Preparation method of early-strength anti-carbonization super-sulfate cement-based material

By modifying the treatment of slag and gypsum, the early strength and carbonization resistance of ultrasulfate cement are improved, and the problems of low early strength and poor carbonization resistance are solved, achieving more stable mechanical properties and extended service life.

CN119038937APending Publication Date: 2024-11-29QINGDAO UNIV OF TECH +3
View PDF 0 Cites 8 Cited by

Patent Information

Application Number
CN202411228516.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The early low strength and poor carbonization resistance of ultrasulfate cement lead to deterioration of mechanical properties and surface sanding during service, which limits its promotion and application.

Method used

By modifying the treatment of slag and gypsum, an efficient supersulfate cement-based material is formed, and the formation of ettringite is promoted by using water-soluble dihydrogen phosphate and magnesium oxide, which improves early strength and condensation rate, and reacts with carbon dioxide through γ-C2S Form calcium carbonate and silica gel to enhance the resistance to carbonization.

Benefits of technology

It significantly improves the early strength and coagulation rate of ultrasulfate cement, while enhancing its resistance to carbonization, prevents mechanical properties and surface sanding, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038937A_ABST
    Figure CN119038937A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an early-strength anti-carbonization super-sulfate cement-based material, which comprises the following steps: (i) dispersing gypsum powder, gamma-C2S powder and water-soluble dihydric phosphate powder into a non-aqueous solvent, grinding, separating out a solid product after grinding, and drying to obtain modified gypsum powder; and (ii) heating a wet material formed by the slag powder and a sodium hydroxide solution, preserving heat, adding excessive Mg < 2 + > solution, uniformly stirring, calcining the obtained mixture, and grinding the calcined product to obtain the modified slag powder. And (iii) taking the following raw materials: the modified slag powder, the modified gypsum powder, an alkali activator, fibers and a water reducing agent. The above raw materials are uniformly mixed to obtain the supersulfate cement-based material. The method provided by the invention not only improves the early strength and coagulation rate of the super sulfate cement, but also improves the carbonization resistance of the super sulfate cement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of super sulfate cement preparation, and in particular to a method for preparing an early strength carbonation-resistant super sulfate cement-based material. Background Art

[0002] Supersulfate cement is a new type of cementitious material made of slag as the main raw material, supplemented by gypsum (sulfate activator), clinker or lime (alkali activator). Compared with traditional Portland cement, supersulfate cement has the advantages of low hydration heat, high late strength, good resistance to sulfate and chloride ion corrosion, etc. In particular, the preparation of supersulfate cement does not require the calcination process of Portland cement. It only needs to grind the raw materials and mix them evenly, which significantly reduces its energy consumption and CO2 emissions. In addition, since supersulfate cement can also consume a large amount of industrial solid waste such as slag, supersulfate cement is a low-carbon emission energy-saving and environmentally friendly building material.

[0003] Although supersulfate cement has many advantages, its disadvantages are also obvious, the most important of which is the long setting and hardening time and low early strength. In addition, since the hydration products of supersulfate cement are mainly composed of calcium silicate hydrate (CSH) and ettringite, ettringite has poor carbonation resistance and is easily decomposed under the action of carbon dioxide and water, resulting in the deterioration of the mechanical properties of supersulfate cement and the phenomenon of surface sanding due to the erosion of carbon dioxide during service, which is one of the main problems restricting the promotion and application of supersulfate cement. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for preparing an early-strength carbonation-resistant supersulfate cement-based material, which not only improves the early strength and setting rate of supersulfate cement, but also improves the carbonation resistance of supersulfate cement. Specifically, the technical solution of the present invention is as follows.

[0005] A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Gypsum powder, γ-C2S powder and water-soluble dihydrogen phosphate powder are dispersed in a non-aqueous solvent and ground. After grinding, a solid product is separated and dried to obtain modified gypsum powder for later use.

[0006] (ii) The wet material formed by slag powder and sodium hydroxide solution is heated and kept warm, and then excess Mg is added 2+ The solution is stirred evenly, and then the obtained mixture is calcined. After completion, the calcined product is ground to obtain modified slag powder for standby use.

[0007] (iii) Take the following raw materials: 68-90 parts by weight of the modified slag powder, 12-25 parts by weight of the modified gypsum powder, 3-7 parts by weight of an alkali activator, 14-20 parts by weight of fiber, and 0.5-1 part by weight of a water reducing agent, and mix the raw materials uniformly to obtain a supersulfate cement-based material.

[0008] Furthermore, in step (i), the γ-C2S powder accounts for 21-27% of the mass of the gypsum powder, and the water-soluble dihydrogen phosphate powder accounts for 8-14% of the mass of the gypsum powder.

[0009] Furthermore, in step (i), the gypsum includes at least one of natural dihydrate gypsum, desulfurized gypsum, phosphogypsum, fluorinated gypsum, titanium gypsum, and the like.

[0010] Furthermore, in step (i), the water-soluble dihydrogen phosphate includes at least one of sodium dihydrogen phosphate, potassium dihydrogen phosphate, ammonium dihydrogen phosphate, etc.

[0011] Furthermore, in step (i), the material-liquid ratio of the gypsum powder, γ-C2S powder, water-soluble dihydrogen phosphate powder and non-aqueous solvent is 1g:20-35ml. Optionally, the non-aqueous solvent includes any one of anhydrous methanol, anhydrous ethanol and the like.

[0012] Furthermore, in step (i), the specific surface area of ​​the modified gypsum powder is not less than 450 m 2 / kg. For example, 450~550m 2 / kg, etc.

[0013] Furthermore, in step (ii), the ratio of the slag powder to the sodium hydroxide solution is 1 g: 0.2-0.3 ml. Optionally, the concentration of the sodium hydroxide solution is 15-30%.

[0014] Furthermore, in step (ii), the insulation temperature is 40-60° C. and the time is 1-2 hours.

[0015] Furthermore, in step (ii), the Mg 2+ With sodium hydroxide solution OH - The molar ratio of Mg is 1.1 to 1.3:1. 2+ The solution includes at least one of a magnesium chloride solution, a magnesium sulfate solution, a magnesium nitrate solution, and the like.

[0016] Furthermore, in step (ii), the calcination treatment is carried out at a temperature of 420-550° C. and for a time of 30-60 min.

[0017] Furthermore, in step (ii), the specific surface area of ​​the modified slag powder is not less than 450 m 2 / kg, such as 450~550m2 / kg, etc.

[0018] Further, in step (ii), the fiber includes at least one of glass fiber, basalt fiber, organic fiber (such as polyethylene fiber, polypropylene fiber, polyacrylonitrile fiber), etc. Optionally, the length of the fiber is 1-10 mm.

[0019] Furthermore, in step (iii), the water reducer includes any one of a polycarboxylate water reducer, a wood sulfonate water reducer, a polycyclic aromatic salt water reducer, and the like.

[0020] Furthermore, in step (iii), the alkali activator includes at least one of calcium hydroxide, calcium oxide, sodium silicate, silicate cement clinker, etc.

[0021] Compared with the prior art, the present invention has at least the following beneficial technical effects: The present invention adopts modified slag and gypsum to prepare supersulfate cement-based materials, which not only improves the early strength and setting rate of supersulfate cement, but also improves the carbonation resistance of supersulfate cement. Wherein, the modified gypsum is formed by gypsum loaded with γ-C2S and water-soluble dihydrogen phosphate, and the modified slag powder is formed by active slag loaded with magnesium oxide. When the modified gypsum and modified slag powder are used to prepare supersulfate cement-based materials, on the one hand, the acidic environment formed by the water-soluble dihydrogen phosphate under the action of mixing water will not only increase the dissolution rate of gypsum, but also increase the concentration of sulfate and calcium ions. Since the formation of hydration product calcium sulfonate depends on sulfate ions and calcium ions, the lower solubility of gypsum leads to the formation rate of calcium sulfonate being limited. After the dissolution rate of gypsum is promoted by the above-mentioned process of the present invention, the formation of calcium sulfonate can be accelerated, thereby improving the early strength and setting rate of supersulfate cement-based materials. On the other hand, the dihydrogen phosphate reacts with the magnesium oxide on the modified slag powder under the action of mixing water, and the formed cementitious product struvite has the characteristics of high strength and high adhesion, and because the rate of the hydration reaction is fast, the early strength and setting rate of the supersulfate cement-based material are further improved. On the other hand, since the present invention first treats the slag powder with sodium hydroxide, the glassy mineral phase of the slag can be depolymerized, and coupled with the high-temperature activation effect during the subsequent calcination treatment, the hydration reaction activity of the slag powder is effectively improved, thereby promoting the improvement of the early strength and setting rate of the supersulfate cement-based material. At the same time, the present invention also uses the step of activating the slag to form magnesium oxide, which reacts with the dihydrogen phosphate used to increase the dissolution rate of gypsum, further improving the early strength of the supersulfate cement-based material. In addition, since the formed ettringite is doped with γ-C2S, the hydration activity of γ-C2S is very weak and almost no hydration reaction occurs, but γ-C2S is highly sensitive to carbon dioxide and can preferentially undergo a carbonation reaction with the carbon dioxide that enters the supersulfate cement-based material to form calcium carbonate and colloid of silica, thereby consuming and fixing the carbon dioxide that has entered the supersulfate cement-based material, which not only improves the carbonation resistance of the ettringite, but also the formation of the calcium carbonate and colloid of silica coated on the surface of the ettringite helps prevent the ettringite from further contacting with carbon dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein: Figure 1 This is a modified gypsum powder sample prepared in the following Example 1.

[0023] Figure 2 The following is a compressive strength test diagram of Example 1.

[0024] Figure 3 This is the carbonization resistance test sample of Example 1 below. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.

[0026] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. The preparation method of the early-strength carbonation-resistant supersulfate cement-based material of the present invention is now further described in conjunction with the accompanying drawings and specific embodiments of the specification.

[0027] Example 1 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Disperse natural dihydrate gypsum powder, γ-C2S powder, and potassium dihydrogen phosphate powder in anhydrous ethanol for mechanical grinding, wherein: the γ-C2S powder accounts for 25% of the mass of the gypsum powder. The potassium dihydrogen phosphate powder accounts for 12% of the mass of the gypsum powder, and the solid-liquid ratio of each powder to anhydrous ethanol is 1g:30ml. After completion, filter out the solid product, dry it at 60°C to remove the anhydrous ethanol, and obtain a specific surface area of ​​about 520m 2 / kg of modified gypsum powder (such as Figure 1 as shown), for standby use.

[0028] (ii) Granulated blast furnace slag powder and 30% sodium hydroxide solution were mixed in a ratio of 1 g:0.2 ml and stirred to form a wet material. The wet material was then placed in a sealed container and heated to 45°C in a water bath for 2 hours. 2+ With the sodium hydroxide solution OH - The magnesium chloride solution was added in a molar ratio of 1.3:1 and stirred evenly. The obtained mixture was dried and heated to 480°C at a heating rate of 10°C / min and calcined for 40 minutes. After cooling to room temperature, the calcined product was ground to obtain a specific surface area of ​​about 500m 2 / kg modified slag powder (such as Figure 1 as shown), for standby use.

[0029] (iii) Take the following raw materials: 80 parts by weight of the modified slag powder prepared in this example, 21 parts by weight of the modified gypsum powder prepared in this example, 5 parts by weight of calcium hydroxide, 17 parts by weight of basalt fiber with a length of 5 mm, and 0.8 parts by weight of polycarboxylate water reducer. Mix the above raw materials and stir them evenly to obtain a supersulfated cement-based material.

[0030] Performance Testing: (1) According to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T 17671-2021), the supersulfate cement-based material prepared in this example was made into test pieces, and then the early compressive strength at the age of 3d was tested (such as Figure 2 The results are shown in the following table.

[0031] (2) The supersulfate cement-based material prepared in this example was mixed with crushed stone, river sand and water to prepare test pieces, which were cured to an age of 28 days, and then carbonized for 28 days according to the Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete (GB / T 50082-2009). The obtained samples (such as Figure 3 The carbonization depth was measured (as shown) and the results are shown in the following table.

[0032] (3) The initial setting time of the supersulfate cement-based material prepared in this example was tested according to the "Test Method for Standard Consistency, Setting Time and Stability of Cement" (GBT1346-2011). The results are shown in the following table: .

[0033] Example 2 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Disperse natural dihydrate gypsum powder, γ-C2S powder, and ammonium dihydrogen phosphate powder in anhydrous ethanol for mechanical grinding, wherein: the γ-C2S powder accounts for 21% of the mass of the gypsum powder. The ammonium dihydrogen phosphate powder accounts for 8% of the mass of the gypsum powder, and the solid-liquid ratio of each powder to anhydrous ethanol is 1g:20ml. After completion, filter out the solid product, dry it at 60°C to remove the anhydrous ethanol, and obtain a specific surface area of ​​454m 2 / kg of modified gypsum powder, set aside.

[0034] (ii) Granulated blast furnace slag powder and 15% sodium hydroxide solution were mixed in a ratio of 1 g:0.3 ml and stirred to form a wet material. The wet material was then placed in a sealed container and heated to 40°C in a water bath for 1.5 hours. 2+ With the sodium hydroxide solution OH -The magnesium sulfate solution was added in a molar ratio of 1.1:1 and stirred evenly. The obtained mixture was dried and heated to 550°C at a heating rate of 10°C / min and calcined for 30 min. After cooling to room temperature, the calcined product was ground to obtain a specific surface area of ​​about 470m 2 / kg of modified slag powder for later use.

[0035] (iii) Take the following raw materials: 68 parts by weight of the modified slag powder prepared in this example, 12 parts by weight of the modified gypsum powder prepared in this example, 3 parts by weight of calcium oxide, 14 parts by weight of glass fiber with a length of 1 mm, and 0.5 parts by weight of polycarboxylate water reducer. Mix the above raw materials and stir them evenly to obtain a supersulfate cement-based material.

[0036] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0037] Example 3 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Desulfurized gypsum powder, γ-C2S powder, and potassium dihydrogen phosphate powder were dispersed in anhydrous methanol for mechanical grinding, wherein: the γ-C2S powder accounted for 27% of the mass of the gypsum powder. The potassium dihydrogen phosphate powder accounted for 14% of the mass of the gypsum powder, and the solid-liquid ratio of each powder to anhydrous methanol was 1g:35ml. After completion, the solid product was filtered out and dried at 60°C to remove the anhydrous methanol, obtaining a specific surface area of ​​558m 2 / kg of modified gypsum powder, set aside.

[0038] (ii) Granulated blast furnace slag powder and 20% sodium hydroxide solution were mixed in a ratio of 1 g:0.2 ml and stirred to form a wet material. The wet material was then placed in a sealed container and heated to 60°C in a water bath for 1 hour. 2+ With the sodium hydroxide solution OH - The magnesium nitrate solution was added in a molar ratio of 1.2:1 and stirred evenly. The obtained mixture was dried and heated to 420°C at a heating rate of 10°C / min for calcination for 60 min. After cooling to room temperature, the calcined product was ground to obtain a specific surface area of ​​about 550m 2 / kg of modified slag powder for later use.

[0039] (iii) Take the following raw materials: 90 parts by weight of the modified slag powder prepared in this example, 25 parts by weight of the modified gypsum powder prepared in this example, 7 parts by weight of 42.5 ordinary Portland cement clinker, 20 parts by weight of polypropylene fibers with a length of 10 mm, and 1 part by weight of sodium wood sulfonate water reducer. Mix the above raw materials and stir them evenly to obtain a supersulfate cement-based material.

[0040] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0041] Example 4 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: Take the following raw materials: specific surface area is about 500m 2 / kg granulated blast furnace slag powder 80 parts by weight, specific surface area of ​​about 520m 2 21 parts by weight of natural dihydrate gypsum powder of 1.57 kg / kg, 5 parts by weight of calcium hydroxide, 17 parts by weight of basalt fiber of 5 mm in length, and 0.8 parts by weight of polycarboxylate water reducer. The above raw materials are mixed and stirred evenly to obtain a supersulfate cement-based material.

[0042] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0043] Example 5 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: Take the following raw materials: 80 parts by weight of the modified slag powder prepared in Example 1 above, with a specific surface area of ​​about 520 m 2 21 parts by weight of natural dihydrate gypsum powder of 1.57 kg / kg, 5 parts by weight of calcium hydroxide, 17 parts by weight of basalt fiber of 5 mm in length, and 0.8 parts by weight of polycarboxylate water reducer. The above raw materials are mixed and stirred evenly to obtain a supersulfate cement-based material.

[0044] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0045] Example 6 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: Take the following raw materials: specific surface area is about 470m 2 68 parts by weight of granulated blast furnace slag powder / kg, 12 parts by weight of modified gypsum powder prepared in Example 2, 3 parts by weight of calcium oxide, 14 parts by weight of glass fiber with a length of 1 mm, and 0.5 parts by weight of polycarboxylate water reducer. The above raw materials are mixed and stirred evenly to obtain a supersulfate cement-based material.

[0046] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0047] Example 7 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Desulfurized gypsum powder and γ-C2S powder were dispersed in anhydrous methanol for mechanical grinding, wherein the γ-C2S powder accounted for 27% of the mass of the gypsum powder, and the solid-liquid ratio of each powder to anhydrous methanol was 1g:35ml. After completion, the solid product was filtered out and dried at 60°C to remove the anhydrous methanol, obtaining a specific surface area of ​​558m 2 / kg of modified gypsum powder, set aside.

[0048] (ii) Take the following raw materials: 90 parts by weight of the modified slag powder prepared in the above Example 3, 25 parts by weight of the modified gypsum powder prepared in this Example, 7 parts by weight of 42.5 ordinary Portland cement clinker, 20 parts by weight of polypropylene fibers with a length of 10 mm, and 1 part by weight of sodium wood sulfonate water reducer. Mix the above raw materials and stir them evenly to obtain a supersulfate cement-based material.

[0049] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0050] Example 8 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Disperse natural dihydrate gypsum powder and diammonium phosphate powder in anhydrous ethanol for mechanical grinding, wherein the diammonium phosphate powder accounts for 8% of the mass of the gypsum powder, and the solid-liquid ratio of each powder to anhydrous ethanol is 1g:20ml. After completion, filter out the solid product, dry it at 60°C to remove the anhydrous ethanol, and obtain a specific surface area of ​​454m2 / kg of modified gypsum powder, set aside.

[0051] (ii) Take the following raw materials: 68 parts by weight of the modified slag powder prepared in the above Example 2, 12 parts by weight of the modified gypsum powder prepared in this example, 3 parts by weight of calcium oxide, 14 parts by weight of glass fiber with a length of 1 mm, and 0.5 parts by weight of polycarboxylate water reducer. Mix the above raw materials and stir them evenly to obtain a supersulfate cement-based material.

[0052] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0053] Example 9 A method for preparing an early-strength carbonation-resistant super-sulfate cement-based material comprises the following steps: (i) Granulated blast furnace slag powder and 20% sodium hydroxide solution by mass fraction were mixed in a ratio of 1g:0.2ml and stirred to form a wet material. The wet material was then placed in a sealed container and heated to 60°C in a water bath for 1 hour. The slag powder was then filtered out, dried, heated to 420°C at a heating rate of 10°C / min, and calcined for 60 minutes. After cooling to room temperature, the calcined product was ground to obtain a specific surface area of ​​about 550m 2 / kg of modified slag powder for later use.

[0054] (ii) Take the following raw materials: 90 parts by weight of the modified slag powder prepared in this example, 25 parts by weight of the modified gypsum powder prepared in the above example 3, 7 parts by weight of 42.5 ordinary Portland cement clinker, 20 parts by weight of polypropylene fibers with a length of 10 mm, and 1 part by weight of sodium wood sulfonate water reducer. Mix the above raw materials and stir them evenly to obtain a supersulfate cement-based material.

[0055] The 3d compressive strength, carbonation resistance and initial setting time of the supersulfate cement-based material prepared in this embodiment were tested by the same method as in the above embodiment 1. The results are shown in the following table: .

[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still repair the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any repair, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an early-strength carbonation-resistant supersulfate cement-based material, characterized in that: The steps include: (i) dispersing gypsum powder, γ-C2S powder and water-soluble dihydrogen phosphate powder in a non-aqueous solvent for grinding, separating out a solid product after grinding, drying the solid product to obtain modified gypsum powder for later use; (ii) The wet material formed by slag powder and sodium hydroxide solution is heated and kept warm, and then excess Mg is added 2+ The solution is stirred evenly, and then the obtained mixture is calcined. After completion, the calcined product is ground to obtain modified slag powder for later use; (iii) taking the following raw materials: 68-90 parts by weight of the modified slag powder, 12-25 parts by weight of the modified gypsum powder, 3-7 parts by weight of an alkali activator, 14-20 parts by weight of fiber, and 0.5-1 part by weight of a water reducing agent; and uniformly mixing the above raw materials to obtain a supersulfate cement-based material.

2. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (i), the γ-C2S powder accounts for 21-27% of the mass of the gypsum powder; the water-soluble dihydrogen phosphate powder accounts for 8-14% of the mass of the gypsum powder; Optionally, in step (i), the gypsum includes at least one of natural dihydrate gypsum, desulfurized gypsum, phosphogypsum, fluorinated gypsum, and titanium gypsum; Optionally, in step (i), the water-soluble dihydrogen phosphate includes at least one of sodium dihydrogen phosphate, potassium dihydrogen phosphate, and ammonium dihydrogen phosphate.

3. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (i), the material-liquid ratio of the gypsum powder, γ-C2S powder, water-soluble dihydrogen phosphate powder and non-aqueous solvent is 1g:20-35ml; Optionally, in step (i), the non-aqueous solvent includes any one of anhydrous methanol and anhydrous ethanol.

4. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (i), the specific surface area of ​​the modified gypsum powder is not less than 450 m 2 / kg.

5. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (ii), the ratio of the slag powder to the sodium hydroxide solution is 1 g: 0.2-0.3 ml; optionally, the concentration of the sodium hydroxide solution is 15-30%.

6. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (ii), the insulation temperature is 40-60° C. and the time is 1-2 hours.

7. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (ii), the Mg 2+ With sodium hydroxide solution OH - The molar ratio is 1.1~1.3:1; Optionally, in step (ii), the Mg 2+ The solution includes at least one of a magnesium chloride solution, a magnesium sulfate solution, and a magnesium nitrate solution.

8. The method for preparing the early-strength carbonation-resistant super-sulfate cement-based material according to claim 1, characterized in that: In step (ii), the calcination temperature is 420-550°C and the time is 30-60 min; Optionally, in step (ii), the specific surface area of ​​the modified slag powder is not less than 450 m 2 / kg.

9. The method for preparing the early strength carbonation resistant super sulfate cement-based material according to any one of claims 1 to 8, characterized in that: In step (ii), the fiber includes at least one of glass fiber, basalt fiber, and organic fiber; optionally, the length of the fiber is 1 to 10 mm.

10. The method for preparing the early strength carbonation resistant super sulfate cement-based material according to any one of claims 1 to 8, characterized in that: In step (iii), the water reducer includes any one of a polycarboxylate water reducer, a wood sulfonate water reducer, and a polycyclic aromatic salt water reducer; Optionally, in step (iii), the alkali activator includes at least one of calcium hydroxide, calcium oxide, sodium silicate, and silicate cement clinker.

Citation Information

Cited By

  • Preparation method of anti-carbonization all-solid waste slag-sulphoaluminate cementing material

    CN120736867A

  • Preparation method of anti-carbonization full-solid waste slag-sulfoaluminate cementitious material

    CN120736867B

  • High-carbonization-resistance super-sulfate cement material as well as preparation method and application thereof

    CN122102635A

  • A high-carbonization-resistance type ultra-sulfate cement material, a preparation method and application thereof

    CN122102635B

  • Composite modified carbonization-resistant agent, carbonization-resistant super-sulfate cement material as well as preparation process and application of carbonization-resistant super-sulfate cement material

    CN122464631A