Multi-layer foam sheet

The multilayer foam sheet design addresses mechanical strength and flexibility issues by controlling bending stress in resin layers, preventing creases and maintaining shock absorption, suitable for electronic devices and adhesive tapes.

JP7561616B2Active Publication Date: 2024-10-04SEKISUI CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020516941
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-31
Filing Date
2020-01-30
Publication Date
2024-10-04
Estimated Expiration
2040-01-30

AI Technical Summary

Technical Problem

Foam sheets used in electronic devices face challenges in achieving both mechanical strength and flexibility, leading to issues like damage during rework and impaired shock absorption when thinned, and creases during winding due to differing radii of curvature in multilayer structures.

Method used

A multilayer foam sheet design with specific bending stress ranges for resin layers, defined by formulas (1) and (2), ensuring flexibility and mechanical strength while preventing creases, using a structure of first and third resin layers with bending stress of 1.6 MPa or less at radii of 152.4 mm, 101.6 mm, and 76.2 mm, and a total thickness of 50 to 2000 μm, with resin layers composed of polyolefin, polyurethane, or thermoplastic elastomers.

Benefits of technology

The solution provides a multilayer foam sheet that suppresses appearance defects like folds and wrinkles, enhances flexibility and mechanical strength, and maintains shock absorption properties, suitable for use in electronic devices and adhesive tapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561616000002
    Figure 0007561616000002
  • Figure 0007561616000003
    Figure 0007561616000003
  • Figure 0007561616000001
    Figure 0007561616000001
Patent Text Reader

Abstract

The multilayer foam sheet (10) comprises, in this order, a first resin layer (11) made of a resin film or a foam, a second resin layer (12) made of a foam, and a third resin layer (13) made of a resin film or a foam, and when the radius of curvature (R) is 152.4 mm, the bending stress of the third resin layer (13) defined by the following formula (1) is 1.6 MPa or less. This makes it possible to provide a multilayer foam sheet that can suppress appearance defects such as creases. Bending stress of the third resin layer = D × S / R (1) D: tensile modulus of elasticity in the MD direction of the third resin layer (MPa) S: Distance (mm) from the neutral point of the first resin layer to the surface of the third resin layer opposite to the second resin layer R: radius of curvature
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multi-layer foam sheet comprising at least one foam layer. [Background technology]

[0002] In electronic devices such as mobile phones, cameras, game devices, electronic notebooks, and personal computers, foamed sheets made of foams are widely used as sealing materials or shock absorbing materials. In addition, foamed sheets may be used inside electronic devices, for example, by applying an adhesive to at least one surface thereof to form an adhesive tape. As a foamed sheet used in these applications, a crosslinked polyolefin resin foamed sheet obtained by foaming and crosslinking a foamable polyolefin resin sheet containing a thermal decomposition type foaming agent has been known (for example, see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-28925 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, foam sheets used inside electronic devices are required to be thinner as electronic devices become smaller and thinner. However, as the foam sheet becomes thinner, its mechanical strength such as tensile strength tends to decrease, and for example, when the foam sheet is used as an adhesive tape, it tends to be damaged during rework. On the other hand, when the foam sheet has a lower expansion ratio in order to increase its mechanical strength, its compressive strength increases, which may impair the inherent properties of the foam sheet, such as its shock absorption properties.

[0005] Therefore, a multilayer foam sheet that combines both properties by laminating layers with strength on both sides of a flexible foam (base layer) has been studied. However, when such a multilayer foam sheet is wound around a core such as a paper core during production, for example, a difference in the radius of curvature occurs between the layer on the core side (inner layer) and the layer on the opposite side (outer layer), so that the inner layer may bend toward the base layer, causing defects due to creases.

[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a multilayer foam sheet that has good flexibility and mechanical strength while suppressing appearance defects such as creases. [Means for solving the problem]

[0007] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by setting the bending stress of at least one of the resin layers provided on both sides of a base layer (foam) in a multilayer foam sheet within a specific range, and have completed the present invention described below.

[0008] That is, the present invention provides the following [1] to

[15] . [1] A multilayer foam sheet comprising a first resin layer made of a resin film or a foam, a second resin layer made of a foam, and a third resin layer made of a resin film or a foam, in that order, wherein the bending stress of the third resin layer defined by the following formula (1) is 1.6 MPa or less when the radius of curvature (R) is 152.4 mm. Bending stress of the third resin layer = D × S / R (1) D: Tensile modulus of elasticity in the MD direction of the third resin layer (MPa) S: Distance (mm) from the neutral point of the first resin layer to the surface of the third resin layer opposite the second resin layer R: radius of curvature [2] The multilayer foam sheet according to [1] above, having a 25% compressive strength of 800 kPa or less. [3] The multilayer foam sheet according to the above [1] or [2], wherein the multilayer foam sheet has a total thickness of 50 to 2000 μm. [4] The multilayer foam sheet according to any one of the above [1] to [3], wherein the third resin layer has a tensile strength in the MD direction of 1.5 N or more. [5] The multilayer foam sheet according to any one of the above [1] to [4], wherein the combined thickness of the first resin layer and the third resin layer is 50% or less of the total thickness of the multilayer foam sheet. [6] The multilayer foam sheet according to any one of the above [1] to [5], wherein the bending stress of the third resin layer defined by the above formula (1) is 1.6 MPa or less when the radius of curvature (R) is 101.6 mm. [7] The multilayer foam sheet according to any one of the above [1] to [6], wherein the bending stress of the third resin layer defined in the above (1) is 1.6 MPa or less when the radius of curvature (R) is 76.2 mm. [8] The multilayer foam sheet according to any one of the above [1] to [7], wherein the bending stress of the first resin layer defined by the following formula (2) is 1.6 MPa or less when the radius of curvature (R2) is 152.4 mm: Bending stress of the first resin layer = D2 × S2 / R2 (2) D2: tensile modulus of elasticity in the MD direction of the first resin layer (MPa) S2: Distance (mm) from the neutral point of the third resin layer to the surface of the first resin layer opposite the second resin layer R2: radius of curvature [9] The multilayer foam sheet according to the above item [8], wherein the bending stress of the first resin layer defined by the above formula (2) is 1.6 MPa or less when the radius of curvature (R2) is 101.6 mm.

[10] The multilayer foam sheet according to [8] or [9] above, wherein the bending stress of the first resin layer defined by the above formula (2) is 1.6 MPa or less when the radius of curvature (R2) is 76.2 mm.

[11] The multilayer foam sheet according to any one of the above [1] to

[10] , wherein the first resin layer has a tensile strength of 1.5 N or more.

[12] The multilayer foam sheet according to any one of the above [1] to

[11] , wherein the resin constituting the second resin layer is at least one selected from the group consisting of polyolefin-based resins, polyurethane-based resins, acrylic-based resins, and thermoplastic elastomers.

[13] The multilayer foam sheet according to any one of the above [1] to

[12] , wherein the resin constituting the second resin layer is at least one selected from the group consisting of polyolefin resins and thermoplastic elastomers.

[14] The multilayer foam sheet according to any one of the above [1] to

[13] , wherein the first resin layer and the third resin layer have a foaming rate of 66% or less.

[15] An adhesive tape comprising the multilayer foam sheet according to any one of the above [1] to

[14] and an adhesive material provided on at least one surface of the multilayer foam sheet. Effect of the Invention

[0009] According to the present invention, it is possible to provide a multilayer foam sheet that has good flexibility and mechanical strength while suppressing defects in appearance such as creases. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing one embodiment of a multi-layer foam sheet. [Diagram 2] FIG. 2 is a cross-sectional view showing another embodiment of a multi-layer foam sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the present invention will be described in detail with reference to embodiments. [Multi-layer foam sheet] The multilayer foam sheet of the present invention comprises, in this order, a first resin layer made of a resin film or a foam, a second resin layer (substrate layer) made of a foam, and a third resin layer made of a resin film or a foam. In the following description, for the sake of simplicity, the first to third resin layers may be referred to as the first to third layers, respectively.

[0012] In the present invention, as shown in Fig. 1, the multilayer foam sheet 10 may be composed of three layers, with a first layer 11 and a third layer 13 directly laminated on both sides of a second layer 12. Alternatively, as shown in Fig. 2, the multilayer foam sheet 10 may include first to third layers 11, 12, and 13, and the first layer 11 and the third layer 13 may be laminated on both sides of the second layer 12 via adhesive layers 14 and 15 such as a pressure-sensitive adhesive layer and an adhesive layer. As shown in Figs. 1 and 2, the first and third layers 11 and 13 may be the outermost layers in the multilayer foam sheet 10.

[0013] In the multilayer foam sheet of the present invention, when the radius of curvature (R) is 152.4 mm, the bending stress of the third layer defined by the following formula (1) is 1.6 MPa or less. Bending stress of the third layer = D × S / R (1) D: Tensile modulus of the third layer in the MD direction (MPa) S: Distance from the neutral point of the first layer to the surface of the third layer opposite the second layer (mm) R: radius of curvature The neutral point is a midpoint C in the thickness direction of the first layer 11 as shown in FIGS. 1 and 2, and the distance S is the distance from the midpoint C to the surface 13A of the third layer 13.

[0014] A multilayer foam sheet is generally stored wound around a core such as a paper core, but during this process, a difference in the radius of curvature between the layer on the core side and the layer on the opposite side occurs, resulting in creases in the layer on the core side. In contrast, in the present invention, the bending stress on one side of the multilayer foam sheet is adjusted to a specific range, so that at least one side of the multilayer foam sheet becomes sufficiently flexible, making it possible to suppress the occurrence of creases even when the sheet is wound around a core. In the present invention, "MD" means machine direction, and refers to a direction that coincides with the extrusion direction of a film layer, etc.

[0015] The above formula (1) means that the bending stress when the third layer is bent at a predetermined radius of curvature is 1.6 MPa or less. Therefore, even if the multilayer foam sheet of the present invention is wound around a winding core such as a paper core having a radius of 152.4 mm (6 inches), the multilayer foam sheet is subjected to a bending stress of only 1.6 MPa or less, which makes it possible to suppress the occurrence of creases. Note that a paper core with a radius of 6 inches is a commonly used winding core for winding foam sheets and the like. Furthermore, the multilayer foam sheet of the present invention has a multilayer structure having three resin layers, which makes it easier to achieve good flexibility and mechanical strength. In the present invention, the bending stress of the third layer when the radius of curvature is 152.4 mm (6 inches) is more preferably 1.55 MPa or less, even more preferably 1.0 MPa or less, and even more preferably 0.6 MPa or less, from the viewpoint of sufficiently suppressing creases. Furthermore, the bending stress when the radius of curvature is 152.4 mm (6 inches) is preferably 0.1 MPa or more, and more preferably 0.2 MPa or more, in order to impart a certain level of tensile strength to the third layer.

[0016] In the present invention, the bending stress of the third layer calculated by formula (1) is preferably 1.6 MPa or less even when the radius of curvature (R) is 101.6 mm (4 inches). When winding a multilayer foam sheet, a winding core such as a paper core with an even smaller diameter, about 4 inches in radius, may be used. As described above, even when the radius of curvature is 101.6 mm, if the bending stress is 1.6 MPa or less, no creases will be generated even when the sheet is wound around a small diameter winding core.

[0017] Furthermore, the bending stress of the third layer calculated by formula (1) is more preferably 1.6 MPa or less even when the radius of curvature is 76.2 mm (3 inches). When winding a multilayer foam sheet, a winding core such as a paper core is generally used that has a very small diameter and a radius of about 3 inches, but as described above, even when the radius of curvature is 76.2 mm, if the bending stress is 1.6 MPa or less, no creases will occur even when the sheet is wound around a very small diameter winding core.

[0018] As described above, in a multilayer foam sheet in which a resin film or a foam is provided on both sides of a base layer (second layer), any one of the resin films or foams provided on both sides becomes the first layer, and any other becomes the third layer. Therefore, in the present invention, it is preferable that one of the resin films or foams provided on both sides has a bending stress calculated by formula (1) of 1.6 MPa or less. This is because when the bending stress of one layer (i.e., the third layer) is 1.6 MPa or less, no creases are generated when the sheet is wound up so that the third layer is on the core side (inside).

[0019] However, in the present invention, it is preferable that the bending stress of both the resin films or foams provided on both sides (i.e., both the first layer and the third layer) is 1.6 MPa or less. That is, when the radius of curvature (R2) is 152.4 mm, it is preferable that the bending stress of the first layer defined by the following formula (2) is 1.6 MPa or less. Bending stress of the first layer = D2 × S2 / R2 (2) D2: Tensile modulus of the first layer in the MD direction (MPa) S2: Distance from the neutral point of the third layer to the surface of the first layer opposite the second layer (mm) R2: radius of curvature The neutral point in formula (2) is the midpoint C2 in the thickness direction of the third layer 13, as shown in FIGS.

[0020] Since the bending stress of both the first and third layers of the multilayer foam sheet is 1.6 MPa or less, no creases will occur even if either the first or third layer is wound up on the core side (inner side), and the multilayer foam sheet can be wound up without any restrictions. In the present invention, the bending stress of the first layer when the radius of curvature is 152.4 mm (6 inches) is more preferably 1.55 MPa or less, even more preferably 1.0 MPa or less, and even more preferably 0.6 MPa or less, from the viewpoint of sufficiently suppressing creases. Furthermore, the bending stress of the first layer when the radius of curvature is 152.4 mm (6 inches) is preferably 0.1 MPa or more, and more preferably 0.2 MPa or more, in order to impart a certain level of tensile strength to the first layer.

[0021] From the viewpoint of being able to wind the multilayer foam sheet without restrictions even around a small diameter winding core, it is more preferable that the bending stress of the first layer calculated by formula (2) is 1.6 MPa or less even when the radius of curvature (R2) is 101.6 mm (4 inches). Moreover, from the viewpoint of being able to wind the multilayer foam sheet without restrictions even around a very small diameter winding core, it is even more preferable that the bending stress of the first layer calculated by formula (2) is 1.6 MPa or less even when the radius of curvature is 76.2 mm (3 inches).

[0022] [Tensile modulus (D), (D2)] In the multilayer foam sheet of the present invention, the tensile modulus (D) in the MD of the third layer is preferably 40 to 500 MPa, more preferably 60 to 450 MPa, and even more preferably 150 to 400 MPa. By setting the tensile modulus (D) of the third layer within the above range, it becomes easy to increase the bending stress while improving the compressive strength, etc. From the same viewpoint, the tensile modulus (D2) in the MD direction of the first layer is preferably from 40 to 500 MPa, more preferably from 60 to 450 MPa, and further preferably from 150 to 400 MPa. The tensile modulus of elasticity in the MD direction of the first layer and the third layer may be determined by measuring as described in the Examples.

[0023] [Tensile strength of the first layer and the third layer] In the multilayer foam sheet of the present invention, for example, the tensile strength in the MD direction of the third layer is 1.5 N or more, and preferably 2.5 N or more. When the tensile strength of the third layer is 2.5 N or more, it is possible to improve the mechanical strength while preventing the occurrence of creases and maintaining the flexibility of the multilayer foam sheet. From these viewpoints, the tensile strength in the MD direction of the third layer is more preferably 4 N or more. Moreover, from the viewpoint of keeping the bending stress below a certain level, the tensile strength may be, for example, 200 N or less, preferably 100 N or less.

[0024] In the multilayer foam sheet, for example, the first layer has a tensile strength in the MD direction of 1.5 N or more, but from the viewpoint of improving mechanical strength while maintaining flexibility, it is preferably 2.5 N or more. It is also preferable that the tensile strength in the MD direction of both the first and third layers is 2.5 N or more. When the tensile strength of both the first and third layers is 2.5 N or more, it becomes easier to improve the mechanical strength of the multilayer foam sheet. The tensile strength in the MD direction of the first layer is more preferably 4 N or more, and the tensile strength in the MD direction of both the first and third layers is further preferably 4 N or more. From the viewpoint of keeping the bending stress at a certain level or less, the tensile strength may be, for example, 200 N or less, and preferably 100 N or less. The tensile strength can be measured in accordance with JIS K6767.

[0025] <25% compression strength of multi-layer foam sheet> The multilayer foam sheet of the present invention preferably has a 25% compression strength of 800 kPa or less. When the multilayer foam sheet has a 25% compression strength of 800 kPa or less, the flexibility of the multilayer foam sheet is improved, and the impact absorption property and the like are also improved. Furthermore, since the multilayer foam sheet has excellent conformability, when used as a base material for an adhesive tape, the adhesive strength of the adhesive tape is likely to be improved. From these viewpoints, the 25% compression strength of the multilayer foam sheet is preferably 700 kPa or less, more preferably 300 kPa or less, and even more preferably 100 kPa or less. The 25% compressive strength of the multilayer foam sheet is preferably 20 kPa or more, more preferably 30 kPa or more, and even more preferably 40 kPa or more. By setting the 25% compressive strength to be equal to or more than these lower limits, it is possible to prevent the flexibility from becoming too high, and it is easy to increase the mechanical strength of the multilayer foam sheet. The 25% compressive strength can be measured in accordance with JIS K6767.

[0026] [Thickness and thickness ratio of each layer] The total thickness of the multilayer foam sheet is not particularly limited, but is preferably 50 to 2000 μm, more preferably 80 to 1800 μm, and even more preferably 150 to 1200 μm. By setting the total thickness of the multilayer foam sheet within such a range, the multilayer foam sheet can be made thinner, and a multilayer foam sheet having good flexibility and mechanical strength can be easily obtained.

[0027] In the present invention, the total thickness of the first layer and the third layer is preferably 50% or less, more preferably 30% or less, and even more preferably 25% or less of the total thickness of the multilayer foam sheet. By setting the total thickness within the above range, it is easy to reduce the compressive strength and increase the flexibility while suppressing the occurrence of creases. In addition, from the viewpoint of increasing the mechanical strength, the total thickness is preferably 2% or more, more preferably 4% or more, and even more preferably 7% or more of the total thickness of the multilayer foam sheet. As shown in Fig. 1, the total thickness of the multilayer foam sheet 10 is the total thickness T1 of the three layers in the case of a three-layer structure consisting of a first layer 11, a second layer 12, and a third layer 13. As shown in Fig. 2, when layers (adhesive layers 14, 15) exist between the first layer 11 and the second layer 12, or between the second layer 12 and the third layer 13, the total thickness is the thickness T2 obtained by adding the thicknesses of the adhesive layers 14, 15 to the total thickness of the first to third layers 11-13.

[0028] The thickness of each of the first layer and the third layer is preferably 1 to 500 μm, more preferably 5 to 250 μm, and even more preferably 10 to 90 μm. Within such ranges, the multilayer foam sheet can be made thinner. Also, the tensile strength of the first layer and the third layer and the 25% compressive strength of the multilayer foam sheet can be easily adjusted within the above ranges. The thicknesses of the first layer and the third layer may be the same or different.

[0029] The thickness of the second layer is not particularly limited, but is preferably 40 to 1900 μm, more preferably 70 to 1600 μm, and even more preferably 100 to 1000 μm. By setting the thickness of the second layer within such a range, the multilayer foam sheet can be made thinner and it becomes easier to obtain a multilayer foam sheet with good flexibility. The thickness of the second layer is typically greater than the thicknesses of the first and third layers. By setting the thickness of the second layer to be greater than the thicknesses of the first and third layers, it becomes easier to increase the flexibility of the multilayer foam sheet.

[0030] The first to third layers will be described in more detail below. <Second Layer> The second layer of the present invention is made of a resin foam. The type of resin constituting the second layer is not particularly limited, but examples thereof include polyolefin resins, acrylic resins, polyurethane resins, and thermoplastic elastomers. These may be used alone or in combination of two or more. Among these, polyolefin resins and thermoplastic elastomers are preferred, and polyolefin resins are more preferred. By using polyolefin resins and thermoplastic elastomers, it becomes easier to ensure the flexibility and mechanical strength of the second layer while improving the foamability. The resin used in the second layer may be used alone or in combination of two or more.

[0031] The polyolefin resin is a thermoplastic resin, and specific examples thereof include polyethylene resin, polypropylene resin, ethylene-vinyl acetate copolymer, etc., and among these, polyethylene resin is preferred. Examples of the polyethylene resin include polyethylene resins polymerized with a polymerization catalyst such as a Ziegler-Natta compound, a metallocene catalyst, or a chromium oxide compound, and preferably, polyethylene resins polymerized with a metallocene catalyst are used.

[0032] (Metallocene catalyst) Examples of metallocene catalysts include compounds such as bis(cyclopentadienyl) metal complexes having a structure in which a transition metal is sandwiched between π-electron unsaturated compounds. More specifically, examples of such compounds include compounds in which one or more cyclopentadienyl rings or analogs thereof exist as ligands on a tetravalent transition metal such as titanium, zirconium, nickel, palladium, hafnium, or platinum. Such metallocene catalysts have uniform properties of active sites, and each active site has the same activity. Polymers synthesized using metallocene catalysts have high uniformity in molecular weight, molecular weight distribution, composition, composition distribution, etc., so when a sheet containing a polymer synthesized using a metallocene catalyst is crosslinked, crosslinking proceeds uniformly. A uniformly crosslinked sheet is foamed uniformly, making it easier to stabilize physical properties. In addition, since it can be stretched uniformly, the thickness of the foam can be made uniform.

[0033] Examples of the ligand include a cyclopentadienyl ring and an indenyl ring. These cyclic compounds may be substituted with a hydrocarbon group, a substituted hydrocarbon group, or a hydrocarbon-substituted metalloid group. Examples of the hydrocarbon group include a methyl group, an ethyl group, various propyl groups, various butyl groups, various amyl groups, various hexyl groups, 2-ethylhexyl groups, various heptyl groups, various octyl groups, various nonyl groups, various decyl groups, various cetyl groups, and a phenyl group. The term "various" refers to various isomers including n-, sec-, tert-, and iso-. Furthermore, a cyclic compound may be polymerized as an oligomer and used as the ligand. Furthermore, in addition to the π-electron unsaturated compounds, monovalent anion ligands such as chlorine and bromine or divalent anion chelate ligands, hydrocarbons, alkoxides, arylamides, aryloxides, amides, arylamides, phosphides, arylphosphides, and the like may be used.

[0034] Examples of metallocene catalysts containing a tetravalent transition metal or ligand include cyclopentadienyltitanium tris(dimethylamide), methylcyclopentadienyltitanium tris(dimethylamide), bis(cyclopentadienyl)titanium dichloride, and dimethylsilyltetramethylcyclopentadienyl-t-butylamide zirconium dichloride. Metallocene catalysts, when combined with a specific cocatalyst (promoter), act as a catalyst during the polymerization of various olefins. Specific examples of the cocatalyst include methylaluminoxane (MAO) and boron-based compounds. The ratio of the cocatalyst to the metallocene catalyst is preferably 100,000 to 1,000,000 times by mole, and more preferably 50 to 5,000 times by mole.

[0035] Moreover, the polyethylene resin is preferably a linear low-density polyethylene. The linear low-density polyethylene is more preferably a linear low-density polyethylene obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more based on the total amount of monomers) with a small amount of α-olefin as required. Specific examples of α-olefin include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene. Among them, α-olefins having 4 to 10 carbon atoms are preferred. The density of the polyethylene resin, for example the linear low-density polyethylene described above, is 0.870 to 0.925 g / cm3 from the viewpoint of flexibility. 3 is preferable, and 0.890 to 0.925 g / cm 3 More preferably, 0.910 to 0.925 g / cm 3As the polyethylene resin, a plurality of polyethylene resins may be used, and a polyethylene resin having a density outside the above-mentioned range may be added.

[0036] The ethylene-vinyl acetate copolymer used as the polyolefin resin is, for example, an ethylene-vinyl acetate copolymer containing 50% by mass or more of ethylene. Examples of polypropylene resins include homopolypropylene and propylene-α-olefin copolymers containing 50% by mass or more of propylene. These may be used alone or in combination of two or more. Specific examples of α-olefins constituting the propylene-α-olefin copolymers include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene, and among these, α-olefins having 6 to 12 carbon atoms are preferred.

[0037] Examples of the thermoplastic elastomer include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, etc. The thermoplastic elastomer may be used alone or in combination of two or more of these components. Of these, olefin-based thermoplastic elastomers and styrene-based thermoplastic elastomers are preferred, and styrene-based thermoplastic elastomers are more preferred.

[0038] Examples of olefin-based thermoplastic elastomers include blend-type, dynamically crosslinked-type, and polymerization-type elastomers. More specifically, examples of such elastomers include thermoplastic elastomers that use thermoplastic crystalline polyolefins such as polypropylene and polyethylene for the hard segments and fully vulcanized or partially vulcanized rubber for the soft segments. The thermoplastic crystalline polyolefin may be, for example, a homopolymer of an α-olefin having 1 to 4 carbon atoms or a copolymer of two or more α-olefins, with polyethylene or polypropylene being preferred.The soft segment component may be, for example, butyl rubber, halobutyl rubber, EPDM, EPM, acrylonitrile / butadiene rubber, NBR, natural rubber, etc., with EPDM being preferred.

[0039] Further, the olefin-based thermoplastic elastomer may be a block copolymer type. The block copolymer type may have a crystalline block and a soft segment block, and more specifically, may be a crystalline olefin block-ethylene-butylene copolymer-crystalline olefin block copolymer (CEBC). In CEBC, the crystalline olefin block is preferably a crystalline ethylene block, and a commercially available example of such a CEBC is "DYNARON 6200P" manufactured by JSR Corporation.

[0040] Examples of the styrene-based thermoplastic elastomer include block copolymers having a polymer or copolymer block of styrene and a polymer or copolymer block of a conjugated diene compound, such as isoprene and butadiene. The styrene-based thermoplastic elastomer used in the present invention may or may not be hydrogenated. When hydrogenated, the hydrogenation can be carried out by a known method.

[0041] Styrene-based thermoplastic elastomers are usually block copolymers, and examples thereof include styrene-isoprene block copolymers, styrene-isoprene-styrene block copolymers, styrene-butadiene block copolymers, styrene-butadiene-styrene block copolymers, styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-ethylene / propylene-styrene block copolymers (SEPS), styrene-ethylene / butylene block copolymers (SEB), styrene-ethylene / propylene block copolymers (SEP), and styrene-ethylene / butylene-crystalline olefin block copolymers (SEBC). As the above-mentioned styrene-based thermoplastic elastomer, a block copolymer is preferable, and among them, SEBS and SEBC are more preferable.

[0042] Commercially available styrene-based thermoplastic elastomers include those manufactured by JSR Corporation under the trade name "DYNARON 8600P" (styrene content: 15% by mass), the trade name "DYNARON 4600P" (styrene content: 20% by mass), and the trade name "DYNARON 1321P" (styrene content: 10% by mass).

[0043] [Additives] The second layer used in the present invention is preferably obtained by foaming a foamable composition containing the above-mentioned resin and a foaming agent, preferably a thermally decomposable foaming agent. As the thermal decomposition type blowing agent, organic blowing agents and inorganic blowing agents can be used. Examples of the organic blowing agent include azo compounds such as azodicarbonamide, azodicarboxylate metal salts (e.g., barium azodicarboxylate), azobisisobutyronitrile, etc., nitroso compounds such as N,N'-dinitrosopentamethylenetetramine, etc., hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), toluenesulfonylhydrazide, etc., and semicarbazide compounds such as toluenesulfonylsemicarbazide, etc. Examples of inorganic foaming agents include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate. Among these, from the viewpoint of obtaining fine bubbles, and from the viewpoints of economy and safety, azo compounds are preferred, and azodicarbonamide is more preferred. The thermally decomposable foaming agents may be used alone or in combination of two or more kinds.

[0044] The amount of the foaming agent in the foamable resin composition is preferably 1 to 20 parts by mass, more preferably 1.5 to 15 parts by mass, and even more preferably 2 to 10 parts by mass, based on 100 parts by mass of the resin. By making the amount of the foaming agent 1 part by mass or more, it is possible to impart appropriate flexibility and impact absorption properties to the multilayer foam sheet. Furthermore, by making the amount of the foaming agent 20 parts by mass or less, it is possible to prevent the second layer from foaming more than necessary, and to improve the mechanical strength, etc., of the second layer.

[0045] The foamable resin composition may contain a decomposition temperature regulator. The decomposition temperature regulator is used to lower the decomposition temperature of the thermal decomposition type foaming agent or to increase or adjust the decomposition rate, and specific examples of the regulator include zinc oxide, zinc stearate, and urea. The decomposition temperature regulator is used in an amount of, for example, 0.01 to 5 parts by mass per 100 parts by mass of the resin in order to adjust the surface state of the second layer.

[0046] The foamable resin composition may contain an antioxidant. Examples of the antioxidant include phenol-based antioxidants such as 2,6-di-t-butyl-p-cresol, sulfur-based antioxidants, phosphorus-based antioxidants, and amine-based antioxidants. The antioxidant is blended in an amount of, for example, 0.01 to 5 parts by mass per 100 parts by mass of the resin.

[0047] In the second layer, the resin is the main component, and the content of the resin is, for example, 70 mass % or more, preferably 80 mass % or more, and more preferably 90 mass % or more, based on the total amount of the second layer. The foamable resin composition may contain, in addition to the above, additives generally used in foams, such as a heat stabilizer, a colorant, a flame retardant, an antistatic agent, and a filler, if necessary.

[0048] [Expansion ratio of the second layer] The expansion ratio of the second layer is not particularly limited, but is preferably 1.1 to 20 cm 3 The expansion ratio is preferably 1.1 cm / g. 3 By increasing the expansion ratio to 20 cm / g or more, the flexibility of the multi-layer foam sheet is increased. 3 By setting the expansion ratio of the second layer to 2.5 to 18 cm / g or less, the strength of the multilayer foam sheet is improved. 3 / g, and more preferably 7.5 to 16 cm 3 The expansion ratio of the second layer is represented by the reciprocal of the apparent density of the second layer.

[0049] [Degree of crosslinking of the second layer] The degree of crosslinking of the second layer is not particularly limited, but is, for example, 5 to 65%, preferably 10 to 55%, and more preferably 20 to 50%. By making the degree of crosslinking of the second layer equal to or greater than these lower limits, it is possible to prevent the flexibility from increasing more than necessary and ensure a certain level of mechanical strength. In addition, by making the degree of crosslinking equal to or less than the upper limits, the flexibility and impact absorption properties are improved.

[0050] <First and third layers> The first layer and the third layer are each a resin film or a foam as described above, and are preferably a resin film. The resin film is a non-foamed resin layer. Hereinafter, the case where both the first layer and the third layer are resin films will be described in more detail.

[0051] In each of the first layer and the third layer, the type of resin constituting the resin film is not particularly limited as long as it satisfies the relationship of the above formulas (1) and (2), and, like the resin in the second layer, examples thereof include polyolefin-based resins, acrylic-based resins, polyurethane-based resins, thermoplastic elastomers, etc. In addition to these, vinyl chloride-based resins, styrene-based resins, polyester-based resins, polyamide-based resins, ionomer-based resins, etc. may also be used. In each of the first layer and the third layer, the resin may be used alone or in combination of two or more kinds. The resin used in the first layer and the resin used in the third layer may be the same or different, but from the viewpoint of productivity and the viewpoint of easily making the physical properties of both layers the same or similar, it is preferable that they are the same.

[0052] The resins constituting each of the first layer and the third layer are preferably thermoplastic resins, and the use of a thermoplastic resin makes it possible to easily adhere the first layer and the third layer to the second layer. Among the above resins, polyolefin resins are preferred for the first layer and the third layer. By using polyolefin resins, it is easy to increase the mechanical strength of the multi-layer foam sheet while reducing the bending stress. In addition, when polyolefin resins or thermoplastic elastomers are used for the second layer, the adhesion of the first and third layers to the second layer can be particularly good.

[0053] Examples of polyolefin resins include polyethylene resins, polypropylene resins, etc. Also usable are ethylene-vinyl acetate copolymers, ethylene-ethyl acrylate copolymers, etc. Examples of the polyethylene resin include polyethylene resins polymerized with a polymerization catalyst such as a Ziegler-Natta compound, a metallocene catalyst, or a chromium oxide compound, and preferably, polyethylene resins polymerized with a metallocene catalyst are used. As the polyethylene resin, for example, low-density polyethylene (density: 0.930 g / cm 3less than 0.930g / cm 3 More than 0.942g / cm 3 less than 0.942g / cm 3 The above are some examples. Here, the low density polyethylene may be, for example, linear low density polyethylene. Details of the linear low density polyethylene are as described in the description of the second layer, and therefore will not be described in detail. In addition, details of the polypropylene resin are as described in the description of the second layer, and therefore will not be described in detail.

[0054] The ethylene-vinyl acetate copolymer used in the first and third layers may be, for example, an ethylene-vinyl acetate copolymer containing 50% by mass or more of structural units derived from ethylene. Furthermore, the ethylene-ethyl acrylate copolymer may be an ethylene-ethyl acrylate copolymer containing 50% by mass or more of structural units derived from ethylene. Among the above, from the viewpoints of adhesion to the second layer, bending stress, and tensile strength, ethylene resin, particularly linear low-density polyethylene, is preferred, and from the same viewpoints, ethylene-vinyl acetate copolymer is also preferred.

[0055] In the first and third layers, the resin is the main component, and the content of the resin is, for example, 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more, based on the total amount of each layer. In addition to the resin, the first and third layers may contain additives such as antioxidants, heat stabilizers, colorants, flame retardants, antistatic agents, and fillers. The first and third layers may be crosslinked. As described later in the manufacturing method 1, the first and third layers may be crosslinked in conjunction with the crosslinking of the second layer, and therefore are preferably crosslinked by ionizing radiation.

[0056] Each of the first layer and the third layer may be a foam as described above. When the first layer and the third layer are foamed, for example, the resin usable in the first and third layers may be blended with a foaming agent as described for the second layer to foam the first and third layers. When the first and third layers are foamed, the foaming ratio is preferably low from the viewpoint of securing a certain mechanical strength, and the foam ratio, which indicates the proportion of bubbles contained in each layer, is low. Specifically, the first layer and the third layer each preferably have a foam content of 66% or less, more preferably 33% or less, and further preferably 0%. When the first and second layers are non-foamed bodies (i.e., resin films), the foam content is 0%. The air bubble ratio can be determined, for example, by observing the cross sections of the first layer and the third layer and calculating the ratio of the area occupied by air bubbles to the area of ​​each layer. Specifically, a cross section is cut out along the thickness direction and photographed with an optical microscope. After that, the air bubbles and the resin part are divided by binarization, and the air bubble area / total area is calculated.

[0057] (adhesive layer) In the present invention, as described above, the first layer and the second layer, or the second layer and the third layer may be directly bonded to each other, or may be bonded to each other via another layer (i.e., an adhesive layer). As the adhesive layer, a known adhesive, pressure-sensitive adhesive, or the like may be used. Alternatively, the adhesive layer may be a double-sided adhesive tape having pressure-sensitive adhesive layers on both sides of a substrate. The adhesive layer may have a thickness that does not significantly affect the physical properties of the multilayer foam sheet, such as mechanical strength and flexibility. Therefore, the thickness of the adhesive layer bonding the first layer and the second layer is preferably thinner than the first layer, and more preferably 1 / 2 or less than the thickness of the first layer. Similarly, the thickness of the adhesive layer bonding the second layer and the third layer is preferably thinner than the third layer, and more preferably 1 / 2 or less than the thickness of the third layer.

[0058] <Method of manufacturing multi-layer foam sheet> (Manufacturing method 1) The multilayer foam sheet of the present invention is not particularly limited, but can be produced, for example, by a method in which a plurality of layers made of a resin composition are laminated to obtain a multilayer laminate sheet, and then the multilayer laminate sheet is foamed (hereinafter also referred to as "production method 1"). In this specification, the term "resin composition" conceptually includes a case in which the composition is made of only one type of resin.

[0059] More specifically, production method 1 includes the following steps I and II. (I) A step of obtaining a multilayer laminate sheet including a layer made of a foamable resin composition, a first layer formed on one side of the layer, and a third layer formed on the other side of the layer. (II) A step of foaming a layer of the foamable resin composition of the multilayer laminate sheet to obtain a multilayer foam sheet.

[0060] Each step will be described below. (Process (I)) The method for obtaining the multilayer laminate sheet in step (I) is not particularly limited, but is preferably performed by co-extrusion molding. Specifically, the resins for forming the first layer and the third layer, and other additives blended as necessary, are fed to the first and third extruders, respectively, and melt-kneaded to obtain a resin composition for forming the first and third layers. In addition, the resin for forming the second layer, a foaming agent such as a thermally decomposable foaming agent, and additives blended as necessary are fed to the second extruder, and melt-kneaded to obtain a foamable resin composition for forming the second layer. Next, the resin compositions supplied from the first to third extruders are joined together so that the composition supplied from the second extruder forms the middle layer, and extruded into a sheet using a T-die or the like to obtain a multilayer laminate sheet having a three-layer structure. In the co-extrusion molding, either the feed block method or the multi-manifold method may be used, but the feed block method is preferred.

[0061] In step (I), it is preferable to further crosslink the multilayer laminate sheet obtained above. As a crosslinking method, an organic peroxide is mixed in advance, and the multilayer laminate sheet obtained in step (I) is heated to crosslink, but it is preferable to crosslink the multilayer laminate sheet by irradiating it with ionizing radiation. Examples of ionizing radiation include electron beams and β rays, and electron beams are preferable. The dose of ionizing radiation is preferably 1 to 10 Mrad, and more preferably 1.5 to 5 Mrad.

[0062] (Step (II)) In step (II), the multilayer laminate sheet obtained in step (I) is foamed to foam the layer made of the foamable resin composition. The layer made of the foamable resin composition may be foamed by treating the foaming agent so that the foaming agent foams. When the foaming agent is a thermally decomposable foaming agent, the multilayer laminate sheet is heated to foam the layer. The heating temperature may be equal to or higher than the temperature at which the thermally decomposable foaming agent decomposes, and is, for example, about 150 to 320°C. The method for heating the multilayer laminate sheet is not particularly limited, and examples thereof include a method for heating the multilayer laminate sheet with hot air, a method for heating with infrared rays, a method for heating in a salt bath, a method for heating in an oil bath, and the like, and these may be used in combination. The multi-layer laminate sheet may be appropriately stretched during or after foaming. In the above description, an example was described in which the first and third layers are resin films (non-foamed bodies). However, in the case in which the first and third layers are foamed bodies, a foaming agent such as a thermally decomposable foaming agent may be blended as an additive into the resin composition for forming the first and third layers, and foamed in step (II).

[0063] (Second manufacturing method) The multilayer foam sheet of the present invention can also be produced by another method, specifically, a method in which a foam constituting the second layer is produced in advance, and a resin film or a foam (first and third layers) is laminated and bonded to both sides of the foam (second layer) (also referred to as a "second production method") can be mentioned.

[0064] In the second production method, the foam may be obtained by melt-kneading the resin for forming the second layer, the thermally decomposable foaming agent, and additives blended as necessary to obtain a foamable resin composition for forming the second layer, and molding the foamable resin composition into a sheet (foamable resin composition sheet). The method for melt-kneading the foamable resin composition and molding it into a sheet is not particularly limited, but it is preferably performed using an extruder.

[0065] The obtained foamable resin composition sheet is preferably crosslinked before foaming, which will be described later. As a crosslinking method, an organic peroxide is mixed in advance, and the foamable resin composition sheet is heated to crosslink, but it is preferable to crosslink the foamable resin composition sheet by irradiating it with ionizing radiation. The type and dose of ionizing radiation are as described in the first production method.

[0066] Next, the foamable resin composition sheet may be foamed. The layer made of the foamable resin composition may be treated so that the foaming agent foams, but when the foaming agent is a thermally decomposable foaming agent, the multilayer laminate sheet is heated to foam it. The heating temperature and heating method are as described in the first manufacturing method. The foamable resin composition sheet may be appropriately stretched while or after foaming.

[0067] Thereafter, a resin film or foam for constituting the first layer and the third layer, which have been separately prepared, is superimposed on a foam for constituting the second layer and bonded to obtain a multilayer foam sheet. Specifically, the layers may be heated and pressed by a press or the like to be thermocompressed. Alternatively, the layers may be bonded together by applying a pressure-sensitive adhesive, adhesive, or the like to the adhesive surfaces between the second layer and the first layer and between the second layer and the third layer, or by applying a double-sided adhesive tape to the adhesive surfaces.

[0068] <Applications of multi-layer foam sheets> The multilayer foam sheet of the present invention is preferably used, for example, inside an electronic device, for example, by disposing it between two members and using it as a shock absorbing material, a sealing material, etc. The multilayer foam sheet can also be made into a frame shape and used inside a portable electronic device. Examples of portable electronic devices include mobile phones, cameras, game devices, electronic notebooks, personal computers, etc. The multilayer foam sheet of the present invention may be made into an adhesive tape as described below and used inside electronic devices.

[0069] The multilayer foam sheet of the present invention may be wound around a core such as a paper core into a roll shape. The multilayer foam sheet is easy to store and transport when it is rolled. As described above, a core having a radius of about 3 to 6 inches (76.2 to 152.4 mm) may be used as the core. When the multilayer foam sheet is wound around the core, the layer having a bending stress of a predetermined value or less may be wound on the core side (inner side) as described above. Therefore, the multilayer foam sheet may be wound so that the third layer is on the core side, but when the bending stress of both the first and third layers is a predetermined value or less as described above, the first layer may be wound so that the first layer is on the core side (inner side).

[0070] [Adhesive tape] The multilayer foam sheet of the present invention may be used in an adhesive tape using the multilayer foam sheet as a substrate. The adhesive tape comprises, for example, a multilayer foam sheet and an adhesive material provided on at least one surface of the multilayer foam sheet. The adhesive tape can be adhered to other members via the adhesive material. The adhesive tape may be a multilayer foam sheet having an adhesive material provided on both surfaces thereof or on one surface thereof.

[0071] The adhesive material may be any material that at least comprises an adhesive layer, and may be a single adhesive layer laminated on the surface of the multilayer foam sheet (i.e., surfaces 11A, 13A of the first or third layer 11, 13, see Figures 1 and 2), or a double-sided adhesive sheet affixed to the surface of the multilayer foam sheet, but is preferably a single adhesive layer. The double-sided adhesive sheet comprises a substrate and adhesive layers provided on both sides of the substrate. The double-sided adhesive sheet is used to adhere one adhesive layer to the multilayer foam sheet and to adhere the other adhesive layer to another member. The adhesive constituting the adhesive layer is not particularly limited, and for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, etc. may be used. In addition, a release sheet such as release paper may be further attached onto the adhesive material. The thickness of the adhesive material is preferably from 5 to 200 μm, more preferably from 7 to 150 μm, and further preferably from 10 to 100 μm.

[0072] The pressure-sensitive adhesive tape of the present invention may be wound around a core to form a roll. The radius of the core is as described above. Even when the multilayer foam sheet is wound in the form of a pressure-sensitive adhesive tape, the thickness of the pressure-sensitive adhesive is thin as described above, so that the multilayer foam sheet can be bent with a radius of curvature generally corresponding to the size of the core. However, the bending stress of the third layer or the first and third layers is within the above-mentioned predetermined range, so that the occurrence of creases can be prevented. EXAMPLES

[0073] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0074] [Measurement method] The methods for measuring and evaluating each physical property are as follows.

[0075] <Tensile modulus of the first layer and the third layer> The tensile modulus of elasticity of the first layer and the third layer was measured using a tensile tester (Tensilon RTF series, manufactured by Yamato Scientific Co., Ltd.) under the measurement conditions in accordance with JIS K6767.

[0076] <Tensile strength of the first layer and the third layer> The first layer and the third layer were cut into a dumbbell shape No. 1 as specified in JIS K6251 4.1. Using this as a sample, the tensile strength was measured at a measurement temperature of 23°C using a tensile tester (product name: Tensilon RTF235, manufactured by A&D Co., Ltd.) in accordance with JIS K6767. <25% compressive strength> The 25% compressive strength of the multilayer foam sheet was measured in accordance with JIS K6767.

[0077] <Apparent density and expansion ratio> The apparent density of the foam was measured in accordance with JIS K7222, and the reciprocal of the apparent density was taken as the expansion ratio. <Crosslinking degree> A test piece of about 100 mg is taken from the foam, and the weight A (mg) of the test piece is precisely weighed. Next, this test piece is immersed in 30 cm of xylene at 120 °C. 3 After immersing the sample in the solution for 24 hours, the insoluble matter on the screen was collected by filtration through a 200-mesh wire screen, vacuum-dried, and the weight B (mg) of the insoluble matter was precisely weighed. The degree of crosslinking (mass%) was calculated from the obtained value using the following formula. Crosslinking degree (mass%) = 100×(B / A)

[0078] <Evaluation (creases)> The short edge of an A4-sized sample is fixed to a specified paper core. After fixing, the sample is wrapped around the paper core with a force of 5N. After this, it is left to stand for 30 seconds, after which the paper core is removed and the condition of the sample inside the wrap is observed to determine whether or not creases have occurred. The judgment standard is that a crease depth of 0.05mm or more is considered to be creased. If there are no creases, it is rated as "A", and if there are creases, it is rated as "B".

[0079] [Example 1] The polyolefin resin for the second layer was a linear low-density polyethylene resin obtained by a metallocene catalyst (manufactured by Japan Polyethylene Co., Ltd., product name "Kernel KF283", density: 0.921 g / cm 3 ) (metallocene LLDPE), and azodicarbonamide were prepared as a thermal decomposition type foaming agent. In addition, zinc oxide (manufactured by Sakai Chemical Industry Co., Ltd., product name "OW-212F") was prepared as a decomposition temperature regulator, and 2,6-di-t-butyl-p-cresol, a phenolic antioxidant, was prepared as an antioxidant. 100 parts by mass of polyethylene resin, 8.0 parts by mass of thermal decomposition type foaming agent, 1 part by mass of decomposition temperature regulator, and 0.5 parts by mass of antioxidant were each supplied to a second extruder and melt-kneaded at 130°C to produce a foamable resin composition.

[0080] Next, a linear low-density polyethylene resin (manufactured by Tamapoly Co., Ltd., product name "SK615P") was prepared as the polyethylene resin for the first layer and the third layer. This polyethylene resin was supplied to the first extruder and the third extruder, respectively, and melt-kneaded at 130°C.

[0081] By co-extruding the foamable resin composition from the second extruder, the polyethylene resin for the first layer from the first extruder, and the polyethylene resin for the third layer from the third extruder, an unfoamed multilayer laminate sheet was obtained having a layer made of the foamable resin composition (second layer) and resin films (first layer and third layer) laminated on both sides of the layer. Next, the multilayer laminate sheet was crosslinked by irradiating it with 2.5 Mrad of an electron beam with an accelerating voltage of 500 kV, and then continuously sent into a foaming furnace maintained at 250°C by hot air and an infrared heater to heat and foam it, thereby obtaining a multilayer foam sheet having a first layer (resin film), a second layer (foam), and a third layer (resin film) in that order.

[0082] [Examples 2 to 14, Comparative Examples 1 to 2] The types of resins used in the first to third layers, the thickness of the second layer, and the thicknesses of the first and third layers were changed as shown in Table 1. In addition, the amount of foaming agent blended was changed to change the expansion ratio of the second layer as shown in Table 1. In addition, the foaming agent was blended to change the foam ratio of the third layer as shown in Table 1. Except for this, a multilayer foam sheet was produced in the same manner as in Example 1. The details of each resin are as follows. SEBS: SEBS, manufactured by JSR Corporation, product name "DYNARON 8600P" SF625P: Linear low-density polyethylene, manufactured by Tamapoly Co., Ltd., product name "SF625P" SB-7: Ethylene-vinyl acetate copolymer, manufactured by Tamapoly Co., Ltd., product name "SB-7" HD: High density polyethylene, manufactured by Tamapoly Co., Ltd., product name "HD"

[0083] Table 1 shows the properties and evaluation results of creases of the multilayer foam sheets obtained in the examples and comparative examples.

[0084] [Table 1] *The bending stress in Table 1 indicates the bending stress of both the first and third layers.

[0085] As is clear from the results of the Examples and Comparative Examples, by setting the bending stress of the third layer at each radius of curvature to 1.6 MPa or less, the occurrence of creases could be suppressed when the third layer was wrapped on the inside around a paper core having that radius of curvature. [Explanation of symbols]

[0086] 10 Multi-layer foam sheet 11 First resin layer 12 Second resin layer 13 Third resin layer 14, 15 Adhesive layer C,C2 Neutral point S,S2 distance

Claims

1. A first resin layer made of a resin film or a foam, a second resin layer made of a foam, and a third resin layer made of a resin film or a foam, in this order; The resin constituting the second resin layer is a main component in the second resin layer, and is at least one polyolefin resin selected from the group consisting of polyethylene resins and polypropylene resins, and the content of the resin is 70 mass% or more based on the total amount of the second resin layer; the first resin layer and the third resin layer are both non-adhesive resin layers, A multilayer foam sheet, wherein the third resin layer has a bending stress of 1.6 MPa or less when the radius of curvature (R) is 152.4 mm, as defined by the following formula (1): Bending stress of third resin layer=D×S / R (1) D: tensile modulus of elasticity in the MD direction of the third resin layer (MPa) S: Distance (mm) from the neutral point of the first resin layer to the surface of the third resin layer opposite to the second resin layer R: radius of curvature

2. 2. The multi-layer foam sheet according to claim 1, having a 25% compressive strength of 800 kPa or less.

3. The multi-layer foam sheet according to claim 1 or 2, wherein the multi-layer foam sheet has a total thickness of 50 to 2000 μm.

4. The multilayer foam sheet according to any one of claims 1 to 3, wherein the third resin layer has a tensile strength in the MD direction of 1.5 N or more.

5. The multilayer foam sheet according to any one of claims 1 to 4, wherein a total thickness of the first resin layer and the third resin layer is 50% or less of a total thickness of the multilayer foam sheet.

6. The multilayer foam sheet according to any one of claims 1 to 5, wherein the bending stress of the third resin layer defined by the above formula (1) is 1.6 MPa or less when the radius of curvature (R) is 101.6 mm.

7. The multilayer foam sheet according to any one of claims 1 to 6, wherein the bending stress of the third resin layer defined in (1) above is 1.6 MPa or less when the radius of curvature (R) is 76.2 mm.

8. The multilayer foam sheet according to any one of claims 1 to 7, wherein the bending stress of the first resin layer defined by the following formula (2) is 1.6 MPa or less when the radius of curvature (R2) is 152.4 mm: Bending stress of first resin layer=D2×S2 / R2 (2) D2: tensile modulus of elasticity in the MD direction of the first resin layer (MPa) S2: Distance (mm) from the neutral point of the third resin layer to the surface of the first resin layer opposite to the second resin layer R2: radius of curvature

9. The multilayer foam sheet according to claim 8, wherein the bending stress of the first resin layer defined by the above formula (2) is 1.6 MPa or less when the radius of curvature (R2) is 101.6 mm.

10. The multilayer foam sheet according to claim 8 or 9, wherein the bending stress of the first resin layer defined by the above formula (2) is 1.6 MPa or less when the radius of curvature (R2) is 76.2 mm.

11. The multilayer foam sheet according to any one of claims 1 to 10, wherein the first resin layer has a tensile strength of 1.5 N or more.

12. The multilayer foam sheet according to any one of claims 1 to 11, wherein the first resin layer and the third resin layer have a foaming rate of 66% or less.

13. 13. An adhesive tape comprising the multilayer foam sheet according to claim 1 and an adhesive material provided on at least one surface of the multilayer foam sheet.

Citation Information

Patent Citations

  • Foam laminated sheet for car interior material

    JP2000141528A

  • Multilayered polypropylene resin foamed sheet and assembling box therefor

    JP2002331624A

  • Styrene-based resin laminated sheet and container

    JP2004230795A

  • Heat insulating material for electronic part and method of manufacturing the same

    JP2011005797A

  • Crosslinked polyolefin resin foamed sheet

    JP2014028925A