High-power gallium nitride electronics using miscut substrates

By employing homoepitaxial GaN layers on bulk GaN substrates with precise misorientation, the limitations of conventional GaN growth on foreign substrates are overcome, resulting in improved surface morphology and electrical properties for high power electronic devices.

JP7561808B2Active Publication Date: 2024-10-04AVOGY INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022178273
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2013-11-04
Filing Date
2022-11-07
Publication Date
2024-10-04
Estimated Expiration
2034-11-03

AI Technical Summary

Technical Problem

Conventional methods for growing gallium nitride (GaN) layers on foreign substrates, such as silicon carbide, limit the usable thickness and are plagued by high defect densities, complicating the creation of vertical power electronic devices like JFETs and other field-effect transistors.

Method used

Utilizing homoepitaxial GaN layers on bulk GaN substrates with a growth plane oriented less than 1 degree from the (0001) plane, achieving a misorientation of 0.15° to 0.65°, which improves surface morphology and electrical properties for high power electronic devices.

Benefits of technology

The method enables thicker GaN layers with lower defect densities, higher electron mobility, and improved breakdown fields, reducing resistance and enhancing device performance, particularly in high voltage applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561808000003
    Figure 0007561808000003
  • Figure 0007561808000004
    Figure 0007561808000004
  • Figure 0007561808000005
    Figure 0007561808000005
Patent Text Reader

Abstract

Gallium nitride (GaN)-based electronic devices, field-effect transistors, diodes, and fabrication methods useful for high-power electronics are provided. The electronic device (PN diode 100) has a hexagonal crystal structure and <0001> The electronic device includes a III-V substrate having a growth surface normal characterized by a misorientation of 0.15° to 0.65° from the direction of the first epitaxial layer 115. The electronic device also includes a first epitaxial layer 115 bonded to the III-V substrate, a second epitaxial layer 120 bonded to the first epitaxial layer, a first contact (cathode 135) electrically connected to the substrate 110, and a second contact (anode 130) electrically connected to the second epitaxial layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001]

[0001] Power electronics is widely used in a variety of applications. Power electronic devices are commonly used in circuits to change the form of electrical energy, for example, from AC to DC, from one voltage level to another, or in other ways. Such devices can operate over a wide range of power levels, from milliwatts in mobile devices to hundreds of megawatts in high voltage power grids. Despite advances in power electronics, there is a need in the field for improved electronic systems and methods of operation. Summary of the Invention [Problem to be solved by the invention]

[0002]

[0002] The present invention relates generally to electronic devices. More specifically, the present invention relates to the fabrication of gallium nitride (GaN)-based epitaxial layers useful for high power electronics. In a particular embodiment, a GaN substrate having a growth surface misoriented from the (0001) plane by less than 1 degree to the <1-100> direction is utilized in the epitaxial growth process. The surface morphology and electrical properties of the epitaxial layers grown on the misoriented substrate are suitable for use in high power electronic devices. The methods and techniques can be applied to a variety of compound semiconductor systems including diodes, FETs, etc. [Means for solving the problem]

[0003] According to an embodiment of the present invention, there is provided an electronic device comprising: a hexagonal crystal structure; <0001> The electronic device includes a III-V substrate having a growth surface normal characterized by a misorientation of 0.15° to 0.65° from the direction. The electronic device also includes a first epitaxial layer coupled to the III-V substrate and a second epitaxial layer coupled to the first epitaxial layer. The electronic device further includes a first contact electrically coupled to the substrate and a second contact electrically coupled to the second epitaxial layer.

[0004] According to an embodiment of the present invention, there is provided a method for manufacturing an electronic device, the method comprising: <0001> The method includes providing a III-V substrate having a growth surface normal characterized by a misorientation of 0.15° to 0.65° from a direction. The method also includes growing a first epitaxial layer coupled to the III-V substrate and growing a second epitaxial layer coupled to the first epitaxial layer. The method further includes forming a first contact electrically coupled to the substrate and forming a second contact electrically coupled to the second epitaxial layer.

[0005]

[0005] Many advantages are achieved by the methods of the present invention over the prior art. For example, embodiments of the present invention provide methods and systems for fabricating epitaxial layers suitable for use in high power electronic devices. In one embodiment, device performance during high voltage operation (e.g., greater than 200V) is improved over prior designs. These and other embodiments of the present invention, along with many of its advantages and features, are described in more detail in the following text and in conjunction with the accompanying drawings. [Brief description of the drawings]

[0006] [Figure 1] 1 is a schematic cross-sectional view of a high voltage PN diode structure according to an embodiment of the present invention. [Figure 2A]FIG. 2 is a schematic diagram showing Miller indices for a hexagonal phase bulk GaN substrate wafer. [Figure 2B] FIG. 1 is a schematic diagram showing the crystal axis direction of a c-plane GaN crystal. [Figure 2C] FIG. 2 is a schematic diagram illustrating the vectorial nature of the miscut angle according to an embodiment of the present invention. [Figure 2D] FIG. 2 is a schematic diagram illustrating the radial vector nature of the miscut angle according to an embodiment of the present invention. [Figure 3A] 1 is a Nomarski micrograph of an epitaxial surface where the substrate misorientation is less than 0.15°. [Figure 3B] 1 is a Nomarski micrograph of an epitaxial surface where the substrate misorientation is greater than 0.65°. [Figure 4A] 1 is a plot showing the surface morphology of various epitaxially grown layers mapped against orthogonal substrate orientations. [Figure 4B] 1 is a graph illustrating wafer quality data as a function of miscut angle according to an embodiment of the present invention. [Figure 5A] 4 is a graph showing forward bias current-voltage characteristics of a high voltage PN diode according to an embodiment of the present invention. [Figure 5B] 4 is a graph showing reverse bias current-voltage characteristics of a high voltage PN diode according to an embodiment of the present invention. [Figure 6] 4 is a graph showing the reverse bias current-voltage characteristics of a high voltage GaN PN diode according to an embodiment of the present invention compared to a GaN PN diode fabricated using a conventional substrate. [Figure 7] 1 is a simplified flow chart illustrating a method for manufacturing an electronic device according to an embodiment of the present invention. [Figure 8A] FIG. 1 shows the crystal planes of a wurtzite crystal. [Figure 8B] FIG. 2 is another diagram showing the crystal faces of a wurtzite crystal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007]

[0020] Embodiments of the present invention relate to electronic devices. More specifically, the present invention relates to the fabrication of gallium nitride (GaN)-based epitaxial layers useful for high power electronics. In a particular embodiment, a GaN substrate having a growth surface misoriented from the (0001) plane by less than 1 degree to the <1-100> direction is utilized in the epitaxial growth process. The surface morphology and electrical properties of the epitaxial layers grown on the misoriented substrate are suitable for use in high power electronic devices. The methods and techniques can be applied to a variety of compound semiconductor systems, including diodes, FETs, etc.

[0008]

[0021] GaN-based electronic and optoelectronic devices are undergoing rapid development. Desirable properties associated with GaN and related alloys and heterostructures include high bandgap energy for visible and ultraviolet light emission, good transport properties (e.g., high electron mobility and saturation velocity), high breakdown field, and high thermal conductivity. In accordance with an embodiment of the present invention, gallium nitride (GaN) epitaxy on quasi-bulk GaN substrates is utilized to fabricate vertical GaN-based semiconductor devices that are not possible using conventional techniques. For example, conventional methods of growing GaN include using foreign substrates such as silicon carbide (SiC). This can limit the usable thickness of GaN layers grown on the foreign substrate due to differences in thermal expansion coefficients and lattice constants between the GaN layer and the foreign substrate. High defect densities at the interface between GaN and the foreign substrate further complicate attempts to create vertical devices, including power electronic devices such as JFETs and other field effect transistors.

[0009]

[0022] Homoepitaxial GaN layers on bulk GaN substrates, on the other hand, are utilized in the embodiments described herein to provide superior properties over conventional techniques and devices. For example, the electron mobility μ is higher for a given background doping level N. Since resistivity is inversely proportional to electron mobility, this provides a low resistivity ρ as given by equation (1): JPEG0007561808000001.jpg1217,(1) Here, q is the elementary charge.

[0010]

[0023] Another superior property offered by homoepitaxial GaN layers on bulk GaN substrates is a high critical electric field for avalanche breakdown. A high critical electric field allows a large voltage to be supported over a smaller length L than materials with a lower critical electric field. A smaller length for current to flow with less resistance results in a lower resistance R than other materials, and the resistance can be determined by the following formula: JPEG0007561808000002.jpg1114,(2) where A is the cross-sectional area of ​​the channel or current path.

[0011]

[0024] In general, a tradeoff exists between the physical size of the device required to support high voltages in the device's off-state and the ability to pass current through the same device with low resistance in the on-state. In many cases, GaN is preferred over other materials to minimize this tradeoff and maximize performance. Also, GaN layers grown on bulk GaN substrates have a lower defect density compared to layers grown on incompatible substrates. The lower defect density results in better thermal conductivity, lower trap-related effects such as dynamic on-resistance, and improved reliability.

[0012]

[0025] 1 is a schematic cross-sectional view of a high-voltage PN diode structure according to an embodiment of the present invention. Referring to FIG. 1, a first gallium nitride (GaN) epitaxial layer 115 (e.g., N -The GaN drift region (GaN drift region) is formed on a GaN substrate 110 having the same conductivity type. The GaN substrate 110 can be a quasi-bulk or bulk GaN material on which the first GaN epitaxial layer 115 is grown. A buffer layer (not shown) can be utilized, as will be apparent to those skilled in the art. The dopant concentration (e.g., doping density) of the GaN substrate 110 can be varied depending on the desired function. For example, the GaN substrate 110 can be 1×10 17 cm -3 ~1×10 19 cm -3 The GaN substrate 110 may have an n+ conductivity type, with a dopant concentration ranging from 0.1 to 0.5. Although the GaN substrate 110 is shown as including a single material composition, multiple layers may be provided as part of the substrate. Also, adhesion layers, buffer layers, and other layers (not shown) may be used during the epitaxial growth process. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.

[0013]

[0026] The properties of the first GaN epitaxial layer 115 can also be varied, depending on the desired function. The first GaN epitaxial layer 115 can function as a drift region for a PN diode, and therefore can be a relatively lightly doped material. For example, the first GaN epitaxial layer 115 can be a 1×10 14 cm -3 ~1×10 18 cm -3 The dopant concentration can be uniform or can vary, for example, as a function of the drift region thickness.

[0014]

[0027] The thickness of the first GaN epitaxial layer 115 can also vary substantially depending on the desired functionality. As discussed above, homoepitaxial growth can allow the first GaN epitaxial layer 115 to be grown much thicker than layers formed using conventional methods. In general, in some embodiments, the thickness can vary, for example, between 0.5 μm and 100 μm. In other embodiments, the thickness is greater than 5 μm. The resulting parallel plane breakdown voltage for the PN diode 100 can vary depending on the embodiment. Some embodiments provide a breakdown voltage of at least 100 V, 300 V, 600 V, 1.2 kV, 1.7 kV, 3.3 kV, 5.5 kV, 13 kV, or 20 kV.

[0015]

[0028] Referring again to FIG. 1, a second GaN epitaxial layer 120 is formed on the first GaN epitaxial layer 201. The second GaN epitaxial layer 120 is used in forming the p-type region of the PN diode and has a different conductivity type than the first GaN epitaxial layer 115. For example, if the first GaN epitaxial layer 115 is formed of n-type GaN material, the second GaN epitaxial layer 120 will be formed of p-type GaN material, and vice versa. As shown in FIG. 1, an insulating region is formed to define the lateral extent of the PN diode. Suitable techniques for forming an insulating region characterized by a high resistance may include ion implantation, etching and epitaxial regrowth of a low conductive material, etching and deposition of insulating material such as oxide and / or nitride, or combinations thereof. Those skilled in the art will recognize many variations, modifications, and alternatives.

[0016]

[0029] The thickness of second GaN epitaxial layer 120 can vary depending on the process used to form the layer and the device design. In some embodiments, second GaN epitaxial layer 120 has a thickness between 0.1 μm and 5 μm. In other embodiments, second GaN epitaxial layer 120 has a thickness between 0.3 μm and 1 μm.

[0017]

[0030] The second GaN epitaxial layer 120 is grown to, for example, about 5×10 17 cm -3 From about 1×10 19 cm -3 In addition, like other epitaxial layers, the dopant concentration of second GaN epitaxial layer 120 can be uniform or non-uniform as a function of thickness. In some embodiments, the dopant concentration increases with thickness such that the dopant concentration is relatively low near first GaN epitaxial layer 115 and increases away from first GaN epitaxial layer 115. Such embodiments provide a higher dopant concentration at the top of second GaN epitaxial layer 120 to which metal contacts can subsequently be formed. Other embodiments utilize a heavily doped contact layer (not shown) to form an ohmic contact.

[0018]

[0031] One method of forming the second GaN epitaxial layer 120, as well as the other layers described herein, may be via a regrowth process using in situ etching and diffusion fabrication processes. These fabrication processes are described in more detail in U.S. patent application Ser. No. 13 / 198,666, filed Aug. 4, 2011, the disclosure of which is incorporated herein by reference in its entirety.

[0019]

[0032] FIG. 1 also illustrates electrical contacts formed for an electronic device according to an embodiment of the present invention. As shown in FIG. 1, a metal structure 135 is formed in electrical contact with the GaN substrate 110. The metal structure 135 can be one or more layers of ohmic metal that serves as a contact for the cathode of the PN diode 100. For example, the metal structure 135 can include titanium-aluminum (Ti / Al) ohmic metal. Other metals and / or alloys can be used, including, but not limited to, aluminum, nickel, gold, or combinations thereof. In some embodiments, the outermost metal of the metal structure 135 can include gold, tantalum, tungsten, palladium, silver, aluminum, or combinations thereof. The metal structure 135 can be formed using any of a variety of methods, such as, for example, sputtering, evaporation, etc.

[0020]

[0033] FIG. 1 also shows an additional metal structure 130 in electrical contact with the second epitaxial layer 120. The additional metal structure 130 can be one or more layers of ohmic metal including metals and / or alloys similar to the metal structure 135. The additional metal structure 130 is formed on the second epitaxial layer 120 to serve as an anode contact for the PN diode 100. The additional metal structure 130 can be formed using various techniques including lift-off and / or deposition with subsequent etching, which can vary depending on the metal used. Examples of metals include nickel-gold (Ni / Au), etc. In some implementations, the additional metal structure 130 is formed in contact with the first epitaxial layer, and a Schottky metal is utilized as appropriate for forming a Schottky diode.

[0021]

[0034] Different dopants can be used to create the n-type and p-type GaN epitaxial layers and structures disclosed herein. For example, n-type dopants can include silicon, oxygen, etc. P-type dopants can include magnesium, beryllium, calcium, zinc, etc.

[0022]

[0035] Although some embodiments are described with respect to GaN substrates and GaN epitaxial layers, the invention is not limited to these particular binary III-V materials, but is applicable to a broader class of III-V materials, particularly III-nitride materials. Also, while a GaN substrate is shown in FIG. 1, embodiments of the invention are not limited to GaN substrates. Other III-V materials, particularly III-nitride materials, are included within the scope of the invention and may be substituted for the illustrated GaN substrate as well as other GaN-based layers and structures described herein. By way of example, binary III-V (e.g., III-nitride) materials, ternary III-V (e.g., III-nitride) materials such as InGaN and AlGaN, quaternary III-nitride materials such as AlInGaN, and doped versions of these materials are included within the scope of the invention.

[0023]

[0036] The fabrication process described in connection with FIG. 1 utilizes a process flow in which an n-type drift layer is grown using an n-type substrate. However, the invention is not limited to this particular configuration. In other embodiments, a substrate with p-type doping is utilized. Additionally, embodiments can use materials with opposite conductivity types to provide devices with different functions. Thus, while some examples relate to the growth of n-type GaN epitaxial layer(s) doped with silicon, in other embodiments, the techniques described herein are applicable to the growth of highly or lightly doped materials, p-type materials, and materials doped with dopants in addition to or other than silicon, such as Mg, Ca, Be, Ge, Se, S, O, Te, etc. The substrates described herein can include single material systems or composite material systems including composite structures of multiple layers. Those skilled in the art will recognize many variations, modifications, and alternatives.

[0024]

[0037] During the growth of the epitaxial layers shown in FIG. 1, the inventors have determined that epitaxial layers grown on substrates characterized by a given miscut angle provide improved performance in terms of high power electronic devices (e.g., operating at high voltages) compared to conventional structures. For epitaxial layers grown on the c-plane of a GaN substrate, the morphology of the layers and, importantly, the performance of devices formed using these epitaxial layers degrade at higher voltages, reducing their applicability for high power applications. Without limiting the embodiments of the present invention, the inventors have determined that misorientation of the growth surface of the substrate from a crystal plane (e.g., the c-plane) by only a small percentage in a given direction improves the morphology of the layers and improves the device performance of devices fabricated using the improved layers.

[0025]

[0038] 8A and 8B are diagrams showing the crystal planes of a wurtzite crystal. In FIG. 8A, the a-plane of a wurtzite crystal is shown, and in FIG. 8B, the m-plane of a wurtzite crystal is shown. The c-axis (0001) is perpendicular to the plane of the figure, and the (000-1) axis points in the plane of the figure. As shown in FIG. 8A, there are six a-planes, all 60° apart. As shown in FIG. 8B, there are six m-planes, all 60° apart. When stacked, the m-planes and a-planes interpenetrate each other with an angle of 30° between them. It will be apparent to those skilled in the art that GaN has a wurtzite crystal structure.

[0026]

[0039] FIG. 2A is a schematic diagram showing Miller indices for a hexagonal phase bulk GaN substrate wafer. The dashed arrows indicate <0001> 2A illustrates the orientation of the <1-100>, <11-20>, and <11-20> directions. The solid arrows 210 indicate the misorientation directions relative to the <1-100> directions utilized for epitaxial growth of high voltage electronic device structures described in accordance with certain embodiments herein. As shown in FIG. 2A, embodiments of the present invention utilize substrates whose growth planes are not aligned with the (0001) plane. As described herein, the normal to the growth plane is aligned with the (0001) plane. <0001> direction (i.e., misorientation angle (θ)) toward the -<1-100> or <1-100> direction by 0<θ<1.0°. According to some embodiments of the invention, the magnitude of θ is in the range of about 0.15°<θ<0.65°. In certain embodiments, the range of the misorientation angle θ is about 0.4°<θ<0.5°.

[0027]

[0040] Thus, according to embodiments of the present invention, the growth surface of a III-V (e.g., GaN) substrate is misoriented from the c-plane toward the positive or negative m-direction at an angle having a value between zero and 1.0°. Additionally, the normal to the growth surface of the substrate can also be misoriented such that it is tilted toward or away from the a-direction. <0001> The misorientation away from the a direction towards the a direction is zero in some embodiments. In the embodiment shown in FIG. 2A, the normal to the growth surface is <0001> A misorientation of -0.15° to -0.65° from the <1-100> direction, and <0001> It is characterized by a zero misorientation from the <11-20> direction to the <11-20> direction.

[0028]

[0041] In some embodiments, the orientation of the growth surface is such that the growth surface is tilted with respect to the (0001) plane, resulting in the normal of the growth surface being tilted less than 1 degree toward the positive <1-100> direction. The inventors have determined that tilting the growth surface by misorienting the growth surface away from the (0001) plane by 0.15° to 0.65° toward the negative m direction or 0.15° to 0.65° toward the positive m direction provides an improvement in the surface morphology of the thick epitaxial layer and accordingly in device performance. Thus, embodiments of the present invention provide a growth surface tilted with respect to the (0001) plane at an angle greater than 0.15° and less than 1 degree. One skilled in the art would recognize many variations, modifications, and alternatives.

[0029]

[0042] FIG. 2B is a schematic diagram illustrating the miscut angle according to an embodiment of the present invention. The solid arrows are associated with the a-plane and the dashed arrows are associated with the m-plane. For this figure, the c-axis is perpendicular to the plane of the figure. According to an embodiment of the present invention, for a GaN wafer, the c-plane is (near) perpendicular to the wafer surface, and thus the m- and a-directions are oriented as shown in FIG. 2B. It should be noted that while the example shown in FIG. 2B utilizes one axis convention, other axis conventions can be utilized, including an axis convention rotated 180° relative to the wafer flat. Both conventions are symmetrically equivalent.

[0030]

[0043] The miscut target direction 250 is shown towards the left (parallel to the plane) for each of the axis conventions. A given specification window 251 is represented as a box centered on the m direction and can also include the a direction. For the axis convention shown, the miscut target is along [-1100]. For the alternative axis convention rotated 180° relative to the wafer plane, the miscut target is along [1-100]. Thus, for both conventions, when the plane is on the bottom side, both miscut targets point to the left.

[0031]

[0044] 2C is a schematic diagram illustrating the vector nature of the miscut angle according to an embodiment of the present invention. As shown in FIG. 2C, the miscut angle R is a vector quantity defined by components in the m and a directions. Both can vary independently across the wafer and can have different effects. Physically, this vector can be considered as the crystallographic c direction projected onto the plane defined by the surface of the wafer, as shown by rectangular region 250.

[0032]

[0045] 2D is a schematic diagram illustrating an alternative specification of the miscut angle according to an embodiment of the present invention, in which the miscut specification 260, rather than being specified by the miscut angle for the m-plane and a-plane components, can be specified by the miscut angle magnitude |R| and θ direction, as shown in region 260.

[0033]

[0046] FIG. 3A is a Nomarski micrograph of an epitaxial surface when the substrate misorientation is less than 0.15°. FIG. 3B is a Nomarski micrograph of an epitaxial surface when the substrate misorientation is greater than 0.65°. As shown in FIG. 3A, the surface morphology of epitaxial layers grown on substrates with misorientation less than 0.15° is characterized by large hexagonal hillocks with lateral dimensions on the order of tens to hundreds of microns and heights up to several microns. The inventors believe that the lateral dimensions of the hillocks increase as the thickness of the epitaxial layer increases. Referring to FIG. 3B, the surface morphology of epitaxial layers grown on substrates with misorientation greater than 0.65° is characterized by a scalloped surface, which may also be referred to as a ridged or scaly surface with lateral and vertical dimensions on the order of several microns. Devices fabricated with epitaxial layers grown on these substrates utilizing both of these substrate misorientation values ​​outside the scope of the present invention are characterized by undesirable levels of device leakage during operation in the high power regime.

[0034]

[0047] As described in further detail in connection with Figure 4A, the inventors have determined that a strong correlation exists between substrate misorientation, surface morphology, and high power device performance. For substrate misorientations of about -0.4° to -0.5° from the m-direction, good surface morphology results in devices with improved high power operating characteristics.

[0035]

[0048] FIG. 4A is a plot showing the surface morphology of various epitaxially grown layers mapped against substrate misorientation in orthogonal directions (i.e., <1-100> and <11-20> directions). The vertical axis represents the miscut angle in degrees toward the a-direction (toward the <11-20> direction). The horizontal axis represents the miscut angle toward the m-direction (toward the <1-100> direction). As shown in FIG. 3, good morphology (black circles) for the epitaxial layers results when the miscut angle (θ) is near zero toward the a-direction and about −0.35° to −0.55° toward the m-direction. In a particular embodiment, a miscut angle of −0.4° to −0.5° toward the m-direction is used.

[0036]

[0049] It should be noted that good surface morphology can be obtained by keeping the miscut angle of the substrate at substantially zero degrees toward the a-direction. Also, referring to FIG. 4A, it should be noted that good surface morphology can also be obtained by adjusting the misorientation in both the a-direction and the m-direction. Increasing the absolute value of the miscut angle in the m-direction will also result in good surface morphology, as shown by the poor surface morphology at a-direction=-0.13° and m-direction=-0.33° (data point 421) and the good surface morphology obtained for a miscut of -0.13° toward the a-direction and m-direction=-0.43° (data point 423). Thus, the change in the miscut angle relative to the a-direction can be compensated by the change in the miscut angle relative to the m-direction. Many variations, modifications, and alternatives will be recognized by those skilled in the art.

[0037]

[0050] Referring to FIG. 4A, 70 data points are shown, representing five points measured on 14 GaN substrates. The data provided in relation to the five points on each substrate included miscut information. The miscut specifications for these wafers were a miscut of -0.4° towards the m-direction and a miscut of 0° towards the a-direction, both with a tolerance of ±0.3°. The five points were imaged using a Nomarski microscope and determined to be good (black circles), bad (x), or borderline (white circles). Good morphology was obtained for a miscut close to 0° towards the a-direction, and a miscut of approximately -0.4° to -0.5° towards the m-direction. Thus, as demonstrated by the data, miscuts of less than -0.3° towards the m-direction were obtained. <0001> Miscutting in the direction of the crystallographic plane results in poor morphology. Furthermore, high miscut angles (i.e. <0001> Any deviation from the normal (greater than ±0.6° relative to the direction) will result in poor morphology.

[0038]

[0051] Considering manufacturing tolerances and variations in crystal plane orientation across the wafer, embodiments of the present invention utilize a target miscut value that produces the largest possible area of ​​material with good surface morphology (and consequently high device yield). As shown in FIG. 4A and described above, a large miscut toward the m-direction can accommodate some variations in the miscut toward the a-direction. With reference to FIG. 4A, an a-direction miscut of -0.13° is represented by the horizontal dashed line. At this value of a-direction miscut, an m-direction miscut of less than 0.35° produces poor morphology, while a larger m-direction miscut results in good morphology. Thus, the m-direction and a-direction miscuts interact to affect morphology, and the larger m-direction miscut can be utilized to accommodate variations in the a-direction miscut.

[0039]

[0052] It should be noted that although substrate specifications may specify a particular miscut orientation for the substrate, orientation variations across the substrate may result in some regions of the substrate being characterized by misorientation within the range provided by embodiments of the present invention, and other regions being characterized by misorientation outside the range provided by embodiments of the present invention. That is, substrate manufacturers allow some margin in miscut variation. Miscut variations tend to be relatively large for quasi-bulk GaN grown by HVPE on non-native substrates. Thus, the surface morphology will vary across the wafer, as shown by the data in FIG. 4A.

[0040]

[0053] As an example, if the substrate specification is a misorientation of 0.3°±0.3° towards the m-direction, regions of the substrate can be characterized by zero misorientation while other regions are characterized by a misorientation of 0.6°. The inventors have determined that for substrates with a range of misorientation angles, the morphology is better in regions with misorientation angles within the range of the embodiments described herein, and this can be correlated to improved device performance.

[0041]

[0054] FIG. 4B is a graph showing wafer quality data as a function of miscut angle according to an embodiment of the present invention. The wafer quality data was measured based on Nomarski images obtained from wafers grown with various miscut angles. Each point represents a vector starting from the origin and ending at the data point. Wafers with "good" quality are indicated by diamond symbols, wafers with "bad" quality are indicated by square symbols, and wafers with borderline quality are indicated by triangle symbols. By considering miscuts toward the a direction, the inventors have confirmed that poor morphology can be related to the miscut angle, not just the magnitude.

[0042]

[0055] FIG. 5A is a graph showing forward bias current-voltage characteristics of a high voltage PN diode according to an embodiment of the present invention. FIG. 5B is a graph showing reverse bias current-voltage characteristics of a high voltage PN diode according to an embodiment of the present invention. As shown in FIG. 5A, the PN diode has a substantially linear IV characteristic and turns on at about 3V. Referring to FIG. 5B, under reverse bias, the PN diode does not substantially conduct current until the voltage reaches about 2500V, at which point breakdown occurs. Thus, embodiments of the present invention are suitable for high voltage (e.g., greater than 400V) operation.

[0043]

[0056] FIG. 6 is a graph showing the reverse bias current-voltage characteristics of a high voltage GaN PN diode according to an embodiment of the invention (solid line) compared to a GaN PN diode fabricated using a conventional substrate, which may include a substrate cut at a misorientation angle (θ) outside the range suitable for use in accordance with embodiments of the invention.

[0044]

[0057] As shown in FIG. 6, under reverse bias, the reverse leakage current is substantially the same up to a voltage of about 700V. At reverse bias voltages above 700V, high voltage PN diodes fabricated according to embodiments of the present invention maintain an approximately linear increase in reverse leakage current with voltage (plotted on a logarithmic scale). Thus, in devices, e.g., PN diodes, Schottky diodes, vertical JFETs, HEMTs, integrated FETs and diodes, combined PN / Schottky diodes, etc., operating at high voltages, e.g., >600V, >1200V, >1700V, etc., the use of substrates with predetermined misorientation angles provides improved performance, particularly in the high voltage regime.

[0045]

[0058] It should be noted that embodiments of the present invention are particularly suited for applications in high power regimes. For low power regimes, such as in connection with some LED and laser operation, and other forward bias operation, the effects of a substrate not miscut within the range provided by embodiments of the present invention are not detectable. This is because the effects that depend on the proper miscut angle cannot be observed in some implementations until the high power regime is entered, as shown in FIG. 6. Thus, embodiments of the present invention are suited for device applications utilizing thick epitaxial layers (e.g., >3 μm thick drift layers) operated in high power regimes (e.g., >200 V). Since conventional GaN devices operate in low power regimes (e.g., less than 200 V), the effects of proper misorientation of the substrate may not have been observed during typical operation. Conversely, the inventors are well aware of the scope of problems presented by conventionally oriented substrates during operation in high power regimes. Thus, embodiments of the present invention are particularly applicable to devices in which one or more epitaxial layers are characterized by low doping and high thickness, e.g., GaN vertical PN diodes. Thus, embodiments of the present invention are particularly suited to devices including epitaxial layers with a thickness of more than 5 μm.

[0046]

[0059] 7 is a simplified flow chart illustrating a method for manufacturing an electronic device according to an embodiment of the present invention. Referring to FIG. 7, the method includes: <0001> The method includes providing (710) a III-V substrate having a growth surface normal characterized by a misorientation of 0.15° to 0.65° from the <11-20> direction. The III-V substrate is an n-type GaN substrate in certain embodiments. In one embodiment, the growth surface normal is misoriented toward the negative <1-100> direction, e.g., within a range of 0.4° to 0.5°. In certain embodiments, the growth surface normal is characterized by a substantially zero degree misorientation toward the <11-20> direction. In other embodiments, the misorientation has components toward / away from both the <1-100> direction and the <11-20> direction.

[0047]

[0060] The method also includes growing (712) a first epitaxial layer coupled to the III-V substrate, and growing (714) a second epitaxial layer coupled to the first epitaxial layer. In some devices, the method includes forming laterally disposed insulating regions in the second epitaxial layer. In some high power device applications, the first epitaxial layer includes an n-type GaN epitaxial layer having a thickness greater than 3 μm, and the second epitaxial layer includes a p-type GaN epitaxial layer. In some implementations, the method also includes forming a third epitaxial layer disposed between the second epitaxial layer and the second contact. The doping density of the third epitaxial layer is higher than the doping density of the second epitaxial layer.

[0048]

[0061] The method further includes forming a first contact (716) electrically connected to the substrate and forming a second contact (718) electrically connected to the second epitaxial layer. As an exemplary device, a PN diode can be fabricated using the techniques described herein, where the first contact is the cathode and the second contact is the anode of the PN diode. The electronic device can also be a Schottky diode.

[0049]

[0062] It should be understood that the specific steps depicted in FIG. 7 provide a particular method of manufacturing an electronic device according to an embodiment of the present invention. Other sequences of steps may be performed according to alternative embodiments. For example, alternative embodiments of the present invention may perform the steps described above in a different order. Also, individual steps depicted in FIG. 7 may include multiple sub-steps that may be performed in various orders, as appropriate for the individual step. Furthermore, additional steps may be added or removed depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.

[0050]

[0063] It is also understood that the examples and embodiments described herein are for illustrative purposes only, and that various modifications or changes therein will be suggested to those skilled in the art and are to be included within the spirit and scope of this application and the scope of the appended claims.

Claims

1. a III-V substrate having a hexagonal crystal structure and a growth surface normal characterized by a misorientation from the [0001] direction to a [1-100] direction at an angle ranging from -0.35° to -0.6° and to a [11-20] direction at an angle ranging from -0.1° to -0.15°; a first epitaxial layer coupled to the III-V substrate; a second epitaxial layer coupled to the first epitaxial layer; one or more recessed regions extending into the second epitaxial layer, each of the one or more recessed regions defining a sidewall surface and a lateral surface in the second epitaxial layer, a doped region extending into the sidewall surface and the lateral surface; a drain contact electrically connected to the III-V substrate; a source contact electrically connected to the second epitaxial layer; a gate contact electrically connected to the doped region; A field effect transistor comprising:

2. The field effect transistor of claim 1 , wherein the III-V substrate comprises an n-type GaN substrate.

3. 2. The field effect transistor of claim 1, wherein the first epitaxial layer comprises an n-type GaN epitaxial layer and the second epitaxial layer comprises an n-type GaN epitaxial layer.

4. The field effect transistor of claim 1 , wherein the doped region comprises a diffusion region.

5. The field effect transistor of claim 1 , wherein the doped region comprises zinc.

6. 2. The field effect transistor of claim 1, wherein the doped region comprises magnesium.

7. 2. The field effect transistor of claim 1, wherein said doped region comprises beryllium.

8. The field effect transistor of claim 1 , wherein the doped region comprises calcium.

9. 2. The field effect transistor of claim 1, wherein the first epitaxial layer has a thickness greater than 5 μm.

10. 2. The field effect transistor of claim 1, wherein a dopant concentration in said first epitaxial layer varies as a function of a thickness of said first epitaxial layer.

11. 2. The field effect transistor of claim 1, wherein a dopant concentration in said second epitaxial layer varies as a function of a thickness of said second epitaxial layer.

12. 2. The field effect transistor of claim 1, wherein said lateral surfaces are substantially perpendicular to a growth direction of the first epitaxial layer.

13. The field effect transistor of claim 1 , wherein the sidewall surfaces are substantially parallel to a growth direction of the second epitaxial layer.

Citation Information

Patent Citations

  • Manufacture of static induction transistor

    JP1984108366A

  • Semiconductor element and its manufacture

    JP2006156958A

  • Gate drive for wide bandgap semiconductor device

    JP2008294437A

  • Method and system for performing epitaxial process on miscut bulk substrate

    JP2012235091A

  • Gallium nitride crystal, homoepitaxial gallium nitride-based device and method for producing the same

    JP2013067556A