Spunbond nonwoven fabric and tile carpet using same
By optimizing the properties of recycled polyester filaments, a spunbond nonwoven fabric with enhanced mechanical properties and cost savings is produced, addressing the challenges of using recycled materials in nonwoven fabrics.
Patent Information
- Application Number
- JP2022558299
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-18
- Filing Date
- 2021-02-19
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-02-19
AI Technical Summary
The use of recycled polyester raw materials in nonwoven fabrics is hindered by the presence of foreign substances such as additives and adhesives in waste materials, leading to deteriorated physical properties and increased costs.
A spunbond nonwoven fabric is produced using a mixed yarn of recycled polyester filaments with specific melting points and optimized intrinsic viscosity, crystallization temperature, and reduced foreign matter content, enhancing spinnability and mechanical properties.
The resulting nonwoven fabric achieves superior mechanical properties and cost-effectiveness by reusing waste materials, maintaining or exceeding the performance of nonwoven fabrics made from pure polyester while reducing raw material costs.
Smart Images

Figure 0007560569000003 
Figure 0007560569000001 
Figure 0007560569000002
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to Korean Patent Application No. 10-2020-0039114 filed on March 31, 2020, and Korean Patent Application No. 10-2021-0022107 filed on February 18, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a spunbond nonwoven fabric for use as a base fabric (base fabric) of a highly functional tile carpet, and to a tile carpet using the same. [Background technology]
[0003] Nonwoven fabrics are products made by arranging filaments in a planar fashion, and are broadly divided into monofilament nonwoven fabrics and long-fiber nonwoven fabrics depending on the length of the filaments. Monofilament nonwoven fabrics are products made by arranging short fibers of 5 mm or less in a planar fashion and entangling the fibers or bonding them with resin, and are characterized by their high elongation. Long-fiber nonwoven fabrics are products made by arranging unbroken fibers in a planar fashion and entangling the fibers or bonding them with resin, and are characterized by their high strength.
[0004] Long fiber nonwoven fabrics, which have the advantage of being strong, are mainly used in construction and civil engineering applications, and have recently been expanded to be used in the interior and exterior materials of automobiles in line with the trend toward lighter automobile materials. Long fiber nonwoven fabrics, which have the same strength as interior materials in the form of woven fabrics or monofilament nonwoven fabrics that were previously used, but are lighter in weight, are being used, and the main product groups in which they are used include carpet tiles, automotive flooring materials (car bets), under covers, and headliner products.
[0005] In the case of long-fiber nonwoven fabrics, by reusing waste materials such as renewable polyester plastics, nonwoven fabrics containing recycled polyester raw materials have been developed that have excellent basic physical properties of nonwoven fabrics, such as tensile strength, while contributing to the reuse of resources and the prevention of environmental pollution. Applications of these nonwoven fabrics are expanding to include nonwoven fabrics for filters and nonwoven fabrics for carpet base fabrics.
[0006] However, the use of recycled polyester raw materials poses problems such as reduced properties (chip agglomeration, poor spinnability, and reduced physical properties of nonwoven fabric) due to differences in the chemical composition of additives and adhesives, as well as the inclusion of a large amount of foreign matter, contained in nonwoven fabric waste. Summary of the Invention [Problem to be solved by the invention]
[0007] In order to solve the above problems, this specification provides a spunbond nonwoven fabric that has a low content of foreign matter, has optimized physical properties as the raw material, and is made by using recycled polyester raw materials that reuse renewable polyester plastic waste, and has excellent basic physical properties as the nonwoven fabric, and is suitable for use as a base fabric for tile carpets, and a manufacturing method thereof.
[0008] The present specification also provides a tile carpet using the spunbond nonwoven fabric. [Means for solving the problem]
[0009] In this specification, The present invention includes a fiber web of a mixed yarn of a first filament made of recycled polyester having a melting point of 255°C or more and a second filament made of a low-melting point copolyester having a melting point 30°C or more lower than that of the first filament, The recycled polyester contains a recycled material of a waste polyester polymer obtained using a monomer composition having a ratio of diethylene glycol to ethylene glycol of 1.30 or less, has an intrinsic viscosity (IV) of 0.60 to 0.80 dl / g, and has a crystallization temperature of 175°C or more and less than 185°C. Provides a spunbond nonwoven fabric.
[0010] The present specification also provides a tile carpet comprising the spunbond nonwoven fabric as a base fabric.
[0011] Hereinafter, a spunbond nonwoven fabric that can be used as a tile carpet base fabric according to an embodiment of the present invention and a method for producing the same will be described in detail.
[0012] Prior to this, unless expressly stated otherwise in this specification, the terminology used is for the purpose of referring to particular embodiments only and is not intended to limit the invention.
[0013] As used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates to the contrary.
[0014] As used herein, the meaning of "comprising" is to embody certain features, regions, integers, steps, operations, elements, components and / or components, and does not exclude the presence or addition of other certain features, regions, integers, steps, operations, elements, components and / or groups.
[0015] In this specification, terms including ordinal numbers, such as "first" and "second," are used for the purpose of distinguishing one component from another component, and are not limited by the ordinal number. For example, within the scope of the present invention, a first component may be named a second component, and similarly, a second component may be named a first component.
[0016] The present inventors have confirmed that it is possible to provide a spunbond nonwoven fabric which satisfies the basic physical properties of tile carpets, such as sound absorption performance and pull-out strength, and which has excellent basic nonwoven properties and enables cost reduction by optimizing the raw material physical properties of the recycled material when recycling waste materials such as recyclable polyester plastics, and thus completed the present invention.
[0017] In other words, even when conventional recycled polyester raw materials are used, the properties are deteriorated due to the presence of foreign matter such as additives and adhesives contained in nonwoven fabric waste, so the objective of this invention is to solve this problem.
[0018] Therefore, the present invention aims to manufacture a spunbond nonwoven fabric with excellent basic properties by using recycled polyester raw material with low foreign matter content and improved raw material properties. In addition, the spunbond nonwoven fabric according to the present invention has physical properties at a level equal to or higher than those of nonwoven fabrics using pure polyester raw materials, and can improve price competitiveness by reducing raw material costs by reusing waste materials.
[0019] The present invention will be described in detail below.
[0020] Spunbond nonwoven fabric and its manufacturing method According to one embodiment of the present invention, there may be provided a spunbond nonwoven fabric comprising a fiber web of a mixed yarn of a first filament made of recycled polyester having a melting point of 255°C or more and a second filament made of a low melting point copolyester having a melting point 30°C or more lower than that of the first filament, the recycled polyester comprising a recycled material of a waste polyester polymer obtained using a monomer composition having a ratio of diethylene glycol to ethylene glycol of 1.30 or less, the intrinsic viscosity (IV) being 0.60 to 0.80 dl / g, and the crystallization temperature being 175°C or more and less than 185°C.
[0021] The present invention relates to a method for producing a spunbond nonwoven fabric by optimizing the physical properties of recycled polyester raw materials, which improves spinnability and operability while also providing excellent mechanical properties such as tensile strength and tensile elongation.
[0022] Specifically, the present specification is characterized by using recycled polyester raw material with low foreign matter content and excellent physical properties. The recycled polyester raw material is optimized in terms of crystallization temperature, number of foreign matter, etc., so that filaments obtained using the recycled polyester raw material can provide a nonwoven fabric with high thickness without reducing physical properties. Therefore, the present specification provides a spunbond nonwoven fabric and a manufacturing method thereof that has excellent mechanical properties such as room temperature properties (tensile strength, tensile elongation) and can be used as a base fabric for finished tile carpets.
[0023] The spunbond nonwoven fabric is provided by using a first filament containing a certain amount of recycled polyester having the above-mentioned physical properties, and a second filament obtained from a low melting point copolyester raw material having a melting point 30° C. lower than that of the first filament. In particular, the spunbond nonwoven fabric uses a recycled polyester raw material that is adjusted to have a certain range of crystallization temperature and minimizes the average foreign matter content when recycling polyester waste, so that the physical properties of the final spunbond nonwoven fabric are at least as good as those of conventional products, providing excellent effects in cost reduction and price competitiveness.
[0024] In addition, when pure polyester raw material is used as the first filament, even if a spunbond with certain physical properties is provided, the cost of using the pure raw material may increase. However, in this specification, by using the recycled raw material as the first filament, it is possible to provide a spunbond nonwoven fabric with physical properties equal to or higher than those of a spunbond nonwoven fabric using pure polyester, while also achieving cost reduction effects.
[0025] The spunbond nonwoven fabric according to one embodiment of the invention will be described in more detail below.
[0026] The spunbond nonwoven fabric contains two types of raw materials having different melting temperatures as first filaments and second filaments.
[0027] Specifically, the spunbond nonwoven fabric may be prepared by forming a web of two types of filaments, including a first filament made of recycled polyester having a melting point of 255°C or more and a second filament obtained from a copolyester raw material having a melting point of 220°C or less, in the form of a mixed spun yarn (Matrix & Binder) based on the weight of the entire nonwoven fabric, and then using a fiber-opening method.
[0028] In particular, the first filament comprises recycled polyester obtained by recycling renewable polyester plastic waste, and is made of the recycled polyester raw material without the addition of other substances.
[0029] The raw material used to provide the recycled polyester is characterized in that a waste polyester polymer is used, which is obtained by using a monomer composition in which the monomer ratio of diethylene glycol to ethylene glycol, specified among the monomers used in the production of the polyester polymer, is adjusted to 1.3 or less. The monomer ratio can be maintained the same in the recycled polyester raw material. Therefore, the ratio of diethylene glycol to ethylene glycol in the recycled polyester raw material may be 1.3 or less.
[0030] In addition, the recycled polyester may be one that has been recycled by optimizing its physical properties so as to satisfy specific crystallization temperature and intrinsic viscosity and minimize the average number of foreign particles.
[0031] In other words, by recycling waste polyester polymers with the adjusted monomer ratio, the physical properties of the raw material can be optimized as described above, the content of foreign matter can be reduced, and a spunbond nonwoven fabric with excellent basic properties of nonwoven fabrics such as spinnability, tensile strength, and tensile elongation can be provided. In particular, by using recycled polyester satisfying the above-mentioned physical properties as the first filament, a nonwoven fabric with excellent price competitiveness can be provided by providing a cost saving effect while satisfying physical properties equivalent to or better than those of nonwoven fabrics using pure polyester raw materials.
[0032] Specifically, the intrinsic viscosity (IV) of the recycled polyester raw material contained in the first filament may be 0.60 to 0.80 dl / g. If the intrinsic viscosity of the recycled polyester is less than 0.60 dl / g, there is a disadvantage that the operability is poor due to problems such as filament breakage, and the effect of improving the mechanical properties of the nonwoven fabric by producing low-viscosity filaments is minimal. In addition, if the intrinsic viscosity of the recycled polyester is 0.80 dl / g or more, problems in the process may occur due to an excessive increase in the internal pressure of the extruder and the pressure of the spinning nozzle during the melt extrusion process.
[0033] The ratio of diethylene glycol to ethylene glycol (DEG / EG) may be 1.3 or less, or 0.5 to 1.3, or 1.2 to 1.3, and if the ratio is 1.3 or more, the increase in amorphous regions reduces the crystallinity of the fibers, resulting in problems such as a decrease in the physical properties of the final nonwoven fabric and uneven fineness. In addition, the monomer ratio may be 1.3 or less, but if the ratio is too low, such as 0.5 or less, the reactivity of polymer formation using the monomers decreases, making it impossible to produce polyester.
[0034] In addition, the crystallization temperature may be 175°C or higher and 185°C or 175 to 180°C. If the temperature is 175°C or lower, there is a problem that the fibers cannot be sufficiently cooled in the fiber cooling process and are stretched, resulting in poor operability such as a sticky phenomenon, and if the temperature is 185°C or higher, there is a problem that the fibers are cut in the high-speed, high-pressure stretching process due to overcooling.
[0035] In addition, the average number of foreign objects having a size of 1.0 to 10.0 μm in the recycled polyester contained in the first filament may be 10 or less, or 2 to 9. If the average number of foreign objects is 10 or more, a phenomenon of chip aggregation may occur, resulting in poor spinnability and reduced physical properties of the nonwoven fabric.
[0036] In addition, the ratio of diethylene glycol to ethylene glycol contained in the recycled polyester may be 1.30 or less. The recycled polyester raw material may contain an average of 10 or less foreign objects having a size of 1.0 to 10.0 μm based on the total weight of the recycled polyester.
[0037] Accordingly, as one example of the invention, the recycled polyester contained in the first filament simultaneously satisfies the conditions that the intrinsic viscosity (IV) is 0.60 to 0.80 dl / g and the crystallization temperature is 175° C. or more and less than 185° C. As described above, the recycled polyester may contain a recycled material of a waste polyester polymer produced using a monomer composition in which the ratio of diethylene glycol to ethylene glycol is 1.30 or less.
[0038] Such a spunbond nonwoven fabric has a weight per unit area of 90 g / m 2 When so, the thickness may be 0.35 mm to 0.40 mm.
[0039] Therefore, according to this specification, by using a certain ratio of the first filament containing the recycled raw material and the second filament described later, it is possible to provide a spunbond nonwoven fabric for tile carpet base fabric, which has excellent spinnability when producing the nonwoven fabric, improves tensile strength and tensile elongation, and has a cost-saving effect by reusing waste materials such as polyester plastics.
[0040] Meanwhile, as described above, the above parameter properties can be achieved by adjusting the range of the monomer content for producing the polyester before recycling.
[0041] Specifically, the recycled polyester may be a recycled raw material of well-known waste polyester. For example, the recycled polyester may be a polyester copolymer containing post-industrial recycled (PIR) polyethylene terephthalate, post-consumer recycled (PCR) polyethylene terephthalate, or a mixture thereof, in the form of chips, which are recycled from waste materials in the manufacturing process of well-known polyesters. In addition, these materials are recycled from waste polyesters in which the ratio of diethylene glycol / ethylene glycol is adjusted to 1.3 or less, and may satisfy all physical property conditions, including crystallization temperature, intrinsic viscosity, and an average number of foreign bodies of 10 or less. The waste polyester may include waste polyesters such as waste fibers or waste containers, which are manufactured in which the ratio of diethylene glycol to ethylene glycol is 1.3 or less. In addition, the material may be a polyester copolymer recycled by a method well known in the art, as long as the monomer ratio is adjusted.
[0042] Here, the first filament may contain a copolymer of adipic acid (AA), isophthalic acid (IPA), neopentyl glycol (NPG), butadiene (BD), or the like, depending on the recycled raw material.
[0043] As a specific example, the recycled polyester contained in the first filament may include recycled raw materials of a waste polyester copolymer of a dicarboxylic acid selected from the group consisting of terephthalic acid, adipic acid (AA) and isophthalic acid (IPA) and a diol compound selected from the group consisting of neopentyl glycol (NPG), diethylene glycol and ethylene glycol.
[0044] In one example, the dicarboxylic acid may be terephthalic acid and isophthalic acid, and the diol compound may be diethylene glycol and ethylene glycol. Therefore, the recycled polyester may be a recycled raw material for a waste polyester copolymer having a monomer composition containing 45 to 75 parts by weight of isophthalic acid (IPA), 47 to 58 parts by weight of ethylene glycol (EG), and 69 to 74 parts by weight of diethylene glycol, relative to 100 parts by weight of terephthalic acid (TPA). The waste polyester copolymer may be a waste generated in a polyester manufacturing process, produced in such a manner that the ratio of diethylene glycol to ethylene glycol is 1.30 or less.
[0045] Therefore, the recycled polyester used as the first filament raw material may include chips recycled from the waste, and the chip-shaped recycled polymer raw material may have the above-mentioned intrinsic viscosity (IV) of 0.60 to 0.80 dl / g, a crystallization temperature of 175°C or higher and lower than 185°C, and an average number of foreign objects having a size of 1.0 to 10.0 μm relative to the total weight of the recycled polyester may be 10 or less.
[0046] In another embodiment, the recycled polyester contained in the first filament may be a recycled material of waste polyethylene terephthalate obtained using a monomer composition having an intrinsic viscosity (IV) of 0.60 to 0.80 dl / g, a crystallization temperature of 175°C or more and less than 185°C, and a ratio of diethylene glycol to ethylene glycol of 1.30 or less, and may be recycled polyethylene terephthalate having an average number of foreign objects having a size of 1.0 to 10.0 μm of 10 or less based on the total weight of the recycled polyethylene terephthalate. As described above, the polyethylene terephthalate is a recycled raw material of waste polyester polymer obtained by polymerizing 100 parts by weight of terephthalic acid (TPA), 45 to 75 parts by weight of isophthalic acid (IPA), 47 to 58 parts by weight of ethylene glycol (EG), and 69 to 74 parts by weight of diethylene glycol.
[0047] On the other hand, the filaments spun into the mixed fiber yarn can be sufficiently drawn using a high-pressure air drawing device so that the spinning speed is 4,500 to 5,500 m / min, thereby producing a filament having a normal fineness of 5 to 10 denier in the case of the first filament, and a filament having a normal fineness of 2 to 5 denier in the case of the second filament.
[0048] The filament fibers thus produced are fixed in a web shape on a conveyor net, and then the thickness of the nonwoven fabric is adjusted by a calendaring process using a heated smooth roll. The nonwoven fabric is then bonded using hot air at a temperature similar to the melting point of the second filament to produce the nonwoven fabric.
[0049] Specifically, the spunbond is provided by the following method.
[0050] In one example, a method for producing a spunbond nonwoven fabric is provided, comprising the steps of: a) spinning a first filament made of a polyester and a recycled polyester, each having a melting point of 255°C or more, and a second filament made of a copolyester having a melting point 30°C or more lower than that of the first filament, and drawing the resulting mixture to produce a mixed yarn; b) laminating the mixed yarn to form a fiber web; and c) performing a calendaring process and heat bonding on the fiber web.
[0051] The step a) comprises preparing a mixed yarn using two types of filaments having different melting points.
[0052] More specifically, the recycled polyester contained in the first filament may be a recycled polyethylene terephthalate chip having a melting point of 255°C or higher, an intrinsic viscosity (IV) of 0.60 to 0.80 dl / g, a crystallization temperature of 175°C or higher and lower than 185°C, and an average number of foreign particles having a size of 1.0 to 10.0 μm of 3 to 10.
[0053] Such recycled polyester is a recycled raw material obtained by recycling waste polyester obtained using a monomer composition having a ratio of diethylene glycol to ethylene glycol of 1.3 or less. As an example, the recycled polyester may be prepared by pulverizing waste polyester produced with a ratio of diethylene glycol to ethylene glycol of 1.3 or less, feeding the pulverized polyester into an extruder, melt extruding the pulverized polyester, and adjusting the physical properties to have the intrinsic viscosity, crystallization temperature, and average number of foreign matters, to produce chips. The size of the pulverized waste polyester is not particularly limited, and the pulverization may be performed by a method well known in the art, and a washing process may be further performed before pulverization.
[0054] Also, the second filaments may include a copolyester having a melting point 30° C. or more lower than that of the first filaments. Thus, the second filaments may use a copolyester having a melting point 30° C. or more or a melting point of 160° C. to 180° C., which includes a copolymer of adipic acid (AA), isophthalic acid (IPA), neopentyl glycol (NPG), or a mixture thereof, compared to that of the first filaments. However, the monomers constituting the copolyester are not limited to the above types, and any monomer may be selected and used without limitation as long as it can provide a polyester copolymer having the specific melting point range.
[0055] The content ratio of the first filaments to the second filaments can be controlled by controlling the amount of molten polymer discharged or by changing the design of the spinneret.
[0056] For example, the blended yarn may include 50-95% by weight, or 60-95% by weight, or 80-95% by weight of a first filament, and 5-50% by weight, or 5-40% by weight, or 5-20% by weight of a second filament. For example, the content ratio of the first filament to the second filament may be 90:10% by weight.
[0057] Meanwhile, a spunbonded nonwoven fabric can be provided by carrying out a process including: b) laminating the mixed yarn to form a fiber web; and c) performing a calendar process and thermal bonding on the fiber web.
[0058] The filaments spun into a blended spun yarn as described above are sufficiently stretched using a high-pressure air stretching device so that the spinning speed is 4,500 to 5,500 m / min, so that the first filament, which is the recycled raw material, has a fineness of 5 to 10 denier, and the second filament, which has a lower melting point than the first filament, has a fineness of 2 to 5 denier.
[0059] The spunbond nonwoven fabric may be obtained under spinning conditions in which the pressure of the spin pack is in the range of 1,600 to 2,500 psi. If the pressure of the spin pack is less than 1,600 psi, the fibers may not come out straight but may come out in a broken manner, which may cause breakage of the fibers (filaments). On the other hand, if the pressure of the spin pack is more than 2,500 psi, the polymer pressure inside the pack is high, so that a pack leak phenomenon may occur in which the polymer cannot pass through the nozzle and is discharged to the outside. Therefore, only when the pressure of the spin pack is within the above-mentioned range can a spunbond nonwoven fabric containing high-quality fibers (filaments) without poor shape or breakage be provided.
[0060] In addition, the step of manufacturing the spunbond nonwoven fabric includes a calendering process using a smooth roll and a hot air process under temperature conditions similar to or corresponding to the melting point of the second filament.
[0061] As an example, the filament fibers produced by the above method are fixed in a web shape on a conveyor net, and then the thickness of the nonwoven fabric is adjusted through a calendar process using a heated smooth roll, and the nonwoven fabric is then bonded using hot air at a temperature similar to the melting point of the second filament to produce a nonwoven fabric.
[0062] The calendering process can be carried out at a temperature of 150 to 200° C., and the thickness of the nonwoven fabric can be adjusted by this process. For example, in order to be suitable for use as a base fabric for tile carpets, the weight per unit area is set to 90 g / m2 in this specification. 2 In this case, the calendering process can be carried out so that the spunbond thickness is 0.35 mm to 0.40 mm.
[0063] The thermal bonding step can be performed under hot air conditions at a temperature 0 to 10° C. higher than the melting point of the low melting point copolyester constituting the second filaments. Therefore, the hot air process can be performed at a temperature corresponding to the melting point of the second filaments, for example, in the range of 160° C. to 180° C.
[0064] Carpet tiles In the present specification, the above-mentioned method can provide a spunbond nonwoven fabric suitable for use as a base fabric for a tile carpet. Also, in the present specification, by using the spunbond nonwoven fabric as a base fabric for a tile carpet, a tile carpet having excellent sound absorption properties and pull-out strength can be provided.
[0065] In one example, the spunbond nonwoven fabric may have a tensile strength of 15 kg.f / 5 cm or more and a tensile elongation of 15% or more, as measured based on the method of KS K ISO-9073-3.
[0066] Therefore, according to another embodiment of the present invention, there is provided a tile carpet comprising a spunbond nonwoven fabric having the above physical properties as a base fabric.
[0067] In the present invention, the nonwoven fabric provided by the above-mentioned method can be used to provide a tile carpet by carrying out tufting, back coating and cutting steps according to well-known methods.
[0068] According to one example of the invention, the nonwoven fabric is subjected to a tufting process (a process of implanting yarn into the nonwoven fabric) with a loop type polypropylene BCF (Bulky Continuous Filament) Yarn of about 3,000 Denier / 150 Filament on the front surface, with a gauge (the distance between needles in a tufting machine is expressed in inches as a unit indicating the density of the needles, and the gauge determines the density of the tufted carpet in the width direction) of about 1 / 10 and a stitch (the density of the tufted carpet in the length direction) of about 10.5. Then, a tufted nonwoven fabric is applied to the back surface with a unit weight of about 40 g / m2. 2 The nonwoven fabric is made of glass fibers, and the 2 The impregnated product is then heat cured in a heat chamber at about 180°C, and the final process is cutting (size: 50cm x 50cm), producing a high-performance finished carpet tile with a pull-out strength (strength of pulling the loop after tufting of the Loop Type) of about 2.0kgf. Effect of the Invention
[0069] The present invention optimizes the physical properties (crystallization temperature, number of foreign objects) of recycled polyester raw materials when recycling waste materials such as renewable polyester plastics, and can produce nonwoven fabrics that have physical properties equivalent to or better than those of nonwoven fabrics made using only pure polyester raw materials, and that are price-competitive in terms of cost savings, etc. In addition, even when recycled polyester raw materials are used, the present invention can produce high-performance spunbond nonwoven fabrics without the conventional problems of chip aggregation, poor spinnability, and deterioration of nonwoven fabric physical properties. [Brief description of the drawings]
[0070] [Figure 1] 1 shows the appearance of the calendar rolls during the production of a nonwoven fabric according to Comparative Example 3 (a) and the surface of a nonwoven fabric sheet (b). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0071] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.
[0072] [Preparing materials] In the following examples, the recycled polyester used as the first filament is a chip-shaped recycled raw material (hereinafter, recycled PET) recycled from polyethylene terephthalate (PET) waste, which is produced by esterification at a temperature of about 220 to 240° C. using a monomer composition containing 45 to 75 parts by weight of isophthalic acid (IPA), 47 to 58 parts by weight of ethylene glycol (EG), and 69 to 74 parts by weight of diethylene glycol, relative to 100 parts by weight of terephthalic acid (TPA). The recycled polyester chips are produced in chip form by crushing the polyethylene terephthalate waste, feeding it into a twin-screw extruder, and melt extruding it.
[0073] Here, the recycled PET used had a monomer content range adjusted to satisfy the ratio of diethylene glycol to ethylene glycol (i.e., diethylene glycol / ethylene glycol ratio) in the range of 1.21:1 to 1.30:1 and an intrinsic viscosity of 0.61 to 0.80 dl / g, as shown in Table 1, and the average number of foreign particles having a size of 1.0 to 10.0 μm was adjusted to 10 or less based on the total weight of the recycled PET.
[0074] In addition, the recycled PET used in the comparative example is a recycled raw material made from PET waste produced in a manner that exceeds the range of monomer usage, and as shown in Table 1, the intrinsic viscosity, crystallization temperature, diethylene glycol / ethylene glycol ratio of the waste, and average number of foreign objects deviate from this composition.
[0075] [Example 1] The first filament was made of recycled polyester (recycled PET) having an intrinsic viscosity (IV) of 0.61 dl / g, a crystallization temperature of 176.5°C, a diethylene glycol / ethylene glycol ratio of 1.27, an average number of foreign bodies of 5.6, and a melting point of 255°C. The second filament was made of a copolyester having a melting point of approximately 220°C. These were each melted at a spinning temperature of approximately 280°C using a continuous extruder, and then mixed and spun so that the content ratio of the first filament to the second filament was 90:10 wt.%, and the extrusion rate and the number of capillaries in the spinneret were adjusted so that the average fineness of the first filament produced by drawing was 8.5 denier.
[0076] Next, the continuous filaments discharged from the capillaries were solidified with cooling air, and then drawn using a high-pressure air drawing device at a spinning speed of 5,000 m / min to produce filament fibers. The pressure range of the spin pack at this time was as shown in Table 2.
[0077] Next, the produced filament fibers are laminated in the form of a web on a conveyor net by a conventional fiber spreading method, and the laminated web is given smoothness and appropriate thickness by a calendaring process using a heated smooth roll.
[0078] The laminated filaments are heat-bonded with hot air at a temperature of about 220°C, resulting in a weight per unit area of 90 g / m 2 A spunbond nonwoven fabric having a thickness (thickness) of 0.33 mm was produced.
[0079] [Example 2] The first filament was made of recycled polyester raw material (recycled PET) having an IV (intrinsic viscosity) of 0.65 dl / g, a crystallization temperature of 175.8°C, a diethylene glycol / ethylene glycol ratio of 1.24, and an average number of foreign objects of 3.1. The first filament was adjusted to the same weight and thickness per unit area to produce a spunbond nonwoven fabric.
[0080] [Example 3] The first filament was made of recycled polyester raw material (recycled PET) having an IV of 0.73 dl / g, a crystallization temperature of 176.0°C, a diethylene glycol / ethylene glycol ratio of 1.21, and an average number of foreign bodies of 2.7, in the same manner as in Example 1. The weight and thickness per unit area were adjusted to be the same, and a spunbond nonwoven fabric was manufactured.
[0081] [Example 4] The first filament was made of recycled polyester material (recycled PET) having an IV of 0.80 dl / g, a crystallization temperature of 176.3°C, a diethylene glycol / ethylene glycol ratio of 1.30, and an average number of foreign objects of 8.4. The first filament was adjusted to the same weight and thickness per unit area to produce a spunbond nonwoven fabric.
[0082] [Comparative Example 1] The same method as in Example 1 was used to manufacture the first filament, which was made of recycled polyester raw material (recycled PET) with an IV of 0.55 dl / g, a crystallization temperature of 176.3°C, a diethylene glycol / ethylene glycol ratio of 1.27, and an average number of foreign objects of 5.1. The weight and thickness per unit area were adjusted to be the same, and a spunbond nonwoven fabric was manufactured.
[0083] [Comparative Example 2] The first filament was made of recycled polyester raw material (recycled PET) with an IV of 1.00 dl / g, a crystallization temperature of 175.9°C, a diethylene glycol / ethylene glycol ratio of 1.21, and an average number of foreign bodies of 1.1, as in Example 1. The first filament was adjusted to the same weight and thickness per unit area to produce a spunbond nonwoven fabric.
[0084] [Comparative Example 3] The first filament was made of recycled polyester raw material (recycled PET) having an IV of 0.68 dl / g, a crystallization temperature of 166.4°C, a diethylene glycol / ethylene glycol ratio of 1.22, and an average number of foreign objects of 2.9. The first filament was adjusted to the same weight and thickness per unit area to produce a spunbond nonwoven fabric.
[0085] [Reference example 1] The same method as in Example 1 was used to manufacture the first filament, which was made of recycled polyester raw material (recycled PET) with an IV of 0.75 dl / g, a crystallization temperature of 176.2°C, a diethylene glycol / ethylene glycol ratio of 1.37, and an average number of foreign objects of 12.4. The weight and thickness per unit area were adjusted to be the same, and a spunbond nonwoven fabric was manufactured.
[0086] [Table 1]
[0087] [Experimental Example] For each of the Examples and Comparative Examples, physical properties were measured by the measurement methods for the following evaluation items, and the results are shown in Table 2.
[0088] Experimental Example 1: Spinnability (Pack pressure) A Dynisco pressure measurement sensor (model name: TB422J-9 / 18-231) was used.
[0089] Specifically, a spinning pack pressure measuring sensor was attached to the rear stage of the gear pump, and the pack pressure was confirmed when the polymer was inserted and discharged under the pack pressure. The normal pack pressure control range is 1,600 to 2,500 psi.
[0090] Experimental Example 2: Tensile strength (kg.f / 5cm) and tensile elongation (%) The KS K ISO-9073-3 (Cut Strip) method was used.
[0091] Specifically, a test piece measuring 5 cm wide x 20 cm long was clamped between a jig measuring 5 cm x 5 cm at the top and bottom and then measured at a tensile speed of 200 mm / min using an INSTRON measuring device.
[0092] Experimental Example 3: Measurement of the number of filament detachments and yarn breakages After 24 hours of observation, the number of broken filaments and the number of detached cops were counted.
[0093] [Table 2]
[0094] As can be seen from the results in Table 2, in comparison with Comparative Examples 1 to 3 and Reference Example 1, Examples 1 to 4 of the present invention were superior in spinnability, tensile strength, and tensile elongation, as the intrinsic viscosity, crystallization temperature, diethylene glycol / ethylene glycol ratio, and average number of foreign matter particles for the first filament (recycled polyester raw material) were all specified.
[0095] In contrast, in Comparative Example 1, the intrinsic viscosity of the first filament was lower than the range of the present application, so spinnability was poor and spinning was impossible due to filament breakage, so tensile strength and tensile elongation could not be measured. In Comparative Example 2, the intrinsic viscosity of the first filament was too high compared to the range of the present application, so the pressure in the spin pack increased excessively, which caused leakage and made spinning impossible.
[0096] In addition, although the pressure in Comparative Example 3 and Reference Example 1 was within the control range of the pressure for a normal spinnable pack, the crystallization temperature of the first filament was excessively low compared to the present application, or the content of foreign matter was high, making it difficult to measure the physical properties. In particular, as shown in Figure 1, in Comparative Example 3, the stickiness of the calendar roll during the production of the nonwoven fabric was severe (Figure 1(a)), and the appearance of the nonwoven fabric surface due to this caused poor sheet quality due to undrawn yarn (Figure 1(b)). In Comparative Example 4, many filament detachments and yarn breakages occurred, and spinning was impossible due to cop detachment, making it impossible to measure the tensile strength and tensile elongation.
Claims
1. The present invention includes a fiber web of a mixed yarn of a first filament made of a recycled polyester having a melting point of 255° C. or more and a second filament made of a low-melting point copolyester having a melting point 30° C. or more lower than that of the first filament, The recycled polyester comprises a recycled material of a waste polyester polymer obtained using a monomer composition having a ratio of diethylene glycol to ethylene glycol of 0.5 to 1.30, has an intrinsic viscosity (IV) of 0.60 to 0.80 dl / g, and has a crystallization temperature of 175°C or more and less than 185°C. Spunbond nonwoven fabric.
2. The spunbond nonwoven fabric of claim 1, wherein the recycled polyester comprises a recycled material of waste polyester polymer having a monomer composition including 45 to 75 parts by weight of isophthalic acid (IPA), 47 to 58 parts by weight of ethylene glycol (EG), and 69 to 74 parts by weight of diethylene glycol, relative to 100 parts by weight of terephthalic acid (TPA).
3. 2. The spunbond nonwoven fabric of claim 1, wherein the combined yarn comprises: 50-95% by weight of a first filament; and 5-50% by weight of a second filament.
4. 2. The spunbond nonwoven fabric according to claim 1, wherein the first filaments have an average fineness of 5 to 10 denier, and the second filaments have an average fineness of 2 to 5 denier.
5. The spunbond nonwoven fabric has a weight per unit area of 90 g / m 2 The spunbond nonwoven fabric of claim 1, wherein the thickness is 0.35 mm to 0.40 mm.
6. 10. The spunbond nonwoven fabric of claim 1, obtained at spinning conditions with a spin pack pressure range of 1,600 to 2,500 psi.
7. The spunbond nonwoven fabric according to claim 1, having a tensile strength of 15 kg.f / 5 cm or more and a tensile elongation of 15% or more, as measured based on the method of KS K ISO-9073-3.
8. A tile carpet comprising the spunbond nonwoven fabric according to any one of claims 1 to 7 as a base fabric.
Citation Information
Patent Citations
Spun bond non-woven fabric made of regenerated polyethylene terephthalate resin and method for producing the same
JP2002194653A
Fluid-permeable structured fiber web
JP2014509530A
Polyethylene terephthalate composition for producing melt-blown nonwoven fabric, and melt-blown nonwoven fabric comprising the same
JP2015010294A