Negative electrode active material and method for producing same
A silicon oxide-based negative electrode active material with a carbon coating and specific XPS peak structures addresses the instability issues in silicon-based batteries, enhancing capacity and cycle characteristics through structural stabilization and lithium diffusion.
Patent Information
- Application Number
- JP2021122790
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-27
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-07-27
AI Technical Summary
Lithium-ion secondary batteries using silicon-based negative electrode materials face challenges in achieving high battery capacity, initial efficiency, and cycle characteristics due to the expansion and contraction of silicon during charging and discharging, leading to structural instability and electrolyte consumption.
A negative electrode active material comprising silicon oxide particles coated with a carbon layer, containing Li2SiO3, with specific peak structures in XPS analysis, and a three-phase structure to stabilize the silicon oxide particles, ensuring stable lithium diffusion and structural integrity.
The solution enhances battery capacity, initial efficiency, and cycle characteristics by stabilizing the silicon oxide structure, preventing crystallinity increase, and ensuring effective lithium diffusion, thus improving overall battery performance.
Smart Images

Figure 0007561099000002 
Figure 0007561099000003 
Figure 0007561099000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode active material and a method for producing the same. [Background technology]
[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are small, lightweight, and capable of obtaining high energy density has been promoted. The application of these secondary batteries is being considered not only for small electronic devices, but also for large electronic devices such as automobiles and power storage systems such as homes.
[0003] Among these, lithium-ion secondary batteries are attracting great attention because they can be easily made small and have a high capacity, and because they offer a higher energy density than lead-acid batteries and nickel-cadmium batteries.
[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.
[0005] While carbon-based active materials are widely used as negative electrode active materials, recent market demands have called for further improvements in battery capacity. To improve battery capacity, the use of silicon as a negative electrode active material is being considered. This is because the theoretical capacity of silicon (4199mAh / g) is more than 10 times greater than that of graphite (372mAh / g), and a significant improvement in battery capacity can be expected. In the development of silicon materials as negative electrode active materials, not only silicon itself but also alloys and compounds such as oxides are being considered. In addition, the active material shape is being considered, ranging from the standard coating type for carbon-based active materials to an integrated type that is directly deposited on the current collector.
[0006] However, when silicon is used as the main raw material for the negative electrode active material, the negative electrode active material expands and contracts during charging and discharging, making it prone to cracking, mainly near the surface layer of the negative electrode active material. In addition, ionic substances are generated inside the active material, making the negative electrode active material prone to cracking. When the surface layer of the negative electrode active material cracks, a new surface is created, increasing the reaction area of the active material. At this time, a decomposition reaction of the electrolyte occurs on the new surface, and a coating, which is a decomposition product of the electrolyte, is formed on the new surface, consuming the electrolyte. This makes the cycle characteristics more likely to deteriorate.
[0007] To date, various studies have been conducted on negative electrode materials and electrode configurations for lithium-ion secondary batteries that use silicon materials as the main material in order to improve the initial battery efficiency and cycle characteristics.
[0008] Specifically, in order to obtain good cycle characteristics and high safety, silicon and amorphous silicon dioxide are simultaneously deposited using a gas phase method (see, for example, Patent Document 1). Also, in order to obtain high battery capacity and safety, a carbon material (electron conductive material) is provided on the surface layer of silicon oxide particles (see, for example, Patent Document 2). Furthermore, in order to improve cycle characteristics and obtain high input / output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio is formed near the current collector (see, for example, Patent Document 3). Also, in order to improve cycle characteristics, oxygen is contained in the silicon active material, and the active material is formed so that the average oxygen content is 40 at% or less and the oxygen content is high in the area close to the current collector (see, for example, Patent Document 4).
[0009] In addition, in order to improve the initial charge / discharge efficiency, the Si phase and SiO 2 , M y Nanocomposites containing metal oxides are used (see, for example, Patent Document 5). In addition, in order to improve cycle characteristics, SiO x(0.8 ≤ x ≤ 1.5, particle size range = 1 μm to 50 μm) is mixed with a carbon material and fired at high temperature (see, for example, Patent Document 6). Further, in order to improve the cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled within a range where the difference between the maximum value and the minimum value of the molar ratio near the active material and current collector interface is 0.4 or less (see, for example, Patent Document 7). Further, in order to improve the battery load characteristics, a metal oxide containing lithium is used (see, for example, Patent Document 8). Further, in order to improve the cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface layer of the silicon material (see, for example, Patent Document 9). Further, in order to improve the cycle characteristics, silicon oxide is used, and conductivity is imparted by forming a graphite film on its surface layer (see, for example, Patent Document 10). In Patent Document 10, regarding the shift value obtained from the RAMAN spectrum of the graphite film, broad peaks appear at 1330 cm -1 and 1580 cm -1 , and the intensity ratio I 1330 / I 1580 is such that 1.5 < I 1330 / I 1580 < 3. Further, in order to improve the high battery capacity and cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (see, for example, Patent Document 11). Further, in order to improve the overcharge and overdischarge characteristics, a silicon oxide in which the atomic ratio of silicon to oxygen is controlled to 1:y (0 < y < 2) is used (see, for example, Patent Document 12).
[0010] In addition, Hitachi Maxell started shipping a rectangular secondary battery for smartphones that adopted a nanosilicon composite in June 2010 for a lithium ion secondary battery using silicon oxide (see, for example, Non-Patent Document 1). The silicon oxide proposed by Hohl is a composite material of Si 0+ ~Si 4+ and has various oxidation states (Non-Patent Document 2). Also, Kapaklis proposed a disproportionation structure in which silicon oxide is divided into Si and SiO 2 by applying a heat load to the silicon oxide (Non-Patent Document 3).
[0011] Miyachi et al. have reported that the Si and SiO oxides that contribute to charging and discharging among the silicon oxides with disproportionated structures are 2 (Non-Patent Document 4), and Yamada et al. have proposed the following reaction formula between silicon oxide and Li (Non-Patent Document 5): 2SiO(Si+SiO 2 ) + 6.85Li+ + 6.85e - → 1.4Li 3.75 Si + 0.4Li 4 SiO 4 + 0.2SiO 2 In the reaction formula, silicon oxide consists of Si and SiO 2 reacts with Li to produce Li silicide, Li silicate, and some unreacted SiO 2 Divided into two.
[0012] The Li silicate formed here is irreversible, and once formed, it is a stable substance that does not release Li. The capacity per mass calculated from this reaction formula is close to the experimental value, and is recognized as the reaction mechanism of silicon oxide. Kim et al. have decomposed the irreversible component, Li silicate, associated with the charge and discharge of silicon oxide into Li 4 SiO 4 As, 7 Li-MAS-NMR and 29 The irreversible capacity was identified using Si-MAS-NMR (Non-Patent Document 6). This irreversible capacity is the weakest point of silicon oxide, and improvement is required. Therefore, Kim et al. have used the Li pre-doping method to form Li silicate in advance, significantly improving the initial efficiency as a battery and creating a negative electrode that can withstand practical use (Non-Patent Document 7).
[0013] Furthermore, instead of doping the electrode with Li, they proposed a method of treating the powder, which improved the irreversible capacity (Patent Document 13). [Prior art documents] [Patent documents]
[0014] [Patent Document 1] JP 2001-185127 A [Patent Document 2] JP 2002-042806 A [Patent Document 3] JP 2006-164954 A [Patent Document 4] JP 2006-114454 A [Patent Document 5] JP 2009-070825 A [Patent Document 6] JP 2008-282819 A [Patent Document 7] JP 2008-251369 A [Patent Document 8] JP 2008-177346 A [Patent Document 9] JP 2007-234255 A [Patent Document 10] JP 2009-212074 A [Patent Document 11] JP 2009-205950 A [Patent Document 12] Japanese Patent Application Publication No. 06-325765 [Patent Document 13] JP 2015-156355 A [Non-patent literature]
[0015] [Non-Patent Document 1] Battery Association of Japan's journal "Denchi", May 1, 2010 issue, page 10 [Non-Patent Document 2] A. Hohl, T. Wieder, PA van Aken, TE Weirich, G. Denninger, M. Vidal, S. Oswald, C. Deneke, J. Mayer, and H. Fuess: J. Non-Cryst. Solids, 320, (2003 ), 255. [Non-Patent Document 3] V. Kapaklis, J. Non-Crystalline Solids, 354 (2008) 612 [Non-Patent Document 4] Mariko Miyachi, Hironori Yamamoto, and Hidemasa Kawai, J. Electrochem. Soc. 2007 volume 154, issue 4, A376-A380 [Non-Patent Document 5] M. Yamada, A. Inaba, A. Ueda, K. Matsumoto, T. Iwasaki, T. Ohzuku, J. Electrochem. Soc., 159, A1630 (2012) [Non-Patent Document 6] Taeahn Kim, Sangjin Park, and Seung M. Oh, J. Electrochem. Soc. volume 154,(2007), A1112-A1117. [Non-Patent Document 7] Hye Jin Kim, Sunghun Choi, Seung Jong Lee, Myung Won Seo, Jae Goo Lee, Erhan Deniz, Yong Ju Lee, Eun Kyung Kim, and Jang Wook Choi,. Nano Lett. 2016, 16, 282-288. Summary of the Invention [Problem to be solved by the invention]
[0016] As mentioned above, in recent years, small electronic devices such as mobile terminals have been improved in performance and functionality, and lithium-ion secondary batteries, which are the main power sources for these devices, are required to have increased battery capacity. As one method to solve this problem, the development of lithium-ion secondary batteries consisting of a negative electrode mainly made of silicon material is desired. In addition, lithium-ion secondary batteries using silicon materials are expected to have initial charge / discharge characteristics and cycle characteristics that are similar to those of lithium-ion secondary batteries using carbon-based active materials. Therefore, by using silicon oxide modified by insertion and partial desorption of Li as the negative electrode active material, cycle characteristics and initial charge / discharge characteristics have been improved. However, sufficient battery characteristics could not be obtained by simply inserting Li and compounding it. This is because the state of the silicon compound that constitutes the bulk changes significantly due to the influence of various factors such as the raw material into which Li is inserted, the conditions of the carbon coating, the conditions for inserting Li, and the heat treatment conditions after insertion.
[0017] The present invention has been made in consideration of the above problems, and aims to provide a negative electrode active material that can increase battery capacity by improving initial efficiency (also referred to as early efficiency) and achieve sufficient battery cycle characteristics, and a method for producing the same. [Means for solving the problem]
[0018] In order to achieve the above object, the present invention provides a negative electrode active material including negative electrode active material particles, the negative electrode active material particles including silicon oxide particles coated with a carbon layer, the silicon oxide particles including Li 2 SiO 3 and in a Si2p spectrum obtained by XPS analysis, the negative electrode active material is characterized in that it has a most intense peak A at about 102 eV, a second most intense peak B at about 100 eV corresponding to a low valence Si compound having a valence of 1 to 3, and the intensity of peak C of Si:0 valence obtained at about 99 eV is half or less of the intensity of peak A.
[0019] The negative electrode active material of the present invention (hereinafter also referred to as silicon-based negative electrode active material) contains negative electrode active material particles (hereinafter also referred to as silicon-based negative electrode active material particles) containing silicon oxide particles, and therefore can improve the battery capacity. 2 SiO 3 By including Li, the initial efficiency is improved, and the slurry can be stabilized before application, resulting in a good electrode and improved battery characteristics. 2 SiO 3 has a peak near 102 eV in the Si2p spectrum obtained by XPS analysis. The fact that this peak is the strongest contributes to stability during charging and discharging and when slurried. In addition, in the negative electrode active material of the present invention, it is necessary that the Si2p spectrum obtained by XPS analysis has a peak of a low-valence Si compound state near 100 eV. This is because it is not the Si-Li reaction but the composite compound of Si, Li, and O that contributes to charging and discharging. However, if this peak becomes too strong, Li 2 SiO 3 The Si2p spectrum has a smaller peak intensity and a worsening structural stability, so it must be the second strongest peak. Also, in the Si2p spectrum, the Si0 peak intensity near 99 eV is higher than that of Li 2 SiO 3 The peak intensity must be less than half of that of the peak intensity of the Si-0 valence. If there are many zero valences of Si, degradation will occur more quickly.
[0020] Here, the negative electrode active material preferably has a structure having three or more phases.
[0021] In this way, when the negative electrode active material has three or more phase structures, the Li silicate (Li 2 SiO 3 ) is unlikely to shift the peak from around 102 eV to around 102.5 eV in the Si2p spectrum obtained by XPS analysis. This is because Li silicate (Li 2 SiO 3 This means that it is possible to prevent the crystallinity of (Cu) from becoming too high, and as a result, the diffusibility of Li can be ensured.
[0022] In addition, the negative electrode active material particles are preferably composed of three or more phase structures from the surface layer to the inside, with the outermost layer having the strongest peak at approximately 531 eV, a peak below that at approximately 528 eV, and a peak below that at approximately 532.5 eV in an O1S spectrum obtained by XPS analysis.
[0023] In the O1s spectrum obtained by XPS analysis of the negative electrode active material particles, the peak near 531 eV indicates the peak of the C,O compound present in the surface layer, and the peak near 528 eV indicates the peak of low-valence Si. Therefore, as described above, in the XPS analysis of the negative electrode active material particles, the O1s spectrum obtained in the surface layer has a peak of the C,O compound, and the O1s spectrum obtained in the lower phase has a peak of low-valence Si, which makes it easier for Li to be inserted into the negative electrode active material particles. In addition, the inside of the negative electrode active material particle bulk has a peak on the higher energy side in the O1s spectrum, which can stabilize the structure.
[0024] In addition, in the negative electrode active material particles, in the O1s spectrum obtained by the XPS analysis, it is preferable that a peak obtained near 532.5 eV is divided into two peaks near 532 eV and 533 eV.
[0025] In this way, the O1s peak that occurs on the highest energy side inside the negative electrode active material particle bulk is divided into two peaks, near 532 eV and near 533 eV, so that the negative electrode active material particle can be composed of a silicate component that has lower resistance and diffuses Li, and a silicate component that stabilizes the structure.
[0026] In addition, the negative electrode active material particles have a peak due to a Si(111) crystal plane obtained by X-ray diffraction using Cu-Kα radiation before charging and discharging the negative electrode active material particles, and the crystallite size corresponding to the crystal plane is 5.0 nm or less, and Li 2 SiO 3The ratio G / H of the intensity G of the peak due to the Si(111) crystal plane to the intensity H of the peak due to the (111) crystal plane is expressed by the following formula (1): 0.4≦G / H≦1.0 (1) It is preferable that the following is satisfied.
[0027] In this way, by having a peak due to the Si(111) crystal plane and a crystallite size corresponding to the crystal plane of 5.0 nm or less, the silicon oxide particles can be made to contain as little crystalline Si as possible. This makes it possible to suppress the reaction with the electrolyte and prevent deterioration of the battery characteristics. As described above, the crystallite size is preferably 5.0 nm or less, and it is preferably substantially amorphous. At this time, Li 2 SiO 3 Although Li also exhibits crystallinity, 2 SiO 3 The higher the crystallinity, the more stable the structure, but the higher the resistance. On the other hand, when the crystallinity is low, it becomes easier to dissolve in the slurry, so there is an optimal range. Therefore, it is preferable to satisfy the above formula (1).
[0028] The negative electrode active material particles preferably have a median diameter of 5.5 μm or more and 15 μm or less.
[0029] If the median diameter of the negative electrode active material particles is 5.5 μm or more, the reaction with the electrolyte is suppressed, and the deterioration of the battery characteristics can be suppressed. On the other hand, if the median diameter of the negative electrode active material particles is 15 μm or less, the expansion of the active material due to charging and discharging can be suppressed, and the electronic contact can be secured.
[0030] The carbon layer preferably has a portion in the outermost layer that exists in a compound state with oxygen.
[0031] In this way, the carbon layer has a portion in the outermost layer that exists in a compound state with oxygen, which allows the production of a substance similar to the coating structure that is produced during charging and discharging, thereby making it possible to further improve the battery characteristics.
[0032] The present invention also relates to a method for producing silicon oxide particles, a method for coating the silicon oxide particles with a carbon layer, a method for inserting lithium into the silicon oxide particles coated with the carbon layer by an oxidation-reduction method, and a method for producing a silicon oxide particle having lithium inserted therein by heat treating the silicon oxide particles having lithium inserted therein. 2 SiO 3 and forming silicon oxide particles containing the compound represented by the formula (I) into silicon oxide particles containing the compound represented by the formula (I), and then manufacturing a negative electrode active material by using the manufactured negative electrode active material particles. The method for manufacturing a negative electrode active material is characterized in that, by adjusting the temperature during the lithium insertion and the temperature during the heat treatment, the silicon oxide particles have, in a Si2p spectrum obtained by XPS analysis, a most intense peak A at about 102 eV, a second most intense peak B at about 100 eV corresponding to a low-valence Si compound having a valence of 1 to 3, and a peak C at about 99 eV for a valence of Si:0, the intensity of which is half or less of that of the peak A.
[0033] According to such a method for producing a negative electrode active material, it is possible to produce a negative electrode active material having each peak of the Si2p spectrum obtained by the above-mentioned XPS analysis. Effect of the Invention
[0034] The negative electrode active material of the present invention can provide high initial efficiency, high capacity, and high cycle characteristics when used as a negative electrode active material for a secondary battery. In addition, the method for producing the negative electrode active material of the present invention can produce a negative electrode active material that has high capacity and good initial charge / discharge characteristics when used as a negative electrode active material for a secondary battery while providing good cycle characteristics. [Brief description of the drawings]
[0035] [Figure 1] 1 shows a Si2p spectrum obtained by XPS analysis in Example 1. [Diagram 2] 1 shows a Si2p spectrum obtained by XPS analysis in Example 2. [Diagram 3] 13 is a Si2p spectrum obtained by XPS analysis in Example 3. [Figure 4] 1 shows a Si2p spectrum obtained by XPS analysis in Comparative Example 1. [Diagram 5] 13 is a Si2p spectrum obtained by XPS analysis in Comparative Example 2. [Figure 6] 13 is a Si2p spectrum obtained by XPS analysis in Comparative Example 3. [Figure 7] 13 is a Si2p spectrum obtained by XPS analysis in Comparative Example 4. [Figure 8] 13 is a Si2p spectrum obtained by XPS analysis in Comparative Example 5. [Figure 9] 1 is an O1s spectrum obtained by XPS analysis in Example 1. [Figure 10] 1 is an O1s spectrum obtained by XPS analysis in Comparative Example 1. [Figure 11] 1 is an O1s spectrum obtained by XPS analysis in Comparative Example 2. [Figure 12] FIG. 1 is a cross-sectional view showing an example of the configuration of a negative electrode for a lithium ion secondary battery containing the negative electrode active material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] Hereinafter, the present invention will be described in detail with reference to the preferred embodiments, but the present invention is not limited thereto.
[0037] As mentioned above, as one method for increasing the battery capacity of a lithium-ion secondary battery, the use of a negative electrode mainly made of silicon oxide as the negative electrode of the lithium-ion secondary battery has been considered. The lithium-ion secondary battery using this silicon oxide is expected to have initial charge / discharge characteristics similar to those of a lithium-ion secondary battery using a carbon-based active material. In addition, in Li-doped SiO, which can improve the initial charge / discharge characteristics, cycle characteristics similar to those of a carbon-based active material are expected. However, a silicon-based negative electrode active material that shows battery characteristics equivalent to those of a carbon-based active material when used as a negative electrode active material of a lithium-ion secondary battery has not yet been proposed.
[0038] Therefore, the inventors of the present invention have conducted extensive research in order to obtain a negative electrode active material that, when used as a negative electrode active material for a secondary battery, can provide high cycle characteristics while improving initial charge / discharge characteristics, thereby increasing battery capacity, and have arrived at the present invention.
[0039] [Negative electrode active material of the present invention] The negative electrode active material of the present invention is a negative electrode active material containing negative electrode active material particles, the negative electrode active material particles containing silicon oxide particles coated with a carbon layer, and the silicon oxide particles are Li 2 SiO 3 and in a Si2p spectrum obtained by XPS analysis, the strongest peak A is present at about 102 eV, the second strongest peak B is present at about 100 eV and corresponds to a low-valence Si compound having a valence of 1 to 3, and the intensity of peak C of Si:0 valence obtained at about 99 eV is half or less of the intensity of peak A.
[0040] XPS analysis can be performed, for example, by using a scanning X-ray photoelectron spectrometer PHI Quantera II manufactured by ULVAC-PHI, Inc. In this case, the X-ray beam diameter can be set to 100 μm, and a neutralization gun can be used.
[0041] The negative electrode active material of the present invention contains negative electrode active material particles containing silicon oxide particles, and therefore the battery capacity can be improved. 2 SiO 3 By forming this, the slurry can be stabilized before application, resulting in a good electrode and improved battery characteristics. 2 SiO 3has a peak near 102 eV in the Si2p spectrum obtained by XPS analysis. The fact that this peak is the strongest contributes to stability during charging and discharging and when slurried. In addition, in the negative electrode active material of the present invention, it is necessary to have a low-valence Si compound state near 100 eV in the Si2p spectrum obtained by XPS analysis. This is because a composite compound of Si, Li, and O contributes to charging and discharging, not a Si-Li reaction. However, if this peak becomes too strong, the Li 2 SiO 3 The Si2p spectrum has a smaller Si peak near 99 eV, and the structural stability is deteriorated. 2 SiO 3 The peak intensity must be less than half of that of the silicon. If the valence of silicon is high, deterioration will occur quickly. The carbon coating not only provides electrical conductivity, but also has a certain effect on water resistance.
[0042] In addition, the negative electrode active material of the present invention preferably has three or more phase structures. When it has three or more phase structures, the Li silicate (Li 2 SiO 3 ) is unlikely to shift the peak from around 102 eV to around 102.5 eV in the Si2p spectrum obtained by XPS analysis. This is because Li silicate (Li 2 SiO 3 This means that it is possible to prevent the crystallinity of (Cu) from becoming too high, and as a result, the diffusibility of Li can be ensured.
[0043] In the negative electrode active material of the present invention, the negative electrode active material particles are preferably composed of three or more phase structures from the surface layer to the inside, in which the outermost layer has the strongest peak at approximately 531 eV, a peak below that at approximately 528 eV, and a peak below that at approximately 532.5 eV in an O1s spectrum obtained by XPS analysis.
[0044] In the O1s spectrum obtained by XPS analysis, the peak near 531 eV indicates the peak of the C,O compound present in the surface layer, and the peak near 528 eV indicates the peak of low-valence Si. Therefore, as described above, the negative electrode active material particles have a peak of the C,O compound in the surface layer and a peak of low-valence Si in the lower phase, which makes it easier for Li to be inserted into the negative electrode active material particles. In addition, in the O1s spectrum, the inside of the negative electrode active material particle bulk has a peak on the higher energy side, which can stabilize the structure.
[0045] In the negative electrode active material of the present invention, the negative electrode active material particles preferably have a peak obtained near 532.5 eV in the O1s spectrum obtained by XPS analysis, which is divided into two peaks near 532 eV and 533 eV. In this way, it is desirable that the O1s peak occurring on the highest energy side inside the negative electrode active material particle bulk is divided into two peaks near 532 eV and 533 eV. This allows the negative electrode active material to be composed of a silicate component that has a lower resistance and diffuses Li, and a silicate component that stabilizes the structure.
[0046] In addition, the negative electrode active material particles of the present invention preferably have the following configuration before charging and discharging the negative electrode active material particles. That is, it is preferable that the negative electrode active material particles have a peak due to the Si(111) crystal plane obtained by X-ray diffraction using Cu-Kα rays, and the crystallite size corresponding to the crystal plane is 5.0 nm or less. Furthermore, in addition to that, Li 2 SiO 3 The ratio G / H of the intensity G of the peak due to the Si(111) crystal plane to the intensity H of the peak due to the (111) crystal plane is expressed by the following formula (1): 0.4≦G / H≦1.0 (1) It is preferable that the following is satisfied.
[0047] In this way, by having a peak due to the Si(111) crystal plane and setting the crystallite size corresponding to the crystal plane to 5.0 nm or less, it is possible to make the silicon oxide particles contain as little crystalline Si as possible. This makes it possible to suppress the reaction with the electrolyte and prevent deterioration of the battery characteristics. As described above, the crystallite size is preferably 5.0 nm or less, and it is preferably substantially amorphous. At this time, Li 2 SiO 3 Although Li also exhibits crystallinity, 2 SiO 3 The higher the crystallinity, the more stable the structure, but the higher the resistance. On the other hand, when the crystallinity is low, it becomes easier to dissolve in the slurry, so there is an optimal range. Therefore, it is preferable to satisfy the above formula (1).
[0048] In the negative electrode active material of the present invention, the negative electrode active material particles preferably have a median diameter of 5.5 μm or more and 15 μm or less. If the negative electrode active material particles have a median diameter of 5.5 μm or more, the reaction with the electrolyte is suppressed, and the deterioration of the battery characteristics can be suppressed. On the other hand, if the negative electrode active material particles have a median diameter of 15 μm or less, the expansion of the active material due to charging and discharging can be suppressed, and electronic contact can be ensured.
[0049] In addition, the carbon layer preferably has a portion that exists in a compound state with oxygen in the outermost layer. In this way, by having a portion that exists in a compound state with oxygen in the outermost layer, a substance similar to the coating structure generated during charging and discharging can be generated, which makes it possible to further improve the battery characteristics. <Non-aqueous electrolyte secondary battery negative electrode>
[0050] [Negative electrode composition] Next, the configuration of the negative electrode of the secondary battery containing such a negative electrode active material of the present invention will be described.
[0051] Fig. 12 shows a cross-sectional view of a negative electrode containing the negative electrode active material of the present invention. As shown in Fig. 12, a negative electrode 10 has a negative electrode active material layer 12 on a negative electrode current collector 11. This negative electrode active material layer 12 may be provided on both sides or only one side of the negative electrode current collector 11. Furthermore, if the negative electrode active material of the present invention is used, the negative electrode current collector 11 may not be necessary.
[0052] [Negative electrode current collector] The negative electrode current collector 11 is made of a material having excellent electrical conductivity and excellent mechanical strength. Examples of the conductive material that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). It is preferable that this conductive material is a material that does not form an intermetallic compound with lithium (Li).
[0053] The negative electrode current collector 11 preferably contains carbon (C) and / or sulfur (S) in addition to the main elements. This is because the physical strength of the negative electrode current collector is improved. In particular, when the current collector has an active material layer that expands during charging, if the current collector contains the above elements, this has the effect of suppressing deformation of the electrode including the current collector. The contents of the above contained elements are not particularly limited, but are preferably 100 mass ppm or less for each. This is because a higher deformation suppression effect can be obtained. Such a deformation suppression effect can further improve cycle characteristics.
[0054] The surface of the negative electrode current collector 11 may be roughened or may not be roughened. The roughened negative electrode current collector is, for example, a metal foil that has been electrolytically treated, embossed, or chemically etched. The unroughened negative electrode current collector is, for example, a rolled metal foil.
[0055] [Negative electrode active material layer] The negative electrode active material layer 12 contains the negative electrode active material of the present invention capable of absorbing and releasing lithium ions, and may further contain other materials such as a negative electrode binder and a conductive assistant from the viewpoint of battery design. The negative electrode active material contains negative electrode active material particles, and the negative electrode active material particles contain silicon oxide particles.
[0056] The negative electrode active material layer 12 may also contain a mixed negative electrode active material containing the negative electrode active material of the present invention (silicon-based negative electrode active material) and a carbon-based active material. This reduces the electrical resistance of the negative electrode active material layer and can alleviate the expansion stress caused by charging. Examples of the carbon-based active material that can be used include pyrolytic carbons, cokes, glassy carbon fibers, organic polymer compound sintered bodies, and carbon blacks.
[0057] As described above, the negative electrode active material of the present invention contains silicon oxide particles. The ratio of silicon to oxygen in the silicon oxide constituting the silicon oxide particles is SiO x It is preferable that the range of x is 0.8≦x≦1.2. If x is 0.8 or more, the oxygen ratio is higher than that of silicon alone, and therefore the cycle characteristics are good. If x is 1.2 or less, the resistance of the silicon oxide particles does not become too high, which is preferable. Among these, SiO x In the composition, it is preferable that x is close to 1, because this allows for high cycle characteristics to be obtained. Note that the composition of the silicon oxide particles in the present invention does not necessarily mean 100% purity, and may contain trace amounts of impurity elements.
[0058] In the negative electrode active material of the present invention, as described above, the negative electrode active material particles contain silicon oxide particles coated with a carbon layer, and the silicon oxide particles contain Li as a Li compound. 2 SiO 3 Furthermore, in the Si2p spectrum obtained by XPS analysis, the silicon oxide particles have the most intense peak A at about 102 eV, the second most intense peak B at about 100 eV corresponding to a low valence Si compound having a valence of 1 to 3, and the intensity of peak C of Si:0 valence obtained at about 99 eV is half or less than the intensity of peak A.
[0059] The degree of Li silicate enlargement and the degree of Si crystallization (for example, the crystallite size corresponding to the Si(111) crystal plane) can be confirmed by XRD (X-ray Diffraction). XRD measurement can be performed, for example, under the following conditions. The X-ray diffraction device used may be, for example, the D8 ADVANCE manufactured by Bruker. The X-ray source is Cu Kα radiation, and a Ni filter is used. Measurements are performed from 10 to 40° with an output of 40 kV / 40 mA, a slit width of 0.3°, a step width of 0.008°, and a counting time of 0.15 seconds per step.
[0060] The negative electrode binder contained in the negative electrode active material layer may be, for example, one or more of polymer materials, synthetic rubber, etc. Examples of the polymer materials include polyvinylidene fluoride, polyimide, polyamideimide, aramid, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, carboxymethyl cellulose, etc. Examples of the synthetic rubber include styrene butadiene rubber, fluorine-based rubber, ethylene propylene diene, etc.
[0061] As the negative electrode conductive assistant, for example, one or more of carbon materials such as carbon black, acetylene black, graphite, Ketjen black, carbon nanotubes, and carbon nanofibers can be used.
[0062] The negative electrode active material layer is formed, for example, by a coating method, in which the silicon-based negative electrode active material is mixed with the binder and, if necessary, a conductive additive and a carbon-based active material, and then the mixture is dispersed in an organic solvent, water, or the like and coated.
[0063] [Method of manufacturing the negative electrode] Next, an example of a method for producing the negative electrode active material of the present invention will be described.
[0064] The method for producing a negative electrode active material of the present invention includes the steps of preparing silicon oxide particles, coating the silicon oxide particles with a carbon layer, inserting lithium into the silicon oxide particles coated with the carbon layer by an oxidation-reduction method, and heat-treating the silicon oxide particles into which lithium has been inserted to obtain Li 2 SiO 3 and forming silicon oxide particles containing the above. The negative electrode active material particles are then used to manufacture a negative electrode active material. At this time, the temperature during lithium insertion and the temperature during heat treatment are adjusted so that the silicon oxide particles have a most intense peak A at about 102 eV, a second most intense peak B at about 100 eV corresponding to a low valence Si compound having a valence of 1 to 3, and a peak C of Si:0 valence obtained at about 99 eV, the intensity of which is half or less than that of peak A, in a Si2p spectrum obtained by XPS analysis.
[0065] More specifically, the negative electrode active material is produced, for example, by the following procedure.
[0066] First, silicon oxide particles are prepared. In the following, silicon oxide particles are prepared using SiO x The case where silicon oxide represented by (0.5≦x≦1.6) is used will be described. First, a raw material that generates silicon oxide gas is heated in the presence of an inert gas and under reduced pressure at a temperature range of 900°C to 1600°C to generate silicon oxide gas. In this case, a mixture of metallic silicon powder and silicon dioxide powder can be used as the raw material. Considering the surface oxygen of the metallic silicon powder and the presence of trace oxygen in the reactor, it is desirable for the mixed molar ratio to be in the range of 0.9<metallic silicon powder / silicon dioxide powder<1.2.
[0067] The generated silicon oxide gas is solidified and deposited on the adsorption plate. Next, the temperature inside the reactor is lowered to 100°C or less, and the silicon oxide deposit is taken out and pulverized into powder using a ball mill, jet mill, or the like. In this manner, silicon oxide particles can be produced. The Si crystallites in the silicon oxide particles can be controlled by changing the vaporization temperature of the raw material that generates the silicon oxide gas, or by heat treatment after the generation of the silicon oxide particles.
[0068] Here, a carbonaceous layer is formed on the surface of the silicon oxide particles. A pyrolytic CVD method is preferable as a method for forming the carbonaceous layer. An example of a method for forming a carbonaceous layer by the pyrolytic CVD method will be described below.
[0069] First, silicon oxide particles are placed in a furnace. Next, a hydrocarbon gas is introduced into the furnace, and the temperature inside the furnace is increased. The decomposition temperature is preferably 900°C or less, and more preferably 850°C or less. By setting the decomposition temperature at 900°C or less, unintended disproportionation of the active material particles can be suppressed. After the temperature inside the furnace is increased to a predetermined temperature, a carbon layer is generated on the surface of the silicon oxide particles. The hydrocarbon gas that is the raw material for the carbon material is not particularly limited, but may be C n H m In the composition, it is desirable for n to be ≦ 2. If n ≦ 2, the production cost can be reduced and the physical properties of the decomposition products can be improved.
[0070] Next, Li is inserted into the silicon oxide particles prepared as described above. This produces negative electrode active material particles containing silicon oxide particles with lithium inserted. That is, this modifies the silicon oxide particles, and a Li compound (Li silicate) is produced inside the silicon oxide particles. In the method for producing a negative electrode active material of the present invention, Li is inserted by the oxidation-reduction method as described above.
[0071] In the modification by the oxidation-reduction method, for example, first, lithium can be inserted by immersing silicon active material particles in solution A in which lithium is dissolved in an ether-based solvent. This solution A may further contain a polycyclic aromatic compound or a linear polyphenylene compound. After lithium insertion, active lithium can be desorbed from the silicon active material particles by immersing the silicon active material particles in solution B containing a polycyclic aromatic compound or its derivative. The solvent for this solution B can be, for example, an ether-based solvent, a ketone-based solvent, an ester-based solvent, an alcohol-based solvent, an amine-based solvent, or a mixed solvent thereof. Alternatively, after immersion in solution A, the obtained silicon active material particles may be heat-treated under an inert gas. The Li compound can be stabilized by heat treatment. After that, washing may be performed using a method such as washing with alcohol, alkaline water in which lithium carbonate is dissolved, weak acid, or pure water.
[0072] As the ether solvent used in solution A, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, or a mixture thereof can be used. Among these, it is particularly preferable to use tetrahydrofuran, dioxane, or 1,2-dimethoxyethane. These solvents are preferably dehydrated and deoxygenated.
[0073] Furthermore, the polycyclic aromatic compound contained in solution A may be one or more of naphthalene, anthracene, phenanthrene, naphthacene, pentacene, pyrene, picene, triphenylene, coronene, chrysene, and derivatives thereof, and the linear polyphenylene compound may be one or more of biphenyl, terphenyl, and derivatives thereof.
[0074] The polycyclic aromatic compound contained in solution B may be one or more of naphthalene, anthracene, phenanthrene, naphthacene, pentacene, pyrene, picene, triphenylene, coronene, chrysene, and derivatives thereof.
[0075] As the ether solvent for solution B, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and the like can be used.
[0076] As the ketone solvent, acetone, acetophenone, etc. can be used.
[0077] As the ester solvent, methyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, and the like can be used.
[0078] As the alcohol-based solvent, methanol, ethanol, propanol, isopropyl alcohol, and the like can be used.
[0079] As the amine solvent, methylamine, ethylamine, ethylenediamine, and the like can be used.
[0080] The Li silicate thus formed is mainly Li 4 SiO 4 In this state, it is difficult to make a battery. 2 SiO 3 The degree of crystallization of Li silicate and Si changes depending on the temperature at this time. In addition, the reaction temperature during Li insertion also plays a role. In particular, if Li is inserted at a temperature close to the boiling point of the solvent used, the crystallinity of Si will appear in the next heat treatment process even though the crystallinity of Li silicate will not be that large. Therefore, the balance between the heat treatment and Li insertion process is important.
[0081] Also, if the temperature during Li insertion is too low, the reactivity is low. At least 50°C or higher is preferable. At such a temperature, the reactivity during Li insertion can be ensured. By increasing the reactivity during Li insertion to a predetermined level or higher, it is possible to prevent the Li concentration in the particle surface layer from becoming too high, and as a result, it is possible to suppress the progress of disproportionation in the surface layer during the heat treatment in the next step.
[0082] The C,O compound in the outermost layer does not contain oxygen, for example the polycyclic aromatic compound biphenyl, and O cannot be introduced from substances that form complexes with Li. Therefore, it is necessary to use O contained in solvent A. When releasing Li from the complex, it is desirable to decompose it by involving the solvent. However, as it is unstable in this state, it is preferable to apply heat treatment to partially decompose it and form a stabilizing layer. This is called a pseudo-SEI coating, and when used as a battery, it enables smart transfer of Li.
[0083] The material that has been subjected to Li doping by the oxidation-reduction method can be subjected to heat treatment at 500°C to 650°C after filtration to control the type and amount (abundance ratio) of Li silicate. When performing such control, it is important to perform heat treatment in a vacuum state or under inert gas. In addition, it is preferable to use a heat treatment device, not limited to the device here, for uniform heat treatment such as a rotary kiln. At this time, various Li silicate states can be created by using the vacuum state, inert gas flow rate (internal pressure), retort thickness, and rotation speed as factors. Those skilled in the art can easily determine experimentally what Li silicate state is created under what conditions. Similarly, silicon enlargement or amorphization of silicon can be controlled. Those skilled in the art can easily determine experimentally what conditions these controls are performed under.
[0084] In the method for producing the negative electrode active material of the present invention, the temperature during the lithium insertion and the temperature during the heat treatment are adjusted to produce silicon oxide particles having the strongest peak A near 102 eV in the Si2p spectrum obtained by XPS analysis, the second strongest peak B corresponding to a low valence Si compound having a valence of 1 to 3 near 100 eV, and the intensity of the peak C of the Si:0 valence obtained near 99 eV is half or less than that of the peak A. Such conditions can be easily obtained experimentally by a person skilled in the art. In particular, the temperature during the lithium insertion and the temperature during the heat treatment are adjusted, but it is preferable to adjust the temperature during SiO deposition and the CVD temperature in addition to them.
[0085] The negative electrode active material prepared as described above is mixed with other materials such as a negative electrode binder and a conductive assistant to form a negative electrode mixture, and then an organic solvent or water is added to form a slurry. Next, the above-mentioned slurry is applied to the surface of the negative electrode current collector and dried to form a negative electrode active material layer. At this time, hot pressing or the like may be performed as necessary. In this manner, a negative electrode can be prepared.
[0086] [Separator] The separator separates the positive and negative electrodes, prevents current short circuit caused by contact between the electrodes, and allows lithium ions to pass through. The separator is formed of a porous film made of, for example, synthetic resin or ceramic, and may have a laminated structure in which two or more types of porous films are laminated. Examples of synthetic resins include polytetrafluoroethylene, polypropylene, and polyethylene.
[0087] [Electrolyte] At least a portion of the active material layer or the separator is impregnated with a liquid electrolyte (electrolytic solution). This electrolytic solution contains an electrolyte salt dissolved in a solvent, and may contain other materials such as additives.
[0088] The solvent may be, for example, a non-aqueous solvent. Examples of non-aqueous solvents include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, or tetrahydrofuran. Among these, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. This is because better characteristics can be obtained. In this case, more advantageous characteristics can be obtained by combining a high-viscosity solvent such as ethylene carbonate or propylene carbonate with a low-viscosity solvent such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. This is because the dissociation property and ion mobility of the electrolyte salt are improved.
[0089] When an alloy-based negative electrode is used, it is particularly desirable that the solvent contains at least one of halogenated chain carbonates or halogenated cyclic carbonates. This allows a stable coating to be formed on the surface of the negative electrode active material during charging and discharging, particularly during charging. Here, the halogenated chain carbonate is a chain carbonate having a halogen as a constituent element (at least one hydrogen is substituted with a halogen). Also, the halogenated cyclic carbonate is a cyclic carbonate having a halogen as a constituent element (i.e., at least one hydrogen is substituted with a halogen).
[0090] The type of halogen is not particularly limited, but fluorine is preferred because it forms a better coating than other halogens. Also, the more halogens there are, the more desirable they are because the resulting coating is more stable and the decomposition reaction of the electrolyte is reduced.
[0091] Examples of halogenated chain carbonates include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. Examples of halogenated cyclic carbonates include 4-fluoro-1,3-dioxolan-2-one, 4,5-difluoro-1,3-dioxolan-2-one, etc.
[0092] It is preferable that the solvent additive contains an unsaturated carbon-bonded cyclic carbonate. This is because a stable coating is formed on the negative electrode surface during charging and discharging, and the decomposition reaction of the electrolyte can be suppressed. Examples of the unsaturated carbon-bonded cyclic carbonate include vinylene carbonate and vinylethylene carbonate.
[0093] It is also preferable that the solvent additive contains sultone (cyclic sulfonic acid ester), because this improves the chemical stability of the battery. Examples of sultones include propane sultone and propene sultone.
[0094] Furthermore, it is preferable that the solvent contains an acid anhydride, because this improves the chemical stability of the electrolyte. As the acid anhydride, for example, propane disulfonic acid anhydride can be mentioned.
[0095] The electrolyte salt may include at least one of light metal salts such as a lithium salt. Examples of the lithium salt include lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ) etc.
[0096] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent, because this provides high ionic conductivity. EXAMPLES
[0097] The present invention will be described in more detail below by showing examples and comparative examples of the present invention, but the present invention is not limited to these examples.
[0098] [Common conditions for the examples] First, the negative electrode active material was prepared as follows. A mixture of silicon metal and silicon dioxide was introduced into a reactor, vaporized in a vacuum of 10 Pa, and deposited on an adsorption plate. After sufficient cooling, the deposit was taken out and pulverized in a ball mill. The SiO xThe value of x was 1.0. The particle size of the silicon oxide particles was then adjusted by classification. After that, the surfaces of the silicon oxide particles were coated with a carbon material by performing pyrolysis CVD at a temperature range of 700°C to 900°C.
[0099] Next, a solvent with a water content reduced to 50 ppm was used to insert lithium into the silicon oxide particles by an oxidation-reduction method, followed by heating at a temperature in the range of 450°C to 650°C for further modification.
[0100] Next, the prepared negative electrode active material (silicon oxide particles), graphite, conductive additive 1 (carbon nanotubes, CNT), conductive additive 2 (carbon particles with a median diameter of approximately 50 nm), sodium polyacrylate, and carboxymethyl cellulose (hereinafter referred to as CMC) were mixed in a dry mass ratio of 9.3:83.7:1:1:4:1, and then diluted with pure water to prepare a negative electrode mixture slurry.
[0101] In addition, an electrolytic copper foil with a thickness of 15 μm was used as the negative electrode current collector. This electrolytic copper foil contained carbon and sulfur at a concentration of 70 mass ppm each. Finally, the negative electrode mixture slurry was applied to the negative electrode current collector and dried at 100° C. for 1 hour in a vacuum atmosphere. After drying, the deposition amount of the negative electrode active material layer per unit area on one side of the negative electrode (also called the area density) was 7.0 mg / cm 2 It was.
[0102] Next, the solvents ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed, and then the electrolyte salt (lithium hexafluorophosphate: LiPF 6 ) was dissolved in the electrolyte to prepare the electrolyte. In this case, the solvent composition was EC:DMC=30:70 in volume ratio, and the content of the electrolyte salt was 1 mol / kg relative to the solvent. As additives, vinylene carbonate (VC) and fluoroethylene carbonate (FEC) were added at 1.0 wt% and 2.0 wt%, respectively.
[0103] Next, a coin battery was assembled as follows. First, a 1 mm thick Li foil was punched out to a diameter of 16 mm and attached to an aluminum clad. The resulting negative electrode was punched out to a diameter of 15 mm, and the Li foil was placed face-to-face with a separator in between. After injecting the electrolyte, a 2032 coin battery was produced.
[0104] The initial efficiency was measured under the following conditions. First, the charge rate was set to 0.03C. At this time, charging was performed in CCCV mode. CV was set to 0V and the final current was set to 0.04mA. The discharge rate was 0.03C, the discharge voltage was 1.2V, and CC discharge was performed.
[0105] Then, the initial efficiency (sometimes called "initial efficiency") was calculated using the formula: initial efficiency (%) = (initial discharge capacity / initial charge capacity) x 100.
[0106] Based on the initial data obtained, a counter positive electrode was designed and a battery was evaluated.
[0107] The cycle characteristics were investigated as follows. First, to stabilize the battery, two cycles of charge and discharge were performed at 0.2C in an atmosphere of 25°C, and the discharge capacity of the second cycle was measured. The battery cycle characteristics were calculated from the discharge capacity of the third cycle, and the battery test was stopped after 100 cycles. Charge and discharge were performed at 0.7C and 0.5C. The charge voltage was 4.3V, the discharge cut-off voltage was 2.5V, and the charge cut-off rate was 0.07C.
[0108] XPS analysis of the negative electrode active material was performed using a scanning X-ray photoelectron spectrometer PHI Quantera II manufactured by ULVAC-PHI, Inc. The X-ray beam diameter was set to 100 μm, and a neutralization gun was used.
[0109] The results of each Example and Comparative Example are summarized in Table 1. Figures 1 to 3 show the Si2p spectra obtained by XPS analysis in Examples 1 to 3, respectively. Figures 4 to 8 show the Si2p spectra obtained by XPS analysis in Comparative Examples 1 to 5, respectively. Figure 9 shows the O1s spectrum obtained by XPS analysis in Example 1. Figures 10 and 11 show the O1s spectrum obtained by XPS analysis in Comparative Example 1, respectively. In each of the XPS spectrum graphs, the curve at the top of the graph shows the measurement results of the particle surface layer, and the curve at the bottom of the graph shows the measurement results of the bulk.
[0110] [Example 1] The Li doping process was carried out at a temperature 15°C lower than the boiling point of the solvent (diglyme), and the stabilization process temperature after doping was 580°C.
[0111] As a result, it was possible to form stable high-valence silicon oxide particles and a small amount of zero-valent silicon, which is the main occlusion and desorption of Li during charging and discharging, and has a negative effect on battery characteristics. As a result, the cycle characteristics and initial efficiency were good.
[0112] [Example 2] The same procedure as in Example 1 was followed except that the temperature during Li doping was set to 60°C lower than the boiling point, and the doping process was carried out slowly. Thereafter, the stabilization process temperature was also set low at 570°C.
[0113] As a result, it was possible to reduce zero-valent silicon more than in Example 1. As a result, the cycle characteristics and initial efficiency were also improved compared to Example 1.
[0114] [Example 3] The same procedure as in Example 1 was followed except that the reaction temperature during Li doping was set to a temperature 10°C lower than the boiling point, and the heat treatment temperature was set to 600°C.
[0115] In Example 3 as well, the negative electrode active material of the present invention satisfied the requirements for the Si2p spectrum obtained by XPS analysis, and the cycle characteristics and initial efficiency were good.
[0116] [Example 4] The same procedure as in Example 1 was followed, except that the temperature during Li doping was set to be 10° C. higher than in Example 1. In addition, the heat treatment temperature was the same as in Example 1.
[0117] In Example 4, the negative electrode active material of the present invention also satisfied the Si2p spectrum requirement obtained by XPS analysis, and the cycle characteristics and initial efficiency were good. However, the Si crystallite size was large and crystallization progressed. As a result, the cycle characteristics were lower than those of Examples 1 to 3, but the results were better than those of the comparative examples described below.
[0118] [Examples 5 to 8] The reaction temperature was set to the same as in Example 1, but the heat treatment temperature was changed to vary the crystallinity.
[0119] As a result, the crystallite size corresponding to the Si(111) crystal plane was 5 nm or less, and a tendency was observed in which the cycle characteristics improved as the crystallinity decreased.
[0120] [Examples 9 to 14] In order to find the optimal particle size for the negative electrode active material particles, the particle size of the raw material was changed.
[0121] As a result, particularly good results were obtained when the median diameter was in the range of 5.5 μm or more and 15 μm or less.
[0122] [Comparative Example 1] In comparison with Example 1, a SiO / C material was produced without carrying out Li doping treatment.
[0123] Since no Li doping treatment was performed, the initial efficiency was low and the battery characteristics were poor. In addition, the maximum value of Si2p was on the high energy side, and the shape was different from that of Example 1. It can be seen that the state of O1s was also uniform.
[0124] [Comparative Example 2] The material of Comparative Example 1 was mixed with LiH, and heat-treated at 620° C. to form a Li-doped material.
[0125] It can be seen that the maximum value of Si2p is close to that of Comparative Example 1, and the waveform of O1s is also similar. It can also be seen that disproportionation and crystallization progress by performing thermal doping, and Si(111) becomes crystalline.
[0126] [Comparative Example 3] The raw material of Comparative Example 1 was doped with Li in the same manner as in Example 1. Then, a heat treatment was carried out at a temperature of 620° C. to fix the Li silicate structure in the bulk.
[0127] A low-valence silicon compound was formed, resulting in an electrochemically unstable structure in which disproportionation is likely to progress with repeated charging and discharging.
[0128] [Comparative Example 4] The raw material of Comparative Example 1 was doped with Li in the same manner as in Example 1. The temperature during Li doping was set 10° C. higher than in Example 1. In addition, the reaction rate with Li was increased.
[0129] The stable high-valence state transitioned to an unstable low-valence state. Repeated charging and discharging caused the disproportionation to progress.
[0130] [Comparative Example 5] The same material as in Comparative Example 4 was subjected to stabilization treatment at the same temperature as in Comparative Example 3.
[0131] As a result, disproportionation occurred, in which the peak of the high valence compound shifted to the high energy side and the peak of the low valence compound shifted to the low energy side, and the battery characteristics deteriorated.
[0132] [Table 1]
[0133] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0134] 10...Negative electrode, 11...Negative electrode current collector, 12...Negative electrode active material layer.
Claims
1. A negative electrode active material including negative electrode active material particles, the negative electrode active material particles contain silicon oxide particles coated with a carbon layer, The silicon oxide particles are Li 2 SiO 3 and in a Si2p spectrum obtained by XPS analysis, the strongest peak A is near 102 eV, the second strongest peak B is near 100 eV and corresponds to a low valence Si compound having a valence of 1 to 3, and the intensity of peak C of Si:0 valence obtained near 99 eV is half or less of the intensity of peak A.
2. The negative electrode active material according to claim 1 , wherein the negative electrode active material has three or more phase structures.
3. 3. The negative electrode active material according to claim 1, wherein the negative electrode active material particles are composed of three or more phase structures from the surface layer to the inside, in which an O1s spectrum obtained by XPS analysis has an outermost layer with the strongest peak at approximately 531 eV, a peak below that with approximately 528 eV, and a peak below that with approximately 532.5 eV.
4. 4. The negative electrode active material according to claim 3, wherein a peak obtained near 532.5 eV in an O1s spectrum obtained by the XPS analysis is divided into two peaks near 532 eV and 533 eV.
5. The negative electrode active material particles have a peak due to a Si (111) crystal plane obtained by X-ray diffraction using Cu-Kα radiation before charging and discharging the negative electrode active material particles, and the crystallite size corresponding to the crystal plane is 5.0 nm or less, and Li 2 SiO 3 The ratio G / H of the intensity G of the peak due to the Si (111) crystal plane to the intensity H of the peak due to the (111) crystal plane is expressed by the following formula (1): 0.4≦G / H≦1.0 (1) 5. The negative electrode active material according to claim 1, which satisfies the following:
6. 6. The negative electrode active material according to claim 1, wherein the negative electrode active material particles have a median diameter of 5.5 μm or more and 15 μm or less.
7. 7. The negative electrode active material according to claim 1, wherein the carbon layer has a portion that exists in a compound state with oxygen in an outermost layer.
8. A step of preparing silicon oxide particles; coating the silicon oxide particles with a carbon layer; inserting lithium into the silicon oxide particles coated with the carbon layer by a redox process; The lithium-intercalated silicon oxide particles are heat-treated to form Li 2 SiO 3 and forming silicon oxide particles containing the and producing a negative electrode active material by using the negative electrode active material particles thus produced, The method for producing a negative electrode active material is characterized in that, by adjusting the temperature during the lithium insertion and the temperature during the heat treatment, the silicon oxide particles have, in a Si2p spectrum obtained by XPS analysis, a most intense peak A at about 102 eV, a second most intense peak B at about 100 eV corresponding to a low valence Si compound having a valence of 1 to 3, and a peak C of Si:0 valence obtained at about 99 eV, the intensity of which is half or less of that of the peak A.
Citation Information
Patent Citations
Nonaqueous electrolytic secondary battery and its manufacture
JP1994325765A
Lithium secondary battery
JP2001185127A
Non-aqueous electrolyte secondary battery
JP2002042806A
Negative electrode material for secondary battery, its manufacturing method, and secondary battery using it
JP2005183264A
Battery
JP2006114454A