Magnetic coated carbon fiber material and preparation method thereof, and heat-conducting wave-absorbing gasket and preparation method thereof

By forming a magnetic cladding layer on the carbon fiber, combining hexagonal boron nitride and carbonyl iron powder in the base material, the problem of insufficient electromagnetic wave absorption performance of carbon fiber materials is solved, and high thermal conductivity and high frequency absorption performance are improved. Suitable for high-performance electronic devices.

CN118996837APending Publication Date: 2024-11-22SHENZHEN HFC SHIELDING PRODS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411085750.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In applications, carbon fiber materials have poor electromagnetic wave absorption performance and cannot effectively absorb high heat and high frequency radiation generated by high-frequency RF modules, which limits the improvement of their thermal conductivity.

Method used

By soaking carbon fibers in a strong acid solution and undergoing plasma treatment, a large number of polar groups are formed, and then reacting with trivalent iron ions to form iron tetraoxide, forming a magnetic coating layer, combining hexagonal boron nitride in the base material and Carbonyl iron powder, a magnetically coated carbon fiber material with high thermal conductivity and high frequency wave absorption properties were prepared.

Benefits of technology

It significantly improves the high-frequency wave absorption and thermal conductivity of carbon fiber materials, and meets the needs of high-performance carbon fiber in aerospace, electronic equipment and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996837A_ABST
    Figure CN118996837A_ABST
Patent Text Reader

Abstract

The invention provides a magnetic coated carbon fiber material and a preparation method thereof, and a heat-conducting wave-absorbing gasket and a preparation method thereof, and belongs to the technical field of carbon fiber material manufacturing. The preparation method of the magnetic coated carbon fiber material comprises the following steps: soaking carbon fibers in a strong acid solution to etch the surfaces of the carbon fibers to obtain pretreated carbon fibers; transferring the pretreated carbon fibers into plasma equipment and carrying out plasma treatment to obtain modified carbon fibers; the modified carbon fibers and a magnetic solution containing ferric ions are mixed and react to obtain the magnetic coated carbon fiber material, and the magnetic coated carbon fiber material has high thermal conductivity and high-frequency wave-absorbing performance and can meet the current requirements for high-performance carbon fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of carbon fiber material manufacturing, and in particular to a magnetic coated carbon fiber material and a preparation method thereof, a thermal conductive wave absorbing gasket and a preparation method thereof. Background Art

[0002] Carbon fiber has anisotropic thermal conductivity, and its thermal conductivity in the fiber direction is as high as 1200W / m·K. Making carbon fiber into anisotropic thermal conductive gaskets can not only increase the thermal conductivity by dozens of times, but also make the product more flexible. It is widely used in aerospace, military, automotive electronics, smart phones, chips and other fields.

[0003] However, the resistivity of carbon fiber itself is low, and electromagnetic waves incident on the surface of carbon fiber will be reflected, resulting in poor wave absorption performance of carbon fiber, which to a certain extent limits the application and promotion of carbon fiber. At the same time, with the rapid development of science and technology, the high heat and high-frequency radiation problems generated by high-frequency RF modules inside electronic equipment are becoming increasingly prominent, which also puts higher requirements on the thermal conductivity and wave absorption performance of carbon fiber. Therefore, in order to solve the problems faced by carbon fiber in the current application process, it is urgent to develop a carbon fiber material with high thermal conductivity and high-frequency wave absorption performance. Summary of the invention

[0004] The purpose of the present application is to provide a magnetic coated carbon fiber material and a preparation method thereof, a thermal conductive wave absorbing gasket and a preparation method thereof. The magnetic coated carbon fiber material has both high thermal conductivity and high-frequency wave absorbing performance, and can meet the current demand for high-performance carbon fiber.

[0005] The embodiment of the present application is implemented as follows:

[0006] In a first aspect, an embodiment of the present application provides a method for preparing a magnetic coated carbon fiber material, comprising the following steps:

[0007] The carbon fiber is immersed in a strong acid solution to etch the surface of the carbon fiber to obtain a pretreated carbon fiber; the pretreated carbon fiber is transferred to a plasma device and subjected to plasma treatment to obtain a modified carbon fiber; the modified carbon fiber and a magnetic solution containing trivalent iron ions are mixed and reacted to obtain a magnetic coated carbon fiber material.

[0008] In the above technical scheme, the carbon fiber is first soaked in a strong acid solution to form a large number of etching sites on the surface of the carbon fiber for polar group loading, and then the pretreated carbon fiber is plasma treated, so that a large number of polar groups such as carbonyl, carboxyl and hydroxyl can be formed at the etching sites on the surface of the carbon fiber. These large numbers of polar groups can react with trivalent iron ions and generate ferroferric oxide in situ. Since ferroferric oxide has unique magnetic and dielectric properties, it has excellent wave absorption performance, and thus the carbon fiber material also has relatively excellent wave absorption performance. In addition, the carbon fiber itself has relatively excellent thermal conductivity, so that the magnetic coated carbon fiber material finally prepared has both high thermal conductivity and high-frequency wave absorption performance. In this application, through the synergistic effect of strong acid solution soaking and plasma treatment, more polar groups are formed on the surface of the carbon fiber, which is beneficial to the subsequent magnetic coating to obtain a carbon fiber material with better wave absorption performance.

[0009] In some optional embodiments, the acid in the strong acid solution is selected from at least one of nitric acid, sulfuric acid and hydrochloric acid.

[0010] Alternatively, H + The molar concentration is 12-20 mol / L.

[0011] Optionally, the carbon fiber is immersed in the strong acid solution for 3 to 8 minutes.

[0012] In the above technical solution, there are many applicable types of acids in the strong acid solution, which can provide more feasible implementation plans, thereby facilitating the promotion and application of the technical solution provided in the embodiment of the present application.

[0013] Furthermore, the H + The molar concentration and immersion time are limited within specific ranges, respectively, which can exert a more suitable etching effect, thereby reducing the damage to the carbon fiber structure itself while meeting the subsequent polar group loading requirements.

[0014] In some optional embodiments, in the plasma treatment step, the discharge power is 1000-5000 W, and the treatment time is 20-40 min.

[0015] In the above technical scheme, the discharge power and time of the plasma treatment are limited within specific ranges respectively, which can make the synergistic effect between the plasma treatment and the strong acid solution immersion better, so that a larger number of polar groups can be loaded on the surface of the carbon fiber, so that a sufficient amount of ferrosoferric oxide can be formed after the subsequent reaction with trivalent iron ions, so as to coat the carbon fiber material more evenly and completely, so that the finally prepared magnetic coated carbon fiber material has better high-frequency wave absorption performance.

[0016] In some optional embodiments, the diameter of the carbon fiber is 10-20 μm, and the length of the carbon fiber is 100-300 μm; and / or, the Fe 3+ The molar concentration is 8-12 mol / L.

[0017] In the above technical solution, the diameter and length of the carbon fiber are respectively limited to a specific range, which is conducive to the subsequent orientation of the carbon fiber; in addition, the Fe 3+ The molar concentration of Fe is limited to a specific range, which can provide a relatively appropriate amount of Fe 3+ , thereby more thoroughly coating the carbon fiber surface, so that the magnetic coated carbon fiber material finally prepared has better high-frequency wave absorbing performance.

[0018] In a second aspect, an embodiment of the present application provides a magnetic coated carbon fiber material, which is prepared using the preparation method of the magnetic coated carbon fiber material provided in the embodiment of the first aspect.

[0019] In the above technical scheme, the magnetic coated carbon fiber material is prepared by the preparation method of the magnetic coated carbon fiber material provided by the first aspect embodiment. Since the carbon fiber surface has a relatively complete and evenly distributed ferroferric oxide coating layer, and the carbon fiber itself has relatively excellent thermal conductivity, the magnetic coated carbon fiber material itself has both high thermal conductivity and high-frequency wave absorption performance.

[0020] In a third aspect, an embodiment of the present application provides a method for preparing a thermally conductive wave-absorbing gasket, comprising the following steps:

[0021] 1 to 300 parts of the magnetic coated carbon fiber material as provided in the second aspect embodiment and a base material are mixed in parts by mass to obtain a mixture; wherein the base material comprises 1 to 100 parts of a thermally conductive filler, 1 to 30 parts of AB glue, 1 to 10 parts of a coupling agent and 0.1 to 1 part of a reaction inhibitor; the mixture is sequentially subjected to extrusion orientation treatment, stacked extrusion treatment and heat curing treatment to obtain a thermally conductive wave-absorbing gasket.

[0022] In the above technical scheme, the magnetic coated carbon fiber material and the base material provided in the second aspect embodiment are mixed in a specific mass ratio and prepared into a gasket. Since the magnetic coated carbon fiber material has both high thermal conductivity and high-frequency wave absorption performance, the finally prepared gasket product also has both high thermal conductivity and high-frequency wave absorption performance.

[0023] In some optional embodiments, the base material further includes 1 to 100 parts of hexagonal boron nitride.

[0024] Optionally, the base material further includes 1 to 100 parts of carbonyl iron powder.

[0025] In the above technical solution, the base material also includes a specific mass fraction of hexagonal boron nitride. On the one hand, hexagonal boron nitride has a low dielectric constant and good wave transmittance, which can reduce the amount of electromagnetic wave reflection on the carbon fiber surface; on the other hand, hexagonal boron nitride can also increase the wave absorption frequency band of carbon fiber, thereby absorbing high-frequency battery waves. Through the combined effect of these two aspects, the gasket finally prepared has relatively excellent high-frequency wave absorption performance.

[0026] Furthermore, carbonyl iron powder itself is a magnetic material with good wave absorption performance. Adding a specific mass fraction of carbonyl iron powder to the base material can also help improve the high-frequency wave absorption performance of the gasket finally prepared.

[0027] In some optional embodiments, the thermally conductive filler and / or the carbonyl iron powder is spherical.

[0028] In the above technical solution, the thermally conductive filler and the carbonyl iron powder are both spherical. This is because the surface of the spherical particles is relatively smooth, and the carbon fiber material is easier to turn when in contact with the spherical particles, thereby facilitating the orientation of the carbon fiber in the orientation treatment step, so as to obtain a gasket with better thermal conductivity. In addition, the thermally conductive filler and the carbonyl iron powder are both spherical, which has the advantage of being easy to fill and mix.

[0029] In some optional embodiments, the particle size of the thermal conductive filler is 1 to 10 μm, and the particle size of the carbonyl iron powder is 1 to 5 μm.

[0030] In the above technical solution, the use of thermal conductive fillers and carbonyl iron powder with specific particle sizes can form a suitable particle size gradation relationship with the magnetic coated carbon fiber material, so that each component in the mixture has a better mixing uniformity.

[0031] In a fourth aspect, an embodiment of the present application provides a heat-conductive and wave-absorbing gasket, which is prepared by the preparation method of the heat-conductive and wave-absorbing gasket provided in the embodiment of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 A process flow chart of a method for preparing a magnetic coated carbon fiber material provided in an embodiment of the present application. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0035] It should be noted that “and / or” in this application, such as “Feature 1 and / or Feature 2”, refers to the three situations of “Feature 1” alone, “Feature 2” alone, or “Feature 1” plus “Feature 2”.

[0036] In addition, in the description of the present application, unless otherwise specified, the meaning of "multiple" in "one or more" refers to two or more; the range of "value a ~ value b" includes the two end values ​​"a" and "b", and the "unit" in "value a ~ value b + unit of measurement" represents the "unit of measurement" of both "value a" and "value b".

[0037] The following is a detailed description of a magnetic coated carbon fiber material and a preparation method thereof, a thermal conductive wave absorbing gasket and a preparation method thereof according to an embodiment of the present application.

[0038] In a first aspect, an embodiment of the present application provides a method for preparing a magnetic coated carbon fiber material, comprising the following steps:

[0039] The carbon fiber is immersed in a strong acid solution to etch the surface of the carbon fiber to obtain a pretreated carbon fiber; the pretreated carbon fiber is transferred to a plasma device and subjected to plasma treatment to obtain a modified carbon fiber; the modified carbon fiber and a magnetic solution containing trivalent iron ions are mixed and reacted to obtain a magnetic coated carbon fiber material.

[0040] In the present application, a strong acid solution is first used to soak the carbon fiber so as to form a large number of etching sites on the surface of the carbon fiber for polar group loading, and then the pretreated carbon fiber is subjected to plasma treatment, so that a large number of polar groups such as carbonyl, carboxyl and hydroxyl groups can be formed at the etching sites on the surface of the carbon fiber. These large numbers of polar groups can react with trivalent iron ions and generate ferroferric oxide in situ. Since ferroferric oxide has unique magnetic and dielectric properties, it has excellent wave absorption performance, and thus the carbon fiber material also has relatively excellent wave absorption performance. In addition, the carbon fiber itself has relatively excellent thermal conductivity, so that the magnetic coated carbon fiber material finally prepared has both high thermal conductivity and high-frequency wave absorption performance. In the present application, through the synergistic effect of strong acid solution soaking and plasma treatment, more polar groups are formed on the surface of the carbon fiber, which is conducive to subsequent magnetic coating to obtain a carbon fiber material with better wave absorption performance.

[0041] As an example, the acid in the strong acid solution is selected from at least one of nitric acid, sulfuric acid and hydrochloric acid.

[0042] In this embodiment, there are many applicable types of acids in the strong acid solution, which can provide more feasible implementation plans, thereby facilitating the promotion and application of the technical solutions provided in the embodiments of the present application.

[0043] As an example, H in a strong acid solution + The molar concentration is 12 to 20 mol / L, for example but not limited to a molar concentration of 12 mol / L, 13 mol / L, 14 mol / L, 15 mol / L, 16 mol / L, 17 mol / L, 18 mol / L, 19 mol / L and 20 mol / L, or a range between any two of the points.

[0044] As an example, the immersion time of the carbon fiber in the strong acid solution is 3 to 8 minutes, for example but not limited to the immersion time being any one of 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes and 8 minutes or a range between any two of them.

[0045] In this embodiment, H in the strong acid solution + The molar concentration and immersion time are respectively limited within specific ranges, which can exert a more suitable etching effect, thereby reducing the damage to the carbon fiber structure itself while meeting the subsequent polar group loading requirements (excessive etching can easily affect the inherent properties of carbon fiber, such as strength, toughness and thermal conductivity; insufficient etching can make it difficult to load sufficient polar groups after plasma treatment, which will accordingly affect the subsequent coating effect of magnetic substances on carbon fiber, making it difficult to effectively improve the high-frequency wave absorption performance of carbon fiber).

[0046] As an example, in the plasma treatment step, the discharge power is 1000-5000 W, for example but not limited to the discharge power is any point value of 1000 W, 2000 W, 3000 W, 4000 W and 5000 W, or a range value between any two of them; the treatment time is 20-40 min, for example but not limited to the treatment time is any point value of 20 min, 25 min, 30 min, 35 min and 40 min, or a range value between any two of them.

[0047] In this embodiment, the discharge power and time of the plasma treatment are limited within specific ranges, respectively, so that the synergistic effect between the plasma treatment and the strong acid solution immersion can be better, so that a larger number of polar groups can be loaded on the surface of the carbon fiber, so that a sufficient amount of ferrosoferric oxide can be formed after the subsequent reaction with trivalent iron ions, so as to more evenly and completely coat the carbon fiber material, so that the finally prepared magnetic coated carbon fiber material has more excellent high-frequency wave absorbing performance.

[0048] As an example, in the step of plasma treatment, the atmosphere of the plasma treatment includes nitrogen and oxygen, wherein the volume proportion of oxygen is ≥50%.

[0049] As an example, in the atmosphere of plasma treatment, the volume percentage of oxygen is 50-80%, for example but not limited to any one of 50%, 60%, 70% and 80% or a range between any two of the volume percentages.

[0050] In this embodiment, in the step of plasma treatment, the atmosphere conditions are limited to specific conditions, which is helpful to generate a sufficient amount of polar groups and stably load them on the etching sites on the surface of the carbon fiber.

[0051] As an example, the diameter of the carbon fiber is 10 to 20 μm, for example but not limited to any point value of 10 μm, 12 μm, 14 μm, 16 μm, 18 μm and 20 μm, or a range value between any two of them; the length of the carbon fiber is 100 to 300 μm, for example but not limited to any point value of 100 μm, 150 μm, 200 μm, 250 μm and 300 μm, or a range value between any two of them.

[0052] In this embodiment, the diameter and length of the carbon fiber are respectively limited within specific ranges, which is beneficial to the subsequent orientation of the carbon fiber.

[0053] It should be noted that the Fe 3+ The setting of the molar concentration is particularly important, which directly determines the coating of the carbon fiber surface by the formed ferroferric oxide, such as whether it is completely coated, the thickness of the coating layer, and the uniformity of the coating layer. These parameters will affect the high-frequency wave absorbing performance of the coated material.

[0054] As an example, Fe in a magnetic solution 3+ The molar concentration is 8 to 12 mol / L, for example but not limited to any one of 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L and 12 mol / L or a range between any two of them.

[0055] In this embodiment, the Fe3+ The molar concentration of Fe is limited to a specific range, which can provide a relatively appropriate amount of Fe 3+ , thereby more thoroughly coating the carbon fiber surface, so that the magnetic coated carbon fiber material finally prepared has better high-frequency wave absorbing performance.

[0056] It should be emphasized that compared with the Fe 3+ The molar concentration of Fe 3+ The molar concentration of Fe is usually 0.1 to 0.5 mol / L. In the embodiment of the present application, the Fe 3+ The molar concentration increases significantly.

[0057] As an example, in the step of mixing and reacting the modified carbon fiber and the magnetic solution, the reaction temperature is 95-120°C, for example but not limited to the reaction temperature being any one of 95°C, 100°C, 105°C, 110°C, 115°C and 120°C or a range between any two of them; the reaction time is 20-40min, for example but not limited to the reaction time being any one of 20min, 25min, 30min, 35min and 40min or a range between any two of them.

[0058] In this embodiment, the treatment temperature and duration in the mixing reaction step are limited to specific ranges, respectively, so that a magnetite coating layer with better coating effect and higher stability can be obtained.

[0059] As an example, before the step of soaking the carbon fiber in the strong acid solution, a treatment step of soaking the carbon fiber in an alkaline solution is also included.

[0060] In this embodiment, soaking the carbon fiber in an alkaline solution can remove various impurities on the surface of the carbon fiber, such as remaining sizing agent, so as to facilitate subsequent etching treatment and improve the cleanliness of the carbon fiber.

[0061] As an example, the alkaline solution is a sodium hydroxide solution. - The molar concentration is 9 to 12 mol / L, for example but not limited to any one of 9 mol / L, 10 mol / L, 11 mol / L and 12 mol / L or a range between any two of them.

[0062] It should be noted that any process or step not specifically described in the preparation process of the magnetic coated carbon fiber material may be arranged according to conventional selections in the art.

[0063] As an example, the process flow chart of the preparation method of the magnetic coated carbon fiber material is exemplarily referred to Figure 1 .

[0064] In a second aspect, an embodiment of the present application provides a magnetic coated carbon fiber material, which is prepared using the preparation method of the magnetic coated carbon fiber material provided in the embodiment of the first aspect.

[0065] In this embodiment, the magnetic coated carbon fiber material is prepared by the preparation method of the magnetic coated carbon fiber material provided by the first aspect embodiment. Since the carbon fiber surface has a relatively complete and evenly distributed ferroferric oxide coating layer, and the carbon fiber itself has relatively excellent thermal conductivity, the magnetic coated carbon fiber material itself has both high thermal conductivity and high-frequency wave absorption performance.

[0066] In a third aspect, an embodiment of the present application provides a method for preparing a thermally conductive wave-absorbing gasket, comprising the following steps:

[0067] 1 to 300 parts of the magnetic coated carbon fiber material as provided in the second aspect embodiment and a base material are mixed in parts by mass to obtain a mixture; wherein the base material comprises 1 to 100 parts of a thermally conductive filler, 1 to 30 parts of AB glue, 1 to 10 parts of a coupling agent and 0.1 to 1 part of a reaction inhibitor; the mixture is sequentially subjected to extrusion orientation treatment, stacked extrusion treatment and heat curing treatment to obtain a thermally conductive wave-absorbing gasket.

[0068] In this embodiment, the magnetic coated carbon fiber material and the base material provided in the second aspect embodiment are mixed in a specific mass ratio and prepared into a gasket. Since the magnetic coated carbon fiber material has both high thermal conductivity and high-frequency wave absorption performance, the finally prepared gasket product also has both high thermal conductivity and high-frequency wave absorption performance.

[0069] It should be noted that the extrusion orientation treatment (i.e. mechanical orientation) is adopted because the mixture is relatively viscous. This is to make the gasket finally prepared have better thermal conductivity. Therefore, mechanical orientation is adopted, and the fixed size space of the extruder is used to apply shear force to the mixture, so that the carbon fibers in the mixture are oriented to form a heat conduction channel.

[0070] It should be noted that the type of thermal conductive filler is not limited and can be set according to conventional selection in the art, for example, it can be at least one of aluminum nitride, aluminum oxide, silicon nitride, zinc oxide and magnesium oxide.

[0071] It should be noted that the type of coupling agent is not limited and can be selected according to conventional methods in the art, for example, it can be a silane coupling agent.

[0072] It should be noted that the type of reaction inhibitor is not limited and can be selected according to the conventional method in the art, for example, it can be ethynyl cyclohexanol.

[0073] As an example, the viscosity of AB glue is 800-1200 Pa / s, for example but not limited to any one of 800 Pa / s, 900 Pa / s, 1000 Pa / s, 1100 Pa / s and 1200 Pa / s or a range between any two of them.

[0074] In this embodiment, the AB glue in the specific viscosity range helps to mix the various components and also provides suitable adhesion.

[0075] It should be noted that the heating and curing step is mainly to vulcanize the AB glue to obtain a heat-conducting and wave-absorbing gasket.

[0076] As an example, in the step of heating and curing, the treatment temperature is 80-100° C. and the treatment time is 10-15 hours.

[0077] In this embodiment, the temperature and duration of the curing process are limited to specific ranges, respectively, so that a better curing effect can be achieved.

[0078] As an example, the base material further includes 1 to 100 parts of hexagonal boron nitride.

[0079] In this embodiment, the base material also includes a specific mass fraction of hexagonal boron nitride. On the one hand, hexagonal boron nitride has a low dielectric constant and good wave transmittance, which can reduce the amount of electromagnetic waves reflected on the surface of carbon fiber; on the other hand, hexagonal boron nitride can also increase the wave absorption band of carbon fiber, thereby absorbing high-frequency battery waves. Through the combined effect of these two aspects, the gasket finally prepared has relatively excellent high-frequency wave absorption performance.

[0080] As an example, the base material further includes 1 to 100 parts of carbonyl iron powder.

[0081] In this embodiment, the carbonyl iron powder itself is a magnetic material with good wave absorption performance. Adding a specific mass fraction of carbonyl iron powder to the base material can also help improve the high-frequency wave absorption performance of the gasket finally prepared.

[0082] As an example, the thermal conductive filler and / or the carbonyl iron powder is spherical.

[0083] In this embodiment, the thermal conductive filler and the carbonyl iron powder are both spherical. This is because the surface of the spherical particles is relatively smooth, and the carbon fiber material is easier to turn when in contact with the spherical particles, thereby facilitating the orientation of the carbon fiber in the orientation treatment step, so as to obtain a gasket with better thermal conductivity.

[0084] As an example, the particle size of the thermally conductive filler is 1 to 10 μm, such as but not limited to any point value of 1 μm, 2 μm, 4 μm, 6 μm, 8 μm and 10 μm, or a range value between any two of them; the particle size of the carbonyl iron powder is 1 to 5 μm, such as but not limited to any point value of 1 μm, 2 μm, 3 μm, 4 μm and 5 μm, or a range value between any two of them.

[0085] In this embodiment, the thermal conductive filler and carbonyl iron powder with specific particle sizes are used to form a suitable particle size gradation relationship with the magnetic coated carbon fiber material, so that each component in the mixture has a better mixing uniformity.

[0086] As an example, after the heating and curing step is completed, a step of cutting the block-shaped gasket is also included.

[0087] In this embodiment, a cutting process step is added after the heating and curing step is completed, so that the size of the gasket can be adaptively adjusted according to actual needs, which is more conducive to the promotion and application of the thermal conductive and absorbing gasket.

[0088] It should be noted that, in the step of cutting, the specific cutting standard is not limited, for example, the cutting can be performed according to the 2 mm standard.

[0089] It should be noted that, in the preparation process of the heat-conducting and wave-absorbing gasket, any process or step not specifically limited may be arranged according to conventional selection in the art.

[0090] In a fourth aspect, an embodiment of the present application provides a heat-conductive and wave-absorbing gasket, which is prepared by the preparation method of the heat-conductive and wave-absorbing gasket provided in the embodiment of the third aspect.

[0091] It should be noted that there is no limitation on the specific application scenarios of thermally conductive and absorbing gaskets. For example, they can be smart phones, computers, routers, switches, network communications, infrared thermal imagers, security equipment, medical electronics, automotive electronics, aerospace, military electronics, optical modules, integrated circuits, heat sinks, and high-frequency IC and RF modules.

[0092] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0093] Example 1

[0094] The present invention provides a method for preparing a gasket, comprising the following steps:

[0095] 1. Preparation of magnetic coated carbon fiber materials

[0096] S1 Carbon fibers (diameter 15 μm, length 200 μm, thermal conductivity 1200 W / mK, purchased from Mitsubishi Chemical brand agent) were placed in a sodium hydroxide solution (OH - The sample was immersed in a solution of 10 mol / L of deionized water for 5 min, then taken out and rinsed with deionized water until neutral and dried.

[0097] S2 The cleaned carbon fiber is placed in a nitric acid solution (H + The carbon fiber was immersed in a solution having a molar concentration of 16 mol / L) for 5 min, then taken out and washed with deionized water until neutral, to obtain pretreated carbon fiber and dried.

[0098] S3 transfers the pretreated carbon fiber to a plasma device for plasma treatment to obtain modified carbon fiber; wherein the atmosphere of the plasma treatment includes nitrogen and oxygen, the volume proportion of oxygen is 60%, the discharge power is 2000W, and the treatment time is 30min.

[0099] S4: the modified carbon fiber and the ferric chloride solution are mixed and reacted at 100°C for 30 minutes. After the reaction is completed, the modified carbon fiber is filtered and dried to obtain a magnetic coated carbon fiber material. 3+ The molar concentration is 10 mol / L.

[0100] 2. Preparation of gasket

[0101] S5: According to the mass percentage, 12 parts of the above-mentioned magnetic coated carbon fiber material, 32 parts of spherical alumina with a particle size of 10 μm (purchased from Dengka brand agent), 35 parts of spherical carbonyl iron powder with a particle size of 5 μm (purchased from Guangdong Jinhong New Materials Co., Ltd.), 15 parts of hexagonal boron nitride (purchased from 3M brand agent), 5 parts of AB glue with a viscosity of 1000 Pa / s (purchased from Guangzhou Chensi New Materials Technology Co., Ltd.), 1 part of silane coupling agent (purchased from Shin-Etsu Chemical brand agent) and 0.01 part of ethynyl cyclohexanol (purchased from Shin-Etsu Chemical brand agent) are mixed and stirred evenly with a planetary mixer to obtain a mixture.

[0102] S6 conveys the mixture to an extruder and performs extrusion orientation treatment to obtain oriented strips; then the oriented strips are stacked and extruded into blocks; then the blocks are transferred to an oven and heat treated at 90°C for 12 hours to vulcanize the AB rubber in the blocks; then, an ultrasonic knife is used to cut the heat-treated blocks according to a standard thickness of 2 mm to obtain sheet gaskets.

[0103] Example 2

[0104] The present embodiment provides a method for preparing a gasket, which differs from the embodiment 1 only in that:

[0105] S5: According to the mass percentage, 18 parts of the above-mentioned magnetic coated carbon fiber material, 32 parts of spherical alumina with a particle size of 10 μm (purchased from Dengka brand agent), 35 parts of spherical carbonyl iron powder with a particle size of 5 μm (purchased from Guangdong Jinhong New Materials Co., Ltd.), 15 parts of hexagonal boron nitride (purchased from 3M brand agent), 6 parts of AB glue with a viscosity of 1000 Pa / s (purchased from Guangzhou Chensi New Materials Technology Co., Ltd.), 1 part of silane coupling agent (purchased from Shin-Etsu Chemical brand agent) and 0.01 part of ethynyl cyclohexanol (purchased from Shin-Etsu Chemical brand agent) are mixed and stirred evenly with a planetary mixer to obtain a mixture.

[0106] Example 3

[0107] The present embodiment provides a method for preparing a gasket, which differs from the embodiment 1 only in that:

[0108] S5: According to the mass proportions, 30 parts of the above-mentioned magnetic coated carbon fiber material with a particle size of 15 μm, 32 parts of spherical alumina with a particle size of 10 μm (purchased from Dengka brand agent), 35 parts of spherical carbonyl iron powder with a particle size of 5 μm (purchased from Guangdong Jinhong New Materials Co., Ltd.), 15 parts of hexagonal boron nitride (purchased from 3M brand agent), 8 parts of AB glue with a viscosity of 1000 Pa / s (purchased from Guangzhou Chensi New Materials Technology Co., Ltd.), 1 part of silane coupling agent (purchased from Shin-Etsu Chemical brand agent) and 0.01 part of ethynyl cyclohexanol (purchased from Shin-Etsu Chemical brand agent) are mixed and stirred evenly with a planetary mixer to obtain a mixture.

[0109] Example 4

[0110] The present embodiment provides a method for preparing a gasket, which differs from the embodiment 1 only in that:

[0111] In step S2, H + The molar concentration is 10 mol / L.

[0112] Example 5

[0113] The present embodiment provides a method for preparing a gasket, which differs from the embodiment 1 only in that:

[0114] In step S5, Fe in the ferric chloride solution 3+ The molar concentration is 5 mol / L.

[0115] Example 6

[0116] The present embodiment provides a method for preparing a gasket, which differs from the embodiment 1 only in that:

[0117] In step S5, hexagonal boron nitride is not added.

[0118] Comparative Example 1

[0119] The comparative example of the present application provides a method for preparing a gasket, which differs from Example 1 only in that:

[0120] Step S2 was not performed, that is, the strong acid solution soaking was not performed.

[0121] Comparative Example 2

[0122] The comparative example of the present application provides a method for preparing a gasket, which differs from Example 1 only in that:

[0123] Step S3 was not performed, that is, no plasma treatment was performed.

[0124] Comparative Example 3

[0125] The comparative example of the present application provides a method for preparing a gasket, which differs from Example 1 only in that:

[0126] Steps S2 and S3 were not performed, that is, strong acid solution immersion and plasma treatment were not performed.

[0127] Test Example 1

[0128] Gasket performance test

[0129] Test method:

[0130] The gaskets prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were numbered respectively, and then the thermal conductivity, thermal resistance, absorption frequency band and absorption loss of each sample were tested.

[0131] The thermal conductivity and thermal resistance were tested using the Ruiling LW-9389 device. Specifically, the relevant parameters were set as follows: hot end temperature was 80°C, pressure was 10psi, test time was 20min, sample size was 25.4*2*25.4mm; ASTMD 5470 standard test method for thermal transmission performance of thin thermal conductive solid materials was used. The absorbing frequency band and absorbing loss were tested in accordance with the GJB2039A-2011 "Test method for reflectivity of radar absorbing materials" standard.

[0132] Table 1 Gasket performance statistics

[0133]

[0134] Referring to Table 1, it can be seen from the test results of Examples 1 to 6 and Comparative Example 1 that after the carbon fiber is immersed in a strong acid solution and then subjected to plasma treatment and magnetic material coating in sequence, compared with directly subjecting the carbon fiber to plasma treatment and magnetic material coating in sequence, the magnetic coated carbon fiber material obtained by the first preparation method has both good thermal conductivity and high-frequency wave absorption performance, and accordingly, the corresponding gasket also has both good thermal conductivity and high-frequency wave absorption performance.

[0135] It can be seen from the test results of Example 1 and Example 4 that when the carbon fiber is immersed in a strong acid solution, the H + The molar concentration is limited within a specific range, which can achieve a better etching effect, thereby facilitating the subsequent loading of polar groups and the effective coating of carbon fibers by magnetic materials, so that the obtained magnetic coated carbon fiber material has both good thermal conductivity and high-frequency wave absorption performance. Correspondingly, the corresponding gasket also has both good thermal conductivity and high-frequency wave absorption performance.

[0136] It can be seen from the test results of Example 1 and Example 5 that the Fe 3+ The molar concentration of Fe is limited to a specific range in order to provide sufficient Fe 3+ , which can realize the effective coating of carbon fiber with magnetic material, so that the obtained magnetic coated carbon fiber material has both good thermal conductivity and high-frequency wave absorption performance. Correspondingly, its corresponding gasket also has both good thermal conductivity and high-frequency wave absorption performance.

[0137] It can be seen from the test results of Example 1 and Example 6 that adding hexagonal boron nitride to the base material can help improve the high-frequency wave absorption performance of the corresponding gasket, and at the same time, can also improve the thermal conductivity of the corresponding gasket to a certain extent.

[0138] It can be seen from the test results of Example 1 and Comparative Examples 1 to 3 that the magnetic coated carbon fiber material prepared by sequentially subjecting the carbon fiber to strong acid solution immersion treatment, plasma treatment and magnetic material coating treatment has better high-frequency wave absorption performance than that obtained by subjecting the carbon fiber to only one or two of the treatments. Correspondingly, the corresponding gasket also has better high-frequency wave absorption performance.

[0139] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A method for preparing a magnetic coated carbon fiber material, characterized in that: The following steps are involved: Soaking the carbon fiber in a strong acid solution so that the surface of the carbon fiber is etched to obtain a pretreated carbon fiber; transferring the pretreated carbon fiber to a plasma device and performing plasma treatment to obtain modified carbon fiber; The modified carbon fiber and a magnetic solution containing trivalent iron ions are mixed and reacted to obtain a magnetic coated carbon fiber material.

2. The method for preparing a magnetic coated carbon fiber material according to claim 1, characterized in that: The acid in the strong acid solution is selected from at least one of nitric acid, sulfuric acid and hydrochloric acid; Optionally, the H in the strong acid solution + The molar concentration is 12-20 mol / L; Optionally, the carbon fiber is immersed in the strong acid solution for 3 to 8 minutes.

3. The method for preparing a magnetic coated carbon fiber material according to claim 1, characterized in that: In the plasma treatment step, the discharge power is 1000-5000W and the treatment time is 20-40min.

4. The method for preparing a magnetic coated carbon fiber material according to claim 1, characterized in that: The diameter of the carbon fiber is 10-20 μm, and the length of the carbon fiber is 100-300 μm; and / or, the Fe 3+ The molar concentration is 8-12 mol / L.

5. A magnetic coated carbon fiber material, characterized in that: The magnetic coated carbon fiber material is prepared by the preparation method of any one of claims 1 to 4.

6. A method for preparing a thermally conductive wave-absorbing gasket, characterized in that: The following steps are involved: 1 to 300 parts of the magnetic coated carbon fiber material according to claim 5 and a base material are mixed to obtain a mixture, wherein the base material comprises 1 to 100 parts of a thermal conductive filler, 1 to 30 parts of an AB glue, 1 to 10 parts of a coupling agent and 0.1 to 1 part of a reaction inhibitor; The mixture is sequentially subjected to extrusion orientation treatment, stacking extrusion treatment and heating curing treatment to obtain a heat-conducting wave-absorbing gasket.

7. The method for preparing the thermally conductive wave absorbing gasket according to claim 6, characterized in that: The base material also includes 1 to 100 parts of hexagonal boron nitride; Optionally, the base material further includes 1 to 100 parts of carbonyl iron powder.

8. The method for preparing the heat-conducting and wave-absorbing gasket according to claim 7, characterized in that: The thermally conductive filler and / or the carbonyl iron powder are spherical.

9. The method for preparing the heat-conducting and wave-absorbing gasket according to claim 7, characterized in that: The particle size of the thermal conductive filler is 1 to 10 μm, and the particle size of the carbonyl iron powder is 1 to 5 μm.

10. A heat-conducting and wave-absorbing gasket, characterized in that: The thermally conductive and wave-absorbing gasket is prepared by the preparation method of any one of claims 6 to 9.

Citation Information

Cited By

  • High-thermal-conductivity wave-absorbing carbon fiber heat-conducting gasket and preparation method thereof

    CN122445192A