Workpiece processing sheet

The polyolefin-based workpiece processing sheet with enhanced flexibility addresses the challenge of pick-up inefficiencies in thinner semiconductor wafers by ensuring effective chip separation.

JP7562278B2Active Publication Date: 2024-10-07LINTEC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020052567
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-24
Publication Date
2024-10-07
Estimated Expiration
2040-03-24

Smart Images

  • Figure 0007562278000002
    Figure 0007562278000002
  • Figure 0007562278000003
    Figure 0007562278000003
  • Figure 0007562278000004
    Figure 0007562278000004
Patent Text Reader

Abstract

To provide a workpiece processing sheet having excellent pickup properties.SOLUTION: Workpiece processing sheets 1A, 1B, 1C each include a base material 11 and an adhesive layer 12 laminated on one side of the base material 11. The base materials 11 of the workpiece processing sheets 1A, 1B and 1C include a resin layer 111a, resin layers 111b, 111c, and resin layers 111d, 111e, 111f, respectively, formed from a resin composition containing a polyolefin-based resin, the base material 11 having a stress relaxation rate after 5 minutes of 10% stretching of 35% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a workpiece processing sheet used for processing a workpiece such as a semiconductor wafer. [Background technology]

[0002] Semiconductor wafers such as silicon and gallium arsenide and various packages are manufactured in a large diameter state, cut (diced) into chips, peeled (picked up), and then transferred to the next process, the mounting process. At this time, the workpieces such as semiconductor wafers are stacked on an adhesive sheet (hereinafter sometimes referred to as a "workpiece processing sheet") that has a base material and an adhesive layer, and are processed by back grinding, dicing, cleaning, drying, expanding, picking up, mounting, etc.

[0003] The workpiece processing sheet is required to have various properties for processing the workpiece well. For example, the workpiece processing sheet is required to have the property of suppressing the generation of cutting chips generated during dicing. In general, when dicing a workpiece using a rotating circular blade (dicing blade), the circular blade may come into contact with the workpiece processing sheet, scraping the workpiece processing sheet and generating cutting chips. Therefore, the workpiece processing sheet is required to have the property of suppressing the generation of the cutting chips and preventing the cutting chips from adversely affecting the product.

[0004] For the purpose of suppressing the generation of the cutting chips, Patent Document 1 discloses an invention in which a polyolefin film irradiated with electron beams or gamma (γ) rays at 1 to 80 Mrad is used as the base film of a dicing sheet. In this invention, it is believed that the irradiation of electron beams or gamma rays forms crosslinks by covalent bonds in the resin constituting the base film, suppressing the generation of cutting chips. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-211234 Summary of the Invention [Problem to be solved by the invention]

[0006] In addition, in the above-mentioned pick-up process, in order to facilitate picking up the obtained chips, the chips are usually pushed up individually from the side of the workpiece processing sheet opposite to the side on which the chips are stacked. This pushing up makes it easier to separate the chips from the workpiece processing sheet. In addition, the pushing up can also prevent the pickup means (collet, etc.) from interfering with the surrounding chips. Therefore, the workpiece processing sheet is required to have the performance to perform the above-mentioned pushing up well and thereby enable good pick-up.

[0007] Conventional inventions such as that disclosed in Patent Document 1 also have a certain degree of pick-up property that enables good pick-up. However, in recent years, workpieces have become thinner and chip sizes have become smaller, and there is a need for pick-up properties superior to those of conventional workpiece processing sheets.

[0008] The present invention has been made in view of the above circumstances, and has an object to provide a workpiece processing sheet having excellent pick-up properties. [Means for solving the problem]

[0009] In order to achieve the above-mentioned object, firstly, the present invention provides a workpiece processing sheet comprising a substrate and an adhesive layer laminated on one side of the substrate, characterized in that the substrate comprises a resin layer formed from a resin composition containing a polyolefin-based resin, and the stress relaxation rate of the substrate after 10% elongation for 5 minutes is 35% or more (Invention 1).

[0010] The workpiece processing sheet according to the above invention (Invention 1) has a resin layer formed from a resin composition containing a polyolefin-based resin, and since the stress relaxation rate of the base material is within the above range, it is possible to perform good pushing up of the workpiece processing sheet, and excellent pick-up properties are achieved.

[0011] In the above invention (Invention 1), the proportion of the polyolefin resin in the resin composition is preferably 30% by mass or more and 100% by mass or less (Invention 2).

[0012] In the above inventions (Inventions 1 and 2), the resin composition preferably contains a thermoplastic elastomer other than the polyolefin resin (Invention 3).

[0013] In the above invention (Invention 3), the thermoplastic elastomer is preferably an olefin-based elastomer (Invention 4).

[0014] In the above invention (Invention 4), the proportion of the olefin-based elastomer in the resin composition is preferably 1% by mass or more and 50% by mass or less (Invention 5).

[0015] In the above inventions (Inventions 1 to 5), the substrate preferably consists of a single resin layer (Invention 6).

[0016] In the above inventions (Inventions 1 to 5), it is preferable that the substrate is made of a plurality of layers, at least one of which is the resin layer (Invention 7).

[0017] In the above inventions (Inventions 1 to 7), the thickness of the substrate is preferably 25 μm or more and 300 μm or less (Invention 8).

[0018] In the above inventions (Inventions 1 to 8), the pressure-sensitive adhesive layer is preferably made of an acrylic pressure-sensitive adhesive (Invention 9).

[0019] In the above inventions (Inventions 1 to 9), a dicing sheet is preferable (Invention 10). Effect of the Invention

[0020] The workpiece processing sheet according to the present invention has excellent pick-up properties. [Brief description of the drawings]

[0021] [Figure 1] 1 is a cross-sectional view of a workpiece processing sheet according to one embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view of a workpiece processing sheet according to another embodiment of the present invention. [Diagram 3] FIG. 11 is a cross-sectional view of a workpiece processing sheet according to yet another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment of the present invention will be described. A cross-sectional view of a workpiece processing sheet according to one embodiment is shown in Fig. 1. The workpiece processing sheet 1A shown in Fig. 1 includes a base material 11 and an adhesive layer 12 laminated on one side of the base material 11.

[0023] A cross-sectional view of a workpiece processing sheet according to another embodiment is shown in Fig. 2. The workpiece processing sheet 1B shown in Fig. 2 also includes a base material 11 and an adhesive layer 12 laminated on one side of the base material 11.

[0024] A cross-sectional view of a workpiece processing sheet according to yet another embodiment is shown in Fig. 3. The workpiece processing sheet 1C shown in Fig. 3 also includes a base material 11 and an adhesive layer 12 laminated on one side of the base material 11.

[0025] In the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment, the base material 11 has a resin layer formed from a resin composition containing a polyolefin resin. In particular, in the workpiece processing sheet 1A shown in FIG. 1, the base material 11 is composed of a single layer of resin layer 111a. In the workpiece processing sheet 1B shown in FIG. 2, the base material 11 is composed of two layers, all of which are resin layers 111b and 111c. Furthermore, in the workpiece processing sheet 1C shown in FIG. 3, the base material 11 is composed of three layers, all of which are resin layers 111d, 111e, and 111f.

[0026] Furthermore, in the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment, the stress relaxation rate of the base material 11 after 10% stretching for 5 minutes is 35% or more.

[0027] As described above, the substrate 11 has a resin layer formed from a resin composition containing a polyolefin resin, and the stress relaxation rate of the substrate 11 is 35% or more after 10% elongation for 5 minutes, so that the substrate 11 has a suitable flexibility and can be easily pushed up to a sufficient height when the workpiece processing sheets 1A, 1B, and 1C are pushed up with a needle. This allows for good pickup.

[0028] From the viewpoint of enabling better push-up, the stress relaxation rate of the substrate 11 is preferably 36% or more, and particularly preferably 40% or more. The upper limit of the stress relaxation rate of the substrate 11 is preferably 60% or less, particularly preferably 50% or less, and further preferably 46% or less, from the viewpoint of the substrate having a predetermined rigidity and enabling the workpieces to be stably stacked. The details of the method for measuring the stress relaxation rate are as described in the test example described later. In this specification, the stress relaxation rate of the substrate 11 after 5 minutes of 10% elongation is calculated from the load when the substrate 11 is elongated by 10% and stopped in that state for 5 minutes and the load after 5 minutes have elapsed. In addition, the stress relaxation rate of the substrate 11 in this specification refers to the average value of the stress relaxation rate measured in the MD direction of the substrate 11 (flow direction during substrate production) and the stress relaxation rate measured in the CD direction of the substrate 11 (direction perpendicular to the MD direction).

[0029] 1. Composition of workpiece processing sheet (1) Base material The substrate 11 in this embodiment includes a resin layer formed from a resin composition containing a polyolefin resin. The substrate 11 may be made of only a single layer, and in that case, as shown in FIG. 1, the substrate 11 is made of only the resin layer 111a. The substrate 11 made of a single resin layer 111a is preferable in terms of reducing manufacturing costs. The substrate 11 may be made of multiple layers, and in that case, at least one of the layers is a resin layer. The substrate 11 shown in FIG. 2 is made of two layers, all of which are resin layers (resin layers 111b and 111c, respectively). The substrate 11 shown in FIG. 3 is made of three layers, all of which are resin layers (resin layers 111d, 111e, and 111f, respectively). A substrate made of multiple layers is preferable in that it can achieve both the effect of improving the pickup property mainly due to the resin layer and the desired effect due to layers other than the resin layer.

[0030] The components other than the polyolefin resin contained in the resin composition for forming the resin layer are not particularly limited as long as they enable the formation of the resin layer. It is also preferable that the resin composition contains a thermoplastic elastomer. By containing the thermoplastic elastomer, it becomes easier to adjust the stress relaxation rate of the substrate 11 to the above-mentioned range, and therefore it becomes possible to achieve better pick-up properties.

[0031] Furthermore, when the base material 11 includes a layer other than the resin layer, the material of the layer is not particularly limited as long as the material enables the formation of the layer and the base material 11.

[0032] (1-1) Polyolefin resin Specific examples of polyolefin resins contained in the resin composition for forming the resin layer are not particularly limited. In this specification, the polyolefin resin refers to a homopolymer or copolymer having an olefin as a monomer, or a copolymer having an olefin and a molecule other than an olefin as a monomer, in which the mass ratio of the part based on the olefin unit in the polymerized resin is 1.0 mass% or more.

[0033] The polymer constituting the polyolefin resin may be linear or may have a side chain. The polyolefin resin may have a functional group. The functional group may be an aromatic ring or an aliphatic ring, or may be an acyclic functional group.

[0034] Examples of olefin monomers constituting polyolefin resins include olefin monomers having 2 to 8 carbon atoms, α-olefin monomers having 3 to 18 carbon atoms, and olefin monomers having a cyclic structure. Examples of olefin monomers having 2 to 8 carbon atoms include ethylene, propylene, 2-butene, and octene. Examples of α-olefin monomers having 3 to 18 carbon atoms include propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, and 1-octadecene. Examples of olefin monomers having a cyclic structure include norbornene, cyclopentadiene, cyclohexadiene, dicyclopentadiene, and tetracyclododecene, as well as derivatives thereof.

[0035] When the polyolefin resin contains polyethylene, the polyethylene may be any one of high density polyethylene, medium density polyethylene, low density polyethylene, very low density polyethylene and linear low density polyethylene, or a mixture of two or more of these.

[0036] The polyolefin resins may be used alone or in combination of two or more.

[0037] Among the specific examples of the polyolefin resins mentioned above, it is preferable to use at least one of polyethylene containing ethylene as a main polymerization unit and polypropylene containing propylene as a main polymerization unit, from the viewpoint of easiness in achieving the above-mentioned stress relaxation rate.

[0038] As the polypropylene, for example, homopolypropylene, random polypropylene and block polypropylene are preferably used. These can be used alone or in combination of two or more. In particular, from the viewpoint of easily achieving the above-mentioned stress relaxation rate, it is preferable to use a mixture of homopolypropylene and random polypropylene.

[0039] The homopolypropylene, random polypropylene and block polypropylene may be commercially available products. Examples of commercially available homopolypropylene include Prime Polypro E111G, Prime Polypro E-100GV, Prime Polypro E-100GPL, Prime Polypro E-200GP, etc., all manufactured by Prime Polymer. Examples of commercially available random polypropylene include Prime Polypro B221WA, Prime Polypro B241, Prime Polypro E222, Prime Polypro E-333GV, etc., all manufactured by Prime Polymer. Examples of commercially available block polypropylene include Prime Polypro E701G, Prime Polypro E702G, Prime Polypro E702MG, etc., all manufactured by Prime Polymer.

[0040] As the polyethylene, it is preferable to use low-density polyethylene, and examples of commercially available products include "Novatec LL" manufactured by Mitsubishi Chemical Corporation, and the Neozex series and Ultraozex series manufactured by Prime Polymer Co., Ltd.

[0041] The proportion of polyolefin resin in the resin composition for forming the resin layer is preferably 30% by mass or more, particularly preferably 40% by mass or more, and more preferably 65% ​​by mass or more. The proportion is preferably 100% by mass or less, particularly preferably 95% by mass or less, and more preferably 90% by mass or less. By having the proportion of polyolefin resin in the resin composition within the above range, the work processing sheets 1A, 1B, and 1C according to this embodiment can easily achieve better pick-up properties.

[0042] (1-2) Thermoplastic elastomer The thermoplastic elastomer is not particularly limited as long as it is other than the polyolefin-based resin and enables the formation of the substrate 11. Examples of the thermoplastic elastomer include, for example, an olefin-based elastomer, a rubber-based elastomer, a urethane-based elastomer, a styrene-based elastomer, an acrylic-based elastomer, and a vinyl chloride-based elastomer. These may be used alone or in combination of two or more kinds.

[0043] Among the above-mentioned elastomers, olefin-based elastomers are preferred from the viewpoint of easily achieving the above-mentioned stress relaxation rate for the substrate 11. In this specification, the term "olefin-based elastomer" refers to a copolymer containing structural units derived from olefin or its derivatives (olefin-based compounds), and means a material that has rubber-like elasticity and thermoplasticity in a temperature range including room temperature.

[0044] Examples of olefin-based elastomers include those containing at least one resin selected from the group consisting of ethylene-α-olefin copolymer, propylene-α-olefin copolymer, butene-α-olefin copolymer, ethylene-propylene-α-olefin copolymer, ethylene-butene-α-olefin copolymer, propylene-butene-α-olefin copolymer, and ethylene-propylene-butene-α-olefin copolymer. Among these, propylene-α-olefin copolymer is preferred, and propylene-ethylene-α-butylene copolymer is particularly preferred.

[0045] The proportion of the thermoplastic elastomer in the resin composition for forming the resin layer is preferably 1% by mass or more, particularly preferably 10% by mass or more, and more preferably 15% by mass or more. The proportion is preferably 60% by mass or less, particularly preferably 30% by mass or less, and more preferably 20% by mass or less. When the proportion of the thermoplastic elastomer in the resin composition is within the above range, it becomes easier to achieve the above-mentioned stress relaxation rate, and therefore the work processing sheets 1A, 1B, and 1C according to this embodiment can easily achieve better pick-up properties.

[0046] In addition, when the thermoplastic elastomer is an olefin-based elastomer, the proportion of the olefin-based elastomer in the resin composition for forming the resin layer is preferably 1% by mass or more, particularly preferably 10% by mass or more, and more preferably 13% by mass or more. In addition, the above proportion is preferably 50% by mass or less, particularly preferably 20% by mass or less, and more preferably 17% by mass or less. By having the proportion of the olefin-based elastomer in the resin composition within the above range, it becomes easier to achieve the above-mentioned stress relaxation rate, and therefore the work processing sheets 1A, 1B, and 1C according to this embodiment can easily achieve better pick-up properties.

[0047] In addition, although the resin composition for forming the resin layer may contain a styrene-based elastomer as a thermoplastic elastomer, from the viewpoint of easily achieving the above-mentioned stress relaxation rate, it is preferable that the content is small, and in particular, it is preferable that the resin composition does not substantially contain a styrene-based elastomer. When a styrene-based elastomer is contained in the resin composition, a pseudo-crosslinked structure between the styrene-based elastomers is easily formed in the formed resin layer. Therefore, by using a resin composition that does not substantially contain a styrene-based elastomer, the formation of the above-mentioned pseudo-crosslinked structure can be reduced, and as a result, the above-mentioned stress relaxation rate is easily achieved. In addition, in this specification, the "styrene-based elastomer" means a copolymer containing a structural unit derived from styrene or its derivative (styrene-based compound), and a material that has rubber-like elasticity and thermoplasticity in a temperature range including room temperature.

[0048] When the resin composition contains a styrene-based elastomer, the proportion thereof is preferably less than 10% by mass, particularly preferably 5% by mass or less, and further preferably 1% by mass or less. The above-mentioned case where the styrene-based elastomer is substantially not contained specifically means that the proportion of the styrene-based elastomer in the resin composition is 0.2% by mass or less.

[0049] (1-3) Other ingredients The resin composition for forming the resin layer may contain other components in addition to the polyolefin resin and thermoplastic elastomer described above. In particular, the resin composition may contain components used in the base material of general work processing sheets.

[0050] Examples of such components include various additives such as antistatic agents, flame retardants, plasticizers, lubricants, antioxidants, colorants, infrared absorbing agents, ultraviolet absorbing agents, ion scavengers, etc. The content of these additives is not particularly limited, but is preferably within a range in which the substrate exhibits the desired function.

[0051] Among them, the resin composition for forming the resin layer preferably contains an antistatic agent. The antistatic agent may be a low molecular weight antistatic agent or a polymeric antistatic agent, but a polymeric antistatic agent is preferred. Examples of the polymeric antistatic agent include vinyl copolymers having sulfonate in the molecule, alkylsulfonates, alkylbenzenesulfonates, betaines, etc. Furthermore, examples of the inorganic protonic acid salts of polyether, polyamide elastomer, polyester elastomer, polyether amide, or polyether ester amide may include salts of inorganic protonic acid. Examples of the inorganic protonic acid salts include alkali metal salts, alkaline earth metal salts, zinc salts, or ammonium salts.

[0052] When the resin composition for forming the resin layer contains an antistatic agent, the proportion of the antistatic agent in the resin composition is preferably 3% by mass or more and 20% by mass or less. When the proportion of the antistatic agent in the resin composition is within the above range, the obtained substrate 11 tends to have good antistatic properties.

[0053] (1-4) Surface treatment of substrate The surface of the substrate 11 on which the adhesive layer 12 is laminated may be subjected to a surface treatment such as a primer treatment, a corona treatment, a plasma treatment, a roughening treatment (matt finish) or the like in order to enhance adhesion to the adhesive layer 12. Examples of the roughening treatment include an embossing method and a sandblasting method. Among these, the embossing method is preferable.

[0054] (1-5) Manufacturing method of substrate The method for producing the substrate 11 in this embodiment is not particularly limited as long as the above-mentioned resin composition is used, and for example, melt extrusion methods such as the T-die method and the round die method, calendar method, solution method such as the dry method and the wet method, etc. can be used. Among these, from the viewpoint of efficiently producing the substrate, it is preferable to adopt the melt extrusion method, and it is particularly preferable to adopt the T-die method.

[0055] When the substrate 11 consisting of a single resin layer is produced by the melt extrusion method, the resin composition is kneaded, and the kneaded product obtained is directly or once produced into pellets, and then formed into a film using a known extruder. In this case, it is preferable to immediately cool the material to room temperature using a cooling roll or the like immediately after extrusion using the extruder, from the viewpoint of facilitating the achievement of the above-mentioned degree of crystallinity.

[0056] In addition, when the substrate 11 consisting of multiple layers is manufactured by the melt extrusion method, the components constituting each layer are kneaded respectively, and the resulting kneaded mixture is extruded directly or after pellets are once produced, by using a known extruder to simultaneously extrude the multiple layers to form a film. In this case, too, from the viewpoint of easily achieving the above-mentioned crystallinity, it is preferable to immediately cool to room temperature immediately after extrusion.

[0057] After the film is formed by the above-mentioned melt extrusion method or the like, the obtained substrate 11 may be irradiated with an electron beam, but it is preferable not to irradiate with the electron beam in order to easily achieve the above-mentioned stress relaxation rate. In general, electron beam irradiation promotes the formation of a crosslinked structure between the resins constituting the substrate. Therefore, by not irradiating with the electron beam and suppressing the excessive formation of the crosslinked structure, it becomes easier to achieve the above-mentioned stress relaxation rate.

[0058] (1-6) Thickness of the substrate In this embodiment, the thickness of the base material 11 is preferably 25 μm or more, and particularly preferably 50 μm or more. The thickness of the base material 11 is preferably 300 μm or less, particularly preferably 200 μm or less, and further preferably 150 μm or less. When the thickness of the base material is 25 μm or more, the workpiece processing sheets 1A, 1B, and 1C tend to have a moderate strength, and the workpieces fixed on the workpiece processing sheets 1A, 1B, and 1C tend to be well supported. When the thickness of the base material 11 is 300 μm or less, the thickness of the workpiece processing sheets 1A, 1B, and 1C tend to have a better flexibility, which can further improve the pick-up property and facilitate good expansion.

[0059] (2) Adhesive layer The adhesive constituting the adhesive layer 12 in this embodiment is not particularly limited as long as it can exert sufficient adhesive strength to the adherend (particularly, sufficient adhesive strength to the workpiece for processing the workpiece). Examples of the adhesive constituting the adhesive layer 12 include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, polyvinyl ether adhesives, etc. Among these, it is preferable to use acrylic adhesives from the viewpoint of easily exerting the desired adhesive strength.

[0060] The adhesive constituting the adhesive layer 12 in this embodiment may be an adhesive not having active energy ray curability, but is preferably an adhesive having active energy ray curability (hereinafter, may be referred to as "active energy ray curable adhesive"). Since the adhesive layer 12 is composed of an active energy ray curable adhesive, the adhesive layer 12 can be cured by irradiation with active energy rays, and the adhesive strength of the workpiece processing sheets 1A, 1B, and 1C to the adherend can be easily reduced. In particular, the irradiation with active energy rays makes it possible to easily separate the processed workpiece from the workpiece processing sheets 1A, 1B, and 1C.

[0061] The active energy ray curable adhesive constituting the adhesive layer 12 may be one mainly composed of a polymer having active energy ray curability, or may be one mainly composed of a mixture of a non-active energy ray curable polymer (a polymer not having active energy ray curability) and a monomer and / or oligomer having at least one or more active energy ray curable groups. The active energy ray curable adhesive may also be a mixture of a polymer having active energy ray curability and a monomer and / or oligomer having at least one or more active energy ray curable groups.

[0062] The active energy ray curable polymer is preferably a (meth)acrylic acid ester polymer (hereinafter sometimes referred to as "active energy ray curable polymer") having a functional group (active energy ray curable group) having active energy ray curability introduced into a side chain. This active energy ray curable polymer is preferably obtained by reacting an acrylic polymer having a functional group-containing monomer unit with an unsaturated group-containing compound having a functional group bonded to the functional group. In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. Furthermore, the term "polymer" also includes the concept of "copolymer".

[0063] The acrylic polymer having the functional group-containing monomer unit described above may be obtained by polymerizing other monomers together with the functional group-containing monomer. As such functional group-containing monomers and other monomers, as well as the unsaturated group-containing compounds described above, known compounds can be used, for example, those disclosed in International Publication No. 2018 / 084021.

[0064] The weight average molecular weight of the active energy radiation curable polymer is preferably 10,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more. The weight average molecular weight is preferably 1,500,000 or less, and even more preferably 1,000,000 or less. The weight average molecular weight (Mw) in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0065] As the above-mentioned active energy ray non-curable polymer component, for example, the above-mentioned acrylic polymer before being reacted with the unsaturated group-containing compound can be used.

[0066] The weight average molecular weight of the acrylic polymer as the non-curable active energy ray polymer component is preferably 10,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more. The weight average molecular weight is preferably 1,500,000 or less, and even more preferably 1,000,000 or less.

[0067] As the above-mentioned monomer and / or oligomer having at least one active energy ray-curable group, for example, an ester of a polyhydric alcohol and (meth)acrylic acid can be used.

[0068] When ultraviolet rays are used as the active energy rays for curing the active energy ray-curable adhesive, it is preferable to add a photopolymerization initiator to the adhesive. In addition, the adhesive may also contain an active energy ray non-curable polymer component or oligomer component, a crosslinking agent, etc.

[0069] The thickness of the adhesive layer 12 in this embodiment is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. The thickness of the adhesive layer 12 is preferably 70 μm or less, more preferably 30 μm or less, and even more preferably 10 μm or less. When the thickness of the adhesive layer 12 is in the above-mentioned range, the workpiece processing sheets 1A, 1B, and 1C according to this embodiment can easily exhibit the desired adhesiveness.

[0070] (3) Release sheet In the workpiece processing sheets 1A, 1B, and 1C according to this embodiment, a release sheet may be laminated on the side of the adhesive layer 12 opposite the substrate 11 (hereinafter sometimes referred to as the "adhesive side") in order to protect said side until it is attached to the workpiece.

[0071] The release sheet may have any structure, and may be, for example, a plastic film that has been subjected to a release treatment using a release agent or the like. Specific examples of the plastic film include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, and polyolefin films such as polypropylene and polyethylene. The release agent may be silicone-based, fluorine-based, or long-chain alkyl-based, and among these, silicone-based, which is inexpensive and provides stable performance, is preferred.

[0072] There is no particular limitation on the thickness of the release sheet, and it may be, for example, 20 μm or more and 250 μm or less.

[0073] (4)Other In the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment, an adhesive layer may be laminated on the surface of the adhesive layer 12 opposite to the substrate 11. In this case, the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment can be used as dicing and die bonding sheets. In the sheet, a workpiece is attached to the surface of the adhesive layer opposite to the adhesive layer 12, and the adhesive layer is diced together with the workpiece to obtain a chip on which the individualized adhesive layer is laminated. The individualized adhesive layer makes it possible for the chip to be easily fixed to the object on which the chip is to be mounted. As the material constituting the above-mentioned adhesive layer, it is preferable to use one containing a thermoplastic resin and a low molecular weight thermosetting adhesive component, one containing a B-stage (semi-cured) thermosetting adhesive component, or the like.

[0074] In addition, in the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment, a protective film forming layer may be laminated on the adhesive surface of the adhesive layer 12. In this case, the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment can be used as a sheet for forming a protective film and dicing. In such a sheet, a workpiece is attached to the surface of the protective film forming layer opposite to the adhesive layer 12, and the protective film forming layer is diced together with the workpiece to obtain a chip on which the individualized protective film forming layer is laminated. As the workpiece, it is preferable to use one having a circuit formed on one side, and in this case, the protective film forming layer is usually laminated on the surface opposite to the surface on which the circuit is formed. The individualized protective film forming layer can be cured at a predetermined timing to form a protective film having sufficient durability on the chip. The protective film forming layer is preferably made of an uncured curable adhesive.

[0075] 2. Manufacturing method of workpiece processing sheet The method for producing the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment is not particularly limited. For example, it is preferable to obtain the workpiece processing sheets 1A, 1B, and 1C by forming an adhesive layer 12 on a release sheet, and then laminating one side of a substrate 11 on the side of the adhesive layer 12 opposite to the release sheet.

[0076] The pressure-sensitive adhesive layer 12 can be formed by a known method. For example, a coating liquid containing a pressure-sensitive adhesive composition for forming the pressure-sensitive adhesive layer 12 and, if desired, a solvent or a dispersion medium is prepared. Then, the coating liquid is applied to the surface having releasability of a release sheet (hereinafter, sometimes referred to as the "release surface"). Then, the obtained coating film is dried to form the pressure-sensitive adhesive layer 12.

[0077] The coating of the coating liquid described above can be carried out by a known method, for example, a bar coating method, a knife coating method, a roll coating method, a blade coating method, a die coating method, a gravure coating method, etc. The nature of the coating liquid is not particularly limited as long as it can be applied, and the coating liquid may contain the components for forming the pressure-sensitive adhesive layer 12 as a solute or as a dispersoid. The release sheet may be peeled off as a processing material, or may protect the pressure-sensitive adhesive layer 12 until it is attached to the adherend.

[0078] When the adhesive composition for forming the adhesive layer 12 contains the above-mentioned crosslinking agent, it is preferable to change the above-mentioned drying conditions (temperature, time, etc.) or to separately provide a heat treatment to advance the crosslinking reaction between the polymer component in the coating film and the crosslinking agent, thereby forming a crosslinked structure with a desired density in the adhesive layer 12. Furthermore, in order to advance the above-mentioned crosslinking reaction sufficiently, after the adhesive layer 12 and the substrate 11 are laminated together, curing may be performed by leaving the adhesive layer 12 to stand for several days in an environment of 23°C and a relative humidity of 50%.

[0079] 3. How to use the workpiece processing sheet The workpiece processing sheets 1A, 1B, and 1C according to the present embodiment can be used for processing workpieces such as semiconductor wafers. That is, after the adhesive surface of the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment is attached to the workpiece, the workpiece can be processed on the workpiece processing sheets 1A, 1B, and 1C. Depending on the processing, the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment can be used as a backgrind sheet, a dicing sheet, an expanding sheet, a pick-up sheet, and the like. Here, examples of the workpiece include semiconductor members such as semiconductor wafers and semiconductor packages, and glass members such as glass plates.

[0080] As described above, the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment can achieve excellent pick-up properties. Therefore, the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment are particularly suitable for use as dicing sheets and pick-up sheets among the above-mentioned workpiece processing sheets.

[0081] In addition, when the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment have the above-mentioned adhesive layer, the workpiece processing sheets 1A, 1B, and 1C can be used as dicing and die bonding sheets. Furthermore, when the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment have the above-mentioned protective film forming layer, the workpiece processing sheets 1A, 1B, and 1C can be used as protective film forming and dicing sheets.

[0082] In addition, when the adhesive layer 12 in the workpiece processing sheets 1A, 1B, and 1C according to the present embodiment is composed of the above-mentioned active energy ray-curable adhesive, it is also preferable to irradiate the adhesive layer 12 with active energy rays during use. That is, when the processing of the workpiece is completed on the workpiece processing sheets 1A, 1B, and 1C and the processed workpiece is to be separated from the workpiece processing sheets 1A, 1B, and 1C, it is preferable to irradiate the adhesive layer 12 with active energy rays before the separation. This hardens the adhesive layer 12, effectively reducing the adhesive force of the adhesive sheet to the processed workpiece, and facilitating the separation of the processed workpiece.

[0083] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0084] For example, in the workpiece processing sheets 1A, 1B, and 1C according to this embodiment, other layers may be laminated between the base material 11 and the adhesive layer 12, or on the side of the base material 11 opposite the adhesive layer 12. EXAMPLES

[0085] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0086] Example 1 (1) Preparation of substrate 70 parts by mass of random polypropylene resin (Prime Polymer Co., Ltd., product name "Prime Polypro E222"), 10 parts by mass of homopolypropylene resin (Prime Polymer Co., Ltd., product name "Prime Polypro E100-GPL"), 15 parts by mass of olefin-based thermoplastic elastomer (Mitsui Chemicals, Inc., product name "Tafmer PN2070", propylene unit: ethylene unit: α-butylene unit = 70:15:15), and 5 parts by mass of antistatic agent (Sanyo Chemical Co., Ltd., product name "Pelestat") were each dried and then kneaded in a twin-screw kneader.

[0087] The pellets thus obtained were put into a hopper of a single-screw extruder equipped with a T-die. The pellets were extruded from the T-die in a melt-kneaded state under conditions of a cylinder temperature of 200° C. and a die temperature of 200° C., and immediately cooled by a cooling roll to obtain a sheet-like substrate having a thickness of 80 μm.

[0088] (2) Preparation of adhesive composition 38 parts by mass of 2-ethylhexyl acrylate, 37 parts by mass of vinyl acetate, and 25 parts by mass of 2-hydroxyethyl acrylate were polymerized by solution polymerization to obtain a (meth)acrylic acid ester polymer. This (meth)acrylic acid ester polymer was reacted with 30 g of methacryloyloxyethyl isocyanate (MOI) per 100 g of the (meth)acrylic acid ester polymer (corresponding to 80 mol % relative to 2-hydroxyethyl acrylate), to obtain an acrylic polymer having an active energy ray curable group introduced into the side chain. The weight average molecular weight (Mw) of this acrylic polymer was measured by the method described below and was found to be 600,000.

[0089] 100 parts by mass (solid content equivalent, the same below) of the acrylic polymer obtained above having active energy ray-curable groups introduced into the side chains, 7 parts by mass of 1-hydroxy-cyclohexyl-phenyl-ketone (manufactured by BASF, product name "Omnirad 184") as a photopolymerization initiator, and 0.2 parts by mass of trimethylolpropane-modified tolylene diisocyanate (manufactured by Tosoh, product name "Coronate L") as a crosslinking agent were mixed in a solvent to obtain a coating solution of an adhesive composition.

[0090] (3) Formation of adhesive layer The adhesive composition coating solution obtained in step (2) above was applied to the release surface of a release sheet (manufactured by Lintec Corporation, product name "SP-PET381031") consisting of a 38 μm-thick polyethylene terephthalate film with a silicone-based release agent layer formed on one side thereof, and the resulting sheet was dried by heating to obtain a laminate consisting of a 5 μm-thick adhesive layer formed on the release sheet.

[0091] (4) Preparation of adhesive sheet One side of the substrate obtained in the above step (1) was bonded to the adhesive layer side of the laminate obtained in the above step (3) to obtain a workpiece processing sheet.

[0092] The weight average molecular weight (Mw) mentioned above is a weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement) and converted into standard polystyrene. <Measurement conditions> Measuring device: Tosoh HLC-8320 GPC columns (passed in the following order): Tosoh Corporation TSK gel superH-H TSK gel superHM-H TSK gel superH2000 Measurement solvent: Tetrahydrofuran ·Measurement temperature: 40℃

[0093] Example 2 A workpiece processing sheet was obtained in the same manner as in Example 1, except that the amount of the base material was changed to 70 parts by mass of random polypropylene resin, 5 parts by mass of homopolypropylene resin, 20 parts by mass of olefin-based thermoplastic elastomer, and 5 parts by mass of antistatic agent.

[0094] Example 3 A workpiece processing sheet was obtained in the same manner as in Example 1, except that the amount of the base material was changed to 65 parts by mass of random polypropylene resin, 5 parts by mass of homopolypropylene resin, 25 parts by mass of olefin-based thermoplastic elastomer, and 5 parts by mass of antistatic agent.

[0095] Example 4 A workpiece processing sheet was obtained in the same manner as in Example 1, except that the amount of the base material was changed to 60 parts by mass of random polypropylene resin, 5 parts by mass of homopolypropylene resin, 30 parts by mass of olefin-based thermoplastic elastomer, and 5 parts by mass of antistatic agent.

[0096] Comparative Example 1 Ethylene-methacrylic acid copolymer (EMAA) (manufactured by Mitsui DuPont Polychemicals, product name "Nucrel N0903HC") was extruded using a small T-die extruder (manufactured by Toyo Seiki Seisakusho, product name "Labo Plastomill") to obtain an EMAA film with a thickness of 80 μm.

[0097] One side of the EMAA film obtained as described above was irradiated with electron beams under the following conditions. The EMAA film after electron beam irradiation was used as a substrate, and a pressure-sensitive adhesive layer was laminated on the surface of the substrate that had been irradiated with electron beams. A workpiece processing sheet was obtained in the same manner as in Example 1. Electron beam irradiation conditions Irradiation amount: 110kGy Number of exposures: 1 Accumulative irradiation dose: 110kGy

[0098] Comparative Example 2 A workpiece processing sheet was produced in the same manner as in Comparative Example 1, except that the irradiation conditions for electron beam irradiation during preparation of the substrate were changed as follows. Electron beam irradiation conditions Irradiation amount: 110kGy Number of exposures: 2 Accumulative irradiation dose: 220kGy

[0099] [Test Example 1] (Measurement of stress relaxation rate of substrate) The substrates prepared in the examples and comparative examples were cut into a shape of test piece type 2 (width 15 mm × length 100 mm) in accordance with JIS K7127:1999 (ISO 5273:1995). Two types of test pieces were prepared: one in which the 100 mm-long side was cut parallel to the MD direction of the substrate (hereinafter sometimes referred to as "MD test piece"), and one in which the 100 mm-long side was cut parallel to the CD direction of the substrate (hereinafter sometimes referred to as "CD test piece").

[0100] For each of the two test pieces obtained, the stress relaxation rate (%) after 10% elongation for 5 minutes at a temperature of 23° C. and a relative humidity of 50% was measured in accordance with JIS K7161:1994 (ISO 5271:1993).

[0101] Specifically, in a tensile testing machine (Shimadzu Corporation, product name "Autograph AG-IS 500N"), both ends of the test piece in the longitudinal direction were fixed with chucks so that the chuck distance was 100 mm. The chuck distance was then moved away from the test piece to 110 mm at a speed of 200 mm / min (i.e., the test piece was stretched by 10%) and the test piece was stopped in that state for 5 minutes. At this time, the load (tensile stress) F when the chucks were moved away from the test piece and the distance reached 110 mm (when the test piece was stretched by 10%) was measured. A , and the load (tensile stress) F 5 minutes after the extension was stopped B The stress relaxation rate (%) was calculated based on the following formula (1): Stress relaxation rate (%) = (F A -F B ) / F A ×100 …(1)

[0102] In the above measurements, the measurement using the MD test piece gives the stress relaxation rate when the substrate is stretched in the MD direction, and the measurement using the CD test piece gives the stress relaxation rate when the substrate is stretched in the CD direction. The former stress relaxation rate is shown in Table 1 as the stress relaxation rate for "MD," and the latter stress relaxation rate is shown in Table 1 as the stress relaxation rate for "CD." Furthermore, the average of these two stress relaxation rates is shown in Table 1 as the "average value." In this specification, the stress relaxation rate of the substrate refers to this "average value."

[0103] [Test Example 2] (Evaluation of pick-up properties) After peeling off the release sheet from the workpiece processing sheet produced in the examples and comparative examples, the exposed surface of the exposed adhesive layer was attached to one side of an 8-inch silicon wafer using a tape mounter (manufactured by Lintec Corporation, product name "RAD2500m / 12"). Next, a dicing ring frame was attached to the periphery of the exposed surface of the workpiece processing sheet (at a position that does not overlap with the silicon wafer). Furthermore, the workpiece processing sheet was cut to fit the outer diameter of the ring frame.

[0104] Thereafter, the silicon wafer was diced into individual chips having a size of 8 mm×8 mm by dicing under the following dicing conditions using a dicing device (manufactured by Disco Corporation, product name “DFD6362”). Dicing Conditions Wafer thickness: 350μm Dicing equipment: Disco, product name "DFD-6362" Blade: Product name "ZH05-SD2000-Z1-90 CC" Blade rotation speed: 30,000 rpm Cutting speed: 50mm / sec Blade height: 0.060mm Cutting water amount: 1.0L / min Cutting water temperature: 20℃

[0105] After dicing, the substrate side of the workpiece processing sheet was irradiated with ultraviolet light (UV) (illuminance: 230 mW / cm) using an ultraviolet irradiation device (manufactured by Lintec Corporation, product name "RAD-2000m / 12"). 2 ,Light intensity: 190mJ / cm 2 ) to cure the adhesive layer.

[0106] Next, using a pickup device, the tip was pushed up using a needle at room temperature with a push-up speed of 5 mm / sec, a holding time of 0.1 msec, and a predetermined push-up amount. At the same time as the push-up, an attempt was made to separate the tip from the workpiece processing sheet using a collet of 8 mm x 8 mm in size. The push-up of the tip and the separation by the collet were repeated while changing the push-up amount stepwise, and the minimum value of the push-up amount (μm) was obtained when the tip was picked up three times in a row without any abnormality. The minimum value is shown in Table 1 as the minimum push-up amount (μm). Furthermore, the expandability was evaluated based on the obtained minimum push-up amount value against the following criteria. The results are also shown in Table 1. The above test was performed within three days of attaching the silicon wafer to the workpiece processing sheet. ◯: The minimum thrust amount was 250 μm or more. ×: The minimum thrust amount was less than 250 μm.

[0107] Details of the abbreviations and other information in Table 1 are as follows: Random PP: Random polypropylene resin (Prime Polymer Co., Ltd., product name "Prime Polypro E222") Homo PP: Homo polypropylene resin (Prime Polymer Co., Ltd., product name "Prime Polypro E100-GPL") TPO: Olefin-based thermoplastic elastomer (manufactured by Mitsui Chemicals, product name "Tafmer PN2070", polypropylene component: polyethylene component: butane component = 70:15:15) AS agent: Antistatic agent (manufactured by Sanyo Chemical Industries, product name "Pelestat") EMAA: Ethylene-methacrylic acid copolymer (manufactured by Mitsui DuPont Polychemicals, product name "Nucrel N0903HC")

[0108] [Table 1]

[0109] As is clear from Table 1, the workpiece processing sheets produced in the examples had excellent pick-up properties. [Industrial Applicability]

[0110] The workpiece processing sheet of the present invention can be suitably used for processing workpieces such as semiconductor wafers. [Explanation of symbols]

[0111] 1A, 1B, 1C...Workpiece processing sheets 11...Base material 111a, 111b, 111c, 111d, 111e, 111f...resin layer 12...Adhesive layer

Claims

1. A workpiece processing sheet comprising a substrate and an adhesive layer laminated on one side of the substrate, The substrate has a resin layer formed from a resin composition containing a polyolefin resin, The stress relaxation rate of the substrate after 10% stretching for 5 minutes is 35% or more and 46% or less. A workpiece processing sheet characterized by the above.

2. A workpiece processing sheet comprising a substrate and an adhesive layer laminated on one side of the substrate, The stress relaxation rate of the substrate after 10% stretching for 5 minutes is 35% or more and 50% or less, The thickness of the substrate is 25 μm or more and 300 μm or less. A workpiece processing sheet characterized by the above.

3. 2. The workpiece processing sheet according to claim 1, characterized in that the proportion of the polyolefin resin in the resin composition is 30% by mass or more and 100% by mass or less.

4. 4. The workpiece processing sheet according to claim 1, wherein the resin composition contains a thermoplastic elastomer other than the polyolefin resin.

5. 5. The workpiece processing sheet according to claim 4, wherein the thermoplastic elastomer is an olefin-based elastomer.

6. The workpiece processing sheet according to claim 5, characterized in that the proportion of the olefin-based elastomer in the resin composition is 1 mass % or more and 50 mass % or less.

7. The workpiece processing sheet according to any one of claims 1 and 3 to 6, characterized in that the base material is made of a single layer of the resin layer.

8. The workpiece processing sheet according to any one of claims 1 and 3 to 6, characterized in that the base material is made up of a plurality of layers, at least one of which is the resin layer.

9. The workpiece processing sheet according to any one of claims 1 to 8, characterized in that the thickness of the substrate is 25 µm or more and 300 µm or less.

10. The workpiece processing sheet according to any one of claims 1 to 9, characterized in that the adhesive layer is made of an acrylic adhesive.

11. The workpiece processing sheet according to any one of claims 1 to 10, characterized in that it is a dicing sheet.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive sheet for sticking wafer and wafer dicing method

    JP1993211234A

  • Polyolefin film

    JP1995300548A

  • Sheet and adhesive tape for processing semiconductor wafer

    JP2008244377A

  • Back grinding film and method for manufacturing the same

    JP2010225681A

  • Laminate film, and film for semiconductor manufacturing using the same

    JP2012248851A