Etching composition, method for etching insulating film using same, and method for manufacturing semiconductor device
The etching composition with phosphoric acid, silane, and ammonium salt addresses low selectivity and stability issues, ensuring precise nitride film removal and stable semiconductor manufacturing processes.
Patent Information
- Application Number
- JP2020148458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Priority Date
- 2019-09-04
- Filing Date
- 2020-09-03
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-09-03
AI Technical Summary
Existing etching compositions for semiconductor manufacturing face challenges such as low selectivity between oxide and nitride films, leading to defects and particle generation, and instability during storage, affecting device characteristics and equipment.
An etching composition comprising phosphoric acid, a silane compound, and an ammonium salt with specific chemical structures, which enhances selectivity and stability, minimizing oxide film etching while effectively removing nitride films.
The composition achieves high selectivity in etching nitride films relative to oxide films, preventing particle generation and maintaining stability over time, thus improving semiconductor device quality and process reliability.
Smart Images

Figure 0007561545000016 
Figure 0007561545000017 
Figure 0007561545000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an etching composition, and more particularly to an etching composition having a high selectivity that can selectively remove a nitride film while minimizing the etching rate of an oxide film. [Background technology]
[0002] Silicon oxide film (SiO 2 Oxide films such as silicon oxide (SiNx) and nitride films such as silicon nitride (SiNx) are typical insulating films, and these silicon oxide films and silicon nitride films are used alone or in a laminate of one or more layers in the semiconductor manufacturing process. Such oxide films and nitride films are also used as hard masks for forming conductive patterns such as metal wiring.
[0003] In the wet etching process for removing the nitride film, a mixture of phosphoric acid and deionized water is generally used. The deionized water is added to prevent a decrease in the etching rate and a change in the etching selectivity of the nitride film relative to the oxide film, but even a slight change in the amount of deionized water supplied can cause defects in the nitride film etching removal process. In addition, phosphoric acid is a strong acid and is corrosive, making it difficult to handle.
[0004] To solve this problem, phosphoric acid (H 3 PO 4 ) with hydrofluoric acid (HF) or nitric acid (HNO 3 A technique for removing a nitride film using an etching composition containing phosphoric acid and silicic acid or a silicate has been known, but this technique has the effect of inhibiting the etching selectivity of the nitride film to the oxide film. A technique for removing a nitride film using an etching composition containing phosphoric acid and silicic acid or a silicate has also been known, but silicic acid and silicates generate particles that may affect the substrate, and thus are not suitable for the semiconductor manufacturing process.
[0005] However, when phosphoric acid is used in the wet etching process for removing the nitride film, not only the nitride film but also the SOD oxide film is etched due to a decrease in the etching selectivity of the nitride film to the oxide film, making it difficult to adjust the effective field oxide height (EFH). As a result, it is not possible to secure sufficient wet etching time for removing the nitride film, or an additional process is required, which induces changes in device characteristics and adversely affects device characteristics.
[0006] Therefore, there is a need for an etching composition that has a high selectivity and is capable of selectively etching a nitride film relative to an oxide film in a semiconductor manufacturing process without causing problems such as generation of particles.
[0007] Meanwhile, silane-based additives, which are additives added to conventional etching compositions, have low solubility and do not ensure proper solubility, resulting in problems of particle precipitation in the etching composition and abnormal growth on the substrate. Such particles remain on the silicon substrate, causing defects in devices realized on the substrate, or remain in equipment used in the etching or cleaning process, causing equipment failure.
[0008] Furthermore, when the etching solution is stored for a long period of time, the etching rates of the nitride film and the silicon oxide film may change, resulting in a change in selectivity. Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide an etching composition having a high selectivity that can selectively remove a nitride film while minimizing the etching rate of an oxide film and does not have problems such as generation of particles that adversely affect device characteristics.
[0010] Another object of the present invention is to provide an etching composition having excellent storage stability.
[0011] It is still another object of the present invention to provide a method for etching an insulating film and a method for manufacturing a semiconductor device using the above etching composition. [Means for solving the problem]
[0012] The present invention provides an etching composition, comprising phosphoric acid, a silane compound containing at least one Si atom, and an ammonium salt represented by the following Chemical Formula 1: [ka] Here, L 1 ~L 3 are independently substituted or unsubstituted hydrocarbylene; R 1 ~R 4 is independently hydrogen, substituted or unsubstituted hydrocarbyl, and X n- is an n-valent anion, where n is an integer from 1 to 3.
[0013] The above X is halogen, C 1 -C 10 The salt may be at least one selected from the group consisting of carboxylate, tosylate, sulfate, mesylate, bisulfate, carbonate, bicarbonate, phosphate, hydrogen phosphate, dihydrogen phosphate, and nitrate.
[0014] The above L 1 ~L 3 are independently substituted or unsubstituted C 1 -C 5 It is more preferable that all of them are the same. For example, the above L 1 ~L 3 Ha-CH 2 CH 2 -or-CH 2 CH(CH 3 )- may also be used.
[0015] The hydrocarbyl may be a substituted or unsubstituted C1 -C 20 or substituted or unsubstituted C 6 -C 20 It may be aryl.
[0016] For example, the above R 1 ~R 3 is hydrogen, and R 4 is hydrogen or C 1 -C 20 More specifically, the above R 4 is hydrogen or -CH 3 may be also possible.
[0017] The ammonium salt of the above chemical formula 1 may be selected from the structures of the following formulas (1) to (14). [ka] (OAc stands for acetate, OTs for tosylate, and OMs for mesylate.)
[0018] The silane compound may be represented by the following formula 2: [ka]
[0019] In the above chemical formula 2, R 51 ~R 54 are each independently hydrogen, substituted or unsubstituted hydrocarbyl, substituted or unsubstituted heterohydrocarbyl, R 51 ~R 54 are present individually or in the form of a ring in which two or more are connected to each other via a heteroatom.
[0020] The etching composition of each of the above-mentioned examples may contain 70 to 95% by weight of phosphoric acid, 0.001 to 5% by weight of a silane compound, and 0.001 to 10% by weight of an ammonium salt represented by Chemical Formula 1.
[0021] The present invention provides a method for etching an insulating film using the above-mentioned etching composition, and a method for manufacturing a semiconductor device including the above-mentioned method for etching an insulating film. Effect of the Invention
[0022] The etching composition according to the present invention has a high etching selectivity for a nitride film relative to an oxide film.
[0023] In addition, by using the etching composition of the present invention, damage to the quality of an oxide film during removal of a nitride film and deterioration of electrical characteristics caused by etching of the oxide film can be prevented, and generation of particles can be prevented, thereby improving device characteristics. [Brief description of the drawings]
[0024] [Figure 1] 1A to 1C are cross-sectional views illustrating process steps of an insulating film etching method according to an embodiment of the present invention. [Diagram 2] 1A to 1C are cross-sectional views illustrating process steps of an insulating film etching method according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention provides an etching composition, particularly an etching composition that has a high selectivity that can minimize the etching rate of an oxide film and selectively remove a nitride film, and has excellent storage stability.
[0026] The etching composition of the present invention contains phosphoric acid, which reacts with silicon nitride to etch the nitride film, and the phosphoric acid reacts with silicon nitride to etch the silicon nitride as shown in the following reaction formula (1). 3Si 3 N 4 +27H 2 O+4H 3 PO 4 →4(NH 4 ) 3 PO 4 +9SiO 2 H 2O(1)
[0027] The etching composition of the present invention contains an ammonium salt represented by the following chemical formula 1. [ka]
[0028] In the above chemical formula 1, L 1 ~L 3 are independently substituted or unsubstituted hydrocarbylene. 1 ~L 3 are independently substituted or unsubstituted C 1 -C 5 Alkylene, for example, -CH 2 CH 2 -, -CH 2 CH(CH 3 )- may be used. 1 ~L 3 It goes without saying that they may be different from each other, or they may all be the same.
[0029] In the above chemical formula 1, R 1 ~R 4 are independently hydrogen, substituted or unsubstituted hydrocarbyl. The hydrocarbyl is a substituted or unsubstituted C 1 -C 20 or substituted or unsubstituted C 6 -C 20 The R 1 ~R 4 Needless to say, may be different from each other, and two or more may be the same. For example, the above R 1 ~R 3 is hydrogen, and R 4 is hydrogen or -CH 3 Substituted or unsubstituted C such as 1 -C 20 It may be an alkyl of the formula:
[0030] In the above chemical formula 1, X n-is an anion having a valence of n, and preferably, n is an integer of 1 to 3. For example, X may be a halogen element such as F, Cl, Br, or I, or a C atom such as acetate. 1 -C 10 The carboxylate, tosylate, sulfate, mesylate, bisulfate, carbonate, bicarbonate, phosphate, hydrogen phosphate, dihydrogen phosphate, and nitrate of the formula (I).
[0031] The ammonium salt represented by Chemical Formula 1 provided in the present invention provides structural stability to the silane compound and inhibits phenomena such as decomposition or abnormal growth of the silane compound, thereby inhibiting particle generation in the etching composition and maintaining the role of inhibiting etching of silicon oxide.
[0032] The ammonium salt contained in the etching composition of the present invention may be any one of the ammonium salts represented by the above chemical formula 1, or may be a mixture of two or more of the ammonium salts. The ammonium salt represented by the chemical formula 1 used in the present invention may be, for example, ammonium salts represented by the following formulas (1) to (14). [ka] (OAc stands for acetate, OTs for tosylate, and OMs for mesylate.)
[0033] The ammonium salt of the above formula 1 can prevent particle generation in the etching composition and can be added in a content of 0.001 to 10 wt% based on the total weight of the etching composition. If the content is less than 0.001 wt%, the particle generation suppression effect is small, and if the content is more than 10 wt%, the ammonium salt may accelerate particle generation.
[0034] The content of the ammonium salt of the above Chemical Formula 1 may be, for example, 0.001 to 5 wt%, 0.001 to 3 wt%, 0.001 to 2 wt%, 0.001 to 1 wt%, 0.005 to 5 wt%, 0.005 to 3 wt%, 0.005 to 2 wt%, 0.005 to 1 wt%, 0.01 to 5 wt%, 0.01 to 3 wt%, 0.01 to 2 wt%, 0.01 to 1 wt%, 0.05 to 5 wt%, 0.05 to 3 wt%, 0.05 to 2 wt%, 0.05 to 1 wt%, 0.1 to 5 wt%, 0.1 to 3 wt%, 0.1 to 2 wt%, 0.1 to 1 wt%, 0.5 to 5 wt%, 0.5 to 3 wt%, 0.5 to 2 wt%, or 0.5 to 1 wt%.
[0035] The etching composition of the present invention contains a silane compound. In the present invention, the silane compound may be any silane compound containing one or more Si atoms, and more preferably may be a silane compound represented by the following formula 2. [ka]
[0036] In the above chemical formula 2, R 51 ~R 54 are each independently hydrogen, C 1 -C 20 or C 1 -C 20 The heterohydrocarbyl may be substituted or unsubstituted, such as the heterohydrocarbyl of R 51 ~R 54 may each be present, or two or more may be connected to each other via a heteroatom in a ring. For example, hydrogen, substituted or unsubstituted C 1 -C 20 or substituted or unsubstituted C 1 -C 20 In this case, the hetero element is not particularly limited, and may be, for example, N, S, O, P, or the like.
[0037] The silane compound represented by the above chemical formula 2 may be contained in an amount of 0.005 to 1% by weight based on the total weight of the etching composition.
[0038] Furthermore, the etching composition of the present invention may further contain an ammonium salt other than the ammonium salt represented by Chemical Formula 1.
[0039] As the ammonium salt, a compound having an ammonium ion and commonly used in the field to which the present invention belongs can be suitably used in the present invention. Examples of such ammonium salts include, but are not limited to, ammonia water, ammonium chloride, ammonium acetate, ammonium phosphate, ammonium peroxodisulfate, ammonium sulfate, and ammonium hydrofluoride. Needless to say, any one of these can be used alone, and two or more can be used in combination.
[0040] Furthermore, the etching composition of the present invention may further contain any additives commonly used in the art to further improve the etching performance, such as surfactants, sequestering agents, corrosion inhibitors, etc.
[0041] The etching composition of the present invention is used for selectively etching and removing a nitride film from a semiconductor element including an oxide film and a nitride film, and the nitride film may include a silicon nitride film, for example, a SiN film, a SiON film, etc.
[0042] The oxide film may be a silicon oxide film, for example, a spin on dielectric (SOD) film, a high density plasma (HDP) film, a thermal oxide film, a borophosphate silicate glass (BPSG) film, a phosphorus silicate glass (PSG) film, a boro silicate glass (BSG) film, a polysilazane (PSZ) film, a fluorinated silicate glass (FSG) film, a low pressure tetra ethyl ortho silicate (LPTEOS) film, a plasma enhanced tetra ethyl ortho silicate (PETEOS) film, a high temperature oxide (HTO) film, a medium temperature oxide (MTO) film, an undoped silicate glass (USG) film, a spin on glass (SOG) film, an advanced planarization layer (APL) film, an atomic layer deposition (ALD) film, a plasma enhanced oxide (PE-oxide) film, an O3-TEOS (O3-Tetra The film may be at least one film selected from the group consisting of a dimethyl ethyl ortho silicate film, and combinations thereof.
[0043] The etching process using the etching composition of the present invention may be carried out by a wet etching method, such as a dipping method or a spraying method.
[0044] An example of an etching process using the etching composition of the present invention is shown in schematic form in Figures 1 and 2. Figures 1 and 2 are cross-sectional views showing an element isolation process for a flash memory device as an example.
[0045] 1, a tunnel oxide film 11, a polysilicon film 12, a buffer oxide film 13, and a pad nitride film 14 are sequentially formed on a substrate 10, and then the polysilicon film 12, the buffer oxide film 13, and the pad nitride film 14 are selectively etched to form a trench. Then, an SOD oxide film 15 is formed until the trench is gap-filled, and a CMP process is performed on the SOD oxide film 15 using the pad nitride film 14 as a polishing stop film.
[0046] 2, the pad nitride film 14 is removed by wet etching using a phosphoric acid solution, and then the buffer oxide film 13 is removed through a cleaning process, thereby forming an element isolation film 15A in the field region.
[0047] The process temperature in the etching step may be in the range of 50 to 300°C, preferably in the range of 100 to 200°C, and more preferably in the range of 156 to 163°C, and the appropriate temperature can be changed as necessary taking into account other steps and other factors.
[0048] As described above, the method for manufacturing a semiconductor device including an etching process using the etching composition of the present invention allows selective etching of a nitride film relative to an oxide film when the nitride film and the oxide film are alternately stacked or mixed together, and also prevents generation of particles, which is a problem in the conventional etching process, and ensures stability and reliability of the process.
[0049] Therefore, this method can be effectively applied to several processes in the manufacture of semiconductor devices where selective etching of nitride layers relative to oxide layers is required. EXAMPLES
[0050] The present invention will be described in more detail below with reference to examples. The following examples are merely illustrative of the present invention, and are not intended to limit the present invention.
[0051] [Synthesis Example 1] 10 g of triethanolamine was placed in a 100 mL round-bottom flask, and 30 ml of ethanol was added thereto, followed by stirring.
[0052] N 2 While maintaining the above conditions, the mixture was cooled to 0° C., and then 4.1 g of acetic acid was gradually added. The external temperature of the flask was raised to 90° C., and the mixture was refluxed for 24 hours.
[0053] The mixture was cooled to an external temperature of 40° C., and the ethanol was removed by vacuum distillation. The mixture was then further vacuum dried for 12 hours to obtain ammonium salt additive 1 of the following formula (1). [ka]
[0054] 1 H-NMR (DMSO-d6): 5.00 (broad, 4H), 3.71 (t, 6H), 2.67 (t, 6H), 1.98 (s, 3H)
[0055] [Synthesis Example 2] 10 g of triethanolamine was placed in a 100 ml round-bottom flask, and then 30 ml of acetonitrile was added, followed by stirring.
[0056] N 2 While maintaining the above conditions, the mixture was cooled to 0° C., and then 4.3 g of dimethyl sulfate was gradually added. The external temperature of the flask was raised to 90° C., and the mixture was refluxed for 60 hours.
[0057] The flask was cooled so that the external temperature became 25° C., and the acetonitrile layer was removed. Then, 30 ml of acetonitrile was again charged into the flask and removed by washing.
[0058] After additional vacuum drying for 12 hours, ammonium salt additive 2 of the following formula (2) was obtained. [ka]
[0059] 1 H-NMR (DMSO-d6): 4.78 (broad, 3H), 3.81 (m, 6H), 3.49 (t, 6H), 3.12 (s, 3H)
[0060] [Synthesis Example 3] 5 g of triisopropanolamine was placed in a 100 ml round-bottom flask, and 30 ml of ethanol was then added, followed by stirring.
[0061] After cooling to 0° C., 1.65 ml of 70% nitric acid was gradually added. The external temperature of the flask was raised to 90° C., and the reaction was carried out under reflux for 20 hours.
[0062] The mixture was cooled to an external temperature of 50° C., and ethanol was removed by distillation under reduced pressure. 50 ml of toluene was added to the concentrated residue, and the mixture was distilled under reduced pressure again, and then further dried in vacuum for 24 hours to obtain ammonium salt additive 3 of the following formula (3). [ka]
[0063] 1 H-NMR (DMSO-d6): 4.94 (broad, 4H), 3.78 (m, 3H), 2.61 (m, 6H), 1.31 (m, 9H)
[0064] [Synthesis Example 4] 10 g of triisopropanolamine was placed in a 100 ml round-bottom flask, and 30 ml of ethanol was then added, followed by stirring.
[0065] After cooling to 0° C., 9.7 g of methyl p-toluenesulfonate was gradually added. The external temperature of the flask was raised to 90° C., and the mixture was refluxed for 24 hours.
[0066] The mixture was cooled to an external temperature of 50° C., and ethanol was removed by distillation under reduced pressure. The concentrated residue was washed with 50 ml of acetone, and then distilled under reduced pressure again and further dried in vacuum for 24 hours to obtain ammonium salt additive 4 of the following formula (4). [ka]
[0067] 1 H-NMR (DMSO-d6): 7.48 (d, 2H), 7.12 (d, 2H), 5.05 (broad, 3H), 3.69 (m, 3H), 2.59 (m, 6H), 2.28 (s, 3H), 1.42 (m, 9H)
[0068] Example 1 A substrate was provided on which a silicon oxide film (SiOx) having a thickness of 500 Å (angstroms) and a silicon nitride film (SiN) having a thickness of 5000 Å were formed by vapor deposition on a semiconductor wafer.
[0069] As shown in Table 1, 99.4 wt% of 85% phosphoric acid was mixed with 0.5 wt% of 3-aminopropylsilanetriol and 10.1 wt% of an ammonium salt additive to prepare an etching composition of 100 wt%.
[0070] Examples 2 to 4 Etching compositions were prepared in the same manner as in Example 1, except that ammonium salt additives 2 to 4 were used.
[0071] Comparative Example 1 An etching composition was prepared in the same manner as in Example 1, except that no ammonium salt additive was used.
[0072] Comparative Example 2 As an ammonium salt additive, (NH 4 An etching composition was prepared in the same manner as in Example 1, except that ammonium acetate (OAc) was used.
[0073] <Preparation of Etching Composition and Measurement of Selectivity> Each of the etching compositions obtained in Examples 1 to 4 and Comparative Example 1 was placed in a round-bottom flask and heated for 60 minutes to 158°C. The silicon wafer was then immersed in the composition for 720 seconds and 6,000 seconds to carry out the etching process.
[0074] After selectively etching the surface of the silicon wafer on which the pattern was formed, the thickness of the silicon oxide film and the nitride film before and after etching was measured using an ellipsometry thin film thickness measuring device (NANO VIEW, SEMG-1000), and the etching rate of the silicon oxide film (SiO E / R, Å), the etching rate of the nitride film (SiN E / R, Å), and the selectivity were calculated from the measured values. The results are shown in Table 1.
[0075] The selectivity ratio represents the ratio of the etching rate of the nitride film to the etching rate of the oxide film, and the etching rate is calculated by dividing the difference between the initial film thickness and the film thickness after etching by the etching time (min).
[0076] [Table 1]
[0077] As can be seen from Table 1, when the etching compositions containing ammonium salt additives 1 to 4 were used as additives to the etching composition, the etching selectivity was significantly higher than that of Comparative Example 1. Also, in terms of the etching rate (SiN E / R) of the silicon nitride film, a significantly superior effect was shown compared to the etching composition of Comparative Example 1, and it was confirmed that an etching composition optimized for the etching process of the silicon nitride film can be provided.
[0078] From these results, it can be seen that the use of the ammonium salt provided by the present invention as an additive improves the stability of the active silicon-based structure, and therefore it is possible to provide an etching composition that can improve the etching rate, etching selectivity, and etching stability of a silicon nitride film, thereby improving the efficiency of the etching process.
[0079] Checking the change in etching composition over time The etching compositions of Comparative Example 1 and Example 1 were stored at about 70° C. for a certain period of time, and then the etching test was performed again under the same conditions every 7 days. The results are shown in Table 2.
[0080] [Table 2]
[0081] As can be seen from Table 2 above, after 21 days, the etching composition of Comparative Example 1 showed a significant decrease in etching rate (SiN E / R) and selectivity. In contrast, the etching composition of Example 1 to which ammonium salt additive 1 was added showed results in which the etching rate (SiN E / R) and selectivity were almost unchanged. From the above results, it can be seen that the etching composition according to one embodiment of the present invention not only has excellent etching rate and selectivity, but also has excellent storage stability, and therefore can maintain excellent etching properties even during long-term storage.
[0082] The above results indicate that the structural stability of the ammonium salt additive 1 allows it to maintain its role in inhibiting the etching of silicon oxide films without the occurrence of phenomena such as decomposition or abnormal growth of 3-aminopropylsilanetriol.
Claims
1. An etching composition for a silicon nitride film, comprising phosphoric acid, a silane compound containing one or more Si atoms, and an ammonium salt represented by the following chemical formula 1: 【Chemistry 1】 Here, L 1 ~L 3 are independently substituted or unsubstituted hydrocarbylene; R 1 ~R 4 are independently hydrogen, substituted or unsubstituted hydrocarbyl, and X n- is an n-valent anion, where n is an integer from 1 to 3.
2. The X is a halogen, C 1 -C 10 2. The silicon nitride film etching composition according to claim 1, wherein the compound is at least one selected from the group consisting of carboxylate, tosylate, sulfate, mesylate, bisulfate, carbonate, bicarbonate, phosphate, hydrogen phosphate, dihydrogen phosphate, and nitrate.
3. Said L 1 ~L 3 is independently a substituted or unsubstituted C 1 -C 5 The silicon nitride film etching composition according to claim 1 , wherein the alkylene is selected from the group consisting of the above.
4. Said L 1 ~L 3 The silicon nitride film etching composition of claim 3 , wherein all of
5. Said L 1 ~L 3 Ha-CH 2 CH 2 -or-CH 2 CH (CH 3 5. The silicon nitride film etching composition according to claim 4, wherein
6. The hydrocarbyl may be a substituted or unsubstituted C 1 -C 20 or substituted or unsubstituted C 6 -C 20 The silicon nitride film etching composition according to claim 1 , wherein the aryl is an aryl of the formula:
7. The R 1 ~R 3 is hydrogen, R 4 is hydrogen or C 1 -C 20 2. The silicon nitride film etching composition of claim 1, wherein the alkyl group is an alkyl group of the formula:
8. The R 4 is hydrogen or -CH 3 The silicon nitride film etching composition according to claim 7,
9. 2. The silicon nitride film etching composition according to claim 1, wherein the formula 1 is selected from the structures of (1) to (14) below: 【Chemistry 2】 (OAc denotes acetate, OTs denotes tosylate, and OMs denotes mesylate.)
10. 2. The silicon nitride film etching composition of claim 1, wherein the silane compound is represented by the following formula 2: 【Chemistry 3】 In the above Chemical Formula 2, R 51 ~R 54 are each independently hydrogen, substituted or unsubstituted hydrocarbyl, substituted or unsubstituted heterohydrocarbyl, R 51 ~R 54 are each present, or two or more of them are connected to each other via a heteroatom to form a ring.
11. The silicon nitride film etching composition according to any one of claims 1 to 10, comprising 70 to 95 wt% phosphoric acid, 0.001 to 5 wt% silane compound, and 0.001 to 10 wt% ammonium salt represented by chemical formula 1.
12. A method for etching a silicon nitride film as an insulating film, comprising using the etching composition for a silicon nitride film according to any one of claims 1 to 11.
13. forming a tunnel oxide layer, a polysilicon layer, a buffer oxide layer, and a pad nitride layer on a substrate in sequence; selectively etching the polysilicon layer, the buffer oxide layer, and the pad nitride layer to form a trench; forming a SOD oxide layer to gap-fill the trench; performing a chemical mechanical polishing (CMP) process on the SOD oxide film using the pad nitride film as a polishing stop; removing the pad nitride film by wet etching using the silicon nitride film etching composition of any one of claims 1 to 11; removing the buffer oxide film.
Citation Information
Patent Citations
Composition for etching and etching method
JP2009206462A
Multi-layer polishing pad
JP2016538139A
Composition for chemical mechanical polishing and chemical mechanical polishing method using the same
JP2017114966A
Tungsten treatment slurry containing cationic surfactant
JP2019501517A
Cationically modified silica raw material dispersion
WO2017169602A1