Method for forming fine structures in the volume of a substrate made of brittle material - Patents.com
The method of using ultrashort pulse laser-induced filamentary damage and etching addresses the limitations of existing structuring techniques, enabling precise and efficient formation of fine, complex structures in glass and glass-ceramic substrates with minimal stress and damage.
Patent Information
- Application Number
- JP2019085719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-04-27
- Filing Date
- 2019-04-26
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2039-04-26
AI Technical Summary
Existing methods for structuring glass and glass-ceramic substrates are limited in precision, cause microcracks and deformations, and are inefficient for producing fine, complex structures with minimal stress and damage.
A method involving ultrashort pulse laser-induced filamentary damage followed by etching to form cavities in the substrate, which does not penetrate through, allowing for precise control of cavity geometry and minimal substrate alteration.
Enables the formation of fine, complex structures with reduced microcracks and deformations, improving processing speed and quality while maintaining substrate strength.
Smart Images

Figure 0007562242000001 
Figure 0007562242000002 
Figure 0007562242000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing fine structures or recesses in a volume of a substrate made of a brittle material, in particular in a glass or glass ceramic element, and further to a glass or glass ceramic element produced by this method and provided with such structures or recesses.
[0002] The precise structuring of transparent, translucent or opaque glasses or glass ceramics is advantageous in many fields of use. In this case, a precision in the range of a few micrometers is required. The structuring concerns holes (round or angular), cavities, passages or any free form. To be able to use in a wide range of fields of use, it is desirable that the processing does not leave any damage, residues or stresses in the edge areas or volumes of the substrate.
[0003] Furthermore, such structuring should enable the most efficient manufacturing process possible. For example, different methods can be used to produce the holes. Besides sandblasting with corresponding masks, ultrasonic machining is an established method. However, both methods are limited in terms of their scaling to small structures, typically about 400 μm for ultrasonic machining and a minimum of 100 μm for sandblasting. Due to the mechanical removal, during sandblasting, additional stresses in the glass arise in connection with flaking in the hole edge region. For structuring thin glasses, both methods are basically not usable.
[0004] Thus, nowadays, multiple laser sources are used for structuring different materials. In this case, almost all known laser sources are used, such as CO2 or CO lasers, diode-pumped ns-, ps- and fs solid-state lasers with wavelengths in the infrared (e.g. 1064 nm), green (532 nm) and UV (365 nm). Excimer lasers operating at very short wavelengths (e.g. 193 nm or 248 nm) are also used for processing.
[0005] US 2015 / 0165563 A1 or US 2015 / 0166395 A1 describe laser methods for forming through holes in thin glass or as a preparation for subsequent separation of glass members.
[0006] Particularly demanding is the processing of glass or glass ceramics, since glass or glass ceramics generally have low thermal conductivity and high susceptibility to damage. Therefore, all laser ablation methods result in more or less intense heat loads or heat inputs. This heat input can certainly be reduced by shorter wavelengths and shorter pulse lengths, but still results in partially critical stresses up to microcracks and deformations in the edge region of the hole. At the same time, this method also produces a more clearly measurable roughness on the hole wall, since all laser methods ablate in clusters, i.e. the respective cluster size determines the residual roughness of the wall.
[0007] Another disadvantage of the laser ablation method is that a sufficiently deep structure can only be achieved by multiple passes of the workpiece to be processed. The processing speed is correspondingly slow. Therefore, the method is only conditionally suitable for use in industrial production. This is particularly true when openings through the glass or structures that generally extend from one side to the opposite side are to be processed. Furthermore, the walls of such structures, such as grooves, have an incline, i.e. are not vertical.
[0008] Another problem occurs, especially when structuring glasses or glass ceramics as brittle materials, in that the processed structures are significantly less strong under bending load, because microcracks occur during structuring. Another disadvantage is that the removed material accumulates.
[0009] A method for machining a through-hole in a glass substrate is described in DE 102013103370 A1, in which an opening is first produced in the glass substrate by means of a laser beam and then subsequent material removal takes place by means of an etching method.
[0010] A disadvantage of this known method is that it is extremely difficult to produce fine and intricate structures in the volume of a glass or glass-ceramic substrate with acceptable effort and high quality (i.e. with regard to the strength of the components).
[0011] The inventors have made efforts to achieve this goal. The object of the present invention is therefore to provide a glass or glass ceramic element with at least one opening or notch, with the strength being reduced as little as possible. In this case, it is desirable that the method of forming the opening in the glass or glass ceramic element produces as few microcracks as possible. At the same time, it is desirable that the process time of the method is improved.
[0012] In particular, it is desirable to be able to freely select the geometric shape for the cutouts, and the cutouts formed in this way should in particular not penetrate all the way through the substrate, i.e. the surface of the substrate located on the side opposite the cutout should remain unchanged.
[0013] This problem is solved surprisingly simply by a method for producing a cavity in a substrate made of a brittle material and a glass or glass ceramic substrate with such a cavity according to one of the independent claims. Preferred embodiments or refinements of the invention emerge from the respective dependent claims.
[0014] The subject of the invention is therefore a method for producing at least one cavity in the volume of a substrate made of a brittle material, preferably comprising a glass or a glass ceramic.
[0015] If simply referred to as a substrate, it is to be understood in the following that a substrate comprising a brittle material is to be understood as being preferably made of or containing glass or glass ceramics.
[0016] The substrate according to the invention may be formed, for example, in the shape of a plate with two opposite sides, but this is not a prerequisite for carrying out the method. It is also not essential that the substrate is formed particularly thin, since no through-openings that limit the thickness of the substrate need be formed. The substrate according to the invention may have a thickness of 500 μm or more.
[0017] The term "filament" is understood below to mean a very fine blind hole, i.e. an opening that does not penetrate the substrate. According to the invention, a filament-like damage is formed by a laser beam of an ultrashort pulsed laser. According to the invention, a substrate with at least one filament-like damage that does not penetrate the substrate can thus be obtained as an intermediate product. The diameter of this filament-like damage can then be expanded by an etching process, thus forming a filament. According to the invention, a substrate with at least one filament that does not penetrate the substrate can thus be obtained as an intermediate product.
[0018] The term "cavity" is understood below to mean an opening or cutout that can be formed by the joining of at least two adjacent filaments as a result of the expansion of the involved filaments in a subsequent etching process. This opening opens towards one side of the substrate, i.e. towards one lateral surface, and thus defines a cutout on the surface of the substrate. The opening can have different geometric shapes or complex structures. A cavity is therefore not a through opening that extends from one lateral surface to the lateral surface located on the opposite side.
[0019] The method according to the invention provides for the following steps: - directing a laser beam of an ultrashort pulse laser onto one of the sides of the substrate and focusing it with a focusing optic to form an extended focus at the substrate; forming a filamentary damage portion in the volume of the substrate by the incident energy of the laser beam, the filamentary damage portion extending into the volume to a predefined depth, in particular without penetrating the substrate; to form a filament-shaped lesion, an ultrashort pulsed laser is applied as a pulse or a pulse packet having at least two consecutive laser pulses; After processing at least two filamentous lesions, exposing the substrate to an etching medium, the etching medium removing material of the substrate at a removal rate of between 2 μm per hour and 20 μm per hour; - expanding at least two filamentous lesions to form filaments; at least 2 filaments, preferably at least 20 filaments, particularly preferably at least 50 filaments, are bonded together to form one cavity;
[0020] According to the invention, the substrate made of brittle material, preferably comprising glass or glass ceramic elements, further comprises at least one cavity, which cavity in the volume of the substrate can be produced by a combined method comprising a laser-based method for forming a filamentary damage and a subsequent etching method for expanding the damage and forming the cavity.
[0021] Preferably, at least two or more adjacent filamentary damages are fabricated in the substrate. Then, the material between the at least two filamentary damages can be removed together by an etching process, thereby forming a cavity. Thus, the dimensions of the cavity are larger than the filamentary damages or filaments, as the etching process removes material. Thus, preferably, the cavity includes at least two or more filamentary damages, thus forming a notch.
[0022] This was surprising, since it was previously assumed that the use of etching methods, i.e. the expansion by the etching medium of very small filamentary damages in the material, required through-openings or openings with a relatively large diameter. Indeed, such through-openings also required surface damage on the opposite side of the substrate. Furthermore, there are limitations on the thickness of the substrate, which do not apply to the present invention.
[0023] The requirement for a through opening is based on the assumption that the etching medium can only penetrate into such small filamentary damage because it is drawn into the filamentary damage from a first side by capillary forces, while gas present in the filamentary damage can escape on the other, opposite side.
[0024] However, the inventors have unexpectedly found that the etching solution can also penetrate into filamentary damage, i.e. into openings or blind holes that do not penetrate the substrate, and widen these openings or blind holes. In accordance with the invention, it is instead possible to widen filamentary damage that does not penetrate the substrate, having a diameter of at most 1 μm, preferably at most 0.8 μm, particularly preferably at most 0.5 μm, measured in the substrate volume, by means of an etching medium. Thus, the substrate or the area of the substrate that is provided for widening is exposed to the etching medium, in which case the opening to be widened is through and does not extend from one side to the other. The surface located on the side opposite to the entrance side of the laser beam therefore remains unchanged.
[0025] If the filamentary damages created by the laser method are located close enough together, a subsequent etching process can dissolve the remaining wall material between two adjacent filamentary damages to form complex cavities.
[0026] The pulse energy of the individual pulses is selected such that this pulse energy is below the ablation threshold of the substrate material, so that the laser light can penetrate into the material and the laser energy is not consumed by the ablation process already at the surface.
[0027] Thus, when the filamentary damages are formed side by side, machining of the filamentary damages and subsequent etching can be particularly effective in forming cavities in the volume of the substrate, the cavities being formed with different taper angles, the taper angle being the angle of the wall of the cavity relative to the adjacent side surface.
[0028] The taper angle is determined in particular by the removal rate in the etching process. At high removal rates, such as in the range of 15 μm / h to 20 μm / h, a rather vertical configuration of the cavities remains, resulting in taper angles in the range of 90°+ / -5°, preferably 90°+ / -3°, particularly preferably 90°+ / -1°. Significant deviations from the vertical configuration of the cavities occur with slower proceeding etching processes. This concerns removal rates in the range of 2 μm / h to 10 μm / h.
[0029] The depth and extent of the filament-like damage created in the volume of the substrate by the incident energy of the laser beam can be made possible by deliberate adjustment of the focal position relative to the substrate, by means of which corresponding optical elements can be provided, by means of which the focal position and depth can be controlled.
[0030] In order to achieve an extended uniform damage to a predefined depth in the volume of the substrate, a burst mode with the injection of pulse packets is particularly advantageous. This means, in particular, that the filamentary damage does not penetrate completely through the substrate, but extends only to a predefined subsection of the thickness of the substrate at the aforementioned point. It is provided that the filamentary damage penetrates less than 80%, preferably less than 70%, particularly preferably less than 50% of the thickness of the substrate. In other words, the length of the filamentary damage is less than 80%, preferably less than 70%, particularly preferably less than 50% of the thickness of the substrate at the damage point.
[0031] In this connection, it should be considered that a further material removal also occurs in the bottom region of the filamentary damage by a subsequent etching process, whereby it is considered advantageous for the filamentary damage to penetrate into the substrate to a depth of less than 80%, preferably less than 70%, with respect to the thickness of the substrate, in order to reliably exclude the occurrence of pre-damage on the opposite side.
[0032] As etching media, etching solutions comparable to plasma etching are suitable. That is to say, according to this embodiment, the etching is carried out wet-chemically. This is advantageous for removing substrate components from the surface during etching. As etching solutions, acidic and alkaline solutions can be used. As acidic etching media, in particular HF, HCI, H2SO4, ammonium bifluoride, HNO3 solutions or mixtures of these acids are suitable. For basic etching media, preferably KOH- or NaOH-alkali solutions come into consideration. With acidic etching solutions, typically high removal rates can be achieved. Basic solutions are suitable, in particular if a slow removal is aimed at. Furthermore, etching is preferably carried out in a temperature range of 40°C to 150°C, preferably 50°C to 120°C, particularly preferably up to 100°C.
[0033] Generally speaking, silicate-containing glasses with a low alkalinity are particularly suitable for the structuring according to the invention. Too high an alkalinity makes etching difficult. It has proven advantageous to use glasses with a basicity in the range of 0.45 to 0.55, preferably 0.48 to 0.54. This makes the glass particularly suitable for controlled etching with basic etching media. However, etching with acidic etching media remains possible. According to another refinement of the invention, it is provided that the glass of the glass element is a silica glass containing less than 17 percent by weight of alkali oxides.
[0034] However, it is also possible by this method to produce cavities in glass ceramics, in particular by means of LAS systems.
[0035] In the burst operation mode defined for the present invention, the laser energy is not emitted as individual pulses, but as a succession of short pulses emitted one after the other, which together form a pulse packet, a so-called burst. Such a pulse packet typically has somewhat more energy than the individual pulses in normal single-shot operation. However, the pulses of a burst themselves contain significantly less energy than the individual pulses. For the pulses in a burst, it may be provided that the pulse energy is flexibly adjustable, in particular that the pulse energy remains substantially constant, or that the pulse energy increases, or that the pulse energy decreases.
[0036] A suitable laser source according to the invention is a neodymium-doped yttrium aluminum garnet laser with a wavelength of 1064 nanometers. Operation with second harmonic generation (SHG) or third harmonic generation (THG) is also possible. When selecting a laser source, it should be noted that the substrate material is at least partially transparent to the corresponding wavelength of the laser beam.
[0037] The laser source is, for example, a 12 mm (1 / e 2 ) diameter, and as an optical element a biconvex lens with a focal length of 16 mm can be used. For the generation of the raw beam, it is possible to use appropriately beam-shaping optical elements, such as, for example, a Galileo telescope. The laser source operates in particular with a repetition rate between 1 kHz and 1000 kHz, preferably between 2 kHz and 200 kHz, particularly preferably between 3 kHz and 100 kHz.
[0038] The repetition rate and / or process speed, i.e. the speed at which the laser beam is guided relative to the substrate, can be selected such that a desired spacing between adjacent filamentary damages is achieved.
[0039] A suitable pulse width of the laser pulse is in the range of less than 100 picoseconds, preferably less than 20 picoseconds. A typical power of the laser source is particularly preferably in the range of 20-300 watts. To obtain filamentary lesions, according to an advantageous refinement of the invention, pulse energies in a burst higher than 400 microjoules are used, more preferably total burst energies higher than 500 microjoules.
[0040] When operating an ultrashort pulse laser in burst mode, the repetition rate is the repetition rate of the emission of the bursts. The pulse width is substantially independent of whether the laser is operated in individual pulse operation or in burst mode. The pulses in a burst typically have a similar pulse length as the pulses in individual pulse operation. The burst frequency is in the range of 15 MHz to 90 MHz, preferably in the range of 20 MHz to 85 MHz, for example 50 MHz, and the number of pulses in a burst is 2 to 20 pulses, preferably 3 to 8 pulses, for example 6 pulses.
[0041] The filamentary damage can be in the form of a series of local defects arranged one after the other, for example in the form of a row of filamentary damage extending deep into the substrate, the row of filamentary damage penetrating into the substrate to a predefined depth, and therefore it is not necessary to use a particularly thin substrate.
[0042] The present invention will now be described in detail with reference to the accompanying drawings, in which: FIG. [Brief description of the drawings]
[0043] [Figure 1] FIG. 1 illustrates an apparatus for laser machining glass elements in preparation for subsequent etching. [Diagram 2] FIG. 2 is a plan view from above of a glass element with processed filamentary damage. [Figure 3a] FIG. 2 is a magnified electron microscope photograph of an edge of a glass element. [Figure 3b] FIG. 2 is an exemplary electron microscope photograph of a cavity wall. [Figure 4] FIG. 1 is a side view showing the arrangement of filamentary damage in a volume of a substrate. [Diagram 5] FIG. 2 is a top plan view of a side of a substrate having a matrix arrangement of filamentary damage. [Figure 6a] FIG. 13 illustrates the mutual influence of previously formed adjacent filamentary lesions during the formation of new filamentary lesions. [Figure 6b] FIG. 13 illustrates the mutual influence of multiple previously formed adjacent filamentary lesions during the formation of a new filamentary lesion. [Figure 7a] FIG. 14 shows the material-dependent relationship for two chains of filamentary damage running close to each other along two straight lines. [Figure 7b] FIG. 1 shows an arrangement for measuring the shielding effect of a chain of multiple filamentary lesions along a straight line. [Figure 8a] FIG. 1 illustrates a method having a three-step refinement for forming filamentous lesions with extremely small spacing relative to each other. [Figure 8b] FIG. 1 shows the relationship between the spacing between two filamentous lesions and the expected filament depth. [Figure 9a] FIG. 13 shows the machining of filament-like damage on the back side to form a back cavity. [Figure 9b] FIG. 13 shows the machining of filament-like damage on the back side to form a back cavity. [Figure 10a] 1A-1C show an embodiment for forming cavities at different depths in a substrate. [Figure 10b] 1A-1C show an embodiment for forming cavities at different depths in a substrate. [Figure 11a] 1A-1D are perspective views of respective ones of substrates having surface structures formed in accordance with the present invention. [Figure 11b]1A-1D are perspective views of respective ones of substrates having surface structures formed in accordance with the present invention. [Figure 11c] 1A-1D are perspective views of respective ones of substrates having surface structures formed in accordance with the present invention. [Figure 12] FIG. 2 is a top plan view of a portion of a glass element with a cavity. [Figure 13a] FIG. 1 is a schematic diagram showing another assembly of two wafers of glass for use as a microfluidic chip. [Figure 13b] FIG. 1 is a schematic diagram showing another assembly of two wafers of glass for use as a microfluidic chip. [Figure 14] FIG. 1 shows an example of a microfluidics cell. [Figure 15] FIG. 1 shows an example of a microfluidics cell. [Figure 16] FIG. 1 shows an assembly for applying an adhesive layer.
[0044] Detailed Description of the Preferred Embodiments In the following detailed description of the preferred embodiments, for the sake of clarity, like reference numerals refer to substantially like parts throughout the embodiments. However, in order to more clearly illustrate the present invention, the preferred embodiments illustrated in the drawings are not necessarily drawn to scale.
[0045] 1 shows an embodiment for a laser processing device 20, by means of which filament-like damage 32 can be processed in a substrate, for example a glass element 1, from which cavities can then be formed in an etching process.
[0046] The device 20 comprises an ultrashort pulse laser 30 with preceding focusing optics 23 and a positioning unit 17, by means of which an impact point 73 of a laser beam 27 of the ultrashort pulse laser 30 can be positioned laterally on a side surface 2 of the glass element 1 to be processed, which is, for example, in the form of a plate. In the example shown, the positioning unit 17 comprises an xy-table, on which one side surface 3 of the glass element 1 rests. However, alternatively or additionally, it is also possible to design the optical elements to be movable in order to move the laser beam 27, so that the impact point 73 of the laser beam 27 can be moved when the glass element 1 is fixed.
[0047] The focusing optics 23 focuses the laser beam 27, in particular with a beam direction perpendicular to the side surface 2 to be irradiated, to form an extended focus. Such a focus can be formed, for example, by a conical lens (so-called axicon) or a lens with a large spherical aberration. The control of the positioning unit 17 and the ultrashort pulse laser 30 is preferably carried out by a program-technically adjusted computing unit 15. In this way, a predefined position for processing the filament-like damage 32 can be reached, which is preferably carried out by reading in position data from the data or via a network.
[0048] In the illustrated example, the illustrated filamentary damage 32 penetrates to a certain depth in the volume of the glass element 1, which in this example corresponds to approximately half the thickness of the plate-like glass element 1. According to the invention, the length of the filamentary damage 32 is less than 80%, preferably less than 70%, particularly preferably less than 50% of the thickness of the substrate at the location of the processed filamentary damage 32.
[0049] According to one embodiment, the following parameters can be used for the laser beam:
[0050] The wavelength of the laser beam is typically 1064 nm for a Nd:YAG laser. A laser beam with a raw beam diameter of 12 mm is formed, which is then focused by an optical element in the form of a biconvex lens with a focal length of 16 mm. The pulse width of the ultrashort pulse laser is less than 20 ps, preferably around 10 ps. The pulses are emitted in a burst with 2 or more, preferably 4 or more pulses. The burst frequency is 12-48 ns, preferably around 20 ns, the pulse energy is at least 200 microjoules, and the burst energy is correspondingly at least 400 microjoules.
[0051] After processing of one or, in particular, a number of filamentary damages 32, the glass element 1 is then removed and placed in an etching bath, in which, in a slow etching process, the substrate material, i.e., in this embodiment, glass, is removed along the filamentary damages 32, so that filaments are formed in the volume of the glass element 1 at the location of such damages 32.
[0052] Preferably, a basic etching bath is used with a pH value of >12, for example a KOH solution of >4 mol / l, preferably >5 mol / l, particularly preferably 6 mol / l but <30 mol / l. Etching is carried out according to one embodiment of the invention at a temperature of the etching bath of >70° C., preferably >80° C., particularly preferably >90° C., regardless of the etching medium used.
[0053] 2 shows a glass element 1 with a multiplicity of filamentary damages 32 in plan view from above on side surface 2. The filamentary damages 32 are arranged in a defined pattern, which can be written into the glass element 1 by the above-mentioned computer-controlled control of the positioning unit 17 and the ultrashort pulse laser 30. In particular, the filamentary damages 32 are processed into the glass element 1 along defined paths, which here for example have a closed rectangular contour or shape. The corners of the lines may be slightly chamfered. It is clear to the skilled person that not only rectangular paths can be followed in this way, but also arbitrarily shaped paths.
[0054] In one embodiment of the method according to the invention, - guiding the impact point 73 of the laser beam 27 on the substrate along a defined path or to a predefined position, - creating a filamentary lesion 32 at a defined location, to a defined depth in the volume of the substrate, by deliberately creating a focal position relative to the substrate; Etching then effects an expansion of the filament-like damage 32 to form a filament in the volume of the substrate.
[0055] In a special embodiment, the optical element 23 is likewise controllably configured, so that the exact focal position and depth in the substrate can be controlled in a particularly simple manner. In this way, it is possible to produce filament-like damage 32 at different heights in the substrate.
[0056] The diameter of the filamentary damage 32 is expanded by a subsequent isotropic etch. In this case, a cavity can be formed by connecting at least two adjacent filaments in a subsequent etching process. The steepness or taper angle of the filamentary damage 32 remains during a slow isotropic etch, i.e., a low removal rate.
[0057] According to the present invention, this expansion to integrate side-by-side filaments is desired in order to form cavities 5 with complex geometries and / or to form cavities 5 containing multiple filaments.
[0058] FIG. 3a shows an electron microscope photograph of a longitudinal section of a number of aligned filamentary damages 32 of a glass element 1 processed according to the invention. An edge with a number of laterally open filaments 6 running parallel to one another can be seen. These filaments 6 are, for example, elongated. In the example shown, the filaments 6 have been formed by an etching process at the site of the former filamentary damage. Integration of adjacent filamentary damages has not yet taken place in this example. In the diagram shown in FIG. 3, in the plan view from above of the cut edge, it can be seen that the longitudinal direction 51 of the filaments 6 runs in particular vertically from one side surface 3 into the volume of the glass element 1.
[0059] FIG. 3 further illustrates the microstructure of filament 6, i.e. Chamfered spherical recess One can clearly see the shape of the sidewalls of the filaments 6 in the form of 7. These spherical recesses 7 adjoin each other, preferably by a slow etching process, and the butting concave rounded parts of the recesses 7 form ridges.
[0060] The spacing between the filaments 6 is made relatively large in this example, at about 50 μm. This spacing can also be chosen smaller, especially if the filaments 6 merge directly into one another without flat edge sections 11. In general, the spacing between the filaments 6 (also called "pitch") is preferably in the range of 3 μm to 70 μm, preferably at least 10 μm, particularly preferably at least 20 μm. This spacing is measured from center to center of the filaments 6.
[0061] 3b shows an exemplary electron microscope photograph of the wall 8 of the cavity 5. The spherically deformed surface of the wall 8 can be clearly seen. The illustrated example is a wall 8 of the cavity 5 which has been processed according to the invention from transparent, colorless borosilicate glass, for example as available under the designation D263T from Schott AG, Mainz. The expansion of the previously processed filamentary damage 32 took place at an etching medium temperature of 80° C. for 19 hours.
[0062] From FIG. 4, which shows a schematic longitudinal section of an already processed glass element 1, which in this example has a total of five filamentary damages 32, it can be clearly seen that the filamentary damages 32 do not pass completely through the glass element 1, but merely form blind holes.
[0063] According to the invention, the filamentary damage 32 is applied with an etching medium. This is unusual in that the etching solution can penetrate into the filamentary damage 32 and cause a uniform, i.e. isotropic, expansion, even though it is formed as a blind hole. The filamentary damage 32 has extremely small dimensions. The filamentary damage 32 underlying the wall 8 shown in FIG. 3b of the cavity 5 has a diameter of at most 1 μm. Even smaller diameters, preferably at most 0.8 μm, particularly preferably at most 0.5 μm, do not interfere with the etching process according to the invention.
[0064] In a particularly preferred embodiment of the invention, a number of filamentary damages 32 are processed side by side into the glass element 1. The length t of the filamentary damages 32 in the glass element 1, the size of the filamentary damages 32 in the cross section and the distance d between two adjacent filamentary damages 32 are x Depending on the shape and the thickness of the cavity 5, it is possible in this way to produce cavities 5 with complex geometries, i.e. cutouts of different basic shapes or cross sections, in the volume of the substrate.
[0065] FIG. 4 illustrates some important geometric relationships related to the configuration of the filamentous damage portion 32 within the glass element 1. In this example, five filamentous damage portions 32 of length t are shown arranged in parallel rows within the volume of a substrate having a thickness T, such as the glass element 1.
[0066] As described above, since the filamentous damage portion 32 does not completely penetrate the substrate, t < T. In order to accelerate the processing of the filamentous damage portions into the substrate, the length of the filamentous damage portions is preferably selected to be as small as possible. This is because the processing of relatively long filamentous damage portions is extremely time-consuming to form a complex structure that requires such a large number of filamentous damage portions. Thus, preferably t < 0.8 * T, preferably t < 0.7 * T, and particularly preferably t < 0.5 * T.
[0067] In addition to the depth in the substrate, the spacing between two adjacent filamentous damage portions is extremely important. This spacing is measured from the center to the center of the filamentous damage portion 32 and is denoted by d in FIG. 4. x Thus, this "pitch" forms a reference for process control.
[0068] To form a three-dimensional inner structure within the volume of the substrate, which has only one opening facing one of the two side surfaces of the substrate and the surface of the side surface located on the opposite side of the substrate remains unchanged, the filamentous damage portions 32 are processed into the volume of the substrate in a two-dimensional structure or pattern starting from one side surface.
[0069] 5 shows a schematic top view of a side of a substrate with a matrix-like arrangement of filamentary damages 32, in this example a 4x5 arrangement. The inner contour that can be formed after the etching process due to this geometric arrangement of filamentary damages 32 is rectangular in shape, as long as the spacing and depth of the filamentary damages 32 meet the above-mentioned requirements. It is clear to the skilled person that different geometric shapes can be formed solely on the basis of the arrangement of the filamentary damages 32 on the side of the substrate, for example inner contours in the glass element 1 with triangular or circular basic shapes or freeform surfaces.
[0070] In FIG. 5, the two-dimensional distance between two adjacent filament-like damaged parts 32 is d x And, d x d perpendicular to y In a matrix arrangement of filamentary lesions 32, the spacing between them may be the same in both directions, but is not required to be, so that d x ≠d y These spacings between adjacent filamentary damages 32 result in a defined formation of the bottom and walls 8 of a cavity 5 during the etching process. This cavity 5 is then deepened further downwards. In the illustrated example, x =d y is selected.
[0071] In order for the filamentary damage 32 to be expanded by the etching process to form cavities with the desired structure, it is important that the filamentary damage 32 is perfectly shaped as it is processed into the substrate material.
[0072] The shaping of the filamentary damages 32 can be adversely affected by contamination on the surface of the substrate, which causes shading of the laser beam, which adversely affects the beam shape or the beam intensity, which leads to undesired deviations in the formation of the filamentary damages 32 in the substrate, i.e. the defined depth and / or the predefined orientation are not achieved.
[0073] Certainly, a small spacing between two adjacent filamentary damages 32 is considered to be advantageous in order to form relatively large structures and minimize the material removal between two adjacent filamentary damages 32 or the time required for this material removal, but on the other hand care must be taken to maintain a defined minimum spacing so as to prevent the filamentary damages 32 from being too spatially close to each other.
[0074] This is due to the fact that the spatial proximity of adjacent filamentary damages 32 to the current working point, i.e. the position where the new filamentary damage 32 is being formed, has a significant influence on the shaping of the just-formed filamentary damage 32 due to the shielding effect of the adjacent filaments. In optical structures working with spherical aberration or Bessel beams, the formation of the filamentary damage 32 relies on the supply of laser energy being as rotationally symmetric as possible with respect to the focal line.
[0075] When a first chain is formed along the path, for example by a filament continuation, the energy supply for forming a new filamentary lesion 32a is only blocked by the already formed adjacent filamentary lesion 32b. This is shown purely by way of example in Fig. 6a, which is intended to clearly show the mutual influence of already formed adjacent filamentary lesions during the formation of a new filamentary lesion.
[0076] The influence of the neighboring filamentary damages 32b on the formation of the new filamentary damages 32a depends entirely on the mutual spacing of the filamentary damages 32, 32a, 32b, the diameter of the formed filamentary damages 32, and thus on the solid angle proportion in which the existing filamentary damages 32b shade the energy supply to the new filamentary damages 32a. In this example, this extent is illustrated by the angle δ. The respective influence zones 33 of the laser beam are represented in this example by circles. The circles show the outer demarcation starting from a midpoint corresponding to the impact point 73 of the laser beam 27. The reference number 34 indicates the influence area that is shaded due to at least partial overlap of the influence zone 33 of the previously processed filamentary damage.
[0077] Another important dimension is the diameter of the filament-forming laser beam on the substrate side 2, 3. When forming a new filamentary damage 32a adjacent to already formed filamentary damages 32b, for example next to an already existing row of filamentary damages 32b, if they are too close together, half of the theoretically provided energy is already blocked at a percentage of the solid angle.
[0078] This is shown purely by way of example in Fig. 6b, which illustrates the mutual influence of already formed adjacent filamentary damages 32b during the formation of a new filamentary damage 32a. In this case, the shielding of the individual solid angle fractions δ is added together to form the total shielding. Overall, therefore, the maximum achievable length of the filamentary damage 32a in the vicinity of the adjacent filamentary damage 32b is a function of the mutual spacing of the filamentary damages. Knowledge of this functional relationship is used according to the invention for the optimization of the process strategy and thus for the method control for the formation of cavities according to the invention.
[0079] This relationship is material-dependent and is briefly outlined with reference to Figures 7a and 7b. To determine the material-dependent relationship, in a first step the shielding effect of the individual filament-like damages 32a is determined (Figure 7a). For this purpose, firstly, the shielding effect of the individual filament-like damages 32a is determined along a first straight line 35 at a constant distance d x Chains with filamentary damage 32a having radius R spaced apart at d x >>R. Preferably, the spacing of the filamentary damage 32a is selected to be large enough to avoid any influence of already existing filamentary damage 32a. This precondition is d x >50 * R, preferably d x >100 * R is given.
[0080] Along a second straight line 36, a second chain of filamentary lesions 32b is formed at the same x-location as the first chain, but at a constantly decreasing spacing d y As a starting value, d y =d x can be selected. A second chain of filamentary damages is formed, with the associated second straight line 36 running continuously close to the first straight line 35. By measuring the formed length of the filamentary damages in relation to their mutual spacing, an optimal spacing can be determined and used for further methods. The determination of the length can also be performed, for example, by optical microscopy, for example by opening the filament line, or by photography in conjunction with image processing methods, for example by edge extraction algorithms.
[0081] Therefore, the optimal spacing between two adjacent filament-like damages 32a, 32b is the minimum spacing d at which there is no reduction in the length of the filament-like damages due to mutual influence or no difference in the etching behavior is observed. y It is.
[0082] In a similar manner, the measurement of the shielding effect of a chain of multiple filament-like defects 32 along a straight line 35 (FIG. 7b) can be carried out. As in the above example, first, the defects are separated from each other by a certain distance d along the straight line 35. x Chains of filamentary lesions 32 with radius R spaced apart at different intervals d are then machined into the substrate. y , individual filamentary lesions 32 are formed, the length of which is then newly determined depending on its spacing relative to the straight line 35.
[0083] In certain cases, it may also be necessary to form the filamentary lesions 32 at a smaller distance from each other than that which has been found to be advantageous based on the shielding measurements described above, meaning that a distance is selected at which a reduction in the length of the filamentary lesions can occur.
[0084] For this purpose, the method illustrated in Figures 8a and 8b can be used with particular advantage: a method comprising several steps is chosen in order to produce, for example, chains of filamentary lesions 132 along a path, more closely spaced relative to one another in this context.
[0085] In a first step, a chain of filamentary damages 132c is formed along a roughly defined path with a maximum possible length and a minimum spacing relative to each other, where the minimum spacing is such that two adjacent filamentary damages 132 do not yet affect each other when irradiated with the laser beam.
[0086] In a second step, another new filamentary lesion 132b is formed with a smaller length, centered between each two adjacent filamentary lesions 132c, which cannot be done at the original length due to the shielding by the adjacent filamentary lesions 132c. Recursive refinement of this process is performed as necessary.
[0087] In Fig. 8a, the method is illustrated with three stages of refinement. Along a path, in this example a straight line of length b, a filamentary lesion 132c with a maximum depth t1 is first formed. This filamentary lesion 132c occurs based on a maintained minimum spacing d1. That is, this step A includes the formation of the longest filamentary lesion 132c.
[0088] Another new filamentary lesion 132b having a depth t2 is formed exactly in the middle of each two adjacent filamentary lesions 132c, which has a distance d1 / 2=d2 from the adjacent filamentary lesions 132c on both sides. That is, this second step B includes the formation of a filamentary lesion 132b that is shorter than the filamentary lesions 132c.
[0089] Finally, in a third step C, another new filamentary lesion 132a with a depth t3 is formed between each two adjacent filamentary lesions 132b. This filamentary lesion 132a has a distance d2 / 2=d3 on both sides to the adjacent filamentary lesion 132b. In this way, a particularly narrow series of filamentary lesions 132 can be achieved. In this case, the filamentary lesions 132 each have a depth that depends on the respective step of their formation. FIG. 8b shows the relationship between the distance d between two filamentary lesions 132 and the expected filament depth t=t(d). In this case, the two adjacent filamentary lesions 132 have different depths.
[0090] The three-step method shown in FIG. 8a allows the formation of a cavity 5 having a width b after the etching process has been performed and a maximum depth t1 plus a size due to the expansion caused by the etching process.
[0091] Of course, the method can also be carried out in more than the above-mentioned three iterations, thereby achieving even closer spacing of the filamentary damages 132. In this case, a number of filamentary damages 32, 132 are processed into the substrate with a minimum spacing that is not yet shielded, and then in one or more iterations, further filamentary damages are formed respectively in the center between two adjacent filamentary damages. In this case, the depth of the filamentary damages arranged next to each other is generally not the same, but depends on the respective iteration in the method sequence in which the filamentary damages were produced.
[0092] In principle, it is also possible for the length of the focal line formed by the beam-forming optical elements to exceed the thickness of the substrate. In this case, however, care must be taken that the side of the substrate facing away from the entrance is not altered, since otherwise undesirable damage would also occur on the rear surface of the substrate in the subsequent etching process. This can be countered, for example, by changing the distance between the optical element 23 of the focusing system and the substrate, i.e. by increasing the distance of the optical element 23 from the surface of the substrate or, in this example, from the surface of the above-mentioned glass element 1, and / or by suitable refocusing by the optical system.
[0093] This is further influenced by the spacing of the filamentary damage, which in turn depends on the defined depth of the cavity and the optical system used. An optical system with spherical aberration, for example an optical element in the form of a biconvex lens with a focal length of 16 mm, a free aperture of 18 mm and a focal length of 12 mm (1 / e 2 When using a raw beam of 1000 nm and a desired depth of the cavities to be formed of up to 0.5 mm, it has proven advantageous for the filamentary damage 32 to be spaced from one another by at least 10 μm, preferably 20 μm.
[0094] It is also possible to form cavities 5 with a relatively large depth, up to about 5 mm. The depth of the cavities 5 may also be selected to be smaller. In this case, a minimum depth of at least 50 μm, preferably at least 100 μm, particularly preferably at least 200 μm, is advantageous so that the advantages of the method according to the invention can also be fully utilized for ablation.
[0095] The spacing of the filamentary damage also influences the shaping of the bottom surface of the cavity. In this case, two basic aspects can be distinguished: 1) The filament-like damage is processed into a raster having the same spacing from each other in a matrix. In this case, d x =d y The etching process forms the bottom of the cavity with a uniform wavy structure. This wavy structure is substantially uniform over the selected interval d x Or d y depends on. 2) The filamentary damage is processed in a continuous line. In this case, the filamentary damage is processed along each adjacent path in a first direction with a first spacing relative to each other of about 4-6 μm. At a second spacing, another path of filamentary damage is added to the first. In this case, the spacing of the paths relative to each other is selected to be greater than the first spacing. For example, this second spacing can be 10 μm or more. The cavity formed in this manner has a bottom with a groove structure after the etching process.
[0096] Of course, in the above-mentioned examples, the arrangement of the paths is selected according to the desired shape of the cavity, i.e. the arrangement may be made in any pattern, for example in the form of a matrix. The chains or paths used to form the cavity do not have to be straight-shaped in this case, but may be selected in any free form.
[0097] For both above mentioned aspects 1) and 2), essentially the resulting structure at the bottom of the cavity is generated by the interplay between the material transformation by the ultrashort pulsed laser and the etching process, this bottom structure is characteristic for the filament formation strategy.
[0098] Both embodiments 1) and 2) mean that the wall 8 of the cavity 5 has a structure with a number of spherical recesses 7 after the etching process, as shown for example in FIG. 3b.
[0099] In a particular embodiment, the cavity 5 formed according to the invention in the volume of the substrate comprises at least two regions with different depths, in which filamentary damages 32, 132 are machined into the substrate with different lengths and / or different focal positions.
[0100] In the case of the so-called surface cavities mentioned above, in which the cavities 5 are formed in the substrate on the laser incidence side, it has been found to be advantageous to first process the relatively deep and thus long filament-like damages 32, 132, and then the relatively short filament-like damages. In the case of the so-called back cavities, in which the cavities 5 are formed in the substrate on the side opposite to the laser incidence side, the reverse order has been found to be advantageous.
[0101] Generally, the formation of a rear cavity has been found to be advantageous, since the filament spacing can be selected small. On the incident side, the filaments can be better processed with a defined depth and direction, since the laser process causes less contamination. Figures 9a and 9b show the processing of filament-like damage 32 on the rear side to form a rear cavity. In this case, a cavity 5 with a bottom is formed, which in the case of the embodiment shown in Figure 9a has a groove-like shape and in the case of the embodiment shown in Figure 9b has a uniform wave-like shape.
[0102] In principle, it is also possible to form cavities in the substrate with different depths, as shown in Fig. 10a, or even to form a step, which may be used to form a blind hole in combination with the through opening 37 as suggested in Fig. 10b, i.e. with a step cross-sectional shape with a concentric cross-section.
[0103] Contrary to what is shown in Figures 10a and 10b, preferably the spacing of the filamentary lesions relative to one another is adjusted so that the filament is formed at its full length, in other words the minimum spacing of two adjacent filamentary lesions relative to one another is maintained without affecting their formation, respectively.
[0104] In an likewise advantageous embodiment, at least one interface of the substrate is wetted with a liquid when filamentary damage is being processed. In this case, different variations can be used. 1) Wetting of the back surface of the substrate, i.e. the side opposite the laser incidence, to reduce the refractive index difference at the back surface. Avoiding or reducing the refractive index difference results in avoiding or minimizing surface damage. 2) Wetting of the front surface of the substrate, i.e. the side facing the laser incidence, to reduce contamination on the top surface, which can lead to undesirable damage and / or effects on the shaping of the filament, i.e. the filament is shaped to a small depth. 3) Double-sided wetting to reduce the refractive index difference on the back side and to reduce contamination on the top surface of the substrate.
[0105] In this case, the formation of the filamentary damage 32, 132 under the liquid has the additional advantage that the open cavities are filled with liquid instead of air, which accelerates the subsequent etching process. A special embodiment is the formation of the filamentary damage under the etching solution as described above.
[0106] 11a, 11b and 11c show in each case a perspective view a substrate, in this example a glass element 200, with a surface structure in which cavities 5 have been formed by the method according to the invention described above. 11b and 11c show a layer structure comprising two or three glass elements 200. The thus structured glass elements 200 (hereinafter also called wafers) and the layer structures formed from these glass elements 200, comprising two or more wafers, are typically used in the field of microfluidics as so-called microfluidic chips or microfluidic cells. Microfluidic chips or microfluidic cells allow the investigation of the properties and reactions of chemical or biological materials in a systematic and automated manner. The reactants involved are typically brought into the flow channels (machined grooves) and reaction chambers through through-holes 50 in the cover glass, and the reaction products are then analyzed. The method according to the invention for forming cavities 5 can be used in the most advantageous manner for forming these extremely fine reaction chambers. Thus, according to another aspect, the invention relates to a microfluidic cell 12 comprising a substrate in the form of a glass element comprising at least one cavity 5 .
[0107] Figure 12 shows a top plan view of a portion of a glass element in which a cavity 5 has been formed by filament forming and etching according to the invention.
[0108] In this case, the desired area of the cavity 5 is >20 μm=d x and 5μm=d yIn the illustrated embodiment, the cavity 5 is formed with a mesh of filamentary damages 32 spaced at a pitch of 10 mm. In this case, the filamentary damages 32 are not molded completely through the glass volume, but only from one side to the desired depth. During a subsequent etching process, the individual filamentary damages 32 are joined to form a consistent surface. This forms the cavity 5 according to the invention. In the illustrated example, the bottom surface of the cavity 5 has a structure with a spherical recess, like the side walls.
[0109] Figures 13a and 13b finally show, in a simplified example for clarity, another arrangement of two substrates, in this example two wafers 9, 10 made of glass, for use as a microfluidic cell 12. In this case, the wafer 9 has a flat and planar shape, whereas the wafer 10, which is also flat and planar, has two through holes 122 as well as a cavity 121. In Figure 13b the layer structure of the microfluidic cell 12 is shown. In this case, the cavity 121 formed according to the invention constitutes a reaction chamber. Both through holes 122 serve for filling and draining.
[0110] The method according to the invention for producing filaments on a substrate made of a brittle material, preferably glass or glass ceramics, can therefore be used to produce particularly fine and delicate surface structures.
[0111] It is therefore particularly well suited for supporting the production of microfluidic chips or cells.
[0112] The manufacture of a microfluidic cell according to another aspect of the invention is described in detail below. The simplest construction of the microfluidic cell is obtained by the combination of a lower part structured with passages and a cover with access to the passages. In the latest prior art, the microfluidic cell is manufactured from a polymer, for example by an injection molding method. Corresponding assemblies are known, for example, from EP 2 719 460 B1 and DE 10 2011 085 371 A1. However, the manufacture of a microfluidic cell from two polymer components results in the following disadvantages: - the polymers are often not resistant to the solvents used or lead to unspecified reactions with the biomolecules used (lack of biocompatibility); The autofluorescence and limited transparency of the polymers affect or hinder the sorting quality during the detection of fluorescent marker substances. Furthermore, polymer surfaces have only limited ability to be functionalized with biomarkers.
[0113] As a solution to this, the production of a three-component microfluidic cell has already been proposed, in which the lower and upper components are made of glass, which allows for a wide range of functionalizations. Furthermore, the passage structures are formed via organic polymer or silicon components, which are connected to the upper and lower parts, for example, by means of an adhesive that is applied already before structuring. Polymer components are described in EP 2547618 B1, and elements made of silicon are described in JP 2013188677 A2 and CN 103992948 B. EP 3037826 A1 further discloses a microfluidic cell having a sandwich structure consisting of an elastomer layer between two glass substrates. The bonding is carried out by direct bonding of surfaces activated, for example, by corona discharge. EP 3088076 A1 also describes a multi-layer cell in which a channel structure is fabricated in a silicon layer.
[0114] However, the combination of glass and polymer materials has the disadvantage that the different expansion coefficients of the components during the analysis, which undergoes different temperature cycles, lead to deformation of the cell and, in extreme cases, to non-sealing of the cell. Furthermore, the problems of biocompatibility and autofluorescence are not solved by this measure. Furthermore, with the plastic interlayer, the problem arises that the often very thin and long channel structures cannot be fully adjusted to the structures of the lower and upper parts during joining due to the lack of strength of the plastic. This adjustment problem is even more severe, since inexpensive production is only possible by producing large substrates with several cells at the same time.
[0115] The solution to the above-mentioned requirements is realized according to one aspect of the invention in that the microfluidic cell is manufactured from three glass components, in which the middle component (also called insert here) consists of structured thin glass and is bonded to the cover and the base by adhesive applied on both sides after structuring. All three components are thus made of inert, non-autofluorescent and easily functionalizable materials. No stresses due to different high thermal expansions occur. By using adhesive technology, the hermeticity of the cell can be easily guaranteed. By applying adhesive to the structured components, the surfaces of the base and the cover facing this cell can be provided with biomarkers inexpensively, individually and completely before the components are joined. Furthermore, adhesive technology makes it possible that particles from the plastic are not trapped and therefore no longer interfere with the joining process, and the hermeticity of the cell remains guaranteed. The requirements regarding the cleanliness of the process environment are therefore correspondingly lower. At least one of the glass components also has a cavity 5 which may be produced by the laser-assisted etching method described herein.
[0116] In particular, to produce a microfluidic cell, a cavity is machined in a disk-shaped glass element 200, in which a laser beam 27 of an ultrashort pulse laser 30 is directed onto one of the sides 2, 3 of the glass element 200 and focused by a focusing optic 23 to form an extended focus at the substrate 1; the incident energy of the laser beam 27 causes a filamentary damage 32 to be formed in the volume of the glass element 200, the filamentary damage 32 penetrating into the volume to a predefined depth, but without penetrating the glass element 200; To form the filamentary damage 32, the ultrashort pulsed laser 30 applies a pulse or a pulse packet comprising at least two consecutive laser pulses, and after processing at least two adjacent filamentary damages 32, - exposing the glass element to an etching medium 33, which - expanding at least two filamentous lesions 32 so that cavities are formed; In other words, in general, the structuring method according to the invention is used for glass elements, the glass element 200 is bonded on at least one of its two side faces to at least one further glass part, so that the opening of the cavity 5 is closed by the glass part and a cavity suitable in particular for the guidance of liquids is formed, the bonding between the glass element 200 and the glass part being effected by means of an applied adhesive, the opening of the cavity 5 in the glass element 200 being avoided when the adhesive is applied. The adhesive is preferably applied to the side face of the glass element 200. However, a structured application to the corresponding face of the glass part is also possible.
[0117] This results in a microfluidic cell 12, which comprises a disk-shaped glass element 200 with at least one cavity 5 open on one side, the side of the glass element 200 on which the cavity 5 is open being bonded to a glass part, so that the cavity 5 is closed by the glass part, and a cavity suitable for guiding a liquid is formed, enclosed between the glass element 200 with the cavity 5 and the glass part, in which the glass element 200 with the cavity 5 and the glass part are bonded by an adhesive layer, which has an open area around the opening of the cavity, so that the part of the wall of the cavity formed by the glass part is adhesive-free and is preferably formed by the material of the glass part closing the cavity 5.
[0118] According to an advantageous embodiment, the microfluidic cell 12 is produced by bonding at least three glass parts. Thus, a hollow structure suitable for the guidance of liquids can also be formed by the intermediate glass element 3 having one or more through-openings, which are then closed when bonding the two further glass parts. Thus, it is provided that a disk-shaped glass element having a thickness of at most 700 micrometers, preferably at most 500 micrometers, is structured in such a way that it has at least one opening, which connects the two parallel side faces of the glass element located opposite each other, and each side of the glass element is bonded to a glass part, so that the opening is closed by the two glass parts and a microfluidic cell with a cavity suitable for the guidance of liquids is formed between the further glass parts. In this case, the bonding of the glass element to at least one of the two glass parts is performed by an applied adhesive, which avoids at least one opening in the glass element when applying the adhesive. The adhesive is further preferably applied to the side of the glass element. However, a structured application to the corresponding face of the glass part is also possible. At least one of the glass elements, i.e. the middle glass element or the outer glass element, has a cavity according to the invention. The opening of this cavity is closed during bonding. The cavity may form a separate cavity or may be part of a cavity formed by an opening in the middle glass element.
[0119] Preferably, thinner glass is used for the intermediate glass element, i.e. glass with a thickness of at most 300 micrometers, for example not more than 210 micrometers. On the contrary, glass elements with a thickness of at most 100 micrometers, for example not more than 70 μm, can be structured and used as glass elements for microfluidic cells. For particularly small structures, thin glass with a thickness of at most 70 μm, preferably at most 50 μm or even only at most 30 μm, can also be structured with openings. Generally, for the production of openings, the same methods are suitable as for the production of cavities that are only open on one side, as already explained above with reference to FIG. 10. Thus, in one embodiment of the invention, it is provided that in addition to the cavities 5 that are open on one side, through openings are formed in the substrate 1, in particular by processing filament-like damage 32 that extends through the substrate and widening the filament-like damage 32 by an etching medium. The walls of such through openings thus typically have a spherical recess, like the cavities 5 that are open on one side. 10b, the through openings may extend from the cavity to the oppositely located side of the substrate, but it is equally possible that one through opening is formed in addition to the cavity 5.
[0120] In this regard, Figures 14 and 15 show in cross section an example of a microfluidic cell 12 with three glass parts, namely a glass element 200 and glass parts 201, 202. The glass element 200 has one or more through openings 101, which are closed by bonding with the glass parts 201, 202 and in this way form one or more cavities 91 of the microfluidic cell 12 for containing and / or guiding liquid. The glass part 201 has a through opening 401, which is connected to the cavities 91 and in this way serves as a filling opening.
[0121] 14 shows an example glass part 201 having a cavity 5 manufactured according to the present invention. This cavity 5 is arranged so as to connect both cavities 91, so that both cavities 9 communicate with each other via the cavity 5.
[0122] 15 shows an embodiment in which a cavity 5 is machined in the glass element 200 arranged between the two glass parts 201, 202. The cavity 5 forms, for example, a passage for connecting a filling opening 401 to the cavity 91. Both embodiments form the basis of an embodiment of the method in which the opening 401 is present or machined in at least one of the glass parts 201, 202. In this case, the glass parts 200, 201 are assembled with the glass element 200 in such a way that the opening 401 forms a connection for guiding a fluid into the cavity 91 formed during bonding.
[0123] The glass portions of the microfluidic cell 12 are bonded together as shown by an adhesive layer 151. The opening 101 and the cavity 5 do not have an adhesive layer 151. The adhesive is generally applied such that the edges of the through openings and cavities are free of adhesive.
[0124] FIG. 16 shows an assembly for coating the glass parts 201, 202 or the side surfaces 2 of the glass element 200 with an adhesive layer 151. The application of the adhesive here is carried out by a structured printing method, in which the adhesive is applied selectively on the respective side surfaces 2 of the glass element 200, avoiding the areas 131 that extend over the openings of the cavities 5 provided in the glass element 200. According to an embodiment of the invention, a printing device 171 is used for this, which comprises a print head 181 controlled by a computer 199. This print head 181 can be, for example, an inkjet print head that is moved over the glass element 200 and ejects the adhesive in the form of droplets during this movement. The computer 199 controls the print head in such a way that the areas 131 in which the elongated cavities 5 are located are left open. For example, the print head 181 can be moved in a meandering manner over the glass element 200. In this case, the print head 181 is reciprocated on a cross beam and moved in a lateral movement or alternatively the glass elements 200 are moved in a row-like manner. Generally, without being limited to the defined printing or application method, a refinement of the invention provides that the adhesive is applied in such a way that the area 131 free from the adhesive layer 151 is larger than the through opening or cavity to be avoided, whereby the edge 161 of the applied adhesive layer 151 is spaced away from, and in particular set back from, the edge 111 of the opening 101 or cavity 5.
[0125] The printing method as shown in FIG. 16 is purely exemplary. Other printing methods are tampon printing, screen printing, stencil printing, roll coating or roll-to-roll coating, coating, stamp transfer. For particularly large quantities, printing methods such as tampon printing or screen printing are suitable. In one embodiment, for the production of the microfluidic cell 12, an acrylate adhesive having a viscosity of 9600 mPa·s is applied to the glass element 200 on both sides by screen printing. The positioning marks allow not only the glass element 200 to be aligned with respect to the glass parts 201, 202, but also the screen printing mask to be aligned with respect to the structure of the microfluidic cell.
[0126] The viscosity of the adhesive may generally also be adapted to the printing process. Thus, for tampon printing, a low viscosity is advantageous, for example in the range of 300 mPa·s. For the exemplary inkjet process as illustrated in FIG. 16, an even lower viscosity is advantageous, preferably below 50 mPa·s.
[0127] A preferred embodiment of the invention provides that a light-curable, preferably UV-curable, adhesive 12 is applied. The adhesive 12 can thus be irradiated with light, preferably UV light, through one of the glass parts 5, 7, so that the adhesive hardens and, upon application to one glass part or both glass parts 201, 202, is rigidly bonded to the glass element 3. Suitable adhesives that may be UV-cured may be silicone-containing adhesives, epoxies and acrylates.
Claims
1. 1. A method for forming a cavity in a substrate made of a brittle material, comprising the steps of: - directing a laser beam (27) of an ultrashort pulse laser (30) towards one of the lateral sides (2, 3) of said substrate (2) and focusing it by a focusing optics (23) to form an extended focus at said substrate (1); forming a filament-like damage (32) in the volume of the substrate (1) by the incident energy of the laser beam (27), the filament-like damage (32) having a diameter of up to 1 μm and penetrating into the volume to a predefined depth, without penetrating the substrate (1); To form the filamentary lesion (32), the ultrashort pulse laser (30) delivers a pulse or a pulse packet having at least two consecutive laser pulses; After processing at least two filamentous wounds (32), - exposing said substrate (1) to an etching medium (33), which removes material of said substrate (1) at a removal rate of between 2 μm per hour and 20 μm per hour; and - expanding said at least two filamentous lesions (32) to form filaments (6); - a method for forming cavities in a substrate made of brittle material, comprising bonding at least two filaments to form a cavity (5), the walls (8) of which have a spherical recess (7), the cavity (5) having a depth of up to 5 mm and the taper angle of the walls of the cavity (5) relative to the adjacent sides of the substrate being in the range of 90° + / - 5°.
2. The method of claim 1 , wherein at least 20 filaments are bonded together to form one cavity.
3. 3. The method of claim 1, wherein t<0.8*T, where t=depth of the filamentary damage (32) in the substrate (1) and T=thickness of the substrate (1) at the location of the damage.
4. 4. The method according to claim 1, wherein the filamentary damage (32) has a diameter of at most 0.8 μm.
5. 5. The method according to claim 1, wherein at least two or more adjacent filament-like damages (32) are machined into the volume to a predefined depth that does not penetrate the substrate (1).
6. 6. The method according to claim 5, wherein each of two filamentary lesions (32) arranged next to each other have different depths.
7. 7. The method according to claim 1, wherein a number of filamentary damages (32) are processed along one path or line.
8. 8. The method according to claim 1, wherein a multiplicity of filamentary damages (32) are processed in the form of a two-dimensional pattern or matrix, in which a plurality of filamentary damages (32) are arranged along a path, and at least two paths are arranged next to each other.
9. The distance d between two adjacent filament-like lesions along one path x and the distance d between the two paths arranged side by side y and therefore, d x = d y The method of claim 8, wherein
10. The distance d between two adjacent filament-like lesions along one path x and the distance d between the two paths arranged side by side y and are different, so d x ≠d y The method of claim 8, wherein
11. d x is at least 10 μm, and d y The method of claim 9 or 10, wherein the thickness is at least 4 μm.
12. 12. The method according to claim 11, wherein when processing the filamentary damage portion (32) on the side of the substrate facing the incidence side of the laser beam (surface cavity), first longer filamentary damage portion (32) and then shorter filamentary damage portion (32) are processed, and when processing the filamentary damage portion (32) on the side of the substrate facing away from the incidence side of the laser beam (rear cavity), first shorter filamentary damage portion (32) and then longer filamentary damage portion (32).
13. 13. The method according to claim 1, further comprising forming through openings in the substrate (1) by machining filament-like damage (32) extending through the substrate (1) and expanding the filament-like damage (32) with the etching medium (33) in addition to the cavity (5).
14. A method for producing a microfluidic cell (12), comprising forming a cavity (5) in a disk-shaped glass element (200) by a method according to any one of claims 1 to 13, - at least one of the lateral sides of the glass element (200) is bonded to at least one further glass part, whereby the opening of the cavity (5) is closed by said glass part and a cavity suitable for the guidance of a liquid is formed, the bonding of the glass element (200) to said glass part being effected by an applied adhesive, A method for manufacturing a microfluidic cell (12).
Citation Information
Patent Citations
Method for manufacturing structure body, liquid drop delivery head and liquid drop delivery device
JP2005152693A
A method of arranging at least one recess or hole in a plate-like workpiece
JP2017534458A
Method and system for scribing and chemically etching brittle materials
JP2018509298A
Multi-layer microfluidic devices
US20020023684A1