with the visibility of the contents.
[0010] Also, Patent Document 4 discloses a technique in which a polyolefin resin sheet containing a propylene-ethylene copolymer and a propylene-butene copolymer in a sealing layer is uniaxially stretched by a tenter system. However, there is a problem with the resistance to bag rupture.
[0011] Also, a technique is known in Patent Document 5 in which a polyolefin resin sheet containing a propylene-ethylene copolymer is uniaxially stretched in the machine direction, but there is a problem with the pin puncture strength.
[0012] Also, a film obtained by uniaxially stretching a polyolefin resin sheet containing a propylene-ethylene-butene random copolymer and an ethylene-butene copolymer elastomer resin by 4 to 6 times is known, as disclosed in Patent Document 6. However, there is a problem in that the heat shrinkage rate is high. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2002-003619 A [Patent Document 2] Patent No. 5790497 [Patent Document 3] Patent No. 5411935 [Patent Document 4] JP 2016-32911 A [Patent Document 5] JP 2018-79583 A [Patent Document 6] JP 2014-141302 A Summary of the Invention [Problem to be solved by the invention]
[0014] The present invention aims to provide a polyolefin-based resin film which, even when laminated with a base film having a large distortion in the molecular orientation axis such as a biaxially oriented polyamide-based resin film, provides a packaging bag obtained from the laminate which has excellent transparency, pinhole resistance due to bending, and blocking resistance, and which can be easily torn without tearing apart. [Means for solving the problem]
[0015] As a result of intensive research into achieving this object, the present inventors have discovered that by controlling the longitudinal heat shrinkage rate and surface orientation relationship of a polyolefin resin film made of a polypropylene resin composition having a propylene-α-olefin random copolymer and an ethylene-propylene block copolymer in a specific ratio, it is possible to laminate the film with a base film having a large distortion in the molecular orientation axis, such as a biaxially oriented polyamide resin film, and to produce a packaging bag having excellent transparency, sealability and bag formability, and which can be easily torn without tearing, thereby completing the present invention. That is, the present invention has the following aspects.
[0016] [1] A polyolefin resin film made of a polyolefin resin composition, said polyolefin resin composition containing at least a propylene-α-olefin random copolymer, and satisfying the following 1) to 5). 1) In the polyolefin resin composition, the content of the olefin block copolymer is 0 to 2 parts by weight based on 100 parts by weight of the propylene-α-olefin random copolymer. 2) In the polyolefin resin composition, the content of the olefin copolymer elastomer resin is 0 to 2 parts by weight based on 100 parts by weight of the propylene-α-olefin random copolymer. 3) In the polyolefin resin composition, the content of the propylene homopolymer is 0 to 40 parts by weight based on 100 parts by weight of the propylene-α-olefin random copolymer. 4) A polyolefin resin film, in which the heat shrinkage rate after heating at 120°C for 30 minutes is 25% or less in the longitudinal direction or width direction of the polyolefin resin film, whichever direction has the larger heat shrinkage rate after heating at 120°C for 30 minutes. 5) The plane orientation coefficient ΔP calculated from the refractive index of the polyolefin resin film is 0.0100 or more and 0.0145 or less.
[0017] [2] The Martens hardness of at least one surface of the polyolefin resin film is 80 N / mm 2 The polyolefin resin film according to [1], which has an indentation creep rate (Cit) of 3.0% or less.
[0018] [3] The polyolefin resin film according to [1] or [2], wherein the haze of the polyolefin resin film is 1% or more and 20% or less.
[0019] [4] The polyolefin resin film according to any one of [1] to [3], wherein the polyolefin resin film has a tear strength of 1.0 N or less in the longitudinal direction or transverse direction in which the heat shrinkage rate is greater after heating at 120° C. for 30 minutes.
[0020] [5] The polyolefin resin film according to any one of [1] to [4], wherein the polyolefin resin film has a puncture strength of 0.12 N / μm or more.
[0021] [6] The polyolefin resin film according to any one of [1] to [5], wherein a concentration of an antiblocking agent in a layer located on at least one surface of the polyolefin resin film is 3000 ppm or less.
[0022] [7] A laminate of the polyolefin resin film according to any one of [1] to [6] and a biaxially oriented film made of at least one polymer selected from the group consisting of polyamide resin films, polyester resin films, and polypropylene resin films.
[0023] [8] The laminate according to [7], wherein the straight-cut ability in the longitudinal direction or width direction in which the thermal shrinkage rate is greater after heating at 120°C for 30 minutes is 8 mm or less, and the tear strength in the longitudinal direction or width direction in which the thermal shrinkage rate is greater after heating at 120°C for 30 minutes is 0.8 N or less.
[0024] [9] A packaging body comprising the laminate described in [7] or [8]. Effect of the Invention
[0025] The polyolefin resin film of the present invention is excellent in transparency, sealability and bag formability, and is suitable for providing a package which does not separate and can be easily torn. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be described in detail below. The polyolefin resin film in the present invention is a polyolefin resin film mainly composed of a propylene-α-olefin random copolymer.
[0027] (Propylene-α-olefin random copolymer) In the present invention, the propylene-α-olefin random copolymer may be a copolymer of propylene and at least one α-olefin having 2 or 4 to 20 carbon atoms other than propylene. As the α-olefin monomer having 2 or 4 to 20 carbon atoms, ethylene, butene-1, pentene-1, 4-methylpentene-1, hexene-1, octene-1, etc. can be used. Although not particularly limited, it is preferable to use ethylene in terms of stretchability and low shrinkage. In addition, at least one type may be used, and two or more types may be mixed and used as necessary. Propylene-ethylene random copolymer is particularly preferable. The melting point of the propylene-α-olefin random copolymer is preferably 125° C. or higher, more preferably 130° C. or higher. When the melting point is 125° C. or higher, straight cutting properties are easily obtained.
[0028] The lower limit of the melt flow rate (MFR) of the propylene-α-olefin random copolymer is preferably 0.6 g / 10 min, more preferably 1.0 g / 10 min, and even more preferably 1.2 g / 10 min. The uniformity of the film thickness may be impaired. The upper limit of the melt flow rate of the random copolymer is preferably 12.0 g / 10 min, more preferably 9.0 g / 10 min, and even more preferably 8.0 g / 10 min. Specific examples include propylene-ethylene random copolymers (Prime Polypro F-724NPC manufactured by Prime Polymer Co., Ltd., MFR 7.0 g / 10 min at 230° C. and a load of 2.16 kg, melting point 142° C.), propylene-ethylene-butene random copolymers (Sumitomo Noblen FL8115A manufactured by Sumitomo Chemical Co., Ltd., MFR 7.0 g / 10 min at 230° C. and a load of 2.16 kg, melting point 148° C.), propylene-ethylene-butene random copolymers (Prime Polypro F-794NV manufactured by Prime Polymer Co., Ltd., MFR 5.7 g / 10 min at 230° C. and a load of 2.16 kg, melting point 134° C.), and propylene-ethylene-butene random copolymers (Sumitomo Noblen FL6745A manufactured by Sumitomo Chemical Co., Ltd., MFR 6.0 g / 10 min at 230° C. and a load of 2.16 kg, melting point 130° C.). Particularly suitable is a propylene-ethylene-butene random copolymer in which the main monomer is propylene and a certain amount of ethylene and butene are copolymerized. In this paper, the random copolymers are named and described in order of the monomer composition ratio that constitutes them.
[0029] (Propylene-ethylene block copolymer) In the present invention, a propylene-ethylene block copolymer can be used, which makes it easier to improve the resistance to rupture of the bag. The propylene-ethylene block copolymer in the present invention is a multi-stage copolymer consisting of a first polymerization step consisting of a copolymerization component of a large amount of propylene and a small amount of ethylene, and a second polymerization step consisting of a copolymerization component of a small amount of propylene and a large amount of ethylene. Specifically, as shown in JP-A-2000-186159, it is preferable to use one that is polymerized by a gas phase method. That is, in the first step, a polymer portion (component A) mainly composed of propylene is polymerized in the substantial absence of an inert solvent, and then in the second step, a copolymer portion (component B) of propylene and ethylene having an ethylene content of 20 to 50 parts by weight is polymerized in the gas phase to obtain a block copolymer, but the block copolymer is not limited to these. The melting point of the propylene-α-olefin block copolymer is preferably 125° C. or higher, more preferably 130° C. or higher, and even more preferably 140° C. or higher. When the melting point is 125° C. or higher, straight cutting properties are easily obtained.
[0030] The melt flow rate (MFR) of the propylene-ethylene block copolymer (measured at 230° C. under a load of 2.16 kg) is not particularly limited, but is preferably 1 to 10 g / 10 min, and more preferably 2 to 7. If it is less than 1 g / 10 min, the viscosity is too high, making it difficult to extrude through a T-die, whereas if it exceeds 10 g / 10 min, problems such as stickiness of the film and poor impact strength (impact strength) of the film occur.
[0031] (copolymer elastomer) In the present invention, a thermoplastic copolymer elastomer mainly composed of polyolefin can be added, which makes it easier to improve the resistance to bag rupture. Furthermore, examples of the olefin-based elastomer include an α-olefin polymer having 2 to 20 carbon atoms or a copolymer of ethylene and an α-olefin, which preferably has a melting point of 110° C. or less, more preferably 100° C. or less, and even more preferably 80° C. or less, or which has no observable melting point. Specific examples include ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-4-methylpentene-1 copolymer, ethylene-1-octene copolymer, propylene homopolymer, propylene-ethylene copolymer, propylene-ethylene-1-butene copolymer, 1-butene homopolymer, 1-butene-ethylene copolymer, 1-butene-propylene copolymer, 4-methylpentene-1 homopolymer, 4-methylpentene-1-propylene copolymer, 4-methylpentene-1-1-butene copolymer, 4-methylpentene-1-propylene-1-butene copolymer, propylene-1-butene copolymer, and the like. Among the ethylene-butene copolymer elastomers, preferred are amorphous or low crystalline elastomers obtained by copolymerizing ethylene and butene, propylene-butene copolymer elastomers, which are crystalline elastomers obtained by copolymerizing propylene and butene as olefin-based thermoplastic copolymer elastomers exhibiting relatively high Shore hardness and good transparency, and mixtures thereof.
[0032] The melt flow rate (MFR) of the olefin-based thermoplastic copolymer elastomer at 230°C and a load of 2.16 kg is 0.2 to 5.0 g / 10 min, and the density is 820 to 930 kg / m 3 It is desirable to use one having a molecular weight distribution (Mw / Mn) of 1.3 to 6.0 as determined by the GPC method. If the melt flow rate (MFR) at a load of 2.16 kg is less than 0.2 g / 10 min, uniform kneading becomes insufficient and fish eyes are likely to occur, while if it exceeds 5.0 g / min, it is not preferable from the viewpoint of bag rupture resistance.
[0033] (Propylene homopolymer) In the present invention, a propylene homopolymer can be used, which makes it easy to reduce the tear strength and increase the transparency. The propylene homopolymer includes isotactic polypropylene, which has high crystallinity and excellent rigidity and heat resistance, and atactic polypropylene, which has low crystallinity and excellent flexibility. As the propylene homopolymer to be used, isotactic polypropylene, which has high crystallinity and suppresses deterioration of the heat shrinkage rate, is preferred. The melt flow rate (MFR) of the propylene homopolymer (measured at 230°C under a load of 2.16 kg) is not particularly limited, but is preferably 1 to 10 g / 10 min, and more preferably 2 to 7. If it is less than 1 g / 10 min, the viscosity is too high and extrusion through a T-die is difficult, whereas if it exceeds 10 g / 10 min, problems such as stickiness of the film and poor impact strength (impact strength) of the film occur.
[0034] (Additives) The polyolefin resin composition of the present invention may contain an antiblocking agent. Although one type of antiblocking agent may be used, the incorporation of two or more types of inorganic particles having different particle sizes and shapes can form complex protrusions even on the unevenness of the film surface, thereby obtaining a higher level of antiblocking effect. The antiblocking agent to be added is not particularly limited, but examples of the antiblocking agent that can be added include inorganic particles such as spherical silica, amorphous silica, zeolite, talc, mica, alumina, hydrotalcite, and aluminum borate, and organic particles such as polymethyl methacrylate and ultra-high molecular weight polyethylene. In the case of a multi-layer structure of two or more layers, the additive may be added to all layers. However, if there are irregularities on the surface of the layer on which the biaxially oriented film is laminated, this may result in poor appearance of the laminated process, so it is preferable to add the additive only to the layer on which the films are heat-sealed together. The layer on which the biaxially oriented films are laminated is called the laminating layer, and its surface is called the laminating surface. The layer on which the films are heat-sealed is called the sealing layer, and its surface is called the sealing surface. The antiblocking agent is preferably added at 3000 ppm or less, more preferably 2500 ppm or less, relative to the polyolefin resin composition of the layer to which it is added. By making it 3000 ppm or less, it is possible to reduce the falling off of the antiblocking agent. The polyolefin resin composition of the present invention may contain an organic lubricant. The lubrication and anti-blocking effect of the laminated film are improved, and the handling of the film is improved. The reason for this is believed to be that the organic lubricant bleeds out and is present on the film surface, thereby exerting the lubricant effect and release effect. It is preferable to add an organic lubricant having a melting point equal to or higher than room temperature. Examples of the organic lubricant include fatty acid amides and fatty acid esters. Specific examples include oleic acid amide, erucic acid amide, behenic acid amide, ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, ethylene bisoleic acid amide, etc. These may be used alone, but it is preferable to use two or more of them in combination, since this makes it possible to maintain the lubricity and anti-blocking effect even under harsh environments.
[0035] The polyolefin resin composition of the present invention may contain, as necessary, suitable amounts of antioxidants, antistatic agents, antifogging agents, neutralizing agents, nucleating agents, colorants, other additives, inorganic fillers, and the like in any layer within the scope of the object of the present invention. As the antioxidant, a phenolic and a phosphite may be used in combination, or a compound having both a phenolic and a phosphite skeleton in one molecule may be used alone. As the neutralizing agent, calcium stearate may be used.
[0036] (Polyolefin resin composition) In the polyolefin resin composition of the present invention, it is preferable that the propylene-ethylene block copolymer is contained in an amount of 0 to 2 parts by weight per 100 parts by weight of the propylene-α-olefin random copolymer. Furthermore, it is even more preferable that the polyolefin resin composition is contained in an amount of 0 to 1 part by weight per 100 parts by weight of the propylene-α-olefin random copolymer. When the propylene-ethylene block copolymer is 2 parts by weight or less, transparency and low-temperature heat sealability tend to be good.
[0037] The polyolefin resin composition of the present invention preferably contains 0 to 2 parts by weight of an olefin thermoplastic copolymer elastomer based on 100 parts by weight of the propylene-α-olefin random copolymer. Furthermore, the polyolefin resin composition preferably contains 0 to 1 part by weight of an olefin thermoplastic copolymer elastomer per 100 parts by weight of the propylene-α-olefin random copolymer. By making the amount 2 parts by weight or less, the heat shrinkage rate and transparency tend to be good.
[0038] In the polyolefin resin composition of the present invention, it is preferable that 0 to 40 parts by weight of propylene homopolymer is contained per 100 parts by weight of propylene-α-olefin random copolymer. Furthermore, it is preferable that 0 to 25 parts by weight of propylene homopolymer is contained per 100 parts by weight of propylene-α-olefin random copolymer. By making it 40 parts by weight or less, it is easy to obtain low-temperature heat sealability and heat seal strength at low temperatures.
[0039] (Polyolefin resin film) The polyolefin resin film of the present invention may be a single layer, or may be a multi-layer film having two or more layers. In the case of a three-layer structure, the intermediate layer may contain recycled pellets of semi-finished products or finished films produced in the manufacturing process, thereby reducing costs without impairing heat seal energy or bag breakage resistance, or the intermediate layer or laminate layer may contain a propylene-α-olefin random copolymer having a low melting point, which is added only to the seal layer, and the intermediate layer or laminate layer may contain a propylene-α-olefin random copolymer having a high melting point, which is used as the main component, thereby enhancing the effect.
[0040] (Method of manufacturing polyolefin resin film) The polyolefin resin film of the present invention can be formed by, for example, inflation method or T-die method, but the T-die method is preferred for increasing transparency and ease of drafting. The inflation method uses air as a cooling medium, whereas the T-die method uses a cooling roll, making it an advantageous manufacturing method for increasing the cooling rate. By increasing the cooling rate, crystallization of the unstretched sheet can be suppressed, making it advantageous to stretch the sheet by a roll in a later process. For these reasons, the T-die method is preferred.
[0041] The lower limit of the cooling roll temperature when the molten raw resin is cast to obtain a non-oriented sheet is preferably 15° C., more preferably 20° C. If it is less than the above, condensation may occur on the cooling roll, resulting in insufficient adhesion. The upper limit of the cooling roll is preferably 60° C., more preferably 50° C. If it exceeds the above, transparency may deteriorate.
[0042] The method for stretching the non-oriented sheet is not particularly limited, and for example, an inflation method, a tenter transverse stretching method, or a roll longitudinal stretching method can be used. The roll longitudinal stretching method is preferred because of ease of control of orientation. The term "longitudinal stretching" as used herein means the direction in which the film flows from the step of casting the raw material resin composition to the step of winding up the stretched film, and the term "transverse direction" means the direction perpendicular to the flow direction.
[0043] By stretching a non-oriented sheet, the straight cut property is developed because the molecular chain structure is regularly aligned in the stretching direction. The lower limit of the stretching ratio is preferably 3.3 times. If it is smaller than this, the yield strength decreases, the tear strength increases, and the straight cutability may be poor. It is more preferably 3.5 times, and even more preferably 3.8 times. The upper limit of the stretching ratio is preferably 5.5 times. If it is greater than this, the orientation will proceed excessively, the sealing energy will decrease, and the resistance to bag breakage after dropping may deteriorate. It is more preferably 5.0 times, and even more preferably 4.7 times.
[0044] The lower limit of the stretching roll temperature is not particularly limited, but is preferably 60° C. If it is lower than this, the stretching stress applied to the film becomes high, and the film may have a thickness variation. It is more preferably 70° C. The upper limit of the stretching roll temperature is not particularly limited, but is preferably 140° C. If it exceeds this limit, the stretching stress applied to the film will be low, and not only will the tear strength of the film decrease, but the film may also be fused to the stretching roll, making production difficult. It is more preferably 130° C., even more preferably 120° C., and particularly preferably 110° C.
[0045] It is preferable to bring the unstretched sheet into contact with a preheat roll to increase the sheet temperature before it is introduced into the stretching step. The lower limit of the preheat roll temperature when stretching a non-oriented sheet is not particularly limited, but is preferably 70°C, more preferably 80°C. If it is less than the above, the stretching stress will be high and thickness fluctuations may occur. The upper limit of the preheat roll temperature is not particularly limited, but is preferably 140°C, more preferably 130°C, and even more preferably 120°C. If it is more than the above, the heat shrinkage rate may increase. This is because thermal crystallization before stretching can be suppressed and residual stress after stretching can be reduced.
[0046] The polyolefin resin film that has been subjected to the longitudinal stretching process is preferably annealed to suppress thermal shrinkage. Annealing methods include roll heating and tentering, but the roll heating method is preferred because of the simplicity of the equipment and ease of maintenance. Annealing reduces the internal stress of the film, suppressing thermal shrinkage of the film and further improving the tearability. Therefore, the heat seal strength is less likely to be sacrificed compared to the conventional method of simply increasing the stretch ratio to increase tearability. The lower limit of the annealing temperature is not particularly limited, but is preferably 80°C. If the temperature is less than the above range, the heat shrinkage rate may be high, the tear strength may be high, and the finish of the packaging bag after bag formation may be deteriorated. The upper limit of the annealing temperature is not particularly limited, but is preferably 125°C. The higher the annealing temperature, the more likely it is that the heat shrinkage rate will decrease, but if the annealing temperature exceeds this limit, the heat seal strength may deteriorate or the film may melt to the manufacturing equipment. The upper limit is more preferably 120°C, and particularly preferably 115°C.
[0047] In the annealing step, a relaxation step can be provided by gradually slowing down the film conveying speed, for example by reducing the rotation speed of the rolls. By providing the relaxation step, the thermal shrinkage rate of the produced polyolefin resin film can be further reduced, and the heat seal strength can also be increased. The upper limit of the relaxation rate in the relaxation step is preferably 10%, more preferably 8%. If it is 10% or less, the film is less likely to sag during transportation and is less likely to wrap around the process. The lower limit of the relaxation rate is preferably 1%, more preferably 3%. If it is 1% or more, the heat shrinkage rate of the polyolefin resin film is less likely to be high.
[0048] In the present invention, it is preferable to activate the surface of the polyolefin resin film described above on the side where the biaxially oriented film of another material is to be laminated by corona treatment, etc. This improves the lamination strength with the base film.
[0049] (film thickness) The lower limit of the thickness of the polyolefin resin film of the present invention is preferably 7 μm, more preferably 10 μm, even more preferably 12 μm, and particularly preferably 15 μm. If it is 15 μm or more, it becomes relatively thicker than the thickness of the base film, so that the straight cutability as a laminate is not easily deteriorated, and the film has a firm feel and is easy to process, and impact resistance is easily obtained and bag breakage resistance is easily obtained. The upper limit of the film thickness is preferably 150 μm, more preferably 80 μm, and even more preferably 50 μm. If it is 150 μm or less, the film does not have too much firmness and is easy to process, and a suitable package is easily produced.
[0050] The characteristics of polyolefin resin films will be described. (Hayes) The lower limit of the haze of the polyolefin resin film of the present invention is preferably 1.0%, more preferably 2.0%. If it is 1.0% or more, the unevenness of the film surface is not extremely small, so blocking of the inner surface of the package is unlikely to occur. The upper limit of the haze is preferably 20.0%, more preferably 15.0%, and even more preferably 10.0%. If it is 20.0% or less, visibility of the package is easily obtained.
[0051] (Heat shrinkage rate) The upper limit of the heat shrinkage rate of the polyolefin resin film of the present invention after heating at 120°C for 30 minutes in the longitudinal direction or transverse direction in which the heat shrinkage rate is larger after heating at 120°C for 30 minutes is 25%. If it exceeds the above range, the tear strength increases and at the same time, the shrinkage during heat sealing increases, which may impair the appearance of the package. The upper limit is preferably 20%, and more preferably 17%. The lower limit of the heat shrinkage rate of the polyolefin resin film of the present invention after heating for 30 minutes at 120° C. is 2% in the longitudinal direction or the transverse direction in which the heat shrinkage rate is larger after heating for 30 minutes at 120° C. If it is attempted to make it smaller than this, the annealing temperature and the annealing time must be significantly increased, which may significantly deteriorate the appearance. The upper limit of the heat shrinkage rate of the polyolefin resin film of the present invention after heating at 120° C. for 30 minutes in the longitudinal direction or the transverse direction in which the heat shrinkage rate is smaller after heating at 120° C. for 30 minutes is 1%. If it is 1% or less, the tear strength in the transverse direction becomes large or the straight cutability is poor. It is preferably 0.5%. The lower limit of the heat shrinkage rate of the polyolefin resin film of the present invention after heating at 120° C. for 30 minutes in the longitudinal direction or the transverse direction, whichever direction has the smaller heat shrinkage rate, is −5%. The film is less likely to elongate, and the appearance of the package is less likely to deteriorate. The preferable range is -3%.
[0052] (Piercing strength) The lower limit of the puncture strength per μm of the polyolefin resin film of the present invention is preferably 0.12 N / μm, more preferably 0.14 N / μm. If it is 0.12 N / μm or more, pinholes are unlikely to occur when the protrusion hits the package. The upper limit of the puncture strength is preferably 1.0 N / μm, more preferably 0.8 N / μm, and even more preferably 0.5 N / μm. If it is 1.0 μm / μm or less, the stiffness is not too strong, and handling when made into a film or laminate is easy.
[0053] (Longitudinal orientation factor) The longitudinal orientation coefficient ΔNx used in the present invention can be calculated by Equation 1. ΔNx=Nx-[(Ny+Nz) / 2] (Equation 1) Nx: Refractive index in the longitudinal direction Ny: Refractive index in the direction perpendicular to the longitudinal direction Nz: Refractive index in the planar direction The lower limit of the longitudinal orientation coefficient ΔNx of the polyolefin resin film of the present invention is preferably 0.010, more preferably 0.015, and even more preferably 0.020. If it is 0.010 or more, the straight cutting property of the package is easily obtained. The upper limit of the longitudinal orientation coefficient ΔNx is preferably 0.0270, more preferably 0.026. If it is 0.0270 or less, the seal strength is not easily reduced.
[0054] (Face orientation coefficient) The plane orientation coefficient ΔP used in the present invention can be calculated from the refractive index. The orientation coefficient in the plane direction can be calculated by Equation 2. ΔP=[(Nx+Ny) / 2]-Nz (Equation 2) x: Refractive index in the longitudinal direction Ny: Refractive index in the direction perpendicular to the longitudinal direction Nz: Refractive index in the surface direction The lower limit of the orientation coefficient ΔP in the plane direction of the polyolefin resin film of the present invention is preferably 0.0100, more preferably 0.0120. If it is 0.0100 or more, the puncture strength of the package is easily obtained. The upper limit of the plane orientation coefficient ΔP is preferably 0.0160, more preferably 0.0150, and even more preferably 0.0140. If it is 0.0160 or less, the seal strength is not likely to decrease.
[0055] (Film melting point) The lower limit of the melting point of the polyolefin resin film of the present invention is not particularly limited, but is preferably 120°C, more preferably 130°C, and even more preferably 140°C or higher. If it is 120°C or higher, heat resistance to heat sealing is easily obtained. The upper limit of the melting point is preferably 150°C, more preferably 145°C. If it is 150°C or lower, low-temperature sealability is easily obtained.
[0056] (Bending pinhole resistance) The flex resistance can be measured by Gelbo pinhole evaluation. The number of pinholes after bending the polyolefin resin film of the present invention 1000 times at 1° C. is preferably 35, more preferably 30, still more preferably 25, and particularly preferably 20. If the number is 35 or less, pinholes are unlikely to occur due to bending impact during transportation of the package.
[0057] (tear strength) The upper limit of the tear strength in the longitudinal direction or transverse direction of the polyolefin resin film of the present invention, in which the heat shrinkage rate is greater after heating at 120° C. for 30 minutes, is preferably 0.8 N. If it is 0.8 N or less, the laminate film is easily torn. It is more preferably 0.6 N, and particularly preferably 0.5 N. The lower limit of the tear strength in the longitudinal direction or transverse direction of the polyolefin resin film of the present invention, in which the heat shrinkage rate is larger after heating at 120° C. for 30 minutes, is preferably 0.1 N. If it is 0.1 N or more, bag rupture resistance is easily obtained. It is more preferably 0.3 N.
[0058] (Acceleration Blocking Strength) The lower limit of the accelerated blocking strength of the polyolefin resin film of the present invention is preferably 20 mN / 70 mm, more preferably 30 mN / 70 mm. If it is 20 mN / 7 mm or more, the film is likely to have a firm feel. The upper limit of the accelerated blocking strength is preferably 100 mN / 70 mm, more preferably 80 mN / 70 mm, and even more preferably 60 mN / 70 mm. If it is 100 mN / 70 mm or less, blocking is unlikely to occur on the inner surface of the package.
[0059] (Martens hardness) The lower limit of the Martens hardness of at least one surface, particularly the sealing surface, of the polyolefin resin film of the present invention is preferably 80 N / mm 2 and more preferably 90N / mm 2 and particularly preferably 100 N / mm 2 That's it. 80N / mm 2 If the resistance is more than this, blocking is unlikely to occur on the inner surface of the package, and more preferably 90N / 70mm 2 The upper limit of the Martens hardness is preferably 140 N / mm 2 and more preferably 130 N / mm 2 and more preferably 120 N / mm 2 140N / mm 2 If the thickness is less than this, the film is not too hard and pinhole resistance due to bending is easily obtained.
[0060] (Indentation creep rate) The lower limit of the indentation creep rate (cit) of the sealing surface of the polyolefin resin film of the present invention is preferably 1.8%, more preferably 2.0%. If it is 1.8% or more, the film does not become hard and bending pinhole resistance is easily obtained. The upper limit of the indentation creep rate (cit) is preferably 3.0%, more preferably 2.8%. If it is 3.0% or less, blocking is less likely to occur on the inner surface of the package.
[0061] (Wetting tension) The lower limit of the wet tension of the surface to be laminated with at least one substrate film selected from the group consisting of the polyolefin resin film of the present invention, polyamide resin film, polyester resin film, and polypropylene resin film is preferably 30 mN / m, more preferably 35 mN / m. If it is 30 mN / m or more, the laminate strength is unlikely to decrease. The upper limit of the wet tension is preferably 55 mN / m, more preferably 50 mN / m. If it is 55 mN / m or less, blocking between the films is unlikely to occur when the polyolefin resin film is wound on a roll.
[0062] (Structure of laminate and manufacturing method) The laminate using the polyolefin resin film of the present invention is a laminate using the polyolefin resin film as a sealant and at least one film selected from the group consisting of polyamide resin film, polyester resin film, and polypropylene resin film. In addition, as a known technique, a coating or deposition process may be applied to these base films for the purpose of imparting adhesiveness or barrier properties, or aluminum foil may be further laminated. Specific examples include biaxially oriented PET film / aluminum foil / sealant, biaxially oriented PET film / biaxially oriented nylon film / sealant, biaxially oriented nylon film / sealant, biaxially oriented polypropylene film / sealant, and biaxially oriented PET film / biaxially oriented nylon film / aluminum foil / sealant. Among these, when a biaxially oriented nylon film is used with a conventional sealant, the straight cutability of the laminate is significantly deteriorated. By using the polyolefin resin film of the present invention as a sealant, a laminate with good straight cutability can be produced in any configuration. As the lamination method, a known method such as a dry lamination method or an extrusion lamination method can be used.
[0063] The properties of the laminate of the present invention will now be described. (Piercing strength) The lower limit of the puncture strength of the laminate of the present invention is preferably 10 N, more preferably 12 N, even more preferably 14 N, and particularly preferably 16 N. If it is 10 N or more, pinholes are unlikely to occur when the protrusions come into contact with a package. The upper limit of the puncture strength is preferably 45 N, more preferably 30 N, and even more preferably 25 N. If it is 45 N or less, the laminate will not feel too stiff and will be easy to handle.
[0064] (Straight cutting ability) The upper limit of the straight cuttability of the laminate of the present invention is preferably 8 mm, more preferably 7 mm, further preferably 6 mm, and particularly preferably 3 mm. If it is 8 mm or less, the package is unlikely to come apart.
[0065] (Tearful farewell) The upper limit of the tearing of the laminate of the present invention is preferably 12 mm, more preferably 10 mm, further preferably 6 mm, and particularly preferably 4 mm. If it is 12 mm or less, the contents are unlikely to spill out when the package is torn.
[0066] (Heat seal strength) The lower limit of the heat seal strength of the laminate of the present invention before retort is preferably 18 N / 15 mm, more preferably 19 N / 15 mm, and even more preferably 20 N / 15 mm. If it is 20 N / 15 mm or more, bag rupture resistance is easily obtained. A heat seal strength of 60 N / 15 mm is sufficient. The upper limit of the heat seal strength per 1 μm is preferably 3.0 N / 15 mm·μm, more preferably 2.0 N / 15 mm·μm. If it is 3.0 N / 15 mm·μm or less, additives such as highly impact resistant resins or fillers are not required, and costs are not likely to be high. There is no particular limit to the lower limit of the heat seal strength per 1 μm, but it is preferably 0.9 N / 15 mm·μm, more preferably 0.95 N / 15 mm·μm, and even more preferably 1.0 N / 15 mm·μm. If it is 0.9 N / 15 mm·μm or more, the seal is less likely to peel off during transportation and the contents are less likely to leak.
[0067] (packaging) The laminate is arranged to enclose the contents, such as foodstuffs, in order to protect the contents from dust, gases, and the like in the natural world, and is called a package. The package is produced by cutting out the laminate, gluing the inner surfaces together with a heated heat seal bar or ultrasonic waves, and forming it into a bag shape. For example, a four-sided sealed bag in which two rectangular laminates are stacked with the sealant side facing inward and the four sides are heat sealed is widely used. The contents may be foodstuffs, but may also be other products such as daily necessities, and the shape of the package may be a shape other than a rectangle, such as a standing pouch or a pillow package. EXAMPLES
[0068] The present invention will be described in detail below with reference to examples, but is not limited thereto. The properties obtained in each example were measured and evaluated by the following methods. In the evaluation, the flow direction of the film in the film production process was defined as the longitudinal direction, and the direction perpendicular to the flow direction was defined as the width direction.
[0069] (1) Resin density The density was evaluated according to JIS K7112:1999 D method (density gradient tube). N=3 measurements were made and the average value was calculated.
[0070] (2) Melt flow rate (MFR) Measurements were made at 230°C and a load of 2.16 kg based on JIS K-7210-1. N=3 measurements were made, and the average value was calculated.
[0071] (3) Hayes Haze was measured according to JIS K7136. Measurements were made on the polyolefin resin film before lamination (N=3), and the average value was calculated.
[0072] (4) Tear strength The film and laminate were cut into rectangular test pieces measuring 150 mm in the stretching direction and 60 mm perpendicular to the stretching direction. A 30 mm cut was made in the center of one of the short sides of the test piece along the stretching direction. The test pieces were conditioned in an atmosphere of 23°C and 50% relative humidity before measurements. The test piece with the notches was gripped with two grips at a distance of 10 mm from each of the short sides, with the distance between the two grips being 40 mm. An Autograph AG-I made by Shimadzu Corporation was then attached and carefully clamped so that the long sides of the test piece were parallel to the imaginary center line of the two grips. The test speed was set to 200 mm / min, the tester was started, and the tear force was recorded until the tear reached the other short side of the test piece, and the average tear force at the points where the test piece had been torn by 25 mm, 50 mm, 75 mm, and 100 mm was calculated. With the inner surface of the wound film facing forward, measurements were taken for both the right-hand piece held in the upper grip and the left-hand piece held in the upper grip, with N=3 for each case, and the average value for each was calculated. The larger value of the measurement results for the right and left sides was used as the tear strength. Similarly, with the polyolefin resin film side of the laminate facing forward, measurements were taken in both cases, with the right-hand piece clamped in the upper grip and the left-hand piece clamped in the upper grip, with N=3 for each case, and the average value for each was calculated. The larger of the measurement results for the right and left sides was used as the tear strength.
[0073] (5)Piercing strength The puncture strength of polyolefin resin films and laminates was measured at 23°C in accordance with "2. Testing Methods for Strength, etc." in "Standards and Criteria for Foods, Additives, etc., Part 3: Apparatus and Containers and Packaging" (Ministry of Health and Welfare Notification No. 20, 1982) in the Food Sanitation Act. A needle with a tip diameter of 0.7 mm was pierced into the film at a piercing speed of 50 mm / min, and the strength at which the needle penetrated the film was measured. The measured value was divided by the film thickness to calculate the puncture strength [N / μm] per 1 μm of film. N=3 measurements were made, and the average value was calculated.
[0074] (6) Longitudinal orientation coefficient, planar orientation coefficient Density was evaluated according to JIS K0062:1999 method for measuring refractive index of chemical products. Measurements were performed with N=3, and the average value was calculated. The longitudinal orientation coefficient ΔNx was calculated using Equation 1, and the in-plane orientation coefficient ΔP was calculated using Equation 2. ΔNx=Nx-[(Ny+Nz) / 2] (Equation 1) ΔP=[(Nx+Ny) / 2]-Nz (Equation 2)
[0075] (7) Melting point The melting point was determined as the temperature of the maximum melting peak in the DSC curve of the polyolefin resin film obtained using a Shimadzu differential scanning calorimeter DSC-60 manufactured by Shimadzu Corporation. The starting temperature was 30°C, the heating rate was 5°C / min, and the end temperature was 180°C. N=3 measurements were made, and the average value was calculated.
[0076] (8) Pinhole resistance due to bending The laminate with the polyolefin resin film was cut into a length of 280 mm and a width of 260 mm. The laminate was cut into a cylindrical shape with a diameter of 89 mm and a height of 260 mm so that the polyolefin resin film was on the inside, and fixed with cellophane tape. The sample was attached to a thermostatic chamber-equipped Gelbo Flex Tester manufactured by Tester Sangyo Co., Ltd., and a bending load was applied at 1°C 1000 times. The sample was removed and the number of pinholes was counted. Measurements were performed with N=3, and the average value was calculated.
[0077] (9) Heat shrinkage rate The film before lamination was cut into 120 mm squares. Marked lines were drawn at 100 mm intervals in both the longitudinal and transverse directions. The sample was hung in an oven kept at 120°C and heat-treated for 30 minutes. The distance between the marked lines was measured, and the thermal shrinkage rate was calculated according to the following formula. Measurements were made with N=3, and the average value was calculated. Heat shrinkage rate = (gauge length before heat treatment - gauge length after heat treatment) / gauge length before heat treatment x 100 (%) (Equation 3)
[0078] (10) Accelerated blocking strength A polyolefin resin film was cut into a length of 148 mm and a width of 105 mm. The seal surfaces were placed facing each other and overlapped. After preheating for 30 minutes in a 50°C environment, the film was sandwiched between 7.0 cm square aluminum plates held at 50°C. The aluminum plate and the sample were pressed at 50°C and 100 kN using a mini test press MP-SCH manufactured by Toyo Seiki Seisakusho Co., Ltd., and held for 15 minutes. The removed sample was cut into a width of 70 mm. The overlapped sample was opened by 30 mm, and a metal rod with a diameter of 3 mm was inserted so that it was parallel to the width. The sample was attached to an autograph AG-I manufactured by Shimadzu Corporation, and the load was measured when the metal rod was moved in the lengthwise direction at a speed of 200 mm / min. Measurements were performed with N=3, and the average value was calculated.
[0079] (11) Martens hardness, indentation creep rate Polyolefin resin film 10 mm The specimen was cut into four pieces, placed on a cover glass coated with adhesive with the measurement surface facing up, and dried for 24 hours. The Martens hardness and indentation creep rate were measured using a Shimadzu Dynamic Ultra-Micro Hardness Tester DUH-211 manufactured by Shimadzu Corporation. The measurement mode was a load-unload test, with a test force of 0.5 mN, a load speed of 6.0 mN / sec, and a load holding time of 2 sec, and a Triangular 15 indenter was used. N=10 measurements were made, and the average value was calculated.
[0080] (12) Straight cutting ability The straight cut property indicates the ability of the laminate to be torn straight in one direction when torn. Measurement was performed in the following manner. In the examples and comparative examples, the straight cut property was exhibited in the stretching direction, so measurements were performed in the stretching direction. The laminate was cut into a strip of 150 mm in the stretching direction and 60 mm in the direction perpendicular to the stretching direction, and a 30 mm cut was made in the center of the short side along the measurement direction. The sample was torn in accordance with JIS K7128-1:1998. When the piece had been torn 120 mm in the stretching direction, not including the 30 mm cut, the distance traveled in the direction perpendicular to the stretching direction was measured and the absolute value was recorded. Measurements were taken with N=3 for both the case where the right-hand piece was clamped in the upper grip, and the case where the left-hand piece was clamped in the upper grip, and the average value for each was calculated. The larger value of the measurement results for the right and left sides was used.
[0081] (13) Parting in Tears The heat seal films of the laminate were placed face to face and heat sealed to create a four-sided sealed bag with an inside dimension of 120 mm in the stretch direction and 170 mm perpendicular to the stretch direction. A notch was made at the edge of the four-sided sealed bag, and it was torn by hand in the stretch direction. The cut was continued to the opposite end, and the deviation of the tear lines of the film on the front and back sides of the bag was measured. The average value was calculated for both the right-hand side facing direction and the left-hand side facing direction, with N=3 for each, and the larger measurement value was used.
[0082] (14) Finished bag making The polyolefin resin film sides of the laminates were overlapped and heat sealed at 0.2 MPa for 1 second with a seal bar width of 10 mm and a heat seal temperature of 220°C to create a four-sided sealed bag with inner dimensions of 120 mm in the longitudinal direction and 170 mm in the transverse direction. The finished state of this four-sided sealed bag was visually inspected. ○: No distortion near the heat-sealed area, and the bag is perfectly rectangular. △: Little distortion near the heat-sealed area. ×: There is a large distortion near the heat seal area, and the edges of the bag are wavy.
[0083] (15) Heat seal strength The heat sealing conditions and strength measurement conditions are as follows. That is, the polyolefin resin film sides of the laminates obtained in the examples and comparative examples were overlapped and heat sealed at a pressure of 0.2 MPa for 1 second with a seal bar width of 10 mm and a heat seal temperature of 220°C, and then allowed to cool. Test pieces of 80 mm in the longitudinal direction and 15 mm in the transverse direction were cut from the films heat sealed at each temperature, and the peel strength of each test piece was measured when the heat sealed portion was peeled off at a crosshead speed of 200 mm / min. The test machine used was a universal material testing machine 5965 manufactured by Instron Instruments. Measurements were performed N=3 times for each, and the average value was calculated.
[0084] (16) Orientation angle The orientation angle (°) of the base film was measured using a molecular orientation meter MOA-6004 manufactured by Oji Scientific Instruments Co., Ltd. A sample was cut out to 120 mm in the longitudinal direction and 100 mm in the transverse direction, and placed on the measuring instrument. The measured angle was taken as the orientation angle. The longitudinal direction was 0°. N=3 measurements were made, and the average value was calculated.
[0085] Example 1 (Polyolefin resin film) For the polypropylene resin films of Examples 1 to 4 and Comparative Examples 1 to 8, raw materials were prepared based on the resin compositions and ratios of each layer shown in Tables 1 and 2 below. As shown in Tables 1 and 2, the preparations for each layer were taken as 100 parts by weight, and behenic acid amide was added as an organic lubricant to the heat seal layer at a content of 260 ppm, to the intermediate layer at a content of 260 ppm, and silica with an average particle size of 4 μm was added as an inorganic antiblocking agent to the heat seal layer at a content of 2000 ppm. These raw materials were mixed uniformly to obtain a mixed raw material for producing a polyolefin resin film. (Raw materials used) Raw material A: Sumitomo Chemical Co., Ltd. Propylene-ethylene-butene random copolymer FL8115A (MFR 7.0 g / 10 min, melting point 148°C) Raw material B: Prime Polymer propylene-ethylene random copolymer F-724NPC (MFR 7.0g / 10min, melting point 149℃) Raw material C: Butene-ethylene random copolymer (melting point 120°C, ethylene content 4.0 parts by weight) Raw material D: Sumitomo Chemical Co., Ltd. Propylene-ethylene block copolymer WFS5293-22 (resin density 891 kg / m 3 , 230℃, MFR3.0g / 10min) Raw material E Sumitomo Chemical Isotactic polypropylene FLX80E4 (MFR7.5g / min, melting point 164℃) Raw material F: Atactic polypropylene Sunattack manufactured by Chiba Fine Chemical Raw material G: Ethylene-butene copolymer elastomer resin, manufactured by Mitsui Chemicals, Toughmer A-4085S (MFR 1.4g / 10min at 190℃ and 2.16kg) Raw material H: Mitsui Chemicals propylene-butene copolymer elastomer resin, Toughmer XM-7070S (MFR 3.0g / 10min at 190℃, 2.16kg) Raw material I: Prime Polymer linear low-density polyethylene Evolue SP1520 (MFR 2.0 g / 10 min, density 0.913 g / cm 3 ) Raw material J: Sumitomo Chemical Co., Ltd. Propylene-ethylene-butene random copolymer FL8115A (MFR 6.0g / 10min, melting point 130℃)
[0086] (Melt Extrusion) The mixed raw materials for the intermediate layer were extruded in a three-stage single-screw extruder with a screw diameter of 90 mm, and the mixed raw materials for the laminate layer and heat seal layer were extruded in three-stage single-screw extruders with diameters of 45 mm and 65 mm, respectively, in the order of laminate layer / intermediate layer / heat seal layer. The preland was made into two stages with a width of 800 mm, and the step part was curved to ensure uniform flow of the molten resin. The extrusion was performed at an outlet temperature of 230° C. The thickness ratios of the laminate layer / intermediate layer / heat seal layer were 25% / 50% / 25%, respectively. (cooling) The molten resin sheet emerging from the die was cooled with a cooling roll at 21°C to obtain an unstretched polyolefin resin film with a thickness of 70 μm. When cooling with the cooling roll, both ends of the film on the cooling roll were fixed with air nozzles, the entire width of the molten resin sheet was pressed against the cooling roll with an air knife, and at the same time, a vacuum chamber was operated to prevent air from being drawn in between the molten resin sheet and the cooling roll. The air nozzles were installed in series on both ends in the direction of film travel. The die was surrounded by a sheet to prevent the molten resin sheet from being exposed to wind.
[0087] (preheat) The unstretched sheet was preheated by leading it to a group of heated rolls and bringing the sheet into contact with the rolls. The temperature of the preheating rolls was 80° C. Multiple rolls were used to preheat both sides of the film. (longitudinal stretching) The unstretched sheet was introduced into a longitudinal stretching machine and stretched 3.5 times by the roll speed difference to a thickness of 20 μm. The temperature of the stretching rolls was 80° C. (Annealing treatment) The film was heat-treated at 100° C. using annealing rolls to give a relaxation rate of 5%. Multiple rolls were used to heat-treat both sides of the film.
[0088] (Corona treatment) One side of the film (the lamination side) was subjected to a corona treatment. (winding) The film-forming speed was 20 m / min. The edge portions of the formed film were trimmed and wound into a roll. The wetting tension of one side of the film (laminate side) was 42 mN / m.
[0089] (Creating a laminate) The obtained polyolefin resin film and a biaxially oriented nylon film (N1102, thickness 15 μm, orientation angle 22° to the longitudinal direction) manufactured by Toyobo Co., Ltd. as a base film were coated with an ester adhesive obtained by mixing 33.6 parts by mass of a base agent (TM569 manufactured by Toyo Morton Co., Ltd.), 4.0 parts by mass of a hardener (CAT10L manufactured by Toyo Morton Co., Ltd.), and 62.4 parts by mass of ethyl acetate at a coating amount of 3.0 g / m 2 The resulting film was wound up and aged at 40° C. for 3 days to obtain a laminate.
[0090] (Examples 2 and 4) In Example 1, the raw materials shown in Table 1 were used, and a 20 μm polyolefin resin film was obtained in the same manner as in Example 1, except that the thickness of the unstretched polyolefin resin film was 80 μm and the longitudinal stretching ratio was 4.0 times. A laminate was obtained in the same manner as in Example 1.
[0091] Example 3 In Example 1, the raw materials shown in Table 1 were used, and a 20 μm polyolefin resin film was obtained in the same manner as in Example 1, except that the thickness of the unstretched polyolefin resin film was 90 μm and the longitudinal stretching ratio was 4.5 times. A laminate was obtained in the same manner as in Example 1.
[0092] Comparative Example 1 In Example 1, no antiblocking agent was added, and the raw materials shown in Table 2 were used, and a 60 μm polyolefin resin film was obtained in the same manner except that the thickness of the unstretched polyolefin resin film was 270 μm, the temperature of the preheat roll was 105° C., the temperature of the stretch roll was 105° C., the longitudinal stretch ratio was 4.5 times, and the annealing temperature was 120° C. A laminate was obtained in the same manner as in Example 1.
[0093] Comparative Example 2 A polyolefin resin film having a thickness of 90 μm was obtained in the same manner as in Example 2, except that the raw materials shown in Table 2 were used and the annealing treatment was not performed.
[0094] Comparative Example 3 In Example 2, no antiblocking agent was added, and the raw materials shown in Table 2 were used, and a 25 μm polyolefin resin film was obtained in the same manner except that the thickness of the unstretched polyolefin resin film was 100 μm, the preheat roll temperature was 102° C., the stretching roll temperature was 102° C., and the annealing temperature was 135° C. A laminate was obtained in the same manner as in Example 1.
[0095] Comparative Example 4 In Example 2, the antiblocking agent in the heat seal layer was 3000 ppm, the raw materials shown in Table 2 were used, the thickness of the unstretched polyolefin resin film was 320 μm, and the film was transversely stretched 8.0 times at a preheating temperature of 135° C. and a stretching temperature of 165° C. using a tenter without longitudinal stretching, and annealed with hot air at 155° C. in the tenter in the same manner to obtain a 40 μm polyolefin resin film. A laminate was obtained in the same manner as in Example 1.
[0096] Comparative Example 5 In Example 2, the antiblocking agent in the heat seal layer was 2400 ppm, the raw materials shown in Table 2 were used, the thickness ratio of the laminate layer / intermediate layer / heat seal layer was 2 / 5 / 29, the thickness of the unstretched polyolefin resin film was 180 μm, the longitudinal stretching ratio was 5.0 times, and no annealing treatment was performed. A 36 μm polyolefin resin film was obtained in the same manner as in Example 1. A laminate was obtained.
[0097] Comparative Example 6 In Comparative Example 1, the antiblocking agent in the heat seal layer was 2400 ppm, the raw materials shown in Table 2 were used, the thickness ratio of the laminate layer / intermediate layer / heat seal layer was 17 / 33 / 10, the thickness of the unstretched polyolefin resin film was 258 μm, the stretching ratio was 4.3 times, and a 60 μm polyolefin resin film was obtained in the same manner as in Example 1, except that no annealing treatment was performed.
[0098] Comparative Example 7 In Example 2, a 20 μm polyolefin resin film was obtained in the same manner as in Example 1, except that the antiblocking agent in the heat seal layer was 3000 ppm, the raw materials shown in Table 2 were used, the thickness of the unstretched polyolefin resin film was 100 μm, and the longitudinal stretching ratio was 5.0 times.
[0099] Comparative Example 8 A polyolefin resin film having a thickness of 20 μm was produced in the same manner as in Example 2, except that the annealing roll temperature was set to 130°C.
[0100] In Comparative Example 1, the transparency (haze) was poor because a block copolymer was mainly used. In Comparative Examples 2, 5, and 6, the annealing treatment was not performed, and therefore the heat shrinkage rate was high and the finished bags were inferior. In Comparative Example 3, since a large amount of propylene homopolymer was used, the melting point was high and the low-temperature sealability was poor. In Comparative Example 4, since the stretching direction was transverse stretching, the plane orientation coefficient was small and the pin puncture strength was poor. In Comparative Example 7, a butene-ethylene random copolymer having a low melting point was used, and therefore the straight cutting property and tear-off property were poor. In Comparative Example 8, the annealing temperature was high, and therefore the heat seal strength was poor. The results are shown in Tables 1 and 2.
[0101] [Table 1]
[0102] [Table 2]
[0103] In Tables 1 and 2, the evaluation results marked as "Not measurable*" indicate that the film was torn in the stretching direction during the property evaluation, and no measurement value could be obtained. [Industrial Applicability]
[0104] INDUSTRIAL APPLICABILITY The present invention can provide a package which is excellent in transparency, sealability, bag-making properties and resistance to rupture, and which can be easily torn without coming apart, thereby making a great contribution to industry.
Claims
1. A polyolefin resin film made of a polyolefin resin composition, the polyolefin resin composition containing at least a propylene-α-olefin random copolymer, and satisfying the following 1) to 7). 1) In the polyolefin resin composition, the content of the olefin block copolymer is 0 to 2 parts by weight per 100 parts by weight of the propylene-α-olefin random copolymer. 2) In the polyolefin resin composition, the content of the olefin copolymer elastomer resin is 0 to 2 parts by weight per 100 parts by weight of the propylene-α-olefin random copolymer. 3) In the polyolefin resin composition, the content of the propylene homopolymer is 0 to 40 parts by weight per 100 parts by weight of the propylene-α-olefin random copolymer. 4) A polyolefin resin film having a heat shrinkage rate of 25% or less after heating at 120°C for 30 minutes in the longitudinal direction or width direction of the polyolefin resin film, whichever direction has a larger heat shrinkage rate after heating at 120°C for 30 minutes. 5) The plane orientation coefficient ΔP calculated from the refractive index of the polyolefin resin film is 0.0100 or more and 0.0145 or less. 6) The polyolefin resin film has an orientation coefficient ΔNx in the longitudinal direction, calculated by the following formula 1, of 0.010 or more. ΔNx=Nx-[(Ny+Nz) / 2] (Formula 1) Nx: refractive index in the longitudinal direction Ny: refractive index in the direction perpendicular to the longitudinal direction Nz: Refractive index in the plane direction 7) The polyolefin resin film has a thickness of 7 μm or more and 80 μm or less.
2. 2. The polyolefin resin film according to claim 1, wherein at least one surface of the polyolefin resin film has a Martens hardness of 80 N / mm2 or more and an indentation creep rate (Cit) of 3.0% or less.
3. 3. The polyolefin resin film according to claim 1, wherein the haze of the polyolefin resin film is from 1% to 20%.
4. The polyolefin resin film according to any one of claims 1 to 3, wherein the polyolefin resin film has a tear strength of 0.8 N or less in the longitudinal direction or the width direction in which the heat shrinkage rate is greater after heating at 120°C for 30 minutes.
5. The polyolefin resin film according to any one of claims 1 to 4, wherein the polyolefin resin film has a puncture strength of 0.12 N / μm or more.
6. 6. The polyolefin resin film according to claim 1, wherein a concentration of an antiblocking agent in a layer located on at least one surface of the polyolefin resin film is 3000 ppm or less.
7. A laminate of the polyolefin resin film according to any one of claims 1 to 6 and a biaxially oriented film made of at least one polymer selected from the group consisting of polyamide resin films, polyester resin films, and polypropylene resin films.
8. The laminate according to claim 7, wherein the laminate has a straight cut ability of 8 mm or less in the longitudinal direction or width direction in which the thermal shrinkage rate is greater after heating at 120°C for 30 minutes, and a tear strength of 0.8 N or less in the longitudinal direction or width direction in which the thermal shrinkage rate is greater.
9. A packaging material comprising the laminate according to claim 7 or 8.
Citation Information
Patent Citations
Composition for lacquer ware base
JP1979011935A
Distribution valve of centralized lubrication device
JP1982090497A
Polyolefin stretched film
JP2002003619A
Packaging material for retort food
JP2014141302A
Tear-directionality sealant film, and film laminate
JP2016032911A