Polarizing film and its manufacturing method
The acetal-modified polyvinyl alcohol polarizing film with a boron-containing compound addresses high-temperature shrinkage and warping issues in LCDs by maintaining optical performance through controlled processing.
Patent Information
- Application Number
- JP2023220550
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Existing polarizing films used in LCDs exhibit high shrinkage stress at high temperatures, leading to warping issues, and reducing boric acid content to mitigate this problem compromises optical performance.
A polarizing film composed of acetal-modified polyvinyl alcohol with a specific acetal structure and a controlled amount of a boron-containing compound, processed through swelling, dyeing, crosslinking, and stretching treatments, to achieve low shrinkage stress and maintain excellent optical performance.
The film exhibits low shrinkage stress at high temperatures, preventing warping and maintaining high image quality in LCD panels, while minimizing the boron content to avoid adverse effects on optical performance.
Smart Images

Figure 0007561262000001 
Figure 0007561262000002 
Figure 0007561262000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film containing an acetal-modified polyvinyl alcohol having a specific acetal structure and a specific amount of a boron-containing compound, and a method for producing the same. [Background technology]
[0002] Polarizing plates, which have the function of transmitting and blocking light, are the basic components of liquid crystal displays (LCDs) along with liquid crystals, which have a light switching mechanism. Polarizing plates are generally manufactured by laminating protective films such as triacetate cellulose (TAC) films on both sides of a polarizing film manufactured by swelling a polyvinyl alcohol (hereinafter sometimes abbreviated as "PVA") film, followed by uniaxial stretching and dyeing.
[0003] LCDs are used in a wide range of applications, including small devices such as calculators and watches, smartphones, notebook computers, LCD monitors, LCD color projectors, LCD televisions, in-car navigation systems, and measuring instruments used both indoors and outdoors. In recent years, there has been a demand for these devices to be thinner, lighter, and larger, and the glass used in LCDs has become larger and thinner. However, when large or thin glass is used, LCD panels are prone to warping, which is a problem. It is said that the main cause of LCD panel warping is the shrinkage of polarizing films at high temperatures, and polarizing films with low shrinkage stress at high temperatures are in demand.
[0004] Patent Document 1 describes that a polarizing film with small shrinkage force at high temperatures and good color tone can be obtained by reducing the boric acid content of the PVA film and providing a step of drying the PVA film between the boric acid treatment step and the water washing step. However, there is a problem that the optical performance is reduced by reducing the boric acid content in the polarizing film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-148806 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in order to solve the above problems, and an object of the present invention is to provide a polarizing film that has small shrinkage stress at high temperatures and excellent optical performance. [Means for solving the problem]
[0007] The above-mentioned problems can be solved by providing a polarizing film containing an acetal-modified polyvinyl alcohol having an acetal structure represented by the following formula (1) and a boron-containing compound, wherein the acetalization degree of the acetal-modified polyvinyl alcohol is 1 to 8 mol %, and the content of boron element derived from the boron-containing compound is 0.1 to 3 parts by mass per 100 parts by mass of the acetal-modified polyvinyl alcohol:
[0008] [ka] [In formula (1), R is a hydrogen atom or a monovalent aliphatic group having 1 to 6 carbon atoms.]
[0009] At this time, the shrinkage stress of the polarizing film is 4 to 20 N / mm 2 The single transmittance is preferably 43.8 to 44.2%, and the polarization degree is preferably 99.6 to 99.999%. The polymerization degree of the acetal-modified polyvinyl alcohol is preferably 1,000 to 4,000, and the saponification degree is preferably 99 to 99.99 mol %. The thickness of the polarizing film is preferably 10 to 20 μm.
[0010] The above-mentioned problems can also be solved by providing a production method for a polarizing film, which includes a swelling treatment for swelling a film containing the acetal-modified polyvinyl alcohol, a dyeing treatment for dyeing the film with a dichroic dye, a crosslinking treatment for immersing the film in an aqueous solution containing a boron-containing compound, a stretching treatment for stretching the film, a washing treatment for washing the film, and a drying treatment for drying the film, in which, in the crosslinking treatment or the stretching treatment, the film is immersed in an aqueous solution containing 1 to 8 mass% potassium iodide and 1 to 8 mass% boron-containing compound, and then, in the washing treatment, the film is washed by immersing it in an aqueous solution containing 1 to 8 mass% potassium iodide and less than 1 mass% boron-containing compound. Effect of the Invention
[0011] The polarizing film of the present invention has a small shrinkage stress at high temperatures and is also excellent in optical performance. Therefore, an LCD panel using the polarizing film of the present invention has high image quality and is not easily warped even when used at high temperatures. Moreover, such a polarizing film can be produced by the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The polarizing film of the present invention contains an acetal-modified polyvinyl alcohol containing an acetal structure represented by the following formula (1) and a boron-containing compound, the acetalization degree of the acetal-modified polyvinyl alcohol being 1 to 8 mol %, and the content of boron element derived from the boron-containing compound being 0.1 to 3 parts by mass per 100 parts by mass of the acetal-modified polyvinyl alcohol. Thus, the polarizing film of the present invention, which contains an acetal-modified PVA containing a specific acetal structure and a relatively small amount of the boron-containing compound, has low shrinkage stress at high temperatures and is also excellent in optical performance.
[0013] [ka]
[0014] [In formula (1), R is a hydrogen atom or a monovalent aliphatic group having 1 to 6 carbon atoms.]
[0015] The acetal-modified PVA contained in the polarizing film of the present invention can be produced by a method of acetalizing PVA using an aldehyde. The PVA to be acetalized can be produced by saponifying a polyvinyl ester obtained by polymerizing a vinyl ester. Examples of vinyl esters include vinyl acetate, vinyl formate, vinyl propionate, vinyl butyrate, vinyl bivalate, vinyl versatate, vinyl laurate, vinyl stearate, vinyl benzoate, and the like, and one or more of these are selected. Among these, vinyl acetate is preferably used in terms of availability, ease of PVA production, cost, and the like. There is no particular restriction on the polymerization temperature, but when methanol is used as the polymerization solvent, the polymerization temperature is preferably around 60° C., which is close to the boiling point of methanol.
[0016] As long as the effects of the present invention are not impaired, the polyvinyl ester may be a copolymer of a vinyl ester and another monomer copolymerizable therewith, but is preferably one obtained by using only a vinyl ester as a monomer. In this case, two or more kinds of vinyl esters may be used, but it is preferable to use one kind.
[0017] Examples of other monomers copolymerizable with the vinyl ester include α-olefins having 2 to 30 carbon atoms, such as ethylene, propylene, 1-butene, and isobutene; (meth)acrylic acid or a salt thereof; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; (meth)acrylamide; N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, diacetone(meth)acrylamide, (meth)acrylamidopropanesulfonic acid or a salt thereof, (meth)acrylamidopropyldimethylamine or a salt thereof, N Examples of the (meth)acrylamide derivatives include methylol (meth)acrylamide or its derivatives; N-vinylamides such as N-vinylformamide, N-vinylacetamide, and N-vinylpyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, dodecyl vinyl ether, and stearyl vinyl ether; vinyl cyanides such as (meth)acrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salt, ester, or acid anhydride; itaconic acid or its salt, ester, or acid anhydride; vinyl silyl compounds such as vinyltrimethoxysilane; and unsaturated sulfonic acids or their salts. The polyvinyl ester may have one or more structural units derived from the other monomers.
[0018] The proportion of structural units derived from other monomers in the polyvinyl ester is preferably 15 mol % or less, more preferably 10 mol % or less, and even more preferably 5 mol % or less, based on the number of moles of all structural units constituting the polyvinyl ester.
[0019] As the aldehyde used for acetalization, a conventionally known aldehyde having 1 to 7 carbon atoms is used. The aldehyde preferably has 2 or more carbon atoms, more preferably 3 or more carbon atoms, and even more preferably 4 or more carbon atoms. On the other hand, the aldehyde preferably has 6 or less carbon atoms, and more preferably 5 or less carbon atoms. Among them, as the aldehyde, an aldehyde having 4 carbon atoms is particularly preferable, and n-butyl aldehyde is most preferable. In the present invention, an acetal-modified PVA obtained by using two or more kinds of aldehydes in combination can also be used.
[0020] The method of acetalizing the PVA is not particularly limited, and examples thereof include a precipitation method and a solid-liquid reaction method. The precipitation method is a method in which PVA is dissolved in a solvent such as water or acetone, and then a catalyst such as an acid and an aldehyde are added to the resulting solution to carry out an acetalization reaction, the resulting acetal-modified PVA is precipitated, and the acid used as the catalyst is neutralized to obtain a solid powder. The solid-liquid reaction method is different from the precipitation method in that a solvent in which the unmodified PVA is not dissolved is used, and otherwise can be performed in the same manner as the precipitation method. In either method, the resulting polyvinyl acetal powder contains impurities such as unreacted aldehyde and salts generated by neutralization. A highly pure acetal-modified PVA can be obtained by extracting or evaporating and removing these impurities using a solvent in which these impurities are soluble. Among these, the solid-liquid reaction method is preferable from the viewpoint of productivity.
[0021] As the acid catalyst, a conventionally known acid can be used, and examples thereof include inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as paratoluenesulfonic acid. The amount of the acid catalyst to be added is not particularly limited, but is usually adjusted so that the final acid concentration in the reaction solution is 0.5 to 5.0 mass%. These acid catalysts may be added in a predetermined amount at once, but in the case of the precipitation method, it is preferable to add them in appropriate portions in order to precipitate relatively fine acetal-modified PVA particles. On the other hand, in the case of the solid-liquid reaction method, it is preferable to add a predetermined amount all at once at the beginning of the reaction in terms of reaction efficiency.
[0022] The acetal-modified PVA contained in the polarizing film of the present invention contains an acetal structure represented by the following formula (1).
[0023] [ka]
[0024] In formula (1), R is a hydrogen atom or a monovalent aliphatic group having 1 to 6 carbon atoms. The aliphatic group may be linear or branched, but is preferably linear. The aliphatic group preferably has 2 or more carbon atoms, more preferably 3 or more carbon atoms. On the other hand, if the aliphatic group has more than 6 carbon atoms, the solubility of the acetal-modified PVA in water decreases, making it difficult to form an acetal-modified PVA film for use in producing a polarizing film. The aliphatic group preferably has 5 or less carbon atoms, more preferably 4 or less carbon atoms. It is particularly preferable that the aliphatic group has 3 carbon atoms, and it is most preferable that the aliphatic group is an n-propyl group.
[0025] The degree of acetalization of the acetal-modified PVA contained in the polarizing film of the present invention must be 1 to 8 mol%. When the degree of acetalization is 1 mol% or more, the shrinkage stress of the resulting polarizing film is reduced. The degree of acetalization is preferably 2 mol% or more, more preferably 3.5 mol% or more. On the other hand, if the degree of acetalization exceeds 8 mol%, the solubility in water is deteriorated, and it becomes difficult to form the acetal-modified PVA film used in the manufacture of the polarizing film. The degree of acetalization is preferably 5.5 mol% or less, more preferably 4.8 mol% or less, even more preferably 4.5 mol% or less, and particularly preferably 4.2 mol% or less. The degree of acetalization is the ratio (mol%) of the vinyl alcohol unit forming the acetal structure represented by the above formula (1) to the total of the monomer units (vinyl alcohol unit, vinyl acetate unit, etc., including the vinyl alcohol unit forming the acetal structure) in the acetal-modified PVA, and is specifically calculated by the method described in the Examples using the acetal-modified PVA as a sample. The acetal structure represented by the above formula (1) contains two monomer units (vinyl alcohol units).
[0026] The saponification degree of the acetal-modified PVA contained in the polarizing film of the present invention is preferably 99 to 99.99 mol%. If the saponification degree is less than 99 mol%, the PVA may dissolve and adhere to the film during the manufacturing process of the polarizing film, which may result in a decrease in the performance of the polarizing film or a decrease in yield. The saponification degree is more preferably 99.3 mol% or more. The saponification degree is calculated by the method described in the Examples using the PVA before acetalization as a sample.
[0027] The polymerization degree of the acetal-modified PVA contained in the polarizing film of the present invention is preferably 1,000 to 4,000. If the polymerization degree is less than 1,000, the acetal-modified PVA may be dissolved during the manufacturing process of the polarizing film, causing the film to break. The polymerization degree is more preferably 1,500 or more, and even more preferably 2,000 or more. On the other hand, if the polymerization degree exceeds 4,000, not only the productivity of the PVA decreases, but also the stretchability of the PVA film may deteriorate during the manufacturing process of the polarizing film, making it more likely to break. The polymerization degree is more preferably 3,500 or less, and even more preferably 3,000 or less. The polymerization degree is calculated by the method described in the examples using the PVA before acetalization as a sample.
[0028] From the viewpoint of improving the handling property and the stretchability, the acetal modified PVA film used in the production of the polarizing film preferably contains a plasticizer. As the plasticizer, a polyhydric alcohol is preferably used, and specific examples thereof include ethylene glycol, glycerin, propylene glycol, diethylene glycol, diglycerin, triethylene glycol, tetraethylene glycol, and trimethylolpropane. The acetal modified PVA film can contain one or more of these plasticizers. Among these, glycerin is preferred from the viewpoint of further improving the stretchability of the acetal modified PVA film.
[0029] The content of the plasticizer in the acetal-modified PVA film is preferably 3 to 20 parts by mass, more preferably 5 to 17 parts by mass, and even more preferably 7 to 14 parts by mass, based on 100 parts by mass of the acetal-modified PVA. When the content is 3 parts by mass or more, the handleability and stretchability of the acetal-modified PVA film are further improved. On the other hand, when the content is 20 parts by mass or less, deterioration in the handleability of the acetal-modified PVA film due to bleeding out of the plasticizer to the surface can be suppressed.
[0030] The content of the acetal-modified PVA in the acetal-modified PVA film is preferably 50 to 100% by mass, more preferably 80% by mass or more, and even more preferably 85% by mass or more, while the content is more preferably 97% by mass or less, even more preferably 95% by mass or less, and particularly preferably 93% by mass or less.
[0031] The thickness of the acetal-modified PVA film is preferably 10 to 60 μm. If the acetal-modified PVA film is too thin, stretching breaks are likely to occur during the production of the polarizing film. On the other hand, if the acetal-modified PVA film is too thick, stretching spots are likely to occur during the production of the polarizing film. The acetal-modified PVA film is preferably a single-layer film, but may be a laminate in which an acetal-modified PVA layer is laminated with another layer such as a thermoplastic resin film. In the case of a laminate, the thickness of the acetal-modified PVA layer is preferably within the above range.
[0032] The swelling degree of the acetal-modified PVA film is preferably 160 to 240%. If the swelling degree is less than 160%, the tension during stretching in the manufacturing process of the polarizing film may be too large, and the film may not be stretched sufficiently. The swelling degree is more preferably 170% or more, and even more preferably 185% or more. On the other hand, if the swelling degree exceeds 240%, the water absorption of the PVA film is too high, and the film is likely to wrinkle or curl at the end during the manufacturing process of the polarizing film. Such wrinkles and curl at the end cause the film to break during stretching. The swelling degree is more preferably 235% or less, and even more preferably 230% or less. In order to control the swelling degree to a predetermined range, for example, the temperature and time during the heat treatment of the PVA film after film formation may be adjusted to the following ranges. The swelling degree of the acetal-modified PVA film is measured by the method described in the examples.
[0033] The film-forming solution used for producing the acetal-modified PVA film may be a film-forming solution in which acetal-modified PVA, if necessary a plasticizer, a surfactant, and other components are dissolved in a liquid medium, or a film-forming solution in which acetal-modified PVA, if necessary a plasticizer, a surfactant, other components, and a liquid medium are contained and acetal-modified PVA is melted. It is preferable that each component in the film-forming solution is uniformly mixed.
[0034] It is preferable to include a surfactant in the film-forming solution in order to improve the film-forming property, suppress the occurrence of thickness unevenness in the obtained acetal-modified PVA film, and improve the peelability of the PVA film from the metal roll or belt. When an acetal-modified PVA film is produced using a film-forming solution containing a surfactant, the resulting PVA film may contain a surfactant. The type of the surfactant is not particularly limited, but from the viewpoint of facilitating the peeling of the acetal-modified PVA film from the metal roll or belt, anionic surfactants and nonionic surfactants are preferred, and anionic surfactants are more preferred. These surfactants can be used alone or in combination of two or more.
[0035] Examples of anionic surfactants include carboxylic acid surfactants such as potassium laurate; sulfate ester surfactants such as polyoxyethylene lauryl ether sulfate and octyl sulfate; Sulfonic acid types such as decylbenzenesulfonate are preferred.
[0036] Suitable examples of nonionic surfactants include alkyl ether types such as polyoxyethylene oleyl ether; alkyl phenyl ether types such as polyoxyethylene octylphenyl ether; alkyl ester types such as polyoxyethylene laurate; alkyl amine types such as polyoxyethylene lauryl amino ether; alkyl amide types such as polyoxyethylene lauric acid amide; polypropylene glycol ether types such as polyoxyethylene polyoxypropylene ether; alkanolamide types such as lauric acid diethanolamide and oleic acid diethanolamide; and allyl phenyl ether types such as polyoxyalkylene allyl phenyl ether.
[0037] The method for forming the acetal-modified PVA film is not particularly limited, but from the viewpoint of obtaining a film having a uniform thickness and width, the cast film-forming method, the extrusion film-forming method, the wet film-forming method, the gel film-forming method, etc. are preferred, and the cast film-forming method and the extrusion film-forming method are more preferred. Among them, the cast film-forming method is particularly preferred from the viewpoint of obtaining an acetal-modified PVA film having a uniform thickness and width and good physical properties.
[0038] Examples of the liquid medium used in the film-forming solution include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, glycerin, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, trimethylolpropane, ethylenediamine, and diethylenetriamine, and one or more of these can be used. Among these, water is preferred from the viewpoints of its small environmental impact and ease of recovery.
[0039] The volatile content of the film-forming solution may be adjusted appropriately depending on the film-forming method and the molecular weight of the acetal-modified PVA, and is preferably 50 to 95% by mass, more preferably 60 to 95% by mass, and even more preferably 70 to 95% by mass. If the volatile content is less than 50% by mass, the viscosity of the film-forming solution becomes too high, making it difficult to filter or degas during preparation, and the resulting acetal-modified PVA film may contain foreign matter or have defects. On the other hand, if the volatile content exceeds 95% by mass, the viscosity of the film-forming solution becomes too low, making it difficult to adjust the thickness of the acetal-modified PVA film to a target value or to adjust it with high accuracy.
[0040] In order to easily adjust the swelling degree of the PVA film to the above range, it is preferable to heat-treat the acetal-modified PVA film obtained by forming the acetal-modified PVA into a film. The heat treatment temperature is preferably 100 to 170°C. The heat treatment time is preferably 1 to 30 minutes. The acetal-modified PVA film that has been dried after film formation may be humidified to adjust the moisture content (water content) to 5 to 15 mass%, and then heat-treated with only one axis of the film fixed. In this case, it is preferable to fix the flow direction of the acetal-modified PVA film. When the heat treatment is performed with only one axis of the film fixed in this way, the stress caused by the reduction in moisture in the film produces the same effect as when the film is gently stretched.
[0041] The polarizing film of the present invention can be produced by a method including a swelling treatment for swelling a film containing acetal-modified polyvinyl alcohol, a dyeing treatment for dyeing the film with a dichroic dye, a crosslinking treatment for immersing the film in an aqueous solution containing a boron-containing compound, a stretching treatment for stretching the film, a washing treatment for washing the film, and a drying treatment for drying the film. In the crosslinking treatment or the stretching treatment, the film is preferably immersed in an aqueous solution containing 1 to 8% by mass of potassium iodide and 1 to 8% by mass of the boron-containing compound, and then, in the washing treatment, the film is preferably washed by immersing the film in an aqueous solution containing 1 to 8% by mass of potassium iodide and less than 1% by mass of the boron-containing compound. This makes it possible to provide a polarizing film with small shrinkage stress at high temperatures and excellent optical performance. As the boron-containing compound, one or more of boric acid, borax, and other borates can be used, and among them, boric acid is preferred.
[0042] The swelling treatment can be carried out by immersing the acetal-modified PVA film in water. The temperature of the water is preferably 20 to 40°C, more preferably 25 to 35°C. The time for immersion in water is preferably 0.1 to 5 minutes, more preferably 0.5 to 3 minutes. The water is not limited to pure water, and may be an aqueous solution in which various components are dissolved, or a mixture of water and a water-soluble organic solvent. The swelling treatment is preferably carried out before the dyeing treatment.
[0043] The dyeing treatment can be carried out by contacting the acetal-modified PVA film with a dichroic dye. An iodine-based dye is preferably used as the dichroic dye. The dyeing treatment may be carried out before or after the stretching treatment described below, but the former is preferred. As the dyeing method, a general method, specifically, a method of immersing the acetal-modified PVA film in a dye bath, is preferably adopted. As the dye bath, a solution (particularly an aqueous solution) containing iodine and potassium iodide is used. The iodine content in the solution is preferably 0.01 to 0.5% by mass, and the potassium iodide content is preferably 0.01 to 10% by mass. The temperature of the dye bath is preferably 20 to 50° C., more preferably 25 to 40° C. The time for immersing the acetal-modified PVA film in the dye bath is preferably 0.1 to 10 minutes, more preferably 0.2 to 5 minutes.
[0044] The crosslinking treatment can be carried out by immersing the acetal-modified PVA film in an aqueous solution containing a boron-containing compound. This can more effectively prevent the acetal-modified PVA from dissolving in water during wet stretching at high temperatures. From this viewpoint, the crosslinking treatment is preferably carried out before the stretching treatment. It is also preferable to carry out the crosslinking treatment after the dyeing treatment. As the boron-containing compound, one or more of boric acid, borax, and other borates can be used, and boric acid is preferred. The content of the boron-containing compound in the aqueous solution is preferably 1 to 8% by mass. The content of the boron-containing compound is more preferably 2% by mass or more, and even more preferably 2.3% by mass or more. On the other hand, the content of the boron-containing compound is more preferably 5% by mass or less, and even more preferably 4% by mass or less. When the content of the boron-containing compound is within the above range, sufficient stretchability can be maintained. The aqueous solution containing the boron-containing compound may contain an auxiliary such as potassium iodide, and the content is usually 1 to 8% by mass. The temperature of the aqueous solution containing the boron-containing compound is preferably 20 to 50° C., more preferably 25 to 40° C. When the temperature is within the above range, the acetal-modified PVA is crosslinked efficiently.
[0045] Apart from the stretching treatment described later, the acetal-modified PVA film may be uniaxially stretched during or between the steps described above. By performing such stretching (pre-stretching), it is possible to prevent the acetal-modified PVA film from being wrinkled. From the viewpoint of polarization performance, the total stretching ratio (a ratio obtained by multiplying the stretching ratios in each step) in the pre-stretching is preferably 4 times or less based on the original length of the raw PVA film before stretching. The stretching ratio in the swelling treatment is preferably 1.05 to 3 times, the stretching ratio in the dyeing treatment is preferably 3 times or less, and the stretching ratio in the crosslinking treatment is preferably 2 times or less.
[0046] The stretching treatment of the acetal-modified PVA film can be performed by uniaxially stretching the film using a wet stretching method or a dry stretching method. In the case of the wet stretching method, it can be performed in an aqueous solution containing a boron-containing compound, or in the dye bath described above. In the case of the dry stretching method, the stretching may be performed at room temperature, or may be performed while heating, or may be performed in air using the acetal-modified PVA film after absorbing water. Among these, the wet stretching method is preferred, and uniaxial stretching in an aqueous solution containing a boron-containing compound is more preferred. The content of the boron-containing compound in the aqueous solution is preferably 1 to 8 mass%. The content of the boron-containing compound is more preferably 1.5 mass% or more, even more preferably 2.0 mass% or more, particularly preferably 2.3 mass% or more, and most preferably 2.5 mass% or more. On the other hand, the content of the boron-containing compound is more preferably 5 mass% or less, and even more preferably 4 mass% or less. As the boron-containing compound, one or more of boric acid, borax, and other borate salts can be used, and among them, boric acid is preferred. The aqueous solution used for wet stretching preferably contains potassium iodide, and the content thereof is preferably 1 to 8 mass %.
[0047] From the viewpoint of significantly reducing the shrinkage force in the stretching direction of the obtained polarized film and further improving the dimensional stability, the stretching temperature in the stretching treatment is preferably 30 to 90° C., more preferably 40 to 80° C., and particularly preferably 50 to 70° C. From the same viewpoint, it is also preferable to use a wet stretching method.
[0048] From the viewpoint of the polarizing performance of the polarizing film, the stretching ratio in the stretching process is preferably 1.2 times or more, more preferably 1.5 times or more, and even more preferably 2 times or more. The total stretching ratio including the stretching ratio in the first stretching (a ratio obtained by multiplying the stretching ratios in each step) is preferably 5.8 times or more based on the original length of the acetal-modified PVA film of the raw roll before stretching. There is no particular upper limit to the total stretching ratio, but it is preferably 7 times or less to prevent stretching breakage.
[0049] There is no particular restriction on the direction of stretching when uniaxially stretching a long acetal-modified PVA film, and the film can be stretched in the length direction (flow direction during production of the acetal-modified PVA film) or width direction (lateral uniaxial stretching). From the viewpoint of further improving the polarization performance, stretching in the length direction is preferable. Uniaxial stretching in the length direction can be performed by using a stretching device equipped with multiple rolls parallel to each other and changing the peripheral speed between the rolls. On the other hand, lateral uniaxial stretching can be performed using a tenter-type stretching machine.
[0050] By subjecting the acetal-modified PVA film to a washing treatment after the stretching treatment, the boric acid content in the film is reduced, and as a result, the shrinkage stress of the resulting polarizing film at high temperatures is reduced. The washing bath used for the washing treatment can be water or an aqueous solution containing potassium iodide. Among these, an aqueous solution containing potassium iodide is preferred, and the content of potassium iodide is preferably 1 to 8 mass%. From the viewpoint of reducing the content of the boron-containing compound in the acetal-modified PVA film, the content of the boron-containing compound in the washing bath is preferably less than 1 mass%, more preferably less than 0.5 mass%, and even more preferably less than 0.1 mass%. The temperature of the washing bath is preferably 15 to 60°C. The time for immersing the acetal-modified PVA film in the washing bath is preferably 1 to 60 seconds. The time is more preferably 50 seconds or less, more preferably 40 seconds or less, and particularly preferably 30 seconds or less.
[0051] The drying temperature in the drying treatment for drying the acetal-modified PVA film is preferably 30 to 150° C., more preferably 50 to 130° C. When the acetal-modified PVA film is dried and its moisture content becomes 10% by mass or less, the film may be heat-treated at 80 to 140° C. for 1 to 15 minutes while applying tension to the film.
[0052] The content of boron element derived from the boron-containing compound in the polarizing film of the present invention must be 0.1 to 3 parts by mass relative to 100 parts by mass of the acetal-modified PVA. Since the content of the boron-containing compound is relatively small, the polarizing film of the present invention has a small shrinkage stress at high temperatures. Moreover, by using the acetal-modified PVA, the optical performance is maintained even if the content of the boron-containing compound is small. When the boron element content is 0.1 parts by mass or more, the optical performance of the obtained polarizing film is improved. From this viewpoint, the boron element content is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, even more preferably 0.9 parts by mass or more, particularly preferably 1.2 parts by mass or more, and most preferably 1.6 parts by mass or more. On the other hand, when the boron element content is 3 parts by mass or less, the shrinkage stress of the obtained polarizing film at high temperatures is reduced. From this viewpoint, the boron element content is preferably 2.5 parts by mass or less, more preferably 2 parts by mass or less, further preferably 1.6 parts by mass or less, and particularly preferably 1.3 parts by mass or less. The boron element content derived from the boron-containing compound in the polarizing film is measured by the method described in the Examples.
[0053] The polarizing film thus obtained is used as a polarizing plate by laminating an optically transparent and mechanically strong protective film on either or both sides. Examples of protective films that can be used include triacetate cellulose (TAC) film, cellulose acetate-acetate (CAB) film, acrylic film, and polyester film. Examples of adhesives that can be used in this case include PVA adhesives and urethane adhesives, with PVA adhesives being the most suitable.
[0054] The polarizing film of the present invention preferably has a single transmittance of 43.8 to 44.2% or more and a polarization degree of 99.6 to 99.999%. When the single transmittance and polarization degree are within the above ranges, an LCD panel with excellent image quality can be obtained. The single transmittance is more preferably 43.95% or more. Also, the polarization degree is more preferably 99.7% or more. From the viewpoint of reducing warping of the resulting LCD panel, the shrinkage stress of the polarizing film is 4 to 20 N / mm 2 The shrinkage stress is preferably 15 N / mm 2 The following is more preferred:
[0055] The thickness of the polarizing film of the present invention is preferably 10 to 20 μm. This contributes to making the polarizing plate thinner. The thickness of the polarizing film is calculated by the method described in the examples.
[0056] The polarizing plate obtained as described above can be used as an LCD component by coating it with an acrylic adhesive or the like and attaching it to a glass substrate. At the same time, it may be attached to a retardation film, a viewing angle improving film, a brightness improving film, or the like. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0058] [Degree of acetalization] Acetal-modified PVA was dissolved in a mixed solution of N-methylpyrrolidone (NMP) and dimethyl sulfoxide-d6 (DMS-d6) (N-methylpyrrolidone:DMSO-d6=9:1, mass ratio), and chromium acetylacetate was added to the solution. A superconducting nuclear magnetic resonance apparatus (Lambda500, manufactured by JEOL Ltd.) was used as the measuring device, and measurements were performed under conditions of resonance frequencies of 13C and 125MHz and a temperature of 80°C. The degree of acetalization was calculated from the peak intensity derived from the methine carbon (95ppm, 103ppm) bonded to R in the acetal structure represented by the above formula (1) and the peak intensity derived from each methylene carbon (62-75ppm) in the main chain of the vinyl alcohol unit, vinyl ester unit, and vinyl acetal unit.
[0059] [Degree of polymerization and degree of saponification] According to JIS-K6726, the degree of polymerization and the degree of saponification of the polyvinyl alcohol before acetal modification were measured and used as the degree of polymerization and the degree of saponification of the acetal-modified PVA.
[0060] [Film swelling degree] The acetal-modified PVA film was cut into 1.5 g pieces and immersed in 1000 g of distilled water at 30° C. After immersion for 30 minutes, the film was taken out, the water on the surface was absorbed with filter paper, and its mass (We) was measured. The film was then dried at 105° C. for 16 hours using a dryer, and its mass (Wf) was measured. The swelling degree of the PVA film was calculated from the obtained masses We and Wf using the following formula. Swelling degree (%) = (We / Wf) x 100
[0061] [Measurement of polarizing film thickness] The polarizing film was left to stand for 16 hours in an environment of 23°C and 50% RH, and then the thickness of the polarizing film was measured using a contact thickness meter manufactured by Ono Sokki Co., Ltd. [configuration: ST-2030 GAUGE STAND, Digital Gauge Counter DG5100, LINEAR GAUGE SENSOR (measurement range 13 mm)].
[0062] [Measurement of total boron content in polarizing film] A polarizing film (mass Jg) that had been conditioned at 23°C and 50% RH for 16 hours was added to distilled water and then heated to obtain an aqueous solution (mass kg, solid content 0.005% by mass) in which the polarizing film had been dissolved. The boron concentration [L (ppm)] in the aqueous solution was measured using a Shimadzu multi-type ICP emission spectrometer (ICP), and the total boron element content (mass%) in the polarizing film was calculated using the following formula. Total boron content in polarizing film (mass%) =[(L×10 -6 ×K) / J]×100
[0063] [Optical performance of polarizing film] (1) Measurement of transmittance Ts Two rectangular samples, 2 cm in the stretch direction and 1.5 cm in the width direction, were taken from the center of the polarizing film, and a spectrophotometer with an integrating sphere ("V7100" manufactured by JASCO Corporation) was used to perform luminosity correction in the visible light region with a C light source and a 2° field of view in accordance with JIS Z8722 (measurement method for object color). For one sample, the light transmittance was measured when tilted at +45° and when tilted at -45° with respect to the stretch direction, and the average value Ts1 (%) was calculated. For the other sample, the light transmittance was measured when tilted at +45° and when tilted at -45° in the same manner, and the average value Ts2 (%) was calculated. Then, Ts1 and Ts2 were averaged according to the following formula to obtain the transmittance Ts (%) of the polarizing film. Ts = (Ts1 + Ts2) / 2
[0064] (2) Measurement of the degree of polarization V The two samples taken in the measurement of transmittance Ts in (1) were stacked so that their stretching directions were parallel to each other to measure the light transmittance T∥ (%), and the light transmittance T⊥ (%) was measured when the samples were stacked so that their stretching directions were perpendicular to each other in the same manner as in the above ``(1) Measurement of transmittance Ts'', and the polarization degree V (%) was calculated using the following formula. V={(T∥-T⊥) / (T∥+T⊥)} 1 / 2 ×100
[0065] [Shrinkage Stress of Film] The shrinkage force of the polarizing film was measured using an autograph "AG-X" with a thermostat and a video extensometer "TR ViewX120S" manufactured by Shimadzu Corporation. A polarizing film conditioned at 20°C / 20%RH for 18 hours was used for the measurement. After setting the thermostat of the autograph "AG-X" to 20°C, a polarizing film [15 cm in the stretching direction and 1.5 cm in the width direction] was attached to the chuck (chuck interval: 5 cm), and simultaneously with the start of tension, the temperature of the thermostat was raised to 80°C. The polarizing film was stretched at a speed of 1 mm / min, and the stretching was stopped when the tension reached 2 N, and the tension was measured for 4 hours in that state. At this time, since the distance between the chucks changes due to thermal expansion, a scale seal was attached to the chucks, and the measurement was performed so that the distance between the chucks could be corrected by the amount that the scale seal attached to the chucks moved using the video extensometer "TR ViewX120S". Note that since a minimum value of tension occurs in the initial stage of measurement (within 10 minutes from the start of measurement), the minimum value of tension was subtracted from the measured value of tension after 4 hours, and the difference was defined as the shrinkage force (N) of the polarizing film, and the value (N) was divided by the sample cross-sectional area (mm 2 ) to obtain the shrinkage stress (N / mm 2 ).
[0066] [Example 1] [Manufacture of PVA Film] 100 parts by mass of PVA modified with n-butylaldehyde (acetalization degree: 3.8 mol%, R in the above formula (1) is a propyl group (carbon number 3), saponification degree: 99.5 mol%, polymerization degree: 2,400), 10 parts by mass of glycerin as a plasticizer, and 0.16 parts by mass of diethanolamine laurate and 0.08 parts by mass of sodium polyoxyethylene lauryl ether sulfate as surfactants were included, and an aqueous solution with an acetal-modified PVA content of 10% by mass was used as a film-forming stock solution. This was cast onto a metal roll at 60°C and then dried, and the obtained film was heat-treated at 157°C for 10 minutes in a hot air dryer to adjust the swelling degree, thereby manufacturing an acetal-modified PVA film with a thickness of 30 μm. The swelling degree of the obtained acetal-modified PVA film was measured. The results are shown in Table 1.
[0067] <Production of polarizing film> From the center of the width direction of the acetal-modified PVA film thus obtained, a rectangular film of 5 cm in the width direction and 9 cm in the machine direction was taken so that a range of 5 cm in the width direction and 5 cm in the machine direction could be uniaxially stretched. This film was immersed in pure water at 30°C for 60 seconds and uniaxially stretched to 2 times in the machine direction for swelling treatment. Next, it was immersed in an aqueous solution (dyeing treatment bath) at 32°C containing 0.04% by mass of iodine and 0.92% by mass of potassium iodide for 120 seconds and uniaxially stretched to 1.2 times (total 2.4 times) in the machine direction to adsorb iodine (dyeing treatment). Next, it was immersed in an aqueous solution (crosslinking treatment bath) at 32°C containing 2.6% by mass of boric acid and uniaxially stretched to 1.25 times (total 3 times) in the machine direction (crosslinking treatment). The film was then immersed in a 59°C aqueous solution (uniaxial stretching bath) containing 2.8% by mass of boric acid and 5% by mass of potassium iodide, and uniaxially stretched in the machine direction to a total of 6.0 times (stretching treatment). It was then immersed in a 22°C aqueous solution containing 3% by mass of potassium iodide for 10 seconds (washing treatment), and finally dried at 80°C for 4 minutes to produce a polarized film with a thickness of 14 μm. The thickness and optical properties of the obtained polarized film were evaluated, and the shrinkage stress and total boron element content were measured. The results are shown in Table 1.
[0068] [Example 2] A polarizing film was produced in the same manner as in Example 1, except that the immersion time of the film in the washing treatment was changed to 20 seconds, and each measurement and evaluation were carried out. The results are shown in Table 1.
[0069] [Example 3] A polarizing film was prepared in the same manner as in Example 1, except that PVA modified with n-butylaldehyde (acetalization degree 5.0 mol%, R in the above formula (1) is a propyl group (carbon number 3), saponification degree 99.5 mol%, polymerization degree 2,400) was used, and each measurement and evaluation were carried out. The results are shown in Table 1.
[0070] [Comparative Example 1] A polarizing film was produced in the same manner as in Example 1 except that the cleaning treatment was not carried out, and the respective measurements and evaluations were carried out. The results are shown in Table 1.
[0071] [Comparative Example 2] A polarizing film was produced in the same manner as in Example 1, except that unmodified PVA (saponification degree 99.5 mol %, polymerization degree 2,400) was used, and each measurement or evaluation was carried out. The results are shown in Table 1.
[0072] [Comparative Example 3] A polarizing film was prepared in the same manner as in Example 1, except that unmodified PVA (saponification degree 99.5 mol%, polymerization degree 2,400) was used and the immersion time of the film in the washing treatment was changed to 20 seconds, and each measurement and evaluation were carried out. The results are shown in Table 1.
[0073] [Table 1]
[0074] When acetal-modified PVA was used (Examples 1 to 3), the shrinkage stress could be significantly reduced while maintaining the polarization performance by reducing the boron element content derived from the boron-containing compound in the polarizing film. On the other hand, when unmodified PVA was used (Comparative Examples 2 and 3), the polarization performance was reduced and the shrinkage stress was not sufficiently reduced when the boron element content in the polarizing film was reduced. Furthermore, even when acetal-modified PVA was used, the shrinkage stress was extremely high when the boron element content exceeded 3 parts by mass (Comparative Example 1).
Claims
1. The present invention comprises an acetal-modified polyvinyl alcohol having an acetal structure represented by the following formula (1) and a boron-containing compound, The acetalization degree of the acetal-modified polyvinyl alcohol is 1 to 4.5 mol %, The polarizing film has a boron element content of 0.1 to 3 parts by mass based on 100 parts by mass of the acetal-modified polyvinyl alcohol. [In formula (1), R is a hydrogen atom or a monovalent aliphatic group having 1 to 6 carbon atoms.]
2. Shrinkage stress is 4 to 20 N / mm 2 The polarizing film according to claim 1, wherein the single transmittance is 43.8 to 44.2% and the polarization degree is 99.6 to 99.999%.
3. 3. The polarizing film according to claim 1, wherein the acetal-modified polyvinyl alcohol has a degree of polymerization of 1,000 to 4,000 and a degree of saponification of 99 to 99.99 mol %.
4. The polarizing film according to any one of claims 1 to 3, which has a thickness of 10 to 20 µm.
5. 5. The method for producing a polarized film according to claim 1, comprising a swelling treatment for swelling a film containing the acetal-modified polyvinyl alcohol, a dyeing treatment for dyeing the film with a dichroic dye, a crosslinking treatment for immersing the film in an aqueous solution containing a boron-containing compound, a stretching treatment for stretching the film, a washing treatment for washing the film, and a drying treatment for drying the film, wherein in the crosslinking treatment or the stretching treatment, the film is immersed in an aqueous solution containing 1 to 8 mass% potassium iodide and 1 to 8 mass% boron-containing compound, and then in the washing treatment, the film is washed by immersing it in an aqueous solution containing 1 to 8 mass% potassium iodide and less than 1 mass% boron-containing compound.
Citation Information
Patent Citations
Manufacturing method of water-resistant polyvinyl alcohol film
CN103059486A
Membrane
JP1998245442A
Production of film
JP1998273506A
Polarizer, manufacturing method of polarizer, and image display device