Battery

A thermally reactive layer in batteries with multiple electrode bodies addresses temperature control during emergencies by using endothermic materials to cool and discharge components, enhancing safety and reliability.

JP7562389B2Active Publication Date: 2024-10-07PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020199413
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-01
Publication Date
2024-10-07
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Existing battery technologies struggle to effectively suppress temperature rises during emergencies, such as internal short circuits, particularly in batteries with multiple electrode bodies, which can lead to excessive heat trapping and potential safety hazards.

Method used

Incorporating a thermally reactive layer between electrode bodies with a thermally reactive material that exhibits endothermic action or suppresses radical chain reactions, and strategically sizing this layer to enhance cooling and discharge of materials during emergencies.

Benefits of technology

The thermally reactive layer effectively suppresses temperature rises by rapidly cooling the battery and discharging electrode materials, thereby improving safety and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562389000006
    Figure 0007562389000006
  • Figure 0007562389000007
    Figure 0007562389000007
  • Figure 0007562389000008
    Figure 0007562389000008
Patent Text Reader

Abstract

To provide a battery in which rise in a battery temperature is suppressed in an emergency.SOLUTION: A battery disclosed herein includes: a plurality of electrode bodies 20b arranged side by side in a first direction X; a current collector member 52 attached to an end of each electrode body 20b in a second direction Y; and a thermal reaction layer 70 including a thermal reaction material, the thermal reaction layer being arranged between the electrode bodies 20b. The thermal reaction layer 70 has a main face 72 extending along the second direction Y and a third direction Z, and a side face 74 extending in the first direction X. When a length of a positive electrode active material layer in the second direction Y is La, the main face 72 has a length in the second direction Y of 0.7 La or more and La or less, and, when a length of each of the electrode bodies 20b in the third direction Z is Lb, the main face 72 has a length in the third direction Z of 0.5 Lb or more and 0.8 Lb or less. When a total thickness of positive electrodes in the first direction X is Lm, the side face 74 has a length in the first direction X of 0.05 Lm or more and 0.5 Lm or less.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a battery, and more particularly to a battery including a plurality of electrode assemblies. [Background technology]

[0002] Secondary batteries such as lithium-ion secondary batteries are usually used in a state where the voltage is controlled to be within a predetermined range. However, if an excessive current is supplied due to an incorrect operation or the like, the voltage may exceed the predetermined range and become overcharged. If the overcharge progresses, it may cause inconvenience such as an increase in the temperature inside the battery.

[0003] As a prior art technique for preventing the progression of overcharging, for example, Patent Document 1 discloses a battery comprising a battery case, a wound electrode body arranged inside the battery case, current collecting members attached to both end faces of the wound electrode body, a gas generating material arranged inside the battery case and generating gas as the temperature rises, and a pressure-activated current interrupt device (CID) that operates when the internal pressure of the battery case rises due to gas generation from the gas generating material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-020930 A Summary of the Invention [Problem to be solved by the invention]

[0005] Although the above technology can activate the CID at an early stage of overcharging, it is difficult to respond to an emergency in which the battery temperature continues to rise even after the CID is activated due to factors such as an internal short circuit. In particular, a battery that has multiple electrode bodies inside a battery case and has a current collecting member attached to the end face of each electrode body is prone to heat buildup inside, causing a particularly large temperature rise. Therefore, there is a need to suppress the rise in battery temperature even in such an emergency.

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a battery that includes a plurality of electrode assemblies and in which an increase in battery temperature is suppressed in the event of an emergency. [Means for solving the problem]

[0007] The present invention discloses a battery comprising a plurality of electrode bodies arranged in a first direction, each of which includes a positive electrode having a positive electrode active material layer and a negative electrode having a negative electrode active material layer, a current collecting member attached to an end of the electrode body in a second direction perpendicular to the first direction and electrically connected to the positive electrode or the negative electrode, and a thermal reaction layer arranged between the plurality of electrode bodies in the first direction, each of which includes a thermal reaction material that produces at least one of an endothermic action and an action of suppressing a chain reaction of radicals at a predetermined temperature or higher. When a direction perpendicular to the first direction and the second direction is defined as a third direction, the thermal reaction layer has a main surface that extends along the second direction and the third direction, and a side surface that extends along the first direction. When the length of the positive electrode active material layer in the second direction is defined as La, the length of the main surface in the third direction is 0.7La or more and La or less, and when the length of the electrode body in the third direction is defined as Lb, the length of the electrode body in the third direction is 0.5Lb or more and 0.8Lb or less. The side surface has a length in the first direction of 0.05Lm or more and 0.5Lm or less, where Lm is the total thickness of the positive electrode in the first direction.

[0008] The battery is provided with a thermal reaction layer of a predetermined size between a plurality of electrode bodies, and includes a thermal reaction material. In an emergency where the battery temperature continues to rise (for example, when an internal short circuit occurs in the electrode body), the thermal reaction material produces at least one of an endothermic effect and an effect of suppressing a radical chain reaction when the temperature exceeds a predetermined temperature. In addition, when gas is generated during the reaction, the force of the generated gas can cause the constituent material of the electrode body adjacent to the thermal reaction layer (for example, the material contained in the positive electrode) to be discharged to the outside of the battery case. Due to these effects, in a battery including a plurality of electrode bodies, the inside of the battery can be rapidly cooled, and the rise in the battery temperature can be effectively suppressed.

[0009] In a preferred embodiment of the battery disclosed herein, the thermal reaction layer has a base and a streak portion that is provided continuously from the base and extends in a strip shape along the second direction or the third direction. The streak portion satisfies at least one of the following (1) to (3): (1) the length of the side surface in the first direction is 1.1 to 2 times that of the base; (2) the base and the side surface contain a binder, and the content of the binder is 1.5 to 2 times that of the base; and (3) the porosity is 1.1 to 1.5 times that of the base. With this configuration, a reaction can be efficiently caused in the streak portion in an emergency, and the rise in the battery temperature can be suppressed to a high level.

[0010] In a preferred embodiment of the battery disclosed herein, the thermally reactive material contains a hydroxide that undergoes a dehydration reaction at or above the predetermined temperature. The hydroxide undergoes a dehydration reaction at or above a predetermined temperature (for example, 100°C or higher, or even 200°C or higher) and generates water vapor gas. When the thermally reactive material contains a hydroxide, a water vapor explosion occurs in an emergency, and the material of the electrode body can be suitably discharged to the outside of the battery case with the force of the explosion. Therefore, the rise in the battery temperature can be effectively suppressed.

[0011] In a preferred embodiment of the battery disclosed herein, the thermally reactive material contains a potassium compound that undergoes a thermal decomposition reaction at or above the predetermined temperature. The potassium compound undergoes a thermal decomposition reaction at or above a predetermined temperature (for example, at or above 100°C, or even at or above 200°C) and functions as a so-called chemical fire extinguishing agent. By including a potassium compound in the thermally reactive material, the electrode body can be suitably cooled. Therefore, the rise in the battery temperature can be effectively suppressed.

[0012] In a preferred embodiment of the battery disclosed herein, the positive electrode active material layer contains a particulate positive electrode active material, and the circularity of the positive electrode active material is 0.45 or more. If the circularity of the active material is 0.45 or more, for example, in an emergency, the positive electrode material can be discharged to the outside of the battery together with the generated gas more quickly, and the increase in the battery temperature can be suppressed to a high level. In addition, in such a configuration, the battery temperature is likely to increase in an emergency. Therefore, it is particularly effective to apply the technology disclosed herein.

[0013] In a preferred embodiment of the battery disclosed herein, the packing density of the positive electrode active material layer is 3 g / cm 3 The packing density of the positive electrode active material layer is 3 g / cm 3 If the above is the case, in an emergency, for example, the positive electrode material can be discharged to the outside of the battery together with the generated gas more quickly, and the increase in the battery temperature can be suppressed to a high level. Also, in such a configuration, the battery temperature is likely to increase in an emergency. Therefore, it is particularly effective to apply the technology disclosed herein. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a perspective view showing a battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic vertical cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 4 is a perspective view showing a schematic view of an electrode assembly attached to a sealing plate. [Figure 4] FIG. 2 is a perspective view showing a schematic view of an electrode body and a thermal reaction layer. [Diagram 5]FIG. 2 is a schematic diagram showing the configuration of an electrode body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, some preferred embodiments of the technology disclosed herein will be described with reference to the drawings. It should be noted that matters other than those specifically mentioned in this specification and necessary for carrying out the present invention (for example, the general configuration and manufacturing process of a battery that does not characterize the present invention) can be understood as design matters of a person skilled in the art based on the prior art in the field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the field. In this specification, the expression "A to B" indicating a range includes the meaning of A or more and B or less, as well as "preferably greater than A" and "preferably smaller than B".

[0016] In this specification, the term "battery" refers to any power storage device capable of extracting electrical energy, and is a concept that includes primary batteries and secondary batteries. In addition, in this specification, the term "secondary battery" refers to any power storage device capable of repeated charging and discharging, and is a concept that includes so-called storage batteries (chemical batteries) such as lithium ion secondary batteries and nickel metal hydride batteries, and capacitors (physical batteries) such as electric double layer capacitors.

[0017] <Battery 100> FIG. 1 is a perspective view of the battery 100. FIG. 2 is a schematic longitudinal sectional view taken along line II-II in FIG. 1. In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the symbols X, Y, and Z in the drawings represent the short side direction, long side direction perpendicular to the short side direction, and up-down direction of the battery 100, respectively. The short side direction X is an example of a first direction, the long side direction Y is an example of a second direction, and the up-down direction Z is an example of a third direction. However, these directions are merely for the convenience of description, and do not limit the installation form of the battery 100 in any way.

[0018] As shown in Fig. 2, the battery 100 includes a battery case 10, an electrode assembly 20, a positive electrode terminal 30, a negative electrode terminal 40, a positive electrode current collector 50, a negative electrode current collector 60, and a thermal reaction layer 70 (see Fig. 4). Although not shown, the battery 100 further includes an electrolyte. The battery 100 is a lithium ion secondary battery. The battery 100 is characterized by including the thermal reaction layer 70, and other configurations may be similar to those of a conventional battery.

[0019] The battery case 10 is a housing that houses the electrode assembly 20. Here, the battery case 10 has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. However, the battery case 10 may be cylindrical or bag-shaped. The material of the battery case 10 may be the same as that used conventionally, and is not particularly limited. The battery case 10 is preferably made of metal, and more preferably made of, for example, aluminum, aluminum alloy, iron, iron alloy, or the like. The battery case 10 may be an aluminum laminate film having a metal layer containing aluminum and a fusion layer containing resin. As shown in FIG. 2, the battery case 10 includes an exterior body 12 having an opening 12h, and a sealing plate (lid) 14 that seals the opening 12h.

[0020] As shown in FIG. 1, the exterior body 12 includes a bottom wall 12a, a pair of long side walls 12b extending from the bottom wall 12a and facing each other, and a pair of short side walls 12c extending from the bottom wall 12a and facing each other. The bottom wall 12a is substantially rectangular. The bottom wall 12a faces the opening 12h. The area of ​​the short side walls 12c is smaller than the area of ​​the long side walls 12b. The sealing plate 14 is attached to the exterior body 12 so as to close the opening 12h of the exterior body 12. The sealing plate 14 faces the bottom wall 12a of the exterior body 12. The sealing plate 14 is substantially rectangular in plan view. The battery case 10 is integrated by joining (for example, welding) the sealing plate 14 to the periphery of the opening 12h of the exterior body 12. The battery case 10 is hermetically sealed (sealed).

[0021] As shown in FIG. 2, the sealing plate 14 is provided with a liquid inlet 15, a discharge valve 17, and two terminal outlet holes 18 and 19. The liquid inlet 15 is for injecting an electrolyte after the sealing plate 14 is assembled to the exterior body 12. The liquid inlet 15 is sealed by a sealing member 16. The discharge valve 17 is configured to break when the pressure inside the battery case 10 reaches a predetermined value or higher, thereby discharging gas inside the battery case 10 to the outside. The discharge valve 17 can also function as an outlet for discharging the constituent material of the electrode body group 20 to the outside of the battery case 10 when the battery 100 reaches a predetermined temperature or higher (for example, 100° C. or higher, or even 200° C. or higher). The terminal outlet holes 18 and 19 are formed at both ends of the sealing plate 14 in the long side direction Y. The terminal outlet holes 18 and 19 penetrate the sealing plate 14 in the up-down direction Z. The terminal withdrawal holes 18, 19 each have an inner diameter large enough to allow the positive electrode terminal 30 and the negative electrode terminal 40 to be inserted therethrough before being attached to the sealing plate 14 (before being crimped).

[0022] The positive electrode terminal 30 is disposed at one end of the sealing plate 14 in the long side direction Y (the left end in FIG. 1 and FIG. 2). The negative electrode terminal 40 is disposed at the other end of the sealing plate 14 in the long side direction Y (the right end in FIG. 1 and FIG. 2). As shown in FIG. 2, the positive electrode terminal 30 and the negative electrode terminal 40 extend from the inside to the outside of the sealing plate 14 through the terminal pull-out holes 18 and 19. The positive electrode terminal 30 and the negative electrode terminal 40 are fixed to the sealing plate 14. Here, the positive electrode terminal 30 and the negative electrode terminal 40 are crimped to the peripheral portion surrounding the terminal pull-out holes 18 and 19 of the sealing plate 14 by crimping. The crimped portions 30c and 40c are formed at the ends of the positive electrode terminal 30 and the negative electrode terminal 40 on the side of the exterior body 12 (the lower end in FIG. 2).

[0023] As shown in Fig. 2, the positive electrode terminal 30 is electrically connected to the positive electrode 22 (see Fig. 5) of the electrode assembly 20 via a positive electrode current collector 50 inside the exterior body 12. The negative electrode terminal 40 is electrically connected to the negative electrode 24 (see Fig. 5) of the electrode assembly 20 via a negative electrode current collector 60 inside the exterior body 12. The positive electrode terminal 30 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90. The negative electrode terminal 40 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90.

[0024] A plate-shaped positive electrode external conductive member 32 and a plate-shaped negative electrode external conductive member 42 are attached to the outer surface of the sealing plate 14. The positive electrode external conductive member 32 is electrically connected to the positive electrode terminal 30. The negative electrode external conductive member 42 is electrically connected to the negative electrode terminal 40. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are members to which bus bars are attached when electrically connecting multiple batteries 100 to each other. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are insulated from the sealing plate 14 by an external insulating member 92.

[0025] FIG. 3 is a perspective view that shows a schematic diagram of the electrode assembly group 20 attached to the sealing plate 14. The electrode assembly group 20 has a plurality of electrode assemblies. The electrode assembly group 20 has three electrode assemblies 20a, 20b, and 20c here. However, the number of electrode assemblies arranged inside one exterior body 12 is not particularly limited, and may be two or may be four or more. The electrode assemblies 20a, 20b, and 20c here are electrically connected in parallel. The electrode assemblies 20a, 20b, and 20c are arranged side by side in the short side direction X. The electrode assemblies 20a, 20b, and 20c have a flattened outer shape. The electrode assemblies 20a, 20b, and 20c here are wound electrode assemblies. The electrode assemblies 20a, 20b, and 20c are arranged in the battery case 12 with the winding axis WL (see FIG. 5) oriented substantially parallel to the long side direction Y. An end face of the electrode body 20a perpendicular to the winding axis WL (in other words, the lamination surface where the positive electrodes 22 and the negative electrodes 24 are laminated) faces the short side wall 12c.

[0026] FIG. 4 is a perspective view showing the electrode body 20b and the thermal reaction layer 70. In the following, the electrode body 20b will be described in detail as an example, but the electrode bodies 20a and 20c can have a similar configuration. The electrode body 20b has a pair of curved portions (R portions) 20r and a flat portion 20f connecting the pair of curved portions 20r. One curved portion 20r (upper side of FIG. 4) faces the sealing plate 14, and the other curved portion 20r (lower side of FIG. 4) faces the bottom wall 12a of the exterior body 12. The flat portion 20f faces the long side wall 12b of the exterior body 12. In the electrode bodies 20a, 20b, and 20c adjacent to each other in the short side direction X, the flat portions 20f face each other. Although not particularly limited, in a high-capacity battery such as one used in a vehicle, the length (average length) Lb of the electrode body 20b in the vertical direction Z is generally 10 mm or more, for example 20 mm or more, or even 50 mm or more, and may be generally 200 mm or less, for example 150 mm or less, or even 100 mm or less.

[0027] 5 is a schematic diagram showing the configuration of the electrode body 20b. The electrode body 20b has a positive electrode 22, a negative electrode 24, and a separator 26. In this embodiment, the electrode body 20b is configured by stacking a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 with a strip-shaped separator 26 interposed therebetween, and winding the stack around a winding axis WL. However, the electrode body 20b may be a laminated electrode body in which a plurality of square-shaped (typically rectangular) positive electrodes and a plurality of square-shaped (typically rectangular) negative electrodes are stacked in an insulated state.

[0028] As shown in FIG. 5, the positive electrode 22 has a positive electrode collector 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode collector 22c. However, the positive electrode protective layer 22p is not essential and can be omitted in other embodiments. The positive electrode collector 22c is strip-shaped. The positive electrode collector 22c is made of a conductive metal. Here, the positive electrode collector 22c is a metal foil, specifically an aluminum foil.

[0029] A plurality of positive electrode tabs 22t are provided at one end of the positive electrode collector 22c in the long side direction Y (the left end in FIG. 5). The plurality of positive electrode tabs 22t protrude toward one side of the long side direction Y (the left side in FIG. 5). The plurality of positive electrode tabs 22t protrude in the long side direction Y beyond the separator 26. The positive electrode tab 22t is a part of the positive electrode collector 22c here, and is made of metal foil (aluminum foil). The positive electrode tab 22t has a portion (current collector exposed portion) where the positive electrode active material layer 22a and the positive electrode protective layer 22p of the positive electrode collector 22c are not formed. As shown in FIG. 2 to FIG. 4, the plurality of positive electrode tabs 22t are stacked at one end of the long side direction Y (the left end in FIG. 2 to FIG. 4) to form a positive electrode tab group 23. The positive electrode tab group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode collector 50. The positive electrode tab group 23 is provided with a positive electrode second current collecting portion 52 (see FIG. 4) which will be described later.

[0030] The positive electrode active material layer 22a is provided in a strip shape along the longitudinal direction of the positive electrode current collector 22c, as shown in Fig. 5. Although not particularly limited, the packing density (average packing density) of the positive electrode active material layer 22a is 3 g / cm 3 It is preferable that the content is 3.5 g / cm or more. 3 More preferably, the density is equal to or higher than this. This allows the battery 100 to have a high energy density. This configuration also allows the battery temperature rise to be suppressed to a high level. In addition, with this configuration, the battery temperature is likely to rise in an emergency. Therefore, it is particularly effective to apply the technology disclosed herein. The packing density of the positive electrode active material layer 22a is approximately 5 g / cm 3 For example, 4g / cm 3 It may be the following.

[0031] The positive electrode active material layer 22a contains a positive electrode active material capable of reversibly absorbing and releasing charge carriers. Examples of the positive electrode active material include lithium transition metal composite oxides such as lithium cobalt oxide, lithium manganate, lithium nickel oxide, lithium nickel manganese composite oxide, lithium nickel cobalt composite oxide, and lithium nickel cobalt manganese composite oxide. From the viewpoint of increasing the capacity of the battery, the positive electrode active material preferably contains a composite oxide containing Ni and Li, in which the Ni content in the composite oxide is in the range of 70 to 100 mol % with respect to the total number of moles of the constituent elements in the composite oxide excluding Li and oxygen.

[0032] A suitable example of the positive electrode active material is a material having the following general formula: LiNi x Co y Al z O2 (wherein x is 0.70 to 0.98, y is 0.01 to 0.15, z is 0.01 to 0.15, and x+y+z=1); Another preferred example is a composite oxide represented by the following general formula: LiNi x Co y Mn z O2 (wherein x is 0.70 to 0.98, y is 0.01 to 0.15, z is 0.01 to 0.15, and x+y+z=1); a part of Ni, Co, and Mn may be substituted with a substituting element such as Al, Ti, P, B, Si, Nb, or C. The surface of the positive electrode active material may be covered with a compound containing a coating element such as Al, Ti, P, B, Si, Nb, or C. The total content of the substituting element and the coating element may be about 0.1 to 7% of the entire positive electrode active material.

[0033] The positive electrode active material is typically particulate. Although not particularly limited, the circularity of the positive electrode active material is preferably 0.45 or more, more preferably 0.5 or more, and even more preferably 0.7 or more. With such a configuration, the rise in battery temperature can be suppressed at a high level. In addition, with such a configuration, the battery temperature is likely to rise in an emergency. Therefore, it is particularly effective to apply the technology disclosed herein. The circularity of the positive electrode active material may be 0.99 or less. In this specification, the "circularity" is an index indicating the degree of sphericity in an image of a particle projected onto a two-dimensional plane by electron microscope observation. Specifically, the circularity of each positive electrode active material particle is calculated by the following formula: (circularity) = (perimeter of a perfect circle having the same area as the image of the particle) / (perimeter of the image of the particle); and the circularity of each particle calculated from the images of the particles is averaged to calculate the circularity. In addition, when the positive electrode active material particle is a perfect circle, the circularity is the maximum "1".

[0034] The positive electrode active material layer 22a may contain any component other than the positive electrode active material, such as a conductive material, a binder, various additive components, etc. As the conductive material, for example, a carbon material such as acetylene black (AB) can be used. As the binder, for example, polyvinylidene fluoride (PVdF) can be used.

[0035] As shown in Fig. 5, the positive electrode protective layer 22p is provided at the boundary between the positive electrode current collector 22c and the positive electrode active material layer 22a in the long side direction Y. The positive electrode protective layer 22p is provided in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (e.g., alumina). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additive components, and the like. The conductive material and the binder may be the same as those exemplified as those that may be contained in the positive electrode active material layer 22a.

[0036] Although not particularly limited, in a high-capacity battery used for vehicles, the length (average length) La of the positive electrode active material layer 22a in the long side direction Y may be approximately 100 mm or more, for example, 130 mm or more, or even 200 mm or more, and approximately 500 mm or less, for example, 300 mm or less. In the electrode body 20b, the total thickness Lm (not shown) of the positive electrode 22 in the short side direction X calculated by the product of the thickness of the entire positive electrode 22 and the number of layers may be approximately 2 mm or more, for example, 5 mm or more, or even 8 mm or more, and approximately 30 mm or less, for example, 20 mm or less. The thickness of the entire positive electrode 22 is the average thickness of the portion where the positive electrode active material layer 22a is formed on the positive electrode current collector 22c.

[0037] The negative electrode 24 may be the same as a conventional one, and is not particularly limited. As shown in FIG. 5, the negative electrode 24 has a negative electrode collector 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode collector 24c. The negative electrode collector 24c is strip-shaped. The negative electrode collector 24c is made of a conductive metal. Here, the negative electrode collector 24c is a metal foil, specifically a copper foil.

[0038] A plurality of negative electrode tabs 24t are provided at one end of the negative electrode collector 24c in the long side direction Y (the right end in FIG. 5). The plurality of negative electrode tabs 24t protrude toward one side of the long side direction Y (the right end in FIG. 5). The plurality of negative electrode tabs 24t protrude in the long side direction Y beyond the separator 26. The plurality of negative electrode tabs 24t protrude in the long side direction Y beyond the separator 26. Here, the negative electrode tab 24t is a part of the negative electrode collector 24c, and is made of metal foil (copper foil). Here, the negative electrode tab 24t has a portion (current collector exposed portion) where the negative electrode active material layer 24a of the negative electrode collector 24c is not formed. As shown in FIG. 2 to FIG. 4, the plurality of negative electrode tabs 24t are stacked at one end of the long side direction Y (the right end in FIG. 2 to FIG. 4) to form a negative electrode tab group 25. The negative electrode tab group 25 is provided at a position symmetrical to the positive electrode tab group 23 in the long side direction Y. The negative electrode tab group 25 is electrically connected to the negative electrode terminal 40 via a negative electrode current collecting portion 60. A negative electrode second current collecting portion 62 (see FIG. 4), which will be described later, is attached to the negative electrode tab group 25.

[0039] As shown in FIG. 5, the negative electrode active material layer 24a is provided in a strip shape along the longitudinal direction of the negative electrode current collector 24c. The length Ln of the negative electrode active material layer 24a in the long side direction Y is equal to or longer than the length La of the positive electrode active material layer 22a in the long side direction Y. The negative electrode active material layer 24a contains a negative electrode active material (e.g., a carbon material such as graphite) capable of reversibly absorbing and releasing charge carriers. The negative electrode active material layer 24a may contain any component other than the negative electrode active material, such as a binder, a dispersant, various additive components, and the like. As the binder, for example, rubbers such as styrene butadiene rubber (SBR) can be used. As the dispersant, for example, celluloses such as carboxymethyl cellulose (CMC) can be used.

[0040] The separator 26 is a member that insulates the positive electrode active material layer 22a of the positive electrode 22 from the negative electrode active material layer 24a of the negative electrode 24. As shown in FIG. 5, the length Ls of the separator 26 in the long side direction Y is equal to or longer than the length Ln of the negative electrode active material layer 24a in the long side direction Y. The separator 26 is preferably a resin porous sheet made of a polyolefin resin such as polyethylene (PE) or polypropylene (PP). The separator 26 may have a substrate made of a resin porous sheet and a heat-resistant layer containing an inorganic filler formed on at least one surface of the substrate.

[0041] The electrolyte may be the same as that used in the past and is not particularly limited. The electrolyte is, for example, a non-aqueous electrolyte containing a non-aqueous solvent and a supporting salt. The non-aqueous solvent contains, for example, carbonates such as ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The supporting salt is, for example, a fluorine-containing lithium salt such as lithium hexafluorophosphate (LiPF6). However, the electrolyte may be in a solid state (solid electrolyte) and integrated with the electrode body group 20.

[0042] The positive electrode current collecting part 50 constitutes a conductive path that electrically connects the positive electrode tab group 23 consisting of the multiple positive electrode tabs 22t to the positive electrode terminal 30. As shown in Fig. 2, the positive electrode current collecting part 50 includes a positive electrode first current collecting part 51 and a positive electrode second current collecting part 52. The positive electrode first current collecting part 51 and the positive electrode second current collecting part 52 may be made of the same metal type as the positive electrode current collector 22c, for example, a conductive metal such as aluminum, an aluminum alloy, nickel, or stainless steel.

[0043] The positive electrode first current collecting part 51 is attached to the inner surface of the sealing plate 14. Here, the positive electrode first current collecting part 51 is fixed to the sealing plate 14 by crimping. The positive electrode first current collecting part 51 has a first region that spreads horizontally along the inner surface of the sealing plate 14, and a second region that extends from one end of the first region in the long side direction Y (the left end in FIG. 2) toward the short side wall 12c of the exterior body 12. In the first region, a through hole (not shown) that penetrates in the vertical direction Z is formed at a position corresponding to the terminal pull-out hole 18 of the sealing plate 14. The first region is electrically connected to the positive electrode terminal 30 by crimping. The first region is insulated from the sealing plate 14 by the internal insulating member 80. The second region extends along the vertical direction Z.

[0044] The positive electrode second current collecting portion 52 extends along the short side wall 12c of the exterior body 12. As shown in FIG. 3 and FIG. 4, the positive electrode second current collecting portion 52 is attached to the electrode body 20b. In a configuration in which the electrode body 20b is provided with the positive electrode second current collecting portion 52, heat is likely to be trapped in an emergency, so that it is particularly effective to apply the technology disclosed herein. The positive electrode second current collecting portion 52 has a current collecting plate connection portion 52a electrically connected to the second region of the positive electrode first current collecting portion 51, a tab joint portion 52c attached to the positive electrode tab group 23 and electrically connected to the multiple positive electrode tabs 22t, and a joint portion 52b connecting the current collecting plate connection portion 52a and the tab joint portion 52c. The positive electrode second current collecting portion 52 is an example of a current collecting member.

[0045] The current collector plate connection portion 52a extends along the up-down direction Z. The current collector plate connection portion 52a is provided with a recess 52d that is thinner than the surrounding area. The recess 52d is provided with a through hole 52e that penetrates in the short side direction X. A joint with the positive electrode first current collector portion 51 is formed in the through hole 52e. The joint is a welded joint formed by welding such as ultrasonic welding, resistance welding, laser welding, etc. The tab joint 52c extends along the up-down direction Z. The tab joint 52c is provided with a joint with the positive electrode tab group 23. The joint is a welded joint formed by welding such as ultrasonic welding, resistance welding, laser welding, etc. with a plurality of positive electrode tabs 22t overlapping each other.

[0046] The negative electrode current collecting part 60 constitutes a conductive path that electrically connects the negative electrode tab group 25 consisting of the multiple negative electrode tabs 24t and the negative electrode terminal 40. As shown in FIG. 2, the negative electrode current collecting part 60 includes a negative electrode first current collecting part 61 and a negative electrode second current collecting part 62. The negative electrode first current collecting part 61 and the negative electrode second current collecting part 62 may be made of the same metal type as the negative electrode current collector 24c, for example, a conductive metal such as copper, a copper alloy, nickel, or stainless steel. The configurations of the negative electrode first current collecting part 61 and the negative electrode second current collecting part 62 may be the same as those of the positive electrode first current collecting part 51 and the positive electrode second current collecting part 52 of the positive electrode current collecting part 50.

[0047] 3 and 4, the negative electrode second current collecting portion 62 has a current collecting plate connection portion 62a electrically connected to the negative electrode first current collecting portion 61, a tab joint portion 62c attached to the negative electrode tab group 25 and electrically connected to the plurality of negative electrode tabs 24t, and a connection portion 62b connecting the current collecting plate connection portion 62a and the tab joint portion 62c. The current collecting plate connection portion 62a has a recess 62d connected to the tab joint portion 62c. The recess 62d is provided with a through hole 62e penetrating in the short side direction X. The negative electrode second current collecting portion 62 is an example of a current collecting member.

[0048] The thermally reactive layer 70 has a function of cooling the electrode body group 20 (electrode bodies 20a, 20b, 20c) when the temperature of the battery 100 reaches a predetermined temperature or higher (for example, 100°C or higher, or even 200°C or higher) in an emergency such as when the temperature of the battery 100 continues to rise. The predetermined temperature varies depending on the type of thermally reactive material described later, and may be a temperature higher than the temperature at which the exhaust valve 17 breaks. The thermally reactive layer 70 shown in FIG. 4 is disposed between the electrode body 20a and the electrode body 20b in the short side direction X. The thermally reactive layer 70 is disposed in the long side direction Y and the vertical direction Z with the center of the electrode body 20b as a reference. The thermally reactive layer 70 may be, for example, bonded to the electrode body 20b and integrated with the electrode body 20b, or may be detachably sandwiched between the electrode body 20a and the electrode body 20b. It is preferable that the thermally reactive layer 70 is disposed between the multiple electrode bodies 20a, 20b, 20c in the short side direction X. The number of the thermally reactive layers 70 is preferably (the number of electrode bodies - 1). The number of the thermally reactive layers 70 is, for example, two (plural).

[0049] The thermally reactive layer 70 is sheet-shaped. The thermally reactive layer 70 has first and second (pair of) main surfaces 72 extending along the long side direction Y and the up-down direction Z, and a side surface 74 extending along the short side direction X. The main surface 72 faces the electrode bodies 20a, 20b, 20c, and at least a part of the main surface 72 is in contact with the electrode bodies 20a, 20b, 20c. The main surface 72 is a surface that is approximately parallel to the flat portion 20f of the electrode bodies 20a, 20b, 20c. The surface shape of the main surface 72 is not particularly limited, and may be flat or ribbed, for example. The side surface 74 is a surface that is approximately perpendicular to the flat portion 20f of the electrode bodies 20a, 20b, 20c.

[0050] In the technology disclosed herein, in the long side direction Y (second direction), the length (average length) L2 of the main surface 72 is 0.7La or more and La or less, when the length of the positive electrode active material layer 22a is La. That is, 0.7La≦L2≦La. In addition, in the up-down direction Z (third direction), the length (average length) L3 of the main surface 72 is 0.5Lb or more and 0.8Lb or less, when the length of the electrode body 20b is Lb. That is, 0.5Lb≦L3≦0.8Lb. In addition, in the short side direction X (first direction), the length (average length, thickness) L1 of the side surface 74 is 0.05Lm or more and 0.5Lm or less, when the total thickness of the positive electrode 22 is Lm. That is, 0.05Lm≦L1≦0.5Lm. By providing the thermal reaction layer 70 of the above size, it is possible to effectively suppress the rise in the battery temperature in an emergency, and thus to improve the safety and reliability of the battery.

[0051] The length L2 of the main surface 72 may be, for example, 0.75 La or more, or even 0.8 La or more, and may be, for example, 0.95 La or less, or even 0.9 La or less. The length L3 of the main surface 72 may be, for example, 0.6 Lb or more, or even 0.65 Lb or more, and may be, for example, 0.75 Lb or less, or even 0.7 Lb or less. The length L1 of the side surface 74 may be, for example, 0.1 Lm or more, or even 0.2 Lm or more, and may be, for example, 0.4 Lm or less, or even 0.3 Lm or less.

[0052] Although not particularly limited, in a high-capacity battery used for in-vehicle applications, the length L2 of the main surface 72 may be approximately 70 mm or more, for example 100 mm or more, or even 140 mm or more, and approximately 500 mm or less, for example 300 mm or less. The length L3 of the main surface 72 may be approximately 5 mm or more, for example 10 mm or more, or even 25 mm or more, and approximately 150 mm or less, for example 100 mm or less. The length L1 of the side surface 74 may be approximately 0.2 mm or more, for example 0.3 mm or more, or even 0.5 mm or more, and approximately 5 mm or less, for example 3 mm or less.

[0053] The thermally reactive layer 70 includes a thermally reactive material that produces at least one of an endothermic effect and an effect of suppressing a radical chain reaction above a predetermined temperature. The thermally reactive material may be a material that undergoes an endothermic reaction above a predetermined temperature. The thermally reactive material may have a cooling effect. The thermally reactive material may be a material that by-produces a gas above a predetermined temperature.

[0054] A suitable example of the thermally reactive material is a hydroxide. The hydroxide undergoes a dehydration reaction at a certain temperature or higher, generating water vapor gas. This reaction is typically an endothermic reaction. The hydroxide can undergo an endothermic effect at a certain temperature or higher. Specific examples of hydroxides include aluminum hydroxide, cobalt hydroxide, calcium hydroxide, zinc hydroxide, zirconium hydroxide, and nickel hydroxide.

[0055] Another suitable example is a potassium compound. Potassium compounds are known as so-called chemical fire extinguishing agents. Potassium compounds undergo a thermal decomposition reaction at a predetermined temperature or higher, and have the effect of suppressing a chain reaction of combustion radicals. Specific examples of potassium compounds include potassium acetate, tripotassium citrate, potassium hydrogen phthalate, dipotassium oxalate, potassium hydrogen carbonate, potassium diphosphate, tripotassium phosphate, potassium propionate, monopotassium citrate, dipotassium citrate, monopotassium trihydrogen ethylenediaminetetraacetate, dipotassium dihydrogen ethylenediaminetetraacetate, tripotassium monohydrogen ethylenediaminetetraacetate, tetrapotassium ethylenediaminetetraacetate, dipotassium phthalate, and potassium hydrogen oxalate.

[0056] When the entire solid content of the thermally reactive layer 70 is taken as 100% by mass, the thermally reactive material may occupy approximately 80% by mass or more, typically 90 to 99.5% by mass, for example 95 to 99% by mass. The thermally reactive layer 70 may contain optional components other than the thermally reactive material, for example, binders and various additive components. As the binder, a vinyl halide resin such as polyvinylidene fluoride (PVdF) may be used. When the entire solid content of the thermally reactive layer 70 is taken as 100% by mass, the binder may occupy approximately 20% by mass or less, typically 0.1 to 10% by mass, for example 1 to 5% by mass.

[0057] The thermal reaction layer 70 is divided into a base 70a and streak portions 70b that differ from the base 70a in size and / or properties (e.g., at least one of the length (thickness) in the short side direction X, the binder content, and the porosity). The base 70a is a portion other than the streak portions 70b. Here, the streak portions 70b are provided continuously from the base 70a and extend in a strip shape along the left-right direction Y. However, in other embodiments, the streak portions may extend along the up-down direction Z. The streak portions 70b may be portions that are thicker than the base 70a (thick portions). The streak portions 70b may be portions that have a higher binder content than the base 70a. The streak portions 70b may be portions that have a higher porosity than the base 70a. It is preferable that the streaks 70b satisfy at least one of the following: (1) a thickness 1.1 to 2 times that of the base 70a; (2) a binder content 1.5 to 2 times that of the base 70a; and (3) a porosity 1.1 to 1.5 times that of the base 70a. This allows a reaction to occur efficiently in the streaks 70b in an emergency, and a rise in the battery temperature can be suppressed to a high level.

[0058] Although not particularly limited, the thickness of the base 70a may be approximately 0.1 to 15 mm, for example, 0.2 to 10 mm. The thickness of the streak portion 70b may be approximately 0.11 to 30 mm, for example, 0.22 to 20 mm. The binder content in the base 70a may be approximately 0.5 to 20 mass % of the total solid content, for example, approximately 1 to 15 mass %. The binder content in the streak portion 70b may be approximately 0.75 to 40 mass % of the total solid content, for example, 1.5 to 30 mass %. The porosity of the base 70a may be approximately 2 to 40%, for example, 5 to 30%. The porosity of the streak portion 70b may be approximately 2.2 to 60%, for example, 5.5 to 45%.

[0059] In FIG. 4, there is one streak portion 70b. However, the number and size of the streak portion 70b are not particularly limited. The number of streak portions 70b may be two or more (multiple streak portions). The number of streak portions 70b is preferably, for example, 1 to 20. The streak portions 70b may be provided so as to be line-symmetrical with respect to the long side direction Y. When the total area of ​​the main surface 72 is taken as 100%, the streak portions 70b may be provided in an area of ​​approximately 50% or less, for example, an area of ​​10 to 50%. The streak portions 70b are preferably provided in an area of ​​20 to 40% of the main surface 72.

[0060] The thermal reaction layer 70 can be produced, for example, by the following method. That is, first, the thermal reaction material and optional components (e.g., binder) as described above are mixed in a predetermined ratio. The mixing method may be a dry method or a wet method. The mixing can be performed using a conventionally known kneading device. Next, the mixture obtained above is formed into a sheet of a predetermined thickness using a rolling roll or the like. The thermal reaction layer 70 can be produced by cutting this sheet-shaped molded body to a predetermined size.

[0061] Battery 100 can be used for various purposes, but can be suitably used, for example, as a power source (driving power source) for a motor mounted on a vehicle such as a passenger car, truck, etc. The type of vehicle is not particularly limited, but examples include a plug-in hybrid vehicle (PHV), a hybrid vehicle (HV), an electric vehicle (EV), etc.

[0062] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to these examples.

[0063] <Test Example 1: Examination of the size of the thermal reaction layer> [Creation of thermal reaction layer] Sheet-like thermal reaction layers (Examples 1 to 6, Comparative Examples 1 to 5) as shown in FIG. 4 were produced. Specifically, aluminum hydroxide as a thermal reaction material and a binder (PVdF) were mixed in a mortar at a ratio of 9:1, and kneaded until they were in the form of a mass to obtain a mixture. Next, this mixture was rolled out with a rolling roll having a flat surface, and molded into a sheet having a length L1 in the short side direction X shown in Table 1 (for example, 2 mm in Example 1). Then, the sheet-like molded body was cut to have the size of the main surface shown in Table 1 (for example, in Example 1, the length L2 in the long side direction Y was 220 mm, and the length L3 in the height direction Z was 60 mm).

[0064] [Battery Construction] Using the above thermal reaction layers (Examples 1 to 6, Comparative Examples 1 to 5), test batteries were constructed. 0.80 Co 0.15 Al 0.05 O2, PVdF as a binder, and acetylene black as a conductive material were weighed out so that the mass ratio was 98:1:1, and mixed in N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode slurry. This positive electrode slurry was applied to both sides of a foil-shaped positive electrode collector mainly composed of Al so that the length (width) La in the long side direction Y was 275 mm, and then dried. This was cut to a predetermined size and rolled with a roll press to prepare a positive electrode sheet having a positive electrode active material layer on both sides of the positive electrode collector. The thickness of the positive electrode active material layer was 150 μm on both sides. The packing density of the positive electrode active material layer was 3.5 g / cm on both sides. 3 It was decided.

[0065] Next, graphite powder as a negative electrode active material, SBR as a binder, and CMC as a dispersant were weighed out so that the mass ratio was 98:1:1, and mixed in water to prepare a negative electrode slurry. This negative electrode slurry was applied to both sides of a copper foil (negative electrode current collector) and dried. This was cut to a predetermined size and rolled with a roll press to prepare a negative electrode sheet having a negative electrode active material layer on both sides of the negative electrode current collector. Next, the positive electrode sheet and the negative electrode sheet prepared above were faced to each other through a polyethylene separator sheet and wound to prepare a wound electrode body as shown in FIG. 5. The length Lb of the electrode body in the height direction Z was 91 mm, and the total thickness Lm of the positive electrode in the short side direction X was 5.9 mm. Then, an aluminum lead was welded to the positive electrode sheet as a current collector, and a nickel lead was welded to the negative electrode sheet as a current collector.

[0066] Next, a non-aqueous electrolyte was prepared by dissolving LiPF6 at a concentration of 1.1 mol / L in a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:3:4, and further adding Li[B(C2O4)2] and LiPO2F2. The electrode body and the non-aqueous electrolyte were then housed in a battery case and sealed to construct a battery.

[0067] [Measurement of maximum heat generation temperature (nail penetration test)] The battery thus prepared was fully charged (4.2V), and then heated to 60°C and subjected to a nail penetration test. Specifically, a round nail (N65, φ3mm) manufactured by Daido Hunt Co., Ltd. was inserted into the battery near the center, and the surface temperature of the battery was measured 1 cm away from the nail and recorded as the maximum heat generation temperature. The results are shown in Table 1. Table 1 also shows the ratio of the maximum heat generation temperature after short circuit to the temperature before short circuit.

[0068] [Table 1]

[0069] When the battery was observed when the nail was inserted, it was confirmed that the constituent material of the electrode body (for example, the positive electrode active material) erupted from the nail insertion hole in all test examples. In addition, as shown in Table 1, in Examples 1 to 6 which have all of the following sizes: the length L2 in the long side direction Y is 0.7La or more and La or less, when the length in the long side direction Y of the positive electrode active material layer is La; the length in the vertical direction Z is 0.5Lb or more and 0.8Lb or less, when the length in the vertical direction Z of the electrode body is Lb; the length (thickness) in the short side direction X is 0.05Lm or more and 0.5Lm or less, when the total thickness in the short side direction X of the positive electrode is Lm; the maximum heat generation temperature was relatively lower than that of Comparative Example 1 to Comparative Example 5 which do not satisfy the above sizes. From this, it was found that by providing a thermal reaction layer of the above size, the rise in the battery temperature in an emergency can be effectively suppressed.

[0070] <Test Example 2: Muscle Examination> In this test example, a thermal reaction layer having a base and a stripe extending from the base in the left-right direction Y was formed, and the usefulness of the stripe was examined. In this test example, potassium propionate was used as the thermal reaction material. The size of the main surface of the thermal reaction layer was 0.75La in the long side direction Y, L2, and 0.65Lb in the up-down direction Z. The length (thickness) of the thermal reaction layer in the short side direction X was 0.2Lm.

[0071] In Examples 7 to 10, when the thermal reaction layer was produced, a rolling roll having a surface shape processed to have a predetermined size and unevenness was used to form streaks of the size and properties shown in Table 2. Other than that, a battery was constructed in the same manner as in the above-mentioned Test Example 1, and the maximum heat generation temperature was recorded. In addition, in Examples 11 to 13, when preparing the thermal reaction layer, a first sheet for forming a base and a second sheet having a larger binder amount than the first sheet were prepared. Next, the second sheet was cut into a rectangular shape (rod shape) of a predetermined size and placed on the surface of the first sheet. Then, the second sheet was rolled with a rolling roll having a flat surface to form a streak part with the size and properties shown in Table 2. Otherwise, a battery was constructed in the same manner as in the above-mentioned Test Example 1, and the maximum heat generation temperature was recorded. In addition, in Examples 14 to 16, when preparing the thermal reaction layer, a pre-sheet having a streak of a predetermined size was prepared using a rolling roll having a surface shape processed to have a predetermined size of projections and recesses. Next, this pre-sheet was rolled with a rolling roll having a flat surface to form streaks of the size and properties shown in Table 2. Otherwise, a battery was constructed in the same manner as in the above-mentioned Test Example 1, and the maximum heat generation temperature was recorded. The results are shown in Table 2.

[0072] [Table 2]

[0073] As shown in Table 2, in Examples 8 to 16 having streaks, the maximum heat generation temperature was relatively lower than that of Example 7 not having streaks. This shows that the inclusion of streaks can effectively suppress the rise in battery temperature in an emergency. In particular, in Examples 8, 9, 11, 12, 14, and 15, in which the streaks satisfy at least one of the following (1) to (3): (1) the thickness is 1.1 to 2 times that of the base; (2) the binder content is 1.5 to 2 times that of the base; and (3) the porosity is 1.1 to 1.5 times that of the base, the rise in battery temperature was more suitably suppressed.

[0074] <Test Example 3: Examination of thermally reactive materials> In this test example, the type of thermal reaction material was examined. In this test example, the size of the main surface of the thermal reaction layer was 0.77La in the long side direction Y, L2, and 0.68Lb in the vertical direction Z. The length (thickness) of the thermal reaction layer in the short side direction X was 0.25Lm. The thickness of the streaks was 1.5 times that of the base, the binder amount of the streaks was 1.8 times that of the base, the porosity of the streaks was 1.8 times that of the base, the number of streaks was 10, and the total area of ​​the streaks was 30%. In Examples 17 to 21, the hydroxides shown in Table 3 were used, and in Examples 22 to 37, the potassium compounds shown in Table 3 were used to prepare the thermal reaction layer. Otherwise, the battery was constructed in the same manner as in the above-mentioned Test Example 2, and the maximum heat generation temperature was recorded. The results are shown in Table 3.

[0075] [Table 3]

[0076] As shown in Table 3, it was found that hydroxides and potassium compounds are useful for lowering the maximum exothermic temperature and can be used as thermal reaction materials.

[0077] <Test Example 4: Examination of Positive Electrode Active Material> In this test example, the properties (circularity) of the positive electrode active material were examined. In this test example, zinc hydroxide was used as the thermal reaction material when the thermal reaction layer was produced. The size of the main surface of the thermal reaction layer was 0.79 La in the long side direction Y, and 0.69 Lb in the vertical direction Z. The length (thickness) of the short side direction X of the thermal reaction layer was 0.27 Lm. The thickness of the streaks was 1.6 times that of the base, the binder amount of the streaks was 1.9 times that of the base, the porosity of the streaks was 1.9 times that of the base, the number of streaks was 9, and the total area of ​​the streaks was 32%. A positive electrode active material with the circularity shown in Table 4 was used, and the packing density was 3.1 g / cm on both sides. 3 A battery was constructed in the same manner as in Test Example 2, except that the positive electrode was prepared as described above, and the maximum heat generation temperature was recorded. The results are shown in Table 4.

[0078] [Table 4]

[0079] As shown in Table 4, when the circularity of the positive electrode active material was 0.45 or more, here 0.45 to 0.99, the maximum heat generation temperature was kept low and the increase in battery temperature was suitably suppressed. The reason for this is thought to be that when the circularity was a predetermined value or more, the positive electrode active material was easily discharged to the outside of the battery case due to the force of the gas generated during the reaction.

[0080] <Test Example 5: Examination of the packing density of the positive electrode active material layer> In this test example, the packing density of the positive electrode active material layer was examined. In this test example, nickel hydroxide was used as the thermal reaction material when the thermal reaction layer was prepared. The size of the main surface of the thermal reaction layer was 0.81 La in the long side direction Y, and 0.71 Lb in the vertical direction Z. The length (thickness) of the short side direction X of the thermal reaction layer was 0.29 Lm. The thickness of the streaks was 1.7 times that of the base, the binder amount of the streaks was 2.1 times that of the base, the porosity of the streaks was 2.1 times that of the base, the number of streaks was 8, and the total area of ​​the streaks was 34%. A battery was constructed in the same manner as in the above-mentioned test example 2, except that a positive electrode was prepared so as to have the packing density shown in Table 5 using a positive electrode active material with a circularity of 0.89, and the maximum heat generation temperature was recorded. The results are shown in Table 5.

[0081] [Table 5]

[0082] As shown in Table 5, the packing density of the positive electrode active material layer is 3 g / cm 3 As described above, when the ratio is 3 to 3.7, the maximum heat generation temperature is kept low and the rise in the battery temperature is appropriately suppressed. The reason for this is considered to be that when the packing density is equal to or higher than a predetermined value, the force of the gas generated during the reaction causes the positive electrode active material layer to form a mass and be easily discharged to the outside of the battery case.

[0083] Although several embodiments of the present invention have been described above, the above embodiments are merely examples. The present invention can be implemented in various other forms. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes of the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. Furthermore, if a technical feature is not described as essential, it can be appropriately deleted. [Explanation of symbols]

[0084] 20 Electrode group 20a, 20b, 20c electrode body 22 Positive electrode 22a Cathode active material layer 24 Negative electrode 52 Positive electrode second current collecting part (current collecting member) 70 Thermal reaction layer 72 Main Surface 74 Side 100 batteries

Claims

1. A plurality of electrode assemblies including a positive electrode having a positive electrode active material layer and a negative electrode having a negative electrode active material layer, the electrode assemblies being arranged side by side in a first direction; a current collecting member attached to an end of the electrode body in a second direction perpendicular to the first direction and electrically connected to the positive electrode or the negative electrode; a thermal reaction layer including a thermal reaction material that produces at least one of an endothermic effect and an effect of suppressing a chain reaction of radicals at a predetermined temperature or higher, and that is disposed between the plurality of electrode bodies in the first direction; When a direction perpendicular to the first direction and the second direction is defined as a third direction, The thermally reactive layer has a main surface extending along the second direction and the third direction and a side surface extending along the first direction, the main surface has a length in the second direction of 0.7La or more and La or less, where La is the length of the positive electrode active material layer in the second direction, and a length in the third direction of 0.5Lb or more and 0.8Lb or less, where Lb is the length of the electrode body in the third direction; The side surface has a length in the first direction of 0.05Lm or more and 0.5Lm or less, when the total thickness of the positive electrode in the first direction is Lm. battery.

2. The thermal reaction layer has a base and a stripe portion that is provided continuously from the base and extends in a strip shape along the second direction or the third direction, The muscle portion includes the following (1) to (3): (1) the length of the side surface in the first direction is 1.1 times or more and 2 times or less than that of the base portion; (2) the base and the side surface contain a binder, and the content of the binder is 1.5 times or more and 2 times or less than that of the base; (3) the porosity is 1.1 times or more and 1.5 times or less than the base; At least one of the following is satisfied:

10. The battery of claim 1.

3. The thermally reactive material includes a hydroxide that undergoes a dehydration reaction at or above the predetermined temperature.

3. The battery of claim 1 or 2.

4. The thermally reactive material includes a potassium compound that undergoes a thermal decomposition reaction at or above the predetermined temperature.

4. The battery of claim 1.

5. The positive electrode active material layer contains a particulate positive electrode active material, The circularity of the positive electrode active material is 0.45 or more.

5. The battery of claim 1.

6. The packing density of the positive electrode active material layer is 3 g / cm 3 That's all.

6. The battery of claim 1 .

Citation Information

Patent Citations

  • High-density electrode and battery using its electrode

    JP2005340152A

  • Positive electrode active material for lithium secondary battery, its manufacturing method, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2008186753A

  • Secondary battery

    JP2010287489A

  • Secondary battery

    JP2013020930A

  • Lithium ion secondary battery

    JP2013065467A