Adhesive sheet

A pressure-sensitive adhesive sheet using biomass-derived polyester resin addresses the environmental and processability limitations of existing adhesive sheets by ensuring a high biomass content and rigidity, enhancing its adhesive performance and suitability for electronic device applications.

JP7562241B2Active Publication Date: 2024-10-07NITTO DENKO CORP
View PDF 22 Cites 0 Cited by

Patent Information

Application Number
JP2019054306
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-03-22
Publication Date
2024-10-07
Estimated Expiration
2039-03-22

AI Technical Summary

Technical Problem

Existing adhesive sheets rely heavily on fossil resource-based materials, and there is a lack of practical applications using polyester resin derived from biomass resources, which limits their environmental sustainability and processability.

Method used

A pressure-sensitive adhesive sheet is developed using a polyester resin derived from biomass resources, with both the adhesive layer and base layer containing biomass-derived carbon, ensuring at least 50% of the total carbon is biomass-based, and the base layer has a thickness ratio of 10% or more to the total sheet, providing high rigidity and processability.

Benefits of technology

The adhesive sheet reduces dependence on fossil resources, enhances processability, and exhibits excellent adhesive properties, including high shear strength and peelability, making it suitable for thin applications in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562241000002
    Figure 0007562241000002
  • Figure 0007562241000003
    Figure 0007562241000003
  • Figure 0007562241000004
    Figure 0007562241000004
Patent Text Reader

Abstract

To provide an adhesive sheet having good workability, the adhesive sheet as a whole having reduced dependency on fossil resources.SOLUTION: This adhesive sheet is provided with a substrate layer containing a polyester resin and an adhesive layer disposed on at least one surface of the substrate layer. At least 50% of the total carbon contained in the adhesive layer is biomass-derived carbon. Moreover, the polyester resin contains biomass-derived carbon.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet. [Background technology]

[0002] Generally, adhesives (also called pressure-sensitive adhesives; the same applies below) are in a soft solid (viscoelastic) state in a temperature range around room temperature, and have the property of easily adhering to an adherend by pressure. Taking advantage of such properties, adhesives, for example in the form of supported adhesive sheets having an adhesive layer on a support, are widely used as a joining means with good workability and high adhesive reliability in various industrial fields such as home appliances, automobiles, various machines, electrical appliances, and electronic devices. Adhesive sheets are preferably used, for example, for fixing members in electronic devices such as mobile phones, smartphones, and tablet computers. Patent documents 1 and 2 are cited as documents disclosing this type of prior art. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6104500 [Patent Document 2] JP 2015-221847 A [Patent Document 3] Patent No. 5316725 [Patent Document 4] International Publication No. 2016 / 186122 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, environmental issues such as global warming have come to be emphasized, and it is desirable to reduce the amount of fossil resource-based materials such as petroleum used. Adhesive sheets are no exception. Focusing on adhesives, natural rubber and rosin are known as materials with a high bio-based degree. By modifying or denaturing these natural resource-derived materials, it is possible to obtain adhesive properties (adhesive retention, heat resistance, etc.) suitable for specific applications such as electronic device applications while maintaining a certain level of bio-based degree. In addition, adhesive sheets with substrates are widely used, which are more advantageous than substrate-less adhesive sheets in terms of punching processability into complex shapes and improving yield during processing. Turning to the substrate material, polyolefins and polylactic acid derived from biomass resources are known, but polyolefins have low rigidity, so there are limitations to their use in applications where thinness is required, such as electronic device applications. Polylactic acid has low strength and tends to be inferior in formability compared to general-purpose plastics, and there are also limitations to the places where it can be applied.

[0005] For polyester resins such as polyethylene terephthalate (PET), those in which the diol used in synthesis is derived from biomass resources have been reported (for example, Patent Documents 3 and 4). However, as described in Patent Documents 3 and 4, ingenuity is required to obtain performance equivalent to that of fossil resource-based materials, and since the contribution to the bio-based degree is small compared to the increased cost, the study of practical application has not progressed. At present, no adhesive sheet using a polyester resin derived from biomass resources has been reported. Therefore, the present inventors have conducted intensive research and created a novel adhesive sheet having practical value using a polyester resin derived from biomass resources. Specifically, the present invention aims to provide an adhesive sheet that can reduce the dependency on fossil resource materials as a whole adhesive sheet by using a polyester resin derived from biomass resources and has good processability. [Means for solving the problem]

[0006] According to the present specification, there is provided a pressure-sensitive adhesive sheet comprising a base layer containing a polyester resin and a pressure-sensitive adhesive layer disposed on at least one surface of the base layer. At least 50% of the total carbon contained in the pressure-sensitive adhesive layer is biomass-derived carbon. The polyester resin also contains biomass-derived carbon. The pressure-sensitive adhesive sheet uses biomass materials for both the pressure-sensitive adhesive layer and the base layer, so that the pressure-sensitive adhesive sheet as a whole can reduce its dependency on fossil resource-based materials. The pressure-sensitive adhesive sheet also has good processability because it has a polyester resin-containing base layer. Specifically, a configuration including a polyester resin-containing base layer makes it easy to punch out a complex shape, and can improve the yield during processing. Such a configuration also tends to have excellent reworkability (peelability) in the event of a failure to attach the sheet. Excellent peelability is also advantageous in terms of recyclability. Furthermore, the polyester resin-containing base layer tends to have high rigidity, making it easy to make the pressure-sensitive adhesive sheet thinner.

[0007] In some preferred embodiments, the ratio of the thickness of the base layer to the total thickness of the pressure-sensitive adhesive sheet is 10% or more. By making the ratio of the thickness of the base layer having a relatively high rigidity equal to or greater than a predetermined value, the ratio of the thickness of the pressure-sensitive adhesive layer is reduced, making it easier to prevent blocking of the pressure-sensitive adhesive, thereby improving processability.

[0008] In some preferred embodiments, the breaking strength of the base layer is 200 MPa or more. By using a base layer having a breaking strength equal to or greater than a certain level, excellent processability is easily obtained, and the pressure-sensitive adhesive sheet can be easily thinned.

[0009] In some preferred embodiments, 50% or more of the total carbon contained in the pressure-sensitive adhesive sheet is biomass-derived carbon. According to the technology disclosed herein, by using biomass materials for both the pressure-sensitive adhesive layer and the substrate layer constituting the pressure-sensitive adhesive sheet, the proportion of biomass-derived carbon in the total carbon contained in the entire pressure-sensitive adhesive sheet can be made 50% or more. In a configuration including a pressure-sensitive adhesive layer and a substrate layer, the amount of fossil resource-based materials used can be effectively reduced.

[0010] In some preferred embodiments, the ratio of the thickness of the substrate layer to the total thickness of the pressure-sensitive adhesive sheet is 50% or less. Biomass carbonization of a polyester resin-containing substrate layer is more difficult in terms of technology, economy, quality, etc. than biomass carbonization of a pressure-sensitive adhesive layer. Therefore, reducing the ratio of the polyester resin-containing substrate layer to the entire pressure-sensitive adhesive sheet can be a realistic and suitable option for reducing the dependency of the pressure-sensitive adhesive sheet as a whole on fossil resource-based materials while maintaining the desired adhesive properties.

[0011] In some preferred embodiments, 5% or more of the total carbon contained in the substrate layer is biomass-derived carbon. By employing a substrate layer containing a predetermined amount or more of biomass-derived carbon, the PSA sheet as a whole can preferably reduce its dependency on fossil resource-based materials.

[0012] Some preferred embodiments of the PSA sheet exhibit a shear adhesive strength of 1.8 MPa or more. PSA sheets that use a predetermined amount or more of biomass material and can exhibit high shear adhesive strength can reduce the environmental impact in various applications that require performance such as adhesive retention.

[0013] The pressure-sensitive adhesive sheet disclosed herein is preferably a double-sided pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive layers are provided on both sides of the base layer. The double-sided pressure-sensitive adhesive sheet is suitable for applications such as fixing parts.

[0014] The adhesive sheet disclosed herein is capable of exhibiting adhesive properties suitable for various applications, has good processability, and can be used to thin the substrate, making it particularly suitable for use in fixing components in electronic devices, which tend to require adhesive properties such as adhesion retention and space saving. In electronic device applications, which are mass-produced, consumed, and obsolete, reducing the environmental load by reducing dependency on fossil resource-based materials has a large impact. [Brief description of the drawings]

[0015] [Figure 1]1 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to an embodiment. [Diagram 2] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to another embodiment. [Diagram 3] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to another embodiment. [Figure 4] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to another embodiment. [Diagram 5] FIG. 2 is an explanatory diagram showing a schematic diagram of a method for measuring a shear adhesive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Preferred embodiments of the present invention will be described below. Matters necessary for carrying out the present invention other than those specifically mentioned in this specification can be understood by those skilled in the art based on the teachings on carrying out the invention described in this specification and the common general technical knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general technical knowledge in the relevant field. In the following drawings, components and parts having the same function may be denoted by the same reference numerals, and duplicated descriptions may be omitted or simplified. In addition, the embodiments shown in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the pressure-sensitive adhesive sheet of the present invention that is actually provided as a product.

[0017] The concept of the adhesive sheet here may include those called adhesive tape, adhesive label, adhesive film, etc. The adhesive layer is typically formed continuously, but is not limited to such a form, and may be an adhesive layer formed in a regular or random pattern such as a dotted or striped pattern. The adhesive sheet disclosed herein may be in the form of a roll or a sheet. Alternatively, it may be an adhesive sheet in the form of a processed form into various shapes.

[0018] In addition, in this specification, the term "adhesive" refers to a material that exhibits a soft solid (viscoelastic) state in a temperature range around room temperature and has the property of easily adhering to an adherend by pressure, as described above. The adhesive referred to here is generally a material having a complex tensile modulus E * (1Hz)<10 7 dyne / cm 2 The material may be a material having the properties satisfying the above (typically, a material having the above properties at 25°C).

[0019] <Composition of adhesive sheet> The adhesive sheet disclosed herein comprises a base layer containing a polyester resin, and an adhesive layer disposed on at least one surface of the base layer. The adhesive sheet may be an adhesive sheet having the adhesive layer on one or both surfaces of a non-releasable base (support base). The adhesive sheet may have, for example, a cross-sectional structure as shown in Figs. 1 to 4. The structure of an adhesive sheet according to one embodiment is shown typically in Fig. 1. An adhesive sheet 1 according to this embodiment is configured as an adhesive sheet with a substrate having single-sided adhesiveness. Before use (i.e., before attachment to an adherend), the adhesive sheet 1 has an adhesive layer 21 provided on one surface 10A (non-releasable) of a base layer 10, and a surface (adhering surface) 21A of the adhesive layer 21 protected by a release liner 31, at least the adhesive layer side of which is a release surface.

[0020] The structure of an adhesive sheet according to another embodiment is shown typically in Fig. 2. Like the adhesive sheet 1 in Fig. 1, the adhesive sheet 2 according to this embodiment is also configured as a one-sided adhesive substrate-attached adhesive sheet, and has a configuration in which an adhesive layer 21 is provided on one surface 10A (non-releasable) of a substrate layer 10. In this adhesive sheet 2, the other surface 10B of the substrate layer 10 is a release surface, and before use, when the adhesive sheet 2 is rolled up, the adhesive layer 21 comes into contact with the other surface 10B, and the surface (adhering surface) 21B of the adhesive layer is protected by the other surface 10B of the substrate layer 10.

[0021] The structure of an adhesive sheet according to yet another embodiment is shown diagrammatically in Fig. 3. An adhesive sheet 3 according to this embodiment is configured as a double-sided adhesive type adhesive sheet with a substrate. The adhesive sheet 3 has adhesive layers 21, 22 provided on each side (both of which are non-removable) of a substrate layer 10. Before use, the adhesive sheet 3 has a configuration in which the adhesive layers are protected by release liners 31, 32, at least the adhesive layer side of which serves as a release surface.

[0022] The structure of a pressure-sensitive adhesive sheet according to yet another embodiment is shown in FIG. 4. Like the pressure-sensitive adhesive sheet in FIG. 3, the pressure-sensitive adhesive sheet 4 according to this embodiment is configured as a double-sided adhesive type substrate-attached pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet 4 has pressure-sensitive adhesive layers 21, 22 provided on each side (both of which are non-removable) of a substrate layer 10, and prior to use, one of the pressure-sensitive adhesive layers 21 is protected by a release liner 31 having release surfaces on both sides. The pressure-sensitive adhesive sheet 4 can be configured such that the pressure-sensitive adhesive layer 22 is also protected by the release liner 31 by rolling the pressure-sensitive adhesive sheet 4 and abutting the other pressure-sensitive adhesive layer 22 against the back surface of the release liner 31.

[0023] <Adhesive layer> (Biomass carbon ratio) The pressure-sensitive adhesive sheet disclosed herein has a biomass carbon ratio (also referred to as biobased ratio) of the pressure-sensitive adhesive layer of 50% or more. A high biomass carbon ratio in the pressure-sensitive adhesive layer means that the amount of fossil resource-based materials, such as petroleum, used is small. From this perspective, the higher the biomass carbon ratio of the pressure-sensitive adhesive layer, the more preferable it is. For example, the biomass carbon ratio of the pressure-sensitive adhesive layer may be 60% or more, 70% or more, 75% or more, or 80% or more. The upper limit of the biomass carbon ratio is 100% by definition, and typically the biomass carbon ratio is less than 100%. From the viewpoint of making it easier to obtain shear adhesive strength, in some embodiments, the biomass carbon ratio of the pressure-sensitive adhesive layer may be, for example, 95% or less, and when adhesive performance is more important, it may be 90% or less, or 85% or less.

[0024] Here, in this specification, "biomass-derived carbon" (sometimes abbreviated as "biomass carbon") means carbon (renewable carbon) contained in biomass materials, i.e., materials derived from renewable organic resources. The above-mentioned biomass materials typically refer to materials derived from biological resources (typically plants that perform photosynthesis) that can be sustainably reproduced in the presence of sunlight, water, and carbon dioxide. Therefore, materials derived from fossil resources that are depleted through use after mining (fossil resource-based materials) are excluded from the concept of biomass materials as used here.

[0025] In addition, in this specification, the "biomass carbon ratio" (also referred to as "biobased degree") refers to the proportion of biomass carbon in the total carbon in the object to be measured (sample), and is measured based on ASTM D6866. Among the methods described in ASTM D6866, Method B, which has high accuracy, is preferred. The same applies to the biobased degrees of the adhesive layer, base layer and adhesive sheet described below. In this specification, the biomass carbon ratio is a ratio relative to a reference value (Modern Reference Standard) determined by a standard substance. 14 This value is calculated from the C concentration ratio (unit: pMC (percent Modern Carbon)).

[0026] In the technology disclosed herein, the type of adhesive constituting the adhesive layer is not particularly limited as long as it satisfies a bio-based degree of 50% or more. The above-mentioned adhesive (which may be an adhesive composition) may contain one or more of various rubber-like polymers such as acrylic polymers, rubber polymers, polyester polymers, urethane polymers, polyether polymers, silicone polymers, polyamide polymers, and fluorine polymers known in the field of adhesives. From the viewpoint of adhesive performance, cost, and the like, an adhesive containing a rubber polymer as a main component (rubber-based adhesive) is preferred. Examples of rubber-based adhesives include natural rubber-based adhesives and synthetic rubber-based adhesives, and modified rubber-based adhesives such as acrylic-modified natural rubber may also be preferably used. The bio-based degree of the adhesive layer can be adjusted depending on the type of polymer constituting the adhesive and its content ratio.

[0027] In some embodiments, the adhesive sheet includes an adhesive layer made of a natural rubber-based adhesive. A natural rubber-based adhesive refers to an adhesive in which more than 50% by weight of the base polymer of the adhesive is one or more polymers selected from natural rubber and modified natural rubber (hereinafter also referred to as natural rubber-based polymer). The base polymer of the adhesive refers to a rubber-like polymer contained in the adhesive, and is not otherwise limited in any way in terms of, for example, the content or the relationship with other components. The rubber-like polymer refers to a polymer that exhibits rubber elasticity in a temperature range around room temperature. The base polymer of the adhesive may contain, in addition to the natural rubber-based polymer, a polymer other than the natural rubber-based polymer as a secondary component. Examples of polymers other than the natural rubber-based polymer include acrylic polymers, synthetic rubber polymers, polyester polymers, urethane polymers, polyether polymers, silicone polymers, polyamide polymers, fluorine-based polymers, and the like, which are well known in the field of adhesives.

[0028] In some preferred embodiments, 20% by weight or more of all repeating units constituting the base polymer of the pressure-sensitive adhesive are repeating units derived from acrylic monomers. That is, 20% by weight or more of the total weight of the base polymer is derived from acrylic monomers. Hereinafter, the ratio of the weight derived from acrylic monomers to the total weight of the base polymer is also referred to as the "acrylic ratio". By including a certain amount or more of repeating units derived from acrylic monomers in the base polymer, the cohesive strength of the natural rubber-based pressure-sensitive adhesive can be increased, and for example, the shear adhesive strength can be improved without the necessity of using a vulcanizing agent or a sulfur-containing vulcanization accelerator.

[0029] From the viewpoint of improving the cohesive strength of the adhesive, the acrylic ratio of the base polymer may be, for example, more than 20% by weight, preferably 24% by weight or more, may be 28% by weight or more, or may be 33% by weight or more. From the viewpoint of placing more importance on the cohesive strength, in some embodiments, the acrylic ratio of the base polymer may be 35% by weight or more, may be 38% by weight or more, or may be 40% by weight or more. The upper limit of the acrylic ratio of the base polymer is set so that the biomass carbon ratio of the adhesive layer is 50% by weight or more. From the viewpoint of increasing the biomass carbon ratio of the adhesive layer, it is advantageous to have a lower acrylic ratio of the base polymer. From this viewpoint, the acrylic ratio of the base polymer is suitably less than 70% by weight, preferably less than 60% by weight, may be less than 55% by weight, or may be less than 50% by weight. From the viewpoint of increasing the biomass carbon ratio, in some embodiments, the acrylic ratio of the base polymer may be less than 45% by weight, may be less than 42% by weight, or may be less than 39% by weight.

[0030] The repeating unit derived from the acrylic monomer contained in the base polymer may be a repeating unit constituting the acrylic-modified natural rubber. The pressure-sensitive adhesive sheet disclosed herein can be preferably implemented in an embodiment in which the base polymer of the pressure-sensitive adhesive contains the acrylic-modified natural rubber. Here, the acrylic-modified natural rubber refers to natural rubber graft-polymerized with an acrylic monomer. The pressure-sensitive adhesive of this embodiment may further contain a base polymer (e.g., natural rubber) that does not contain a repeating unit derived from the acrylic monomer. In addition, the base polymer of the pressure-sensitive adhesive may further contain a repeating unit derived from the acrylic monomer as a repeating unit constituting a polymer other than the acrylic-modified natural rubber.

[0031] In this specification, the acrylic monomer refers to a monomer having at least one (meth)acryloyl group in one molecule. Here, "(meth)acryloyl" refers to acryloyl and methacryloyl in a comprehensive sense. Therefore, the concept of the acrylic monomer here can include both a monomer having an acryloyl group (acrylic monomer) and a monomer having a methacryloyl group (methacrylic monomer).

[0032] In the acrylic modified natural rubber, the acrylic monomer to be graft polymerized to the natural rubber is not particularly limited, and examples thereof include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 8 carbon atoms at the ester end, such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; (meth)acrylic acid; and the like. These can be used alone or in combination of two or more. Acrylic monomers preferred from the viewpoint of improving cohesive strength include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 2 carbon atoms at the ester end and (meth)acrylic acid. Acrylic monomers not containing a carboxy group are advantageous from the viewpoint of reducing corrosiveness, and from this viewpoint, (meth)acrylic acid alkyl esters are preferred. Among them, methyl methacrylate (MMA) and ethyl methacrylate are preferred, and MMA is particularly preferred.

[0033] The proportion of the weight of the repeating unit derived from an acrylic monomer in the total weight of the acrylic-modified natural rubber (hereinafter also referred to as the acrylic modification rate) is not particularly limited as long as it is in the range of more than 0% by weight and less than 100% by weight. From the viewpoint of enhancing the effect of improving the cohesive strength, the acrylic modification rate of the acrylic-modified natural rubber is suitably 1% by weight or more, and may be 5% by weight or more, 10% by weight or more, or 15% by weight or more. From the viewpoint of obtaining a higher cohesive strength, in some embodiments, the acrylic modification rate may be, for example, more than 20% by weight, 24% by weight or more, 28% by weight or more, 33% by weight or more, 35% by weight or more, 38% by weight or more, or 40% by weight or more. From the viewpoint of increasing the biomass carbon ratio, the acrylic modification rate of the acrylic-modified natural rubber is suitably less than 80% by weight, and is preferably less than 70% by weight, and may be less than 60% by weight, less than 55% by weight, less than 50% by weight, or less than 45% by weight.

[0034] The acrylic-modified natural rubber can be produced by a known method, or a commercially available product can be used. Examples of methods for producing the acrylic-modified natural rubber include a method of adding an acrylic monomer to natural rubber and polymerizing it, a method of mixing a pre-oligomerized acrylic monomer with natural rubber and adding it, and an intermediate method between these. The ratio of the amounts of natural rubber and the acrylic monomer used and other production conditions can be appropriately set so that an acrylic-modified natural rubber having a desired acrylic modification rate is obtained. The natural rubber used for producing the acrylic-modified natural rubber is not particularly limited, and can be appropriately selected from various commonly available natural rubbers such as ribbed smoked sheet (RSS), pale crepe, standard Malaysian rubber (SMR), and standard Vietnamese rubber (SVR). The natural rubber used in combination with the acrylic-modified natural rubber can also be selected from the same various natural rubbers. The natural rubber is typically used after mastication by a conventional method.

[0035] The Mooney viscosity of the natural rubber used to produce the acrylic modified natural rubber is not particularly limited. For example, the Mooney viscosity under the measurement condition of MS(1+4)100°C (i.e., Mooney viscosity MS 1+4 The Mooney viscosity MS of the natural rubber can be in the range of about 10 to 120 (100°C). 1+4 (100°C) may be, for example, 100 or less, 80 or less, 70 or less, or 60 or less. Mooney viscosity MS 1+4 When the Mooney viscosity MS (100°C) of the natural rubber is small, the initial tack tends to be easily developed. This is advantageous in terms of improving the workability of application to an adherend. From this viewpoint, in some embodiments, 1+4 (100°C) may be 50 or less, 40 or less, or 30 or less. Mooney viscosity MS 1+4 (100°C) can be adjusted by a common method such as mastication.

[0036] The addition of acrylic monomers to natural rubber can be carried out in the presence of a radical polymerization initiator. Examples of radical polymerization initiators include general peroxide initiators, azo initiators, and redox initiators that are a combination of peroxides and reducing agents. These can be used alone or in combination of two or more. Among them, peroxide initiators are preferred. Examples of peroxide initiators include diacyl peroxides, such as aromatic diacyl peroxides typified by benzoyl peroxide (BPO) and aliphatic diacyl peroxides such as dialkyloyl peroxides (e.g., dilauroyl peroxide). Other examples of peroxide initiators include t-butyl hydroperoxide, di-t-butyl peroxide, t-butyl peroxybenzoate, dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-bis(t-butylperoxy)cyclododecane. The peroxide initiators can be used alone or in combination of two or more.

[0037] The base polymer of the adhesive may contain only one or more kinds of acrylic-modified natural rubber, or may contain acrylic-modified natural rubber in combination with other polymers. The proportion of acrylic-modified natural rubber in the entire base polymer is not particularly limited and may be appropriately set within a range of more than 0% by weight to 100% by weight or less. In some embodiments, the proportion of acrylic-modified natural rubber may be, for example, 10% by weight or more, and from the viewpoint of obtaining good retention characteristics (e.g., high shear adhesive strength), it is advantageous to set it to 25% by weight or more, and preferably to 40% by weight or more. In some embodiments, the proportion of acrylic-modified natural rubber may be more than 50% by weight, may be 65% by weight or more, may be 80% by weight or more, or may be 90% by weight or more. Note that when only acrylic-modified natural rubber is used as the base polymer, the proportion of acrylic-modified natural rubber in the entire base polymer is 100% by weight.

[0038] As the polymer to be used in combination with the acrylic modified natural rubber, for example, a rubber-based polymer may be preferably adopted from the viewpoint of compatibility. As the rubber-based polymer, both natural rubber and synthetic rubber (for example, styrene-butadiene rubber, styrene-butadiene block copolymer, styrene-isoprene block copolymer, etc.) can be used. From the viewpoint of improving the biomass carbon ratio, it is particularly preferable to use natural rubber, which is a biomass material. The base polymer may contain only the acrylic modified natural rubber and natural rubber, or may contain a combination of the acrylic modified natural rubber, the natural rubber, and other polymers. In some embodiments, the proportion of the polymer other than the acrylic modified natural rubber and the natural rubber is suitably less than 30% by weight of the entire base polymer, preferably less than 20% by weight, and may be less than 10% by weight.

[0039] When natural rubber is used, the ratio of natural rubber to the total amount of acrylic modified natural rubber and natural rubber can be more than 0% by weight, for example, 5% by weight or more, 10% by weight or more, 25% by weight or more, or 40% by weight or more. By increasing the ratio of natural rubber, the biomass carbon ratio of the adhesive tends to improve. The ratio of natural rubber to the total amount of the acrylic modified natural rubber and natural rubber can be less than 100% by weight, and may be 95% by weight or less, 75% by weight or less, or 60% by weight or less. From the viewpoint of obtaining a higher shear adhesive strength, in some embodiments, the content ratio of the natural rubber may be 50% by weight or less, 45% by weight or less, 35% by weight or less, or 25% by weight or less.

[0040] Other polymers that can be used in combination with the acrylic modified natural rubber include acrylic polymers and polyester polymers. The acrylic polymers can be formed from monomer components that include monomers having carbon derived from biomass. As the polyester polymer, at least one of the polycarboxylic acid (typically dicarboxylic acid) and the polyol (typically diol) forming the polymer is preferably a compound that contains carbon derived from biomass in part or in whole, for example, a compound derived from a plant. As the dicarboxylic acid derived from biomass, for example, a dimer acid derived from an unsaturated fatty acid derived from a plant (sebacic acid, oleic acid, erucic acid, etc.) can be used. As the diol derived from biomass, for example, a dimer diol obtained by reducing the above dimer acid, or a biomass ethylene glycol obtained using biomass ethanol as a raw material can be used. The biomass carbon ratio of such a polyester polymer may be, for example, more than 40%, preferably more than 50%, and may be 70% or more, 85% or more, 90% or more, or 100%. From the standpoint of compatibility, etc., the content of the polyester-based polymer is suitably less than 20% by weight, preferably less than 10% by weight, and may be less than 5% by weight of the entire base polymer.

[0041] (Crosslinking agent) A crosslinking agent is preferably used in the adhesive layer of the adhesive sheet disclosed herein. The crosslinking agent can be useful for increasing the cohesive strength of the adhesive. This can effectively improve the shear adhesive strength. The crosslinking agent can be selected from various crosslinking agents known in the field of adhesives. Examples of such crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, and amine-based crosslinking agents. The crosslinking agents can be used alone or in combination of two or more.

[0042] The amount of the crosslinking agent used is not particularly limited. The amount of the crosslinking agent used may be selected from the range of, for example, 0.001 to 15 parts by weight relative to 100 parts by weight of the base polymer. From the viewpoint of achieving a good balance between improved cohesive strength and good adhesion to the adherend, the amount of the crosslinking agent used relative to 100 parts by weight of the base polymer is preferably 12 parts by weight or less, may be 8 parts by weight or less, may be 6 parts by weight or less, and is suitably 0.005 parts by weight or more, and may be 0.01 parts by weight or more.

[0043] The crosslinking agent is preferably selected from non-sulfur-containing crosslinking agents. Here, the non-sulfur-containing crosslinking agent means a crosslinking agent that does not contain sulfur (S) at least intentionally, and is therefore a material that is clearly distinguished from vulcanizing agents that are generally used as crosslinking agents for natural rubber. A crosslinking agent that contains a compound that does not contain sulfur as a constituent element as an active ingredient is a typical example of the non-sulfur-containing crosslinking agent referred to here. By using a non-sulfur-containing crosslinking agent as a crosslinking agent, it is possible to prevent sulfur derived from the crosslinking agent from being brought into the adhesive layer. This can be an advantageous feature in adhesive sheets used in the electronic device field, where the presence of sulfur is undesirable. It is preferable that the adhesive sheet disclosed herein does not use a vulcanizing agent in the adhesive layer.

[0044] In some embodiments, the crosslinking agent preferably includes at least an isocyanate-based crosslinking agent. The isocyanate-based crosslinking agent may be used alone or in combination of two or more. The isocyanate-based crosslinking agent may be used in combination with another crosslinking agent, such as an epoxy-based crosslinking agent.

[0045] As the isocyanate crosslinking agent, a polyisocyanate crosslinking agent having two or more isocyanate groups per molecule is preferably used. The number of isocyanate groups per molecule of the polyisocyanate crosslinking agent is preferably 2 to 10, for example, 2 to 4, typically 2 or 3. Examples of the polyisocyanate crosslinking agent include aromatic polyisocyanates such as tolylene diisocyanate and xylylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate; and aliphatic polyisocyanates such as hexamethylene diisocyanate. More specifically, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl diisocyanate; trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name "Coronate L"); "), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, trade name "Coronate HX") are examples of isocyanate adducts; polyisocyanates such as polyether polyisocyanate and polyester polyisocyanate; adducts of these polyisocyanates with polyols; and polyisocyanates obtained by multifunctionalizing these polyisocyanates with isocyanurate bonds, biuret bonds, allophanate bonds, and the like.

[0046] When an isocyanate-based crosslinking agent is used, the amount of the isocyanate-based crosslinking agent used may be, for example, about 0.1 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or more than 1.5 parts by weight, relative to 100 parts by weight of the base polymer. From the viewpoint of obtaining a higher use effect, the amount of the isocyanate-based crosslinking agent used relative to 100 parts by weight of the base polymer may be, for example, more than 2.0 parts by weight, 2.5 parts by weight or more, or 2.7 parts by weight or more. In addition, the amount of the isocyanate-based crosslinking agent used relative to 100 parts by weight of the base polymer is suitably 10 parts by weight or less, and may be 7 parts by weight or less, or 5 parts by weight or less. Using an isocyanate-based crosslinking agent in an amount that is not too large can be advantageous from the viewpoint of avoiding a decrease in adhesion to the adherend due to excessive crosslinking.

[0047] As the epoxy-based crosslinking agent, a polyfunctional epoxy compound having two or more epoxy groups in one molecule can be used. For example, N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Commercially available epoxy crosslinking agents include, for example, products sold by Mitsubishi Gas Chemical Company under the trade names "Tetrad C" and "Tetrad X."

[0048] When an epoxy-based crosslinking agent is used, the amount of the epoxy-based crosslinking agent used can be, for example, 0.005 parts by weight or more relative to 100 parts by weight of the base polymer, and from the viewpoint of obtaining a higher effect of use, it may be 0.01 parts by weight or more, or may be 0.02 parts by weight or more. In addition, the amount of the epoxy-based crosslinking agent used relative to 100 parts by weight of the base polymer is preferably 2 parts by weight or less, and may be 1 part by weight or less, 0.5 parts by weight or less, or 0.1 parts by weight or less. Using an epoxy-based crosslinking agent in an amount that is not too large can be advantageous from the viewpoint of avoiding a decrease in adhesion to the adherend due to excessive crosslinking.

[0049] When an isocyanate-based crosslinking agent is used in combination with another crosslinking agent (i.e., a nonisocyanate-based crosslinking agent), the relationship between the amount of the isocyanate-based crosslinking agent and the amount of the nonisocyanate-based crosslinking agent (e.g., an epoxy-based crosslinking agent) is not particularly limited. From the viewpoint of more suitably achieving both adhesion to the adherend and cohesive strength, in some embodiments, the content of the nonisocyanate-based crosslinking agent can be about 1 / 2 or less of the content of the isocyanate-based crosslinking agent on a weight basis, or about 1 / 5 or less, or about 1 / 10 or less, or about 1 / 20 or less, or about 1 / 30 or less. In addition, from the viewpoint of suitably exerting the effect of using an isocyanate-based crosslinking agent in combination with a nonisocyanate-based crosslinking agent (e.g., an epoxy-based crosslinking agent), it is appropriate that the content of the nonisocyanate-based crosslinking agent is about 1 / 1000 or more, for example, about 1 / 500 or more, of the content of the isocyanate-based crosslinking agent.

[0050] In order to make the crosslinking reaction of any of the above-mentioned crosslinking agents proceed more efficiently, a crosslinking catalyst may be used. As the crosslinking catalyst, for example, a tin catalyst such as dioctyltin dilaurate can be preferably used. The amount of the crosslinking catalyst used is not particularly limited, but can be, for example, about 0.0001 to 1 part by weight per 100 parts by weight of the base polymer.

[0051] Other examples of crosslinking agents that can be used in the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet disclosed herein include monomers having two or more polymerizable functional groups in one molecule, ie, polyfunctional monomers. Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl diol (meth)acrylate, and hexyl diol di(meth)acrylate.

[0052] When a polyfunctional monomer is used as a crosslinking agent, its amount varies depending on the molecular weight and number of functional groups of the polyfunctional monomer, but is suitably in the range of about 0.01 to 3.0 parts by weight relative to 100 parts by weight of the base polymer. From the viewpoint of obtaining a higher effect, in some embodiments, the amount of the polyfunctional monomer used may be, for example, 0.02 parts by weight or more, or 0.03 parts by weight or more relative to 100 parts by weight of the base polymer. On the other hand, from the viewpoint of avoiding a decrease in tack due to an excessive improvement in cohesive force, the amount of the polyfunctional monomer used may be 2.0 parts by weight or less, 1.0 parts by weight or less, or 0.5 parts by weight or less relative to 100 parts by weight of the base polymer.

[0053] The pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet disclosed herein may be subjected to a crosslinking treatment by electron beam irradiation (electron beam crosslinking) for the purpose of improving cohesive strength, etc. Electron beam crosslinking can be performed instead of or in combination with the use of any of the crosslinking agents described above.

[0054] (tackifier) The adhesive in the technology disclosed herein may be a composition containing a tackifier (typically a tackifier resin). The use of a tackifier can improve the performance of the adhesive sheet (for example, one or both of the shear adhesive strength and the peel strength). The tackifier is not particularly limited, and various tackifier resins such as rosin-based tackifier resins, terpene-based tackifier resins, hydrocarbon-based tackifier resins, and phenol-based tackifier resins can be used. Such tackifiers can be used alone or in combination of two or more.

[0055] Specific examples of rosin-based tackifying resins include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; modified rosins (hydrogenated rosin, disproportionated rosin, polymerized rosin, other chemically modified rosins, etc.) obtained by modifying these unmodified rosins through hydrogenation, disproportionation, polymerization, etc.; and various other rosin derivatives. Examples of the rosin derivatives include rosin esters such as unmodified rosin esterified with alcohols (i.e., rosin esters), and modified rosins (hydrogenated rosin, disproportionated rosin, polymerized rosin, etc.) esterified with alcohols (i.e., modified rosin esters); unsaturated fatty acid modified rosins obtained by modifying unmodified rosin or modified rosin (hydrogenated rosin, disproportionated rosin, polymerized rosin, etc.) with unsaturated fatty acid; and unsaturated fatty acid modified rosins obtained by modifying rosin esters with unsaturated fatty acid. rosin esters; rosin alcohols obtained by reducing the carboxyl groups in unmodified rosin, modified rosin (hydrogenated rosin, disproportionated rosin, polymerized rosin, etc.), unsaturated fatty acid modified rosins, or unsaturated fatty acid modified rosin esters; metal salts of rosins (particularly rosin esters) such as unmodified rosin, modified rosin, and various rosin derivatives; rosin phenolic resins obtained by adding phenol to rosins (unmodified rosin, modified rosin, various rosin derivatives, etc.) using an acid catalyst and then thermally polymerizing the resulting mixture.

[0056] Examples of terpene-based tackifying resins include terpene-based resins such as α-pinene polymers, β-pinene polymers, and dipentene polymers; modified terpene-based resins obtained by modifying these terpene-based resins (phenol-modified, aromatic-modified, hydrogen-modified, hydrocarbon-modified, etc.); etc. Examples of the modified terpene resins include terpene-phenol-based resins, styrene-modified terpene-based resins, aromatic-modified terpene-based resins, and hydrogenated terpene-based resins.

[0057] Examples of hydrocarbon-based tackifying resins include various hydrocarbon resins such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone-indene resins. Examples of the aliphatic hydrocarbon resin include polymers of one or more aliphatic hydrocarbons selected from olefins and dienes having about 4 to 5 carbon atoms. Examples of the olefins include 1-butene, isobutylene, and 1-pentene. Examples of the dienes include butadiene, 1,3-pentadiene, and isoprene. Examples of aromatic hydrocarbon resins include polymers of vinyl-containing aromatic hydrocarbons having about 8 to 10 carbon atoms (styrene, vinyltoluene, α-methylstyrene, indene, methylindene, etc.). Examples of aliphatic cyclic hydrocarbon resins include alicyclic hydrocarbon resins obtained by cyclizing and dimerizing so-called "C4 petroleum fractions" or "C5 petroleum fractions" and then polymerizing them; polymers of cyclic diene compounds (cyclopentadiene, dicyclopentadiene, ethylidene norbornene, dipentene, etc.) or hydrogenated products thereof; alicyclic hydrocarbon resins obtained by hydrogenating the aromatic rings of aromatic hydrocarbon resins or aliphatic / aromatic petroleum resins; etc.

[0058] When the adhesive layer disclosed herein contains a tackifier, a tackifier derived from a plant (a vegetable tackifier) ​​may preferably act as the tackifier from the viewpoint of improving the biomass carbon ratio of the adhesive layer. Examples of vegetable tackifiers include the above-mentioned rosin-based tackifier resin and terpene-based tackifier resin. The vegetable tackifier may be used alone or in combination of two or more. When the adhesive layer disclosed herein contains a tackifier, the proportion of the vegetable tackifier in the total amount of the tackifier is preferably 30% by weight or more (e.g., 50% by weight or more, typically 80% by weight or more). In a particularly preferred embodiment, the proportion of the vegetable tackifier in the total amount of the tackifier is 90% by weight or more (e.g., 95% by weight or more, typically 99 to 100% by weight). The technology disclosed herein may be preferably implemented in an embodiment that does not substantially contain a tackifier other than the vegetable tackifier.

[0059] In the technology disclosed herein, a tackifier resin having a softening point (softening temperature) of about 60° C. or higher (preferably about 80° C. or higher, more preferably about 95° C. or higher, for example, about 105° C. or higher) can be preferably used. Such a tackifier resin can realize a PSA sheet with higher performance (for example, higher shear adhesive strength). The upper limit of the softening point of the tackifier resin is not particularly limited. From the viewpoint of compatibility, etc., in some embodiments, the softening point of the tackifier resin may be, for example, about 200° C. or lower, about 180° C. or lower, about 140° C. or lower, or about 120° C. or lower. The softening point of the tackifier resin here is defined as a value measured by the softening point test method (ring and ball method) specified in either JIS K5902:2006 or JIS K2207:2006.

[0060] The content of the tackifier resin is not particularly limited, and can be appropriately set according to the desired adhesive performance (shear adhesive strength, peel strength, etc.). In some embodiments, the content of the tackifier resin relative to 100 parts by weight of the base polymer may be, for example, 5 parts by weight or more, appropriately 15 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, or 65 parts by weight or more. In addition, in consideration of the balance of adhesive performance, in some embodiments, the content of the tackifier resin relative to 100 parts by weight of the base polymer may be, for example, 200 parts by weight or less, appropriately 150 parts by weight or less, 120 parts by weight or less, 100 parts by weight or less, or 85 parts by weight or less.

[0061] (Other Ingredients) The pressure-sensitive adhesive layer may contain, as necessary, various additives that are common in the field of pressure-sensitive adhesive compositions, such as leveling agents, plasticizers, fillers, colorants (pigments, dyes, etc.), antistatic agents, antiaging agents, UV absorbers, antioxidants, light stabilizers, etc. As for such various additives, conventionally known ones can be used in the usual manner.

[0062] The content of the filler in the adhesive layer can be, for example, 0 parts by weight or more and 200 parts by weight or less (preferably 100 parts by weight or less, for example 50 parts by weight or less) relative to 100 parts by weight of the base polymer. From the viewpoint of preventing the filler from falling off from the adhesive layer, in some embodiments, the content of the filler relative to 100 parts by weight of the base polymer is suitably less than 30 parts by weight, preferably less than 20 parts by weight, more preferably less than 10 parts by weight, may be less than 5 parts by weight, or may be less than 1 part by weight. The adhesive layer may not use a filler.

[0063] The content of the plasticizer in the adhesive layer can be, for example, 0 parts by weight or more and 35 parts by weight or less relative to 100 parts by weight of the base polymer. From the viewpoint of obtaining a good shear adhesive strength suitable for fixing the member, the content of the plasticizer is preferably 25 parts by weight or less, more preferably 15 parts by weight or less. In addition, from the viewpoint of reducing the amount of volatile matter that may be generated due to the presence of the plasticizer, in some embodiments, the content of the plasticizer relative to 100 parts by weight of the base polymer is suitably less than 10 parts by weight, may be less than 5 parts by weight, may be less than 3 parts by weight, or may be less than 1 part by weight. In particular, in adhesive sheets used inside electronic devices or adhesive sheets used in precision electronic devices, it is advantageous to reduce the content of the plasticizer or not use a plasticizer.

[0064] The adhesive layer preferably does not contain a vulcanizing agent and does not contain a sulfur-containing vulcanization accelerator (such as a thiuram-based vulcanization accelerator, a dithiocarbamate-based vulcanization accelerator, or a thiazole-based vulcanization accelerator). This can be an advantageous feature for an adhesive sheet used in the field of electronic devices where the presence of sulfur is undesirable. The adhesive layer of the adhesive sheet disclosed herein preferably does not contain any material containing sulfur, including but not limited to vulcanizing agents and vulcanization accelerators.

[0065] The adhesive layer (layer made of adhesive) of the adhesive sheet disclosed herein may be a layer formed from an adhesive composition having such a composition. The form of the adhesive composition is not particularly limited, and may be, for example, an aqueous adhesive composition, a solvent-based adhesive composition, a hot melt-type adhesive composition, an active energy ray curable adhesive composition, or the like. Here, the aqueous adhesive composition refers to an adhesive composition in a form containing an adhesive (adhesive layer forming component) in a solvent (aqueous solvent) mainly composed of water, and is a concept that includes an aqueous dispersion-type adhesive composition in which the adhesive is dispersed in water, and a water-soluble adhesive composition in which the adhesive is dissolved in water. In addition, the solvent-type adhesive composition refers to an adhesive composition in a form containing an adhesive in an organic solvent. The adhesive sheet disclosed herein may be preferably implemented in an embodiment having an adhesive layer formed from a solvent-type adhesive composition.

[0066] The formation of the adhesive layer from the adhesive composition can be carried out by a conventionally known method. For example, a method (direct method) of forming an adhesive layer by directly applying (typically applying) the adhesive composition to a substrate and curing the composition can be preferably adopted. A method (transfer method) of forming an adhesive layer on a surface (release surface) having releasability by applying the adhesive composition to the surface and curing the composition, and transferring the adhesive layer to a substrate can also be adopted. The release surface can be the surface of a release liner, the back surface of a substrate treated for release, or the like. The adhesive composition can be cured by subjecting the adhesive composition to a curing treatment such as drying, crosslinking, polymerization, or cooling. Two or more types of curing treatments can be carried out simultaneously or stepwise.

[0067] The pressure-sensitive adhesive composition can be applied using a known or commonly used coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a die coater, a bar coater, a knife coater, a spray coater, etc. Alternatively, the pressure-sensitive adhesive composition may be applied by impregnation, a curtain coating method, or the like. From the viewpoints of promoting the crosslinking reaction, improving production efficiency, etc., the pressure-sensitive adhesive composition is preferably dried under heating. The drying temperature can be, for example, about 40 to 150° C., and is preferably about 60 to 130° C. After drying the pressure-sensitive adhesive composition, aging may be further performed for the purpose of adjusting the component migration in the pressure-sensitive adhesive layer, advancing the crosslinking reaction, and relaxing distortion that may exist in the substrate or pressure-sensitive adhesive layer, etc.

[0068] In the pressure-sensitive adhesive sheet disclosed herein, the thickness of the pressure-sensitive adhesive layer is not particularly limited and can be appropriately selected depending on the purpose. Considering the balance between adhesion and cohesion to the adherend, the thickness of the pressure-sensitive adhesive layer can be, for example, about 2 μm to 500 μm. From the viewpoint of adhesion to the adherend, the thickness of the pressure-sensitive adhesive layer is suitably 3 μm or more, and preferably 5 μm or more. From the viewpoint of easily realizing a pressure-sensitive adhesive sheet that exhibits better shear adhesive strength, in some embodiments, the thickness of the pressure-sensitive adhesive layer may be, for example, 8 μm or more, preferably 12 μm or more, 15 μm or more, 20 μm or more, or 25 μm or more. In addition, from the viewpoint of thinning the pressure-sensitive adhesive sheet, the thickness of the pressure-sensitive adhesive layer may be, for example, 200 μm or less, 150 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, or 30 μm or less. In an embodiment where a greater emphasis is placed on a thinner film, the thickness of the pressure-sensitive adhesive layer may be, for example, 20 μm or less, 15 μm or less, or 12 μm or less. When the pressure-sensitive adhesive sheet disclosed herein is a double-sided pressure-sensitive adhesive sheet having pressure-sensitive adhesive layers on both sides of a substrate, the thicknesses of the pressure-sensitive adhesive layers may be the same or different.

[0069] <Base material layer> The pressure-sensitive adhesive sheet disclosed herein includes a substrate layer containing a polyester resin. This allows the pressure-sensitive adhesive sheet to exhibit good processability. The polyester resin used in the substrate layer is a biomass polyester resin containing biomass-derived carbon. By using a biomass polyester resin as the substrate layer material, the pressure-sensitive adhesive sheet as a whole can exhibit good processability while reducing its dependency on fossil resource-based materials. Examples of biomass polyester resins include biomass polyethylene terephthalate (PET) resin, biomass polyethylene naphthalate (PEN) resin, biomass polybutylene terephthalate (PBT) resin, biomass polybutylene naphthalate (PBN) resin, biomass polyethylene furanoate (PEF) resin, and biomass polytrimethylene terephthalate resin. Among these, biomass PET resin, biomass PEN resin, biomass PBT resin, and biomass PBN resin are preferred, and biomass PET resin is more preferred. As the biomass polyester resin, typically, a polyester resin containing a polyester obtained by polycondensation of a dicarboxylic acid and a diol as a main component is used. The polyester resin can be made biomass-based by using a compound derived from biomass for at least one (eg, both) of the dicarboxylic acid and the diol used in the synthesis.

[0070] The form of the substrate layer containing the biomass polyester resin is not particularly limited, and in some preferred embodiments, the substrate layer of the pressure-sensitive adhesive sheet contains a polyester resin film from the viewpoints of dimensional stability, thickness accuracy, economy (cost), processability, tensile strength, etc. A configuration including a polyester resin film layer makes it easy to punch out complex shapes, and also tends to have excellent reworkability (peeling ability) in the event of a failure to attach. Excellent peelability is also advantageous in terms of recyclability. Furthermore, since it has high rigidity, it is possible to form a thin substrate layer while maintaining the desired mechanical properties. For example, in the field of electronic devices, the resin film is unlikely to be a source of dust (for example, fine fibers or particles such as paper powder). In this specification, the "resin film" is a typically non-porous film, and is a concept that is distinguished from so-called nonwoven fabrics and woven fabrics.

[0071] Examples of dicarboxylic acids constituting the polyester (also referred to as "dicarboxylic acid units" in the polyester after synthesis) include phthalic acid, isophthalic acid, terephthalic acid, 2-methylterephthalic acid, 5-sulfoisophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylketonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, and 3,4-naphthalenedicarboxylic acid. Examples of such dicarboxylic acids include aromatic dicarboxylic acids such as phthalenedicarboxylic acid; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, and 1,12-dodecanedicarboxylic acid; unsaturated dicarboxylic acids such as maleic acid, maleic anhydride, and fumaric acid; and derivatives thereof (for example, lower alkyl esters of the above dicarboxylic acids such as terephthalic acid). These may be used alone or in combination of two or more.

[0072] The dicarboxylic acid constituting the polyester may be one mainly composed of terephthalic acid. Specific examples of the polyester resin in this embodiment include PET resin and PBT resin. In this embodiment, the proportion of terephthalic acid in the total dicarboxylic acid constituting the polyester is suitably about 50% by weight or more, and from the viewpoint of fully exerting the effect of using terephthalic acid, it is preferably about 90% by weight or more (typically 95% by weight or more, for example, 99 to 100% by weight). Terephthalic acid may be used in the synthesis of polyester in the form of a derivative such as a lower alkyl ester of terephthalic acid.

[0073] As the dicarboxylic acid, a biomass-derived dicarboxylic acid can be preferably used. This allows the polyester resin to contain a predetermined amount of biomass carbon. In some embodiments, the dicarboxylic acid can be a biomass-derived terephthalic acid or a derivative thereof. There is no particular limitation on the method for obtaining a biomass-derived dicarboxylic acid. For example, the method described in Chemische Technik, vol. 38, No. 3, p116-119; 1986, in which isobutanol is obtained from corn, sugars, or wood, then converted to isobutylene, which is dimerized to obtain isooctene, and p-xylene is synthesized through radical cleavage, recombination, and cyclization, and this is oxidized to obtain terephthalic acid, can be mentioned (International Publication No. 2009 / 079213).

[0074] The ratio of biomass-derived dicarboxylic acids (e.g., terephthalic acid) among the dicarboxylic acids (e.g., terephthalic acid) constituting the polyester is not particularly limited. From the viewpoint of improving the biobased content, the ratio of biomass-derived dicarboxylic acids to the total dicarboxylic acids constituting the polyester is about 1% by weight or more (e.g., 1 to 100% by weight), and is preferably about 10% by weight or more, and may be, for example, about 50% by weight or more, about 80% by weight or more, about 90% by weight or more, or about 99% by weight or more. Substantially all of the dicarboxylic acids may be biomass-derived dicarboxylic acids. In some other embodiments (e.g., an embodiment in which the diol constituting the polyester contains a biomass-derived diol), the ratio of biomass-derived dicarboxylic acids to the total dicarboxylic acids may be less than 1% by weight, and the polyester may be substantially free of biomass-derived diol.

[0075] Examples of the diol constituting the polyester include aliphatic diols such as ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,2-butanediol, 2,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, and polyoxytetramethylene glycol; alicyclic diols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,1-cyclohexanedimethylol, and 1,4-cyclohexanedimethylol; aromatic diols such as xylylene glycol, 4,4'-dihydroxybiphenyl, 2,2-bis(4'-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone; and the like. These can be used alone or in combination of two or more. From the viewpoint of transparency, etc., aliphatic diols are preferred, and ethylene glycol is particularly preferred. The proportion of the aliphatic diol (preferably ethylene glycol) in the diol constituting the polyester is preferably 50% by weight or more (e.g., 80% by weight or more, typically 95% by weight or more). The diol may be substantially composed of ethylene glycol alone.

[0076] The diol constituting the polyester (also referred to as "diol unit" in the polyester after synthesis) may be mainly composed of ethylene glycol. Specific examples of the polyester resin in this embodiment include biomass PET resin and biomass PEN resin. In this embodiment, the proportion of ethylene glycol in the total diol constituting the polyester is suitably about 50% by weight or more, and from the viewpoint of fully exerting the effect of using ethylene glycol, it is preferably about 90% by weight or more (typically 95% by weight or more, for example 99 to 100% by weight).

[0077] As the diol, a biomass-derived diol (typically, a biomass diol obtained from biomass ethanol as a raw material) can be preferably used. This allows the polyester resin to contain a predetermined amount of biomass carbon. In some preferred embodiments, as the diol, a biomass-derived ethylene glycol (typically, a biomass ethylene glycol obtained from biomass ethanol as a raw material) can be used.

[0078] The ratio of the biomass-derived diol (preferably ethylene glycol) among the diols (preferably ethylene glycol) constituting the polyester is not particularly limited. From the viewpoint of improving the biobased content, the ratio of the biomass-derived diol to the total diols constituting the polyester is about 1% by weight or more (for example, 1 to 100% by weight), and is preferably about 10% by weight or more, for example, about 50% by weight or more, about 80% by weight or more, about 90% by weight or more, or about 99% by weight or more. Substantially all of the diols may be biomass-derived diols. In some other embodiments (for example, an embodiment in which the dicarboxylic acid constituting the polyester contains a biomass-derived dicarboxylic acid), the ratio of the biomass-derived diol to the total diols may be less than 1% by weight, and the polyester may be substantially free of biomass-derived diols.

[0079] The polyester may be substantially composed of a dicarboxylic acid and a diol, but may be copolymerized with a trivalent or higher polyvalent carboxylic acid, a trivalent or higher polyol, a monocarboxylic acid, a monoalcohol, a hydroxycarboxylic acid, a lactone, or the like, within a range that does not impair the effects of the technology disclosed herein, for the purpose of introducing a desired functional group or adjusting the molecular weight. These other copolymerization components may be derived from biomass or may not be derived from biomass. The proportion of the other copolymerization components is suitably, for example, less than 30 mol%, typically less than 10 mol% (or even less than 1 mol%). The technology disclosed herein may also be preferably implemented in an embodiment in which the monomer components of the polyester do not substantially contain the other copolymerization components.

[0080] The method for obtaining the polyester disclosed herein is not particularly limited, and a polymerization method known as a polyester synthesis method can be appropriately adopted. The monomer raw material used for the synthesis of the polyester can be obtained by polycondensing dicarboxylic acid and diol at an appropriate molar ratio from the viewpoint of polymerization efficiency, molecular weight control, etc. More specifically, the polyester can be synthesized by proceeding with the reaction between the carboxy group of the dicarboxylic acid and the hydroxyl group of the diol while removing water (produced water) and the like generated by the above reaction from the outside of the reaction system. As a method for removing the above-mentioned produced water from the reaction system, a method of blowing an inert gas into the reaction system and removing the produced water together with the inert gas from the reaction system, a method of distilling the produced water from the reaction system under reduced pressure (reduced pressure method), and the like can be used. The reduced pressure method can be preferably adopted because it is easy to shorten the synthesis time and is suitable for improving productivity. The above-mentioned reaction may be any of batch polymerization, semi-continuous polymerization, and continuous polymerization.

[0081] The reaction temperature when the above reaction (including esterification and polycondensation) is carried out, and the degree of vacuum (pressure in the reaction system) when a vacuum method is adopted, can be appropriately set so that a polymer with the desired properties (for example, molecular weight) can be efficiently obtained. Although not particularly limited, from the viewpoint of reaction rate and prevention of deterioration, it is appropriate to set the above reaction temperature to 180°C to 290°C (for example, 250°C to 290°C). Although not particularly limited, from the viewpoint of removal of generated water, reaction efficiency, etc., it is appropriate to set the above degree of vacuum to 10 kPa or less (typically 10 kPa to 0.1 kPa), for example, 4 kPa to 0.1 kPa. From the viewpoint of maintaining a stable pressure in the reaction system, it is appropriate to set the pressure in the reaction system to 0.1 kPa or more.

[0082] In the above reaction, a known or conventional catalyst may be used in an appropriate amount for esterification and condensation, as in the synthesis of a general polyester. Examples of the transesterification catalyst include magnesium-, manganese-, calcium-, cobalt-, lithium-, titanium-, zinc-, and barium-based compounds, and examples of the polymerization catalyst include various metal compounds such as titanium-, aluminum-, germanium-, antimony-, tin-, and zinc-based compounds; strong acids such as p-toluenesulfonic acid and sulfuric acid; and the like. In the above synthesis, a solvent may or may not be used. The above synthesis can be carried out without substantially using an organic solvent (meaning, for example, that an organic solvent is intentionally used as a reaction solvent in the above reaction). In the above reaction, an additive component such as a stabilizer (phosphorus compound, etc.) may be optionally added.

[0083] The polyester resin-containing layer used in the technology disclosed herein may contain a polymer other than the polyester in addition to the polyester. Examples of the polymer other than the polyester include polyolefin resins such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-butene copolymer; urethane resin; polyether; acrylic resin; rubbers such as natural rubber, modified natural rubber, and synthetic rubber (chloroprene rubber, styrene-butadiene rubber, and nitrile rubber); vinyl chloride resin; vinylidene chloride resin; vinyl acetate resin; polystyrene; polyacetal; polyimide; polyamide; fluororesin; and cellophane. These may be used alone or in combination of two or more. The polymer other than the polyester may be a polymer derived from a biomass resource or a polymer derived from a fossil resource. Examples of biomass resins other than polyester include biomass polyethylene resins such as biomass high density polyethylene (biomass HDPE) resin, biomass low density polyethylene (biomass LDPE) resin, and biomass linear low density polyethylene (biomass LLDPE) resin, and biomass polyolefin resins such as biomass polypropylene (biomass PP) resin; polylactic acid; biomass poly(3-hydroxybutyrate-co-3-hydroxyhexanoate); biomass polyamide resins such as polyhexamethylene sebacamide and poly(xylylene sebacamide); biomass polyurethane resins such as biomass polyester ether urethane resin and biomass polyether urethane resin; cellulose-based resins; etc. These can be used alone or in combination of two or more.

[0084] In an embodiment in which the polyester resin-containing layer contains a polymer other than the polyester in addition to the polyester, the content of the polymer other than the polyester is suitably less than 100 parts by weight relative to 100 parts by weight of the polyester, preferably about 50 parts by weight or less, more preferably about 30 parts by weight or less, and even more preferably about 10 parts by weight or less. The content of the polymer other than the polyester may be about 5 parts by weight or less, or about 1 part by weight or less, relative to 100 parts by weight of the polyester. The technology disclosed herein can be preferably implemented, for example, in an embodiment in which 99.5 to 100% by weight of the polymer contained in the polyester resin-containing layer is polyester.

[0085] The manufacturing method of the biomass polyester resin-containing layer (preferably a biomass polyester resin film) disclosed herein is not particularly limited, and may be any conventionally known method other than the use of biomass polyester resin. For example, a biomass polyester resin-containing layer (preferably a biomass polyester resin film) may be produced by using a biomass polyester resin prepared by a known polyester synthesis method using the above-mentioned materials, or a commercially available polyester derived from biomass resources (for example, Teijin's product name "Plantpet"), and, if necessary, by blending an appropriate amount of various additives and appropriately employing a film molding method such as extrusion molding, inflation molding, T-die casting molding, or calendar roll molding.

[0086] The biobased content of the biomass polyester resin-containing layer (preferably a biomass polyester resin film) disclosed herein is not particularly limited, and is preferably about 1% or more, and more preferably about 5% or more. From the viewpoint of reducing the dependency on fossil resource-based materials, the biobased content of the biomass polyester resin-containing layer is preferably about 8% or more, more preferably about 12% or more (e.g., about 15% or more), and may be about 30% or more, about 60% or more, or about 90% or more. The upper limit of the biobased content of the biomass polyester resin-containing layer is 100%, and from the viewpoint of cost-effectiveness, etc., it may be selected from the range of less than 50%, less than 40%, or less than 30% (e.g., less than 20%).

[0087] The thickness of the biomass polyester resin-containing layer (preferably the biomass polyester resin film layer) is not particularly limited and can be appropriately selected depending on the purpose. The thickness of the biomass polyester resin-containing layer is suitably about 1 μm or more, and from the viewpoint of handleability and processability, it may be, for example, 1.5 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, or 6 μm or more. By making the thickness of the biomass polyester resin-containing layer a predetermined value or more, the processability into a complex shape and the reworkability (peelability) in the event of a failure to apply tend to be improved. In addition, from the viewpoint of making the pressure-sensitive adhesive sheet thinner, in some embodiments, the thickness of the biomass polyester resin-containing layer may be, for example, 150 μm or less, 100 μm or less, 50 μm or less, 25 μm or less, 20 μm or less, 10 μm or less, 7 μm or less, less than 5 μm, or less than 4 μm. According to the technology disclosed herein, good processability can be achieved in a configuration using a thin biomass polyester resin-containing layer as described above.

[0088] The substrate layer disclosed herein may have a single layer structure, or may have a multi-layer structure of two layers, three layers or more. From the viewpoint of shape stability, it is preferable that the resin film has a single layer structure. That is, the substrate layer may be made of a biomass polyester resin-containing layer. When the substrate layer has a multi-layer structure, at least one of the layers is a biomass polyester resin-containing layer (typically a biomass polyester resin film layer). In the substrate layer of the multi-layer structure, the other layers are not particularly limited, and various sheet-like substrates can be used, for example, resin films other than biomass polyester resin films, paper, cloth, rubber sheets, foam sheets, metal foils, composites thereof, etc. can be used. Examples of resin films other than biomass polyester resin films include polyolefin resin films formed from PE, PP, ethylene-propylene copolymers, ethylene-butene copolymers, etc.; biomass polyolefin resin films; urethane resin films; biomass urethane resin films; vinyl chloride resin films; vinylidene chloride resin films; vinyl acetate resin films; polystyrene films; polyacetal films; polyimide films; polyamide films; fluororesin films; cellophane; and the like. Examples of the rubber sheet include a natural rubber sheet, a butyl rubber sheet, etc. Examples of the foam sheet include a foamed polyurethane sheet, a foamed polyolefin sheet, etc. Examples of the metal foil include an aluminum foil, a copper foil, etc.

[0089] The base layer (e.g., biomass polyester resin film layer) may contain various additives such as fillers (inorganic fillers, organic fillers, etc.), antioxidants, antioxidants, UV absorbers, antistatic agents, lubricants, plasticizers, colorants (pigments, dyes, etc.) as necessary. The blending ratio of various additives is usually about 30% by weight or less (e.g., 20% by weight or less, typically 10% by weight or less). For example, when a pigment (e.g., a white pigment) is contained in the base layer, the content is suitably about 0.1 to 10% by weight (e.g., 1 to 8% by weight, typically 1 to 5% by weight).

[0090] The surface of the substrate layer on which the adhesive layer is disposed (the surface on the side of the adhesive layer) may be subjected to a known or conventional surface treatment such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, formation of an undercoat layer, etc. Such a surface treatment may be a treatment for improving the adhesion between the substrate layer and the adhesive layer, in other words, the anchoring property of the adhesive layer to the substrate layer. Alternatively, the substrate layer may not be subjected to a surface treatment for improving the anchoring property on the surface on the side of the adhesive layer. When forming an undercoat layer, the undercoat agent (primer) used for the formation is not particularly limited and can be appropriately selected from known ones. The thickness of the undercoat layer is not particularly limited, and may be, for example, more than 0.01 μm, and is suitably 0.1 μm or more, and may be 0.2 μm or more from the viewpoint of enhancing the effect. The thickness of the undercoat layer is preferably less than 1.0 μm, and may be 0.7 μm or less, or may be 0.5 μm or less.

[0091] In the case of a single-sided pressure-sensitive adhesive sheet in which a pressure-sensitive adhesive layer is provided on one side of a substrate layer, the surface of the substrate layer on which the pressure-sensitive adhesive layer is not formed (back surface) may be subjected to a release treatment using a release treatment agent (back surface treatment agent). The back surface treatment agent that can be used to form the back surface treatment layer is not particularly limited, and silicone-based back surface treatment agents, fluorine-based back surface treatment agents, long-chain alkyl-based back surface treatment agents, and other known or commonly used treatment agents can be used according to the purpose and use. The back surface treatment agent can be used alone or in combination of two or more.

[0092] The bio-based content of the substrate layer is greater than 0%, for example, approximately 1% or more, and is suitably approximately 5% or more. From the viewpoint of reducing the dependency on fossil resource-based materials, the bio-based content of the substrate layer is preferably approximately 8% or more, more preferably approximately 12% or more (e.g., approximately 15% or more), and may be selected from the range of approximately 30% or more, approximately 60% or more, or approximately 90% or more. The upper limit of the bio-based content of the substrate layer is 100%, and from the viewpoint of cost-effectiveness, etc., it may be selected from the range of less than 50%, less than 40%, or less than 30% (e.g., less than 20%).

[0093] The breaking strength of the substrate layer disclosed herein is not particularly limited, and is suitably, for example, about 100 MPa or more (for example, about 150 MPa or more), and from the viewpoint of processability and handling, is preferably about 200 MPa or more (for example, about 220 MPa or more), may be about 250 MPa or more, or may be about 300 MPa or more (for example, about 340 MPa or more). The upper limit of the breaking strength of the substrate layer is suitably, for example, about 800 MPa or less, and from the viewpoint of conformity to the adherend surface, etc., is preferably about 500 MPa or less, more preferably about 460 MPa or less, may be about 400 MPa or less, may be about 350 MPa or less, or may be about 300 MPa or less. The breaking strength of the substrate layer can be measured based on JIS C 2318.

[0094] The thickness of the base layer is not particularly limited and can be appropriately selected depending on the purpose, for example, within the range of about 1 μm to 500 μm. From the viewpoint of the handleability and processability of the base layer, the thickness of the base layer may be, for example, 1.5 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, or 6 μm or more. By making the thickness of the base layer a predetermined value or more, the processability into a complex shape and the reworkability (peelability) in the event of a failure to apply tend to be improved. In addition, from the viewpoint of making the pressure-sensitive adhesive sheet thinner, in some embodiments, the thickness of the base layer may be, for example, 150 μm or less, 100 μm or less, 50 μm or less, 25 μm or less, 20 μm or less, 10 μm or less, 7 μm or less, less than 5 μm, or less than 4 μm. According to the technology disclosed herein, in a configuration using a thin base layer as described above, good processability can be exhibited.

[0095] In addition, the thickness of the base layer in the total thickness of the adhesive sheet (including the thickness of the adhesive layer and the base layer, but not including the thickness of the release liner) is appropriately set according to the purpose, and is not limited to a specific range. For example, the thickness of the base layer in the total thickness of the adhesive sheet is suitably about 1% or more (for example, about 5% or more), and from the viewpoint of ease of punching into complex shapes, improvement of yield during processing, and further reworkability (peelability) in the event of a failure to apply, it is preferably about 10% or more, may be about 15% or more, may be about 20% or more, may be about 25% or more, or may be about 30% or more (for example, about 40% or more). In addition, the ratio of the thickness of the base layer in the total thickness of the adhesive sheet is suitably about 90% or less (for example, about 70% or less), and preferably about 50% or less, may be about 30% or less, may be about 20% or less, or may be about 15% or less. By limiting the thickness ratio of the base material layer, the properties of the adhesive can be more easily exhibited, and in embodiments in which an adhesive with a high bio-based content is used, it can also reduce the dependence of the adhesive sheet as a whole on fossil resource-based materials.

[0096] <Release liner> The adhesive sheet disclosed herein may be provided in a form in which a release liner is attached to the adhesive surface (the surface of the adhesive layer that is attached to the adherend) as necessary (the form of an adhesive sheet with a release liner). The release liner is not particularly limited, and may be, for example, a release liner in which the surface of a liner substrate such as a resin film or paper is release-treated, or a release liner made of a low-adhesion material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin-based resin (PE, PP, etc.). As the resin film (layer) of the release liner, a polyester resin film such as a PET resin film; a polyolefin resin film such as PP or an ethylene-propylene copolymer, or a thermoplastic resin film such as a polyvinyl chloride film may be preferably used. From the viewpoint of strength and processability, a polyester resin film is more preferable. In addition, for example, a release treating agent such as a silicone-based, fluorine-based, long-chain alkyl-based, fatty acid amide-based, or molybdenum sulfide, or silica powder, may be used for the release treatment. A release-treated resin film (for example, a polyester resin film) may be preferably used as the release liner. The release treatment layer can be provided on at least one surface (eg, both surfaces) of the resin film.

[0097] The thickness of the release liner is not particularly limited, and from the viewpoint of conformity to the adhesive surface and peeling workability, it can be, for example, about 5 μm to 200 μm, and preferably about 10 μm to 100 μm. In an embodiment in which each adhesive surface of the double-sided pressure-sensitive adhesive sheet is protected by two release liners, it is preferable to make the thicknesses of the release liners different from the viewpoint of peeling workability of the release liners. For example, the thickness of the first release liner can be about 10 to 200 μm (typically about 30 to 100 μm, for example about 50 to 80 μm), and the thickness of the second release liner can be about 5 μm or more and less than 100 μm (typically about 8 μm or more and less than 50 μm, for example about 12 to 40 μm). The thickness of the first release liner is preferably about 1.5 to 5 times (for example 2 to 3 times) the thickness of the second release liner.

[0098] <Adhesive sheet> The thickness (total thickness) of the adhesive sheet disclosed herein (including the adhesive layer and base layer, but excluding the release liner) is not particularly limited and can be, for example, in the range of approximately 2 μm to 1000 μm. In some embodiments, the thickness of the adhesive sheet is preferably about 5 μm to 500 μm (e.g., 10 μm to 300 μm, typically 15 μm to 200 μm) in consideration of adhesive properties, etc. Alternatively, in some embodiments where emphasis is placed on thinning, the thickness of the adhesive sheet may be 100 μm or less (e.g., 5 μm to 100 μm), 70 μm or less (e.g., 5 μm to 70 μm), or 45 μm or less (e.g., 5 μm to 45 μm).

[0099] In the pressure-sensitive adhesive sheet disclosed herein, more than 40% of the total carbon contained in the pressure-sensitive adhesive sheet is preferably biomass-derived carbon. That is, the biomass carbon ratio of the pressure-sensitive adhesive sheet is preferably more than 40%. By using a pressure-sensitive adhesive sheet with such a high biomass carbon ratio, the amount of fossil resource-based materials used can be reduced. From this perspective, it can be said that the higher the biomass carbon ratio of the pressure-sensitive adhesive sheet, the more preferable it is. The biomass carbon ratio of the pressure-sensitive adhesive sheet is preferably 50% or more, and may be 60% or more, 70% or more, 75% or more, or 80% or more. The upper limit of the biomass carbon ratio is 100% by definition, and in some embodiments, the biomass carbon ratio of the pressure-sensitive adhesive sheet is less than 100%. From the viewpoint of making it easier to obtain shear adhesive strength, in some embodiments, the biomass carbon ratio of the pressure-sensitive adhesive sheet may be, for example, 95% or less, and when adhesive performance is more important, it may be 90% or less, or 85% or less.

[0100] In some preferred embodiments, the pressure-sensitive adhesive sheet exhibits a shear adhesive strength of 1.8 MPa or more. A pressure-sensitive adhesive sheet exhibits strong resistance to a force (i.e., shear force) that tends to displace the adhesive interface, and therefore has excellent retention performance of the adherend. From the viewpoint of exhibiting higher retention performance, the shear adhesive strength of the pressure-sensitive adhesive sheet is preferably 2.0 MPa or more, more preferably 2.2 MPa or more. In some embodiments, the shear adhesive strength may be 2.4 MPa or more, or 2.6 MPa or more. There is no particular upper limit to the shear adhesive strength, and generally, the higher the shear adhesive strength, the more preferable it is. On the other hand, from the viewpoint of facilitating an increase in the biomass carbon ratio of the pressure-sensitive adhesive layer, in some embodiments, the shear adhesive strength may be, for example, 20 MPa or less, 15 MPa or less, 10 MPa or less, or 7 MPa or less. The shear adhesive strength is measured by the method described in the Examples below.

[0101] The pressure-sensitive adhesive sheet according to some embodiments preferably has a peel strength against a stainless steel plate of 5N / 20mm or more. The pressure-sensitive adhesive sheet exhibiting the above characteristics is firmly bonded to the adherend, and therefore can be preferably used in an embodiment where re-peeling is not intended. From the viewpoint of realizing a more reliable bond, the peel strength may be, for example, 10N / 20mm or more, preferably 11N / 20mm or more, 12N / 20mm or more, 13N / 20mm or more, 14N / 20mm or more, or 15N / 20mm or more. The upper limit of the peel strength is not particularly limited, and generally, the higher the peel strength, the more preferable it is. On the other hand, from the viewpoint of easily increasing the biomass carbon ratio of the pressure-sensitive adhesive layer, in some embodiments, the peel strength may be, for example, 50N / 20mm or less, 40N / 20mm or less, or 30N / 20mm or less. Hereinafter, the peel strength is also referred to as the peel strength against SUS.

[0102] The above-mentioned peel strength against SUS can be measured by the following method. That is, the adhesive sheet is cut to a size of 20 mm wide and 150 mm long to prepare a measurement sample. In an environment of 23°C and 50% RH, the adhesive surface of the measurement sample is exposed, and the adhesive surface is pressed against a stainless steel plate (SUS304BA plate) as an adherend by rolling a 2 kg rubber roller back and forth once. After leaving it in an environment of 50°C for 2 hours, the peel strength (180° peel adhesive strength) (N / 20mm) is measured in an environment of 23°C and 50% RH according to JIS Z0237:2000 using a tensile tester under conditions of a peel angle of 180° and a tensile speed of 300 mm / min. As the tensile tester, a universal tensile compression tester (apparatus name "tensile compression tester, TCM-1kNB" manufactured by Minebea Co., Ltd.) can be used. The same method is adopted for the examples described later. In addition, when performing the measurement, in the case of a double-sided pressure-sensitive adhesive sheet or a pressure-sensitive adhesive sheet with a substrate that is easily deformed, the pressure-sensitive adhesive sheet to be measured can be reinforced by attaching an appropriate backing material to the pressure-sensitive adhesive sheet to be measured. For example, a PET film with a thickness of about 25 μm can be used as the backing material.

[0103] The pressure-sensitive adhesive sheet according to some embodiments preferably has a heat-resistant peel strength against a stainless steel plate of 4N / 20mm or more, more preferably 5N / 20mm or more, and even more preferably 7N / 20mm or more. A pressure-sensitive adhesive sheet exhibiting the above characteristics can realize a more reliable bond. The upper limit of the heat-resistant peel strength is not particularly limited, and generally the higher the better. On the other hand, from the viewpoint of easily increasing the biomass carbon ratio of the pressure-sensitive adhesive layer, in some embodiments, the heat-resistant peel strength may be, for example, 30N / 20mm or less, or may be 20N / 20mm or less. The heat-resistant peel strength is measured in the same manner as the above-mentioned SUS peel strength, except that the adhesive surface of the measurement sample is pressure-bonded to a stainless steel plate (SUS304BA plate) in an environment of 23°C and 50% RH, and then left in an environment of 80°C for 30 minutes, and then the peel strength is measured in the same environment.

[0104] In some embodiments, the pressure-sensitive adhesive sheet has a peel strength against a polypropylene (PP) plate (PP peel strength) of preferably 8N / 20mm or more, more preferably 10N / 20mm or more, and even more preferably 13N / 20mm or more. The pressure-sensitive adhesive sheet exhibiting the above characteristics can be firmly bonded to a low-polarity adherend such as a polyolefin resin. The upper limit of the PP peel strength is not particularly limited, and generally the higher the better. On the other hand, from the viewpoint of easily increasing the biomass carbon ratio of the pressure-sensitive adhesive layer, in some embodiments, the PP peel strength may be, for example, 40N / 20mm or less, 30N / 20mm or less, or 25N / 20mm or less. The PP peel strength is measured in the same manner as the SUS peel strength described above, except that a polypropylene resin plate is used as the adherend.

[0105] In some embodiments, the ratio of the SUS peel strength to the PP peel strength, i.e., the PP / SUS peel strength ratio, may be, for example, 0.5 or more, preferably 0.7 or more, and may be 0.9 or more. The PP / SUS peel strength ratio may be, for example, 3 or less, 2 or less, or 1.5 or less. The PP / SUS peel strength ratio being closer to 1 means that the difference in peel strength due to the material of the adherend is smaller. Such a pressure-sensitive adhesive sheet is preferred because it is highly versatile and suitable for joining and fixing different materials.

[0106] In some embodiments, the pressure-sensitive adhesive sheet has a peel strength against a polyethylene (PE) plate (PE peel strength) of 1.5 N / 20 mm or more, preferably 3 N / 20 mm or more, more preferably 5 N / 20 mm or more, and even more preferably 8 N / 20 mm or more. The pressure-sensitive adhesive sheet exhibiting the above characteristics can be firmly bonded to a low-polarity adherend such as a polyolefin resin. The upper limit of the PE peel strength is not particularly limited, and generally the higher the better. On the other hand, from the viewpoint of easily increasing the biomass carbon ratio of the pressure-sensitive adhesive layer, in some embodiments, the PE peel strength may be, for example, 30 N / 20 mm or less, or 20 N / 20 mm or less. The PE peel strength is measured in the same manner as the SUS peel strength described above, except that a polyethylene resin plate is used as the adherend.

[0107] The pressure-sensitive adhesive sheet disclosed herein is preferably halogen-free (particularly, chlorine-free). A halogen-free pressure-sensitive adhesive sheet can be realized by avoiding the use of materials containing halogen. For example, in the pressure-sensitive adhesive layer, it is desirable to avoid the use of halogenated polymers (e.g., chlorinated rubbers such as polychloroprene rubber) and additives containing halogen. It is also desirable to avoid the use of halogenated resins (e.g., vinyl chloride resins) and additives containing chlorine as components of the substrate.

[0108] The pressure-sensitive adhesive sheet disclosed herein is preferably configured to satisfy one or more of the following: (A) chlorine content is 0.09% by weight (900 ppm) or less; (B) bromine content is 0.09% by weight (900 ppm) or less; (C) the total content of chlorine and bromine is 0.15% by weight (1500 ppm) or less. It is more preferable to satisfy at least (A), more preferably to satisfy (A) and (C), and particularly preferable to satisfy all of (A), (B), and (C). The chlorine content and bromine content are measured by known methods such as fluorescent X-ray analysis and ion chromatography.

[0109] <Application> The use of the pressure-sensitive adhesive sheet disclosed herein is not particularly limited, and pressure-sensitive adhesive sheets used for various applications may be the subject of the present invention. The pressure-sensitive adhesive sheet disclosed herein is typically in the form of a double-sided pressure-sensitive adhesive sheet, and may be preferably used for applications in which members are fixed or joined. In such applications, it is particularly meaningful for the pressure-sensitive adhesive sheet to exhibit good shear adhesive strength. A typical application is that the sheet is attached to a component constituting an electronic device to fix, join, reinforce, or the like the component. From the viewpoint of thinning, in some embodiments, a form of a double-sided pressure-sensitive adhesive sheet with a substrate using a thin substrate may be preferably adopted. As the thin substrate layer, a substrate layer having a thickness of 10 μm or less (for example, less than 5 μm) may be preferably used.

[0110] The adhesive sheet disclosed herein is suitable for, for example, component fixing applications in portable electronic devices. Non-limiting examples of the portable electronic devices include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices (for example, wristwear-type devices worn on the wrist like wristwatches, modular-type devices worn on a part of the body with clips or straps, eyewear-type devices including glasses-type devices (monocular and binocular types, including head-mounted types), clothing-type devices attached to shirts, socks, hats, etc. in the form of accessories, and earwear-type devices attached to the ears like earphones), digital cameras, digital video cameras, audio devices (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game devices, electronic dictionaries, electronic organizers, electronic books, in-vehicle information devices, portable radios, portable televisions, portable printers, portable scanners, portable modems, etc. The adhesive sheet disclosed herein can be preferably used, for example, for the purpose of fixing a pressure-sensitive sensor to other members in a portable electronic device equipped with a pressure-sensitive sensor among such portable electronic devices. In some preferred embodiments, the adhesive sheet can be used to fix a pressure-sensitive sensor and other members in an electronic device (typically a portable electronic device) that has a function that allows an absolute position to be specified on a plate (typically a touch panel) corresponding to the screen using a device for indicating a position on the screen (typically a pen-type or mouse-type device) and a device for detecting the position. Note that in this specification, "portable" does not mean that it is merely portable, but rather that it has a level of portability that allows an individual (a standard adult) to carry it relatively easily.

[0111] The matters disclosed in this specification include the following. (1) A pressure-sensitive adhesive sheet comprising a base layer containing a polyester resin and a pressure-sensitive adhesive layer disposed on at least one surface of the base layer, 50% or more of the total carbon contained in the pressure-sensitive adhesive layer is biomass-derived carbon, The pressure-sensitive adhesive sheet, wherein the polyester resin contains biomass-derived carbon. (2) The pressure-sensitive adhesive sheet according to (1) above, wherein the thickness of the base layer accounts for 10% or more of the total thickness of the pressure-sensitive adhesive sheet. (3) The pressure-sensitive adhesive sheet according to (1) or (2) above, wherein the breaking strength of the base layer is 200 MPa or more. (4) The pressure-sensitive adhesive sheet according to any one of (1) to (3) above, wherein 50% or more of the total carbon contained in the pressure-sensitive adhesive sheet is biomass-derived carbon. (5) The pressure-sensitive adhesive sheet according to any one of (1) to (4) above, wherein the thickness of the base layer accounts for 50% or less of the total thickness of the pressure-sensitive adhesive sheet. (6) The pressure-sensitive adhesive sheet according to any one of the above (1) to (5), wherein 5% or more of the total carbon contained in the base layer is biomass-derived carbon. (7) The pressure-sensitive adhesive sheet according to any one of (1) to (6) above, which has a shear adhesive strength of 1.8 MPa or more. (8) The pressure-sensitive adhesive sheet according to any one of the above (1) to (7), which is a double-sided pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive layers are provided on both sides of the base layer. (9) The pressure-sensitive adhesive sheet according to any one of (1) to (8) above, which is used for fixing components of an electronic device.

[0112] (10) The pressure-sensitive adhesive sheet according to any one of (1) to (9) above, wherein the pressure-sensitive adhesive layer is made of a natural rubber-based pressure-sensitive adhesive. (11) The pressure-sensitive adhesive sheet according to any one of (1) to (10) above, wherein 20% by weight or more (typically 20% by weight or more and 70% by weight or less) of all repeating units constituting the base polymer of the pressure-sensitive adhesive are derived from acrylic monomers. (12) The pressure-sensitive adhesive sheet according to any one of (1) to (11) above, wherein the pressure-sensitive adhesive layer contains a tackifier derived from a plant (vegetable tackifier). (13) The adhesive sheet according to (12) above, wherein the content of the vegetable tackifier is 30 parts by weight or more (typically 30 parts by weight or more and 100 parts by weight or less) per 100 parts by weight of the base polymer contained in the adhesive layer. (14) The pressure-sensitive adhesive sheet according to (12) or (13) above, wherein the vegetable tackifier comprises at least one selected from the group consisting of terpene resins and modified terpene resins. (15) The pressure-sensitive adhesive sheet according to any one of (1) to (14) above, wherein the pressure-sensitive adhesive layer contains a crosslinking agent, and the crosslinking agent is selected from non-sulfur-containing crosslinking agents. (16) The pressure-sensitive adhesive sheet according to (15) above, wherein the crosslinking agent includes an isocyanate-based crosslinking agent. (17) The pressure-sensitive adhesive sheet according to any one of (1) to (16), wherein the pressure-sensitive adhesive layer contains less than 10 parts by weight of filler per 100 parts by weight of the base polymer (typically, equal to or more than 0 parts by weight and less than 10 parts by weight). (18) The pressure-sensitive adhesive sheet according to any one of (1) to (17) above, which has a peel strength from a stainless steel plate of 5 N / 20 mm or more (for example, 5 N / 20 mm or more and 50 N / 20 mm or less). (19) The pressure-sensitive adhesive sheet according to any one of (1) to (18) above, wherein the pressure-sensitive adhesive layer contains an acrylic-modified natural rubber as a base polymer. (20) The pressure-sensitive adhesive sheet according to (19) above, wherein the acrylic-modified natural rubber is natural rubber graft-polymerized with methyl methacrylate. (21) The pressure-sensitive adhesive sheet according to (19) or (20) above, wherein the weight of the repeating units derived from acrylic monomers accounts for at least 1 wt % and less than 80 wt % of the total weight of the acrylic-modified natural rubber. (22) The pressure-sensitive adhesive sheet according to any one of (1) to (21) above, which is halogen-free. EXAMPLES

[0113] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "parts" and "%" are by weight unless otherwise specified.

[0114] <Evaluation method> [Shear adhesive strength] A measurement sample is prepared by cutting an adhesive sheet (typically a double-sided adhesive sheet) to a size of 10 mm x 10 mm. In an environment of 23°C and 50% RH, each adhesive surface of the measurement sample is placed on the surface of two stainless steel plates (SUS304BA plates) and pressed against each other by rolling a 2 kg roller back and forth once. After leaving this in the same environment for two days, a tensile tester is used to measure the shear adhesive strength [MPa] at a tensile speed of 10 mm / min and a peel angle of 0 degrees. Specifically, as shown in FIG. 5, one adhesive surface 50A of the measurement sample 50 is attached to a stainless steel plate 61, and the other adhesive surface 50B of the measurement sample 50 is attached to a stainless steel plate 62 and pressed against each other. This is pulled in the direction of the arrow in FIG. 5 (i.e., the shear direction) at the above-mentioned speed, and the peel strength per 10 mm x 10 mm is measured. The shear adhesive strength [MPa] is calculated from the obtained value. In the case of a one-sided adhesive sheet (single-sided adhesive sheet), the non-adhesive side of the sheet is fixed to a stainless steel plate with an adhesive or the like, and the rest of the measurement can be performed in the same manner as above. A universal tensile / compression tester (product name "TG-1kN", manufactured by Minebea Co., Ltd.) can be used as the tensile tester.

[0115] [Workability] A measurement sample is prepared by cutting an adhesive sheet with a release liner into a size of 5 cm x 10 cm. The measurement sample is placed with the release liner side facing up, and two slits of about 8 cm in length are made in the center of the measurement sample, parallel to each other and spaced 1 cm apart, using a cutter. The slits are made deep enough to penetrate the measurement sample. The measurement sample is continuous with non-slit portions of about 1 cm on both ends of the slit. Next, a 2 kg roller is made to travel back and forth five times on the top surface of the measurement sample in the direction along the longitudinal direction of the slit, passing through the slit. After that, the measurement sample is cut with scissors near both ends of the slit (cutting in a direction perpendicular to the longitudinal direction of the slit) to remove the non-slit portions. The measurement sample is slowly pulled in the direction of separation at the slit, and the presence or absence of glue overflow is visually confirmed. Those without glue overflow are evaluated as "○", and those with glue overflow are evaluated as "×".

[0116] <Example 1> (Preparation of Pressure-Sensitive Adhesive Composition) A toluene solution containing 49 parts of natural rubber (RSS Class 1, after mastication) was added with 36 parts of methyl methacrylate (MMA) and 0.4 parts of a peroxide initiator to carry out solution polymerization, yielding a toluene solution of acrylic modified natural rubber A in which MMA was grafted onto the natural rubber. As the peroxide initiator, BPO (manufactured by NOF Corporation, product name "Niper BW") and dilauroyl peroxide (manufactured by NOF Corporation, product name "Perloyl L") were used in a weight ratio of approximately 1:1.7. To the toluene solution of the acrylic-modified natural rubber A, 70 parts of a terpene-based tackifier resin (manufactured by Yasuhara Chemical Co., Ltd., product name "YS Resin PX1150N", softening temperature: 115±5°C), 3 parts of an antioxidant (phenol-based antioxidant, product name "Irganox 1010", manufactured by BASF) and 4 parts of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were added per 100 parts of the acrylic-modified natural rubber A contained in the solution, and the mixture was stirred uniformly to prepare a pressure-sensitive adhesive composition A of this example.

[0117] (Preparation of adhesive sheet) The above-mentioned adhesive composition A was applied to the release surface of a 38 μm-thick first release liner (manufactured by Mitsubishi Polyester Corporation, product name "Diafoil MRF38"), one side of which is a polyester film with a release surface made of a silicone-based release treatment agent, and dried at 100 ° C for 2 minutes to form a 4 μm-thick first adhesive layer. The above-mentioned adhesive composition A was applied to the release surface of a 25 μm-thick second release liner (manufactured by Mitsubishi Polyester Corporation, product name "Diafoil MHA25"), one side of which is a polyester film with a release surface made of a silicone-based release treatment agent, and dried at 100 ° C for 2 minutes to form a 4 μm-thick second adhesive layer. A 2 μm-thick PET resin film substrate molded using biomass PET resin was prepared, and the first and second adhesive layers formed on the first and second release liners were attached to each side of this PET resin film substrate, respectively, to prepare an adhesive sheet (transfer method). The release liner was left on the adhesive layer as it was and used to protect the surface (adhesive surface) of the adhesive layer. In this way, a double-sided adhesive sheet with a total thickness of 10 μm was obtained, which had a first adhesive layer (4 μm thick) on one side of a base layer (2 μm thick) and a second adhesive layer (4 μm thick) on the other side. The biomass PET resin is a biomass PET resin synthesized using terephthalic acid or its derivative and plant-derived ethylene glycol as a biomass resource-derived raw material.

[0118] <Example 2> A 6 μm thick PET resin film formed from biomass PET resin was used as the base layer, and the first and second pressure-sensitive adhesive layers were each 12 μm thick. Otherwise, a double-sided pressure-sensitive adhesive sheet with a total thickness of 30 μm was obtained in the same manner as in Example 1.

[0119] <Example 3> A 12 μm thick PET resin film formed from biomass PET resin was used as the base layer, and the first and second pressure-sensitive adhesive layers were each 19 μm thick. Otherwise, a double-sided pressure-sensitive adhesive sheet with a total thickness of 50 μm was obtained in the same manner as in Example 1.

[0120] <Example 4> A 25 μm thick PET resin film formed from biomass PET resin was used as the base layer, and the first and second pressure-sensitive adhesive layers were each 38 μm thick. The rest of the process was the same as in Example 1, to obtain a double-sided pressure-sensitive adhesive sheet with a total thickness of 100 μm.

[0121] <Example 5> A double-sided PSA sheet with a total thickness of 50 μm was obtained in the same manner as in Example 3, except that a 12 μm-thick PET resin film (manufactured by Toray Industries, Inc., product name "Lumirror S10") was used as the base layer.

[0122] <Example 6> A double-sided PSA sheet with a total thickness of 100 μm was obtained in the same manner as in Example 4, except that a 25 μm-thick PET resin film (manufactured by Toray Industries, Inc., product name "Lumirror S10") was used as the base layer.

[0123] <Example 7> The above-mentioned adhesive composition A was applied to the release surface of a 38 μm-thick release liner (manufactured by Mitsubishi Polyester Corporation, product name "Diafoil MRF38"), one side of which was a polyester film with a release surface made of a silicone-based release agent, and dried at 100° C. for 2 minutes to form an adhesive layer with a thickness of 10 μm. The release surface of a 25 μm-thick release liner (manufactured by Mitsubishi Polyester Corporation, product name "Diafoil MHA25"), one side of which was a polyester film with a release surface made of a silicone-based release agent, was attached to this adhesive layer. In this way, a substrate-less double-sided adhesive sheet was obtained in a form in which both sides were protected by the above-mentioned two polyester release liners.

[0124] <Examples 8-10> Substrate-less double-sided adhesive sheets for each example were obtained in the same manner as in Example 5, except that the amount of adhesive composition A applied was adjusted so that the thickness of the adhesive layer was 30 μm (Example 8), 50 μm (Example 9), or 100 μm (Example 10), respectively.

[0125] <Measurement and Evaluation> The adhesive sheet obtained in each example was measured for shear adhesive strength by the method described above to evaluate processability. The bio-based content of the adhesive layer and the base layer of the adhesive sheet in each example was also measured based on ASTM D6866. The bio-based content of the adhesive sheet was then calculated by multiplying the bio-based content of the adhesive layer by its thickness ratio and the bio-based content of the base layer by its thickness ratio. The results are shown in Table 1.

[0126] [Table 1]

[0127] As shown in Table 1, Examples 1 to 4, which used PSA sheets having a PSA layer with a biomass carbon ratio of 50% or more and a polyester resin-containing substrate layer containing biomass-derived carbon, used biomass materials in both the PSA layer and the substrate layer, and compared with Examples 5 and 6, which used non-biomass substrate layers, as can be seen from a comparison between Examples 3 and 5, which used substrate layers of the same thickness, the bio-based content of the PSA sheet as a whole was increased while maintaining the same performance in terms of shear adhesive strength. In addition, Examples 1 to 4 used a substrate layer containing a biomass polyester resin, and therefore had excellent processability. In contrast, Examples 7 to 10, which used substrate-less PSA sheets, were unable to obtain good processability. From the above results, it can be seen that an adhesive sheet having a biomass polyester resin-containing base layer and an adhesive layer with a biomass carbon ratio of 50% or more can reduce the dependence on fossil resource materials for the adhesive sheet as a whole, while also achieving good processability.

[0128] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]

[0129] 1,2,3,4 Adhesive sheet 10 Base material layer 21, 22 Adhesive layer 31,32 Release liner 50 measurement samples 50A,50B Adhesive surface 61,62 Stainless steel plate

Claims

1. A double-sided adhesive sheet used to fix components of an electronic device, The adhesive layer includes a base layer containing a polyester resin (excluding a polylactic acid film), and a pressure-sensitive adhesive layer. the pressure-sensitive adhesive layer is disposed on both sides of the base layer, 50% or more of the total carbon contained in the pressure-sensitive adhesive layer is biomass-derived carbon, The polyester resin contains biomass-derived carbon, The content of biomass-derived carbon in the total carbon contained in the base material layer is less than 20%, A pressure-sensitive adhesive sheet having a shear adhesive strength of 1.8 MPa or more.

2. The pressure-sensitive adhesive sheet according to claim 1 , wherein the thickness of the base layer accounts for 10% or more of the total thickness of the pressure-sensitive adhesive sheet.

3. The pressure-sensitive adhesive sheet according to claim 1 , wherein the base layer has a breaking strength of 200 MPa or more.

4. The pressure-sensitive adhesive sheet according to any one of claims 1 to 3, wherein 50% or more of the total carbon contained in the pressure-sensitive adhesive sheet is biomass-derived carbon.

5. The pressure-sensitive adhesive sheet according to any one of claims 1 to 4, wherein a ratio of the thickness of said base layer to a total thickness of said pressure-sensitive adhesive sheet is 50% or less.

6. The pressure-sensitive adhesive sheet according to any one of claims 1 to 5, wherein 5% or more and less than 20% of the total carbon contained in the base layer is biomass-derived carbon.

Citation Information

Patent Citations

  • Method of forming impregnated waterproof layer on concrete surface

    JP1978016725A

  • Flywheel power source

    JP1986004500A

  • Pressure-sensitive adhesive tape

    JP1994228508A

  • Film for biodegradable protection

    JP2003231216A

  • Pressure-sensitive adhesive tape

    JP2003301152A