Carbon nanotube composite wire

The carbon nanotube composite wire with a sintered silver flake layer addresses conductivity and flexibility issues by forming a conductive network that maintains integrity under strain.

JP7562372B2Active Publication Date: 2024-10-07TOKUSEN IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020181997
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-30
Publication Date
2024-10-07
Estimated Expiration
2040-10-30

AI Technical Summary

Technical Problem

Existing composite wires containing carbon nanotubes and metal particles suffer from insufficient conductivity and flexibility, particularly when bent, due to limitations in the conductive effect of metal powders and the inflexibility of sintered silver layers.

Method used

A carbon nanotube composite wire is developed with a sintered layer of silver flakes bonded to the surface of carbon nanotubes or yarns, enhancing conductivity through a network of silver flakes and maintaining flexibility by local bonding without complete melting.

Benefits of technology

The composite wire achieves excellent electrical conductivity and flexibility, suitable for applications like electric cables, with a conductive network that resists damage from bending strains.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562372000005
    Figure 0007562372000005
  • Figure 0007562372000006
    Figure 0007562372000006
  • Figure 0007562372000007
    Figure 0007562372000007
Patent Text Reader

Abstract

To provide a carbon nanotube composite wire 2 with excellent conductivity and flexibility.SOLUTION: A carbon nanotube composite wire 2 has a carbon nanotube 6 and a sintered layer 8 attached to the surface of the carbon nanotube 6. The sintered layer 8 contains many silver flakes 14. These silver flakes 14 are bonded to each other by sintering. The flat surface 16 of the silver flakes 14 partially overlaps or contacts the flat surfaces 16 of other adjacent silver flakes 14. Such adjacency of the silver flakes 14 forms a conductive network.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite wire comprising silver flakes and carbon nanotubes. [Background technology]

[0002] Carbon nanotubes have excellent electrical conductivity, thermal conductivity, and specific strength. Applications of carbon nanotubes are being considered in various fields. Individual carbon nanotubes are very small. Therefore, the use of an assembly of many carbon nanotubes as a structural element is being considered. Examples of such an assembly include webs and yarns.

[0003] Carbon nanotubes can be produced by chemical vapor deposition. This method results in an array of carbon nanotubes, in which a large number of carbon nanotubes are oriented in a certain direction. From this array, carbon nanotubes are gradually pulled out. These carbon nanotubes form a web. The web is in the form of a sheet. The web is twisted to produce yarn.

[0004] The electrical conductivity of yarns, which are an aggregate of carbon nanotubes, is insufficient, and various proposals have been made to improve the electrical conductivity of such yarns.

[0005] JP 2011-38203 A describes a composite wire containing carbon nanotubes and gold, silver or copper particles. In this composite wire, a large number of carbon nanotubes are twisted. Gold, silver or copper particles are dispersed in these carbon nanotubes. These particles can contribute to the electrical conductivity of the composite wire.

[0006] JP 2018-53408 A describes a composite wire containing carbon nanotubes and silver particles. In this composite wire, a layer of many silver particles is attached to the carbon nanotubes. The silver particles are bonded to each other by sintering. The layer of silver particles can contribute to the electrical conductivity of the composite wire. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP2011-38203A [Patent Document 2] JP2018-53408A Summary of the Invention [Problem to be solved by the invention]

[0008] In the composite wire described in JP 2011-38203 A, the conductive effect of the metal powder is limited.

[0009] The electrical conductivity of the composite wire described in JP 2018-53408 A is also insufficient. Moreover, the sintered layer of the silver particles in this composite wire lacks flexibility. When the composite wire is bent during use, the sintered layer is damaged.

[0010] An object of the present invention is to provide a carbon nanotube composite wire having excellent electrical conductivity and flexibility. [Means for solving the problem]

[0011] The carbon nanotube composite wire according to the present invention has a carbon nanotube and a sintered layer attached to the surface of the carbon nanotube. The sintered layer contains a large number of silver flakes. The silver flakes are bonded to each other by sintering.

[0012] According to another aspect, the carbon nanotube composite wire of the present invention has a number of carbon nanotubes and a sintered layer attached to the surface of each carbon nanotube. The sintered layer includes a number of silver flakes. The silver flakes are bonded to each other by sintering.

[0013] According to yet another aspect, the carbon nanotube composite wire of the present invention has a yarn and a sintered layer attached to a surface of the yarn. The yarn has a large number of carbon nanotubes. The sintered layer includes a large number of silver flakes. The silver flakes are bonded to each other by sintering.

[0014] According to yet another aspect, the carbon nanotube composite wire of the present invention includes a yarn and a second sintered layer attached to a surface of the yarn. The yarn includes a number of filaments. Each filament includes a carbon nanotube and a first sintered layer attached to a surface of the carbon nanotube. Each of the first sintered layer and the second sintered layer includes a number of silver flakes. The silver flakes are bonded to each other by sintering.

[0015] The method for producing a carbon nanotube composite wire according to the present invention includes the steps of: obtaining a web or yarn comprising a multiplicity of carbon nanotubes; depositing a silver powder comprising a multiplicity of silver flakes on the carbon nanotubes; and Bonding these silver flakes together by sintering Includes.

[0016] According to another aspect, a method for producing a carbon nanotube composite wire according to the present invention includes the steps of: obtaining a web comprising a multiplicity of carbon nanotubes; attaching a silver powder comprising a multiplicity of silver flakes to the carbon nanotubes; bundling these carbon nanotubes to obtain a yarn; and Bonding these silver flakes together by sintering Includes.

[0017] According to still another aspect, a method for producing a carbon nanotube composite wire according to the present invention includes the steps of: obtaining a web comprising a multiplicity of carbon nanotubes; attaching a silver powder comprising a multiplicity of silver flakes to the carbon nanotubes; bundling these carbon nanotubes to obtain a yarn; depositing a silver powder containing a multiplicity of silver flakes on the yarn; and A step of bonding the silver flakes contained in the yarn together by sintering. Includes.

[0018] According to still another aspect, a method for producing a carbon nanotube composite wire according to the present invention includes the steps of: obtaining a web comprising a multiplicity of carbon nanotubes; bundling these carbon nanotubes to obtain a yarn; depositing a silver powder containing a multiplicity of silver flakes on the yarn; and Bonding these silver flakes together by sintering Includes.

[0019] Preferably, sintering is carried out at a temperature of 500° C. or more for a time of 60 seconds or less.

[0020] Preferably, the silver powder has an average particle diameter D50 of 0.10 μm or more and 0.50 μm or less. Preferably, the silver powder has an average aspect ratio of 20 or more. Effect of the Invention

[0021] In the carbon nanotube composite wire according to the present invention, electrons are conducted through the network of silver flakes. The silver flakes are bonded together by sintering, so the sintered layer is unlikely to be damaged even when the composite wire is bent. This composite wire has excellent electrical conductivity and flexibility. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a front view showing a part of a carbon nanotube composite wire according to one embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic enlarged cross-sectional view showing a part of the carbon nanotube composite wire of FIG. [Diagram 3] FIG. 3 is a schematic enlarged perspective view showing silver flakes contained in the sintered layer of the carbon nanotube composite wire of FIG. [Figure 4] FIG. 4 is a conceptual diagram showing equipment used in the method for producing the carbon nanotube composite wire of FIG. [Diagram 5] FIG. 5 is a perspective view showing an array used in the manufacturing method by the equipment of FIG. [Figure 6] FIG. 6 is a flow diagram showing a method for producing a carbon nanotube composite wire using the equipment of FIG. [Figure 7] FIG. 7 is a front view showing one step of the manufacturing method shown in FIG. [Figure 8] FIG. 8 is a plan view showing the process of FIG. [Figure 9] FIG. 9 is a micrograph showing the carbon nanotube composite wire according to the first embodiment of the present invention. [Figure 10] FIG. 10 is a micrograph showing a sintered layer of the carbon nanotube composite wire of FIG. [Figure 11] FIG. 11 is a micrograph showing the sintered layer of the carbon nanotube composite wire of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, the present invention will be described in detail based on preferred embodiments with reference to the drawings as appropriate.

[0024] 1 shows a carbon nanotube composite wire 2 according to one embodiment of the present invention. This composite wire 2 has a large number of filaments 4. These filaments 4 are bundled together to form the composite wire 2. The filaments 4 may be twisted to form the composite wire 2. A plurality of composite wires 2 may be twisted together.

[0025] Fig. 2 shows a schematic diagram of a portion of a carbon nanotube composite wire 2. Fig. 2 shows a filament 4 exposed on the surface of the composite wire 2. Arrow A in Fig. 2 indicates the length direction of this filament 4. This filament 4 has a carbon nanotube 6 and a sintered layer 8.

[0026] The carbon nanotube 6 is hollow. The carbon nanotube 6 has a carbon layer 10 and a cavity 12. The cross-sectional shape of the carbon nanotube 6 is generally circular. The outer diameter of the carbon nanotube 6 is usually 0.5 nm or more and 100 nm or less. The length of the carbon nanotube 6 is usually 0.5 μm or more and 10 mm or less. The carbon nanotube 6 may have a single-wall structure, a double-wall structure, or a multi-wall structure.

[0027] The sintered layer 8 is attached to the surface of the carbon nanotube 6. In FIG. 2, the sintered layer 8 covers a part of the outer circumferential surface of the carbon nanotube 6. Therefore, the carbon nanotube 6 is partially exposed. The sintered layer 8 may cover the entire outer circumferential surface of the carbon nanotube 6.

[0028] 2, the sintered layer 8 includes a large number of silver flakes 14. Each silver flake 14 extends generally along a length direction A. Therefore, the thickness direction of the silver flake 14 generally coincides with the radial direction of the carbon nanotubes 6.

[0029] FIG. 3 is an enlarged perspective view showing a silver flake 14. This silver flake 14 has a shape of a thin plate. This silver flake 14 has two flat surfaces 16. Each flat surface 16 is substantially parallel to the other flat surface 16. In FIG. 3, an arrow T indicates the thickness of the silver flake 14. The thickness T is the distance between the flat surface 16 and the other flat surface 16. The thickness T is relatively small. In other words, the flat surface 16 is close to the other flat surface 16. In the present invention, a shape in which two flat surfaces 16 close to each other can be confirmed by microscopic observation is called a "flake".

[0030] The main component of the silver flakes 14 is silver. The structure of the silver flakes 14 is silver crystal. This structure may be single crystal or polycrystalline. Preferably, the structure of the silver flakes 14 is single crystal. The silver flakes 14 may have a silver base and an organic compound attached to the surface of the base. The organic compound is chemically bonded to the base. The ratio of silver in the silver flakes 14 is preferably 99.0 mass % or more, and particularly preferably 99.5 mass % or more. The sintered layer 8 may have silver flakes 14 that do not contain organic compounds. The electrical resistance of the silver flakes 14 that are mainly composed of silver is low. Instead of the silver flakes 14, or together with the silver flakes 14, flakes that are mainly composed of copper may be used.

[0031] 2, the flat surface 16 of the silver flake 14 partially overlaps or partially contacts the flat surface 16 of another adjacent silver flake 14. A conductive network is formed by the adjacency of the silver flakes 14. The sintered layer 8 including the silver flakes 14 can contribute to the electrical conductivity of the composite wire 2.

[0032] The sintered layer 8 shown in FIG. 2 is formed by sintering. The silver flakes 14 are bonded to other adjacent silver flakes 14 by sintering. In sintering, the silver flakes 14 are heated. The silver atoms are diffused by heating, and the silver flakes 14 can be bonded to other adjacent silver flakes 14. The silver flakes 14 may be locally melted by heating. A liquid phase is formed by this melting, and the silver flakes 14 can be bonded to other adjacent silver flakes 14 by solidifying this liquid phase. In sintering, there are few silver flakes 14 that are entirely in a liquid phase. In other words, each silver flake 14 generally maintains its flake shape even after sintering. Therefore, in a micrograph of the sintered layer 8, the outline of each silver flake 14 can be generally seen.

[0033] As described above, the bonds between the silver flakes 14 are localized. Moreover, as is clear from FIG. 2, the sintered layer 8 has spaces surrounded by the silver flakes 14. Therefore, this sintered layer 8 is highly deformable. This sintered layer 8 has excellent flexibility. When the composite wire 2 is bent, bending stress, compressive stress, tensile stress, etc. are generated in the sintered layer 8. Even if these stresses are generated, damage such as cracks is unlikely to occur in the sintered layer 8. This sintered layer 8 can deform in accordance with the carbon nanotubes 6. In other words, this composite wire 2 has excellent flexibility. The composite wire 2, which has excellent conductivity and flexibility, is suitable for electric cables.

[0034] Fig. 4 shows an equipment 18 used in the method for producing the carbon nanotube composite wire 2 of Fig. 1. The equipment 18 includes a first spreader 20, a concentrator 22, a second spreader 24, and a heating furnace 26.

[0035] FIG. 5 shows an array 28 used in the manufacturing method using the equipment 18 in FIG. 4, together with a substrate 30. The array 28 has a block shape. This array 28 is an assembly of a large number of carbon nanotubes 6. For ease of explanation, the carbon nanotubes 6 are hatched in FIG. 5. These carbon nanotubes 6 are aligned in the thickness direction (Z direction) of the array 28. In other words, each carbon nanotube 6 is generally standing upright relative to the substrate 30. Various methods can be used to manufacture the array 28. A typical method is chemical vapor deposition. In this method, the carbon nanotubes 6 grow gradually upward from the substrate 30.

[0036] Fig. 6 is a flow diagram showing a method for manufacturing a carbon nanotube composite wire 2 using the equipment 18 of Fig. 4. In this manufacturing method, first, drawing of carbon nanotubes 6 from an array 28 is started (STEP 1).

[0037] This drawing process is shown in Figures 7 and 8. Drawing is performed from the side surface 32 of the array 28. One or a small number of carbon nanotubes 6 are chucked and drawn out. Following the drawn carbon nanotube 6, other carbon nanotubes 6 are successively drawn out from the array 28. At this time, the carbon nanotubes 6 are bonded to each other by van der Waals forces. The carbon nanotubes 6 proceed downstream (to the right in Figure 7).

[0038] By continuing this drawing, a web 34 is formed (STEP 2). As shown in Fig. 7, the thickness (size in the Z direction) of the web 34 is small. As shown in Fig. 8, the width (size in the Y direction) of the web 34 is large. In other words, the web 34 is sheet-like.

[0039] The web 34 is sent to the first spreader 20. The first spreader 20 sprays (or spreads) a dispersion 36 of silver powder onto the web 34 (STEP 3). In the dispersion 36, a large number of silver particles are dispersed in a solvent. These silver particles contain silver flakes 14. The preferred solvent is an organic solvent, water, or an aqueous solution. A volatile organic solvent is preferred. Preferred organic solvents include alcohols such as methanol and ethanol, acetone, and dimethyl sulfoxide. Preferred aqueous solutions include aqueous polyvinyl alcohol solutions. After spraying, the solvent volatilizes. The volatilization may be accelerated by a dryer. The volatilization of the solvent leaves silver particles on the web 34. The silver particles adhere to the surfaces of the carbon nanotubes 6.

[0040] The web 34 is fed to the concentrator 22. The concentrator 22 has a first roller 40a and a second roller 40b. The web 34 is passed between the first roller 40a and the second roller 40b. The top 42 of the first roller 40a is located above the bottom 44 of the second roller 40b. Therefore, in FIG. 7, the web 34 abuts against the vicinity of the top 42 of the first roller 40a and also abuts against the vicinity of the bottom 44 of the second roller 40b. The web 34 in this state is under tension.

[0041] In this concentrator 22, the first roller 40a moves relative to the second roller 40b. The direction of this movement is the axial direction (Y direction) of the first roller 40a. As the first roller 40a moves, the carbon nanotubes 6 rub against the first roller 40a and the second roller 40b. This rubbing causes the carbon nanotubes 6 to intertwine with each other. The first roller 40a and the second roller 40b repeat relative reciprocating movements. This repetition causes the carbon nanotubes 6 to be densely concentrated (STEP 4). A yarn 45 is obtained by the concentration. In this yarn 45, silver particles are dispersed from the surface to the inside. These silver particles include silver flakes 14. The carbon nanotubes 6 may be concentrated by other methods. As another method, drawing by a die is exemplified. The yarn 45 obtained by the concentration may be twisted. A large number of unconcentrated carbon nanotubes 6 may be twisted.

[0042] The yarn 45 is sent to the second spreader 24. The second spreader 24 sprays (or spreads) the dispersion 36 of silver powder onto the web 34 (STEP 5). The components of the dispersion 36 are the same as the components of the dispersion 36 sprayed by the first spreader 20. In other words, the dispersion 36 in which a large number of silver particles are dispersed in a solvent is sprayed by the second spreader 24. After spraying, the solvent volatilizes. The volatilization may be accelerated by a dryer. The silver particles remain on the yarn 45 due to the volatilization of the solvent. The silver particles adhere to the surface of the yarn 45. The dispersion 36 having a different component from the component of the dispersion 36 sprayed by the first spreader 20 may be sprayed by the second spreader 24. The dispersion 36 having a different concentration from the concentration of the dispersion 36 sprayed by the first spreader 20 may be sprayed by the second spreader 24. Instead of spraying, the silver particles may be deposited on the surface of the yarn 45 by immersing the yarn 45 in the dispersion liquid 36 .

[0043] The yarn 45 is fed to the heating furnace 26. In the heating furnace 26, the yarn 45 is heated (STEP 6). By heating, the silver flakes 14 are sintered with adjacent silver flakes 14. By this sintering, a sintered layer 8 is formed, and a carbon nanotube composite wire 2 is obtained. The network of silver flakes 14 in the sintered layer 8 contributes to the electrical conductivity of the carbon nanotube composite wire 2. The inside of the heating furnace 26 may be an inert atmosphere or an air atmosphere. In Figures 7 and 8, the yarn 45 is continuously supplied to the heating furnace 26. The yarn 45 may be heated in a batch manner.

[0044] By heating at a relatively high temperature for a relatively short time, the silver flakes 14 can be bonded together while preventing the silver flakes 14 from completely melting. From this viewpoint, the temperature in the heating furnace 26 is preferably 100°C or higher, more preferably 300°C or higher, and particularly preferably 500°C or higher. From the viewpoint of suppressing the volatilization of the carbon nanotubes 6 due to heating, the temperature in the heating furnace 26 is preferably 800°C or lower. The heating time is preferably 1 second or longer, and preferably 60 seconds or shorter. Because the heating time is short, even if the heating furnace 26 is in an air atmosphere, oxidation of the yarn 45 is unlikely to occur. By using the heating furnace 26 in an air atmosphere, the carbon nanotube composite wire 2 can be obtained at low cost.

[0045] The sintered layer 8 (first sintered layer) derived from the silver flakes 14 introduced by spraying the dispersion liquid 36 by the first spreader 20 (STEP 3) is attached to the surface of each carbon nanotube 6. This first sintered layer mainly contributes to electrical conductivity inside the composite wire 2. The first sintered layer may cover the entire surface of the carbon nanotubes 6, or may cover only a portion of the surface. A first sintered layer that covers only a portion of the surface of the carbon nanotubes 6 is easy to manufacture. In the yarn 45, carbon nanotubes 6 with a sintered layer 8 attached and carbon nanotubes 6 without a sintered layer 8 attached may be mixed.

[0046] The sintered layer 8 (second sintered layer) derived from the silver flakes 14 introduced by spraying the dispersion liquid 36 by the second spreader 24 (STEP 3) covers the surface of the yarn 45. This second sintered layer contributes to electrical conductivity mainly on the surface of the composite wire 2. The second sintered layer may cover the entire surface of the yarn 45 or may cover only a part of it. From the viewpoint of electrical conductivity, it is preferable that the second sintered layer covers the entire surface of the yarn 45.

[0047] The first sintered layer and the second sintered layer are mixed in this composite wire 2. The first sintered layer and the second sintered layer are partially continuous with each other. Therefore, in this composite wire 2, the boundary between the two layers is difficult to clearly see.

[0048] The spraying of the dispersion liquid 36 by the first spreader 20 (STEP 3) may be omitted. In this case, silver particles are supplied only to the yarn 45 after converging (STEP 4). This composite wire 2 does not have a first sintered layer, but has a second sintered layer.

[0049] The spraying of the dispersion liquid 36 by the second spreader 24 (STEP 5) may be omitted. In this case, silver particles are supplied only to the web 34 before focusing (STEP 4). This composite wire 2 has a first sintered layer but does not have a second sintered layer.

[0050] After bundling (STEP 4), the yarn may be heated to sinter the silver flakes 14, and the yarn 45 may be sprayed with dispersion 36 (STEP 5), and may be further sintered by heating (STEP 6).

[0051] The silver powder may contain silver particles other than the silver flakes 14. Examples of silver particles other than the silver flakes 14 include chunky particles, spherical particles, polyhedral particles, and spiral particles.

[0052] From the viewpoint of electrical conductivity, the mass ratio of carbon nanotubes 6 to silver particles in composite wire 2 is preferably 50 / 50 or less, more preferably 30 / 70 or less, and particularly preferably 20 / 80 or less. This ratio is preferably 5 / 95 or more.

[0053] From the viewpoint of electrical conductivity, the ratio of the silver flakes 14 in the silver powder is preferably 30% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The ideal ratio is 100% by mass.

[0054] The average particle diameter D50 of the silver powder is preferably 0.50 μm or less. Silver powder having an average particle diameter D50 of 0.50 μm or less can contribute to the electrical conductivity and flexibility of the carbon nanotube composite wire 2. From this viewpoint, the average particle diameter D50 is more preferably 0.45 μm or less, and particularly preferably 0.40 μm or less. From the viewpoint of the handleability of the silver powder, the average particle diameter D50 is preferably 0.10 μm or more.

[0055] The cumulative 95 volume % particle size D95 of the silver powder is preferably 1.00 μm or less. Silver powder having a particle size D95 of 1.00 μm or less can contribute to the conductivity and flexibility of the carbon nanotube composite wire 2. From this viewpoint, the particle size D95 is more preferably 0.90 μm or less, and particularly preferably 0.80 μm or less.

[0056] The maximum particle diameter Dmax of the silver powder is preferably 3.00 μm or less. Silver powder having a maximum particle diameter Dmax of 3.00 μm or less can contribute to the electrical conductivity and flexibility of the carbon nanotube composite wire 2. From this viewpoint, the maximum particle diameter Dmax is more preferably 2.50 μm or less, and particularly preferably 2.00 μm or less.

[0057] The average particle diameter D50, cumulative 95% by volume particle diameter D95, and maximum particle diameter Dmax are measured using a laser diffraction particle size distribution analyzer. An example of the measuring device is the "LA-950V2" manufactured by Horiba, Ltd.

[0058] The average thickness Tave of the silver powder is preferably 1 nm or more and 100 nm or less. Silver powder with an average thickness Tave of 1 nm or more can be easily manufactured. From this viewpoint, the average thickness Tave is more preferably 10 nm or more, and particularly preferably 20 nm or more. Silver powder with an average thickness Tave of 100 nm or less can contribute to the conductivity and flexibility of the carbon nanotube composite wire 2. From this viewpoint, the average thickness Tave is more preferably 80 nm or less, and particularly preferably 50 nm or less. The average thickness Tave is calculated by averaging the thicknesses T (see FIG. 3) of 100 randomly selected silver particles. Each thickness T is measured visually based on an SEM photograph.

[0059] The aspect ratio (D50 / Tave) of the silver powder is preferably 20 or more. Silver powder with an aspect ratio (D50 / Tave) of 20 or more can contribute to the conductivity and flexibility of the carbon nanotube composite wire 2. From this viewpoint, the aspect ratio (D50 / Tave) is preferably 30 or more, and particularly preferably 35 or more. From the viewpoint of ease of manufacture, the aspect ratio (D50 / Tave) is preferably 1000 or less.

[0060] The silver flakes 14, which have a smooth surface, contribute to the electrical conductivity of the composite wire 2. The arithmetic mean roughness Ra of the silver flakes 14 is preferably 10.0 nm or less, more preferably 7.0 nm or less, and particularly preferably 5.0 nm or less. The arithmetic mean roughness Ra is measured by an atomic force microscope (AFM). The arithmetic mean roughness Ra is measured on the flat surface 16. EXAMPLES

[0061] The effects of the present invention will be clarified by the following examples, but the present invention should not be construed as being limited based on the description of these examples.

[0062] [Experiment 1] [Example 1] A carbon nanotube composite wire was obtained by the procedure shown in FIG. 6 using the equipment shown in FIG. 7 and FIG. 8. A dispersion containing silver powder with an average particle diameter D50 of 0.23 μm was sprayed by the first and second spreaders. The silver powder contained silver flakes. In this composite wire, the mass ratio of carbon nanotubes to silver particles was 10 / 90. The diameter of this composite wire was about 20 μm. FIG. 9 shows a micrograph of this composite wire. FIG. 10 shows a further enlarged micrograph of this composite wire viewed from the radial direction. FIG. 11 shows a further enlarged micrograph of the cross section of the sintered layer.

[0063] [Example 2-4] A carbon nanotube composite wire was obtained in the same manner as in Example 1, except that silver powder having an average particle diameter D50 shown in Table 1 below was used.

[0064] [Comparative Example 1] A composite wire was obtained in the same manner as in Example 1, except that the silver powder was completely melted by performing heating for a long period of time in the heating step. In this composite wire, the silver flakes no longer retained their original shape.

[0065] [Comparative Example 2] Except for not performing heating in a heating furnace, a composite wire was obtained in the same manner as in Example 1. In this composite wire, the silver flakes were not sintered together.

[0066] [Comparative Example 3] A carbon nanotube composite wire was obtained in the same manner as in Example 1, except that spherical silver particles were used.

[0067] [Comparative Example 4] A carbon nanotube yarn was obtained in the same manner as in Example 1, except that the silver powder dispersion was not sprayed.

[0068] [Conductive] The electrical resistivity of the composite wires (or yarns) was measured and the results, along with the ratings, are shown in Tables 1 and 2 below.

[0069] [Crack resistance] The composite wire (or yarn) was wound around a cylinder and then restored, and the surface of the composite wire was observed and rated according to the following criteria. The results are shown in Tables 1 and 2 below. A: There are no cracks in the filament. B: A few filaments have microcracks. C: Many filaments have microcracks. D: Large cracks in the filament.

[0070] [Table 1]

[0071] [Table 2]

[0072] As shown in Tables 1 and 2, the carbon nanotube composite wires of the respective Examples are excellent in electrical conductivity and crack resistance. From these evaluation results, the superiority of the present invention is clear.

[0073] [Experiment 2] [Example 5] A carbon nanotube composite wire was obtained using the equipment shown in Figures 7 and 8. A dispersion containing silver powder with an average particle diameter D50 of 0.23 μm was sprayed by the first spreader. This silver powder contains silver flakes. The dispersion was not sprayed by the second spreader. In this composite wire, the mass ratio of carbon nanotubes to silver particles was 50 / 50. The diameter of this composite wire was about 100 μm.

[0074] [Examples 6-8] A carbon nanotube composite wire was obtained in the same manner as in Example 5, except that silver powder having an average particle diameter D50 shown in Table 3 below was used.

[0075] [Comparative Example 5] A composite wire was obtained in the same manner as in Example 5, except that the silver powder was completely melted by performing heating for a long period of time in the heating step. In this composite wire, the silver flakes no longer retained their original shape.

[0076] [Comparative Example 6] Except for not performing heating in a heating furnace, a composite wire was obtained in the same manner as in Example 5. In this composite wire, the silver flakes were not sintered together.

[0077] [Comparative Example 7] A carbon nanotube composite wire was obtained in the same manner as in Example 5, except that spherical silver particles were used.

[0078] [Conductive] The electrical resistivity of the composite wires (or yarns) was measured and the results, along with the ratings, are shown in Tables 3 and 4 below.

[0079] [Crack resistance] After the composite wire (or yarn) was wound around the cylinder and restored, the surface of the composite wire was observed and rated according to the following criteria. The results are shown in Tables 3 and 4 below. A: There are no cracks in the filament. B: A few filaments have microcracks. C: Many filaments have microcracks. D: Large cracks in the filament.

[0080] [Table 3]

[0081] [Table 4]

[0082] As shown in Tables 3 and 4, the carbon nanotube composite wires of the respective Examples are excellent in electrical conductivity and crack resistance. From these evaluation results, the superiority of the present invention is clear. [Industrial Applicability]

[0083] The carbon nanotube composite wire according to the present invention can be used in various applications where electrical conductivity is required. [Explanation of symbols]

[0084] 2. Carbon nanotube composite wire 4. Filament 6. Carbon nanotubes 8. Sintered layer 12 Carbon layer 14. Silver flakes 16. Flat surface 20...First spreader 22...Focusing machine 24...Second spreader 26...Heating furnace 28. Array 34. Web 36...Dispersion liquid 40a···First roller 40b Second roller 45... yarn

Claims

1. The present invention relates to a method for manufacturing a carbon nanotube using a sintered layer. The sintered layer contains a large number of silver flakes, These silver flakes are bonded together by sintering to create a carbon nanotube composite wire.

2. The present invention relates to a method for manufacturing a carbon nanotube having a sintered layer, the method comprising: The sintered layer contains a large number of silver flakes, These silver flakes are bonded together by sintering to create a carbon nanotube composite wire.

3. The present invention relates to a method for manufacturing a sintered yarn, the method comprising: the yarn comprises a large number of carbon nanotubes; The sintered layer contains a large number of silver flakes, These silver flakes are bonded together by sintering to create a carbon nanotube composite wire.

4. a yarn and a second sintered layer attached to a surface of the yarn; the yarn having a multiplicity of filaments; Each filament has a carbon nanotube and a first sintered layer attached to a surface of the carbon nanotube; each of the first sintered layer and the second sintered layer includes a number of silver flakes; These silver flakes are bonded together by sintering to create a carbon nanotube composite wire.

5. obtaining a web or yarn comprising a multiplicity of carbon nanotubes; attaching a silver powder comprising a number of silver flakes to the carbon nanotubes; and bonding the silver flakes together by sintering A method for producing a carbon nanotube composite wire, comprising:

6. obtaining a web comprising a multiplicity of carbon nanotubes; attaching a silver powder comprising a number of silver flakes to the carbon nanotubes; bundling the carbon nanotubes to obtain a yarn; and bonding the silver flakes together by sintering The method of claim 5, comprising:

7. obtaining a web comprising a multiplicity of carbon nanotubes; attaching a silver powder comprising a number of silver flakes to the carbon nanotubes; bundling the carbon nanotubes to obtain a yarn; depositing a silver powder comprising a multiplicity of silver flakes on said yarn; and bonding the silver flakes contained in the yarn together by sintering. The method of claim 6, comprising:

8. obtaining a web comprising a multiplicity of carbon nanotubes; bundling the carbon nanotubes to obtain a yarn; depositing a silver powder comprising a multiplicity of silver flakes on said yarn; and The method of claim 5 including the step of bonding the silver flakes together by sintering.

9. The method according to any one of claims 5 to 8, wherein the sintering is carried out at a temperature of 500°C or higher for a time of 60 seconds or less.

10. The method according to any one of claims 5 to 9, wherein the silver powder has an average particle diameter D50 of 0.10 µm or more and 0.50 µm or less.

11. The method according to any one of claims 5 to 10, wherein the silver powder has an average aspect ratio of 20 or more.

Citation Information

Patent Citations

  • Method for preparing high heat and electricity conductive adhesive from nanosilver modified carbon nanotubes

    CN109777335A

  • JP1974035116A

  • Carbon nanotube fiber composite and method for producing carbon nanotube fiber composite

    JP2011038203A

  • Conductive paste and conductive film

    JP2017069175A

  • Metal composite carbon nano-tube twist yarn and method for producing the same

    JP2018053408A