Composite papermaking functional material and its preparation method and application

By using aluminum sulfate as a dealkalinizing agent and a dehydration system of glycerol and zinc nitrate during the hydrothermal synthesis of calcium silicate, the pH of calcium silicate is reduced and the problem of the incompatibility of finished calcium silicate products with paper pulp is solved. Water consumption is reduced and paper performance is improved.

CN117776248BActive Publication Date: 2024-10-18YANCHENG CHENGXIN MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311851307.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-18
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

During the hydrothermal synthesis of calcium silicate, the pH of the finished calcium silicate is high, making it unsuitable for paper pulp. In addition, the existing dealkalization method consumes a large amount of water resources and increases production costs.

Method used

A low-modulus sodium silicate solution and lime milk are used for dynamic hydrothermal synthesis, aluminum sulfate is used as a dealkalizing agent, calcium sulfate dihydrate is converted into calcium sulfate hemihydrate through dehydration operation, the pH is reduced, and glycerol and zinc nitrate are used The dehydration system carries out the dehydration reaction.

Benefits of technology

It effectively reduces the pH of the finished calcium silicate product, improves the compatibility with paper pulp, reduces the amount of water used for alkali elution and wastewater treatment, reduces production costs, and improves the physical properties of paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117776248B_ABST
    Figure CN117776248B_ABST
Patent Text Reader

Abstract

The present invention provides a composite papermaking functional material and its preparation method and application, which belongs to the field of papermaking technology, including: providing a low modulus sodium silicate solution and lime milk; the low modulus sodium silicate solution is prepared by alkali dissolution of quartz sand, and the lime milk is prepared by digestion of quicklime; the low modulus sodium silicate solution and the lime milk are subjected to a dynamic hydrothermal synthesis reaction to obtain a precursor slurry; after the precursor slurry is centrifuged and washed and pulped, a dealkalizing agent is used to dealkalize the obtained pulping liquid to obtain a low-pH slurry; a dehydration system is provided, and the low-pH slurry is converted into a calcium silicate-calcium sulfate hemihydrate composite suspension by a dehydration operation, and the calcium silicate-calcium sulfate hemihydrate composite material is a composite papermaking functional material; the dealkalizing agent is aluminum sulfate. The composite papermaking functional material of the present invention uses a dealkalizing agent to reduce the pH of the finished product, and uses a composite effect to improve the basic physical properties of paper, and has a good prospect in the application of paper fillers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking, and in particular to a composite papermaking functional material and a preparation method and application thereof. Background Art

[0002] With the deterioration of the earth's environment, along with the environmental pollution caused by the plant pulping process and the large consumption of plant raw materials, water and energy, the limitations of traditional papermaking technology and raw materials are becoming increasingly serious and need to be improved. In recent years, with the development of the papermaking industry and the increasingly fierce market competition, papermakers have also paid more and more attention to how to reduce paper costs and transportation costs. In order to reduce the amount of fiber raw materials added during use and improve the paper's uniformity, brightness, printing adaptability and other paper properties, targeted papermaking fillers are added during the papermaking process to improve the overall performance of the paper. Different paper types have a large difference in the amount of papermaking fillers added, the maximum can be as high as about 40%. Compared with the price of plant fiber, the price of papermaking fillers is only one-tenth of the price of plant fiber, or even lower, which significantly reduces the cost of paper production and reduces the use of plant fiber, with significant environmental benefits.

[0003] There are many kinds of paper fillers on the market, and the commonly used ones are talcum powder, kaolin, calcium carbonate, etc. Different fillers have different properties, so the physical and chemical properties of fillers in paper are also different. The raw materials of commonly used paper fillers are mainly inorganic minerals, but the use of these non-renewable minerals for paper filling not only consumes a large amount of natural mineral resources, but also brings serious damage to the vegetation and natural environment in the mining area.

[0004] As a porous honeycomb material that can be chemically synthesized, calcium silicate also has the characteristics of low relative density, high specific surface area, soft texture, high sedimentation volume, low abrasion value and good whiteness stability. Its high sedimentation volume is conducive to the uniform transportation of fillers and improves the dispersion of fillers. It can also improve the bulk and light scattering of paper, etc., and it has a good prospect as a papermaking filler. However, in the hydrothermal synthesis process of calcium silicate, alkaline reagents such as liquid alkali and lime milk are used, which leads to a high pH value of the finished calcium silicate product, which is incompatible with the pH value of pulp in the papermaking process. Although previous studies have reported that sulfuric acid or hydrochloric acid can be used as a dealkalizing agent for the calcium silicate synthesis reaction, hydrochloric acid and sulfuric acid are strong acids that are easy to corrode equipment and have a high risk factor. The addition of hydrochloric acid will introduce chloride ion impurities, which will easily corrode equipment over a long period of time and will also have an adverse effect on the performance of paper. Therefore, in the prior art, clean water washing is mostly used during dealkalization. Washing the reaction product with clean water consumes a large amount of water, which easily causes a waste of water resources, is not conducive to the current concept of sustainable industrial development, and will increase the amount of wastewater treated and the treatment cost, and also increase the production cost of the filler. Summary of the invention

[0005] The present invention provides a composite papermaking functional material and a preparation method and application thereof, which are used to solve the problems that the pH value of the calcium silicate product is high due to the high pH value of the reaction system in the process of hydrothermal synthesis of calcium silicate, the high pH value of the existing calcium silicate product is incompatible with the pH value of pulp, and the large amount of washing water and wastewater treatment caused by water washing and de-alkali, and the high production cost.

[0006] To achieve the above object, the present invention provides a method for preparing a composite papermaking functional material, comprising:

[0007] 1) providing a low modulus sodium silicate solution and lime milk; the low modulus sodium silicate solution is prepared by alkali dissolution of quartz sand, and the lime milk is prepared by digestion of quicklime;

[0008] 2) subjecting a low modulus sodium silicate solution and lime milk to a dynamic hydrothermal synthesis reaction to obtain a precursor slurry;

[0009] 3) After the precursor slurry is centrifuged and beaten, a dealkalizing agent is used to dealkalize the resulting beaten liquid to obtain a low pH slurry;

[0010] 4) providing a dehydration system, using a dehydration operation to convert the low pH pulp into a calcium silicate-calcium sulfate hemihydrate composite material suspension, the calcium silicate-calcium sulfate hemihydrate composite material is a composite papermaking functional material; the dealkalizer is aluminum sulfate; the dehydration system includes propylene glycol and zinc nitrate.

[0011] The method uses low modulus sodium silicate solution obtained by alkali dissolution of quartz sand and lime milk obtained by digestion of active quicklime as raw materials, and uses a hydrothermal method to prepare calcium silicate. The method uses a dealkalizing agent aluminum sulfate to reduce the pH of the overall slurry, and then uses a dehydration operation to convert the impurity calcium sulfate dihydrate generated during dealkalization into a usable filler calcium sulfate hemihydrate, thereby preparing a calcium silicate-calcium sulfate hemihydrate composite material, which also solves the problem of high pH of the finished calcium silicate product caused by the high pH of the reaction system during the hydrothermal synthesis of calcium silicate, and further improves the problem that the existing calcium silicate product has a high pH and is incompatible with the pH of pulp. Compared with calcium silicate fillers, the composite papermaking functional material can further improve the basic physical properties of paper by using the composite effect, and improve the bulk and whiteness of paper to a certain extent, and has a good prospect in the application of paper fillers.

[0012] It is further configured that the modulus of the low modulus sodium silicate solution is 1.0-1.2, and the SiO2 concentration therein is 40-70 g / L.

[0013] It is further configured that the dynamic hydrothermal synthesis reaction process is as follows: after the low modulus sodium silicate solution is heated to 75-80°C, lime milk and water are added thereto, and after stirring and heating to 75-80°C at a rate of 300-600r / min, the solution is stirred and reacted for 0.5-1h to obtain a precursor slurry.

[0014] Preferably, the weight ratio of the low modulus sodium silicate solution, water and lime milk is 1:(1-1.3):(1.5-2).

[0015] The main component of the precursor slurry obtained by dynamic hydrothermal synthesis reaction is calcium silicate. When calcium silicate is used as a papermaking filler, its higher sedimentation volume is beneficial to the dispersion of the papermaking filler, making it evenly distributed in the fiber slurry, thereby helping to improve the retention rate of the papermaking filler. It also increases the bonding space and area between the fiber and the papermaking filler by virtue of its porosity and large specific surface area, weakening the negative impact of the papermaking filler on the strength of the paper, while also increasing the bulk of the paper.

[0016] It is further configured that the centrifugal washing and pulping operation process is as follows: the precursor slurry is centrifuged and filtered, the filter cake obtained by centrifugation is reversely washed 2-3 times, and then water is added to the filter cake obtained by washing and pulped for 30-40 minutes, and the pulping liquid obtained by pulping is stirred and heated to 80-95°C at a rate of 300-600r / min for use.

[0017] Preferably, the total amount of water used for reverse washing is 2-3 times the mass of the filter cake obtained by centrifugation; and the amount of water added in the pulping operation is 1-1.5 times the mass of the filter cake obtained by washing.

[0018] It is further configured that the dealkalization operation process is as follows: add the dealkalizing agent aluminum sulfate to the pulping liquid, react for 1-1.5 hours at a temperature of 80-95°C and a rotation speed of 300-600r / min to obtain a low pH slurry with a pH of 8-11.

[0019] Preferably, in the dealkalization operation, the amount of the dealkalizing agent added is 5-20 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200-230 parts by weight.

[0020] The dealkalizing agent aluminum sulfate can convert the residual alkali liquid in the pulping liquid into soluble neutral salts, and then wash and remove these soluble salts in the form of ions, thereby reducing the pH of the pulping liquid and the composite papermaking functional materials, so that the compatibility of the composite papermaking functional materials with the fiber pulp is significantly improved, and the problem of high pH of the finished product caused by the high pH of the reaction system during the hydrothermal synthesis of calcium silicate is solved, thereby improving the problem that the existing calcium silicate finished product has a high pH and is incompatible with the pH of pulp, and also avoiding the problems of large washing water consumption and wastewater treatment volume and high production cost caused by water washing and de-alkali.

[0021] It is further configured that the dehydration operation process is as follows:

[0022] 4.1) adding glycerol-zinc nitrate dehydration system and solubility inhibitor to the low pH slurry, heating the resulting mixed system to 90-110° C., and reacting at a speed of 300-600 r / min for 0.5-1 h;

[0023] 4.2) Adding a coating agent to the mixed system after the reaction, and continuing the reaction at a temperature of 90-110° C. and a rotation speed of 300-600 r / min for 0.5-1 h to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0024] The low-pH pulp contains 10-20% of calcium sulfate dihydrate formed by dealkalization, which is not effective as a papermaking filler. Therefore, the dehydration system and dehydration operation are used to dehydrate the calcium sulfate dihydrate without leaving the calcium silicate. After the reaction, calcium sulfate hemihydrate is obtained, thereby converting the impurity-type calcium sulfate into a beneficial component that can be used as a papermaking filler, realizing the conversion of calcium sulfate dihydrate with high added value and high utilization in the production of calcium silicate. Calcium sulfate hemihydrate has a strong positive charge adsorption effect, which can adsorb a large amount of positively charged charges in the pulp, forming a bridging effect between the fiber and the paper, and can improve the physical properties of paper as a papermaking filler.

[0025] Preferably, in the dehydration operation, the amount of glycerol added is 5-10 parts by weight, the amount of zinc nitrate added is 1-2 parts by weight, the amount of solubility inhibitor added is 1-3 parts by weight, and the amount of coating agent added is 1-5 parts by weight.

[0026] The glycerol-zinc nitrate system acting as a dehydration system can dehydrate the calcium sulfate dihydrate crystal into calcium sulfate hemihydrate. The zinc nitrate therein acts as a strong electrolyte and completely ionizes nitrate ions and zinc ions in the solution of the mixed system. The zinc ions can effectively reduce the activation energy in the solution and promote the dehydration of the unstable calcium sulfate dihydrate crystal. The glycerol effectively reduces the water activity in the solution, and the decrease in water activity can also promote the dehydration conversion of calcium sulfate dihydrate.

[0027] It is further configured that the solubility inhibitor is selected from at least one of sodium dodecylbenzene sulfonate, sodium citrate, fatty alcohol polyoxyethylene ether, polyoxyethylene ethyl ether, potassium sodium tartrate, fatty alcohol sodium sulfate, polyethylene glycol, sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, and sodium polyacrylate. The solubility inhibitor is mainly used to change the crystal structure, promote the further development of the calcium sulfate hemihydrate crystal form, improve the crystal stability, and reduce the solubility of calcium sulfate hemihydrate.

[0028] It is further configured that the coating agent is selected from at least one of phenolic resin, urea-formaldehyde resin, and polyamide polyamine epichlorohydrin. The coating agent can coat the calcium sulfate hemihydrate, further reduce the solubility of the calcium sulfate hemihydrate in the mixed system, which is beneficial to improving the yield and comprehensive quality of the composite material, and is also beneficial to improving the retention rate of the composite papermaking functional material.

[0029] The present invention also provides a composite papermaking functional material, which is prepared by the aforementioned composite papermaking functional material preparation method.

[0030] The composite papermaking functional material prepared by the present invention has low density, high specific surface area, and large sedimentation volume, and can improve the bulk and light scattering type, ink absorbency and dispersibility of paper. It exists in a colloidal state in paper pulp, can absorb a large amount of positively charged fibers, and is not easy to be delaminated with plant fibers, so that its retention rate is increased. The composite papermaking functional material promotes the improvement of paper performance as a new type of papermaking filler, can replace mineral fillers such as calcium carbonate, porcelain clay, talcum powder, etc. widely used in the current papermaking industry, avoids the problem of using non-renewable mineral resources as papermaking fillers in traditional papermaking processes, and can significantly save the amount of plant fibers, with low raw material prices and production costs, and significant environmental benefits.

[0031] The present invention also provides an application of a composite papermaking functional material in papermaking. The composite papermaking functional material is prepared by the aforementioned preparation method of the composite papermaking functional material. The composite papermaking functional material is added to papermaking pulp as a papermaking filler.

[0032] The calcium silicate and calcium sulfate hemihydrate composite in the composite papermaking functional material can fully fill and intercept the plant fibers, and have both physical filling and chemical bonding with the plant fibers, thereby forming a relatively stable structure with the plant fibers, which is not prone to stratification. The finished paper has good quality and there will be no "powdering" of fillers on the surface of the paper. The comprehensive properties of the paper (such as tensile strength and tear index, bulk and whiteness, etc.) are improved, the amount of plant fibers used is significantly saved, and the resources are abundant and the price is low, which reduces the cost of papermaking.

[0033] Preferably, the papermaking pulp includes but is not limited to bleached chemical pulp, unbleached chemical pulp, semi-chemical pulp, chemical mechanical pulp, deinked pulp, OCC pulp or other plant fiber raw materials, and any combination thereof after pulping. The composite papermaking pulp is suitable for various papermaking pulps and is used to make various papers, such as tissue paper, packaging paper / board and other special purpose papers.

[0034] In the preparation method of the present invention, a dealkalizing agent is used to reduce the pH value of the finished calcium silicate product, thereby solving the problem of high pH value of the finished calcium silicate product caused by high pH value of the reaction system during the hydrothermal synthesis of calcium silicate, thereby improving the problem that the existing finished calcium silicate product has high pH value and is incompatible with the pH value of pulp, and also avoiding the problems of large amount of washing water and wastewater treatment and high production cost caused by water washing and de-alkali treatment.

[0035] The preparation method of the present invention, in an environment where calcium silicate exists, also utilizes a dehydration reaction to convert the impurity-type calcium sulfate dihydrate generated during the dealkalization process into a usable filler-type calcium sulfate hemihydrate, thereby avoiding the negative impact of byproducts on papermaking functional materials and paper properties, and can also utilize the composite effect of calcium silicate and calcium sulfate hemihydrate to improve the physical properties of paper (especially tensile strength and tear index, bulk and whiteness, etc.). The method provides a new type of papermaking functional material that can be widely used, is simple and easy to operate, has strong operability, and has widely available raw materials, low cost, and is easy to achieve large-scale industrial production and application.

[0036] The composite papermaking functional material of the present invention combines calcium silicate and calcium sulfate hemihydrate by utilizing hydrothermal reaction, dehydration reaction and the like, thereby increasing the bonding and bridging effect between the composite papermaking functional material and plant fibers, having the advantages of increasing the retention rate of the composite papermaking functional material and improving the physical properties of paper, being able to replace mineral fillers such as calcium carbonate, porcelain clay, talcum powder and the like that are widely used in the current papermaking industry, avoiding the problem of using non-renewable mineral resources as papermaking fillers in traditional papermaking processes, and at the same time being able to significantly save the amount of plant fibers used and reduce papermaking costs.

[0037] When the composite papermaking functional material of the present invention is used as a papermaking filler in papermaking, it can be used to make various types of paper, and the filling process is simple. The composite papermaking functional material and the plant fiber have both physical filling and chemical bonding, and are not prone to stratification. The finished paper has good quality and will not have the phenomenon of "powdering" of filler on the surface of the finished paper. The comprehensive performance of the paper is improved, and it has significant advantages in saving plant pulp fibers. The production cost of paper is significantly reduced, and it has high economic significance and ecological and environmental significance, and is easy to promote industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1These are SEM photos of the finished composite materials of Example 3 and Example 8, A-Example 3, B-Example 8. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work also fall within the scope of protection of the present invention.

[0041] The following examples use conventional instruments and equipment in the art. Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources, and their specifications are conventional specifications in the art. If no specific techniques or conditions are specified in the following examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0042] It should be noted that, in the present invention and the following embodiments, concentrations, ratios, etc. not otherwise specified are all weight concentrations, weight ratios, etc., "%" means weight percentage, and "parts" means parts by weight, which are common writing habits used by those skilled in the art and are therefore not described in detail in the present invention.

[0043] As a preferred embodiment, the preparation process of the low modulus sodium silicate solution is as follows:

[0044] 1.1) Quartz sand, water and sodium hydroxide solution with a mass concentration of 20-40% are subjected to hydrothermal reaction at a pressure of 0.6-0.8 MPa and a temperature of 160-180° C. for 2-4 hours to obtain a water glass solution;

[0045] 1.2) cooling the water glass solution to 60-75°C, filtering, and obtaining a water glass mother solution with a SiO2 concentration of 180-230 g / L;

[0046] 1.3) Adding a sodium hydroxide solution with a mass concentration of 15-40% to the above water glass mother liquor to reduce its modulus to 1.0-1.2 and SiO2 concentration to 40-70g / L, to prepare a low modulus sodium silicate solution.

[0047] Preferably, in the hydrothermal reaction, the weight ratio of quartz sand, water and sodium hydroxide solution is 1:(2-3.5):(1-1.3).

[0048] Preferably, the SiO2 content in the quartz sand is greater than 90%.

[0049] In another embodiment, the sodium silicate solution can be prepared by hydrothermal reaction of quartz sand, water and excess sodium hydroxide solution to directly prepare a low modulus sodium silicate solution with a modulus of 1.0-1.2 and a SiO2 concentration of 40-70 g / L in one step.

[0050] As a preferred embodiment, the preparation process of lime milk is as follows: add 5-8 times the weight of water to quicklime, stir and digest for 0.5-1h to obtain lime milk.

[0051] Preferably, the calcium oxide content in quicklime is >90%.

[0052] As a preferred embodiment, the preparation method also includes a drying and pulverizing operation, and the drying and pulverizing operation process is as follows: filtering the calcium silicate-calcium sulfate hemihydrate composite material suspension while hot, drying and breaking up the filter cake obtained by filtration, and the obtained calcium silicate-calcium sulfate hemihydrate composite material is a composite papermaking functional material.

[0053] As an improvement to the above embodiment, 0.5-1.0 parts by weight of a whisker stabilizer is also added during the dehydration operation, wherein the whisker stabilizer contains nitroethanol and triethanolamine in a weight ratio of 1:(1-1.5). Specifically, the whisker stabilizer is added to the low pH slurry together with the solubility inhibitor.

[0054] The enhancement effect of the whisker stabilizer increases with the increase of the addition amount, but when the addition amount is large, the growth trend of the effect becomes slow, excessive addition is easy to waste reagents, and the effect is not significant when the addition amount is small. Therefore, the two in the above-mentioned limited range cooperate to form a complex adsorption with the calcium particles on the crystal surface, so that the active growth sites of calcium ions on the crystal surface are reduced, and the growth rate of the crystal along the c-axis direction (the crystal surface corresponding to the c-axis is mainly composed of calcium ions) is effectively inhibited, thereby regulating the aspect ratio of the hemihydrate calcium sulfate crystal, making its longitudinal and lateral differences smaller, and enhancing the stability and gelling effect, which is helpful to improve the retention rate, and can also improve the tensile strength and tear index of the paper, thereby improving the strength, folding endurance and bursting resistance of the paper.

[0055] The present invention also provides a papermaking method, comprising the following steps:

[0056] 1) After the chemical coniferous wood pulp and the chemical hardwood wood pulp are pulped separately, water is added to dilute them respectively until the pulp mass concentration reaches 10-12%, and then the chemical coniferous wood pulp and the chemical hardwood wood pulp are mixed in a mass ratio of 1: (3.5-5), and then the pulp is refined. After the pulping is completed, the refined pulp is diluted with water to a mass concentration of 0.1-0.3%, so as to obtain a diluted pulp with a beating degree of 30-45° SR;

[0057] 2) Add 20-30 wt% of papermaking filler to the diluted slurry and mix them evenly to form papermaking pulp. Add the auxiliary agent to the papermaking pulp, mix with the papermaking pulp for 20-40 seconds, and then put it on the net to form paper.

[0058] Preferably, the papermaking filler is the aforementioned composite papermaking functional material of the present invention, or a combination of the composite papermaking functional material and talcum powder.

[0059] More preferably, in the combined papermaking filler, the mass ratio of the composite papermaking functional material to talcum powder is 2:1.

[0060] Preferably, the additives include 2-3 wt% of a sizing agent and 0.003-0.01 wt% of a retention aid.

[0061] The papermaking method has a simple process for adding composite papermaking functional materials, low equipment requirements, little change to existing papermaking processes and equipment, high operability, good combination effect of composite papermaking functional materials and plant fibers, and is easy to promote industrialization; the paper produced has high bulk and whiteness, high tensile strength and tear index, and at the same time has significant advantages in saving plant pulp fibers, and the cost of paper production is significantly reduced. It has high economic significance and ecological and environmental significance, and is of great promotion value.

[0062] It should be noted that the sizing agent and the retention agent can be any commonly used agent in the art. In the embodiment of the present invention, the sizing agent is AKD stock solution, and the retention agent is cationic polyacrylamide.

[0063] The present invention is further described in detail below in conjunction with the examples. However, it should be understood that the examples are for illustrative purposes only and are not intended to limit the scope of the present invention.

[0064] Embodiment 1:

[0065] A method for preparing a composite papermaking functional material comprises the following steps:

[0066] 1) Quartz sand, water and a sodium hydroxide solution with a mass concentration of 20% are subjected to a hydrothermal reaction at a pressure of 0.6 MPa and a temperature of 160° C. for 4 hours to obtain a water glass solution; the SiO2 content in the quartz sand is greater than 90%; in the above hydrothermal reaction, the weight ratio of the quartz sand, water and the sodium hydroxide solution is 1:2:1.3.

[0067] 2) After cooling the water glass solution to 60° C., the solution was filtered to obtain a water glass mother solution having a SiO2 concentration of 180 g / L.

[0068] 3) Adding a sodium hydroxide solution with a mass concentration of 15% to the above-mentioned water glass mother liquor to reduce its modulus to 1.0-1.2 and SiO2 concentration to 40g / L, thereby preparing a low modulus sodium silicate solution.

[0069] 4) Add 5 times the weight of water to quicklime, stir and digest for 0.5 hours to obtain lime milk. The calcium oxide content in the quicklime is > 90%.

[0070] 5) After heating the low modulus sodium silicate solution to 75°C, add lime milk and water thereto, stir and heat to 75°C at a rate of 300 r / min, and stir and react for 1 hour to obtain a precursor slurry. The weight ratio of the low modulus sodium silicate solution, water and lime milk is 1:1:1.5.

[0071] 6) The precursor slurry is centrifuged and filtered, and the filter cake obtained by centrifugation is reverse washed twice, and then water is added to the filter cake obtained by washing and pulped for 30 minutes, and the pulping liquid obtained by pulping is stirred and heated to 80° C. at a rate of 300 r / min for use. The total water consumption for reverse washing is twice the mass of the filter cake obtained by centrifugation. The amount of water added in the pulping operation is 1 times the mass of the filter cake obtained by washing.

[0072] 7) Adding aluminum sulfate as a dealkalizing agent to the pulping liquid, reacting for 1.5 hours at a temperature of 80°C and a rotation speed of 300 r / min, to obtain a low-pH pulp with a pH of 8-11. The amount of the dealkalizing agent added is 5 parts by weight, and the weight of the washed filter cake in the pulping liquid is 200 parts.

[0073] 8) Adding a glycerol-zinc nitrate dehydration system and a solubility inhibitor to the low pH slurry, heating the resulting mixed system to 90° C., and reacting at a speed of 300 r / min for 1 hour; adding a coating agent to the reacted mixed system, and continuing to react at a temperature of 90° C. and a speed of 300 r / min for 1 hour to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0074] The added amount of the glycerol is 5 parts by weight, the added amount of zinc nitrate is 1 part by weight, the added amount of the solubility inhibitor sodium citrate is 1 part by weight, and the added amount of the coating agent phenolic resin is 1 part by weight.

[0075] 9) filtering the calcium silicate-calcium sulfate hemihydrate composite material suspension while hot, drying and breaking up the filter cake obtained by filtration, and the obtained calcium silicate-calcium sulfate hemihydrate composite material is the composite papermaking functional material.

[0076] Embodiment 2:

[0077] A method for preparing a composite papermaking functional material comprises the following steps:

[0078] 1) Quartz sand, water and a sodium hydroxide solution with a mass concentration of 40% are subjected to a hydrothermal reaction at a pressure of 0.8 MPa and a temperature of 180° C. for 2 hours to obtain a water glass solution; the SiO2 content in the quartz sand is greater than 90%; in the above hydrothermal reaction, the weight ratio of the quartz sand, water and the sodium hydroxide solution is 1:3.5:1.

[0079] 2) After cooling the water glass solution to 75°C, filter it to obtain a water glass mother solution with a SiO2 concentration of 230 g / L.

[0080] 3) Adding a sodium hydroxide solution with a mass concentration of 40% to the above-mentioned water glass mother liquor to reduce its modulus to 1.0-1.2 and SiO2 concentration to 70g / L, thereby preparing a low modulus sodium silicate solution.

[0081] 4) Add 8 times the weight of water to quicklime, stir and digest for 1 hour to obtain lime milk. The calcium oxide content in the quicklime is > 90%.

[0082] 5) After heating the low modulus sodium silicate solution to 80°C, add lime milk and water thereto, stir and heat to 80°C at a rate of 600 r / min, and stir and react for 0.5 h to obtain a precursor slurry. The weight ratio of the low modulus sodium silicate solution, water and lime milk is 1:1.3:2.

[0083] 6) The precursor slurry is centrifuged and filtered, and the filter cake obtained by centrifugation is reversely washed three times, and then water is added to the filter cake obtained by washing and pulped for 40 minutes. The pulping liquid obtained by pulping is stirred and heated to 95°C at a rate of 600r / min for use. The total water consumption for reverse washing is 3 times the mass of the filter cake obtained by centrifugation. The amount of water added in the pulping operation is 1.5 times the mass of the filter cake obtained by washing.

[0084] 7) Adding aluminum sulfate as a dealkalizing agent to the pulping liquid, reacting for 1 hour at a temperature of 95°C and a rotation speed of 600 r / min, to obtain a low-pH pulp with a pH of 8-11. The amount of the dealkalizing agent added is 20 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 230 parts.

[0085] 8) Adding a glycerol-zinc nitrate dehydration system and a solubility inhibitor to the low pH slurry, heating the resulting mixed system to 110° C., and reacting at a speed of 600 r / min for 0.5 h; adding a coating agent to the mixed system after the reaction, and continuing to react at a temperature of 110° C. and a speed of 600 r / min for 0.5 h to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0086] The added amount of the glycerol is 10 parts by weight, the added amount of zinc nitrate is 2 parts by weight, the added amount of the solubility inhibitor potassium sodium tartrate is 3 parts by weight, and the added amount of the coating agent urea-formaldehyde resin is 5 parts by weight.

[0087] 9) filtering the calcium silicate-calcium sulfate hemihydrate composite material suspension while hot, drying and breaking up the filter cake obtained by filtration, and the obtained calcium silicate-calcium sulfate hemihydrate composite material is the composite papermaking functional material.

[0088] Embodiment 3:

[0089] A method for preparing a composite papermaking functional material comprises the following steps:

[0090] 1) Quartz sand, water and a sodium hydroxide solution with a mass concentration of 30% are subjected to a hydrothermal reaction at a pressure of 0.7 MPa and a temperature of 175° C. for 3 hours to obtain a water glass solution; the SiO2 content in the quartz sand is greater than 90%; in the above hydrothermal reaction, the weight ratio of the quartz sand, water and the sodium hydroxide solution is 1:3.5:1.3.

[0091] 2) After cooling the water glass solution to 75°C, filter it to obtain a water glass mother solution with a SiO2 concentration of 210 g / L.

[0092] 3) Adding a sodium hydroxide solution with a mass concentration of 20% to the above-mentioned water glass mother liquor to reduce its modulus to 1.0-1.2 and SiO2 concentration to 60g / L, thereby preparing a low modulus sodium silicate solution.

[0093] 4) Add 6 times the weight of water to quicklime, stir and digest for 1 hour to obtain lime milk. The calcium oxide content in the quicklime is > 90%.

[0094] 5) After heating the low modulus sodium silicate solution to 80°C, add lime milk and water thereto, stir and heat to 80°C at a rate of 300 r / min, and stir and react for 0.5 h to obtain a precursor slurry. The weight ratio of the low modulus sodium silicate solution, water and lime milk is 1:1.3:1.5.

[0095] 6) The precursor slurry is centrifuged and filtered, and the filter cake obtained by centrifugation is reversely washed three times, and then water is added to the filter cake obtained by washing and pulped for 40 minutes. The pulping liquid obtained by pulping is stirred and heated to 95°C at a rate of 600r / min for use. The total water consumption for reverse washing is 3 times the mass of the filter cake obtained by centrifugation. The amount of water added in the pulping operation is 1.5 times the mass of the filter cake obtained by washing.

[0096] 7) Adding aluminum sulfate as a dealkalizing agent to the pulping liquid, reacting for 1 hour at a temperature of 95°C and a rotation speed of 600 r / min, to obtain a low-pH pulp with a pH of 8-11. The amount of the dealkalizing agent added is 20 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200 parts.

[0097] 8) Adding a glycerol-zinc nitrate dehydration system and a solubility inhibitor to the low pH slurry, heating the resulting mixed system to 100° C., and reacting at a speed of 600 r / min for 0.5 h; adding a coating agent to the reacted mixed system, and continuing to react at a temperature of 100° C. and a speed of 600 r / min for 0.5 h to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0098] The added amount of the glycerol is 10 parts by weight, the added amount of zinc nitrate is 1 part by weight, the added amount of the solubility inhibitor sodium polyacrylate is 1 part by weight, and the added amount of the coating agent polyamide polyamine epichlorohydrin is 3 parts by weight.

[0099] 9) filtering the calcium silicate-calcium sulfate hemihydrate composite material suspension while hot, drying and breaking up the filter cake obtained by filtration, and the obtained calcium silicate-calcium sulfate hemihydrate composite material is the composite papermaking functional material.

[0100] Embodiment 4:

[0101] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that: in step 7), the amount of the dealkalizing agent added is 20 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200 parts; in step 8), the amount of glycerol added is 8 parts by weight, the amount of zinc nitrate added is 1 part by weight, the amount of solubility inhibitor sodium polyacrylate added is 1 part by weight, and the amount of the coating agent polyamide polyamine epichlorohydrin added is 3 parts by weight.

[0102] Embodiment 5:

[0103] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that: in step 7), the amount of the dealkalizing agent added is 15 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200 parts; in step 8), the amount of glycerol added is 10 parts by weight, the amount of zinc nitrate added is 1 part by weight, the amount of solubility inhibitor sodium polyacrylate added is 2 parts by weight, and the amount of the coating agent polyamide polyamine epichlorohydrin added is 3 parts by weight.

[0104] Embodiment 6:

[0105] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that: in step 7), the amount of the dealkalizing agent added is 10 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200 parts; in step 8), the amount of glycerol added is 10 parts by weight, the amount of zinc nitrate added is 1 part by weight, the amount of solubility inhibitor sodium polyacrylate added is 1 part by weight, and the amount of the coating agent polyamide polyamine epichlorohydrin added is 3 parts by weight.

[0106] Embodiment 7:

[0107] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that: in step 7), the amount of the dealkalizing agent added is 5 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200 parts; in step 8), the amount of glycerol added is 10 parts by weight, the amount of zinc nitrate added is 1 part by weight, the amount of solubility inhibitor sodium polyacrylate added is 1 part by weight, and the amount of the coating agent polyamide polyamine epichlorohydrin added is 3 parts by weight.

[0108] Embodiment 8:

[0109] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that:

[0110] In step 8), a glycerol-zinc nitrate dehydration system, a solubility inhibitor, and a crystal stabilizer are added to the low pH slurry, the resulting mixed system is heated to 100° C., and reacted at a speed of 600 r / min for 0.5 h; a coating agent is added to the reacted mixed system, and the reaction is continued for 0.5 h at a temperature of 100° C. and a speed of 600 r / min to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0111] The amount of glycerol added is 10 parts by weight, the amount of zinc nitrate added is 1 part by weight, the amount of solubility inhibitor sodium polyacrylate added is 1 part by weight, the amount of crystal stabilizer added is 1 part by weight, and the amount of coating agent polyamide polyamine epichlorohydrin added is 3 parts by weight. The crystal stabilizer contains nitroethanol and triethanolamine in a weight ratio of 1:1.

[0112] Comparative Example 1:

[0113] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that:

[0114] Step 6) directly add the glycerol-zinc nitrate dehydration system and the solubility inhibitor to the obtained pulping liquid, heat the obtained mixed system to 100°C, and react at a speed of 600r / min for 0.5h; add the coating agent to the mixed system after the reaction, and continue to react at a temperature of 100°C and a speed of 600r / min for 0.5h to obtain a composite material suspension; filter the composite material suspension while hot, dry and break up the filter cake obtained by filtration, and the obtained composite material is a composite papermaking functional material. That is, in this comparative example, the precursor slurry obtained by the dynamic hydrothermal synthesis reaction is not subjected to a dealkalization operation.

[0115] Comparative Example 2:

[0116] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that:

[0117] In step 8), a solubility inhibitor is added to the low pH slurry, the resulting mixed system is heated to 100°C, and the reaction is carried out at a speed of 600r / min for 0.5h; a coating agent is added to the mixed system after the reaction, and the reaction is continued for 0.5h at a temperature of 100°C and a speed of 600r / min to obtain a calcium silicate-calcium sulfate composite material suspension. The amount of the solubility inhibitor sodium polyacrylate added is 1 part by weight, and the amount of the coating agent polyamide polyamine epichlorohydrin added is 3 parts by weight. That is, in this comparative example, the glycerol-zinc nitrate dehydration system is not added to the low pH slurry.

[0118] Comparative Example 3:

[0119] A method for preparing a composite papermaking functional material comprises the following steps:

[0120] Step 1) is consistent with step 1) in Example 3;

[0121] Step 2) is consistent with step 2) in Example 3;

[0122] Step 3) is consistent with step 3) in Example 3;

[0123] Step 4) is consistent with step 4) in Example 3;

[0124] Step 5) is consistent with step 5) in Example 3;

[0125] Step 6), the precursor slurry is centrifuged and filtered, and the filter cake obtained by centrifugation is reverse washed 3 times until the Na2O content in the wet filter cake after washing is less than 2%, and the dealkalization is completed. At this time, the total water consumption of the reverse washing is 10 times the mass of the filter cake obtained by centrifugation. Then water is added to the filter cake obtained by washing and pulping is performed for 40 minutes, and the pulping liquid obtained by pulping is stirred and heated to 95°C at a rate of 600r / min for standby use. The amount of water added in the pulping operation is 1.5 times the mass of the filter cake obtained by washing.

[0126] Step 7) is consistent with step 8) in Example 3;

[0127] Step 8) is consistent with step 9) in Example 3.

[0128] That is, in this comparative example, water washing and de-alkalization operation were adopted, and no de-alkalization agent was used.

[0129] Comparative Example 4:

[0130] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that:

[0131] In step 8), a glycerol-zinc nitrate dehydration system, a solubility inhibitor, and a crystal stabilizer are added to the low pH slurry, the resulting mixed system is heated to 100° C., and reacted at a speed of 600 r / min for 0.5 h; a coating agent is added to the reacted mixed system, and the reaction is continued for 0.5 h at a temperature of 100° C. and a speed of 600 r / min to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0132] The added amount of the above-mentioned glycerol is 10 parts by weight, the added amount of zinc nitrate is 1 part by weight, the added amount of the solubility inhibitor sodium polyacrylate is 1 part by weight, the added amount of the crystal stabilizer-nitroethanol is 1 part by weight, and the added amount of the coating agent polyamide polyamine epichlorohydrin is 3 parts by weight.

[0133] Comparative Example 5:

[0134] A method for preparing a composite papermaking functional material, which is different from Example 3 only in that:

[0135] In step 8), a glycerol-zinc nitrate dehydration system, a solubility inhibitor, and a crystal stabilizer are added to the low pH slurry, the resulting mixed system is heated to 100° C., and reacted at a speed of 600 r / min for 0.5 h; a coating agent is added to the reacted mixed system, and the reaction is continued for 0.5 h at a temperature of 100° C. and a speed of 600 r / min to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension.

[0136] The added amount of the above-mentioned glycerol is 10 parts by weight, the added amount of zinc nitrate is 1 part by weight, the added amount of the solubility inhibitor sodium polyacrylate is 1 part by weight, the added amount of the crystal stabilizer-triethanolamine is 1 part by weight, and the added amount of the coating agent polyamide polyamine epichlorohydrin is 3 parts by weight.

[0137] Test Example 1:

[0138] pH testing of finished composite materials

[0139] Test method: The finished composite materials obtained in Examples 3 to 7 and Comparative Examples 1 to 3 were used as test samples. 10 g of each test sample was taken, and each test sample was prepared into a 10 g / 100 mL mixed solution. The pH value was measured, and the results are shown in Table 1. Three parallels were set for each test group, and the average value was taken.

[0140] Table 1

[0141] Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example 1 Comparative Example 2 Comparative Example 3 pH 9.52 9.50 10.15 10.68 10.12 11.98 9.51 12.73

[0142] It can be seen from the results in the above table that with the decrease of the content of aluminum sulfate in the dealkalizing agent, the pH of the composite material increases significantly, indicating that the dealkalizing agent aluminum sulfate plays a role in reducing the pH of the product during the reaction. However, if the pH of the papermaking filler is too high, it will destroy the dynamic balance of the pulp and increase the cost of papermaking. Therefore, using a dealkalizing agent to reduce the pH of the functional material for papermaking is beneficial to reducing the cost of papermaking. Although no dehydration system was added during the preparation process of Comparative Example 2, it did not affect the dealkalizing effect of the dealkalizing agent. In Comparative Example 3, a water washing and de-alkalization operation was used, and the pH of the composite material obtained was significantly higher than that of other test groups, and the total water consumption for washing in Comparative Example 3 was 10 times the mass of the filter cake obtained by centrifugation, while the total water consumption for reverse washing in Example 3 was 3 times the mass of the filter cake obtained by centrifugation. It can be seen that the addition of a dealkalizing agent can significantly reduce the amount of water used for washing, and at the same time, it can also reduce the amount of washing wastewater treated and the treatment cost.

[0143] Test Example 2:

[0144] Paper performance test

[0145] Test method: The finished composite materials obtained in Examples 3 to 7 and Comparative Example 2 were used as test samples. Each test sample was used to make paper, and a commercially available calcium silicate filler with a pH of 9.84 was used as a control group. The obtained paper was tested for performance according to the provisions of GB / T20810-2018. The results are shown in Table 2. Three parallels were set for each test group, and the average value was taken.

[0146] The papermaking steps of each test sample are as follows:

[0147] 1) After the chemical coniferous wood pulp and the chemical hardwood wood pulp are pulped, water is added to dilute them respectively until the pulp mass concentration reaches 10-12%, and then the chemical coniferous wood pulp and the chemical hardwood wood pulp are mixed in a mass ratio of 1:4, and then the pulp is refined. After the pulping is completed, the refined pulp is diluted with water to obtain a diluted pulp with a beating degree of 30° SR;

[0148] 2) Add 30 wt% of papermaking filler to the diluted slurry and mix well to form papermaking pulp. Add the additive to the papermaking pulp and mix with the papermaking pulp for 20-40 seconds before forming on the net. The papermaking is 70 g / m 2 In the above papermaking filler, the mass ratio of the test sample to talcum powder is 2:1. The auxiliary agent includes 3wt% of sizing agent AKD stock solution and 0.003wt% of retention agent cationic polyacrylamide.

[0149] Table 2

[0150]

[0151] It should be noted that, from the results in Table 1, it can be seen that the pH values ​​of the composite materials of Comparative Examples 1 and 3 are too high. The higher pH value of papermaking fillers will destroy the pH balance of pulp and increase papermaking costs, so no paper testing experiments were conducted.

[0152] As shown in Table 2, in Comparative Example 2, since the dehydration system glycerol-zinc nitrate was not added, the tensile index, tear index, bulk and whiteness of the obtained paper were significantly lower than those of other test groups. The results of Comparative Example 3 and Example 4 show that as the amount of glycerol added in the dehydration system decreases, the performance of the paper decreases. This may be caused by the fact that the mixed system of the dehydration reaction cannot achieve complete dehydration, and the content of the obtained calcium sulfate hemihydrate decreases. Therefore, the amount of glycerol and zinc nitrate added to the dehydration system cannot be too small to avoid losing the dehydration effect. The results of Comparative Example 3 and Example 5-Example 7 show that as the amount of dealkalizer added decreases, the performance of the paper decreases. It can be seen that the amount of dealkalizer is proportional to the amount of calcium sulfate hemihydrate generated. Therefore, too low an amount of dealkalizer added will reduce the performance of the composite papermaking functional material and paper of the present invention, but the performance of the paper can also be regulated by adjusting the amount of dealkalizer added.

[0153] By comparing the results of Example 3 and the control group, it was found that the composite papermaking functional material of the present invention has better compatibility and bonding with pulp when adding fillers due to the composite effect of calcium silicate and calcium sulfate hemihydrate, compared with calcium silicate fillers, and can more significantly improve the tensile strength and tear index of paper, and also improve the bulk and whiteness values ​​of paper to a certain extent. It can be seen that the composite papermaking functional material of the present invention has better application prospects.

[0154] Test Example 3:

[0155] Test method: The finished composite materials obtained in Example 3, Example 8 and Comparative Examples 4 and 5 were used as test samples. The pH of the finished composite materials of Example 8 and Comparative Examples 4-5 was measured according to the method in Test Example 1. Paper was made according to the method in Test Example 2, and the performance of the obtained paper was tested according to the provisions of GB / T20810-2018. The results are shown in Figure 1. Figure 1 , as shown in Table 3. Each test group was set up with 3 parallels, and the average value was taken.

[0156] At the same time, according to the operation of step 7) to step 9) in Example 3 and Example 8, a hemihydrate calcium sulfate product was prepared using an equal amount of calcium sulfate dihydrate from the same batch, and the prepared hemihydrate calcium sulfate product was subjected to microstructural analysis, specifically using SEM to analyze the microscopic morphology of the crystals.

[0157] Figure 1 The SEM photos of the finished composite materials of Example 3 and Example 8 are shown in Figure 1, A-Example 3, B-Example 8. The results show that compared with the crystals of Example 3, the crystals of Example 8 are transformed from the long columnar bodies of Example 3 to short columnar bodies with better integrity, indicating that the crystal stabilizer in Example 8 inhibits the longitudinal development of the columnar bodies, making the longitudinal and lateral differences smaller, which helps to improve the crystal stability and gelling effect.

[0158] Table 3

[0159] Example 8 Comparative Example 4 Comparative Example 5 pH of finished composite material 9.53 9.51 9.55 Tensile strength N·m / g 43.3 40.9 41.3 <![CDATA[Tear index mN·m 2 / g]]> 10.76 9.98 10.04 <![CDATA[Bulk thickness cm 3 / g]]> 2.76 2.77 2.75 Whiteness % 96.3 96.1 96.0

[0160] As shown in Table 3, the pH of the finished composite materials obtained in Example 8, Comparative Examples 4 and 5 is not significantly different from that in Example 3, indicating that the crystal stabilizer does not affect the pH of the finished composite materials. When different composite materials are used for papermaking, the tensile strength and tear index of the paper obtained in Example 8 are improved compared with those in Example 3, while the bulk and whiteness are not significantly different from those in Example 3. The indicators of Comparative Example 4 and Example 3 are not significantly different. The indicators of Comparative Example 5 are slightly better than those of Example 3, but far less than the improvement in Example 8. It can be seen that the addition of the crystal stabilizer within the scope defined by the present invention does not affect the pH of calcium sulfate hemihydrate, but synergistically improves its crystal morphology, so that the composite papermaking functional material has better gelling properties, increases the filler retention rate, and thus improves the strength, folding resistance and burst resistance of the paper.

[0161] It should be noted that in the present invention, the detailed steps of some operations are not described in detail, but belong to the prior art known to those skilled in the art, so they will not be repeated here. In addition, in the present invention, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for simplicity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible secondary ranges and individual values ​​(including integers and fractions) within the range.

[0162] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. In the present invention, not all possible combinations of the various technical features in the various embodiments or embodiments are described. As long as there is no contradiction in the combination of these technical features, the various technical features in the various embodiments or embodiments can be arbitrarily combined, and all possible combinations should be considered to be within the scope of this specification. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some or all of the technical features therein can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a composite papermaking functional material, It is characterized in that include: 1) Providing low modulus sodium silicate solution and lime milk; The low modulus sodium silicate solution is prepared by alkali dissolution of quartz sand, and the lime milk is prepared by digestion of quicklime; 2) subjecting the low modulus sodium silicate solution and lime milk to a dynamic hydrothermal synthesis reaction to obtain a precursor slurry; 3) After the precursor slurry is centrifuged and beaten, a dealkalizing agent is used to dealkalize the resulting beaten liquid to obtain a low pH slurry; 4) providing a dehydration system, and utilizing a dehydration operation to convert the low pH slurry into a calcium silicate-calcium sulfate hemihydrate composite material suspension, wherein the calcium silicate-calcium sulfate hemihydrate composite material is the composite papermaking functional material; The dealkalizing agent is aluminum sulfate; the dehydration system includes glycerol and zinc nitrate; The dehydration operation process is as follows: 4.1) adding glycerol-zinc nitrate dehydration system and solubility inhibitor to the low pH slurry, heating the resulting mixed system to 90-110° C., and reacting at a speed of 300-600 r / min for 0.5-1 h; 4.2) adding a coating agent to the mixed system after the reaction, and continuing the reaction for 0.5-1h at a temperature of 90-110°C and a rotation speed of 300-600r / min to obtain a calcium silicate-calcium sulfate hemihydrate composite material suspension; In the dehydration operation, the amount of glycerol added is 5-10 parts by weight, the amount of zinc nitrate added is 1-2 parts by weight, the amount of solubility inhibitor added is 1-3 parts by weight, and the amount of coating agent added is 1-5 parts by weight; The solubility inhibitor is selected from at least one of sodium dodecylbenzene sulfonate, sodium citrate, fatty alcohol polyoxyethylene ether, polyoxyethylene ethyl ether, potassium sodium tartrate, fatty alcohol sodium sulfate, polyethylene glycol, sodium tripolyphosphate, sodium pyrophosphate, sodium hexametaphosphate, and sodium polyacrylate; The coating agent is selected from at least one of phenolic resin, urea-formaldehyde resin and polyamide polyamine epichlorohydrin.

2. The method for preparing the composite papermaking functional material according to claim 1, It is characterized in that The modulus of the low modulus sodium silicate solution is 1.0-1.2, wherein SiO 2 The concentration is 40-70g / L.

3. The method for preparing the composite papermaking functional material according to claim 1, It is characterized in that The dynamic hydrothermal synthesis reaction process is as follows: after heating the low modulus sodium silicate solution to 75-80°C, adding lime milk and water thereto, stirring and heating to 75-80°C at a rate of 300-600r / min, keeping the temperature and stirring for 0.5-1h to obtain a precursor slurry; the weight ratio of the low modulus sodium silicate solution, water and lime milk is 1:(1-1.3):(1.5-2).

4. The method for preparing the composite papermaking functional material according to claim 1, It is characterized in that The centrifugal washing and beating operation process is as follows: the precursor slurry is centrifuged and filtered, the filter cake obtained by centrifugation is reversely washed 2-3 times, and then water is added to the filter cake obtained by washing and beating for 30-40 minutes, and the beating liquid obtained by beating is stirred and heated to 80-95°C at a rate of 300-600r / min for use; the total water consumption of the reverse washing is 2-3 times the mass of the filter cake obtained by centrifugation; the amount of water added in the beating operation is 1-1.5 times the mass of the filter cake obtained by washing.

5. The method for preparing the composite papermaking functional material according to claim 1, It is characterized in that The dealkalization operation process is as follows: add the dealkalizing agent aluminum sulfate to the pulping liquid, react for 1-1.5 hours at a temperature of 80-95°C and a rotation speed of 300-600r / min to obtain a low-pH pulp with a pH of 8-11; in the dealkalization operation, the amount of the dealkalizing agent added is 5-20 parts by weight, and the weight of the filter cake obtained by washing in the pulping liquid is 200-230 parts.

6. A composite papermaking functional material, It is characterized in that The composite papermaking functional material is prepared by the preparation method of the composite papermaking functional material according to any one of claims 1 to 5.

7. Application of a composite papermaking functional material in papermaking, It is characterized in that The composite papermaking functional material is prepared by the preparation method of the composite papermaking functional material according to any one of claims 1 to 5, and the composite papermaking functional material is added to papermaking slurry as a papermaking filler.

Citation Information

Patent Citations

  • Method for lowering pH value of active calcium silicate

    CN102190309A

  • Application of synthetic calcium carbonate as high paper filler and preparation method of high paper filler

    CN107287980A