Silica-supported calcium phosphate crystals
By using silicate as an inorganic source to produce calcium phosphate crystals with partial silicate ion replacement, the method addresses the challenge of organic residue in bone replacement materials, facilitating easy production and phase transitions for effective bone remodeling.
Patent Information
- Application Number
- JP2020191183
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-17
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-11-17
AI Technical Summary
Existing methods for producing bone replacement materials using organic silica sources face challenges due to the presence of residual organic molecules that hinder commercialization, and there is a need for an inorganic silica source that can be easily integrated into calcium phosphate crystals for bone remodeling applications.
The production of calcium phosphate crystals is achieved using silicate as an inorganic silica source, allowing for the partial replacement of hydroxide or halide ions with silicate ions, and the crystals can be further processed into powders, blocks, or porous bodies by hydrolyzing easily soluble calcium phosphate in an aqueous silicate solution and immersing the resulting crystals in specific solutions.
This method enables the easy production of silicic acid-containing calcium phosphate crystals, which can undergo phase transitions without solution precipitation, supporting bone remodeling and providing a stable inorganic silica source for bone replacement materials.
Smart Images

Figure 0007562137000001 
Figure 0007562137000002 
Figure 0007562137000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a silica-supported calcium phosphate crystal, more particularly to a calcium phosphate crystal that contains calcium ions and phosphate ions and may further contain hydroxide ions and / or halide ions, in which at least one of the calcium ions, phosphate ions, hydroxide ions, and halide ions contained in the crystal structure is partially substituted with silicate ions. [Background technology]
[0002] The bone remodeling process, which is bone metabolism, controls the rate of bone replacement by bone substitutes. Osteocytes and immune cells play essential and central roles in the bone remodeling process. By controlling these cells, the bone remodeling process can be controlled (e.g., Non-Patent Document 1).
[0003] Silicate ions are known to enhance osteoblast activity and increase bone production (Non-Patent Document 2, Patent Document 3). ORTHOREBIRTH Co., Ltd. sells a cotton-shaped artificial bone filler called ReBOSSIS as a commercially available product. This product is characterized by its cotton-shaped form and its main ingredients being β-TCP (β-tricalcium phosphate), bioabsorbable polymer, and SiV (silicon-containing calcium carbonate), which promotes bone formation.
[0004] When silica is supported on calcium phosphate or calcium carbonate, organic silica is usually used as the silica source (Non-Patent Document 4). However, the organic molecules that remain after the hydrolysis of organic silica are a major concern in commercialization. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] BMC Med.,9, 66-75 (2011) [Non-Patent Document 2] Acta Biomater., 5, 57-62 (2008) [Non-Patent Document 3] Mater. Sci. Eng.: C, 42, 672-680 (2014) [Non-Patent Document 4] J. Mater. Chem. B, 2, 1250 (2014) Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a technique for simply producing a material useful for bone filling using an inorganic silica source. [Means for solving the problem]
[0007] The present inventors have found that silica-supported calcium phosphate crystals can be easily produced by using a silicate as an inorganic silica source, and have completed the present invention. The present invention is as follows.
[0008] [1] A calcium phosphate crystal containing calcium ions and phosphate ions and optionally containing hydroxide ions and / or halide ions, wherein at least one of the calcium ions, phosphate ions, hydroxide ions, and halide ions contained in the crystal structure is partially substituted with silicate ions. [2] The crystal described in [1], wherein the calcium phosphate is octacalcium phosphate. [3] The crystal described in [2], wherein the hydration layer constituting the crystal structure of the octacalcium phosphate contains silicate ions. [4] The crystal according to [1], which contains an apatite phase. [5] The crystal according to [4], wherein the apatite phase does not contain carbonate. [6] The crystal described in [4], wherein the apatite phase contains carbonate. [7] A powdery composition comprising the crystal according to any one of [1] to [6]. [8] A block material comprising the crystal according to any one of [1] to [6]. [9] A porous body comprising the crystal according to any one of [1] to [6].
[0009]
[10] A method for producing crystalline silicic acid-containing calcium phosphate, comprising a step of hydrolyzing a ceramic containing at least one of calcium and phosphate in an aqueous solution containing a silicate.
[11] The method according to
[10] , wherein the ceramic is a readily soluble calcium phosphate.
[12] The method according to
[10] or
[11] , wherein the calcium phosphate obtained by the hydrolysis step is octacalcium phosphate.
[13] The method according to
[11] or
[12] , wherein the readily soluble calcium phosphate is calcium hydrogen phosphate dihydrate, calcium hydrogen phosphate, calcium dihydrogen phosphate hydrate, calcium dihydrogen phosphate anhydrate, tricalcium phosphate α-phase, or tricalcium phosphate β-phase.
[0010]
[14] A step of hydrolyzing a readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; and further processing the obtained siliceous calcium phosphate crystals, A method for producing crystalline silicic acid-containing calcium phosphate.
[15] The further treating step includes immersing the siliceous calcium phosphate in a solution; The siliceous calcium phosphate crystal is a siliceous calcium phosphate crystal containing an apatite phase. The manufacturing method described in
[14] .
[16] The manufacturing method described in
[15] , wherein the solution does not contain carbonate and the apatite phase does not contain carbonate.
[17] The manufacturing method described in
[15] , wherein the solution contains carbon dioxide and the apatite phase contains carbon dioxide.
[0011]
[18] A step of hydrolyzing a readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; Obtaining a powdered composition containing the silicic acid-containing calcium phosphate crystals obtained; and immersing the obtained powder composition in a solution; A method for producing a powdered composition of siliceous apatite.
[19] A step of hydrolyzing a readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; Obtaining a block material containing the obtained silicic acid-containing calcium phosphate crystals; and The process includes immersing the obtained block material in a solution. A method for producing a block material of siliceous apatite.
[20] A step of hydrolyzing a readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; Obtaining a porous body containing the silicic acid-containing calcium phosphate crystals obtained; and immersing the obtained porous body in a solution; A method for producing a porous body of silicic acid-containing apatite. Effect of the Invention
[0012] According to the present invention, it is possible to easily produce a material useful for bone filling using an inorganic silica source. In particular, if octacalcium phosphate can be loaded with silicic acid, it is expected that other calcium phosphates can also be loaded with silicic acid, since octacalcium phosphate is a precursor of other calcium phosphates and undergoes phase transition to other calcium phosphates without undergoing dissolution-precipitation reactions. [Brief description of the drawings]
[0013] [Figure 1] 1 is a graph showing the results (XRD pattern) of Example 1 according to one embodiment of the present invention. [Diagram 2] 1 is a graph showing the results (silicon content) of Example 1 according to one embodiment of the present invention. [Diagram 3]1 is a graph showing the results (FT-IR) of Example 1 according to one embodiment of the present invention. [Figure 4] 1 is a graph showing the results (NMR spectrum) of Example 1 according to one embodiment of the present invention. [Diagram 5] 1 is a photograph (a drawing substitute photograph) showing the results (SEM image) of Example 1 according to one aspect of the present invention. [Figure 6] 3 is a graph showing the results (XRD pattern) of Example 2 according to one embodiment of the present invention. [Figure 7] 3 is a graph showing the results (FT-IR) of Example 2 according to one embodiment of the present invention. [Figure 8] 4 is a graph showing the results (silicon content) of Example 2 according to one embodiment of the present invention. [Figure 9] 3 is a graph showing the results (XRD pattern) of Example 3 according to one embodiment of the present invention. [Figure 10] 1 is a photograph (a drawing substitute photograph) showing the results (SEM image) of Example 3 according to one embodiment of the present invention. [Figure 11] 3 is a graph showing the results (XRD pattern) of Example 4 according to one embodiment of the present invention. [Figure 12] 1 is a photograph (a drawing substitute photograph) showing the results (SEM image) of Example 4 according to one embodiment of the present invention. [Figure 13] 1 is a photograph (drawing substitute photograph) showing the results (shape of a sample) of Example 5 according to one embodiment of the present invention. [Figure 14] 3 is a graph showing the results (XRD pattern) of Example 5 according to one embodiment of the present invention. [Figure 15] 1 is a graph showing the results (FT-IR) of Example 5 according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] One aspect of the present invention is The present invention relates to a method for producing silicic acid-containing calcium phosphate crystals (preferably octacalcium phosphate crystals), the method comprising the step of hydrolyzing a ceramic containing at least one of calcium and phosphoric acid, preferably a readily soluble calcium phosphate, in an aqueous solution containing a silicate, such as silicate ions or silicic acid colloid, that produces silicate ions capable of reacting with the ceramic via the solution.
[0015] The readily soluble calcium phosphate is preferably calcium hydrogen phosphate dihydrate, calcium hydrogen phosphate anhydrate, calcium dihydrogen phosphate hydrate, calcium dihydrogen phosphate anhydrate, tricalcium phosphate α-phase, tricalcium phosphate β-phase, tetracalcium phosphate (TTCP), or amorphous calcium phosphate (ACP).
[0016] Examples of the silicate include water glass (Na2SiO3), potassium silicate, cesium silicate, and ammonium hexafluorosilicate. Among these, water glass is preferred because the counter cation, sodium ion, induces the formation of octacalcium phosphate (Ca8(HPO4)2(PO4)4·5H2O; OCP). In addition, water glass is preferred because it is basic and therefore compatible with conventional OCP preparation methods.
[0017] The conditions for hydrolyzing the readily soluble calcium phosphate in the silicate solution or the aqueous solution containing colloidal particles include the following.
[0018] The concentration of the silicate in the silicate solution or the aqueous solution containing colloidal particles is preferably 0.001 mol / L or more, more preferably 0.01 mol / L or more, and even more preferably It is preferably 0.1 mol / L or more, while it is preferably 10.0 mol / L or less, more preferably 5.0 mol / L or less, and even more preferably 2.0 mol / L or less.
[0019] The content of the readily soluble calcium phosphate in the aqueous solution containing the silicate is not particularly limited, and may be appropriately set depending on the phase of the readily soluble calcium phosphate used and the composition of the solution.
[0020] The reaction temperature during the hydrolysis is preferably 0°C or higher, more preferably 4°C or higher, and even more preferably 25°C or higher, while it is preferably 99°C or lower, more preferably 90°C or lower, and even more preferably 80°C or lower.
[0021] The reaction time during the hydrolysis is preferably 10 minutes or more, more preferably 30 minutes or more, and even more preferably 1 hour or more, while it is preferably 14 days or less, more preferably 7 days or less, and even more preferably 5 days or less.
[0022] The pH during the hydrolysis is not particularly limited, but may be set so that silicic acid ions or colloidal silicic acid are stably dispersed in the solution.
[0023] This embodiment may include a step of washing the obtained silicic acid-containing calcium phosphate crystals and a step of drying them thereafter. The washing step may include washing the obtained silicic acid-containing calcium phosphate crystals with, for example, distilled water, and may be performed according to a conventional method. The drying step may include drying the obtained silicic acid-containing calcium phosphate crystals with, for example, a dryer, after the washing step.
[0024] Another aspect of the present invention is A step of hydrolyzing the readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; further processing the obtained siliceous calcium phosphate crystals, A method for producing crystalline siliceous calcium phosphate (preferably crystalline octacalcium phosphate).
[0025] The above-mentioned embodiment is applied to the step of obtaining the silicic acid-containing calcium phosphate crystals.
[0026] By further treating the obtained crystalline silicic acid-containing calcium phosphate, crystalline silicic acid-containing calcium phosphate can be produced. For example, the step of further treating the obtained silicic acid-containing calcium phosphate crystals includes a step of immersing the silicic acid-containing calcium phosphate crystals in a solution, whereby silicic acid-containing calcium phosphate crystals containing an apatite phase can be produced as the silicic acid-containing calcium phosphate crystals.
[0027] The end of the reaction here refers to a state in which a thermodynamically stable phase is completely formed, there is no further change in the composition of the solution, the temperature, or the pressure, and no new reaction occurs macroscopically.
[0028] The composition of the solvent other than water contained in the aqueous solution is not particularly limited, but the solvent may be any solvent that can be mixed with water in any ratio or that can be uniformly dispersed in a colloidal state.
[0029] Examples of the solvent include primary alcohols such as methanol, ethanol, propan-1-ol, butan-1-ol, pentan-1-ol, hexane-1-ol, heptan-1-ol, octan-1-ol, nonan-1-ol, and decan-1-ol, 2-propanol (isopropyl alcohol), butan-2-ol, and pentan-2-ol. , secondary alcohols such as hexane-2-ol and cyclohexanol, tertiary alcohols such as tert-butyl alcohol, 2-methylbutan-2-ol, 2-methylpentan-2-ol, 2-methylhexane-2-ol, 3-methylpentan-3-ol, and 3-methyloctan-3-ol, monohydric alcohols such as ethylene glycol and diethylene glycol, trihydric alcohols such as glycerin, aromatic ring alcohols such as phenol, polyethers such as polyethylene glycol (PEG) and polypropylene glycol (PPG), polycarboxylic acids such as polyacrylic acid and polycarbalic acid, fatty acids such as acetic acid, valeric acid, caproic acid, lauric acid, palmitic acid, stearic acid, oleic acid, and linoleic acid, alkanes such as pentane, butane, hexane, septane, and octane, ethers such as dimethyl ether, methyl ethyl ether, and diethyl ether, aromatic compounds such as benzene, toluene, picric acid, and TNT, naphthalene, azulene, anthracene, and tetrahydrofuran. helical hydrocarbons, organic halogen compounds such as chloromethane, dichloromethane, chloroform, and carbon tetrachloride, esters such as ethyl acetate, methyl butyrate, methyl salicylate, ethyl formate, ethyl butyrate, ethyl caproate, octyl acetate, dibutyl phthalate, ethylene carbonate, and ethylene sulfide, cycloalkanes such as cyclopentane, cyclohexane, and decalin, bicycloalkanes, ketones such as acetone, methyl ethyl ketone, and diethyl ketone, aldehydes such as formaldehyde, acetaldehyde, propionaldehyde, butanal, pentanal, hexanal, and vanillin, amine compounds such as aminomethane, aminoethane, ethylenediamine, triethylamine, and aniline, sugars such as glucose, fructose, and threitol, thiols such as methanethiol, ethanethiol, propanethiol, and thiophenol, and disulfide compounds such as dimethyl sulfide, diphenyl sulfide, asparagusic acid, cystamine, and cystine. These may be used alone or in combination.
[0030] The solution may or may not contain carbon dioxide, which is both preferred embodiments. When the solution contains carbon dioxide, the apatite phase contains carbon dioxide, and when the solution does not contain carbon dioxide, the apatite phase does not contain carbon dioxide.
[0031] Examples of the carbonate source in the solution include carbon dioxide gas, ammonium carbonate, sodium hydrogen carbonate, sodium carbonate, potassium hydrogen carbonate, potassium carbonate, lithium carbonate, etc. These may be used alone or in combination.
[0032] The solution may contain other ions and other molecules in addition to the above. They may be added to the solution depending on the application, since they are incorporated in small amounts into the final product, the siliceous calcium phosphate crystals containing the apatite phase. In particular, it is common to add an aqueous solution of sodium hydroxide or hydrochloric acid for pH adjustment.
[0033] The other ions to be added to the solution include salts of inorganic compounds and salts of organic compounds, and particularly salts that dissolve well and exhibit their functions when contacted with a solvent such as distilled water. The salts of inorganic compounds include not only anhydrous salts but also hydrated salts. Examples of the salts of inorganic compounds and salts of organic compounds include alkali metal salts such as sodium salts, potassium salts, lithium salts, rubidium salts, and cesium salts; alkaline earth metal salts such as magnesium salts and strontium salts; transition metal salts such as aluminum salts, zinc salts, iron salts, nickel salts, cobalt salts, and copper salts; rare earth salts such as lanthanum salts, cerium salts, yttrium salts, praseodymium salts, neodymium salts, samarium salts, europium salts, holmium salts, and dysprosium salts; inorganic salts such as ammonium salts; tris(hydroxymethyl), aminomethane salts, phenylglycine alkyl ester salts, dicyclohexylamine salts, N,N'-dibenzylethylenediamine salts, ethylenediamine salts, glucosamine salts, guanisidine salts, diethylamine salts, triethylamine salts, N-methylglucamine salts, t-octylamine salts, dibenzoyl Examples of the salts include organic amine salts such as diethanolamine salts, morpholine salts, procaine salts, diethanolamine salts, N-benzyl-N-phenethylamine salts, piperazine salts, chloroprocaine salts, and tetramethylammonium salts; and phenol salts.
[0034] The other molecules to be added to the solution include molecules having in their composition a functional group that chemically bonds with calcium, such as a carboxyl group, a silanol group, a phosphate group, a sulfo group, a hydroxyl group, or a thiol group.
[0035] Here, a molecule having a carboxyl group refers to a molecule having one or more functional groups represented by -COOH in its composition.
[0036] Molecules having a carboxyl group include substances classified as monocarboxylic acids, dicarboxylic acids, tricarboxylic acids, carboxylic acid thiols, halogenated carboxylic acids, amino acids, aromatic acids, hydroxy acids, sugar acids, nitrocarboxylic acids, polycarboxylic acids, etc., their derivatives, and polymerized substances of these. These are acetic acid, propionic acid, butyric acid, formic acid, valeric acid, succinic acid, citric acid, mercaptoundecanoic acid, thioglycolic acid, asparagusic acid, α-riboic acid, β-riboic acid, dihydroriboic acid, chloroacetic acid, malonic acid, aconitic acid, malic acid, oxalic acid, tartaric acid, malonic acid, glutaric acid, adipic acid, fumaric acid, maleic acid, oxaloacetic acid, α-ketoglutaric acid, oxalosuccinic acid, pyruvic acid, isocitric acid, α-alanine, β-alanine, arginine, asparagine, aspartic acid, cysteine, glutamine, glutamic acid, glycine, histidine, isoleucine, leucine, lysine, methionine, phenylalanine, proline, serine, threonine, tryptophan, tyrosine, valine, cysteine, hydroxyproline, o-phosphoserine, desmolysine, selenoic acid ... Examples of the acidic acid include cinnamic acid, novaline, octobin, mannovin, saccharopine, N-methylglycine, dimethylglycine, trimethylglycine, citrulline, glutathione, creatine, γ-aminobutyric acid, theanine, lactic acid, folinic acid, folic acid, pantothenic acid, benzoic acid, salicylic acid, o-phthalic acid, m-phthalic acid, p-phthalic acid, nicotinic acid, picolinic acid, gallic acid, mellitic acid, cinnamic acid, jasmonic acid, undecylenic acid, levulinic acid, iduronic acid, glucuronic acid, galacturonic acid, glyceric acid, gluconic acid, muramic acid, sialic acid, mannuronic acid, glycolic acid, glyoxylic acid, ethylenediaminetetraacetic acid (EDTA), nitroacetic acid, nitrohydrocinnamic acid, nitrobenzoic acid, polyacrylic acid, polycitric acid, polyitaconic acid, and salts thereof. These may be used alone or in combination.
[0037] Here, a molecule having a silanol group refers to a molecule having a functional group represented by -SiO4R3 in its composition, where R is H or an alkyl group.
[0038] Examples of molecules having a silanol group include γ-methacryloxypropyltrimethoxysilane (γ-MPTS), tetraethyl orthosilicate (TEOS), orthosilicic acid, metasilicic acid, metadisilicic acid, and salts thereof.
[0039] Here, a molecule having a phosphate group refers to a functional group represented by -PO4R2 in the composition, where R is H or an alkyl group.
[0040] Molecules having phosphate groups include adenosine triphosphate (ATP), adenosine diphosphate (ADP), nucleotides, glucose-6-phosphate, flavin mononucleotide, polyphosphate, 10-methacryloyloxydecyl dihydrogen phosphate (MDP), phytic acid, and salts thereof.
[0041] Here, a molecule having a sulfo group refers to a functional group represented by -SO3R in the composition. R is , H or an alkyl group.
[0042] Examples of molecules having a sulfo group include benzenesulfonic acid, taurine, sodium linear alkylbenzenesulfonate, xylene silanol, bromophenol blue, methyl orange, 4,4'-diisothiocyano-2,2'-stilbenedisulfonic acid (DIDS), azorubine, amaranth, indigo carmine, water blue, cresol red, Coomassie brilliant blue, Congo red, sulfanilic acid, tartrazine, thymol blue, tosyl azide, new coccine, pyranine, methylene blue, hydroxyethylpiperazineethanesulfonic acid (HEPES), sodium cyclamate, saccharin, taucollolic acid, isethionic acid, cysteic acid, 10-camphorsulfonic acid, 4-hydroxy-5-aminonaphthalene-2,7-disulfonic acid, methanesulfonic acid, ethanesulfonic acid, and salts thereof.
[0043] Here, a molecule having a hydroxyl group refers to a functional group represented by -OH in the composition.
[0044] Molecules having hydroxyl groups include compounds classified as alcohols, 2-hydroxyethyl methacrylate (HEMA), hydroxylamines, hydroxamic acids, phenols, compounds classified as aldols, compounds classified as sugars, compounds classified as glycols, inositol, compounds classified as sugar alcohols, pantetheine, and salts thereof.
[0045] Here, a molecule having a thiol group refers to a functional group represented by -SH in the composition, where R is H or an alkyl group.
[0046] Examples of molecules having a thiol group include captopril, methanethiol, ethanethiol, cysteine, glutathione, thiophenol, acetylcysteine, 1,2-ethanedithiol, cysteamine, dithioerythritol, dithiothreitol, dimercaprol, thioglycolic acid, tiopronin, 2-naphthalenethiol, bucillamine, furan-2-ylmethanethiol, D-penicillamine, mycothiol, mesna, 3-methyl-2-butene-1-thiol, 3-mercaptopyruvic acid, and salts thereof.
[0047] The conditions for immersing the silicic acid-containing calcium phosphate in the solution include the following.
[0048] When the solution contains carbon dioxide, the concentration of the carbonate source in the aqueous solution is preferably 0.01 mol / L or more, more preferably 0.05 mol / L or more, even more preferably 0.1 mol / L or more, while being preferably 10.0 mol / L or less, more preferably 5.0 mol / L or less, even more preferably 3.0 mol / L or less.
[0049] The concentration of the silicic acid-containing calcium phosphate in the aqueous solution is not particularly limited.
[0050] The reaction temperature during the immersion is preferably 25°C or higher, more preferably 37°C or higher, and even more preferably 50°C or higher, while it is preferably 99°C or lower, more preferably 95°C or lower, and even more preferably 90°C or lower.
[0051] The reaction time during the immersion is preferably 30 minutes or more, more preferably 1 hour or more, and even more preferably 2 hours or more, while it is preferably 14 days or less, more preferably 10 days or less, and even more preferably 7 days or less.
[0052] The pH during the immersion is not particularly limited, but is preferably 4.0 or higher, more preferably 6.0 or higher, and even more preferably 8.0 or higher.
[0053] This embodiment may include a step of washing the siliceous calcium phosphate crystals and a subsequent step of drying. The washing step may include washing the silicic acid-containing calcium phosphate crystals with, for example, distilled water, and may be performed according to a conventional method. The drying step may include drying the silicic acid-containing calcium phosphate crystals with, for example, a dryer, after the washing step.
[0054] The obtained silicic acid-containing calcium phosphate crystals can be made into the form of a powder composition, a block material, or a porous body by a conventional method. In any of the forms, the powder composition of silicic acid-containing apatite, the block material of silicic acid-containing apatite, and the porous body of silicic acid-containing apatite can be produced by immersing them in the above-mentioned solution, respectively.
[0055] That is, in another aspect of the present invention, A step of hydrolyzing the readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; Obtaining a powdered composition containing the silicic acid-containing calcium phosphate crystals obtained; and immersing the obtained powder composition in a solution; Method for producing a powdered composition of siliceous apatite; A step of hydrolyzing the readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; Obtaining a block material containing the obtained silicic acid-containing calcium phosphate crystals; and The process includes immersing the obtained block material in a solution. A method for producing a block material of siliceous apatite; and A step of hydrolyzing the readily soluble calcium phosphate in an aqueous silicate solution to obtain silicic acid-containing calcium phosphate crystals; Obtaining a porous body containing the silicic acid-containing calcium phosphate crystals obtained; and immersing the obtained porous body in a solution; Method for producing porous silica-containing apatite Examples include:
[0056] For the step of immersing the powder composition, block material, or porous body in the solution, the conditions for immersing the silicic acid-containing calcium phosphate in the solution are applied.
[0057] This embodiment may include a step of washing the obtained powder composition, block material, or porous body, and a step of drying the same thereafter. The washing step may include washing the obtained powder composition, block material, or porous body with, for example, distilled water, and may be performed according to a conventional method. The drying step may include drying the obtained powder composition, block material, or porous body with, for example, a dryer after the washing step.
[0058] Another aspect of the present invention is The present invention relates to a calcium phosphate crystal that contains calcium ions and phosphate ions and may further contain hydroxide ions and / or halide ions, in which at least one of the calcium ions, phosphate ions, hydroxide ions, and halide ions contained in the crystal structure is partially substituted with silicate ions.
[0059] The crystals include, for example, octacalcium phosphate, hydroxyapatite, etc., as the calcium phosphate. Examples of suitable materials include apatite and carbonate apatite. In addition, when the calcium phosphate is octacalcium phosphate, the crystal according to this embodiment refers to a silicic acid-containing octacalcium phosphate crystal produced by the production method according to the above embodiment.
[0060] The silicate ion content of the crystal is preferably 10 atomic % or more, more preferably 12 atomic % or more, and even more preferably 15 atomic % or more, and is preferably 50 atomic % or less, more preferably 30 atomic % or less, and even more preferably 25 atomic % or less. In addition, as the stoichiometric composition of calcium phosphate, the ratio of Ca to PO4 is 50% or more in a single compound.
[0061] The crystals preferably include an apatite phase. In addition, the crystals are preferably either in an embodiment in which the apatite phase contains carbonate or in an embodiment in which the apatite phase does not contain carbonate.
[0062] The crystals refer to particles that give clear diffraction peaks in the XRD pattern of a powder sample and that exhibit a unique external shape due to the crystal structure when grown in a free space that does not inhibit crystal growth.
[0063] When the calcium phosphate is octacalcium phosphate, the crystal preferably contains silicate ions in the hydration layer that constitutes the crystal structure of the octacalcium phosphate.
[0064] The crystallographic information of the crystals can be obtained by, for example, X-ray diffraction (XRD) in a conventional manner using an apparatus such as MiniFlex600 (Rigaku Corporation, Japan).
[0065] The element contents in the crystals can be evaluated in accordance with a conventional method, for example, by X-ray fluorescence analysis (XRF) using an apparatus such as SEA2210 (Seiko Instruments Technology Inc., Japan).
[0066] The chemical oscillation scheme of the crystal can be evaluated by, for example, Fourier transform infrared spectroscopy (FT-IR) in accordance with a conventional method, using, for example, a Nicolet NEXUS670 (Thermo Fisher Scientific, Inc., USA).
[0067] The microstructure of the crystal can be evaluated by a field emission scanning electron microscope (FE-SEM) according to a conventional method. An example of the apparatus is JSM-6700F (JEOL Ltd., Japan). In order to prevent charge accumulation on the surface of the crystal, the crystal may be sputter-coated with Os or the like.
[0068] Another aspect of the present invention is a powdery composition comprising the crystal. The form of the powder composition is not limited as long as it contains the crystals. The powder composition may be a powder consisting of the crystals (i.e., the content of the crystals in the powder composition is 100%), but may also contain other components. The content of the crystals in the powder composition is preferably 1% or more, more preferably 10% or more, and even more preferably 30% or more. The content can be calculated by measuring the peak intensity in XRD.
[0069] Another aspect of the present invention is a block material containing the crystal. The embodiment of the block material is not limited as long as it contains the crystals. The block material may be a block material made of the crystals (i.e., the content of the crystals in the block material is 1 The crystal content in the block material is preferably 1% or more, more preferably 10% or more, and even more preferably 30% or more. The content can be measured, for example, by using XRD.
[0070] Another aspect of the present invention is a porous body containing the crystals. The shape of the pores is not particularly limited. Examples of the pores are usually interconnected porous bodies, isolated pore bodies, honeycomb structures, etc. The porosity is not particularly limited. It is preferably 30% or more, more preferably 50% or more, and particularly preferably 70% or more. The pore size is not particularly limited, but is preferably 10 μm or more and 1000 μm or less, particularly preferably 100 μm or more and 700 μm or less, and more preferably 200 μm or more and 500 μm or less. EXAMPLES
[0071] The following examples are not to be construed as limiting. The X-ray diffraction (XRD: MiniFlex600, Rigaku Corporation, Japan) patterns in the following examples were measured using a Cu target and a wavelength of 0.15406 nm.
[0072] [Example 1] Preparation of silica-supported OCP powder Sodium silicate solution reagent purchased from FUJIFILM Wako Pure Chemical Industries, Ltd. was diluted with distilled water to prepare 1 mol / L Na2SiO3. 20 mL of this diluted solution was dispensed into a 50 mL centrifuge tube, and 2.39 g of calcium hydrogen phosphate dihydrate (DCPD) powder, also purchased from FUJIFILM Wako Pure Chemical Industries, Ltd., was added thereto and reacted at 60°C for 24 hours. After the reaction, the sample was washed several times with distilled water and then completely dried in a dryer at 40°C.
[0073] (Characteristics evaluation) Crystallographic information of the samples was obtained by X-ray diffraction (XRD: MiniFlex600, Rigaku Corporation, Japan) with an accelerating voltage and amplitude of 40 kV and 15 mA, respectively. The diffraction angle was continuously scanned at 2θ values from 3° to 70° at a scanning speed of 5° / min for characterization and from 2° to 12° at a scanning speed of 1° / min for crystallographic parameter analysis.
[0074] In addition, Fourier transform infrared spectroscopy (FT-IR: Nicolet NEXUS670, Thermo Fisher Scientific, USA) was used to measure the concentration of triglycine sulfate using an attenuated total reflection prism made of GeSe (32 scans, resolution 2 cm). -1 ) was used to characterize the chemical oscillation scheme of the samples. Air atmosphere was used as the background for performing the measurements.
[0075] In addition, the microstructure of the samples was evaluated by a field emission scanning electron microscope (FE-SEM: JSM-6700F, JEOL Ltd., Japan) at an accelerating voltage of 5 kV. To prevent charge accumulation on the surface, the samples were sputter-coated with Os.
[0076] In addition, the chemical composition of the samples was evaluated by X-ray fluorescence analysis (XRF:SEA2210, Seiko Instruments Technology Inc., Japan) at an acceleration voltage of 15 kV. This allowed us to measure the silicon content, which is difficult to measure by ICP-AES. In addition, other elements were also measured to determine the element ratios.
[0077] The samples were evaluated by XRD. Figure 1 shows the XRD patterns of samples treated with different sodium silicate concentrations. When the sodium silicate concentration was 1 mol / L, a diffraction peak characteristic of OCP was observed at around 4.7°. On the other hand, when the concentration was lower than that, a strong diffraction peak was observed. In both cases, apatite was formed. For convenience, the samples that showed OCP peaks are referred to as OCP-silica.
[0078] The silicon content in the sample was measured by XRF. Figure 2 shows the relationship between the content of silicate ions in the sample and the concentration of the treated sodium silicate solution. At low concentrations, a large amount of the starting material DCPD remained, so the measurement data is omitted here. The silica content in OCP-silica was approximately 18 atomic %.
[0079] Next, the state of the functional groups in the OCP sample was evaluated using FT-IR. Figure 3 shows the FT-IR spectrum of the sample. As reference samples, the spectra of silicon dioxide powder and OCP prepared in a solution not containing silicon (OCP-Na) are also shown. In addition to the calcium phosphate peaks observed in OCP-Na, the absorption bands of silicon dioxide were also observed in OCP-silica. This suggests that silicate ions are supported in OCP-silica.
[0080] In addition, when the absorption band of P5 PO4, which corresponds to the water-bearing layer and is a factor governing interlayer development, was evaluated under magnification, the absorption band of P5 PO4 was hardly observed in OCP-silica.
[0081] In the case of OCP-silica, the absorption band of P5 PO4 was hardly observed, but since it has a layered structure, the state of PO4 was further evaluated. 31 The P solid-state NMR spectrum is shown. Of the four P absorption peaks in OCP (P1, P2 / P4, P3, P5 / P6), no peaks corresponding to P5 / P6, which are equivalent to PO4 present in the water-containing layer, were observed in OCP-silica. This shows that silicate ions have been substituted at the P5 / P6 positions, i.e., in the water-containing layer.
[0082] The microstructure of OCP-silica was observed by SEM. Figure 5 shows an SEM image of the sample. OCP-silica had a structure in which amorphous particles of about 10-20 nm were densely assembled. It also had a pseudomorphic structure that maintained the shape of the starting material, DCPD.
[0083] [Example 2] Preparation of silica-containing apatite from OCP-silica Using the OCP-silica powder prepared in Example 1 as a starting material, an attempt was made to prepare silica-supported apatite. 0.4 g of OCP-silica powder was immersed in 20 mL of 0-2 mol / L (NH4)2CO3 solution and reacted at 80°C for 3 days. After the treatment, the powder was washed several times with distilled water and then completely dried at 80°C.
[0084] (Characteristics evaluation) Crystallographic information of the samples was obtained by X-ray diffraction (XRD: MiniFlex600, Rigaku Corporation, Japan) with an accelerating voltage and amplitude of 40 kV and 15 mA, respectively. The diffraction angle was continuously scanned at 2θ values from 3° to 70° at a scanning speed of 5° / min for characterization and from 2° to 12° at a scanning speed of 1° / min for crystallographic parameter analysis.
[0085] In addition, Fourier transform infrared spectroscopy (FT-IR: Nicolet NEXUS670, Thermo Fisher Scientific, USA) was used to measure the concentration of triglycine sulfate using an attenuated total reflection prism made of GeSe (32 scans, resolution 2 cm). -1 ) was used to characterize the chemical oscillation scheme of the samples. Air atmosphere was used as the background for performing the measurements.
[0086] In addition, the chemical composition of the samples was evaluated by X-ray fluorescence analysis (XRF:SEA2210, Seiko Instruments Technology Inc., Japan) at an acceleration voltage of 15 kV. This allowed us to measure the silicon content, which is difficult to measure by ICP-AES. In addition, other elements were also measured to determine the element ratios.
[0087] The samples were evaluated by XRD. Figure 6 shows the XRD patterns of the samples treated with different (NH4)2CO3 concentrations. Regardless of the (NH4)2CO3 concentration, the samples after treatment were a single phase of apatite.
[0088] Next, the dynamics of carbonate content in the sample was measured by FT-IR. Figure 7 shows the FT-IR spectrum of the sample. In the sample spectrum, both the absorption band of PO4 and the absorption band corresponding to silanol groups were observed, indicating that silicate ions were contained. In addition, as the (NH4)2CO3 concentration increased, a band (1400-1500 cm) corresponding to the CO3 absorption band in the sample appeared. -1 ) absorption intensity was found to increase.
[0089] The silicic acid content in the samples was measured by XRF. Figure 8 shows the silicic acid content of the samples. The treated apatite samples contained approximately 15-17 atomic % of silicate ions. This content was about 90-95% of the starting material, OCP-silica.
[0090] [Example 3] Preparation of calcium phosphate carrying silicic acid by heat treatment of silicic acid carrying OCP An attempt was made to prepare other calcium phosphates from OCP-silica by placing an appropriate amount of the OCP-silica prepared in Example 1 on an alumina baking dish and heating it in an electric furnace. The advantage of this method is that there is no exchange of materials via a solution, so the composition of the product is the same as that of the OCP-silica used as the starting material, except for volatile components.
[0091] The XRD patterns of the samples after heating are shown in Figure 9. For the samples heated from 200°C to 800°C, the OCP peak disappeared and it was observed that the apatite single phase was formed. On the other hand, when heated to 1000°C or higher, in addition to the apatite peak, the peak of cristobalite, a silicon dioxide compound, was confirmed.
[0092] The microstructure of the samples was observed using an SEM. Figure 10 shows an SEM image of the sample that underwent the heating experiment. For samples up to 800°C, no significant change in overall shape was observed compared to the samples before heating, but for samples heated to 1000°C or higher, it was observed that a granular structure had formed in the OCP-silica substrate, and at 1250°C this tendency became even more pronounced, with the size of the granular structure increasing.
[0093] [Example 4] Preparation of silicic acid-loaded OCP granules Sodium silicate solution reagent purchased from Fujifilm Wako Pure Chemical Industries, Ltd. was diluted with distilled water to prepare 1 mol / L Na2SiO3. 10 mL of this diluted solution was dispensed into a 50 mL centrifuge tube, and then 1 mL and 9 mL of calcium hydrogen phosphate disodium and sodium dihydrogen phosphate, both purchased from Fujifilm Wako Pure Chemical Industries, Ltd., were dissolved in distilled water to prepare 1 mol / L solutions, respectively, and mixed. The solution was liquid immediately after mixing, but soon became a jelly-like gel. This jelly-like gel was strongly stirred with a vibrator or the like to destroy the gel structure formed by mixing, breaking it into fine particles and becoming a gel fluid with fluidity.
[0094] Calcium dihydrogen phosphate hydrate powder purchased from Fujifilm Wako Pure Chemical Industries, Ltd. and tricalcium phosphate β-phase powder were weighed out in a molar ratio of 1:1, and then mixed thoroughly in a dry state in an automatic mortar to obtain brushite cement powder, which was then stored at 70°C.
[0095] An appropriate amount of the powder prepared in the previous section was put into a pan-type granulator, rotated at 40 rpm, and adjusted so that the powder would flow down the bottom of the pan-type granulator. Distilled water was sprayed with a spray bottle to induce a hardening reaction, yielding particles made of granular calcium hydrogen phosphate dihydrate molded bodies. These were classified with an automatic vibrating sieve to obtain granules of 250-500 μm. These were heated at 70°C to obtain granular particles made of calcium hydrogen phosphate.
[0096] 1 g of the granular calcium hydrogen phosphate particles prepared in the previous section was immersed in the gel fluid prepared as described above and reacted at 70°C for 2 days. After the reaction, the sample was washed with distilled water to After removing the reaction solution and gel fluid, the mixture was dried at 40° C. to obtain a sample consisting of granular particles as shown in FIG.
[0097] The prepared sample was identified by XRD in the same manner as in Examples 1 and 2, and it was confirmed to be a single phase of octacalcium phosphate, as shown in Figure 11. Furthermore, silicon ions and silanol groups were detected in the sample by FT-IR and XRF measurements, which revealed that the granular particles were composed of octacalcium phosphate supported by silicic acid.
[0098] When the granular particles were observed under an SEM, it was found that the plate-like crystals were densely intertwined, as shown in Figure 12, and that silicic acid-supported octacalcium phosphate crystals were formed by the dissolution-precipitation reaction, maintaining the granular particles.
[0099] [Example 5] Preparation of silicic acid-loaded apatite granules from silicic acid-loaded OCP granules 0.4 g of the silicic acid-supported OCP granules prepared in Example 4 was mixed with 0-2 mol / L ammonium carbonate. The reaction was carried out at 80°C for 3 days. After the reaction, the sample was distilled. After washing thoroughly with water, it was dried.
[0100] The shape of the sample after the reaction retained the general shape of the silicic acid-loaded OCP granules used as the starting material, regardless of the carbonate concentration (Figure 13).
[0101] The sample after the reaction was measured by XRD in the same manner as in Example 4, and it was confirmed that the sample was a single phase apatite (FIG. 14).
[0102] The dynamics of carbonate content in the sample was measured by FT-IR. Figure 15 shows the FT-IR spectrum of the sample. In the sample spectrum, both the absorption band of PO4 and the absorption band corresponding to silanol groups were observed, indicating that silicate ions were contained. In addition, as the (NH4)2CO3 concentration increased, a band (1400-1500 cm) corresponding to the CO3 absorption band in the sample appeared. -1 ) was found to have an increased absorption intensity (Figure 15).
Claims
1. A calcium phosphate crystal containing calcium ions and phosphate ions and optionally containing hydroxide ions and / or halide ions, wherein at least one of the calcium ions, the phosphate ions, the hydroxide ions, and the halide ions contained in the crystal structure is partially substituted with silicate ions, the calcium phosphate is octacalcium phosphate; The hydrated layer constituting the crystal structure of the octacalcium phosphate contains silicate ions. crystal.
2. A powdered composition comprising the crystal of claim 1.
3. A block material comprising the crystal of claim 1.
4. A porous body comprising the crystal according to claim 1.
5. A method comprising the steps of: immersing the crystal according to claim 1 in a solution to obtain a crystal of a siliceous acid-containing calcium phosphate containing an apatite phase. A method for producing siliceous apatite.
6. The method of claim 5, wherein the solution is carbonate-free and the apatite phase is carbonate-free.
7. The method of claim 5 , wherein the solution contains carbonate and the apatite phase contains carbonate.
Citation Information
Patent Citations
Preparation method of carbonated silicon-containing HA (Hydroxyapatite) nano powder
CN102040207A
Compositions and methods for delivering bmp-2 amplifiers / co-activators to enhance bone formation
JP2009541358A
Biomedical materials
JP2010523250A
Silicate-substituted hydroxyapatite
JP2012514573A
Ion-substituted calcium phosphate particles
JP2013500935A