Resin composition for monofilament and use thereof, and method for producing monofilament
A poly(3-hydroxyalkanoate) resin composition is used to create a monofilament with high strength and elongation for artificial turf, addressing the environmental concerns of microplastic pollution by providing a durable and biodegradable solution.
Patent Information
- Application Number
- PCT/JP2024/011960
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
The environmental impact of discarded petroleum-derived plastics, particularly artificial turf that breaks down into microplastics in coastal waters, necessitates a biodegradable and durable alternative with high strength and elongation for applications like artificial turf.
A poly(3-hydroxyalkanoate) resin composition with a melting point peak temperature of 140°C or higher and a crystal fusion enthalpy of 65 J/g or less is used to create a monofilament with high tensile strength and elongation, manufactured through extrusion and stretching, suitable for artificial turf applications.
The resulting monofilament exhibits high strength and elongation, enabling it to withstand stress without breaking, while being biodegradable and environmentally friendly, thus addressing the issue of microplastic pollution from artificial turf.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000029_0000
Abstract
Description
Resin composition for monofilament and its use, and method for producing monofilament
[0001] The present invention relates to a monofilament resin composition containing a poly(3-hydroxyalkanoate)-based resin, a monofilament, artificial turf, and a method for producing the monofilament.
[0002] A large amount of petroleum-derived plastics is discarded every year, and the resulting lack of landfill sites and environmental pollution are becoming serious issues. In recent years, microplastics have also become a major problem in the marine environment.
[0003] In particular, recent surveys have found large amounts of broken pieces of artificial turf in the form of microplastics in nearby waters, making countermeasures urgently needed. It is thought that artificial turf breaks down when people walk on it, and is washed away by rainwater and reaches the sea.
[0004] Poly(3-hydroxyalkanoate) resins have excellent seawater degradability and are materials that can solve environmental problems caused by discarded plastics. Patent Document 1 describes films and fibers that have been imparted with elasticity by stretching aliphatic polyesters.
[0005] International Publication No. 2020 / 230807
[0006] Patent Document 1 discloses stretchable films and fibers that contain an aliphatic polyester copolymer and have a specific crystal structure and degree of orientation. However, since the films and fibers are produced by first obtaining a molded body and then performing a stretching treatment, there is room for improvement in terms of industrial productivity.
[0007] In view of the above-mentioned current situation, an object of the present invention is to provide a monofilament containing a poly(3-hydroxyalkanoate)-based resin composition and having high strength and elongation.
[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that by using a poly(3-hydroxyalkanoate)-based resin composition having a high melting point and a low crystalline melting enthalpy, monofilaments having both high strength and elongation can be produced with good productivity, and have thus completed the present invention.
[0009] That is, the present invention relates to a resin composition for monofilaments, which contains a poly(3-hydroxyalkanoate)-based resin component, and which has a melting point peak temperature of 140°C or higher and a crystalline melting enthalpy of 65 J / g or lower in differential scanning calorimetry.
[0010] The present invention also relates to a monofilament containing the resin composition and having a fineness of 15 to 5000 dtex, a tensile strength of 0.5 to 6 cN / dtex, and a tensile elongation of 50% or more, and to an artificial turf having turf yarns planted in a base fabric, the turf yarns containing the monofilament.
[0011] The present invention further relates to a method for producing a monofilament containing the resin composition for monofilaments, which comprises the following steps (i) and (ii) in order:
[0012] (i) a step of extruding the resin composition in a molten state from a spinning nozzle, cooling it, and forming it into a raw yarn; and (ii) a step of stretching the raw yarn in at least one direction.
[0013] According to the present invention, a monofilament containing a poly(3-hydroxyalkanoate)-based resin composition and having high strength and elongation can be provided. Furthermore, the monofilament of the invention can be suitably used for applications such as artificial turf. Furthermore, by using the resin composition of the present invention, it is possible to produce the monofilament with good productivity.
[0014] FIG. 1 is a schematic diagram of a monofilament manufacturing apparatus.
[0015] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0016] The resin composition for monofilaments according to this embodiment (also referred to as "poly(3-hydroxyalkanoate)-based resin composition") is a resin composition for monofilaments that contains a poly(3-hydroxyalkanoate)-based resin component and has a melting point peak temperature of 140°C or higher and a crystalline fusion enthalpy of 65 J / g or lower in differential scanning calorimetry. (Poly(3-hydroxyalkanoate)-based resin composition) The poly(3-hydroxyalkanoate) resin composition may be a single poly(3-hydroxyalkanoate)-based resin or a mixture of two or more poly(3-hydroxyalkanoate)-based resins.
[0017] The poly(3-hydroxyalkanoate) resin component according to this embodiment preferably contains a copolymer of at least two types of 3-hydroxybutyrate units, which differ from each other in type and / or content ratio of the hydroxyalkanoate units, with other 3-hydroxyalkanoate units, because this facilitates control of the melting point and crystalline melting enthalpy, as described below. Note that the other 3-hydroxyalkanoate units refer to 3-hydroxyalkanoate units other than 3-hydroxybutyrate units.
[0018] The poly(3-hydroxyalkanoate) resin is preferably a polymer having a 3-hydroxyalkanoate unit, specifically a polymer containing a unit represented by the following general formula (1): [—CHR—CH 2 -CO-O-] (1) In the general formula (1), R is C p H 2p+1 where p is an integer of 1 to 15. Examples of R include linear or branched alkyl groups such as methyl, ethyl, propyl, methylpropyl, butyl, isobutyl, t-butyl, pentyl, and hexyl. p is preferably an integer of 1 to 10, and more preferably an integer of 1 to 8.
[0019] The poly(3-hydroxyalkanoate) resin is preferably a poly(3-hydroxyalkanoate) resin produced by a microorganism, in which all 3-hydroxyalkanoate units are contained as (R)-3-hydroxyalkanoate units.
[0020] The poly(3-hydroxyalkanoate) resin composition according to this embodiment has a melting point of 140°C or higher and a crystalline melting enthalpy of 65 J / g or lower, and the melting point and crystalline melting enthalpy are defined, for example, by differential scanning calorimetry as follows:
[0021] An aluminum pan is filled with 4 to 10 mg of a resin sample, and the resin sample is melted by heating it from 30°C to 180°C at a rate of 10°C / min using a differential scanning calorimeter under a nitrogen stream. In the endothermic curve obtained, the temperature at which the endothermic heat reaches its maximum is taken as the melting point (also referred to as the "melting point peak temperature"), and the endothermic heat calculated from the melting point peak region is taken as the crystalline melting enthalpy. The crystalline melting enthalpy is an index of the degree of crystallinity, and a low crystalline melting enthalpy means a low degree of crystallinity.
[0022] The poly(3-hydroxyalkanoate) resin preferably contains 3-hydroxyalkanoate units (particularly units represented by general formula (1)) in an amount of 50 mol % or more, more preferably 60 mol % or more, and even more preferably 70 mol % or more of the total structural units. The poly(3-hydroxyalkanoate) resin may contain only one or more types of 3-hydroxyalkanoate units as structural units of the polymer, or may contain one or more types of 3-hydroxyalkanoate units as well as other units (e.g., 4-hydroxyalkanoate units).
[0023] Examples of methods for producing the poly(3-hydroxyalkanoate) resin composition of the present invention, which exhibits the melting behavior of the present invention, such as the melting peak temperature and the crystalline melting enthalpy calculated from the melting peak, include, when the poly(3-hydroxyalkanoate) resin is a copolymer, appropriately adjusting the copolymerization ratio of each monomer constituting the copolymer; mixing a component other than the poly(3-hydroxyalkanoate) resin component, such as a plasticizer, with the poly(3-hydroxyalkanoate) resin component; and mixing at least two poly(3-hydroxyalkanoate) resins having different melting behaviors. In particular, mixing at least two polyhydroxyalkanoate resins having different melting behaviors is preferred. Specifically, mixing at least two poly(3-hydroxyalkanoate) resins having different crystalline melting enthalpies when used alone is preferred. This makes it easy to make the melting point peak temperature of the poly(3-hydroxyalkanoate) resin composition in differential scanning calorimetry analysis 140°C or higher and to make the crystalline melting enthalpy calculated from all melting peaks 65 J / g or lower.
[0024] The poly(3-hydroxyalkanoate) resin is preferably a homopolymer or copolymer containing 3-hydroxybutyrate (hereinafter sometimes referred to as 3HB) units. In particular, it is preferable that all of the 3-hydroxybutyrate units are (R)-3-hydroxybutyrate units. Furthermore, the poly(3-hydroxyalkanoate) resin is preferably a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units. The other hydroxyalkanoate units refer to hydroxyalkanoate units other than 3-hydroxybutyrate units.
[0025] Specific examples of poly(3-hydroxyalkanoate) resins include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (abbreviation: P3HB3HV), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH). , poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), etc. In particular, from the viewpoints of achieving both strength and elongation of the monofilament and productivity, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) and poly(3-hydroxybutyrate-co-4-hydroxybutyrate) are preferred.
[0026] When the poly(3-hydroxyalkanoate) resin component contains a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, the average content ratio of 3-hydroxybutyrate units and other hydroxyalkanoate units to all monomer units constituting the poly(3-hydroxyalkanoate) resin component is preferably 3-hydroxybutyrate units / other hydroxyalkanoates = 93 / 7 to 80 / 20 (mol % / mol %), more preferably 92 / 8 to 82 / 18 (mol % / mol %), and even more preferably 90 / 10 to 84 / 16 (mol % / mol %), from the viewpoint of achieving both the tensile strength and tensile elongation of the monofilament and productivity.
[0027] The average content ratio of each monomer unit in all monomer units constituting the poly(3-hydroxyalkanoate)-based resin component can be determined by a method known to those skilled in the art, for example, the method described in paragraph
[0047] of WO 2013 / 147139. The average content ratio means the molar ratio of each monomer unit in all monomer units constituting the poly(3-hydroxyalkanoate)-based resin component, and when the poly(3-hydroxyalkanoate)-based resin component is a mixture of two or more poly(3-hydroxyalkanoate)-based resins, it means the molar ratio of each monomer unit contained in the entire mixture.
[0028] When the poly(3-hydroxyalkanoate) resin component according to the present embodiment contains two or more types of copolymers of 3-hydroxybutyrate units and other hydroxyalkanoate units that differ from each other in the type and / or content ratio of the other hydroxyalkanoate units, it preferably contains a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units (hereinafter sometimes referred to as "copolymer (A)") in which the content ratio of the other hydroxyalkanoate units is 6 mol % or less, and a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units (hereinafter sometimes referred to as "copolymer (B)") in which the content ratio of the other hydroxyalkanoate units is 24 mol % or more. Copolymers of 3-hydroxybutyrate units and other hydroxyalkanoate units, in which the content of other hydroxyalkanoate units is 6 mol % or less, often have a melting point of 140°C or higher. Therefore, it is easy to adjust the melting point of a poly(3-hydroxyalkanoate)-based resin composition containing a mixture of two or more poly(3-hydroxyalkanoate)-based copolymers to 140°C or higher, and they tend to enable rapid crystallization during processing into monofilaments, and are therefore preferably used.
[0029] The upper limit of the content of other hydroxyalkanoate units in a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, in which the content of other hydroxyalkanoate units is 6 mol% or less, is preferably 5 mol% or less, more preferably 4 mol% or less, and particularly preferably 3 mol% or less, and the lower limit is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, and particularly preferably 1 mol% or more.
[0030] A copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units in which the content of other hydroxyalkanoate units is 24 mol% or more has a low degree of crystallinity or is substantially amorphous, and therefore makes it easier to adjust the crystalline fusion enthalpy of a poly(3-hydroxyalkanoate)-based resin composition containing two or more poly(3-hydroxyalkanoate)-based copolymers to 65 J / g or less, i.e., makes it easier to lower the degree of crystallinity. Therefore, it is preferable to use such a copolymer because it allows easy stretching of monofilaments and can increase the elongation of the monofilaments to 50% or more.
[0031] The content of the other hydroxyalkanoate units in the copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units is 24 mol% or more, and the lower limit of the content of the other hydroxyalkanoate units is preferably 25 mol% or more, more preferably 26 mol% or more, and particularly preferably 27 mol% or more.The upper limit is preferably 99 mol% or less, more preferably 50 mol% or less, even more preferably 40 mol% or less, and particularly preferably 30 mol% or less.
[0032] When the components of the poly(3-hydroxyalkanoate) resin composition according to the present embodiment contain a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, in which the content of other hydroxyalkanoate units is 24 mol % or more, the content of the copolymer (B) in the poly(3-hydroxyalkanoate) resin composition is preferably 20 wt % or more and 50 wt % or less, in view of rapid crystallization during processing into monofilaments and the ability to increase the elongation of the monofilaments to 50% or more.
[0033] The poly(3-hydroxyalkanoate) resin composition according to the present embodiment may further contain, in addition to the copolymer (A) and the copolymer (B), a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units (hereinafter, sometimes referred to as "copolymer (C)"), in which the content of other hydroxyalkanoate units is more than 6 mol % and less than 24 mol %.
[0034] The weight average molecular weight of the poly(3-hydroxyalkanoate) resin is not particularly limited, but is preferably 200,000 to 2,000,000, more preferably 250,000 to 1,500,000, and even more preferably 300,000 to 1,000,000, from the viewpoint of easily obtaining preferable strength and elongation.
[0035] Furthermore, when the poly(3-hydroxyalkanoate) resin component is a mixture of two or more poly(3-hydroxyalkanoate) resins, the weight-average molecular weight of each poly(3-hydroxyalkanoate) resin is not particularly limited, but from the viewpoint of easily obtaining desirable strength and elongation, the weight-average molecular weight of the entire poly(3-hydroxyalkanoate) resin component is preferably 200,000 to 2,000,000, more preferably 250,000 to 1,500,000, and even more preferably 300,000 to 1,000,000.
[0036] The weight-average molecular weight of the poly(3-hydroxyalkanoate) resin or poly(3-hydroxyalkanoate) resin component can be measured in terms of polystyrene using gel permeation chromatography (HPLC GPC system manufactured by Shimadzu Corporation) using a chloroform solution. As the column for the gel permeation chromatography, a column appropriate for measuring the weight-average molecular weight may be used.
[0037] The method for producing poly(3-hydroxyalkanoate) resins is not particularly limited, and may be a production method using chemical synthesis or a production method using a microorganism. Among these, a production method using a microorganism is preferred. Known methods can be applied to the production method using a microorganism. For example, known bacteria that produce copolymers of 3-hydroxybutyrate and other hydroxyalkanoates include Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB. In particular, with regard to P3HB3HH, in order to increase the productivity of P3HB3HH, Alcaligenes eutrophus AC32 strain (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997)) or the like into which genes encoding P3HA synthases have been introduced is more preferred, and microbial cells obtained by culturing these microorganisms under appropriate conditions and allowing P3HB3HH to accumulate within the cells are used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxyalkanoate) resin synthesis-related genes have been introduced may be used depending on the poly(3-hydroxyalkanoate) resin to be produced, or the culture conditions, including the type of substrate, may be optimized.
[0038] The method for obtaining a blend of two or more poly(3-hydroxyalkanoate)-based resins is not particularly limited, and may be a method of obtaining a blend by microbial production or a method of obtaining a blend by chemical synthesis. Alternatively, a blend may be obtained by melt-kneading three or more resins using an extruder, kneader, Banbury mixer, roll, or the like, or by dissolving two or more resins in a solvent, mixing, and drying. (Other Resins) The monofilament resin composition according to this embodiment may contain resins other than the poly(3-hydroxyalkanoate)-based resin, as long as the effects of the invention are not impaired. Examples of such other resins include aliphatic polyester-based resins such as polybutylene succinate adipate, polybutylene succinate, polycaprolactone, and polylactic acid, and aliphatic aromatic polyester-based resins such as polybutylene adipate terephthalate, polybutylene sebacate terephthalate, and polybutylene azelate terephthalate. Only one type of other resin may be included, or two or more types may be included.
[0039] The content of the other resin is not particularly limited, but is preferably 30 parts by weight or less, more preferably 20 parts by weight or less, and even more preferably 10 parts by weight or less, relative to 100 parts by weight of the total of the poly(3-hydroxyalkanoate)-based resin components. The lower limit of the content of the other resin is not particularly limited, and may be 0 parts by weight.
[0040] (Additives) The resin composition for monofilaments according to this embodiment may contain additives to the extent that the effects of the present invention are not impaired. Examples of additives that can be used depending on the purpose include crystallization nucleating agents, lubricants, plasticizers, antistatic agents, flame retardants, conductive agents, heat insulating agents, crosslinking agents, antioxidants, ultraviolet absorbers, colorants, inorganic fillers, organic fillers, preservatives, and hydrolysis inhibitors. Biodegradable additives are particularly preferred.
[0041] Examples of crystallization nucleating agents include pentaerythritol, orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, and boron nitride. Among these, pentaerythritol is preferred because of its particularly excellent effect of promoting crystallization of the poly(3-hydroxyalkanoate)-based resin component. The amount of crystallization nucleating agent used is not particularly limited, but is preferably 0.1 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, and even more preferably 0.7 to 1.5 parts by weight, per 100 parts by weight of the total of the poly(3-hydroxyalkanoate)-based resin components. Furthermore, one type of crystallization nucleating agent may be used, or two or more types may be used, and the usage ratio can be appropriately adjusted depending on the purpose.
[0042] Examples of lubricants include behenamide, oleamide, erucamide, stearamide, palmitamide, N-stearylbehenamide, N-stearylerucamide, ethylenebisstearamide, ethylenebisoleamide, ethylenebiserucamide, ethylenebislauricamide, ethylenebiscapricamide, p-phenylenebisstearamide, and polycondensates of ethylenediamine, stearic acid, and sebacic acid. Among these, behenamide and erucamide are preferred because of their particularly excellent lubricating effect on poly(3-hydroxyalkanoate)-based resin components. The amount of lubricant used is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and even more preferably 0.1 to 1.5 parts by weight, per 100 parts by weight of the poly(3-hydroxyalkanoate)-based resin components. The lubricant may be used alone or in combination of two or more kinds, and the ratio of use can be adjusted appropriately depending on the purpose.
[0043] Examples of plasticizers include glycerin ester compounds, citrate ester compounds, sebacate compounds, adipate compounds, polyether ester compounds, benzoate ester compounds, phthalate ester compounds, isosorbide ester compounds, polycaprolactone compounds, and dibasic acid ester compounds. Among these, glycerin ester compounds, citrate ester compounds, sebacate compounds, and dibasic acid ester compounds are preferred because of their particularly excellent plasticizing effect on poly(3-hydroxyalkanoate) resin components. Examples of glycerin ester compounds include glycerin diacetomonolaurate. Examples of citrate ester compounds include acetyl tributyl citrate. Examples of sebacate ester compounds include dibutyl sebacate. Examples of dibasic acid ester compounds include benzyl methyl diethylene glycol adipate. The amount of plasticizer used is not particularly limited, but is preferably 1 to 20 parts by weight, more preferably 2 to 15 parts by weight, and even more preferably 3 to 10 parts by weight, per 100 parts by weight of the poly(3-hydroxyalkanoate) resin component in total. One type of plasticizer may be used, or two or more types may be used, and the usage ratio can be adjusted appropriately depending on the purpose.
[0044] (Method for producing resin composition) The resin composition according to this embodiment can be produced by melt-kneading the components. After melt-kneading, the components may be pelletized. This will be specifically described below.
[0045] First, a poly(3-hydroxyalkanoate) resin component and any optional additives are added and melt-kneaded using an extruder, kneader, Banbury mixer, roll, or the like to prepare a resin composition. The resin composition may be extruded into a strand shape and then cut to obtain pellets having particle shapes such as cylindrical, elliptical, spherical, cubic, and rectangular parallelepiped shapes. The prepared pellets are desirably thoroughly dried at 40 to 80°C to remove moisture before being subjected to the next molding step.
[0046] The temperature at which the melt-kneading is carried out cannot be generally defined because it depends on the melting point, melt viscosity, etc. of the resin used, but the resin temperature of the melt-kneaded product at the outlet of the spinning nozzle is preferably 135 to 200° C., more preferably 140 to 195° C., even more preferably 145 to 190° C., and particularly preferably 150 to 185° C. If the resin temperature of the melt-kneaded product is less than 135° C., the poly(3-hydroxyalkanoate) resin component may remain unmelted, and if it exceeds 200° C., the poly(3-hydroxyalkanoate) resin component may undergo thermal decomposition.
[0047] The resin composition for monofilaments according to this embodiment refers to a resin composition used to manufacture monofilaments through a molding process. Here, the monofilament refers to a thread-like molded product consisting of a single fiber, and in this application, there is no particular limitation as long as it can be formed from a resin. [Monofilament] The monofilament according to this embodiment contains the resin composition for monofilaments.
[0048] The monofilament containing the poly(3-hydroxyalkanoate) resin composition according to this embodiment preferably has a tensile strength of 0.4 to 6 cN / dtex, more preferably 0.5 to 5 cN / dtex, and even more preferably 0.6 to 4 cN / dtex.
[0049] The monofilament containing the poly(3-hydroxyalkanoate) resin composition according to this embodiment preferably has a tensile elongation of 50% or more, more preferably 70% or more, and even more preferably 100% or more.
[0050] When the tensile strength and tensile elongation of the monofilament according to the present embodiment are within the above ranges, it can maintain practical strength while being stretched when subjected to stress such as tension, thereby preventing breakage, making it applicable to a wide range of applications. In particular, the monofilament of the present application has the characteristic that it not only has elongation when tensile, but also returns to its original length almost like a rubber band when the stress is released. When used as turf yarn for artificial turf, it is particularly preferable because it can prevent breakage when worn by people walking on the artificial turf or when rubbed during sports.
[0051] The tensile strength and tensile elongation of the monofilament according to the present embodiment refer to the tensile strength and tensile elongation measured at an initial length of 20 mm and a speed of 20 mm / min according to JIS L 1015:2021 "Testing Method for Staples of Chemical Fibers." For measuring the tensile strength and tensile elongation, for example, a tensile measuring device (Shimadzu Corporation, Autograph AG-1) can be used.
[0052] The monofilament containing the poly(3-hydroxyalkanoate) resin composition according to this embodiment preferably has a fineness of 15 to 5000 dtex, more preferably 1000 to 5000 dtex, and even more preferably 1000 to 3000 dtex.
[0053] The fineness of the monofilament is the mass per unit length, and is expressed in units of dtex as the mass (g) per 10,000 m. The fineness of the monofilament can be measured by an autobibroscope method.
[0054] The monofilament containing the poly(3-hydroxyalkanoate) resin composition according to this embodiment preferably has a fineness of 15 to 5000 dtex, a tensile strength of 0.4 to 6 cN / dtex, and a tensile elongation of 50% or more.
[0055] Examples of the cross-sectional shape (cross-section perpendicular to the longitudinal direction) of the monofilament according to this embodiment include a circular shape (a concept that also includes an oval shape), a quadrangular shape (a concept that also includes a rectangular shape and a diamond shape), a Y-shape, an X-shape, an H-shape, and a multi-lobed shape.
[0056] The monofilament according to this embodiment can be suitably used for marine materials, agricultural materials, civil engineering materials, sports equipment materials, automotive materials, medical materials, etc. Specifically, the monofilament according to this embodiment can be used as, for example, fishing line, fishing nets, aquaculture nets, seaweed seedling threads, artificial turf yarns, toothbrush bristles, beverage extraction filters (woven fabrics for tea bags), insect nets, animal nets, sutures, surgical nets, stents, prosthetic materials, 3D printing filaments, tennis strings, hook-and-loop fasteners, tire cords, printing screens, wigs, hose reinforcements, weft knitted fabrics for clothing, grass-cutting cords (wire materials), screen nets, woven fabrics, turf, core filaments of filament-core spun yarns, ribbons, etc. [Method for Manufacturing the Monofilament] In the method for manufacturing the monofilament according to this embodiment, the monofilament is manufactured by melt spinning.
[0057] The production method includes the steps of (i) discharging a molten resin composition from a spinning nozzle, cooling it, and forming it into a raw yarn, and (ii) stretching the raw yarn in at least one direction.
[0058] The method for producing the monofilament according to this embodiment may be continuous or discontinuous as long as it includes the steps (i) and (ii) described above, but is preferably carried out continuously in terms of ease of drawing.
[0059] The following describes the manufacturing method using the monofilament manufacturing apparatus 1 shown in Figure 1 as an example. (Step (i)) The step (i) is a step of discharging a molten resin composition from a spinning nozzle, cooling it, and forming it into a raw yarn.
[0060] The cooling method is not particularly limited as long as it can cool and solidify the molten resin composition to a temperature at which the resin composition can crystallize, and can be performed using, for example, a water bath or cold air.
[0061] As shown in FIG. 1, in the step (i), first, the resin composition according to this embodiment is charged into a material charging section 2a.
[0062] Next, the material fed from the material feeding section 2 a is heated and kneaded in the kneading extruder 2 b to obtain the molten material. The material to be fed may be a pelletized resin composition, or each component constituting the resin composition may be fed separately.
[0063] The kneading extruder 2b is a screw extruder, and may be a single-screw extruder or a twin-screw extruder.
[0064] Then, the melt obtained in the kneading extruder 2d is discharged from a spinning nozzle 2d having a discharge hole, thereby obtaining a molten, filamentous resin composition (raw yarn (A)).
[0065] The flow rate of the melt discharged from the discharge hole of the spinning nozzle 2d is adjusted by the gear pump 2c as required.
[0066] The temperature of the spinning nozzle 2d is, for example, preferably 150 to 190°C, and more preferably 160 to 180°C.
[0067] The spinning nozzle 2d has one or more discharge holes, and may have a plurality of discharge holes.
[0068] The spinning nozzle 2d has a plurality of discharge holes, so that a plurality of monofilaments can be produced simultaneously.
[0069] Examples of the shape of the discharge hole include a circular shape (including an elliptical shape), a square shape (including a rectangular shape and a diamond shape), a Y-shape, an X-shape, an H-shape, and a multi-lobe shape.
[0070] Regarding the size of the discharge hole, for example, when the shape of the discharge hole is circular, the diameter of the discharge hole is preferably 0.5 mm to 20 mm, more preferably 1.0 mm to 10 mm.
[0071] When the nozzle hole has a circular shape, the length (L) of the nozzle hole divided by the diameter (D) of the nozzle hole, in other words, L / D, is preferably 1-10, and more preferably 2-5.
[0072] The rate at which the molten material is discharged from one discharge hole is preferably 0.20 to 2.0 kg / hr, more preferably 0.40 to 1.2 kg / hr.
[0073] In the step (i), the resin composition is cooled by passing the raw yarn through a water bath 3a. In this step, crystallization is promoted at least on the surface of the raw yarn, thereby suppressing adhesion of the raw yarn to a jig 3c, such as a roll or a bar, that changes the direction of the raw yarn in the water bath 3a.
[0074] The temperature of the water bath 3a is preferably 25 to 60°C, more preferably 30 to 40°C.
[0075] In the step (i), by adjusting the time for which the raw yarn is passed through the water bath 3a at 25 to 60°C, it is possible to prevent the raw yarn in a softened state from sticking to the jig 3c that changes the direction of the raw yarn, and to facilitate temperature adjustment in the subsequent drawing step (ii).
[0076] In the step (i), the time for passing the raw yarn through the water bath 3a at 25 to 60°C is preferably 2 minutes or less, more preferably 1 minute or less, because this prevents excessive crystallization of the raw yarn and facilitates temperature control in the drawing step (ii). This prevents the raw yarn from becoming hard. This makes it easier to draw the raw yarn in the step (ii). As a result, the strength of the monofilament can be easily increased.
[0077] The time for passing the raw yarn through the water bath 3a at 25 to 60°C in the step (i) can be adjusted by adjusting the passing distance of the raw yarn through the water bath 3a and the take-up speed in the take-up roll section 4. (Step (ii)) In the step (ii), the raw yarn is drawn in at least one direction.
[0078] Although the specific stretching method is not particularly limited, a method of stretching the raw yarn in the stretching direction is preferred. Stretching the raw yarn in the stretching direction means pulling the raw yarn in the stretching direction.
[0079] The method for stretching the raw yarn in the stretching direction is not particularly limited. In the case of batch-type stretching, both ends of the raw yarn may be gripped and pulled in the stretching direction.
[0080] When the raw yarn is drawn in the conveying direction while being continuously conveyed, the raw yarn can be drawn in the conveying direction, for example, by varying the rotation speed of the rolls between the take-up roll section 4 and the drawing roll section 6. The draw ratio in the conveying direction can be determined by the ratio of the rotation speed of the rolls before drawing to the rotation speed of the rolls after drawing.
[0081] In step (ii), the raw yarn is stretched to increase the orientation of the crystals of the polymer component contained in the raw yarn, thereby increasing the strength of the monofilament.
[0082] In step (ii), it is preferable to draw the raw yarn, which has been reduced in adhesion to the rolls and has not been subjected to excessive crystallization in step (i), at a speed difference between the take-up roll section 4 and the drawing roll section 6.
[0083] The draw ratio in step (ii) is preferably 3 times or more, more preferably 4 times or more, even more preferably 5 times or more, and particularly preferably 6 times or more, in that filaments having higher strength and elongation are likely to be obtained.
[0084] In an embodiment using the take-up roll unit 4 and the stretching roll unit 6, the stretch ratio can be calculated by the following formula: Draw ratio = Speed (m / min) of the stretching roll unit 6 / Speed (m / min) of the take-up roll unit 4 The speed (m / min) of the stretching roll unit is the length per unit time of the raw yarn transported by the stretching roll. When two or more stretching rolls are used in step (ii) (when stretching is performed using multiple stretching rolls), the fastest speed is defined as the stretching roll speed (m / min). The speed (m / min) of the take-up roll unit is the length per unit time of the raw yarn taken up by the take-up roll.
[0085] In order to stably draw the raw yarn during the step (ii), it is preferable to heat the raw yarn at an appropriate temperature in the heating section 5, and the temperature of the raw yarn is preferably 60° C. or lower, more preferably 55° C. or lower, and particularly preferably 50° C. or lower. In addition, since the raw yarn is less susceptible to the influence of the ambient air temperature, the temperature is preferably 25° C. or higher, more preferably 30° C. or higher, and particularly preferably 35° C. or higher.
[0086] To enhance the orientation of the polymer component crystals, it is desirable to draw a raw yarn in a series of steps in which the polymer component crystals have formed but are not excessively crystallized. In the case of poly(3-hydroxyalkanoate)-based resins, if the polymer component crystallizes poorly, the resin tends to stick and is difficult to mold into a raw yarn. Furthermore, the formation of oriented crystals is difficult, making it difficult to sufficiently increase the strength of the monofilament. Furthermore, if the polymer component crystallizes excessively, the resin becomes too solid, making the raw yarn difficult to draw. Furthermore, if the raw yarn is forcibly pulled in an attempt to draw the raw yarn, the raw yarn breaks, making it impossible to produce a monofilament. Furthermore, when drawing a raw yarn in which crystallization has progressed excessively, the crystals are heated to partially melt the crystals, but this melting of the crystals on the surface of the raw yarn makes the raw yarn sticky, making it difficult to heat to a drawable state.
[0087] In this embodiment, the raw yarn is heated and drawn at a speed difference between the take-up roll section 4 and the drawing roll section. This reduces the elastic modulus of the raw yarn in the heated section compared to other sections, and drawing is mainly performed in the heated section. This makes it easier to control the drawing state, and as a result, it becomes easier to obtain monofilaments with a stable fineness.
[0088] The method for heating the yarn in the heating unit 5 is not particularly limited as long as it adjusts the yarn to the desired temperature. Examples include passing the yarn through a water bath whose temperature is controlled within the above-mentioned temperature range, blowing temperature-controlled air onto the yarn, using auxiliary heating means such as an infrared heater, contacting the yarn with a roll whose temperature is controlled to a predetermined temperature, and using a heating furnace whose temperature is controlled to a predetermined temperature. These methods may be used alone or in combination. [Artificial Turf] The artificial turf of this embodiment includes a base fabric formed in a sheet shape and turf material (also referred to as "turf yarn") containing the monofilament of this embodiment. Artificial turf is generally produced by planting a large number of turf materials resembling grass blades on a base fabric.
[0089] In the artificial turf according to this embodiment, the base fabric is preferably a plain weave fabric made of a thermoplastic resin such as polypropylene or polyethylene, but may also be made of other woven fabrics or other materials.
[0090] Furthermore, in the artificial turf according to this embodiment, the turf material may be cylindrical or flat.
[0091] The following items list preferred embodiments of the present disclosure, but the present invention is not limited to them. [Item 1] A resin composition for monofilaments containing a poly(3-hydroxyalkanoate)-based resin component, wherein the resin composition has a melting point peak temperature of 140°C or higher in differential scanning calorimetry analysis and a crystalline fusion enthalpy of 65 J / g or less as calculated from all melting point peaks. [Item 2] The resin composition for monofilaments according to Item 1, wherein the poly(3-hydroxyalkanoate)-based resin component comprises a copolymer of two or more types of 3-hydroxybutyrate units and other hydroxyalkanoate units, the types and / or content ratios of which differ from each other. [Item 3] The resin composition for monofilaments according to Item 1 or 2, wherein the poly(3-hydroxyalkanoate)-based resin component comprises: a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units, wherein the content of the other hydroxyalkanoate units is 6 mol% or less; and a copolymer (B) of 3-hydroxybutyrate units and other hydroxyalkanoate units, wherein the content of the other hydroxyalkanoate units is 24 mol% or more. [Item 4] The resin composition for monofilaments according to Item 3, wherein the content of copolymer (B) in the poly(3-hydroxyalkanoate)-based resin component is 20 wt% or more and 50 wt% or less. [Item 5] The resin composition for monofilaments according to any one of Items 2 to 4, wherein the other hydroxyalkanoate units are 3-hydroxyhexanoate units. [Item 6] A monofilament comprising the resin composition for monofilaments according to any one of Items 1 to 5. [Item 7] The monofilament according to item 6, having a fineness of 15 to 5000 dtex, a tensile strength of 0.4 to 6 cN / dtex, and a tensile elongation of 50% or more. [Item 8] The monofilament according to item 7, having a fineness range of 1000 to 5000 dtex. [Item 9] An artificial turf having turf yarns planted in a base fabric, the turf yarns comprising the monofilament according to any one of items 6 to 8.[Item 10] A method for producing a monofilament containing the resin composition for monofilaments according to Items 1 to 5, comprising the following steps (i) and (ii) in order: (i) a step of discharging the resin composition in a molten state from a spinning nozzle, followed by cooling and forming the resin composition into a raw yarn; and (ii) a step of stretching the raw yarn in at least one direction.
[0092] The present invention will be specifically explained below with reference to examples, but the technical scope of the present invention is not limited to these examples.
[0093] The substances used in the examples and comparative examples are shown below.
[0094] [Poly(3-hydroxyalkanoate)-based resin (P3HA)] P3HB3HH-1 (copolymer (A)): P3HB3HH (average content ratio 3HB / 3HH = 97.2 / 2.8 (mol% / mol%), weight average molecular weight is 660,000 g / mol) The P3HB3HH-1 was produced in accordance with the method described in Example 2 of International Publication WO2019 / 142845. P3HB3HH-2 (copolymer (B)): P3HB3HH (average content ratio 3HB / 3HH = 71.8 / 28.2 (mol% / mol%), weight average molecular weight is 660,000 g / mol) The P3HB3HH-2 was produced in accordance with the method described in Example 9 of International Publication WO2019 / 142845. P3HB3HH-3: X131A (Kaneka Biodegradable Polymer PHBH (registered trademark)) (average content ratio 3HB / 3HH = 94 / 6 (mol % / mol %), weight average molecular weight 600,000 g / mol) [Additives] Additive-1: Pentaerythritol (manufactured by Mitsubishi Chemical Corporation: Neuraizer P) Additive-2: Behenic acid amide (manufactured by Nippon Fine Chemicals Co., Ltd.: BNT-22H) The evaluation methods used in the examples and comparative examples are described below. [Measurement of Melting Point Peak Temperature and Crystalline Melting Enthalpy in Differential Scanning Calorimetry] Approximately 4 to 10 mg of the poly(3-hydroxyalkanoate) resin composition obtained in each Example or Comparative Example was weighed using a differential scanning calorimeter (TA Instruments, Model DSC25). The poly(3-hydroxyalkanoate) resin composition was heated from 30°C to 180°C at a heating rate of 10°C / min under a nitrogen stream, and the melting point peak temperature at which the endotherm reached a maximum was determined in the DSC curve. Furthermore, a straight line was drawn between the baselines before and after the melting initiation and completion of the melting in the DSC curve, and the total heat quantity calculated as the area of the melting region enclosed by the straight line and the DSC curve was determined as the crystalline melting enthalpy. [Monofilament Fineness] The monofilament fineness was measured using an autobibroscope method. [Tensile Strength and Tensile Elongation of Monofilament] The tensile strength and tensile elongation of the monofilament were measured using a tensile measuring device (Shimadzu Corporation, Autograph AG-1) in accordance with JIS L 1015:2021 "Test Method for Chemical Fiber Staples," with the monofilament pulled at an initial length of 20 mm and a speed of 20 mm / min, and the breaking strength at break was defined as the tensile strength, and the elongation up to break was defined as the tensile elongation.(Example 1) [Production of pellets of poly(3-hydroxyalkanoate)-based resin composition] A blend of 30 wt% P3HB3HH-1 (content ratio in all P3HA components), 30 wt% P3HB3HH-2, and 40 wt% P3HB3HH-3 was mixed with 1 part by weight of additive-1 (content relative to 100 parts by weight of all P3HA components), and 1 part by weight of additive-2 (content relative to 100 parts by weight of all P3HA components) and further blended to obtain a resin mixture. The obtained resin mixture was extruded into a φ26 mm co-rotating twin-screw extruder with the cylinder and spinning nozzle temperatures set to 150 ° C. The extruded resin material was passed through a water bath filled with hot water at 40 ° C. to solidify the strands, and then cut with a pelletizer to obtain pellets of the resin composition.
[0095] The melting peak temperature and crystalline melting enthalpy of the resulting poly(3-hydroxyalkanoate) resin composition were measured, and the melting peak temperature was 152°C and the crystalline melting enthalpy was 57 J / g. [Preparation of Monofilaments] Pellets of the poly(3-hydroxyalkanoate) resin composition were placed in a single-screw extruder (screw diameter: 30 mm) with the cylinder and spinning nozzle set at 165°C, melted, and extruded from a spinning nozzle having five 1.5 mm diameter circular nozzle holes. The resulting yarns were passed through a hot water bath set at 35°C and taken up at a speed of 6 m / min with a take-up roll to obtain five raw yarns. These were then passed through a 3 m long hot water bath filled with 40°C hot water and taken up at a speed of 40 m / min with a draw roll to obtain five monofilaments stretched 7 times. The stretch ratio during monofilament production was defined by the following formula:
[0096] Draw ratio = speed of draw roll (m / min) / speed of take-up roll (m / min) The fineness, tensile strength, and tensile elongation of the obtained monofilament were measured, and the results were a fineness of 2,500 dtex, a tensile strength of 1.0 cN / dtex, and a tensile elongation of 140%. (Example 2) Pellets and monofilaments of the composition were prepared in the same manner as in Example 1, except that the raw materials for the poly(3-hydroxyalkanoate)-based resin composition in Example 1 were changed to the blending ratio shown in Table 1. The melting point peak temperature and crystalline fusion enthalpy of the obtained resin composition were measured, and the fineness, tensile strength, and tensile elongation of the monofilament were measured, and the evaluation results are shown in Table 1. (Comparative Example 1) Pellets and monofilaments of the composition were prepared in the same manner as in Example 1, except that the raw materials for the poly(3-hydroxyalkanoate)-based resin composition in Example 1 were changed to the blending ratio shown in Table 1. The melting peak temperature and crystalline fusion enthalpy of the resulting resin composition were measured, and the fineness, tensile strength and tensile elongation of the monofilament were measured. The evaluation results are shown in Table 1.
[0097]
[0098] The monofilaments containing the poly(3-hydroxyalkanoate) resin compositions of the examples have sufficient tensile strength and elongation, and by selecting the fineness depending on the application, they can be used for a variety of applications.
[0099] 1: Monofilament manufacturing apparatus, 2a: Material input section, 2b: Kneading extruder, 2c: Gear pump, 2d: Spinning nozzle, 3a: Water bath, 3b: Water tank, 3c: Jig, 4: Take-up roll section, 5: Heating section, 6: Stretching roll section, 7: Winding roll section
Claims
1. A resin composition for monofilaments containing a poly(3-hydroxyalkanoate)-based resin component, the resin composition having a melting point peak temperature of 140°C or higher in differential scanning calorimetry analysis and a crystalline fusion enthalpy calculated from all melting point peaks of 65 J / g or less.
2. The monofilament resin composition according to claim 1, wherein the poly(3-hydroxyalkanoate) resin component comprises a copolymer of two or more types of 3-hydroxybutyrate units and other hydroxyalkanoate units, the types and / or content ratios of which differ from each other.
3. A resin composition for monofilaments according to claim 1 or 2, wherein the poly(3-hydroxyalkanoate) resin component comprises: a copolymer (A) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of the other hydroxyalkanoate units being 6 mol % or less; and a copolymer (B) of 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of the other hydroxyalkanoate units being 24 mol % or more.
4. A resin composition for monofilaments according to claim 3, wherein the content of said copolymer (B) in said poly(3-hydroxyalkanoate)-based resin component is 20% by weight or more and 50% by weight or less.
5. The resin composition for monofilaments according to claim 2, wherein the other hydroxyalkanoate units are 3-hydroxyhexanoate units.
6. A monofilament comprising the resin composition for monofilaments according to claim 1 or 2.
7. The monofilament according to claim 6, having a fineness of 15 to 5,000 dtex, a tensile strength of 0.4 to 6 cN / dtex, and a tensile elongation of 50% or more.
8. The monofilament according to claim 7, wherein the fineness ranges from 1,000 to 5,000 dtex.
9. An artificial turf having grass yarns planted in a base fabric, the grass yarns including the monofilament according to claim 6.
10. A method for producing a monofilament containing the resin composition for monofilaments according to claim 1 or 2, comprising the following steps (i) and (ii) in that order: (i) discharging the resin composition in a molten state from a spinning nozzle, cooling it, and forming it into a raw yarn; and (ii) stretching the raw yarn in at least one direction.
Citation Information
Patent Citations
Biodegradable polyester resin composition
WO2013147139A1
Transformed microorganism for producing PHA copolymer comprising 3HH monomer unit at high composition rate and method for producing PHA using same
WO2019142845A1
Aliphatic polyester copolymer
WO2020230807A1
Absorbable suture containing medium-chain PHA (Polyhydroxyalkanoate)
CN103628174A
Biodegradable fiber and method for producing the same
JP2002371431A
Cited By
Production system and method of elastic high-linear-density fibers
CN119736721A