Coil component and method for manufacturing the coil component
The coil component design with metal and ceramic particles achieves improved insulation and compact size by optimizing particle size ratios and conductor arrangements, enhancing reliability and voltage withstand.
Patent Information
- Application Number
- JP2019193546
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-10-24
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-10-24
AI Technical Summary
Coil components require high insulation reliability and compact size, but increasing the distance between internal conductors for improved insulation leads to increased size.
A coil component design incorporating metal magnetic particles and ceramic particles with specific size ratios and distributions, along with a conductive material for conductors, ensures insulation reliability without significant size increase.
The design enhances insulation reliability and withstand voltage while maintaining a compact size, suitable for applications requiring high insulation properties.
Smart Images

Figure 0007560245000003 
Figure 0007560245000004 
Figure 0007560245000005
Abstract
Description
[Technical field]
[0001] The present invention relates generally to coil components and methods for manufacturing coil components. [Background technology]
[0002] Various magnetic materials have been used as the magnetic substrate of electronic components. For example, ferrite is often used as the magnetic material for coil components such as inductors. Ferrite has high magnetic permeability and is therefore suitable as a magnetic material for the substrate of coil components.
[0003] Metallic magnetic materials containing metallic magnetic particles are known as magnetic materials for electronic components other than ferrite. Metallic magnetic materials have a higher saturation magnetic flux density than ferrite, making them suitable as materials for the magnetic substrate of coil components through which large currents flow.
[0004] An insulating film is provided on the surface of each metal magnetic particle contained in the magnetic base to prevent short circuits between adjacent metal magnetic particles. However, a magnetic base made of a metal magnetic material has a problem that it has a lower volume resistivity and is more susceptible to insulation breakdown than a magnetic base made of ferrite. JP2017-092431A discloses a coil component in which three or more metal magnetic particles are arranged between the internal conductors to improve insulation in the region between the internal conductors of the magnetic base. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-092431 A Summary of the Invention [Problem to be solved by the invention]
[0006] Coil components are required to be compact as well as have high insulation reliability. Increasing the distance between opposing parts of the internal conductors improves insulation reliability, but this increases the dimension in the thickness direction.
[0007] It is an object of the present invention to provide a coil component that can be miniaturized while ensuring insulation reliability between internal conductors, and a method for manufacturing such a coil component. Other objects of the present invention will become apparent throughout the description of the entire specification. [Means for solving the problem]
[0008] A coil component according to one embodiment of the present invention includes a base including metal magnetic particles having a first average particle size and ceramic particles having a second average particle size smaller than the first average particle size, and a coil conductor provided within the base including a first conductor portion and a second conductor portion provided within the base so as to face the first conductor portion. In one embodiment, in an inter-conductor region of the base between the first conductor portion and the second conductor portion, a volume ratio of the ceramic particles to a total volume of the metal magnetic particles and the ceramic particles is 3 vol% or more.
[0009] In one embodiment of the present invention, the content ratio of the ceramic particles to the metal magnetic particles in the inter-conductor regions is 15 vol % or less.
[0010] In one embodiment of the present invention, the first conductor portion and the second conductor portion are made of a conductive material containing a metal, and the substrate is substantially free of atoms of the metal in the inter-conductor region.
[0011] In one embodiment of the invention, the ceramic particles are made of silica, alumina, zirconia, or titania.
[0012] In one embodiment of the present invention, the second average particle size is 1 / 50 or less of the first average particle size. In one embodiment of the present invention, the second average particle size is 1 / 200 or more of the first average particle size.
[0013] One embodiment of the present invention relates to a circuit board including the above-mentioned coil component.
[0014] One embodiment of the present invention relates to an electronic component including the above-mentioned circuit board.
[0015] A method for manufacturing a coil component according to an embodiment of the present invention includes the steps of: preparing a molded body including metal magnetic particles having a first average particle size and ceramic particles having a second average particle size smaller than the first average particle size, and having a coil conductor disposed therein; and heating the molded body at a temperature lower than the melting temperature of the ceramic particles. In one embodiment, the volume ratio of the ceramic particles to the total volume of the metal magnetic particles and the ceramic particles is 3 vol% or more. Effect of the Invention
[0016] According to the present invention, a coil component capable of improving the reliability of insulation is provided. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a perspective view of a coil component according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an exploded perspective view of the coil component of FIG. [Diagram 3] 2 is a cross-sectional view that illustrates a schematic cross section taken along line XX in FIG. 1. [Figure 4] 4 is an enlarged cross-sectional view showing a schematic enlargement of a region A in FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, various embodiments of the present invention will be described with reference to the drawings as appropriate. Note that components common to multiple drawings are given the same reference numerals throughout the multiple drawings. Please note that the drawings are not necessarily drawn to scale for the sake of convenience of explanation.
[0019] A coil component 1 according to one embodiment of the present invention will be described with reference to Figs. 1 to 4. The coil component 1 is an example of a coil component to which the present invention is applied. In the illustrated embodiment, the coil component 1 is a laminated inductor. This laminated inductor can be used as a power inductor incorporated in a power line and various other inductors. The present invention can be applied to various coil components other than the laminated inductor shown in the drawings.
[0020] As shown in the figure, the coil component 1 comprises a base 10, a coil conductor 25 provided within the base 10, an external electrode 21 provided on the surface of the base 10, and an external electrode 22 provided on the surface of the base 10 at a position spaced from the external electrode 21.
[0021] The coil component 1 is mounted on a circuit board 2. The circuit board 2 is provided with two land portions 3a, 3b. The coil component 1 may be mounted on the circuit board 2 by joining each of the external electrodes 21, 22 to the corresponding land portions 3 of the circuit board 2 by soldering. The circuit board 2 may include the coil component 1 and various electronic components other than the coil component 1. The circuit board 2 may be mounted on various electronic devices. Examples of electronic devices in which the circuit board 2 may be mounted include electronic devices used in smartphones, tablets, game consoles, and electrical equipment of automobiles, as well as various other electronic devices. The uses of the coil component 1 are not limited to those explicitly described in this specification.
[0022] The base body 10 is formed in a roughly rectangular parallelepiped shape. The base body 10 has a first main surface 10a, a second main surface 10b, a first end surface 10c, a second end surface 10d, a first side surface 10e, and a second side surface 10f. The outer surface of the main body 10 is defined by these six surfaces. The first main surface 10a and the second main surface 10b face each other, the first end surface 10c and the second end surface 10d face each other, and the first side surface 10e and the second side surface 10f face each other. In FIG. 1, the first main surface 10a is located on the upper side of the main body 10, so the first main surface 10a may be referred to as the "upper surface". Similarly, the second main surface 10b may be referred to as the "lower surface". The magnetically coupled coil component 1 is disposed so that the second main surface 10b faces the circuit board 2, and therefore the second main surface 10b is sometimes referred to as the "mounting surface." When referring to the up-down direction of the magnetically coupled coil component 1, the up-down direction in FIG. 1 is used as a reference. In this specification, unless otherwise understood in the context, the "length" direction, "width" direction, and "thickness" direction of the coil component 1 are the "L-axis" direction, "W-axis" direction, and "T-axis" direction in FIG. 1, respectively. The L-axis, W-axis, and T-axis are mutually orthogonal. The coil axis Y extends along the T-direction. For example, the coil axis Y passes through the intersection of the diagonals of the first main surface 10a having a rectangular shape in a plan view, and extends in a direction perpendicular to the first main surface 10a.
[0023] In one embodiment of the present invention, the coil component 1 is formed so that the length dimension (dimension in the L-axis direction) is 0.2 to 6.0 mm, the width dimension (dimension in the W-axis direction) is 0.1 to 4.5 mm, and the thickness dimension (dimension in the T-axis direction) is 0.1 to 4.0 mm. These dimensions are merely examples, and the coil component 1 to which the present invention is applicable may have any dimensions as long as they are not contrary to the spirit of the present invention. In one embodiment, the coil component 1 is formed to have a low height. For example, the coil component 1 is formed so that its width dimension is larger than its thickness dimension.
[0024] As shown in Figures 2 and 3, the base 10 has a plurality of stacked magnetic layers. As shown in the figures, the base 10 includes a main body portion 20, an upper cover layer 18 provided on the upper surface of the main body portion 20, and a lower cover layer 19 provided on the lower surface of the main body portion 20. The main body portion 20 includes stacked magnetic layers 11 to 16. In the base 10, the upper cover layer 18, the magnetic layer 11, the magnetic layer 12, the magnetic layer 13, the magnetic layer 14, the magnetic layer 15, the magnetic layer 16, the magnetic layer 17, and the lower cover layer 19 are stacked in this order from top to bottom in Figure 2.
[0025] The upper cover layer 18 includes four magnetic layers 18a to 18d. In the upper cover layer 18, the magnetic layer 18a, the magnetic layer 18b, the magnetic layer 18c, and the magnetic layer 18d are stacked in this order from bottom to top in FIG.
[0026] The lower cover layer 19 includes four magnetic layers 19a to 19d. In the lower cover layer 19, the magnetic layer 19a, the magnetic layer 19b, the magnetic layer 19c, and the magnetic layer 19d are stacked in this order from top to bottom in FIG.
[0027] The magnetic layers 11 to 16 are provided with corresponding conductor patterns C11 to C16. These conductor patterns C11 to C16 form a coil conductor 25. The coil conductor 25 has a coil axis Y. The conductor patterns C11 to C16 are formed so as to extend around the coil axis Y. In the illustrated embodiment, the coil axis Y extends in the T-axis direction and coincides with the lamination direction of the magnetic layers 11 to 16.
[0028] In another embodiment of the present invention, the magnetic layers 11 to 16 may be laminated in the L-axis direction. In this case, by forming the conductor patterns C11 to C16 on the surfaces of the magnetic layers 11 to 16, the coil axis Y faces the L-axis direction, which is the same as the lamination direction of the magnetic layers 11 to 16. In another embodiment of the present invention, the magnetic layers 11 to 16 may be laminated in the W-axis direction. In this case, by forming the conductor patterns C11 to C16 on the surfaces of the magnetic layers 11 to 16, the coil axis Y faces the W-axis direction, which is the same as the lamination direction of the magnetic layers 11 to 16.
[0029] The coil component 1 may include any number of insulating layers as necessary in addition to the insulating layers 11 to 16, the insulating layers 18a to 18d, and the insulating layers 19a to 19d. Some of the insulating layers 11 to 16, the insulating layers 18a to 18d, and the insulating layers 19a to 19d may be omitted as appropriate. Although the boundaries between the magnetic layers are shown in FIG. 3, the boundaries between the magnetic layers may not be visible in the base of an actual coil component to which the present invention is applied.
[0030] The conductor patterns C11 to C16 are formed on the corresponding insulating layers 11 to 16, respectively. The conductor patterns C11 to C16 are formed by printing such as screen printing, plating, etching, or any other known method. The vias V1 to V5 are formed at predetermined positions of the insulating layers 11 to 15, respectively. The vias V1 to V5 are formed by forming through holes penetrating the insulating layers 11 to 15 in the T-axis direction at predetermined positions of the insulating layers 11 to 15, and filling the through holes with a conductive material. The conductor patterns C11 to C16 and the vias V1 to V5 contain a metal with excellent conductivity, for example, Ag, Pd, Cu, Al, or an alloy of these.
[0031] In this specification, the region of the base 10 between adjacent conductor patterns among the conductor patterns C11 to C16 is referred to as an inter-conductor region. In other words, the inter-conductor region is a part of the base 10, and is a region sandwiched between adjacent conductor patterns. Five inter-conductor regions 10X are shown in Fig. 3. One of the inter-conductor regions 10X is between the conductor pattern C11 and the conductor pattern C12 adjacent to the adjacent pattern C11. The other inter-conductor regions 10X are also arranged between adjacent conductor patterns as shown in the figure.
[0032] The inter-conductor region 10X will be further described with reference to Fig. 4. Fig. 4 shows an enlarged view of region A in Fig. 3. Region A includes a part of conductor pattern C12, a part of conductor pattern C13, and a part of inter-conductor region 10X between conductor pattern C12 and conductor pattern C13. As shown in the figure, the base 10 includes a plurality of metal magnetic particles 31 and a plurality of ceramic particles 32 in the inter-conductor region 10X.
[0033] The metal magnetic particles 31 are particles or powder made of a soft magnetic metal material. The soft magnetic metal material for the metal magnetic particles 31 is, for example, particles of (1) metallic Fe or Ni, (2) alloys Fe-Si-Cr, Fe-Si-Al, or Fe-Ni, (3) amorphous Fe-Si-Cr-BC or Fe-Si-B-Cr, (4) or a mixture of these materials.
[0034] The average particle size of the metal magnetic particles 31 is, for example, 2 μm to 10 μm. The average particle size of the metal magnetic particles 31 is not limited to the range of 2 μm to 10 μm and can be changed as appropriate. In this specification, the "average particle size" of the magnetic particles means the volume-based average particle size unless otherwise interpreted. The volume-based average particle size of the magnetic particles is measured by a laser diffraction scattering method in accordance with JIS Z 8825. As the laser diffraction / scattering device, for example, a laser diffraction / scattering type particle size distribution measuring device (model number: LA-960) manufactured by Horiba, Ltd., Kyoto City, Kyoto Prefecture, Japan, can be used.
[0035] The metal magnetic particles 31 may include two types of metal magnetic particles having different average particle diameters. When the metal magnetic particles 31 include two types of metal magnetic particles having different average particle diameters, the larger of the metal magnetic particles 31 has an average particle diameter of, for example, 2 μm to 10 μm, and the smaller of the metal magnetic particles 31 has an average particle diameter of, for example, 1 / 20 to 1 / 2 of the larger. The smaller of the metal magnetic particles 31 having different average particle diameters has an average particle diameter of, for example, 0.2 μm to 1 μm. The metal magnetic particles 31 may include three or more types of metal magnetic particles having different average particle diameters.
[0036] An insulating film is provided on the surface of the metal magnetic particle 31. The insulating film on the surface of the metal magnetic particle 31 may be, for example, an oxide film formed by oxidizing the surface of the metal magnetic particle 31. An insulating coating film may be provided on the surface of the metal magnetic particle 31. This coating film may be, for example, a thin film made of silica or containing silica.
[0037] The ceramic particles 32 are particles or powder made of a ceramic material having an average particle size smaller than that of the metal magnetic particles 31. The ceramic particles 32 are made of a ceramic material having a higher electrical resistivity than that of the metal magnetic particles 31. The ceramic particles 32 are, for example, particles made of silica, alumina, zirconia, or titania, or mixed particles of these. The ceramic particles 32 have higher insulating properties than the metal magnetic particles 31 provided with an insulating film.
[0038] The average particle size of the ceramic particles 32 is, for example, 10 to 50 nm. The average particle size of the ceramic particles 32 may be 1 / 50 or less of the average particle size of the metal magnetic particles 31. The average particle size of the ceramic particles 32 may be 1 / 100 or less of the average particle size of the metal magnetic particles 31. In one embodiment, the average particle size of the ceramic particles 32 may be 1 / 200 or more of the average particle size of the metal magnetic particles 31. The average particle size of the ceramic particles 32 may be 1 / 50 or less and 1 / 200 or more of the average particle size of the metal magnetic particles 31. When the metal magnetic particles 31 include two or more types of metal magnetic particles having different average particle sizes, the average particle size of the ceramic particles 32 is compared with the average particle size of the largest average particle size of the multiple types of metal magnetic particles 31. In other words, the average particle size of the ceramic particles 32 may be 1 / 50 or less of the average particle size of the largest average particle size of the multiple types of metal magnetic particles 31.
[0039] In one embodiment of the present invention, the content of ceramic particles 32 relative to the total volume of metal magnetic particles 31 and ceramic particles 32 in inter-conductor region 10X of base 10 is 3 vol% or more in terms of volume ratio. In one embodiment of the present invention, the content of ceramic particles 32 relative to the total volume of metal magnetic particles 31 and ceramic particles 32 in inter-conductor region 10X of base 10 is 15 vol% or less in terms of volume ratio.
[0040] The volume of the metal magnetic particles 31 contained in the base 10 is obtained by measuring the particle size of each metal magnetic particle appearing on a cross section obtained by cutting the base 10 using the laser diffraction scattering method according to JIS Z 8825 described above, and converting the particle size obtained as a result of this measurement into a volume. When converting from particle size to volume, each magnetic particle is assumed to be spherical, in consideration of the measurement principle of the laser diffraction scattering method according to JIS Z 8825. The volume of the ceramic particles 32 is also measured and calculated in the same manner as the volume of the metal magnetic particles 31.
[0041] In one embodiment of the present invention, the inter-conductor region 10X is substantially free of atoms of the metal contained in the coil conductor 25. For example, when the conductor patterns C11-C16 contain a certain metal (e.g., Ag), if the elemental amount of the metal contained in the inter-conductor region 10X is 1% or less of the elemental amount of the metal contained in a predetermined region in the conductor patterns C11-C16, it can be determined that the inter-conductor region 10X is substantially free of atoms of the metal contained in the coil conductor 25. More specifically, the coil component 1 is cut along its thickness direction (T direction) to expose a cross section including at least one of the conductor patterns C11-C16 and the inter-conductor region 10X, and energy dispersive X-ray analysis (EDS) is performed on the region included in the conductor patterns C11-C16 and the region included in the inter-conductor region 10X of the cross section, thereby making it possible to compare the elemental amount of the metal contained in the conductor patterns C11-C16 with the elemental amount of the metal contained in the inter-conductor region 10X. For example, when the conductor patterns C11 to C16 contain Ag, the amount of Ag element in a 1 μm square region A1 in the conductor pattern C12 shown in FIG. 4 and a 1 μm square region A2 in the inter-conductor region 10X are analyzed by EDS, and when the count value of the detection peak of Ag element obtained in the region A2 is 1 / 100 or less of the count value of the detection peak of Ag element obtained in the region A1, it can be determined that the inter-conductor region 10X does not substantially contain atoms of the metal contained in the conductor patterns C11 to C16 (i.e., the metal contained in the coil conductor 25). Since the base of the conventional coil component does not contain ceramic particles corresponding to the ceramic particles 32 of the above embodiment, the metal atoms contained in the conductor patterns diffuse into the inter-conductor region. Therefore, the metal atoms contained in the coil conductor (conductor pattern) are present in the inter-conductor region of the base of the conventional coil component. In contrast, in the embodiment of the present invention, since the inter-conductor region 10X contains 3 vol % or more of ceramic particles 32, metal atoms do not diffuse from the conductor patterns C11-C16 to the inter-conductor region 10X. As a result, the metal atoms contained in the conductor patterns C11-C16 are substantially absent in the inter-conductor region 10X.As a result, the physical properties of the inter-conductor regions 10X of the substrate 10 are not affected by the metal atoms contained in the conductor patterns C11-C16 (for example, by the diffusion of the metal atoms into the inter-conductor regions 10X). For example, the insulation resistance of the inter-conductor regions 10X is not affected by the metal atoms contained in the conductor patterns C11-C16. In other words, the metal atoms contained in the conductor patterns C11-C16 do not substantially reduce the insulation resistance value of the inter-conductor regions 10X.
[0042] The base 10 may contain a binder for strengthening the bond between the metal magnetic particles 31. The binder contained in the base 10 may be a thermosetting resin with excellent insulating properties, such as an epoxy resin, a phenolic resin, a polyimide resin, a silicone resin, a polystyrene (PS) resin, a high density polyethylene (HDPE) resin, a polyoxymethylene (POM) resin, a polycarbonate (PC) resin, a polyvinyldiene fluoride (PVDF) resin, a phenolic resin, a polytetrafluoroethylene (PTFE) resin, a polybenzoxazole (PBO) resin, a polyvinyl alcohol (PVA) resin, a polyvinyl butyral (PVB) resin, or an acrylic resin.
[0043] The base 10 may also contain metal magnetic particles 31 and ceramic particles 32 in regions other than the inter-conductor regions 10X. The content of the ceramic particles 32 in the regions of the base 10 other than the inter-conductor regions 10X may be less than the content of the ceramic particles 32 in the inter-conductor regions 10X. For example, in a core region of the base 10 located inside the coil conductor 25 in the radial direction centered on the Y-axis, the content of the ceramic particles 32 can be made less than the content in the inter-conductor regions 10X. This allows the content of the metal magnetic particles 31 in the core region to be increased, thereby improving the effective permeability of the coil device 1.
[0044] Next, an example of a method for manufacturing the coil component 1 will be described. In one embodiment of the present invention, the coil component 1 is manufactured by a sheet manufacturing method using a magnetic sheet. When manufacturing the coil component 1 by the sheet manufacturing method, first, an upper laminate which becomes the upper cover layer 18, an intermediate laminate, and a lower laminate which becomes the lower cover layer 19 are formed. The upper laminate is formed by stacking a plurality of magnetic sheets which become the magnetic layers 18a to 18d, the lower laminate is formed by stacking a plurality of magnetic sheets which become the magnetic layers 19a to 19d, and the intermediate laminate is formed by stacking a plurality of magnetic sheets which become the magnetic layers 11 to 16. The magnetic sheet is manufactured by, for example, putting a slurry obtained by kneading a particle group including the metal magnetic particles 31 and the ceramic particles 32 with a resin into a molding die and applying a predetermined molding pressure. As the resin which is kneaded with the metal magnetic particles 31 and the ceramic particles 32, for example, a resin material having excellent insulating properties such as polyvinyl butyral (PVB) resin or epoxy resin can be used.
[0045] The intermediate laminate is formed by stacking a plurality of magnetic sheets on which conductor patterns corresponding to the conductor patterns C11 to C16 are formed. Each of the magnetic sheets for the intermediate laminate is formed with a through hole penetrating in the stacking direction, and the conductor patterns corresponding to the conductor patterns C11 to C16 are formed on the magnetic sheets with the through holes formed therein by screen printing or the like. At this time, the metal material constituting each conductor pattern is embedded in the through hole of the magnetic sheets to form vias. After forming each of the sheets including the conductor patterns C11 to C16, the base film is removed, and the sheets are stacked in order from the sheet including the conductor pattern C16 to the sheet including the conductor pattern C11 to obtain the intermediate laminate.
[0046] Next, the intermediate laminate produced as described above is sandwiched between an upper laminate and a lower laminate from above and below, and the upper laminate and the lower laminate are thermocompression-bonded to the intermediate laminate to obtain a main laminate. Next, the main laminate is diced into pieces of a desired size using a cutting machine such as a dicing machine or a laser processing machine to obtain a chip laminate.
[0047] Next, the chip stack is degreased, and the degreased chip stack is heat-treated. The chip stack is heat-treated at a temperature lower than the melting temperature of the ceramic particles 32 contained in the chip stack. The ceramic particles 32 melt at 1000°C or higher. When the ceramic particles 32 are silica, the ceramic particles melt at about 1500°C. The chip stack is heat-treated, for example, at 400°C to 900°C for 20 minutes to 120 minutes. The ceramic particles 32 are not oxidized or reduced during the heat treatment of the stack. A material that does not undergo oxidation or reduction reactions at temperatures below 900°C is selected for the ceramic particles 32.
[0048] Next, a conductive paste is applied to both ends of the heat-treated chip stack to form external electrodes 21 and external electrodes 22. Through the above steps, coil component 1 is obtained.
[0049] The coil component 1 may be manufactured by a method known to those skilled in the art other than the sheet manufacturing method, such as a slurry build method or a thin film process manufacturing method. By manufacturing the coil component 1 by the slurry build method or the thin film process manufacturing method, it is easy to make the content of the ceramic particles 32 in the inter-conductor region 10X of the base 10 different from the content of the ceramic particles 32 in the core region of the base 10 located inside the coil conductor 25 in the radial direction centered on the Y axis. For example, by making the content of the ceramic particles 32 in the core region of the base 10 less than the content of the ceramic particles 32 in the inter-conductor region 10X, the content of the metal magnetic particles 31 in the core region can be increased, and the effective permeability of the coil component 1 can be improved.
[0050] The illustrated laminated inductor is an example of a coil component to which the present invention can be applied, and the present invention can be applied to various types of coil components other than laminated inductors. For example, the present invention can also be applied to planar coils.
[0051] The coil component according to the present invention may be manufactured by a compression molding process instead of a lamination process. When manufacturing the coil component 1 by a compression molding process, a particle group including the metal magnetic particles 31 and the ceramic particles 32 is first kneaded with a binder resin to create a slurry. Next, the slurry is placed in a molding die in which a coil conductor is placed, and a molding pressure is applied to obtain a molded body including the coil conductor inside. Next, the molded body is subjected to a heat treatment at a temperature lower than the melting temperature of the ceramic particles 32 to obtain the base body 10. Next, the base body 10 is coated with a conductor paste to form the external electrodes 21 and 22 on the surface of the base body 10. In this manner, the coil component 1 is manufactured by a compression molding process. EXAMPLES
[0052] An embodiment of the present invention will be described. First, metal magnetic particles having a composition of Fe-Si-Cr (Fe: 92 wt%, Si: 3.5%, Cr: 4.5 wt%) were prepared. Then, the metal magnetic particles and silica particles as ceramic particles were mixed in the ratio shown in Table 1 to obtain a mixed powder. In Table 1, the contents of the metal magnetic particles and the ceramic particles relative to the total volume of the metal magnetic particles and the ceramic particles in this mixed powder are expressed in volume ratio conversion. Next, this mixed powder was kneaded with polyvinyl butyral to prepare a slurry. Next, this slurry was formed into a long sheet using a coating machine such as a die coater, and cut to prepare multiple rectangular parallelepiped magnetic sheets with a thickness of 8 μm. In this way, nine types of magnetic sheets (nine types of magnetic sheets: first magnetic sheet to ninth magnetic sheet) with different contents of ceramic particles were prepared in multiple numbers.
[0053] Next, through holes were provided at predetermined positions of the first magnetic sheet using a laser or the like, and then the through holes were filled with conductive paste containing Ag, and the conductive paste containing Ag was printed on the magnetic sheet in a predetermined pattern. The first magnetic sheets on which the conductive patterns were formed in this way were stacked so that the conductive patterns formed on the different first magnetic sheets were electrically connected to each other via the conductors filled in the through holes, and temporary pressure bonding was performed at 60°C to obtain a laminate. Similarly, laminates were produced using each of the second magnetic sheet to the ninth magnetic sheet. Next, each of these nine types of laminates was cut into individual pieces by a dicing machine. Next, the individualized chip laminates were degreased, and the degreased chip laminates were subjected to a heat treatment at 800°C. External electrodes were formed on the evaluation chips after the heat treatment to obtain nine types of evaluation coil conductors (samples A1 to A9). The dimensions of the evaluation coil conductor in the L direction, W direction, and T direction were 1.6 mm, 0.8 mm, and 0.8 mm, respectively, and the coil conductor had 4.5 turns inside.
[0054] Twenty pieces each of Samples A1 to A9 were prepared, and a deflection test was performed on each of the coil conductors for evaluation of Samples A1 to A9. The deflection test was performed as follows. First, the coil conductors for evaluation were mounted on a glass epoxy board with a thickness of 0.8 mm. The board was attached between a pair of support pillars with a radius of 2.5 mm arranged at 90 mm intervals, and the center of the lower surface of the board attached between the support pillars was pressed to a depth of 10 mm at a speed of 2.5 mm / sec with an indenter whose tip had a curvature radius of R340, thereby deflecting the board. This deflection test was performed while monitoring the resistance of the evaluation coil. Among the coil conductors for evaluation, those that had no conductive breakdown and no visible cracks when the indenter was pressed to a depth of 10 mm were determined to be good products.
[0055] The results of the deflection test are shown in Table 1. As shown in Table 1, for samples A1 to A6, which had a ceramic particle content of 15 vol% or less, no electrical breakdown or cracks occurred in any of the 20 evaluation coil components. Thus, it was found that even when the base of the coil conductor contains ceramic particles, the coil component has sufficient deflection strength as long as the content is 15 vol% or less. [Table 1]
[0056] As described above, increasing the content of ceramic particles 32 in the inter-conductor region 10X reduces the flexural strength. If the content of ceramic particles 32 in the inter-conductor region 10X is further increased, for example to 100 vol%, delamination is likely to occur during the manufacturing process. This delamination during the manufacturing process is undesirable as it reduces the yield. Furthermore, when the content of ceramic particles 32 in the inter-conductor region 10X reaches 100 vol%, the inductance of the coil component is degraded.
[0057] Next, nine types of magnetic sheets (first magnetic sheet to ninth magnetic sheet) were prepared in the same manner as in the preparation process of samples A1 to A9. Next, a conductive paste containing Ag was printed in a predetermined pattern on each of the two first magnetic sheets. The two first magnetic sheets on which the conductive patterns were printed were stacked so that the conductive patterns faced each other. A predetermined number of first magnetic sheets on which the conductive patterns were not printed on the upper and lower surfaces of the two first magnetic sheets were stacked and temporarily pressed at 60°C to obtain a laminate. Similarly, a laminate was prepared using each of the second magnetic sheet to the ninth magnetic sheet. Next, each of these nine types of laminates was divided into individual pieces by a dicing machine. Next, the individual chip laminates were degreased, and the degreased chip laminates were subjected to a heat treatment at 800°C. External electrodes were formed on the evaluation chips after the heat treatment to obtain nine types of evaluation capacitor chips (samples B1 to B9). The dimensions of this evaluation capacitor chip in the L direction, W direction, and T direction are 1.6 mm×0.8 mm×0.8 mm, respectively.
[0058] In addition, for each of the evaluation capacitor chips of samples B1 to B9, the voltage applied between the external electrodes was increased stepwise, and the voltage at which a short circuit occurred was measured. The voltage at which a short circuit occurred was divided by the distance between the electrodes, and the value was shown in Table 2 as the withstand voltage of each sample. [Table 2]
[0059] As shown in Table 2, samples B3 to B9, which contained 3 vol% or more of ceramic particles, had a withstand voltage of 2.0 V / μm or more. For inductors in power systems, where a coil component with a high current is desired, a withstand voltage of 2 V / μm or more is desirable. As shown in Table 2, it was found that a substrate with a withstand voltage of 2 V / μm or more can be obtained if the content of ceramic particles is 3 vol% or more. By using this substrate as the substrate for a coil component, a coil component with a withstand voltage of 2 V / μm or more can be obtained.
[0060] Next, the effects of the above embodiment will be described. In the above embodiment, since the base 10 contains the ceramic particles 32 in the inter-conductor regions 10X, which have higher insulating properties than the metal magnetic particles 31, the volume resistivity in the inter-conductor regions 10X of the base 10 can be improved. This provides a coil component 1 with improved insulation resistance, i.e., withstand voltage, between the conductor patterns C11 to C16. In particular, when the content of the ceramic particles 32 is 3 vol% or more, a coil component 1 with a high withstand voltage of 2 V / μm or more can be obtained.
[0061] According to the above embodiment, since the average particle size of the ceramic particles 32 is smaller than the average particle size of the metal magnetic particles 31, the ceramic particles 32 penetrate into the gaps between the metal magnetic particles 31. Therefore, the volume of the inter-conductor region 10X is hardly increased even when the ceramic particles 32 are added. Therefore, the above embodiment can improve the volume resistivity of the inter-conductor region 10X while suppressing an increase in the size of the inter-conductor region 10X. By setting the average particle size of the ceramic particles 32 to 1 / 50 or 1 / 100 of the average particle size of the metal magnetic particles 31 or less, the ceramic particles 32 can easily penetrate between the particles of the metal magnetic particles 31. In this case, since the size of the inter-conductor region 10X does not substantially increase even when the ceramic particles 32 are added, the volume resistivity can be improved without increasing the size of the inter-conductor region 10X. If the average particle size of the ceramic particles 32 is smaller than 1 / 200 of the average particle size of the metal magnetic particles 31, the ceramic particles 32 are less likely to penetrate into the gaps between the metal magnetic particles 31 due to aggregation of the slurry, etc. For this reason, it is preferable that the average particle size of ceramic particles 32 is at least 1 / 200 of the average particle size of metal magnetic particles 31 .
[0062] The conductor patterns C11 to C16 contain a metal. A part of this metal is present in the conductor patterns C11 to C16 as a cation. A metal element (e.g., Fe) contained in the metal magnetic particles 31 is oxidized in a heat treatment during the manufacture of the coil component 1. When electrons released when the metal magnetic particles 31 are oxidized react with cations (Ag+) of a metal (e.g., Ag) in the conductor patterns C11 to C16 in the inter-conductor region 10X, the metal (Ag) precipitates in the inter-conductor region 10X. That is, the metal contained in the conductor patterns C11 to C16 can diffuse into the inter-conductor region 10X. According to the above embodiment, the presence of the ceramic particles 32 in the inter-conductor region 10X reduces the contact area between the conductor patterns C11 to C16 and the metal magnetic particles 31 contained in the inter-conductor region 10X, so that atoms of the metal contained in the conductor patterns C11 to C16 are less likely to diffuse into the inter-conductor region 10X. In one embodiment, metal atoms contained in the conductor patterns C11-C16 are substantially absent in the inter-conductor regions 10X. If the metal atoms contained in the conductor patterns C11-C16 diffuse into the inter-conductor regions 10X, this can cause a deterioration in the insulation properties of the inter-conductor regions 10X. However, according to the above embodiment, the metal atoms contained in the conductor patterns C11-C16 do not diffuse into the inter-conductor regions 10X, so that the insulation resistance, i.e., the voltage resistance, of the inter-conductor regions 10X can be further improved.
[0063] According to the above embodiment, in the inter-conductor region 10X of the base 10, the content of the ceramic particles 32 relative to the total volume of the metal magnetic particles 31 and the ceramic particles 32 is 15 vol% or less in terms of volume ratio, so that it is possible to improve the volume resistivity of the inter-conductor region 10X while suppressing deterioration of the flexural strength of the base 10 caused by adding the ceramic particles 32. The flexural strength of the base 10 including the metal magnetic particles 31 is ensured by the bonding between the metal magnetic particles 31 in the base 10. By setting the content of the ceramic particles 32 to 15 vol% or less, the bonding between the metal magnetic particles 31 is not inhibited, and as a result, it is possible to prevent or suppress a decrease in the flexural strength of the base 10.
[0064] According to the above embodiment, the heating in the manufacturing process of the coil component 1 is performed at a temperature lower than the melting temperature of the ceramic particles 32, which makes it possible to prevent distortion of the shape of the base 10 due to the flow of the ceramic particles 32. This makes it possible to prevent a decrease in insulation resistance, i.e., voltage resistance, caused by a decrease in the gap between opposing portions of the coil conductor 25.
[0065] According to the above embodiment, the withstand voltage of the coil component 1 can be made higher than that of the conventional coil component. As a result, even if the distance between opposing portions of the coil conductor 25 is designed to be smaller than the distance between the coil conductors in a conventional coil component that does not contain ceramic particles, the insulation resistance can be obtained equivalent to that of the conventional coil component. This allows the size of the component to be reduced in height.
[0066] Compared to information and communication devices such as smartphones, coil components used in automotive electrical equipment may not only pass a large current but also be subjected to a high voltage. For this reason, coil components used in automotive electrical equipment may be required to have insulation properties at least twice as high as those of conventional coil components mainly used in information and communication devices. The coil components according to the above-described embodiments may also be used in applications requiring such high insulation properties.
[0067] The dimensions, materials, and arrangement of each component described in this specification are not limited to those explicitly described in the embodiments, and each component can be modified to have any dimensions, materials, and arrangement that can be included in the scope of the present invention. Also, components not explicitly described in this specification can be added to the described embodiments, and some of the components described in each embodiment can be omitted. [Explanation of symbols]
[0068] 1 Coil parts 10 Base 10X Interconductor Area 21, 22 External electrode 25 Coil conductor 31 Metal magnetic particles 32 Ceramic particles C11~C16 Conductor pattern
Claims
1. A process for preparing a laminate comprising: stacking a plurality of magnetic sheets, each including a magnetic sheet having a conductor pattern formed thereon, the magnetic sheets including the magnetic sheet having a metal magnetic particle, a ceramic particle, and a resin, such that the conductor patterns formed on adjacent magnetic sheets face each other and an inter-conductor region is formed between the facing conductor patterns; a heat treatment step of heating the laminate at a temperature of 400° C. to 900° C., which is lower than the melting temperature of the ceramic particles; Equipped with In the inter-conductor region of the laminate after the heat treatment step, a volume ratio of the ceramic particles to a total volume of the metal magnetic particles and the ceramic particles is 3 vol% or more; the metal magnetic particles have a first average particle size and have an insulating film containing silica on a surface thereof; the ceramic particles have a second average particle size smaller than the first average particle size. A method for manufacturing a multilayer inductor.
2. The laminate after the heat treatment step includes a plurality of insulating layers including the inter-conductor regions, and the conductor patterns respectively disposed between the plurality of insulating layers, The laminate is formed such that boundaries between the plurality of insulating layers are not visible in areas other than the inter-conductor areas. The method for producing the laminated inductor according to claim 1 .
3. The ceramic particles include silica, alumina, zirconia, or titania. The method for producing the laminated inductor according to claim 1 or 2.
4. A method for manufacturing a laminated inductor described in any one of claims 1 to 3, wherein in the inter-conductor region of the laminate after the heat treatment process, a plurality of the metal magnetic particles are bonded by a bonding material.
5. A method for manufacturing a laminated inductor as described in Claim 4, wherein the bonding material includes the resin contained in the laminate, or the resin which has undergone the heat treatment process.
6. A method for manufacturing a laminated inductor as described in claim 4, wherein the bonding material includes a thermosetting resin.
Citation Information
Patent Citations
Composite magnetic material, magnetic element and manufacturing method of them
JP2002305108A
Method of manufacturing dust core
JP2011035005A
Dust core and manufacturing method thereof
JP2011233860A
Multilayer inductor
JP2017092431A
Coil component and manufacturing method thereof
JP2017228768A