Semiconductor device manufacturing method and plasma processing method

The plasma processing method for GAA FETs addresses the challenge of etching selectivity and process complexity by using multiple cycles of anisotropic and isotropic etching with protective insulating films, achieving effective gate-substrate insulation and reducing defects, thus enhancing transistor performance.

JP7560673B2Active Publication Date: 2024-10-02HITACHI HIGH TECH CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023535741
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-09
Publication Date
2024-10-02
Estimated Expiration
2042-08-09

AI Technical Summary

Technical Problem

The existing methods for manufacturing Gate All Around (GAA) type Field Effect Transistors (FETs) face challenges in achieving effective insulation and separation between the gate and semiconductor substrate while maintaining strain integrity, leading to potential defects and increased process complexity due to the lack of etching selectivity between different SiGe sacrificial layers.

Method used

A plasma processing method involving multiple cycles of anisotropic and isotropic etching with protective insulating films is employed to selectively remove the second SiGe sacrificial layer, ensuring etching selectivity and reducing the number of process steps by using a combination of different insulating film materials to protect the first SiGe layer during the etching process.

Benefits of technology

This method effectively insulates and separates the gate from the semiconductor substrate, reducing defects and process complexity, while maintaining strain integrity and improving transistor performance by minimizing the number of process steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560673000001
    Figure 0007560673000001
  • Figure 0007560673000002
    Figure 0007560673000002
  • Figure 0007560673000003
    Figure 0007560673000003
Patent Text Reader

Abstract

In relation to production steps for a device having a structure in which a gate is insulated and separated from a Si substrate in a three-dimensional structure of a GAA-type FET or the like having a laminated channel in which fine line-shaped or sheet-shaped channels are vertically laminated in the substrate, the present invention provides a method that does not complicate the production steps without changing a SiGe sacrificial layer for forming the laminated channel and the Ge compositional makeup in the SiGe sacrificial layer required for insulating and separating the gate and the substrate. In order to achieve the above, after etching of a laminated film formed of a Si channel 4B and a SiGe sacrificial layer 3B, a protective insulating film 9 is formed on a sidewall of the laminated film by film formation / etching, and this is performed a plurality of times with different protective film materials. Thereafter, a Si sacrificial layer 4A and a SiGe sacrificial layer 3A remaining in a lower portion are removed by isotropic etching to form a region in which the insulating separation membrane is embedded. By conducting, in a continuous process using the same device, the forming of the laminated film of the protective insulating film to the removing of the sacrificial layer by etching, it is possible to simplify the steps.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a semiconductor device and a plasma processing method. [Background technology]

[0002] High integration of transistors is essential for the continuous improvement of the functions and performance of integrated circuit chips. High integration of transistors has been achieved mainly by miniaturizing the transistors. In order to miniaturize the transistors while maintaining or improving the transistor performance, many improvements have been made to the transistor structure and the materials that compose the transistors. Examples of such improvements include the source and drain regions in metal oxide semiconductor field effect transistors (MOSFETs). These include the introduction of strain into the MOSFET, the introduction of high dielectric gate insulating films and metals, and the introduction of new structures such as a shift from a planar type to a fin type.

[0003] Fin-type FETs have a structure that improves gate controllability by covering the periphery of the fin-type channel, which has a three-dimensional structure, with a gate, and can suppress the short channel effect (i.e., increased leakage current) caused by the reduction in gate length that accompanies transistor miniaturization. As miniaturization continues, it is expected that the channel will become a wire (thin line) or sheet-like laminate, and that the periphery of the channel will be covered with the gate, becoming a gate-all-around FET (GAA: Gate All Around). In a GAA FET, the entire periphery of the wire- or sheet-like channel (nanowire channel or nanosheet channel) is covered with the gate, which improves gate controllability compared to a fin-type FET and enables further suppression of the short-channel effect.

[0004] However, in a GAA FET, the gate that covers the channel is also in contact with the semiconductor substrate, so a FET is also formed on the semiconductor substrate side at the same time. Since the gate has a planar structure with poor gate controllability, this can cause degradation of the transistor characteristics.

[0005] Non-Patent Document 1 refers to the problem of degradation of transistor characteristics due to a planar FET, i.e., a parasitic FET, formed on the semiconductor substrate side, and points out the need to provide an insulating film directly under the gate to provide insulation isolation between the gate and the semiconductor substrate.

[0006] Patent Document 1 discloses a specific process for forming an insulating separation film between the gate and the semiconductor substrate. That is, a second SiGe sacrificial layer having a higher germanium (Ge) composition than the SiGe sacrificial layer is formed under a stacked structure consisting of a silicon (Si) channel and a silicon germanium (SiGe) sacrificial layer for forming a nanowire channel or nanosheet channel. Then, in the process, only the second SiGe sacrificial layer is selectively etched away from the stacked structure whose sidewall is exposed, and the removed region is filled with an insulating film. This makes it possible to insulate the nanowire channel or nanosheet channel from the silicon substrate.

[0007] Patent Document 2 describes a Si / SiGe nanowire channel or nanosheet channel. The sidewalls of the laminated film are covered with a protective film, and the sidewalls of the second SiGe sacrificial layer present at the bottom of the SiGe / Si laminated structure are A process is disclosed in which the second SiGe sacrificial layer is removed by exposing only the walls, and the removed region is filled with an insulating film. During etching of the second SiGe sacrificial layer, since the SiGe sacrificial layer in the SiGe / Si laminated film is covered with the protective film, it is not necessary to make the Ge composition in the second SiGe sacrificial layer higher than the Ge composition in the SiGe sacrificial layer in the SiGe / Si laminated film, and concerns about strain relaxation due to the introduction of a high Ge composition SiGe layer are alleviated. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] US Patent Application Publication No. 2019 / 0393351 [Patent Document 2] US Patent Application Publication No. 2020 / 0105756 [Non-patent literature]

[0009] [Non-Patent Document 1] J. Zhang, et al., “Full Bottom Dielectric Isolation to Enable Stacked Nanosheet Transistor for Low Power and High Performance Applications”, Proceedings of IEDM 2019, 2019, pp. 250~253 Summary of the Invention [Problem to be solved by the invention]

[0010] In the case of forming an insulating separation film between a gate and a semiconductor substrate as disclosed in Patent Document 1, a Si / SiGe laminated film for forming a nanowire channel or a nanosheet channel is formed under the Si / SiGe laminated film. The Ge composition of the second SiGe sacrificial layer is set to be larger than the Ge composition of the first SiGe sacrificial layer in the upper Si / SiGe stacked film. It is necessary to have a large amount of Ge and etching selectivity. Usually, the Ge composition of the first SiGe sacrificial layer in the upper Si / SiGe laminated film is set to 15 to 25%, and the Ge composition of the second SiGe sacrificial layer is set to 40 to 50%. In this case, the amount of strain caused by the difference in lattice constant between Si and SiGe becomes large in the second SiGe sacrificial layer, and there is a concern that defects due to strain relaxation may easily occur. The critical thickness at which this occurs is approximately 20 nm or less at the standard epitaxial growth temperature (550°C to 600°C) for forming a SiGe layer. Considering distortion during the formation of the upper Si / SiGe laminated film, It is estimated that the thickness of the second SiGe sacrificial layer needs to be designed to be extremely thin, about 10 nm or less. The thickness is extremely thin from the viewpoint of securing a sufficient process margin and providing effective insulation and isolation between the gate and the semiconductor substrate. In addition, the second SiGe sacrificial layer is removed by removing the second SiGe sacrificial layer and the upper Si / SiGe laminated film from the gate and gate This is performed after etching in the vertical direction along the spacer pattern. That is, when the second SiGe sacrificial layer is etched away, the sidewall of the first SiGe sacrificial layer in the upper Si / SiGe laminated film is also etched away. Since the second SiGe sacrificial layer is exposed, the first SiGe sacrificial layer is also exposed to etching when the second SiGe sacrificial layer is etched. Although the Ge compositions of the two films are different, they are the same SiGe layer, so it is difficult to provide perfect etching selectivity. When the second SiGe sacrificial layer is etched, a certain amount of the first SiGe sacrificial layer in the upper Si / SiGe laminated film is also unavoidably etched. This may affect subsequent processes, leading to concerns about the occurrence of defects such as an increase in transistor leakage current.

[0011] In contrast, in the process for the GAA FET disclosed in Patent Document 2, the Si / SiGe laminated film and the After etching the second SiGe sacrificial layer of the upper Si / SiGe laminated film portion vertically along the pattern, an insulating film is deposited on the sidewall to protect only the upper Si / SiGe laminated film portion with the insulating film, and only the second SiGe sacrificial layer is exposed. In the above-mentioned patent, the first SiGe sacrificial layer of the upper Si / SiGe laminated film is protected by an insulating film during etching of the second SiGe sacrificial layer. The etching selectivity issue in Reference 1 is resolved. In addition, it is possible to make the Ge composition of the second SiGe sacrificial layer equal to that of the first SiGe sacrificial layer of the upper Si / SiGe laminated film, which improves strain relaxation. This allows the second SiGe sacrificial layer to be set to a thick film thickness, making it possible to secure a sufficient process margin and reducing concerns about transistor malfunction due to strain relaxation. However, there is a concern that the number of process steps in the GAA FET process disclosed in Patent Document 2 will be significantly increased compared to the process disclosed in Patent Document 1. In Patent Document 2, only the upper Si / SiGe laminated film portion is protected by the insulating film, and the second SiGe sacrificial layer is The method for exposing only the sacrificial layer is carried out by the following process. First, the Si / SiGe laminated film and The second SiGe sacrificial layer at the bottom and the second SiGe sacrificial layer at the bottom are etched vertically along the pattern, and then an insulating film having a certain thickness is isotropically deposited to protect the etched sidewalls. After this, the grooves formed by the pattern are filled with a coating film such as a spin-on carbon film, and the carbon film is further etched vertically by a certain amount. Here, the amount of etching is adjusted so that the upper end of the carbon film after etching is positioned between the upper and lower ends of the second SiGe sacrificial layer. Next, a film such as titanium nitride (TiN) is deposited on the carbon film to fill the grooves formed by the pattern again, and the underlying carbon film is etched. The carbon film is removed. When the insulating film exposed at this time is etched away in the horizontal direction, the sidewall of the second SiGe sacrificial layer is exposed. Thereafter, the second SiGe sacrificial layer is selectively etched away. Finally, the TiN film and the insulating film are etched away to expose the second SiGe sacrificial layer. The above process has nine additional steps, such as film formation and etching, compared to the process disclosed in Patent Document 1, which significantly increases the number of process steps. In addition, when etching the carbon film by a certain amount in the vertical direction, it is difficult to adjust the amount of etching so that the upper end of the etched carbon film is located between the upper and lower ends of the second SiGe sacrificial layer whose side walls are covered with an insulating film, because there is no method for directly evaluating the relative positions of the SiGe sacrificial layer and the upper end of the carbon film.

[0012] This disclosure relates to a method for manufacturing a gate-array FET in which the gate and the semiconductor substrate are insulated from each other by using a Si / SiGe The present invention provides a plasma processing method capable of carrying out a process of patterning a laminated film and a second SiGe sacrificial layer formed thereunder, protecting the sidewalls of the laminated film with an insulating film laminated film, and etching and removing only the second SiGe sacrificial layer, and capable of carrying out processes from the patterning to the removal of the second SiGe sacrificial layer continuously using the same apparatus. [Means for solving the problem]

[0013] A brief summary of representative aspects of this disclosure is as follows.

[0014] One embodiment of the present disclosure includes: A first step of depositing a protective insulating film on a side wall of a semiconductor laminate film, the side wall being partially etched vertically; a second step of anisotropically etching the protective insulating film in a vertical direction to expose a surface of the semiconductor laminate film; a third step of repeating the first step and the second step a number of times using an insulating film material different from the protective insulating film to form a laminated film of the protective insulating film on the sidewall; The semiconductor device manufacturing method or plasma processing method includes a fourth step of removing the semiconductor laminated film existing under the protective insulating film by isotropic etching. Effect of the Invention

[0015] According to an embodiment of the present disclosure, in a manufacturing process of a three-dimensional structure device such as a GAA type FET, in a process of insulating and isolating a gate and a silicon substrate to suppress the formation of a planar type parasitic FET formed on the silicon substrate side, it is possible to suppress the occurrence of defects, and The device characteristics allow continuous processing in which multiple steps are performed in one device, making it possible to significantly suppress an increase in the number of process steps.

[0016] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Brief description of the drawings]

[0017] [Figure 1A] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1B] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1C] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1D] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1E] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1F] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1G] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1H] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1I] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1J] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1K] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1L] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1M] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 1N] 3 is a bird's-eye view showing a manufacturing process of a GAA FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 2A] 4 is an enlarged cross-sectional view showing a step of forming an insulating separation film between a gate and a semiconductor substrate in Example 1. FIG. [Figure 2B] 4 is an enlarged cross-sectional view showing a step of forming an insulating separation film between a gate and a semiconductor substrate in Example 1. FIG. [Figure 2C] 4 is an enlarged cross-sectional view showing a step of forming an insulating separation film between a gate and a semiconductor substrate in Example 1. FIG. [Figure 2D] 4 is an enlarged cross-sectional view showing a step of forming an insulating separation film between a gate and a semiconductor substrate in Example 1. FIG. [Figure 3A] 4A to 4C are cross-sectional views of an element isolation region showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 3B] 4A to 4C are cross-sectional views of an element isolation region showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 3C] 4A to 4C are cross-sectional views of an element isolation region showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 3D] 4A to 4C are cross-sectional views of an element isolation region showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 3E] 4A to 4C are cross-sectional views of an element isolation region showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 3F] 4A to 4C are cross-sectional views of an element isolation region showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Figure 4] FIG. 2 is a flow diagram of a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the first embodiment. [Diagram 5] FIG. 1 is a diagram illustrating an example of the configuration of a plasma processing apparatus. [Figure 6A] 11 is a bird's-eye view showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the second embodiment. [Figure 6B] 11 is a bird's-eye view showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the second embodiment. [Figure 6C] 11 is a bird's-eye view showing a manufacturing process of a GAA type FET in which a gate and a semiconductor substrate are insulated from each other according to the second embodiment. [Figure 6D] 11 is a bird's-eye view showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the second embodiment. [Figure 7A] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7B] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7C] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7D] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7E] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7F] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7G] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7H]10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7I] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7J] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 7K] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 8] FIG. 11 is a flow diagram of a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the third embodiment. [Figure 9A] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9B] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9C] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9D] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9E] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9F] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9G] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9H] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9I] 10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. [Figure 9J]10A to 10C are cross-sectional views showing a manufacturing process of a GAA type FET in which the gate and the semiconductor substrate are insulated from each other according to the fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiment of the present disclosure will be described based on the drawings. Note that the present disclosure is not limited to the examples described below, and various modifications are possible within the scope of its technical concept. In all the drawings for explaining the examples, the same reference numerals are given to members having the same functions, and repeated explanations thereof may be omitted. It goes without saying that many modifications are possible to the contents disclosed as the present embodiment, such as changing the combination of materials and manufacturing processes. In addition, the drawings are not necessarily drawn to scale accurately, and important parts are drawn in a schematic manner with emphasis so that the logic is clear. In addition, the drawings may be represented in a schematic manner compared to the actual embodiment in order to make the explanation clearer, but they are merely examples and do not limit the interpretation of the present disclosure. EXAMPLES

[0019] In the first embodiment, a series of steps (also called a step of forming a gate-semiconductor substrate insulating separation film 11 or a step of forming a gate-semiconductor substrate insulating separation film) for insulating and isolating a gate and a semiconductor substrate in a manufacturing process (a manufacturing method of a semiconductor device or a plasma processing method) of a GAA type FET (Gate All Around type Field Effect Transistor) as a semiconductor device, and a process of stacking a plurality of sidewall protective films made of different materials in the above steps will be described in detail. First, the above steps will be described with reference to Figs. 1A to 1N, 2A to 2D, 3A to 3F, and 4. The manufacturing method or plasma processing method of a semiconductor device described in the embodiment is a method of forming a GAA type FET in which a gate and a semiconductor substrate are isolated and insulated by an insulating film and a stacked channel is formed in a gate formation region in which thin wire-like or sheet-like channels are stacked in a direction perpendicular to the substrate.

[0020] 1A to 1N are perspective views showing the process from the step of insulating and isolating the gate and the semiconductor substrate to the completion of the FET structure in the manufacturing process of a GAA type FET. K is the etching of the Si / SiGe (silicon / silicon germanium) laminated film according to this embodiment. 1L to 1M show a process of embedding an insulating film (embedded insulating film) for insulating and isolating the gate and the semiconductor substrate in the removed second SiGe sacrificial layer area. FIG. 1N shows a GAA FET structure including the embedded insulating film (between the gate and substrate). FIGS. 2A to 2D show an enlarged view of a region including the lower part of the Si / SiGe laminated film to the Si substrate in the process shown in FIGS. 1D to 1G. 3A to 3F are cross-sectional views of a FET in a process corresponding to that in FIGS. 1C to 1K. 1A shows an element isolation region other than the channel region, that is, a cross-sectional view of a gate taken along line AA' shown in Fig. 1A. Fig. 4 shows a flow diagram of a series of manufacturing steps shown in Figs. 1A to 1K.

[0021] In FIG. 1A, a laminated film is formed on a single crystal Si substrate (semiconductor substrate) 1, in which a single crystal SiGe layer (first semiconductor layer) 3 and a single crystal Si layer (second semiconductor layer) 4 are alternately laminated in a plurality of layers. The laminated film of the SiGe layer 3 and the Si layer 4 has a second SiGe sacrificial layer 3A at the bottom, a Si sacrificial layer 4A on the second SiGe sacrificial layer 3A, and a first SiGe sacrificial layer 3B and a Si channel 4B are laminated alternately on the Si sacrificial layer 4A. The laminated film of the SiGe layer 3 and the Si layer 4 is formed by epitaxial growth using, for example, a chemical vapor deposition (CVD) method, and the SiGe The composition of Ge in the layer 3 is designed to be the same in the second SiGe sacrificial layer 3A and the first SiGe sacrificial layer 3B. The Ge composition may be, for example, 15 to 40%. The second SiGe sacrificial layer 3A and each of the first SiGe sacrificial layers 3B are formed so as to be lattice-matched to the Si substrate 1, and strain energy resulting from the difference in lattice constant between SiGe and Si is contained within each of the SiGe layers. The film thickness of the second SiGe sacrificial layer 3A, and the number of repeated laminations of the first SiGe sacrificial layer 3B and the Si channel 4B and their respective film thicknesses are determined based on the characteristics required for the FET, as well as the strain energy contained in the SiGe layer, the amount of defects in the SiGe layer 3, and the like. The thickness of the second SiGe sacrificial layer 3A is preferably about 10 to 50 nm, the thickness of the first SiGe sacrificial layer 3B is preferably about 8 to 20 nm, and the thickness of the Si channel is preferably about 10 to 50 nm. The number of repeated laminations of the first SiGe sacrificial layer 3B and the Si channel 4B is about 5 to 10 nm. For example, it is preferable that each of them has 3 to 6 layers. The thickness of the Si sacrificial layer 4A is, for example, 5 to 20 nm. Epitaxial growth by the CVD method is performed using, for example, hydrogen-diluted monosilane (SiH4), disilane (Si2H6), germane (GeH4), etc. as source gas. In addition, although the uppermost layer is the Si channel 4B in Fig. 1A, the first SiGe sacrificial layer 3B may be the uppermost layer.

[0022] The laminated film of the SiGe layer 3 and the Si layer 4 is processed into a line-shaped pattern in a plan view. The pattern width is, for example, about 5 to 15 nm when forming a thin nanowire channel. In the case of forming a sheet-shaped nanosheet channel, the length is adjusted to, for example, about 10 to 100 nm. In contrast, the nanosheet channel has slightly worse controllability by the gate compared to the nanowire, but can obtain a large driving current.

[0023] The channel shape is determined in consideration of the required application of the device. The line pattern is periodic or a similar pattern. For example, when a laser using argon fluoride gas (ArF) as a light source is used, the pattern period is, for example, 40 nm to 80 nm. If the pattern period is, for example, 20 nm or more and 40 nm or less, self-aligned quadruple patterning (SAQP) can be used. In addition, it can be used for exposure to extreme ultraviolet (EUV) rays with a wavelength of 13.5 nm. When the pattern period is, for example, up to 40 nm, single patterning is used. If the pattern period is, for example, 20 nm or more and 40 nm or less, the SADP can be used.

[0024] After forming a laminated film pattern of a SiGe layer 3 and a Si layer 4, a groove of a partially patterned Si substrate 1 is Then, an element isolation (STI: Shallow Trench Isolation) insulating film (referred to as an STI insulating film) 2 for forming an element isolation region is deposited, and the STI insulating film 2 is etched back to obtain the structure of the insulating film 2 shown in FIG. 1A. The STI insulating film 2 is formed, for example, by using a CVD method or the like. The material of the STI insulating film 2 is a silicon oxide film (SiO2), a silicon oxynitride film (SiON), or a silicon carbon film. It may be an oxide film (SiCO) or the like. The upper surface of the STI insulating film 2 after the etch-back may be set at any position, but the most desirable form is to adjust the amount of etching so that it is located between the upper end and the lower end of the second SiGe sacrificial layer 3A.

[0025] On the laminated film pattern of the SiGe layer 3 and the Si layer 4, a dummy gate insulating film 5 made of SiO2 or an insulating film equivalent thereto and a dummy gate insulating film made of amorphous Si or polycrystalline (poly)Si are formed. Then, a hard mask 7 made of an insulating film such as SiO2, silicon nitride film (Si3N4), or SiON is formed. The dummy gate insulating film 5 may be formed by using, for example, a CVD method or a thermal oxidation method. Alternatively, the dummy gate insulating film 5 may be formed by oxidizing the SiGe layer 3 and the Si layer 4 using a chemical vapor deposition (CVD) method or a plasma oxidation method. The thickness of the dummy gate insulating film 5 is desirably in the range of 1 to 3 nm, for example. The dummy gate 6 and the hard mask 7 may be formed by a film forming method such as a CVD method. The thickness of the dummy gate 6 and the hard mask 7 is desirably adjusted in the range of 20 to 200 nm, for example. The dummy gate insulating film 5, the dummy gate 6, and the hard mask 7 are formed by stacking the SiGe layer 3 and the Si layer 4. The patterning is performed in a direction perpendicular to the film pattern. The above patterning is performed by using a method such as SADP or single exposure depending on the gate pitch. For example, the gate pitch is set to 40 to 70 nm, the width of the dummy gate 6, i.e., the gate length, is set to a range of 10 to 30 nm, and the patterning is performed in a direction perpendicular to the film pattern. The hard mask 7, the dummy gate 6, and the dummy gate insulating film 5 are etched along the line. Here, the etching of the hard mask 7 and the dummy gate 6 may be performed by, for example, vertical etching using dry etching. The etching of the dummy gate insulating film 5 may be performed by, for example, dry etching. It is preferable to use isotropic etching using etching or wet etching. Also, the etching of the dummy gate insulating film 5 is not performed in the main process shown in FIG. 1A, but is performed in the spacer insulating film shown in FIG. 1B. The hard mask 7, the dummy gate 6, and the dummy gate insulating film 5 may be formed after etching. After the etching, a gate sidewall spacer (gate sidewall spacer film) 8 is formed by, for example, a CVD method. 1A. The gate sidewall spacer 8 is, for example, a low dielectric constant It is preferable to use a SiON film, a silicon carbon oxynitride film (SiOCN), or a SiCO film. The horizontal film thickness of the gate sidewall spacer 8 is adjusted in the range of, for example, 5 to 15 nm.

[0026] From the structure shown in FIG. 1A, the gate sidewall spacer 8 is anisotropically etched in the vertical direction, and When a SiCO film is used for the gate sidewall spacer 8, the anisotropic etching of the gate sidewall spacer 8 is performed using, for example, a mixture of tetrafluoromethane (CF4) and octafluorocyclobutane (C4F8 In the case where the gate sidewall spacer 8 is made of a SiOCN film, the gate sidewall spacer 8 is anisotropically etched using a gas mixture of, for example, fluoromethane. A mixed gas of CH3F, oxygen (O2), and helium (He) is preferably used. The above etching is performed under conditions that allow selective etching of the laminated film pattern of the SiGe layer 3 and the Si layer 4. If the dummy gate insulating film 5 is not etched in FIG. 1A, the above gate sidewall spacer 8 is etched under etching conditions that use the dummy gate insulating film 5 as a stopper. The etching amount is adjusted so that the upper end of the gate sidewall spacer 8 is located between the upper and lower ends of the hard mask 7 after the etching. The side walls of the gate are adjusted so as to be entirely covered with the gate side wall spacer 8. , which corresponds to 101 in the process flow diagram of FIG.

[0027] In FIG. 1C, a laminated film pattern of a SiGe layer 3 and a Si layer 4 is formed along the sidewall of a gate sidewall spacer 8. The anisotropic etching is performed in the vertical direction. The etching time of this anisotropic etching is adjusted so as to etch the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B and the Si sacrificial layer 4A, and it is desirable to end the etching at a structure of the laminated film in a state where the second SiGe sacrificial layer 3A is exposed. The depth to which the second SiGe sacrificial layer 3A is etched by over-etching is, for example, 0. The thickness of the SiGe layer 3 and the Si layer 4 is preferably adjusted to a range of about 100 nm to about 40 nm. For this etching, for example, chlorine (Cl2), CF4, or a gas equivalent thereto, or a mixed gas of these (Cl2 and CF4), or a gas containing nitrogen trifluoride (NF3) or O2 in addition to these (Cl2 and CF4), may be used. The etching of the laminated film of the SiGe layer 3 and the Si layer 4 in this step corresponds to 102 in the process flow diagram of FIG. 4, and may be performed continuously in the chamber of the same device after the etching 101 of the gate sidewall spacer 8 shown in FIG. 1B is performed. FIG. 3A shows the device isolation region (FIG. 1B) other than the channel region of the FET after this step. 1A shows a cross section of the gate taken along line AA' in FIG.

[0028] After that, the ALD (Atomic Layer Deposition) method was used to form the first A first protective insulating film 9 is deposited to obtain the structure shown in FIG. 1D. The protective insulating film 9 is The upper surface and sidewall of the gate sidewall spacer 8, the exposed first SiGe sacrificial layer 3B and the Si channel 4B are The material of the protective insulating film 9 is deposited on the side walls of the laminated film formed of the SiGe layer 3 and the Si layer 4, the side walls of the Si sacrificial layer 4A, the upper surface of the second SiGe sacrificial layer 3A, and the STI insulating film 2. In consideration of the etching selectivity of the above, it is preferable that the insulating film contains nitrogen, and it is preferable that the insulating film contains silicon and nitrogen, for example, a Si3N4 film or a SiON film equivalent thereto. The thickness of the protective insulating film 9 is controlled to, for example, about 2 to 3 nm. The protective insulating film 9 is formed by the ALD method. In the case of a Si3N4 film formed by the method described above, the source of Si is, for example, bis(tert-butylamino) Silane (Bis(tertbutylamino)silane:BTBAS), bis(diethylamino)silane (Bis(DiEthylAmino)Silane:BDEAS), or dichlorosilane (SiH2Cl2) is used as the nitrogen source. N2 gas, a mixture of N2 gas and hydrogen (H2) gas, or ammonia (NH3) gas, etc. In addition, the protective insulating film 9 may be a film that does not contain nitrogen, such as SiO2. Alternatively, the film may be formed by a CVD method or the like. In this process, an enlarged view including the lower part of the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B in FIG. 1D to the second SiGe sacrificial layer 3A is shown in FIG. 2A. The sidewalls of the laminated film consisting of the first SiGe sacrificial layer 3B and the Si channel 4B and the Si sacrificial layer 4A often have a tapered shape that is slightly inclined from the vertical direction at the bottom of the pattern. This reflects the characteristics of dry etching during pattern formation shown in FIG. 1C, and is caused by the fact that reaction products or raw material gases are likely to accumulate on the sidewalls during etching. The taper angle is controlled by the ion energy during etching, the etching gas, the pressure inside the etching chamber, etc., but is also adjusted taking into consideration damage to the underlying second SiGe sacrificial layer 3A. The angle (θ1 in FIG. 2A) between the sidewall and the upper surface of the second SiGe sacrificial layer 3A is, for example, in the range of 80 to 90 degrees. In FIG. 1C, the first SiGe sacrificial layer 3B The width of the groove pattern formed in the laminated film consisting of the Si channel 4B and the Si sacrificial layer 4A is 20 nm, assuming, for example, a gate pitch of 56 nm, a gate length of 20 nm, and a horizontal film thickness of the gate sidewall spacer 8 of 8 nm. It is expected that the width of the groove pattern will be further reduced as transistors are miniaturized, and in the future, it is predicted to be, for example, about 10 to 15 nm. In this case, taking the above taper angle into consideration, it is expected that the width of the groove pattern at the bottom of the groove will be, for example, about 10 nm or less. When a protective insulating film 9 is formed on such a narrow pattern, the vertical It is assumed that the film thickness in the direction (t2 in FIG. 2A) is thicker than the film thickness in the horizontal direction on the sidewall (t1 in FIG. 2A). The film thickness t1 in the horizontal direction of the protective insulating film 9 on the pattern sidewall is set to, for example, 2 to 3 nm. Then, the film thickness t2 in the vertical direction at the bottom of the groove is expected to be, for example, 3 to 6 nm. This step shown in FIG. 1D corresponds to 103 in the process flow diagram of FIG. 4, and the first SiGe sacrificial layer 3B shown in FIG. Following etching 102 of the laminated film consisting of the Si channel 4B and the Si sacrificial layer 4A, FIG. 3B shows the channel of the FET after this process. 1A shows a cross section of a gate in an element isolation region other than the region (line AA′ in FIG. 1A).

[0029] In the step shown in FIG. 1E, the protective insulating film 9 is etched in the vertical direction. The etching is performed under selective etching conditions for the hard mask 7, gate sidewall spacer 8, second SiGe sacrificial layer 3A, and STI insulating film 2. For example, when the protective insulating film 9 is a Si3N4 film, the etching gas may be, for example, a gas in which Cl2 or the like has been added to a mixed gas of a halogen gas such as CF4 or C4F8 and O2, or a gas equivalent thereto. This etching exposes the top surface of the second SiGe sacrificial layer 3A. FIG. 2B shows an enlarged view of the above process, including the lower part of the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B up to the second SiGe sacrificial layer 3A. In this etching, the vertical The etching time is determined taking into consideration the thickness of the protective insulating film 9 in the vertical direction at the bottom of the groove. Since the thickness of the protective insulating film 9 in the horizontal direction is thicker than the thickness of the protective insulating film 9 on the side walls of the groove, At the bottom of the groove, the protective insulating film 9 on the side wall is also partially etched away, and as shown in FIG. 2B, the Si There is a possibility that the sacrificial layer 4A and a part of the first SiGe sacrificial layer 3B are exposed. The lower part has an eave structure as shown in FIG. 2B, and the angle θ2 formed by the side wall of the laminated film composed of the Si sacrificial layer 4A, the first SiGe sacrificial layer 3B, and the Si channel 4B and the eave is an acute angle of 90 degrees or less. In FIG. 3C, a gate cross-section in the element isolation region (the AA' line in FIG. 1A) other than the channel region of the FET after this process is shown. Due to over-etching in the etching of the protective insulating film 9, the STI insulating film 2 is also slightly etched. The process shown in FIG. 1E corresponds to process 104 in the process flow diagram of FIG. 4 and may be continuously performed in the chamber of the same apparatus following the film formation process 103 of the protective insulating film 9 shown in FIG. 1D. Following the above process, using the ALD method, a second protective insulating film 10 is deposited on the first protective insulating film 9 to obtain the structure shown in FIG. 1F. A laminated film of the protective insulating film is formed by the first protective insulating film 9 and the second protective insulating film 10. In the laminated film of the protective insulating film, the lower layer side is the first protective insulating film 9, and the upper layer side is the second protective insulating film 10. The insulating film material of the first protective insulating film 9 and the insulating film material of the second protective insulating film 10 are made of different insulating film materials. The second protective insulating film 10 is deposited on the hard mask 7, the gate sidewall spacer 8, the upper surface and side walls of the protective insulating film 9, the upper surface of the second SiGe sacrificial layer 3A, and the STI insulating film 2. An enlarged view including from the lower part of the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B to the second SiGe sacrificial layer 3A after depositing the second protective insulating film 10 is shown in FIG. 2C. In FIG. 2C, the horizontal film thickness (t3 in FIG. 2C) of the second protective insulating film 10 is equal to (t3 = t1) or thinner (t3 < t1) than the horizontal film thickness t1 of the first protective insulating film 9.

[0030] Following the above process, using the ALD method, a second protective insulating film 10 is deposited on the first protective insulating film 9 to obtain the structure shown in FIG. 1F. A laminated film of the protective insulating film is formed by the first protective insulating film 9 and the second protective insulating film 10. In the laminated film of the protective insulating film, the lower layer side is the first protective insulating film 9 and the upper layer side is the second protective insulating film 10. The insulating film material of the first protective insulating film 9 and the second protective insulating film 10 are made of different insulating film materials. The second protective insulating film 10 is deposited on the hard mask 7, the gate sidewall spacer 8, the upper surface and side walls of the protective insulating film 9, the upper surface of the second SiGe sacrificial layer 3A, and the STI insulating film 2. An enlarged view including from the lower part of the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B to the second SiGe sacrificial layer 3A after depositing the second protective insulating film 10 is shown in FIG. 2C. In FIG. 2C, the horizontal film thickness (t3 in FIG. 2C) of the second protective insulating film 10 is equal to (t3 = t1) or thinner (t3 < t1) than the horizontal film thickness t1 of the first protective insulating film 9. layer 3A, and the STI insulating film 2. An enlarged view including from the lower part of the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B to the second SiGe sacrificial layer 3A after depositing the second protective insulating film 10 is shown in FIG. 2C. In FIG. 2C, the horizontal film thickness (t3 in FIG. 2C) of the second protective insulating film 10 is equal to (t3 = t1) or thinner (t3 < t1) than the horizontal film thickness t1 of the first protective insulating film 9. When the film thickness t1 is, for example, 2 to 3 nm, the film thickness t3 is preferably, for example, 1 to 3 nm. When the lower part of the sidewall of the laminated film consisting of the Si sacrificial layer 4A and the first SiGe sacrificial layer 3B and the Si channel 4B is exposed in the step shown in FIG. 2B, the second protective insulating film 10 is formed by the raw material gas passing through the flow path a1, through the eaves formed on the lower part of the first protective insulating film 9, the exposed Si sacrificial layer 4A, and the The second protective insulating film 10 is also deposited on the sidewall of the laminated film consisting of the first SiGe sacrificial layer 3B and the Si channel 4B. Since the second protective insulating film 10 is deposited isotropically, the first protective insulating film 9 is vertically deposited from the eaves portion. The film formation in the direction of the first protective insulating film 9 overlaps with the film formation in the horizontal direction from the sidewall of the laminated film consisting of the Si sacrificial layer 4A, the first SiGe sacrificial layer 3B, and the Si channel 4B, so that the film thickness (t4 in FIG. 2C) of the second protective insulating film 10 becomes thicker than the film thickness t3 in the horizontal direction of the second protective insulating film 10 on the sidewall of the first protective insulating film 9. By setting the thickness t3 to be thinner than the thickness t1, the thickness (t5 in FIG. 2C) of the second protective insulating film 10 in the vertical direction on the second SiGe sacrificial layer 3A is equal to the sum of the thickness t3 and the thickness t1 (t3+t1=t5) or is smaller than the sum of the thickness t3 and the thickness t1 (t3+t1>t5). The second protective insulating film 10 is a film that can be isotropically formed with good controllability even for a complex shape with finer unevenness. The second protective insulating film 10 is a film containing aluminum elements and oxygen elements, such as an aluminum oxide (Al2O3) film or an aluminum oxynitride (AlON) film equivalent thereto. When forming an Al2O3 film, it is preferable to use, for example, trimethylaluminum (TMA: Al(CH3)3) as the raw material of aluminum (Al) and vaporized water (H2O) as the raw material of oxygen. The precursor, consisting of Al(CH3)3, reacts with the hydroxyl groups formed on the surface by the supply of H2O. Because of its high reactivity with (OH group), Al2O3 film can be formed with good coverage even on uneven surfaces. Therefore, the Al2O3 film can be formed in the pattern inside the narrow opening of FIG. 2C. The second protective insulating film 10 may be an oxide film or a nitride film that does not use Al, and may be formed by a CVD method or the like. This step shown in FIG. 1F and FIG. 2C corresponds to step 105 in the process flow diagram of FIG. 4, and the first protective insulating film shown in FIG. 1E and FIG. 2B is formed isotropically. This step may be performed in the same chamber as the etching step 104 for the insulating film 9. FIG. 3D shows the element isolation region (not shown in FIG. 1A) other than the channel region of the FET after this step. The gate cross section taken along line AA' is shown.

[0031] 1G, the second protective insulating film 10 is etched in the vertical direction. The etching process removes the first protective insulating film 9, the hard mask 7, the gate sidewall spacer 8, the second SiGe sacrificial film 9, and the second SiGe sacrificial film 10. The etching is performed under selective etching conditions for the sacrificial layer 3A and the STI insulating film 2. For example, when the second protective insulating film 10 is an Al2O3 film, the etching gas may be, for example, boron trichloride (BCl3), a mixed gas of BCl3 and Cl2, or a mixed gas of these with argon (Ar), N2, or O2, or a gas equivalent thereto. This etching exposes the upper surface of the second SiGe sacrificial layer 3A. FIG. 2D shows an enlarged view of the above process, including the lower part of the laminated film of the first SiGe sacrificial layer 3B and the Si channel 4B to the second SiGe sacrificial layer 3A. When this etching is performed, even when ions generated from the etching gas are incident on the substrate 1 obliquely rather than vertically, the ions are etched from the first protective insulating film 9 side. The light is reflected by the wall and changes its angle (a2 in FIG. 2D). As shown in FIG. 2C, the opening pattern formed in the Si sacrificial layer 4A, the first SiGe sacrificial layer 3B, and the Si channel 4B has the smallest opening width near the eaves of the first protective insulating film 9 after the second protective insulating film 10 is formed. Almost all of the etching gas ions reflected by the side wall of the protective insulating film 9 are directed toward the second protective insulating film 10. The second protective insulating film 10 deposited on the side wall of the pattern under the overhang is consumed in the vertical etching of the Si sacrificial layer 4A, and is not etched. The above process makes it possible to open the upper part of the second SiGe sacrificial layer 3A while protecting the side walls of the opening pattern formed in the Si sacrificial layer 4A, the first SiGe sacrificial layer 3B, and the Si channel 4B. Note that FIG. 3E shows the area other than the channel region of the FET after this process. The cross section of the gate in the element isolation region (line AA′ in FIG. 1A) is shown. The STI insulating film 2 is also slightly etched due to over-etching in the etching of the second protective insulating film 10. This step shown in FIG. 1G and FIG. 2D corresponds to step 106 in the process flow diagram in FIG. 4, and FIG. 1F and Following the film formation step 105 of the second protective insulating film 10 shown in FIG. 2C, It is preferable to perform the steps continuously. The gas and deposition conditions may be changed) is not limited to two cycles, but may be repeated several times. That is, when the combination of the first step, the film forming step (103, 105), and the second step, the etching step (104, 106), is considered as one cycle, in FIG. This means that the combination of the film forming step and the etching step is performed in two cycles (the first cycle is step 103 and step 104, and the second cycle is step 105 and step 106), constituting the third step. The gas and film forming conditions may be different between step 103 and step 104 in the first cycle and step 105 and step 106 in the second cycle. Also, the film forming step (103, 105) and the etching step (104, 106) may be different from each other. The number of cycles of is not limited to two, and may be multiple cycles by repeating multiple times.

[0032] 1H (fourth step), the second SiGe sacrificial layer 3A is etched in the vertical direction. The above etching is performed under selective etching conditions for the second protective insulating film 10, the first protective insulating film 9, the hard mask 7, the gate sidewall spacer 8, the STI insulating film 2, and the Si substrate 1. The etching gas may be, for example, a gas containing a halogen-based element, such as HBr, CF2Cl2, or bromotrifluoromethane (CF3Br), or a gas in which HBr contains about 1 to 5% CF4, or a mixed gas of these. It is preferable to use a gas obtained by adding O2, a rare gas such as Ar or He, or an inert gas such as N2, or a mixture of these gases. It is preferable to adjust conditions such as the gas flow ratio, the ion energy during etching, the combination of etching gases, and the pressure inside the etching chamber so that the etching of the second SiGe sacrificial layer 3A maintains verticality and the etching rate is about 1 to 10 times the etching rate of the Si substrate 1. This step shown in FIG. 1H corresponds to step 107 in the process flow diagram of FIG. 4, and is preferable to perform this step continuously in the chamber of the same device following the etching step 106 of the second protective insulating film 10 shown in FIG. 1G and FIG. 2D.

[0033] 1I (fourth step), the second SiGe sacrificial layer 3A is isotropically etched away. The above etching is performed under selective etching conditions for the second protective insulating film 10, the first protective insulating film 9, the hard mask 7, the gate sidewall spacer 8, the STI insulating film 2, the Si substrate 1, and the Si sacrificial layer 4A. The etching gas may be, for example, sulfur hexafluoride (SF6), CF4, or NF3. It is preferable to use a gas containing fluorine such as fluorine, a mixed gas of these, or a gas containing these with O2, a rare gas such as Ar or He, or an inert gas such as N2, or a mixed gas of these. By adjusting conditions such as the gas flow ratio, the ion energy during etching, the combination of etching gases, and the pressure inside the etching chamber, the etching of the second SiGe sacrificial layer 3A is adjusted so that the etching is isotropic and the etching rate is, for example, about 1 to 200 times the etching rate of the Si substrate 1. This step shown in FIG. 1I corresponds to step 108 in the process flow diagram of FIG. 4, and Following the vertical etching step 107 of the second SiGe sacrificial layer 3A shown in FIG. In addition, the present process shown in FIG. 1I may be performed by omitting the vertical etching process 107 of the second SiGe sacrificial layer 3A shown in FIG. 1H and by etching the second protective insulating film 10 shown in FIG. 1G. Following etching 106, this may be performed continuously in the chamber of the same apparatus.

[0034] In the step (fourth step) shown in FIG. 1J, the Si sacrificial layer 4A is isotropically etched away. The above etching is performed under selective etching conditions for the second protective insulating film 10, the first protective insulating film 9, the hard mask 7, the gate sidewall spacer 8, the STI insulating film 2, and the first SiGe sacrificial layer 3B. The etching gas includes gases containing fluorine such as SF6, CF4, or NF3, or mixtures of these gases. It is preferable to use a gas containing H2, O2, N2, or a mixture of these gases. By adjusting the gas flow ratio, ion energy during etching, combination of etching gases, pressure inside the etching chamber, and other conditions, it is preferable to adjust the etching of the Si sacrificial layer 4A to be isotropic and the etching rate to be, for example, about 1 to 100 times the etching rate of the first SiGe sacrificial layer 3B. This step shown in FIG. 1J corresponds to step 109 in the process flow diagram of FIG. 4, Following the etching removal step 108 of the second SiGe sacrificial layer 3A shown in FIG. 1I, the chamber of the same apparatus It is recommended that these steps be performed consecutively.

[0035] In the step shown in FIG. 1K, the second protective insulating film 10 and the first protective insulating film 9 are sequentially isotropically etched. The second protective insulating film 10 is etched under selective etching conditions for the first protective insulating film 9, the hard mask 7, the gate sidewall spacer 8, the STI insulating film 2, and the lower surface of the first SiGe sacrificial layer 3B and the Si substrate 1. For example, when the second protective insulating film 10 is an Al2O3 film, the etching gas The etching gas may be a mixture of O2, BCl3, and Ar, or a gas equivalent thereto. This etching is performed for a time 1 to 2 times longer than the etching time required to etch the second protective insulating film 10 by the thickness thereof, under conditions in which the second protective insulating film 10 is almost completely removed. After the second protective insulating film 10, the first protective insulating film 9 is removed by isotropic etching. The etching is performed under selective etching conditions for the hard mask 7, the gate sidewall spacer 8, the STI insulating film 2, the lower surface and sidewall of the first SiGe sacrificial layer 3B, the Si channel 4B, and the Si substrate 1. For example, when the protective insulating film 9 is a Si3N4 film, the etching gas may be trifluoromethane (CHF3), difluoromethane (CH2F2), or CH3F, or a mixture of fluorocarbon gas such as CF4 or C4F8 and H2, or a gas equivalent thereto. As in the etching of the second protective insulating film 10, this etching is performed by etching the first protective insulating film 9 to the thickness of the film. The etching is performed for a time 1 to 2 times longer than the etching time required for removing the first protective insulating film 9, under conditions such that the first protective insulating film 9 is almost completely removed. This step exposes the first SiGe sacrificial layer 3B and the sidewall of the Si channel 4B. This step corresponds to step 110 in the process flow diagram of FIG. 4, and is performed continuously in the chamber of the same device after the etching removal step 109 of the Si sacrificial layer 4A shown in FIG. 1J. That is, the gate sidewall spacer vertical etching step 101 (FIG. 1B) to the first and second protective insulating film isotropic etching removal step 110 (FIG. 1K) in FIG. 4 can be performed in the same device. FIG. 3F shows the process corresponding to FIG. 1K, in which the FET 1A shows a gate cross section in an element isolation region (line AA′ in FIG. 1A) other than the channel region. Due to the effect of overetching caused by etching (FIGS. 1G and 3E), the upper surface of the STI insulating film 2 has a curved shape in the region of the gap between adjacent gate sidewall spacers 8. The shape contributes to isotropic film deposition when depositing an interlayer insulating film (FIG. 1N: second interlayer insulating film 16) in a subsequent process, so that the film density of the interlayer insulating film is kept constant at the bottom of the gap, thereby suppressing the occurrence of cavities in the interlayer insulating film due to a decrease in film density.

[0036] Following the above series of steps, in the step shown in FIG. 1L, a gate-substrate isolation insulating film 11 is deposited as a buried insulating film (first insulating film). The gate-substrate isolation insulating film 11 is formed by using, for example, a CVD method, and after the gate-substrate isolation insulating film 11 is formed, a hard mask 7 is removed. Chemical mechanical polishing (CMP) is used as a topcoat to polish the gate-substrate. A planarization process is performed to planarize the surface of the inter-plate isolation insulating film 11. The material of the gate-substrate isolation insulating film 11 may be, for example, SiO2, SiON, SiCO, etc. By the above film formation, the region where the second SiGe sacrificial layer 3A and the Si sacrificial layer 4A were present is filled with the gate-substrate isolation insulating film 11.

[0037] In the next step, the gate-substrate isolation insulating film 11 is etched back to obtain the structure shown in FIG. 1M. The amount of etching may be adjusted so that the upper surface of the gate-substrate isolation insulating film 11 after the etch back is located between the lower and upper surfaces of the first SiGe sacrificial layer 3B, which is the lowest layer. This step forms a gate-substrate insulating film between the stacked film consisting of the first SiGe sacrificial layer 3B and the Si channel 4B and the Si substrate 1. The structure is separated by an insulating film 11 between the substrate and the laminated film (the insulating film 11 between the substrate and the laminated film is a gate-substrate insulating film). The gate-substrate isolation insulating film 11 can be called a buried insulating film 11 in other words.

[0038] After that, a GAA type FET formation process is performed to obtain the transistor structure shown in Fig. 1N. In this process, the gate sidewall inner spacer 12 is formed, the source and drain 15 is formed, the second interlayer insulating film 16 is formed, the hard mask 7 and the dummy gate 6, the dummy gate insulating film 5 and the first SiGe sacrificial layer 3B are etched away, the gate insulating film 13 and the gate metal 14 are formed, and the contact barrier 15 is formed. This comprises the formation of metal 17 and contact metal 18, followed by back-end metal wiring steps.

[0039] The gate sidewall inner spacer 12 is formed, for example, by selectively isotropically etching the first SiGe sacrificial layer 3B with respect to the Si channel 4B and other surrounding films to remove a portion of the first SiGe sacrificial layer 3B and form a groove, then forming a low dielectric constant film using a CVD method or the like and depositing it in the groove formed in the first SiGe sacrificial layer 3B, and then removing a portion of the low dielectric constant film by isotropic etching. This makes it possible to obtain the gate sidewall inner spacer 12 formed inside the groove of the first SiGe sacrificial layer 3B. The low dielectric constant film forming the gate sidewall inner spacer 12 is, for example, a SiCO film, SiOCN, or SiON film, or a film similar thereto, or a combination of these. It is preferable to use a laminated film. The isotropic etching of the first SiGe sacrificial layer 3B is performed under the same conditions as those for the isotropic etching of the second SiGe sacrificial layer 3A shown in FIG. 1I, and the etching time is adjusted so that the etching amount of the first SiGe sacrificial layer 3B is, for example, about 1 to 10 nm. For isotropic etching of the low dielectric constant film, for example, when the low dielectric constant film is a SiCO film, it is preferable to use, as the etching gas, a mixed gas of a fluorine-containing gas such as CHF3, CH2F2, CH3F, or NF3 with N2 or O2, or a gas equivalent thereto.

[0040] The source and drain 15 are formed, for example, by selectively epitaxially growing Si or SiGe on the sidewalls of the Si channel 4B. Separate Si or SiGe films are formed on the n-type FET region and the n-type FET region. It is preferable to selectively grow Si doped with n-type impurities such as phosphorus (P) or arsenic (As), and selectively grow SiGe doped with p-type impurities such as boron (B) in the p-type FET region.

[0041] The second interlayer insulating film 16 is formed by, for example, a CVD method. The material of the second interlayer insulating film 16 may be, for example, SiO2, SiON, or SiCO. The hard mask 6, the dummy gate insulating film 5, and the first SiGe sacrificial layer 3B are etched away using etching gas and etching conditions suited to the respective materials. When the hard mask 7 is a Si3N4 film, the etching gas may be CHF3, CH2F2, or CH3F. The dummy gate 6 made of poly-Si may be dry-etched using gas such as SF6, CF4, or HBr or a gas equivalent thereto, or wet-etched using a tetramethylammonium hydroxide solution (TMAH) or the like. The dummy gate insulating film 5 is removed by wet-etching using a hydrofluoric acid (HF) solution or the like. The first SiGe sacrificial layer 3B may be subsequently etched away under the same conditions as those for the isotropic etching of the second SiGe sacrificial layer 3A shown in FIG. 1I. The gate insulating film 13 may be made of a high dielectric material such as hafnium oxide (HfO2) or Al2O3, or a laminated film of these high dielectric materials. stomach.

[0042] The gate metal 14 is, for example, a p-work function control metal that determines the threshold voltage of a p-type FET and a It is preferable that the p-work function control metal film is made of an n-work function control metal that determines the threshold voltage and a gate buried metal. For example, titanium nitride (TiN) or tantalum nitride (TaN) or a metal compound having a work function equivalent thereto is used for the p-work function control metal film. The film may be made of, for example, titanium aluminum (TiAl), a metal in which carbon (C), oxygen (O), nitrogen (N) or the like is contained in TiAl, or a metal compound having a work function equivalent to these. The gate buried metal film is deposited for the purpose of reducing the metal resistance in the gate, and can be made of a material such as tungsten (W). The film is formed by the ALD method or the ALD method.

[0043] The contact barrier metal 17 and the contact metal 18 are formed by partially etching the second interlayer insulating film 16 through patterning, where the source and drain 15 of the n-type FET region and the p-type FET region are exposed. For the contact barrier metal 17, for example, TiN or TaN or a metal equivalent thereto is used, and for the contact metal 18, for example, W or cobalt (Co) is used. The thickness of the contact barrier metal 17 is designed to be, for example, about 1 to 3 nm. In the above-mentioned GAA FET structure, the gate metal 14 and the Si substrate 1 are separated by a gate-substrate isolation insulating film 11. 2, the Si substrate 1 is insulated and isolated from the other components, thereby preventing the Si substrate 1 from operating as a parasitic FET.

[0044] By performing the steps of forming the gate-semiconductor substrate insulating separation film 11 (steps shown in FIGS. 1A to 1N) in a plasma processing apparatus equipped with an ALD film formation function and anisotropic and isotropic etching control functions, a series of steps shown in FIG. 4, that is, gate sidewall spacer vertical etching (101 in FIG. 4) shown in FIG. 1B to first and second protective insulating films, etc. shown in FIG. 1K can be performed. The entire process up to the isotropic etching removal (110 in FIG. 4) is carried out in the same plasma processing equipment. The plasma processing apparatus includes an etching apparatus using inductively coupled plasma (ICP), an etching apparatus using capacitively coupled plasma (CCP), a microwave electron cyclotron The etching apparatus may be either an etching apparatus using an electron cyclotron resonance (ECR) plasma or an etching apparatus using an electron cyclotron resonance (ECR) plasma.

[0045] As an example, FIG. 5 shows the configuration of a plasma processing apparatus 200 using microwave ECR plasma. The plasma processing apparatus 200 includes a processing chamber 201, which is connected to a vacuum exhaust device (not shown) via a vacuum exhaust port 202. The inside of the processing chamber 201 is kept at a vacuum of about 0.1 to 10 Pa. In addition, a window 203 having a role of transmitting microwaves and airtightly sealing the processing chamber 201, and a perforated plate 204 for blocking ions are arranged in the processing chamber 201. The processing chamber 201 is divided into an upper portion 201A of the processing chamber 201 and a lower portion 201B of the processing chamber 201 by the perforated plate 204. The window 203 is made of a material that transmits microwaves, and a dielectric material such as quartz is used. The perforated plate 204 has a plurality of holes, and the material of the perforated plate 204 is preferably made of a dielectric material such as quartz or alumina.

[0046] The gas supply mechanism includes a gas source 205, a gas supply device 206, and a gas inlet 207. A raw material gas is supplied. The gas source 205 has a plurality of gases required for processing. The gas supply device 206 has a control valve for controlling the supply and cutoff of gas, and a mass flow controller for controlling the gas flow rate. The gas inlet 207 is provided between the window portion 203 and the porous plate 204. There are.

[0047] A waveguide 209 for propagating electromagnetic waves is connected to the upper portion of the processing chamber 201. A high frequency power source 208 for plasma generation, which is a high frequency power source, is connected to the The frequency power supply 208 is a power supply for generating electromagnetic waves for generating plasma. The microwaves used are those with a frequency of 2.45 GHz. The microwaves propagate through the waveguide 209 and enter the processing chamber 201. The microwaves are incident vertically into the processing chamber 201 by having an extending vertical waveguide and a waveguide converter that also functions as a corner for bending the direction of the microwaves by 90 degrees. The microwaves propagate vertically inside the processing chamber 201 via a window 203. A magnetic field generating coil 210 disposed on the outer periphery of the processing chamber 201 forms a magnetic field in the processing chamber 201. A microwave generated by a plasma generating high frequency power supply 208 is The microwaves generate a high density plasma in the processing chamber 201 by interacting with the magnetic field generated by the magnetic field generating coil 210 .

[0048] A sample stage 212 is disposed below the processing chamber 201, facing the window portion 203. The sample stage 212 is made of, for example, aluminum or titanium. The sample stage 212 holds a semiconductor substrate 211, which is a sample, on its upper surface. The central axes of the waveguide 209, processing chamber 201, sample stage 212, and semiconductor substrate 211 are aligned. An electrode for electrostatically adsorbing the semiconductor substrate 211 is provided inside the sample stage 212, and the semiconductor substrate 211 is electrostatically adsorbed to the sample stage 212 by applying a DC voltage. Furthermore, the sample stage 212 has a contact hole 214 for controlling the isotropy and anisotropy of etching. For this purpose, a high frequency voltage is applied from the high frequency bias power supply 213. The number may be, for example, 400 kHz.

[0049] Each mechanism of the plasma processing apparatus 200 is controlled by a control signal 221 from a control unit 220. The control unit 220 controls the processing conditions (anisotropic etching process, isotropic etching process, etc.) executed by the plasma processing apparatus 200. Depending on the process (e.g., laser processing, ALD film formation process, etc.), a control signal 221 is used to instruct each mechanism to perform a predetermined operation. The control unit 220 controls each mechanism by instructing the row. The high frequency power supply 208 is controlled to control ON / OFF of the electromagnetic wave for generating plasma. The control unit 220 controls the gas supply mechanism to adjust the type, flow rate, etc. of gas introduced into the processing chamber 201. The control unit 220 also controls the high frequency bias power supply 213 to control the intensity of the high frequency voltage applied to the semiconductor substrate 211 on the sample stage 212.

[0050] When anisotropic etching is performed using the plasma processing apparatus 200, the control unit 220 controls the magnetic field generating coil 210 so that plasma is generated in the lower portion 201B of the processing chamber 201 below the porous plate 204. Since the porous plate 204 is made of a dielectric material, the microwaves pass through the porous plate 204 and interact with a magnetic field in the lower portion 201B of the processing chamber 201 to generate plasma. Furthermore, a high-frequency bias is applied to the sample stage 212 on which the Si substrate 1 serving as the semiconductor substrate 211 is placed. As a result, ions in the plasma are attracted to the Si substrate 1 without being blocked by the porous plate 204, etc., making it possible to perform etching while maintaining perpendicularity.

[0051] When isotropic etching is performed using the plasma processing apparatus 200, the control unit 220 controls the magnetic field generating coil 210 so that the plasma generation position is located at the upper portion 201A of the processing chamber 201 above the porous plate 204. Since ions in the plasma generated in the upper part 201A of the processing chamber 201 are blocked by the porous plate 204, only radicals in the plasma are supplied to the lower part 201B of the processing chamber. This enables isotropic etching using radicals.

[0052] When forming a film by the ALD method using the plasma processing apparatus 200, the following cycle process controlled by the control unit 220 may be applied. For example, when forming a Si3N4 film by the ALD method, In this case, the Si source BTBAS or BDEAS, or the gas SiH2Cl2 is used. When BTBAS or BDEAS is used, the liquid source is vaporized and sent to the gas line as a gas. The source gas is sent to the processing chamber 201 together with the carrier gas Ar, and the front side of the Si It is adsorbed on the substrate surface as a precursor. Then, it is purged using a purge gas such as Ar gas. Unnecessary precursors are exhausted from the processing chamber 201. Then, N2 gas or a mixture of N2 gas and H2 gas is Gas containing nitrogen, such as argon or NH3 gas, is flowed into the processing chamber 201 to generate plasma and react with the substrate surface. After this, an inert gas, such as Ar, is again flowed into the processing chamber 201 to purge the processing chamber 201, and unnecessary gases in the processing chamber 201 are exhausted. This series of processes achieves the following in principle: In essence, a Si3N4 film with an atomic layer thickness is deposited on the substrate surface. By repeating this process (performing a cycle process), a thin insulating film is formed by the ALD method. For example, when forming an Al2O3 film by the ALD method, Al(CH3)3 is used as the precursor of Al, vaporized H2O is used as the source of oxygen, and the same cycle as that for Si3N4 is used. It is advisable to carry out a sol-gel process to form an Al2O3 film. EXAMPLES

[0053] In the second embodiment, the gate-semiconductor substrate insulating separation film (311 in FIG. 6B: the gate A method for protecting a side wall of a Si channel when forming a semiconductor substrate insulating isolation film (corresponding to a semiconductor substrate insulating isolation film 11) is provided.

[0054] 6A shows the same diagram after removing the Si sacrificial layer 4A shown in FIG. 1J among the gate-semiconductor substrate insulating separation film forming steps (steps shown in FIG. 1A to FIG. 1N) described in Example 1. In this example, steps 101 to 109 in FIG. 4, that is, steps from vertical etching of the gate sidewall spacer shown in FIG. 1B to isotropic etching removal of the Si sacrificial layer 4A shown in FIG. 1J, are continuously processed in the same plasma processing device 200, and then the Si substrate 1 is taken out of the plasma processing device 200.

[0055] 6B, a gate-substrate isolation insulating film 311 is deposited, and the surface is planarized by CMP using a hard mask 307 as a stopper. For example, the film is formed by using a CVD method or the like. The material of the gate-substrate isolation insulating film 311 is, for example, SiO2, SiON, SiCO, etc. are used. By the above film formation, the region between the first SiGe sacrificial layer 303 and the Si substrate 301 is filled with the gate-substrate isolation insulating film 311, and the gate-substrate isolation insulating film 311 is also deposited on the side walls of the first protective insulating film 309 and the second protective insulating film 310.

[0056] In the step shown in FIG. 6C, the gate-substrate isolation insulating film 311 is etched back in the vertical direction. The amount of etching is preferably adjusted so that the upper surface of the gate-substrate isolation insulating film 311 after the etch-back is located between the lower surface of the second protective insulating film 310 and the upper surface of the lowermost first SiGe sacrificial layer 303. During this etch-back, the sidewalls of the laminated film consisting of the first SiGe sacrificial layer 303 and the Si channel 304 are protected by the first protective insulating film 309 and the second protective insulating film 310, so that the sidewalls of the Si channel 304 are not damaged by ions or radicals during the etch-back. This makes it possible to fabricate GAA-type FETs in which degradation of transistor characteristics due to etching damage is suppressed.

[0057] Next, in the step shown in FIG. 6D, the second protective insulating film 310 and the first protective insulating film 309 are sequentially removed by isotropic etching. The etching conditions other than the etching time may be the same as those in the first embodiment. After etching, the second protective insulating film 310 and the first protective insulating film 309 may be left so as to fill the inside of the groove formed between the gate-substrate isolation insulating film 311 and the first SiGe sacrificial layer 303. The etching times of the second protective insulating film 310 and the first protective insulating film 309 are adjusted so that the upper surfaces of the second protective insulating film 310 and the first protective insulating film 309 after etching are approximately aligned with the upper surface of the gate-substrate isolation insulating film 311. The remaining second protective insulating film 310 and first protective insulating film 309 are present in the groove, so that the groove can be used as a starting point in the subsequent process. This can suppress the occurrence of cavities. EXAMPLES

[0058] In the third embodiment, a method for simplifying the process of forming the gate sidewall inner spacer (12 in the first embodiment) is provided. Figures 7A to 7K are cross-sectional views of the process using this method, and Figure 8 is a flow diagram of the process using this method.

[0059] FIG. 7A shows a cross-sectional view in a direction perpendicular to the gate corresponding to the anisotropic etching process of the laminated film consisting of the first SiGe sacrificial layer 3B (402B in FIG. 7A) and the Si channel 4B (403B in FIG. 7A) shown in FIG. 1C. However, unlike FIG. 1C in which etching is performed up to the Si sacrificial layer 4A, the etching is stopped at the top of the Si sacrificial layer 403A. In this embodiment, after etching the laminated film consisting of the first SiGe sacrificial layer 402B and the Si channel 403B in the vertical direction in FIG. 7A, it is desirable to end the etching in a state in which the Si sacrificial layer 403A is exposed. The depth to which the Si sacrificial layer 403A is etched by overetching is preferably adjusted to a range of, for example, 0 nm to about 90% of the film thickness of the Si sacrificial layer 403A. This process corresponds to 502 in the process flow of FIG. 8, and the gate sidewall spacer shown in FIG. 1B is formed. It is preferable that this be performed continuously in the chamber of the same device, following the etching of the substrate 8 (501 in FIG. 8).

[0060] In FIG. 7B, the first SiGe sacrificial layer 402B is isotropically etched. The etching conditions are the same as those in Example 1. The hard mask 406, the gate sidewall spacer 407, and the STI insulating film (FIG. The etching is performed under selective etching conditions for the first SiGe sacrificial layer 402B and the Si channel 403B and the Si sacrificial layer 403A. The etching time is adjusted so that the etching amount is, for example, about 1 to 10 nm. This process corresponds to 503 in the process flow of FIG. 8, and is performed on the first SiGe sacrificial layer 402B and the Si channel 403B shown in FIG. 7A. Following the anisotropic etching of the laminated film (502 in FIG. 8), It is best to do this consecutively.

[0061] In FIG. 7C, a first protective insulating film 408 is deposited by a film formation technique using the ALD method. The first protective insulating film 408 is deposited on the upper surface and sidewalls of the hard mask 406 and the gate sidewall spacer 407, the sidewalls of the laminated film consisting of the first SiGe sacrificial layer 402B and the Si channel 403B, the upper surface of the Si sacrificial layer 403A, and the STI insulating film (not shown). Here, the first protective insulating film 408 is also formed in the groove formed by isotropically etching the first SiGe sacrificial layer 402B in FIG. 7B, and the first protective insulating film 408 is also deposited in the groove formed by isotropically etching the first SiGe sacrificial layer 402B in FIG. In this region, the first protective insulating film 408 is also formed on the upper and lower surfaces of the exposed Si channel 403B. The material of the first protective insulating film 408 is a laminated film consisting of the first SiGe sacrificial layer 402B and the Si channel 403B, and the Si sacrificial layer 403A. In consideration of the etching selectivity with respect to the surrounding STI insulating film (not shown), the insulating film containing nitrogen is It is preferable that the film is a Si3N4 film or a SiON film equivalent thereto. The thickness of the protective insulating film 408 is controlled to, for example, about 2 to 3 nm. The conditions may be the same as those in Example 1. This step corresponds to 504 in the process flow of FIG. Following the isotropic etching of the first SiGe sacrificial layer 402B shown in FIG. 7B (503 in FIG. 8), It is preferable to carry out the steps continuously in a chamber.

[0062] In the step shown in FIG. 7D, the first protective insulating film 408 is etched in the vertical direction. The etching includes a hard mask 406, a gate sidewall spacer 407, a Si sacrificial layer 403A, and an STI insulating film (not shown). For example, when the first protective insulating film 408 is a Si3N4 film, the etching conditions may be the same as those in the first embodiment. After this process, the upper surface of the Si sacrificial layer 403A is exposed. The etching conditions are controlled so that the remaining thickness of the Si sacrificial layer 403A after this etching is, for example, 10% to 100% of the initial thickness of the Si sacrificial layer 403A. The horizontal distance between the opening area of ​​the Si sacrificial layer 403A exposed after etching the protective insulating film 408 and the first SiGe sacrificial layer 402B is wider than that in the case of FIG. 1E in the first embodiment. Even if the first protective insulating film 408 is over-etched, unlike the case shown in FIG. 2B, The possibility that the sidewall of the first SiGe sacrificial layer 402B is exposed is low. This process corresponds to 505 in the process flow of FIG. 8, and is performed in the same process following the formation of the first protective insulating film 408 shown in FIG. 7C (504 in FIG. 8). It is preferable to perform the above steps consecutively in a chamber at the same location.

[0063] In the step shown in FIG. 7E, a second protective insulating film 409 is formed on the first protective insulating film 408 by the ALD method. The second protective insulating film 409 includes the hard mask 406, the gate sidewall spacer 407, and After the first protective insulating film 408 is formed, the first SiGe sacrificial layer 402B is deposited on the upper surface and sidewalls of the first protective insulating film 408, the upper surface of the Si sacrificial layer 403A, and the STI insulating film (not shown). If any gaps remain due to grooves formed by isotropic etching, a second protective insulating film 409 is formed in this process to fill the gaps. For the second protective insulating film 409, an Al2O3 film, an AlON film, or the like is used, which can be isotropically formed with good controllability even for complex shapes with finer unevenness. For example, when forming an Al2O3 film, the same conditions as those in Example 1 may be used. This step corresponds to 506 in the process flow of FIG. 8, and may be performed in succession in the chamber of the same device following the anisotropic etching of the first protective insulating film 408 shown in FIG. 7D (505 in FIG. 8). .

[0064] In the step shown in FIG. 7F, the second protective insulating film 409 is etched in the vertical direction. The etching is performed under selective etching conditions for the first protective insulating film 408, the hard mask 406, the gate sidewall spacer 407, the Si sacrificial layer 403A, and the STI insulating film (not shown). In the case of an Al2O3 film, the etching conditions may be the same as those in Example 1. The upper surface of the Si sacrificial layer 403A is exposed. The etching conditions are controlled so that the remaining thickness of the Si sacrificial layer 403A after this etching is, for example, 10% to 100% of the initial thickness of the Si sacrificial layer 403A. In the step of FIG. 7E, the second protective insulating film 409 is formed so as to fill the gap formed in the side wall of the first protective insulating film 408. In the subsequent etching of the Si sacrificial layer 403A and the second SiGe sacrificial layer 402A, the distance between the sidewall of the second protective insulating film 409 and the sidewall of the Si channel 403B can be sufficiently maintained. The corners of the sidewall of panel 403B are sufficiently protected. When the thickness of the first protective insulating film 408 becomes thin at the corner of the side wall of the Si channel 403B, There is a concern that the corners of the sidewalls of the Si channel 403B may be damaged during the etching that follows this step. This step corresponds to 507 in the process flow of Fig. 8, and may be performed continuously in the chamber of the same apparatus following the deposition of the second protective insulating film 409 shown in Fig. 7E (506 in Fig. 8).

[0065] In the step shown in FIG. 7G, the Si sacrificial layer 403A and the second SiGe sacrificial layer 402A are etched in the vertical direction. This etching is anisotropic selective etching using the hard mask 406, the gate sidewall spacer 407, and the second protective insulating film 409 as masks. The Si sacrificial layer 403A and the second SiGe sacrificial layer 402A are The second protective insulating film 409 is etched vertically along the sidewall thereof. In this step, the etching is terminated when the Si substrate 1 is exposed. The etching in this step may be performed under the same conditions as those used in anisotropic etching of the laminated film pattern of the SiGe layer 3 and the Si layer 4 in FIG. 1C of the first embodiment. This step corresponds to 508 in the process flow of FIG. 8, and is the second step shown in FIG. 7F. This may be performed successively in the chamber of the same device following the anisotropic etching of the protective insulating film 409 (507 in FIG. 8).

[0066] In the step shown in FIG. 7H, the second SiGe sacrificial layer 402A and the Si sacrificial layer 403A are sequentially removed by isotropic etching. The etching of the second SiGe sacrificial layer 402A may be performed under selective etching conditions for the second protective insulating film 409, the first protective insulating film 408, the hard mask 406, the gate sidewall spacer 407, the STI insulating film (not shown), the Si sacrificial layer 403A, and the Si substrate 401, similar to the conditions used in FIG. 1I of the first embodiment. The etching of the Si sacrificial layer 403A may be performed under selective etching conditions for the second protective insulating film 409, the first protective insulating film 408, the hard mask 406, the gate sidewall spacer 407, the STI insulating film (not shown), the Si sacrificial layer 403A, and the Si substrate 401, similar to the conditions used in FIG. 1I of the first embodiment. The selective etching conditions for the protective insulating film 408, the hard mask 406, the gate sidewall spacer 407, the STI insulating film (not shown), and the second SiGe sacrificial layer 402B may be similar to those used in FIG. 1J of the first embodiment. This process corresponds to 509 in the process flow of FIG. 8 and is shown in FIG. 7G. Following anisotropic etching (508 in FIG. 8) of the first Si sacrificial layer 403A and the second SiGe sacrificial layer 402A, This may be carried out continuously in a chamber of the apparatus.

[0067] In the step shown in FIG. 7I, the second protective insulating film 409 and the first protective insulating film 408 are sequentially removed by isotropic etching. The etching of the second protective insulating film 409 removes the first protective insulating film 408, the hard mask 406, the gate sidewall spacer 407, the STI insulating film (not shown), and the first SiGe sacrificial layer 402B. The etching is performed under selective etching conditions for the lower surface and the Si substrate 401. For example, when the second protective insulating film 409 is an Al2O3 film, the etching conditions shown in FIG. 1K of the first embodiment may be used. The etching of the protective insulating film 408 is a selective etching with respect to the hard mask 406, the gate sidewall spacer 407, the STI insulating film (not shown), the first SiGe sacrificial layer 402B, the Si channel 403B, and the Si substrate 401. For example, when the first protective insulating film 408 is a Si3N4 film, the etching conditions may be the same as those shown in FIG. 1K of the first embodiment. The side walls of the first SiGe sacrificial layer 402B and the Si channel 403B are exposed. The upper and lower surfaces of the Si channel 403B in the groove region formed by isotropically etching the first SiGe sacrificial layer 402B are also exposed at the same time. This process corresponds to 510 in the process flow diagram of FIG. 8, and is the same as the first process shown in FIG. 7H. Following the etching removal of the SiGe sacrificial layer 402A and the Si sacrificial layer 403A (509 in FIG. 8), In other words, the process flow shown in FIG. 8 includes the gate sidewall spacer vertical etching 501 (FIG. 1B) and the first and second protective insulating film isotropic etching. This makes it possible to continuously perform the steps up to the step of removing the silicide film 510 (FIG. 7I) in the same chamber of the same device.

[0068] Next, in the step shown in FIG. 7J, a gate-substrate isolation insulating film 410 is deposited, and the surface is planarized by CMP using the hard mask 406 as a stopper. The gate-substrate isolation insulating film 410 is For example, the film is formed by using a CVD method or the like. The material of the gate-substrate isolation insulating film 410 is, for example, By the above film formation, the region between the lower surface of the first SiGe sacrificial layer 402B and the Si substrate 401 is filled with the gate-substrate isolation insulating film 410, and the grooves between the side walls of the first SiGe sacrificial layer 402B and the upper and lower Si channels 403B are also filled with the gate-substrate isolation insulating film 410. do.

[0069] In the step shown in FIG. 7K, the gate-substrate isolation insulating film 410 is anisotropically etched in the vertical direction. The etching of the gate-substrate isolation insulating film 410 is performed under selective etching conditions for the hard mask 406, the gate sidewall spacer 407, the STI insulating film (not shown), and the sidewall of the Si channel 403B. The etching time is controlled so that the upper surface of the gate-substrate isolation insulating film 410 after etching is positioned between the lower surface and the upper surface of the bottom layer of the first SiGe sacrificial layer 402B. Thus, the grooves between the sidewalls of the first SiGe sacrificial layer 402B and the upper and lower Si channels 403B are filled with the interlayer insulating film 410, and simultaneously with the formation of the gate-substrate isolation insulating film 410, a gate sidewall inner spacer can be formed.

[0070] As described above, in this embodiment, the gate sidewall inner spacer is formed between the gate and the semiconductor substrate insulating layer. This makes it possible to form the first SiGe sacrificial layer 402B at the same time as the separation, and simplifies the process steps. Also, as shown in FIG. 7D, the first SiGe sacrificial layer 402B is prevented from being exposed when the protective insulating film is etched. Also, in this embodiment, the Si sacrificial layer 403A and the second SiGe sacrificial layer 402A are etched in a state in which the sidewalls of the first SiGe sacrificial layer 402B and the Si channel 403B stacked film have an uneven shape, but as shown in FIG. 7F, by providing the second protective insulating film 409, damage to the corners of the sidewalls of the Si channel 403B can also be reduced. EXAMPLES

[0071] In the fourth embodiment, a method is provided in which the protective insulating film is also used to reinforce the gate sidewall inner spacer.

[0072] 9A shows a cross-sectional view after isotropic etching of the first SiGe sacrificial layer 402B shown in FIG. 7B using the same process as in Example 3. In this example, the gate side shown in 501 in FIG. The wall spacer vertical etching and the first SiGe sacrificial film isotropic etching shown in 503 are performed in the same equipment. After these steps are performed continuously in the chamber of the apparatus, the Si substrate 601 is once taken out of the apparatus.

[0073] Then, in FIG. 9B, a low dielectric constant film 608 for forming a gate sidewall inner spacer is formed. For example, a CVD method is used to form the low dielectric constant film 608. For example, a SiCO film, a SiOCN film, a SiON film, a film similar thereto, or a laminated film of these may be used. After this process, the Si substrate 601 is again placed in the plasma processing apparatus that performed the process shown in FIG. 9A, and the processes shown in FIG. 9C and subsequent The process is carried out.

[0074] In FIG. 9C, the low dielectric constant film 608 is isotropically etched to form the gate sidewall inner slit. The above etching is performed under the same conditions as in Example 1, and the etching time is adjusted so that the sidewall of the Si channel 603B is exposed. After this etching, the sidewall of the gate sidewall inner spacer 608 is expected to have a curved shape.

[0075] In FIG. 9D, a first protective insulating film 609 is deposited by a film formation technique using the ALD method. The first protective insulating film 609 is formed on the hard mask 606 and the upper surface and side walls of the gate sidewall spacer 607, The first protective insulating film 609 is deposited on the sidewall of the sidewall inner spacer 608, the sidewall of the Si channel 603B, the upper surface of the Si sacrificial layer 603A, and the STI insulating film (not shown). 1D of 1 may be used. This process may be performed in succession in the chamber of the same device after the isotropic etching of the low dielectric constant film 608 shown in FIG. 9C. .

[0076] In the step shown in FIG. 9E, the first protective insulating film 609 is etched in the vertical direction. The etching includes a hard mask 606, a gate sidewall spacer 607, a Si sacrificial layer 603A, and an STI insulating film (not shown). The etching is performed under selective etching conditions for the first protective insulating film 609 (first insulating film 609 being a Si3N4 film). For example, when the first protective insulating film 609 is a Si3N4 film, the etching conditions shown in Example 1 may be used. After this process, the upper surface of the Si sacrificial layer 603A is exposed. The etching conditions are controlled so that the remaining film thickness of the Si sacrificial layer 603A after this etching is, for example, 10% to 100% of the initial film thickness of the Si sacrificial layer 603A. In the step shown in FIG. 9F, a second protective insulating film 610 is formed on the first protective insulating film 609 by the ALD method. The second protective insulating film 610 includes the hard mask 606, the gate sidewall spacer 607, and It is deposited on the upper surface and sidewalls of the first protective insulating film 609, the upper surface of the Si sacrificial layer 603A, and the STI insulating film (not shown). If a gap remains due to the curved shape of the gate sidewall spacer 607 after the deposition of the first protective insulating film 609 as shown in FIG. 9D, the second protective insulating film 610 is deposited in this process so as to fill the gap. The second protective insulating film 610 may be, for example, an Al2O3 film or an AlON film, which can be isotropically deposited with good controllability even on a complex shape with finer unevenness. For example, when forming an Al2O3 film, the same conditions as those in Example 1 may be used. The process is as follows: after the anisotropic etching of the first protective insulating film 609 shown in FIG. 9E, It is recommended that these be performed consecutively in a single chamber.

[0077] In the step shown in FIG. 9G, the second protective insulating film 610 is etched in the vertical direction. The etching is performed under selective etching conditions for the first protective insulating film 609, the hard mask 606, the gate sidewall spacer 607, the Si sacrificial layer 603A, and the STI insulating film (not shown). In the case of an Al2O3 film, the etching conditions may be the same as those in Example 1. The upper surface of the Si sacrificial layer 603A is exposed. The etching conditions are controlled so that the remaining thickness of the Si sacrificial layer 603A after this etching is, for example, 10% to 100% of the initial thickness of the Si sacrificial layer 603A. This step is performed in the same chamber as the deposition of the second protective insulating film 610 shown in FIG. 9F. , it is advisable to carry out these steps consecutively.

[0078] In the step shown in FIG. 9H, the Si sacrificial layer 603A and the second SiGe sacrificial layer 602A are etched in the vertical direction. This etching is anisotropic selective etching using the hard mask 606, the gate sidewall spacer 607, and the second protective insulating film 610 as masks. The Si sacrificial layer 603A and the second SiGe sacrificial layer 602A are The second protective insulating film 610 is etched vertically along the sidewall thereof. In this step, the etching is terminated when the Si substrate 601 is exposed. The etching in this step may be performed under the same conditions as those used in anisotropic etching of the laminated film pattern of the SiGe layer 3 and the Si layer 4 in FIG. 1C of the first embodiment. This step is anisotropic etching of the second protective insulating film 610 shown in FIG. 9G. It is preferable that these steps be performed successively in the chamber of the same apparatus.

[0079] In the step shown in FIG. 9I, the second SiGe sacrificial layer 602A and the Si sacrificial layer 603A are sequentially removed by isotropic etching. The etching of the second SiGe sacrificial layer 602A may be performed under selective etching conditions for the second protective insulating film 609, the first protective insulating film 608, the hard mask 606, the gate sidewall spacer 607, the STI insulating film (not shown), the Si sacrificial layer 603A, and the Si substrate 601, similar to the conditions used in FIG. 1I of the first embodiment. The etching of the Si sacrificial layer 603A may be performed under selective etching conditions for the second protective insulating film 610, the first protective insulating film 608, the hard mask 606, the gate sidewall spacer 607, the STI insulating film (not shown), the Si sacrificial layer 603A, and the Si substrate 601, similar to the conditions used in FIG. 1I of the first embodiment. The protective insulating film 609, the hard mask 606, the gate sidewall spacer 607, the gate sidewall inner spacer 608, the STI insulating film (not shown), and the first SiGe sacrificial layer 602B are selectively etched using selective etching conditions. 1J in Example 1. This step may be performed in the same chamber as the anisotropic etching of the Si sacrificial layer 603A and the second SiGe sacrificial layer 602A shown in FIG. 9H.

[0080] In the step shown in FIG. 9J, the second protective insulating film 610 and the first protective insulating film 609 are isotropically etched in sequence. The second protective insulating film 610 is etched under selective etching conditions for the first protective insulating film 609, the hard mask 606, the gate sidewall spacer 607, the STI insulating film (not shown), and the lower surface of the first SiGe sacrificial layer 602B, and the Si substrate 601. For example, when the second protective insulating film 610 is an Al2O3 film, the etching conditions shown in FIG. 1K of the first embodiment may be used. Here, the isotropic etching of the second protective insulating film 610 is performed by adjusting the etching time so that the sidewall of the first protective insulating film 609 is exposed after etching, but the sidewall of the gate sidewall inner spacer 608 is not exposed. The second protective insulating film 610 is adjusted so as to remain in the gaps caused by the curved shape. The etching of the first protective insulating film 609 is preferably performed by etching the second protective insulating film 610, the hard mask 606, the gate sidewall spacer 607, the STI insulating film (not shown), the gate sidewall inner spacer 608, and the like. The etching is performed under selective etching conditions for the spacer 608, the lower surface of the first SiGe sacrificial layer 602B, the Si channel 603B, and the Si substrate 601. For example, when the first protective insulating film 609 is a Si3N4 film, the etching conditions shown in FIG. 1K of the first embodiment may be used. In the etching in this process, the etching time is adjusted so that the gate sidewall spacer 607, the gate sidewall inner spacer 608, and the sidewalls of the Si channel 603B are exposed. However, due to the curved shape of the sidewall of the gate sidewall inner spacer 608, It is desirable to adjust so that the second protective insulating film 610 and the first protective insulating film 609 filling the gaps resulting from the above-mentioned process remain. This process is preferably performed in succession in the chamber of the same device, following the etching removal process of the second SiGe sacrificial layer 602A and the Si sacrificial layer 603A shown in FIG. 9I. That is, the isotropic etching of the low dielectric constant film for forming the gate sidewall inner spacer 608 shown in FIG. 9C is performed. It becomes possible to perform the etching process and the isotropic etching process of second protective insulating film 610 and first protective insulating film 609 shown in FIG. 9J consecutively in the chamber of the same device.

[0081] Thereafter, the process shown in FIG. 1L and subsequent figures of the first embodiment is carried out to complete the GAA FET. Since only the first protective insulating film 609 and the second protective insulating film 610 are filled in, current leakage caused by minute holes due to the recessed shape of the gate sidewall inner spacer 608 can be avoided. This makes it possible. [Explanation of symbols]

[0082] 1, 301, 401, 601: silicon substrate, 2, 302: element isolation (STI) insulating film, 3: single crystal silicon germanium layer, 3A, 402A, 602A: second silicon germanium sacrificial layer, 3B, 303, 402B, 602B: first silicon germanium sacrificial layer, 4: single crystal silicon layer, 4A, 403A, 603A: silicon sacrificial layer, 4B, 304, 403B, 603B: silicon channel layer, 5, 305, 404, 604: dummy gate 3, 4, 5, 6, 306, 405, 605: polycrystalline silicon dummy gate; 7, 307, 406, 606: hard mask; 8, 308, 407, 607: gate sidewall spacer; 9, 309, 408, 609: first protective insulating film; 10, 310, 409, 610: second protective insulating film; 11, 311, 410: gate-substrate isolation insulating film; 12, 608: gate sidewall inner spacer; 13: gate insulating film; 14: gate metal; 15: source / drain; 16: second interlayer insulating film; 17: contact barrier metal; 18: contact metal; 101, 501: gate sidewall spacer vertical etching process; 102, 502: silicon / silicon germanium Vertical etching process of the silicon laminated film, 503: first SiGe sacrificial film isotropic etching, 103, 504: first A protective insulating film depositing step, 104, 505: a first protective insulating film vertical etching step, 105, 506: a second protective insulating film depositing step, 106, 507: a second protective insulating film vertical etching step, 107: a second silicon Germanium sacrificial film anisotropic etching step, 108: second silicon germanium sacrificial film isotropic isotropic etching process, 109: silicon sacrificial film isotropic etching process, 508: silicon sacrificial film / Second silicon germanium sacrificial film anisotropic etching, 509: silicon sacrificial film / second silicon germanium sacrificial film isotropic etching, 110, 510: first / second protective insulating film isotropic etching 201: processing chamber (chamber), 201A: upper region of the processing chamber, 201B: lower region of the processing chamber, 202: vacuum exhaust port, 203: window, 204: porous plate, 205: gas source, 206: gas supply device, 207: gas inlet, 208: high frequency power supply for generating plasma, 209: waveguide, 210: magnetic field generating coil, 211: semiconductor substrate, 212: sample stage, 213: high frequency bias power supply, 220: control unit, 221: control signal, t1: horizontal thickness of first protective insulating film, t2: vertical thickness of first protective insulating film at bottom of groove, t3: horizontal thickness of second protective insulating film, t4: horizontal thickness of second protective insulating film at bottom of groove, t5: vertical thickness of second protective insulating film at bottom of groove, θ1: angle between side wall of silicon / silicon germanium laminate film and upper surface of second silicon germanium sacrificial layer 3A, θ2: angle between side wall of silicon / silicon germanium laminate film and lower surface of first protective insulating film after etching, a1: raw material gas flow path during formation of second protective insulating film, a2: ion irradiation path during etching of second protective insulating film.

Claims

1. A method for manufacturing a semiconductor device having a stacked channel in which thin line-shaped or sheet-shaped channels are stacked in a direction perpendicular to a substrate in a gate formation region, the gate and a semiconductor substrate being insulated and separated by an insulating film, comprising the steps of: The semiconductor device has a laminated film in which first semiconductor layers and second semiconductor layers are alternately laminated in a plurality of layers on the semiconductor substrate, the gate and gate sidewall spacer film are formed on the laminated film, a part of the laminated film is etched away along the gate sidewall spacer film, and a structure in which a part or all of a bottom first semiconductor layer or a part or all of a bottom second semiconductor layer formed on the bottom first semiconductor layer remains unetched, a first step of depositing a protective insulating film on a side wall of the laminated film formed by the etching and including the first semiconductor layer and the second semiconductor layer; a second step of anisotropically etching the protective insulating film in a vertical direction to expose a surface of the lowermost first semiconductor layer or the lowermost second semiconductor layer; a third step of repeating the first step and the second step a plurality of times using an insulating film material different from the protective insulating film to form a laminated film of the protective insulating film, which is made of the protective insulating film and a plurality of protective insulating films different from the protective insulating film, on the sidewall; A method for manufacturing a semiconductor device, comprising a fourth step of etching away the lowermost first semiconductor layer, or the lowermost first semiconductor layer and the lowermost second semiconductor layer.

2. In claim 1, A method for manufacturing a semiconductor device, comprising the steps of: successively carrying out the first step through the fourth step in the same plasma processing apparatus.

3. In claim 1, 2. A method for manufacturing a semiconductor device, comprising the steps of: forming a first semiconductor layer on a first insulating film; forming a second semiconductor layer on the first insulating film;

4. In claim 1, a first semiconductor layer and a second semiconductor layer formed on the first semiconductor layer and a second semiconductor layer formed on the second semiconductor layer, the first semiconductor layer being formed on the second semiconductor layer and the second semiconductor layer;

5. In claim 1, A method for manufacturing a semiconductor device, characterized in that after the second step, sidewalls of a second or subsequent first semiconductor layer stacked on the bottom first semiconductor layer are exposed, and the sidewalls are covered by the stacked film of the protective insulating film formed in the third step.

6. In claim 1, A method for manufacturing a semiconductor device, comprising the steps of: vertically etching the gate sidewall spacer film to form the gate sidewall spacer film; removing a portion of the laminated film consisting of the first semiconductor layer and the second semiconductor layer by vertical etching; and successively performing the first to fourth steps and a step of removing the laminated film of the protective insulating film by isotropic etching in the same plasma processing apparatus.

7. In claim 1, a step of vertically etching the gate sidewall spacer film to form the gate sidewall spacer film, a step of vertically etching and removing a portion of the laminated film consisting of the first semiconductor layer and the second semiconductor layer, and a step of successively performing the first to fourth steps in the same plasma processing apparatus, and a step of depositing and vertically etching a first insulating film for insulating and isolating the gate and the semiconductor substrate in a subsequent step.

8. In claim 1, A method for manufacturing a semiconductor device, comprising the steps of: removing a portion of the laminate film consisting of the first semiconductor layer and the second semiconductor layer by vertical etching; isotropically etching a sidewall of the first semiconductor layer other than the bottom layer; and then performing the first to fourth steps and a step of removing the laminate film of the protective insulating film by isotropic etching successively in the same plasma processing apparatus.

9. In claim 1, a step of isotropically etching a sidewall of the first semiconductor layer other than the bottom layer after removing a part of the laminated film consisting of the first semiconductor layer and the second semiconductor layer by vertical etching, and depositing a low dielectric constant film in a groove portion formed by the isotropic etching; a step of partially removing the low dielectric constant film by isotropic etching and forming a gate sidewall inner spacer made of the low dielectric constant film in the groove portion, the first step to the fourth step, and a step of partially removing the stacked film of the protective insulating film by isotropic etching are successively performed in a same plasma processing apparatus, and after the successive steps, the stacked film of the protective insulating film fills a gap formed on a sidewall of the gate sidewall inner spacer.

10. A plasma processing method for performing a plasma processing on a structure having a laminated film in which first semiconductor layers and second semiconductor layers are alternately laminated on a semiconductor substrate, a gate and a gate sidewall spacer film are further formed on the laminated film, a part of the laminated film is etched away along the gate sidewall spacer film, and a part or all of a bottom first semiconductor layer or a part or all of a bottom second semiconductor layer formed on the bottom first semiconductor layer remains unetched, a first step of depositing a protective insulating film on a side wall of the laminated film formed by the etching and including the first semiconductor layer and the second semiconductor layer; a second step of anisotropically etching the protective insulating film in a vertical direction to expose a surface of the lowermost first semiconductor layer or the lowermost second semiconductor layer; a third step of repeating the first step and the second step a plurality of times using an insulating film material different from the protective insulating film to form a laminated film of the protective insulating film on the sidewall; a fourth step of removing the lowermost first semiconductor layer, or the lowermost first semiconductor layer and the lowermost second semiconductor layer, by isotropic etching; Plasma treatment method.

11. In claim 10, A plasma processing method, comprising the steps of: vertical etching of the gate sidewall spacer film to form the gate sidewall spacer film; a step of removing a portion of the laminate film consisting of the first semiconductor layer and the second semiconductor layer by vertical etching; the first step to the fourth step; and a step of removing the laminate film of the protective insulating film by isotropic etching, all of which are performed in succession within one plasma processing apparatus.

12. In claim 10, A plasma processing method, comprising: a step of vertically etching the gate sidewall spacer film to form the gate sidewall spacer film; a step of vertically etching and removing a portion of the stacked film consisting of the first semiconductor layer and the second semiconductor layer; and the first to fourth steps, all of which are performed in one plasma processing apparatus.

13. In claim 10, a step of isotropically etching a sidewall of the first semiconductor layer other than the bottom first semiconductor layer, and then performing the first to fourth steps and a step of isotropically etching the stacked film of the protective insulating film in succession within one plasma processing apparatus.

14. In claim 10, a step of isotropically etching a sidewall of the first semiconductor layer other than the bottom first semiconductor layer after removing a part of the laminated film consisting of the first semiconductor layer and the second semiconductor layer by vertical etching, and depositing a low dielectric constant film in a groove portion formed by the isotropic etching; a step of partially removing the low dielectric constant film by isotropic etching and forming a gate sidewall inner spacer composed of the low dielectric constant film in the groove portion, the first step to the fourth step, and a step of partially removing the stacked film of the protective insulating film by isotropic etching, all of which are performed in one plasma processing apparatus.

15. In any one of claims 10 to 14, The plasma processing method, wherein in the first step and the third step, the protective insulating film is deposited by an ALD method.

Citation Information

Patent Citations

  • Multi-gate device and association method thereof

    JP2022027614A

  • Transistor gate structure and forming method

    JP2022027740A

  • Nanosheet substrate isolated source / drain epitaxy by nitrogen implantation

    US20190109052A1

  • Dielectric isolation layer between a nanowire transistor and a substrate

    US20190393351A1

  • Gate-all-around integrated circuit structures having depopulated channel structures using bottom-up approach

    US20200105756A1