Polyimide film having high dimensional stability and method for producing same
A polyimide film with controlled dimensional changes and balanced thermal expansion is produced to maintain flatness and prevent wrinkles during metal foil lamination, addressing the issue of film distortion in flexible laminates.
Patent Information
- Application Number
- JP2023528935
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-24
- Filing Date
- 2021-11-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-11-22
AI Technical Summary
Polyimide films used in flexible metal foil laminates suffer from loss of flatness and wrinkle formation after metal foil lamination processes such as coating, sputtering, or vapor deposition.
A polyimide film is produced through a method involving the use of a thermomechanical analyzer to measure dimensional changes, ensuring a specific dimensional change range is maintained by controlling the heating and cooling processes, and incorporating a stretching process to achieve a balanced thermal expansion coefficient.
The resulting polyimide film maintains excellent flatness even after lamination with metal foil, reducing wrinkle formation and enhancing its suitability for applications requiring high flatness.
Smart Images

Figure 0007561987000002 
Figure 0007561987000003 
Figure 0007561987000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide film that maintains its flatness and does not develop wrinkles even after a metal foil is coated, sputtered, or evaporated thereon, and a method for producing the same. [Background technology]
[0002] Polyimide (PI) is a polymeric material that has the highest levels of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials, based on imide rings, which have excellent chemical stability along with a rigid aromatic main chain. Polyimide films have been attracting attention as a material for various electronic devices that require the above-mentioned properties. Examples of microelectronic components to which polyimide films can be applied include flexible thin circuit boards with high circuit integration density that can accommodate the trend toward lighter and smaller electronic products. Polyimide films are widely used, particularly as insulating films for thin circuit boards. The thin circuit board generally has a structure in which a circuit including a metal foil is formed on an insulating film. Such a thin circuit board is broadly called a flexible metal foil clad laminate (FMC), and when a thin copper plate is used as the metal foil, it is more narrowly called a flexible copper clad laminate (FCCL).
[0003] Examples of methods for producing flexible metal foil laminates include (i) a casting method in which polyamic acid, a precursor of polyimide, is cast or applied onto a metal foil and then imidized, (ii) a metallizing method in which a metal layer is directly formed on a polyimide film by sputtering, and (iii) a lamination method in which a polyimide film and a metal foil are bonded together by heat and pressure via a thermoplastic polyimide. In particular, the metallizing method is a method for producing flexible metal foil laminates by sputtering a metal such as copper on a polyimide film having a thickness of, for example, 20 to 38 μm, and sequentially depositing a tie layer and a seed layer. This method is advantageous in forming ultra-fine circuits with a circuit pattern pitch of 35 μm or less, and is widely used to manufacture flexible metal foil laminates for COF (chip on film). Recently, polyimide films used in flexible metal foil laminates produced by a metallizing method or the like have a problem in that the flatness decreases and wrinkles occur after metal foil is laminated. Therefore, there is a strong demand for a polyimide film that maintains its flatness even after lamination with a metal foil. The matters described in the above background art are intended to aid in understanding the background of the invention, and may include matters that are not prior art already known to a person having ordinary skill in the field to which the art pertains. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Korean Patent No. 10-1375276 [Patent Document 2] Korean Patent Publication No. 2016-0002402 Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, an object of the present invention is to provide a polyimide film that maintains its flatness and does not develop wrinkles even after a metal foil is coated, sputtered, or evaporated onto the polyimide film. However, the problems to be solved by the present invention are not limited to those described above, and other problems not described above will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0006] In order to achieve the above object, one aspect of the present invention provides a polyimide film which satisfies the following formula (1) in dimensional change measurement by a thermomechanical analyzer (TMA) while undergoing a heating process from 25°C to 400°C and then a cooling process from 400°C to 25°C: Formula (1) Dimension measurement in TD direction (cooling, 50℃) - Dimension measurement in TD direction (heating, 50℃) < 0μm In the above formula 1, The dimension measurement in the TD direction (cooling, 50°C) is the dimension measurement in the TD direction measured at 50°C during the cooling process. The dimension measurement in the TD direction (heating, 50° C.) is the dimension measurement in the TD direction measured at 50° C. at the beginning of the heating process.
[0007] Another aspect of the present invention provides a method for producing the polyimide film, the method including the steps of: providing a polyamic acid solution obtained from a dianhydride acid component and a diamine component; casting and applying the polyamic acid solution onto a support and heating to produce a self-supporting film of the polyamic acid solution; and imidizing the self-supporting film and stretching it to produce a polyimide film.
[0008] Another aspect of the present invention provides a flexible metal foil laminate comprising the above-described polyimide film and an electrically conductive metal foil.
[0009] Another aspect of the present invention provides an electronic component comprising the flexible metal foil laminate described above. Effect of the Invention
[0010] The present invention provides a polyimide film having a specific range of dimensional change, thereby providing a polyimide film that has excellent flatness even after lamination of a metal foil. Such a polyimide film is applicable to various fields where a polyimide film with excellent flatness is required, for example, flexible metal foil laminates produced by a metallizing method, or electronic parts including such flexible metal foil laminates. [Brief description of the drawings]
[0011] [Figure 1] 1 is a graph showing the results of dimensional change measurement using a thermomechanical analyzer (TMA) for films of Examples 1 and 2 of the present application, which are subjected to a heating process from 25° C. to 400° C. and then a cooling process from 400° C. to 25° C. [Diagram 2] 1 is a graph showing the results of dimensional change measurement using a thermomechanical analyzer (TMA) for films of Comparative Examples 1 to 3 of the present application, which are subjected to a temperature increase process from 25° C. to 400° C. and then a cooling process from 400° C. to 25° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The terms or words used in this specification and the claims should not be interpreted limited to their ordinary and dictionary meanings, but should be interpreted in a meaning and concept that is consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention. Therefore, the configuration of the embodiment described in this specification is one of the most preferred embodiments of the present invention. It should be understood that the above are merely embodiments and do not represent the entire technical idea of the present invention, and that there may be various equivalents and modifications that can replace these at the time of filing this application.
[0013] In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.
[0014] As used herein, "dianhydride acid" is intended to include precursors or derivatives thereof which may not technically be dianhydrides but which nevertheless react with diamines to form polyamic acids which can be converted back to polyimides.
[0015] As used herein, "diamine" is intended to include precursors or derivatives thereof which may not technically be diamines, but which nevertheless react with dianhydrides to form polyamic acids which can be converted back to polyimides.
[0016] Whenever an amount, concentration, or other value or parameter is given herein as a range, a preferred range, or a list of an upper preferred value and a preferred lower value, this is to be understood as specifically disclosing all ranges formed by any pair of upper range limits or preferred values and any lower range limits or preferred values, regardless of whether a range is otherwise disclosed. Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range.
[0017] The polyimide film according to one embodiment of the present invention satisfies the following formula (1) in dimensional change measurement by a thermomechanical analyzer (TMA) when undergoing a heating process from 25°C to 400°C and a subsequent cooling process from 400°C to 25°C. Formula (1) Dimensional measurement in TD direction (width direction of film, perpendicular to MD direction) (cooling, 50℃) - Dimensional measurement in TD direction (heating, 50℃) < 0μm In the above formula 1, The dimension measurement in the TD direction (cooling, 50°C) is the dimension measurement in the TD direction measured at 50°C during the cooling process. The dimension measurement in the TD direction (heating, 50° C.) is the dimension measurement in the TD direction measured at 50° C. at the beginning of the heating process.
[0018] That is, as shown in the above formula (1), the polyimide film of the present invention has a negative value obtained by subtracting the measured dimension in the TD direction (heating, 50° C.) from the measured dimension in the TD direction (cooling, 50° C.). Such a negative calculated value is due to the fact that the polyimide film shrinks in the TD direction during the cooling process after heating.
[0019] Preferably, the value of the polyimide film of the present invention calculated by the formula (1) is −5 μm or less, more preferably, the value according to the formula (1) is −10 μm or less, and even more preferably, the value according to the formula (1) is −20 μm or less.
[0020] The polyimide film having a negative value calculated by the above formula (1) maintained its flatness even after lamination of a metal foil by coating, sputtering or vapor deposition, and hardly any wrinkles were generated.
[0021] When the value calculated by the above formula (1) is 0 or more, the polyimide film has a reduced flatness and many wrinkles after lamination of a metal foil by coating, sputtering or vapor deposition. Such a calculated value of 0 or more is due to the fact that the polyimide film expands in the TD direction during the cooling process after heating.
[0022] Here, the measurement of dimensional change by the thermomechanical analyzer (TMA) was carried out under the following conditions. Measurement mode: tension mode, load 5g, Sample length: 15mm, Sample width: 4mm, Heating start temperature: 25℃, End temperature of heating: 400℃ (no maintenance time at 400℃) Cooling end temperature: 25℃, High temperature and cooling rate: 10℃ / min, Measurement atmosphere: nitrogen.
[0023] The polyimide film of the present invention may have a thermal expansion coefficient (CTE) in the MD direction (continuous film-forming direction; longitudinal direction of the film, perpendicular to the TD direction) of 2 to 6.5 ppm / °C, and a thermal expansion coefficient in the TD direction of 1 to 6 ppm / °C.
[0024] In addition, the value obtained by subtracting the thermal expansion coefficient in the TD direction from the thermal expansion coefficient in the MD direction may be 0 or more and 2.5 ppm / ° C. or less.
[0025] In addition, the polyimide film may have an elastic modulus of 5 GPa or more and 11 GPa or less, and a glass transition temperature of 360°C or more and 400°C or less.
[0026] On the other hand, the polyimide film of the present invention is not limited to pyromellitic dianhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), diphenylsulfone-3,4,3',4'-tetracarboxylic dianhydride (DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenyl one or more dianhydride acid components selected from the group consisting of benzene bis(trimellitic acid monoester anhydride), p-biphenylene bis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 2,3,6,7-naphthalene tetracarboxylic acid dianhydride, 1,4,5,8-naphthalene tetracarboxylic acid dianhydride, and 4,4'-(2,2-hexafluoroisopropylidene)diphthalic dianhydride; Paraphenylenediamine (PPD), metaphenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (DABA), 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'- Diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl)sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3 ,4'-Diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminodiphenylmethane) 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(3-aminophenoxy)benzene (TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenylsulfide)benzene, 1,3-bis(4-aminophenylsulfide)benzene, 1,4-bis(4-aminophenylsulfide) 1,3-bis(3-aminophenylsulfone)benzene, 1,3-bis(4-aminophenylsulfone)benzene, 1,4-bis(4-aminophenylsulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[3-(3-aminophenoxy)phenyl]ketone, bis[3-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[3-(3- aminophenoxy)phenyl]sulfide, bis[3-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-, (4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl] The diamine components are obtained by reacting one or more diamine components selected from the group consisting of 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.
[0027] The polyimide film is preferably obtained by imidization reaction of a polyamic acid solution containing a dianhydride acid component including one or more of 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) and pyromellitic dianhydride (PMDA) and a diamine component including one or more of paraphenylenediamine (PPD) and 4,4'-diaminodiphenyl ether (ODA).
[0028] In addition, the content of the 3,3',4,4'-biphenyltetracarboxylic dianhydride is 40 mol% or more and 60 mol% or less, and the content of the pyromellitic dianhydride is 40 mol% or more and 60 mol% or less, relative to the total content of the dianhydride acid components (100 mol%), With respect to 100 mol% of the total content of the diamine components, the content of the paraphenylenediamine may be 80 mol% or more and 90 mol% or less, and the content of the 4,4'-diaminodiphenyl ether may be 10 mol% or more and 20 mol% or less.
[0029] The polyamic acid of the present invention can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize the mixture; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the amount of the dianhydride component to polymerize the mixture; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and the remaining dianhydride component is added continuously thereto, thereby polymerizing the diamine component and the dianhydride component so that the molar amounts of the diamine component and the dianhydride component are substantially equal; (4) A method in which a dianhydride component is placed in a solvent, a portion of the diamine compound is mixed with the reactive components in a ratio of 95 to 105 mol %, and then another dianhydride component is added, and the remaining diamine component is added, thereby polymerizing the diamine component and the dianhydride component so that the molar amounts of the diamine component and the dianhydride component are substantially equal; (5) A method of reacting some diamine components and some dianhydride acid components in a solvent so that one of them is in an excess amount to form a first composition, reacting some diamine components and some dianhydride acid components in another solvent so that one of them is in an excess amount to form a second composition, and then mixing the first composition and the second composition to complete polymerization, in which if the diamine component is in excess when the first composition is formed, the second composition contains an excess of dianhydride acid component, and if the dianhydride acid component is in excess in the first composition, the second composition contains an excess of diamine component, and the first composition and the second composition are mixed to polymerize so that the total amount of diamine components and dianhydride acid components used in these reactions are substantially equimolar.
[0030] In one embodiment, a method for producing a polyimide film according to the present invention includes the steps of: providing a polyamic acid solution derived from a dianhydride acid component and a diamine component; casting the polyamic acid solution onto a support and heating it to produce a self-supporting film of the polyamic acid solution; and imidizing the self-supporting film and stretching it to produce a polyimide film.
[0031] The stretching is biaxial stretching, and tension is applied so that the stretching ratios in the MD and TD directions are equal. The stretching ratio can be determined by the balance between the MD and TD directions of the polyimide film through the TMA measurement. That is, the balance between the MD and TD directions of the polyimide film obtained through stretching indicates that the value obtained by subtracting the thermal expansion coefficient in the TD direction from the thermal expansion coefficient in the MD direction is 0 or more and 2.5 ppm / °C or less.
[0032] In the present invention, the above-mentioned polymerization method of polyamic acid can be defined as a random polymerization method, and a polyimide film prepared from the polyamic acid of the present invention prepared by the above-mentioned process can be preferably applied from the viewpoint of maximizing the effect of the present invention of improving flatness. However, the polymerization method produces a polymer chain having a relatively short repeating unit length, so that there may be a limit to the excellent properties of the polyimide chain derived from the dianhydride acid component. Therefore, the polymerization method of polyamic acid preferably used in the present invention may be a block polymerization method.
[0033] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited, and any solvent that dissolves the polyamic acid can be used, but an amide-based solvent is preferable. Specifically, the organic solvent may be an organic polar solvent, specifically, an aprotic polar solvent, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more as necessary. In one example, the organic solvent is preferably N,N-dimethylformamide or N,N-dimethylacetamide.
[0034] In addition, in the polyamic acid production process, fillers can be added to improve various properties of the film, such as sliding properties, thermal conductivity, COVID-19 resistance, Knoop hardness, etc. The fillers to be added are not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc. The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm. If the particle size is below this range, the modifying effect is unlikely to be achieved, whereas if it exceeds this range, the surface properties may be significantly impaired or the mechanical properties may be significantly reduced.
[0035] The amount of the filler to be added is not particularly limited, and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.01 to 90 parts by weight, based on 100 parts by weight of polyimide. The amount is preferably 0.02 to 80 parts by weight. If the amount of the filler added is less than this range, the modifying effect of the filler is unlikely to be exhibited, and if the amount exceeds this range, the mechanical properties of the film may be significantly impaired. The method of adding the filler is not particularly limited, and any known method may be used.
[0036] In the production method of the present invention, the polyimide film can be produced by a thermal imidization method or a chemical imidization method. It can also be produced by a hybrid imidization method in which thermal imidization and chemical imidization are carried out in parallel.
[0037] The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared dryer. The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600°C, specifically, by heat-treating the gel film at 200 to 500°C, more specifically, by heat-treating the gel film at 300 to 500°C, to imidize the amic acid groups present in the gel film. However, even during the process of forming the gel film, a portion of the amic acid (approximately 0.1 mol % to 10 mol %) may be imidized, and for this reason, the polyamic acid composition may be dried at a variable temperature in the range of 50°C to 200°C, which can also be included in the category of the thermal imidization method.
[0038] In the case of chemical imidization, a polyimide film can be produced using a dehydrating agent and an imidization agent according to methods known in the art.
[0039] As an example of the composite imidization method, a dehydrating agent and an imidization agent are added to a polyamic acid solution, which is then heated at 80 to 200°C, preferably 100 to 180°C, partially cured and dried, and then heated at 200 to 400°C for 5 to 400 seconds to produce a polyimide film.
[0040] The present invention provides a flexible metal foil laminate comprising the above-mentioned polyimide film and an electrically conductive metal foil. The metal foil to be used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment applications, the metal foil may be, for example, copper or a copper alloy, stainless steel or its alloy, nickel or a nickel alloy (including alloy 42), aluminum or an aluminum alloy.
[0041] In general flexible metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and can be preferably used in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer.
[0042] In the present invention, the thickness of the metal foil is not particularly limited, and may be any thickness that allows the metal foil to exhibit sufficient function depending on the application.
[0043] The flexible metal foil laminate according to the present invention can be obtained by laminating, coating, sputtering or vapor-depositing a metal foil on at least one surface of the polyimide film.
[0044] In addition, the flexible metal foil laminate can be used as a 2-layer FCCL, particularly for mobile phones, displays (LCD, PDP, OLED, etc.), and can be used for FPCB and COF.
[0045] The electronic component including the flexible metal foil laminate may be, for example, but not limited to, a communication circuit for a mobile terminal, a communication circuit for a computer, or a communication circuit for aerospace applications. EXAMPLES
[0046] The action and effect of the present invention will be described in more detail below with reference to specific manufacturing examples and examples of the present invention. However, these manufacturing examples and examples are presented only as examples of the present invention and do not limit the scope of the present invention.
[0047] Manufacturing example: Manufacturing of polyimide film The polyimide film of the present invention can be produced by the following conventional method known in the art: First, the above-mentioned dianhydride acid and diamine component are reacted in an organic solvent to obtain a polyamic acid solution. In this case, the solvent is generally an amide-based solvent, and an aprotic polar solvent, such as N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methyl-pyrrolidone, or a combination thereof, can be used.
[0048] The dianhydride and diamine components may be added in the form of powder, lump, or solution. It is preferable to add them in the form of powder at the beginning of the reaction and then add them in the form of a solution to control the polymerization viscosity.
[0049] The resulting polyamic acid solution can be mixed with an imidization catalyst and a dehydrating agent and applied to a substrate.
[0050] Examples of the catalyst used include tertiary amines (e.g., isoquinoline, β-picoline, pyridine, etc.), and examples of the dehydrating agent include, but are not limited to, anhydrous acids. In addition, examples of the support used above include, but are not limited to, glass plates, aluminum foils, circular stainless steel belts, stainless steel drums, etc.
[0051] The film coated on the support is gelled on the support by dry air and heat treatment. The gelled film is separated from the support and heat treated to complete the drying and imidization. The heat-treated film is then heat-treated under a certain tension to remove residual stress inside the film that may have been generated during the film-forming process.
[0052] Specifically, 500ml of DMF was added while injecting nitrogen into a reactor equipped with a stirrer and nitrogen inlet / outlet pipes, and the temperature of the reactor was set to 30°C, and then biphenyltetracarboxylic dianhydride (50mol%), pyromellitic dianhydride (50mol%), paraphenylenediamine (13mol%), and 4,4'-diaminodiphenyl ether (87mol%) were added in a controlled composition ratio and in a specified order to completely dissolve.Then, the temperature of the reactor was raised to 40°C under a nitrogen atmosphere, and stirring was continued for 120 minutes to produce polyamic acid with a primary reaction viscosity of 1,500cP.
[0053] The polyamic acid thus produced was stirred so as to have a final viscosity of 100,000 to 120,000 cP. The catalyst and dehydrating agent were added to the prepared final polyamic acid with the adjusted contents, and then a polyimide film was produced using an applicator.
[0054] Examples and Comparative Examples The polyimide films were prepared according to the above Preparation Examples, except that the stretching degree of each of the Examples and Comparative Examples was adjusted as shown in Table 1 below. That is, when the stretching degree of Example 1 was taken as 100%, the stretching degree of Example 2 was 120%, and the stretching degrees of Comparative Examples 1 to 3 were 150%, 140% and 70%, respectively.
[0055] [Table 1]
[0056] The coefficient of thermal expansion (CTE), glass transition temperature, elastic modulus, and flatness after lamination with metal foil of the prepared polyimide film were measured. In addition, a metal layer was formed on the prepared polyimide film by sputtering, and the film flatness (wrinkle formation) after coating was confirmed.
[0057] (1) Measurement of dimensional change The dimensional change was measured by a thermomechanical analyzer (TMA) during the heating process from 25°C to 400°C and the subsequent cooling process from 400°C to 25°C.
[0058] (2) Measurement of thermal expansion coefficient The coefficient of thermal expansion (CTE) was measured using a TA thermomechanical analyzer, model Q400. The polyimide film was cut to a width of 4 mm and a length of 20 mm, and then heated from room temperature to 400°C at a rate of 10°C / min while applying a tension of 0.05 N under a nitrogen atmosphere. Then, the temperature was increased to 400°C at a rate of 10°C / min, and the temperature was cooled again at a rate of 10°C / min to measure the slope in the range from 50°C to 200°C.
[0059] (3) Film Flatness Measurement Wrinkles in the MD direction of the produced polyimide film were confirmed by visual inspection.
[0060] (4) Measurement of glass transition temperature Glass transition temperature (T g ) measured the loss modulus and storage modulus of each film using DMA, and determined the inflection point in the tangent graph of these values as the glass transition temperature.
[0061] (5) Measurement of elastic modulus The elastic modulus of the polyimide film was measured according to the standard of ASTM D882.
[0062] Graphs showing the measurement results of dimensional changes in Examples 1 and 2 are shown in Figures 1a and 1b, respectively. Graphs showing the measurement results of dimensional changes in Comparative Examples 1 to 3 are shown in Figures 2a, 2b, and 2c, respectively. As shown in Fig. 1, the values calculated by formula (1) in Examples 1 and 2 were negative numbers, and as shown in Fig. 2, the values calculated by formula (1) in Comparative Examples 1 to 3 were positive numbers.
[0063] Examples where the film flatness after coating was measured and the calculated value according to formula (1) was a negative number The polyimide films of No. 1 and No. 2 had extremely excellent film flatness (no or almost no wrinkles were formed) compared to the polyimide films of Comparative Examples 1 to 3, which had positive values calculated by formula (1).
[0064] The examples of the polyimide film and the method for manufacturing the polyimide film of the present invention are merely preferred examples that enable a person having ordinary skill in the art to easily carry out the present invention, and the present invention is not limited to the above-mentioned examples, and therefore the scope of the present invention is not limited. Therefore, the true technical scope of the present invention should be determined by the technical ideas of the appended claims. In addition, it is obvious to a person skilled in the art that various substitutions, modifications and changes are possible within the scope of the present invention, and it is self-evident that the parts that can be easily modified by a person skilled in the art are also included in the scope of the present invention. [Industrial Applicability]
[0065] The present invention provides a polyimide film having a specific range of dimensional change, thereby providing a polyimide film that has excellent flatness even after lamination of a metal foil. Such a polyimide film is applicable to various fields where a polyimide film with excellent flatness is required, for example, flexible metal foil laminates produced by a metallizing method or electronic parts including such flexible metal foil laminates.
Claims
1. A polyimide film that satisfies the following formula (1) in a dimensional change measurement by a thermomechanical analyzer (TMA) during a heating process from 25° C. to 400° C. and a cooling process from 400° C. to 25° C., The polyimide film has a stretch degree in the range of 100% to 120%; The stretching is biaxial stretching in which the stretch ratios in the MD and TD directions of the polyimide film are equal; and The value of the formula (1) is −32 when the stretching degree is 100%, and −20 when the stretching degree is 120%. Formula (1) -32 μm≦Measured dimension in TD direction (cooling, 50° C.) -Measured dimension in TD direction (heating, 50° C.) ≦-20 μm (In the above formula 1, TD dimension measurement (cooling, 50° C.) is the TD dimension measurement taken at 50° C. during the cooling process; The measured dimension in the TD direction (heating, 50°C) is the measured dimension in the TD direction measured at 50°C during the heating process.
2. 2. The polyimide film according to claim 1, which has a thermal expansion coefficient in the MD direction of 2 to 6.5 ppm / °C and a thermal expansion coefficient in the TD direction of 1 to 6 ppm / °C.
3. 3. The polyimide film according to claim 2, wherein a value obtained by subtracting the thermal expansion coefficient in the TD direction from the thermal expansion coefficient in the MD direction is 0 or more and 2.5 ppm / °C or less.
4. The elastic modulus is 5 GPa or more and 11 GPa or less, 2. The polyimide film according to claim 1, having a glass transition temperature of 360° C. or more and 400° C. or less.
5. Pyromellitic dianhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), diphenylsulfone-3,4,3',4'-tetracarboxylic dianhydride (DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylenebis(trimethylsilyl) one or more dianhydride acid components selected from the group consisting of m-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, and 4,4'-(2,2-hexafluoroisopropylidene)diphthalic dianhydride; Paraphenylenediamine (PPD), metaphenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (DABA), 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'- Diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl)sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3 ,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenyl methane, 3,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl methane, 2,2-bis(3-aminodiphenyl aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(3-aminophenoxy)benzene (TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenylsulfonyl), 1,3-bis(4-aminophenylsulfide)benzene, 1,4-bis(4-aminophenylsulfide)benzene, 1,3-bis(3-aminophenylsulfone)benzene, 1,3-bis(4-aminophenylsulfone)benzene, 1,4-bis(4-aminophenylsulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'- Bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[3-(3-aminophenoxy)phenyl]ketone, bis[3-(4-aminophenoxy)phenyl] bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[3-(3-aminophenoxy)phenyl]sulfide, bis[3-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-amino 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane,The polyimide film according to claim 1, obtained by imidizing and reacting one or more diamine components selected from the group consisting of 2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.
6. a dianhydride acid component including at least one of 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) and pyromellitic dianhydride (PMDA); 2. The polyimide film according to claim 1, obtained by imidizing a polyamic acid solution containing a diamine component including at least one of paraphenylenediamine (PPD) and 4,4'-diaminodiphenyl ether (ODA).
7. The content of the 3,3',4,4'-biphenyltetracarboxylic dianhydride is 40 mol% or more and 60 mol% or less, and the content of the pyromellitic dianhydride is 40 mol% or more and 60 mol% or less, relative to 100 mol% of the total content of the dianhydride acid components; 7. The polyimide film according to claim 6, wherein the content of the paraphenylenediamine is 80 mol% or more and 90 mol% or less, and the content of the 4,4'-diaminodiphenyl ether is 10 mol% or more and 20 mol% or less, relative to 100 mol% of the total content of the diamine components.
8. A method for producing the polyimide film according to any one of claims 1 to 7, comprising the steps of: providing a polyamic acid solution derived from a dianhydride acid component and a diamine component; The polyamic acid solution is cast onto a support and heated to self-heat the polyamic acid solution. Producing a support film; and imidizing the self-supporting film and stretching the film to produce a polyimide film.
9. A flexible metal foil laminate comprising the polyimide film according to any one of claims 1 to 7 and an electrically conductive metal foil.
10. 10. The flexible metal foil laminate of claim 9, wherein the metal foil is formed by coating, sputtering or vapor deposition.
11. An electronic component comprising the flexible metal foil laminate of claim 10.
Citation Information
Patent Citations
Method for manufacturing adhesive sheet, adhesive sheet and flexible metal clad laminated plate made by using the same
JP2005186574A
Polyimide film
JP2014012827A
Polyimide film and method for producing the same
JP2020152765A
Method for manufacturing laminated plate using thermoplastic polyimide adhesive film with improved slip properties
KR101375276B1
KR2016-0002402