Slurry composition, electrode, electrode manufacturing method, secondary battery, battery pack and vehicle
Optimizing the particle size distribution of niobium titanium oxide particles in slurry compositions for electrodes addresses dispersion issues, resulting in electrodes with reduced resistance and enhanced performance in secondary batteries.
Patent Information
- Application Number
- JP2021076434
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-28
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2041-04-28
AI Technical Summary
The dispersion strength of slurry compositions containing niobium titanium oxide particles in electrodes is insufficient, leading to increased resistance and decreased capacity due to aggregation of raw material components, which can cause damage such as chipping and reduction of crystallinity, affecting the performance of secondary batteries.
A slurry composition is formulated with niobium titanium-containing composite oxide particles, a conductive agent, and a resin material in a specific particle size distribution, optimized to have a peak position of 0.8 μm to 3 μm and cumulative frequency ratios of 20% to 35% for particles up to 1 μm, ensuring appropriate dispersion and reducing material damage.
The optimized slurry composition results in electrodes with lower electronic and ionic resistance, extending the lifespan and improving input/output performance of secondary batteries.
Smart Images

Figure 0007562473000007 
Figure 0007562473000008 
Figure 0007562473000009
Abstract
Description
[Technical field]
[0001] The embodiments relate to a slurry composition, an electrode, a method for producing an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] The use of an electrode containing niobium titanium oxide as a negative electrode active material in a secondary battery has been considered. This electrode is produced, for example, by applying a slurry containing niobium titanium oxide particles, a conductive agent, and a binder to a current collector, drying it, and performing a pressing process. If the dispersion strength during the preparation of the slurry is insufficient, the raw material components will aggregate, causing an increase in resistance or a decrease in capacity. If the dispersion strength during the preparation of the slurry is increased in order to avoid this, it will cause chipping of niobium titanium oxide particles, a decrease in the crystallinity of the particle surface, and damage to the conductive agent such as breakage of carbon black. As a result, the resistance of the electrodes increases and the capacity of the battery decreases.
[0003] There is a demand for optimizing the dispersion state of a slurry containing niobium titanium oxide particles. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-48671 A [Patent Document 2] JP 2019-40890 A Summary of the Invention [Problem to be solved by the invention]
[0005] The embodiments aim to provide a slurry composition capable of realizing an electrode having a long life and excellent input / output performance, an electrode having a long life and excellent input / output performance and a manufacturing method thereof, a secondary battery having a long life and excellent input / output performance, a battery pack including the secondary battery, and a vehicle including the battery pack. [Means for solving the problem]
[0006] According to an embodiment, a slurry composition is provided that includes an active material containing niobium titanium-containing composite oxide particles, a conductive agent, a resin material, and a solvent containing water. The volume-based cumulative frequency distribution of particle diameters based on the particle size distribution of the slurry composition measured by a laser diffraction scattering method has a peak position in the range of 0.8 μm to 3 μm. In addition, the ratio of the cumulative frequency from the smallest particle diameter to a particle diameter of 1 μm is in the range of 20% to 35%. In the cumulative frequency distribution, the ratio of the cumulative frequency from the smallest particle size to 2 μm particle size is in the range of 50% to 70%.In the cumulative frequency distribution, the ratio of the cumulative frequency from the smallest particle size to 5 μm particle size is in the range of 80% to 95%.
[0007] According to another embodiment, a method for producing a slurry-type current collector comprising the steps of: applying the slurry composition to a current collector; a step of drying the slurry composition applied to the current collector to form an active material-containing layer on the current collector; a step of pressing the active material-containing layer; A method for manufacturing an electrode is provided, comprising:
[0008] According to another embodiment, there is provided an electrode comprising an active material containing niobium titanium-containing composite oxide particles, an active material-containing layer containing a conductive agent and a resin material, and a current collector on which the active material-containing layer is formed. The volume-based cumulative frequency distribution of particle diameters based on the particle size distribution of the active material-containing layer measured by a laser diffraction scattering method has a peak position in the range of 0.8 μm to 3 μm, and the ratio of the cumulative frequency from the smallest particle diameter to a particle diameter of 1 μm is in the range of 20% to 35%. In the cumulative frequency distribution, the ratio of the cumulative frequency from the smallest particle size to 2 μm particle size is in the range of 50% to 70%.In the cumulative frequency distribution, the ratio of the cumulative frequency from the smallest particle size to 5 μm particle size is in the range of 80% to 95%.
[0009] According to another embodiment, a positive electrode and As a negative electrode, the electrode of the embodiment, Non-aqueous electrolyte A secondary battery is provided, comprising:
[0010] According to another embodiment, a battery pack including the secondary battery of the embodiment is provided.
[0011] According to another embodiment, a vehicle including a battery pack of the embodiment is provided. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a graph showing the cumulative frequency distribution of particle diameters on a volume basis based on the particle size distribution measured by a laser diffraction scattering method for the slurry compositions of the Examples and Comparative Examples. [Diagram 2] FIG. 2 is a partially cutaway cross-sectional view of a secondary battery according to the embodiment. [Diagram 3] FIG. 3 is a side view of the battery of FIG. 2 . [Figure 4] 2 is a cross-sectional view of the secondary battery according to the embodiment, taken in a direction perpendicular to the terminal extending direction. [Diagram 5] FIG. 5 is an enlarged cross-sectional view of part A in FIG. 4 . [Figure 6] FIG. 2 is an exploded perspective view of the battery pack according to the embodiment. [Figure 7] FIG. 7 is a block diagram showing an electrical circuit of the battery pack of FIG. 6. [Figure 8] 1 is a schematic diagram showing an example of a vehicle equipped with a secondary battery according to an embodiment; [Figure 9] FIG. 13 is a diagram illustrating another example of a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (First embodiment) According to the first embodiment, a slurry composition is provided that includes an active material containing niobium titanium-containing composite oxide particles, a conductive agent, a resin material, and a solvent containing water. The cumulative frequency distribution of the particle size based on the volumetric basis of the particle size distribution of the slurry composition by the laser diffraction scattering method has a peak position in the range of 0.8 μm to 3 μm, and the ratio of the cumulative frequency from the smallest particle size to the particle size of 1 μm is in the range of 20% to 35%. The particle size distribution of the above slurry composition is a unimodal distribution with a peak position close to fine particles. The above particle size distribution reflects at least the particle size of the niobium titanium-containing composite oxide particles and the conductive agent, and more specifically, reflects the particle size of the primary particles or secondary particles of the niobium titanium-containing composite oxide, the conductive agent, and the aggregates containing the niobium titanium-containing composite oxide and the conductive agent.
[0014] The reason why the peak position of the cumulative frequency distribution is set to the range of 0.8 μm or more and 3 μm or less is as follows. When the peak position exceeds 3 μm, aggregation of the niobium titanium-containing composite oxide particles or the conductive agent occurs, and the dispersibility of the slurry composition is low. Therefore, the conductive path between the niobium titanium-containing composite oxide particles in the active material-containing layer of the electrode is insufficient, and the resin material such as the binder is unevenly distributed, so that the resistance of the electrode increases and the life performance of the secondary battery decreases. When the peak position is less than 0.8 μm, damage to each component such as cracking and chipping of the niobium titanium-containing composite oxide particles and breaking and breaking of the conductive agent occurs. Therefore, the resistance of the electrode increases and the life performance of the secondary battery decreases. A more preferable range of the peak position is 0.9 μm or more and 2 μm or less.
[0015] The ratio of the cumulative frequency from the smallest particle size to 1 μm in the cumulative frequency distribution is set to a range of 20% to 35% for the following reasons: When the ratio exceeds 35%, the slurry composition contains many fine particles, resulting in over-dispersion and damage to each component. On the other hand, when the ratio is less than 20%, the slurry composition contains few fine particles, resulting in insufficient dispersibility of the slurry composition, resulting in a large amount of aggregation of the niobium titanium-containing composite oxide particles or the conductive agent.
[0016] By satisfying the cumulative frequency distribution, the components are appropriately dispersed in the slurry composition, and the niobium titanium-containing composite oxide particles are less likely to chip or lose crystallinity, and damage to materials such as the breakage of the conductive agent is reduced. Therefore, the slurry composition makes it possible to provide an electrode with low electronic resistance and ionic conduction resistance, and a secondary battery that has both a long life and high input / output performance.
[0017] In the cumulative frequency distribution of the slurry composition, it is desirable that the ratio of the cumulative frequency of the smallest particle size to a particle size of 2 μm is in the range of 50% to 70%. This makes it possible to optimize the ratio of fine particles in the slurry composition, reduce damage to the raw material components, and further suppress the aggregation of the niobium titanium-containing composite oxide particles or the conductive agent, thereby further improving the life performance and input / output performance of the electrode and secondary battery.
[0018] In addition, it is preferable that the ratio of the cumulative frequency of the particles from the smallest particle size to the particle size of 5 μm is in the range of 80% to 95% in the cumulative frequency distribution of the slurry composition. This makes it possible to optimize the ratio of fine particles in the slurry composition, reduce damage to the raw material components, and further suppress the aggregation of the niobium titanium-containing composite oxide particles or the conductive agent, thereby further improving the life performance and input / output performance of the electrode and secondary battery.
[0019] The viscosity of the slurry composition measured at 25°C and 100 rpm using a Brookfield viscometer is preferably in the range of 1.5 Pa·s to 5 Pa·s. If the viscosity is low, there is a risk of particle settling in the slurry composition. In addition, the drying process in the electrode manufacturing process is prone to uneven drying, which leads to uneven distribution of resin materials such as binders in the active material-containing layer. This can lead to an increase in the resistance of the battery and a decrease in its lifespan. On the other hand, if the viscosity is high, it may be difficult to apply the slurry composition to the current collector, or the piping of the application device may become clogged.
[0020] Each component contained in the slurry composition will be described.
[0021] The morphology of the niobium titanium-containing composite oxide particles is not limited, and may be a single primary particle, a secondary particle formed by aggregation of primary particles, or a mixture of primary particles and secondary particles.
[0022] The average particle size of the niobium titanium-containing composite oxide particles may be in the range of 0.5 μm or more and 3 μm or less.
[0023] The crystal structure of the niobium titanium-containing composite oxide particles can be, for example, orthorhombic or monoclinic.
[0024] As an example of an orthorhombic titanium-containing composite oxide, Li 2+a M(I) 2-b Ti 6-c M(II) d O 14+σ Here, M(I) is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M(II) is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0025] As an example of monoclinic niobium titanium composite oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li x Examples include Nb2TiO7 (0≦x≦5).
[0026] Another example of monoclinic niobium titanium composite oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δHere, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0027] At least a portion of the surface of the niobium titanium-containing composite oxide particles may be coated with a conductive material, examples of which include a carbon coating and an electronically conductive inorganic material coating.
[0028] The niobium titanium-containing composite oxide particles function as an active material. The slurry composition may contain an active material other than the niobium titanium-containing composite oxide. Examples of other active materials include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, and hollandite type titanium composite oxide. The content of the niobium titanium-containing composite oxide particles in the active material can be 50% by mass or more and 100% by mass or less.
[0029] The content of the active material in the slurry composition can be in the range of 68% by mass to 96% by mass.
[0030] The conductive agent is blended to improve the current collecting performance and to suppress the contact resistance between the active material such as niobium titanium composite oxide and the current collector. Examples of the conductive agent include fibrous carbon materials and granular carbon materials. Examples of the fibrous carbon materials include vapor grown carbon fiber (VGCF) and carbon nanotubes. On the other hand, examples of the granular carbon materials include carbon black such as acetylene black, and thin or scaly graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. Alternatively, instead of using the conductive agent, the surface of the active material particles may be coated with a carbon coat or an electronically conductive inorganic material coat.
[0031] The content of the conductive agent in the slurry composition can be in the range of 1 part by mass to 20 parts by mass relative to 100 parts by mass of the active material.
[0032] The resin material may be a binder, a viscosity modifier, a dispersant, or a combination of two or more of these.
[0033] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, and imide compounds. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0034] The viscosity modifier is for imparting viscosity to the slurry composition. Examples of the viscosity modifier include carboxymethyl cellulose (CMC) and salts of CMC. One of these may be used as the viscosity modifier, or two or more of them may be used in combination as the viscosity modifier.
[0035] The dispersant is for improving the dispersibility of the conductive agent. Examples of the dispersant include polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyvinyl chloride (PVC), dodecylbenzenesulfonic acid sodium salt, dodecylsulfonic acid sodium salt, cellulose nanofiber, etc. One of these may be used as the dispersant, or two or more may be used in combination as the dispersant.
[0036] The content of the resin material in the slurry composition can be in the range of 1 part by mass to 10 parts by mass with respect to 100 parts by mass of the active material.
[0037] As the aqueous solvent, for example, water can be used.
[0038] The slurry composition may further contain lithium ion conductive inorganic solid particles. Examples of the lithium ion conductive inorganic solid electrolyte include a lithium ion conductive oxide-based solid electrolyte and a lithium ion conductive sulfide-based solid electrolyte. The lithium ion conductive oxide-based solid electrolyte may be a lithium phosphate solid electrolyte having a NASICON structure. Examples of the lithium phosphate solid electrolyte having a NASICON structure include a lithium phosphate solid electrolyte having a general formula Li 1+x M2(P 1-y M' y O4)3 (M and M' are one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, Si and Al, x is 0≦x≦0.5, y is 0≦y≦0.2), Li 1+x+y Al x (Ti,Ge) 2-x S y P 3-y O 12Examples include solid electrolytes represented by (0 < x ≤ 2, 0 ≤ y < 3). As NASICON-type lithium phosphate solid electrolytes, there are LATP (Li 1+x Al x Ti 2-x (PO4)3 (where 0 ≤ x ≤ 0.5)), Li 1+x Al x Zr 2-x (PO4)3 (where 0 ≤ x ≤ 0.5), and Li 1+x Al x Ge 2-x (PO4)3 (where 0 ≤ x ≤ 0.5), etc. LATP may be substituted with one or more elements selected from the group consisting of Ge, Sr, Zr, Sn, and Si, and a part of it may be amorphous.
[0039] As lithium ion conductive oxide-based solid electrolytes, amorphous LIPON (Li 2.9 PO 3.3 N 0.46 ), or garnet-type LLZ (Li7La3Zr2O 12 ) may be used.
[0040] The content of lithium ion conductive inorganic solid particles in the slurry composition can be in the range of 0 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the active material.
[0041] The slurry composition is prepared, for example, by stirring the active material, the conductive agent, and the resin material together with the solvent. The desired cumulative frequency distribution can be obtained, for example, by adjusting the order of adding the raw materials, the solid content ratio of the composition, the stirring speed, the stirring time, and the like. The niobium titanium-containing composite oxide particles and the lithium ion conductive inorganic solid particles have low electrical conductivity. Therefore, when a fibrous carbon material is used as the conductive agent, the surface of the niobium titanium-containing composite oxide particles can be covered with the fibrous carbon material by adding the niobium titanium-containing composite oxide particles and the viscosity modifier to the aqueous solvent in which the fibrous carbon material is dispersed, and stirring these together in the first stirring. Therefore, it becomes possible to use the fibrous carbon material in the conductive path between the niobium titanium-containing composite oxide particles. When the lithium ion conductive inorganic solid particles are used, it becomes possible to use the fibrous carbon material in the conductive path between the niobium titanium-containing composite oxide particles, between the lithium ion conductive inorganic solid particles, and between these particles, by adding the niobium titanium-containing composite oxide particles, the lithium ion conductive inorganic solid particles, and the viscosity modifier to the aqueous solvent in which the fibrous carbon material is dispersed, and stirring these together in the second stirring. After the first or second stirring, a third stirring may be performed in which a binder and, if necessary, a granular carbon material are added to the resulting mixture and the mixture is further stirred. Note that kneading may be performed in the stirring step.
[0042] Furthermore, the method is not limited to adding the conductive agent in two stages as described above. For example, the active material, conductive agent, and resin material may be kneaded in the presence of a solvent and with a high solids ratio, and then the slurry composition may be prepared by adding more solvent to reduce the solids ratio and stirring.
[0043] By stirring or kneading the slurry composition in a state where the solid content ratio of the slurry composition is high, it is possible to efficiently disperse aggregates of the raw material, and by stirring or kneading the slurry composition in a state where the solid content ratio of the slurry composition is low, damage to the raw material can be reduced.
[0044] To simultaneously prevent the aggregation of the raw materials and prevent damage to the raw materials, it is necessary to consider not only the solid content ratio but also the rotation speed and mixing time of the mixing device (e.g., a planetary centrifugal mixer) that mixes the slurry composition.
[0045] The desired cumulative frequency distribution can be obtained by comprehensively taking into consideration the blending ratio of the raw materials, the order in which the raw materials are added, the solid content ratio, the rotation speed of the mixer, the mixing time, etc. The particle size distribution of the slurry composition is measured by a laser diffraction scattering method. Examples of particle size distribution measuring devices include MicrotracMT3000 and MicrotracMT3000II manufactured by Microtrac. The slurry is charged into the device until it reaches a measurable concentration, and then ultrasonic waves are irradiated at 30 W for 60 seconds, after which the measurement is performed. By irradiating the ultrasonic waves, the slurry is dispersed in the water solvent, and the agglomeration of the conductive agent particles and the active material particles can be dissolved. The viscosity of the slurry composition using a Brookfield viscometer is measured by the following method. An example of a Brookfield viscometer is the TVB-10 viscometer manufactured by Toki Sangyo Co., Ltd. The slurry composition is placed in a container of specified dimensions, and the H6 rotor is placed so as to be immersed to a specified depth. With the temperature of the slurry composition kept at 25°C and the viscometer temperature calibrated by an appropriate method, the rotor speed is gradually increased from 5 rpm to 100 rpm to measure the viscosity.
[0046] The slurry composition of the first embodiment described above contains niobium titanium-containing composite oxide particles, a conductive agent, a resin material, and water, and the cumulative frequency distribution of particle size on a volume basis based on the particle size distribution of the slurry composition by a laser diffraction scattering method has a peak position in the range of 0.8 μm to 3 μm, and the ratio of the cumulative frequency from the smallest particle size to a particle size of 1 μm is in the range of 20% to 35%, so that it is possible to realize an electrode and a secondary battery that have both a long life and high input / output performance. Second embodiment The electrode of the second embodiment may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The surface of the current collector on which the active material-containing layer is formed is preferably a surface (e.g., a main surface) that intersects with the thickness direction of the current collector. The active material-containing layer includes an active material containing niobium titanium-containing composite oxide particles, a conductive agent, and a resin material. The volume-based cumulative frequency distribution of particle size based on the particle size distribution by the laser diffraction scattering method of the active material-containing layer has a peak position in the range of 0.8 μm to 3 μm, and the ratio of the cumulative frequency from the smallest particle size to the particle size of 1 μm is in the range of 20% to 35%. The particle size distribution of the active material-containing layer is a unimodal distribution with a peak position closer to fine particles.
[0047] The reason why the peak position of the cumulative frequency distribution is set to the range of 0.8 μm or more and 3 μm or less is as follows. When the peak position exceeds 3 μm, aggregation of niobium titanium-containing composite oxide particles or conductive agent occurs in the active material-containing layer. Therefore, the conductive path between niobium titanium-containing composite oxide particles in the active material-containing layer of the electrode is insufficient, and resin materials such as binders are unevenly distributed, so that the resistance of the electrode increases and the life performance of the secondary battery decreases. When the peak position is less than 0.8 μm, damage to each component such as cracking and chipping of niobium titanium-containing composite oxide particles and separation and breakage of the conductive agent occurs. Therefore, the resistance of the electrode increases and the life performance of the secondary battery decreases. A more preferable range of the peak position is 0.9 μm or more and 2 μm or less.
[0048] The ratio of the cumulative frequency from the smallest particle size to 1 μm in the cumulative frequency distribution is set to a range of 20% to 35% for the following reasons: When the ratio exceeds 35%, there are many fine particles in the active material-containing layer, which means that there is excessive dispersion, causing damage to each component. On the other hand, when the ratio is less than 20%, there are few fine particles in the active material-containing layer, and there is a lot of aggregation of the niobium titanium-containing composite oxide particles or the conductive agent in the active material-containing layer.
[0049] By the active material-containing layer satisfying the above-mentioned cumulative frequency distribution, each component is appropriately dispersed in the active material-containing layer, and chipping and deterioration of crystallinity of the niobium titanium-containing composite oxide particles are reduced, and damage to materials such as breakage of the conductive agent is reduced. Therefore, the electronic resistance and ionic conduction resistance of the electrode can be reduced, and it is possible to provide a secondary battery that achieves both a long life and high input / output performance.
[0050] In the cumulative frequency distribution of the active material-containing layer, it is desirable that the ratio of the cumulative frequency from the smallest particle size to a particle size of 2 μm is in the range of 50% to 70%. This makes it possible to optimize the ratio of fine particles in the active material-containing layer, reduce damage to the raw material components, and further suppress the aggregation of the niobium titanium-containing composite oxide particles or the conductive agent, thereby further improving the life performance and input / output performance of the electrode and secondary battery.
[0051] In addition, in the cumulative frequency distribution of the active material-containing layer, it is desirable that the ratio of the cumulative frequency from the smallest particle size to a particle size of 5 μm is in the range of 80% to 95%. This makes it possible to optimize the ratio of fine particles in the active material-containing layer, reduce damage to the raw material components, and further suppress the aggregation of the niobium titanium-containing composite oxide particles or the conductive agent, thereby further improving the life performance and input / output performance of the electrode and secondary battery.
[0052] The components contained in the active material-containing layer may be similar to those described in the first embodiment.
[0053] The content of the active material in the active material-containing layer can be in the range of 68% by mass or more and 96% by mass or less. The content of the conductive agent in the active material-containing layer can be in the range of 1 part by mass to 20 parts by mass per 100 parts by mass of the active material.
[0054] The content of the resin material in the active material-containing layer can be in the range of 1 part by mass to 10 parts by mass with respect to 100 parts by mass of the active material.
[0055] The content of the lithium ion conductive inorganic solid particles in the active material-containing layer can be in the range of 0 to 20 parts by mass per 100 parts by mass of the active material.
[0056] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted into and extracted from the active material. One example of the current collector is copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0057] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.
[0058] The electrode can be produced, for example, by the following method. The slurry composition of the first embodiment is applied to one or both sides of a current collector. The coater can be, for example, a slit coater. The applied slurry is then dried to obtain a laminate of the active material-containing layer and the current collector. Then, the laminate is pressed. In this manner, an electrode is produced. In order to obtain the electrode in a predetermined shape or size, cutting may be performed as necessary. Cutting can be performed, for example, after drying, after pressing, or in both steps after drying and pressing.
[0059] The particle size distribution of the active material-containing layer is measured by a laser diffraction scattering method. Examples of particle size distribution measuring devices include MicrotracMT3000 and MicrotracMT3000II manufactured by Microtrac. The active material-containing layer scraped off from the current collector using a spatula or the like is put into the device to a measurable concentration, and then ultrasonic waves are irradiated at 30 W for 60 seconds, after which the measurement is performed. By applying ultrasonic irradiation, the active material-containing layer is dispersed in the water solvent, and the aggregation of the conductive agent particles and the active material particles can be dissolved.
[0060] The method for removing the electrodes from the battery is described below. The battery is disassembled in a glove box filled with argon to remove the electrode group. The electrode group may be washed and vacuum dried to remove the non-aqueous electrolyte in the electrode group. The electrodes are removed from the electrode group, and the above particle size distribution measurement is carried out.
[0061] According to the electrode of the second embodiment described above, the volume-based cumulative frequency distribution of particle diameters based on the particle size distribution measured by a laser diffraction scattering method of the active material-containing layer containing niobium titanium-containing composite oxide particles, a conductive agent, and a resin material has a peak position in the range of 0.8 μm or more and 3 μm or less, and the ratio of the cumulative frequency from the smallest particle diameter to the particle diameter of 1 μm is in the range of 20% or more and 35% or less, so that it is possible to achieve both a long life and high input / output performance. (Third embodiment) According to a third embodiment, a secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte is provided. The electrode according to the second embodiment can be used for at least one of the positive electrode and the negative electrode.
[0062] Hereinafter, an example of a secondary battery using the electrode of the second embodiment as the negative electrode will be described. The secondary battery of the embodiment includes a positive electrode, a negative electrode, and a non-aqueous electrolyte, and may also include a separator and an exterior member. Each component will be described below. 1) Positive electrode The positive electrode may include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer may be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer may include a positive electrode active material, and optionally a conductive agent and a binder.
[0063] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain one type of compound alone as the positive electrode active material, or may contain two or more types of compounds in combination. Examples of oxides and sulfides include compounds that can insert and remove Li or Li ions.
[0064] Examples of such compounds include, for example, manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≦ 1, Li x Fe 1-y Mn y PO4; 0 < x ≦ 1, 0 < y ≦ 1, Li x CoPO4; 0 < x ≦ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≦ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.
[0065] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), a lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), a lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and a lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0066] The lithium nickel cobalt manganese composite oxide and the lithium manganese composite oxide having a spinel structure contribute to the improvement of the output performance.
[0067] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. The positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. The positive electrode active material with a primary particle size of 1 μm or less can allow the solid-state diffusion of lithium ions to proceed smoothly.
[0068] The specific surface area of the positive electrode active material is preferably 0.1 m 2 / g or more and 10 m 2 / g or less. The positive electrode active material having a specific surface area of 0.1 m 2 / g or more can sufficiently secure the Li ion storage and release sites. The positive electrode active material having a specific surface area of 10 m 2 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.
[0069] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethylcellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0070] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0071] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in proportions of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0072] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0073] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0074] By setting the amount of the conductive agent to 3% by mass or more, the above-mentioned effects can be achieved. Also, by setting the amount of the conductive agent to 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0075] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.
[0076] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.
[0077] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0078] For example, the positive electrode is prepared by suspending a positive electrode active material, a conductive agent, and a binder in a solvent to prepare a slurry. The slurry is then applied to one or both sides of a current collector. The applied slurry is then dried to obtain a laminate of an active material-containing layer and a current collector. Then, the laminate is pressed. In this manner, the positive electrode is produced. Alternatively, the positive electrode may be produced by the following method. First, the active material, the conductive agent, and the binder are mixed to obtain a mixture. Then, the mixture is formed into pellets. Then, the pellets are placed on the current collector to obtain a positive electrode. 2) Nonaqueous electrolyte The non-aqueous electrolyte may be, for example, a liquid non-aqueous electrolyte or a gel non-aqueous electrolyte. The liquid non-aqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.
[0079] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.
[0080] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0081] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.
[0082] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.
[0083] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0084] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.
[0085] The inorganic solid electrolyte is a solid material that has Li-ion conductivity. 3) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0086] 4) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0087] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0088] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0089] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0090] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.
[0091] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0092] An example of a secondary battery according to an embodiment will be described with reference to FIGS.
[0093] 2 and 3 show an example of a secondary battery using a metal container.
[0094] The electrode group 1 is housed in a rectangular cylindrical metal container 2. The electrode group 1 is formed, for example, by winding a positive electrode 3 and a negative electrode 4 in a flat spiral shape around an axis parallel to the short side direction with a separator 5 interposed between them. As shown in FIG. 3, a strip-shaped positive electrode lead 6 is electrically connected to each of a plurality of points on the end of the positive electrode 3 located on the end face of the electrode group 1 intersecting with the stacking direction of the electrodes. In addition, a strip-shaped negative electrode lead 7 is electrically connected to each of a plurality of points on the end of the negative electrode 4 located on this end face. The plurality of positive electrode leads 6 are electrically connected to a positive electrode current collector tab 8 in a bundled state. The positive electrode lead 6 and the positive electrode current collector tab 8 constitute a positive electrode terminal. In addition, the negative electrode lead 7 is connected to a negative electrode current collector tab 9 in a bundled state. The negative electrode lead 7 and the negative electrode current collector tab 9 constitute a negative electrode terminal. A metal sealing plate 10 is fixed to the opening of the metal container 2 by welding or the like. The positive electrode current collecting tab 8 and the negative electrode current collecting tab 9 are each pulled out to the outside through an extraction hole provided in a sealing plate 10. The inner circumferential surface of each extraction hole in the sealing plate 10 is covered with an insulating member 11 to prevent a short circuit due to contact with the positive electrode current collecting tab 8 and the negative electrode current collecting tab 9.
[0095] 4 and 5 show an example of a secondary battery using an exterior member made of a laminate film.
[0096] As shown in FIG. 4 and FIG. 5, the flat wound electrode group 1 is housed in a bag-shaped exterior member 12 made of a laminate film in which a metal layer is interposed between two resin films. The flat wound electrode group 1 is formed by spirally winding a laminate in which a negative electrode 4, a separator 15, a positive electrode 3, and a separator 15 are laminated in this order from the outside around an axis parallel to the short side direction, and press-molding the laminate. The outermost negative electrode 4 has a configuration in which a negative electrode layer (negative electrode active material-containing layer) 4b containing a negative electrode active material is formed on one side of the inner surface side of a negative electrode current collector 4a as shown in FIG. 5, and the other negative electrodes 4 are configured by forming a negative electrode layer 4b on both sides of the negative electrode current collector 4a. The positive electrode 3 is configured by forming a positive electrode layer (positive electrode active material-containing layer) 3b on both sides of a positive electrode current collector 3a.
[0097] Near the outer peripheral end of the wound electrode group 1, the negative electrode terminal 13 is connected to the negative electrode current collector 4a of the outermost negative electrode 4, and the positive electrode terminal 14 is connected to the positive electrode current collector 3a of the inner positive electrode 3. These negative electrode terminal 13 and positive electrode terminal 14 extend outward from an opening of the bag-shaped exterior member 12. The opening of the bag-shaped exterior member 12 is heat-sealed to seal the wound electrode group 1. When heat-sealing, the negative electrode terminal 13 and positive electrode terminal 14 are sandwiched by the bag-shaped exterior member 12 at this opening.
[0098] The secondary battery of the third embodiment described above includes the electrode of the second embodiment as the negative electrode, and therefore can improve the life performance and input / output performance. (Fourth embodiment) The battery pack according to the fourth embodiment may include one or more secondary batteries (single cells) according to the third embodiment. A plurality of secondary batteries may be electrically connected in series, in parallel, or in a combination of series and parallel to form a battery pack. The battery pack according to the embodiment may include a plurality of battery packs.
[0099] The battery pack according to the embodiment may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0100] The battery pack according to the embodiment may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and inputting current to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When charging the battery pack, a charging current (including regenerative energy of the power of a vehicle such as an automobile) is supplied to the battery pack through the external terminal for current flow.
[0101] Figures 6 and 7 show an example of a battery pack 50. This battery pack 50 includes a plurality of flat batteries having the structure shown in Figure 6. Figure 6 is an exploded perspective view of the battery pack 50, and Figure 7 is a block diagram showing the electrical circuit of the battery pack 50 of Figure 6.
[0102] A plurality of unit cells 51 are stacked so that the negative electrode terminals 13 and positive electrode terminals 14 extending outward are aligned in the same direction, and are fastened together with adhesive tape 52 to form a battery pack 53. These unit cells 51 are electrically connected in series as shown in FIG.
[0103] The printed wiring board 54 is disposed facing the side surface of the battery cell 51 from which the negative electrode terminal 13 and the positive electrode terminal 14 extend. A thermistor 55, a protective circuit 56, and an external terminal 57 for supplying electricity to an external device as an external terminal for supplying electricity are mounted on the printed wiring board 54 as shown in Fig. 7. An insulating plate (not shown) is attached to the surface of the printed wiring board 54 facing the assembled battery 53 to prevent unnecessary connection with the wiring of the assembled battery 53.
[0104] The positive electrode lead 58 is connected to the positive electrode terminal 14 located in the bottom layer of the battery pack 53, and its tip is inserted into and electrically connected to a positive electrode connector 59 of the printed wiring board 54. The negative electrode lead 60 is connected to the negative electrode terminal 13 located in the top layer of the battery pack 53, and its tip is inserted into and electrically connected to a negative electrode connector 61 of the printed wiring board 54. These connectors 59, 61 are connected to the protection circuit 56 through wires 62, 63 formed on the printed wiring board 54.
[0105] The thermistor 55 detects the temperature of the cell 51, and the detection signal is sent to the protection circuit 56. The protection circuit 56 can cut off the positive side wiring 64a and the negative side wiring 64b between the protection circuit 56 and a terminal 57 for supplying electricity to an external device as an external terminal for supplying electricity under a predetermined condition. The predetermined condition is, for example, when the temperature detected by the thermistor 55 becomes equal to or higher than a predetermined temperature. The predetermined condition is also when overcharging, overdischarging, overcurrent, etc. of the cell 51 is detected. This detection of overcharging, etc. is performed for each cell 51 or for all the cells 51. When detecting each cell 51, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 51. In the case of FIG. 6 and FIG. 7, wiring 65 for voltage detection is connected to each cell 51, and a detection signal is transmitted to the protection circuit 56 through these wirings 65.
[0106] Protective sheets 66 made of rubber or resin are disposed on the three side surfaces of the battery pack 53 excluding the side surfaces from which the positive electrode terminal 14 and the negative electrode terminal 13 protrude.
[0107] The battery pack 53 is stored in a storage container 67 together with the protective sheets 66 and the printed wiring board 54. That is, the protective sheets 66 are arranged on both inner surfaces in the long side direction and on the inner surface in the short side direction of the storage container 67, and the printed wiring board 54 is arranged on the inner surface on the opposite side in the short side direction. The battery pack 53 is located in a space surrounded by the protective sheets 66 and the printed wiring board 54. A lid 68 is attached to the top surface of the storage container 67.
[0108] Note that heat shrink tape may be used to secure the battery pack 53, instead of the adhesive tape 52. In this case, protective sheets are placed on both sides of the battery pack, the heat shrink tape is wrapped around it, and then the heat shrink tape is thermally shrunk to bind the battery pack.
[0109] 6 and 7 show a configuration in which the cells 51 are connected in series, but they may be connected in parallel to increase the battery capacity. Alternatively, a combination of series and parallel connections may be used. The assembled battery pack may be further connected in series or parallel.
[0110] 6 and 7 includes one battery pack, the battery pack according to the embodiment may include multiple battery packs. The multiple battery packs are electrically connected in series, in parallel, or in a combination of series and parallel connections.
[0111] The battery pack may be modified as appropriate depending on the application. The battery pack according to the embodiment is suitable for use in applications that require excellent cycle performance when a large current is drawn. Specifically, the battery pack is used as a power source for digital cameras, or as a vehicle battery for, for example, two- to four-wheeled hybrid electric vehicles, two- to four-wheeled electric vehicles, power-assisted bicycles, or railroad vehicles (e.g., trains), or as a stationary battery. In particular, the battery pack is suitable for use as an on-board battery mounted on a vehicle.
[0112] The battery pack of the fourth embodiment described above includes the secondary battery of the embodiment, and therefore can achieve excellent life performance and input / output performance. Fifth embodiment A vehicle of the fifth embodiment includes one or more secondary batteries of the embodiment, or includes a battery pack of the embodiment.
[0113] In a vehicle such as an automobile equipped with the battery pack according to the fifth embodiment, the battery pack may, for example, recover regenerative energy of the vehicle's motive power. The vehicle may also include a mechanism for converting the kinetic energy of the vehicle into regenerative energy.
[0114] FIG. 8 shows an example of a car equipped with a battery pack according to an embodiment.
[0115] An automobile 71 shown in Fig. 8 is equipped with a battery pack 72 according to an embodiment in an engine compartment at the front of the vehicle. The location of the battery pack in the automobile is not limited to the engine compartment. For example, the battery pack can be equipped at the rear of the automobile or under the seat.
[0116] Fig. 9 is a diagram illustrating a schematic configuration of an example of a vehicle according to the embodiment. A vehicle 300 illustrated in Fig. 9 is an electric vehicle.
[0117] The vehicle 300 shown in FIG. 9 includes a vehicle power supply 301, a vehicle ECU (Electric Control Unit) 380 which is a higher-level control means for the vehicle power supply 301, an external terminal 370, an inverter 340, and a drive motor 345.
[0118] The vehicle 300 has a vehicle power supply 301 mounted, for example, in the engine compartment, the rear of the vehicle body, or under a seat. However, in Fig. 9, the mounting location of the secondary battery in the vehicle 300 is shown only diagrammatically.
[0119] The vehicle power supply 301 includes a plurality of (eg, three) battery packs 312 a , 312 b , and 312 c , a battery management unit (BMU) 311 , and a communication bus 310 .
[0120] The three battery packs 312a, 312b, and 312c are electrically connected in series. The battery pack 312a includes an assembled battery 314a and an assembled battery monitoring device (VTM: Voltage Temperature Monitoring) 313a. The battery pack 312b includes an assembled battery 314b and an assembled battery monitoring device 313b. The battery pack 312c includes an assembled battery 314c and an assembled battery monitoring device 313c. The battery packs 312a, 312b, and 312c can be removed independently and replaced with different battery packs.
[0121] Each of the assembled batteries 314a to 314c includes a plurality of secondary batteries connected in series. Each secondary battery is a secondary battery according to the embodiment. Each of the assembled batteries 314a to 314c is charged and discharged via a positive terminal 316 and a negative terminal 317.
[0122] In order to collect information related to the maintenance of the vehicle power supply 301, the battery management device 311 communicates with the assembled battery monitoring devices 313a to 313c to collect information such as the voltage and temperature of the secondary batteries of the assembled batteries 314a to 314c included in the vehicle power supply 301.
[0123] A communication bus 310 is connected between the battery management unit 311 and the assembled battery monitoring units 313a to 313c. The communication bus 310 is configured so that one set of communication lines is shared by a plurality of nodes (the battery management unit and one or more assembled battery monitoring units). The communication bus 310 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0124] The assembled battery monitoring devices 313a to 313c measure the voltage and temperature of each of the secondary batteries constituting the assembled batteries 314a to 314c based on commands communicated from the battery management device 311. However, the temperature can be measured at only a few points per assembled battery, and it is not necessary to measure the temperatures of all of the secondary batteries.
[0125] The vehicle power supply 301 may also have an electromagnetic contactor (for example, a switch device 333 shown in FIG. 9) for connecting and disconnecting the positive and negative terminals. The switch device 333 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 314a to 314c are charged, and a main switch (not shown) that is turned on when the battery output is supplied to a load. The pre-charge switch and the main switch include a relay circuit (not shown) that is turned on and off by a signal supplied to a coil arranged near the switch element.
[0126] The inverter 340 converts the input DC voltage into a three-phase AC high voltage for driving the motor. The output voltage of the inverter 340 is controlled based on a control signal from a battery management device 311 (described later) or a vehicle ECU 380 for controlling the overall operation of the vehicle. The three-phase output terminals of the inverter 340 are connected to the three-phase input terminals of the drive motor 345.
[0127] The drive motor 345 rotates by the electric power supplied from the inverter 340, and transmits the rotation to the axles and drive wheels W via, for example, a differential gear unit.
[0128] Although not shown, the vehicle 300 is equipped with a regenerative braking mechanism that rotates the drive motor 345 when the vehicle 300 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 340 and converted into a direct current. The direct current is input to the vehicle power supply 301.
[0129] One terminal of a connection line L1 is connected to the negative terminal 317 of the vehicle power supply 301 via a current detection unit (not shown) in the battery management device 311. The other terminal of the connection line L1 is connected to the negative input terminal of the inverter 340.
[0130] One terminal of a connection line L2 is connected to a positive terminal 316 of the vehicle power supply 301 via a switch device 333. The other terminal of the connection line L2 is connected to a positive input terminal of an inverter 340.
[0131] The external terminal 370 is connected to a battery management unit 311, which will be described later. The external terminal 370 can be connected to, for example, an external power source.
[0132] The vehicle ECU 380 controls the battery management device 311 in cooperation with other devices in response to operation inputs from the driver or the like, and manages the entire vehicle. Between the battery management device 311 and the vehicle ECU 380, data transfer regarding the maintenance of the vehicle power supply 301, such as the remaining capacity of the vehicle power supply 301, is performed via a communication line.
[0133] According to the vehicle of the embodiment, it includes a battery pack including a secondary battery according to the embodiment, and the battery packs (for example, the battery packs 312a, 312b, and 312c) are excellent in life performance and input / output performance, so a vehicle excellent in charge / discharge performance and high in reliability can be obtained. Furthermore, since each battery pack is inexpensive and highly safe, the cost of the vehicle can be suppressed and the safety can be enhanced.
Example
[0134] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings, but the present invention is not limited to the embodiments described below. (Example 1) (Preparation of slurry composition) Carbon fibers were dispersed in pure water to prepare a carbon fiber dispersion. As the carbon fibers, carbon nanotubes were used. The carbon fiber dispersion, the active material, the lithium ion-conductive inorganic solid particles, and the viscosity modifier were mixed, and this mixture was stirred using a planetary mixer (Awatori Renkato) manufactured by THINKY Corporation to prepare a first slurry. Table 2 shows the solid content ratio, stirring speed (rotation speed), and stirring time of the first slurry. As the active material, particles of niobium titanate composite oxide (Nb2TiO7) having an average particle diameter of about 1 μm were used. As the viscosity modifier, carboxymethyl cellulose (CMC) was used. As the lithium ion-conductive inorganic solid particles, lithium phosphorus solid electrolyte particles (Li -4 Al 1+x+y Al x (Ti,Ge) 2-x Si y P 3-y O 12 (0 < x ≦ 2, 0 ≦ y < 3)) were used. The first slurry was mixed with granular carbon and a binder, and the mixture was stirred using a planetary centrifugal mixer to prepare a second slurry. At this time, the solid content ratio of the second slurry was 60% by mass. During stirring, the stirring speed was 1500 rpm and the stirring time was 2 minutes. As the granular carbon, acetylene black (AB) with an average particle size of 0.2 μm was used. As the binder, styrene butadiene rubber was used. In the second slurry, the amounts of the inorganic solid particles, carbon fiber, granular carbon, viscosity modifier, and binder relative to 100 parts by mass of the active material were 4 parts by mass, 3 parts by mass, 3 parts by mass, 2 parts by mass, and 3 parts by mass, respectively.
[0135] The second slurry was mixed with pure water to a solid content ratio of 49% by mass, and further stirred using a planetary centrifugal mixer to prepare a third slurry. The stirring speed of the third slurry was set to 1000 rpm, and the stirring time was set to 1 minute.
[0136] The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) based on the obtained particle size distribution is shown in Figure 1. The horizontal axis of Figure 1 is a logarithmic scale (log) for particle size (μm), and the vertical axis shows the cumulative frequency ratio (%) of particle size (μm) based on the volume. Table 1 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm in the cumulative frequency distribution.
[0137] The viscosity of the slurry composition was measured at 25° C. and 100 rpm using a Brookfield viscometer by the method described above, and the results are shown in Table 1. (Preparation of negative electrode) The above slurry composition was applied to both sides of a current collector, and the coating was dried to form an active material-containing layer. An aluminum foil with a thickness of 12 μm was used as the current collector. After drying this at 130° C. under vacuum for 12 hours, the current collector and the active material-containing layer were rolled with a roll press to obtain a negative electrode. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0138] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution on a volume basis of particle size (μm) was created based on the obtained particle size distribution, resulting in a cumulative frequency distribution with a profile similar to that shown in Figure 1. (Examples 2-11 and Comparative Examples 1-4) A slurry composition was prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed and stirring time of each of the first slurry, the second slurry and the third slurry were set to the values shown in Table 2. An electrode was manufactured in the same manner as in Example 1 using the prepared slurry composition. Table 1 shows the peak position, the ratio of the cumulative frequency from the small particle size side to a particle size of 1 μm, the ratio of the cumulative frequency from the small particle size side to a particle size of 2 μm, and the ratio of the cumulative frequency from the small particle size side to a particle size of 5 μm in the cumulative frequency distribution of the slurry composition and electrode of the examples and comparative examples. Table 1 also shows the B-type viscosity of the slurry composition. The cumulative frequency distribution of the slurry composition of Comparative Example 2 is also shown in FIG. 1. (Input / output performance evaluation) A three-electrode glass cell was fabricated and the input / output performance was evaluated. The size of the electrodes was a square with each side measuring 2 cm. Lithium metal was used for the counter electrode and reference electrode. The non-aqueous electrolyte was a mixture of ethylene carbonate and diethyl carbonate in which lithium hexafluorophosphate (LiPF6) was dissolved. The volume ratio of ethylene carbonate to diethyl carbonate in the mixed solvent was 1:2. The concentration of LiPF6 was 1 mol / L. The amount of non-aqueous electrolyte was 25 mL. First, the three-electrode glass cell was charged at a current density of 1C in an environment of 25°C until the state of charge (SOC) reached 100%. Then, the cell was discharged at a current density of 0.2C until the SOC reached 0%, and the discharge capacity W1 was measured. Next, the three-electrode glass cell was charged again at a current density of 1C until the SOC reached 100%. Then, the cell was discharged at a current density of 5C until the SOC reached 0%, and the discharge capacity W2 was measured. The capacity ratio W2 / W1 was calculated by dividing the discharge capacity W2 by the discharge capacity W1. The capacity ratio W2 / W1 is shown in Table 3. <Cycle performance evaluation> The cycle performance was evaluated using a three-electrode glass cell. The battery was charged at a current density of 1C in an environment of 25°C until the SOC reached 100%. Then, the battery was discharged at a current density of 1C until the SOC reached 0%, and the discharge capacity was measured. This charge / discharge cycle was counted as one cycle, and the battery was repeatedly charged / discharged until the discharge capacity retention rate relative to the first discharge capacity reached 80%. The number of charge / discharge cycles is shown in Table 3.
[0139] [Table 1]
[0140] [Table 2]
[0141] [Table 3]
[0142] As is clear from Tables 1 to 3, Examples 1 to 11 are superior to Comparative Examples 1 to 4 in terms of input / output performance and cycle life performance indicated by the capacity ratio W2 / W1. FIG. 1 compares the cumulative frequency distribution of the slurry composition of Example 1 with the cumulative frequency distribution of the slurry composition of Comparative Example 2. As is clear from FIG. 1, the slurry composition of Example 1 has a higher ratio of the volume of fine particles to the total volume of the particle group than Comparative Example 2.
[0143] In Comparative Example 1, the peak position of the cumulative frequency distribution is less than 0.8 μm. This is because the stirring speeds of the first and second slurries were high and the stirring times were long, causing damage such as cracking or chipping of the niobium titanium-containing composite oxide particles and separation or breakage of the conductive agent.
[0144] In Comparative Example 2, the peak position of the cumulative frequency distribution exceeds 3 μm. This is because the second slurry was stirred in a state where the solid content ratio was low, causing aggregation of the niobium titanium-containing composite oxide particles or the conductive agent.
[0145] In Comparative Example 3, the ratio of the cumulative frequency of particles up to 1 μm is less than 20%. This is because the stirring time of the first slurry is short, causing aggregation of the niobium titanium-containing composite oxide particles or the conductive agent.
[0146] In Comparative Example 4, the ratio of the cumulative frequency of particle sizes up to 1 μm exceeds 35%. This is because the stirring speed of the second slurry is high and the stirring time is long, causing damage such as cracking or chipping of the niobium titanium-containing composite oxide particles and separation or breakage of the conductive agent. Example 12 (Preparation of Slurry Composition) Carbon fibers similar to those described in Example 1 were dispersed in pure water to prepare a carbon fiber dispersion. The carbon fiber dispersion, active material, lithium ion conductive inorganic solid particles, and viscosity modifier were mixed, and the mixture was stirred using a THINKY Corporation centrifugal mixer (Awatori Rentaro) to prepare a first slurry. The solid content ratio, stirring speed (number of revolutions), and stirring time of the first slurry are shown in Table 5. The active material, viscosity modifier, and lithium ion conductive inorganic solid particles used were similar to those described in Example 1. Granular carbon and a binder were mixed into the first slurry, and the mixture was stirred using a planetary centrifugal mixer to prepare a second slurry. The solid content ratio, stirring speed, and stirring time of the second slurry are shown in Table 5. As the granular carbon, flake graphite with an average particle size of 3 μm was used. As the binder, the same one as described in Example 1 was used. In the second slurry, the amounts of the inorganic solid particles, carbon fiber, granular carbon, viscosity modifier, and binder relative to 100 parts by mass of the active material were 5 parts by mass, 3 parts by mass, 3 parts by mass, 2 parts by mass, and 4 parts by mass, respectively.
[0147] The second slurry was mixed with pure water to give a solid content ratio shown in Table 5, and the mixture was further stirred using a planetary centrifugal mixer to prepare a third slurry. The stirring speed and stirring time are shown in Table 5.
[0148] The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0149] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0150] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0151] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. Example 13 The active material was a niobium titanium-containing composite oxide (TiNb 1.9 Mo 0.075 Mg 0.025 O7) particles were used. A slurry composition was prepared in the same manner as described in Example 1, except that this active material was used and the solid content ratio, stirring speed, and stirring time of each of the first slurry, second slurry, and third slurry were set to the values shown in Table 5. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method in the above-mentioned manner, and a cumulative frequency distribution based on the volume of the particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm in the cumulative frequency distribution. Table 4 also shows the B-type viscosity of the slurry composition.
[0152] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0153] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0154] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. Example 14 As the binder, polyvinylidene fluoride was used. The slurry composition was prepared in the same manner as described in Example 1, except that this binder was used and the solid content ratio, stirring speed, and stirring time of each of the first slurry, the second slurry, and the third slurry were set to the values shown in Table 5. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method in the above-mentioned manner, and a cumulative frequency distribution based on the volume of the particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm in the cumulative frequency distribution. Table 4 also shows the B-type viscosity of the slurry composition.
[0155] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0156] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0157] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. Example 15 (Preparation of Slurry Composition) Carbon fiber was dispersed in pure water to prepare a carbon fiber dispersion. Vapor-grown carbon fiber (VGCF) was used as the carbon fiber. The carbon fiber dispersion, active material, lithium ion conductive inorganic solid particles, and viscosity modifier were mixed, and the mixture was stirred using a THINKY Corporation centrifugal mixer (Awatori Rentaro) to prepare a first slurry. The solid content ratio, stirring speed (rotation speed), and stirring time of the first slurry are shown in Table 5. The active material, viscosity modifier, and lithium ion conductive inorganic solid particles were the same as those described in Example 1. Granular carbon and a binder were mixed with the first slurry, and the mixture was stirred using a planetary centrifugal mixer to prepare a second slurry. The solid content ratio, stirring speed, and stirring time of the second slurry are shown in Table 5. The granular carbon and binder used were the same as those described in Example 1. In the second slurry, the amounts of inorganic solid particles, carbon fiber, granular carbon, viscosity modifier, and binder per 100 parts by mass of active material were 4 parts by mass, 2 parts by mass, 3 parts by mass, 3 parts by mass, and 3 parts by mass, respectively.
[0158] The second slurry was mixed with pure water to give a solid content ratio shown in Table 5, and the mixture was further stirred using a planetary centrifugal mixer to prepare a third slurry. The stirring speed and stirring time are shown in Table 5.
[0159] The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0160] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0161] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0162] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. (Example 16) The first slurry was prepared using the same raw materials as described in Example 1, except that PVP was used as a dispersant. The solid content ratio, stirring speed (rotation speed), and stirring time of the first slurry are shown in Table 5. The second and third slurries were prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed (rotation speed), and stirring time were set to the values shown in Table 5. In the obtained slurry composition, the amounts of inorganic solid particles, carbon fiber, granular carbon, viscosity modifier, dispersant, and binder relative to 100 parts by mass of active material were 4 parts by mass, 2 parts by mass, 3 parts by mass, 3 parts by mass, 1 part by mass, and 3 parts by mass, respectively. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0163] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0164] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0165] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. (Example 17) The first slurry was prepared using the same raw materials as described in Example 1, except that PVB was used as a dispersant. The solid content ratio, stirring speed (rotation speed), and stirring time of the first slurry are shown in Table 5. The second slurry and the third slurry were prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed (rotation speed), and stirring time were set to the values shown in Table 5. In the obtained slurry composition, the amounts of the inorganic solid particles, carbon fiber, granular carbon, viscosity modifier, dispersant, and binder relative to 100 parts by mass of the active material were 4 parts by mass, 2 parts by mass, 3 parts by mass, 3 parts by mass, 1 part by mass, and 3 parts by mass, respectively. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0166] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0167] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0168] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. (Example 18) The first slurry was prepared using the same raw materials as described in Example 1, except that cellulose nanofibers were used as a dispersant. The solid content ratio, stirring speed (rotation speed), and stirring time of the first slurry are shown in Table 5. The second and third slurries were prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed (rotation speed), and stirring time were set to the values shown in Table 5. In the obtained slurry composition, the amounts of inorganic solid particles, carbon fibers, granular carbon, viscosity modifier, dispersant, and binder relative to 100 parts by mass of active material were 4 parts by mass, 2 parts by mass, 3 parts by mass, 3 parts by mass, 1 part by mass, and 3 parts by mass, respectively. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0169] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0170] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0171] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. (Example 19) The slurry was prepared in the same manner as in Example 1, except that the first slurry was prepared using PVP and cellulose nanofiber as dispersant 1 and dispersant 2, respectively. The second and third slurries were prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed (rotation speed), and stirring time were set to the values shown in Table 5. In the obtained slurry composition, the amounts of inorganic solid particles, carbon fibers, granular carbon, viscosity modifier, dispersant 1, dispersant 2, and binder relative to 100 parts by mass of active material were 4 parts by mass, 3 parts by mass, 3 parts by mass, 2 parts by mass, 1 part by mass, 1 part by mass, and 3 parts by mass, respectively. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0172] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0173] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0174] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. (Example 20) A slurry was prepared in the same manner as in Example 1, except that the first slurry was prepared without using lithium ion conductive inorganic solid particles. The second and third slurries were prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed (number of revolutions), and stirring time were set to the values shown in Table 5. In the obtained slurry composition, the amounts of carbon fiber, granular carbon, viscosity modifier, and binder per 100 parts by mass of active material were 3 parts by mass, 3 parts by mass, 2 parts by mass, and 3 parts by mass, respectively. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0175] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0176] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0177] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. Example 21 Slurries were prepared in the same manner as in Example 1, except that acetylene black (AB) with an average particle size of 0.2 μm and scaly carbon with an average particle size of 4 μm were used as granular carbon 1 and granular carbon 2. The second and third slurries were prepared in the same manner as in Example 1, except that the solid content ratio, stirring speed (rotation speed), and stirring time were set to the values shown in Table 5. In the obtained slurry compositions, the amounts of inorganic solid particles, carbon fibers, granular carbon 1, granular carbon 2, viscosity modifier, and binder per 100 parts by mass of active material were 4 parts by mass, 3 parts by mass, 3 parts by mass, 3 parts by mass, 2 parts by mass, and 3 parts by mass, respectively. The particle size distribution of the slurry composition was measured by the laser diffraction scattering method as described above, and a cumulative frequency distribution based on the volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the cumulative frequency ratio from the smallest particle size to a particle size of 1 μm, the cumulative frequency ratio from the smallest particle size to a particle size of 2 μm, and the cumulative frequency ratio from the smallest particle size to a particle size of 5 μm. Table 4 also shows the B-type viscosity of the slurry composition.
[0178] (Preparation of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0179] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0180] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6. Example 22 Carbon fiber, an active material, lithium ion conductive inorganic solid particles, granular carbon, a dispersant, a viscosity modifier, a binder, and water were mixed, and this mixture was stirred using a planetary mixer (Awatori Renkatarou) manufactured by THINKY to prepare a first slurry. Table 5 shows the solid content ratio, stirring speed (rotation speed), and stirring time of the first slurry. As the active material, particles of niobium titanate composite oxide (Nb2TiO7) with an average particle size of about 1 μm were used. As the viscosity modifier, carboxymethyl cellulose (CMC) was used. As the lithium ion conductive inorganic solid particles, lithium phosphorus solid electrolyte particles (Li -4 S / cm) having a NASICON type structure with an average particle size of 0.5 μm and a lithium ion conductivity of 1×10 1+x+y Al x (Ti, Ge) 2-x Si y P 3-y O 12 (0 < x ≦ 2, 0 ≦ y < 3)) were used. As the dispersant, PVP was used. As the granular carbon, acetylene black (AB) with an average particle size of 0.2 μm was used. As the binder, styrene butadiene rubber was used. In the first slurry, the amounts of inorganic solid particles, carbon fiber, granular carbon, viscosity modifier, dispersant, and binder with respect to 100 parts by mass of the active material were 4 parts by mass, 3 parts by mass, 3 parts by mass, 2 parts by mass, 1 part by mass, and 3 parts by mass, respectively.
[0181] Pure water was mixed with the first slurry, and further stirring was performed using a planetary mixer to prepare a second slurry. Table 5 shows the solid content ratio, stirring speed (rotation speed), and stirring time of the second slurry. The particle size distribution of the slurry composition by laser diffraction scattering method was measured by the above-mentioned method, and a cumulative frequency distribution based on volume of particle size (μm) was created from the obtained particle size distribution. Table 4 shows the peak position, the ratio of the cumulative frequency from the smaller particle size to 1 μm in the cumulative frequency distribution, the ratio of the cumulative frequency from the smaller particle size to 2 μm, and the ratio of the cumulative frequency from the smaller particle size to 5 μm. Table 4 also shows the Brookfield viscosity of the slurry composition.
[0182] (Fabrication of negative electrode) Using the above slurry composition, a negative electrode was obtained in the same manner as described in Example 1. The density of the active material-containing layer after pressing was 2.5 g / cm 3 It was.
[0183] The particle size distribution of the negative electrode active material-containing layer was measured by the laser diffraction scattering method as described above, and the cumulative frequency distribution of particle size (μm) on a volume basis based on the obtained particle size distribution was calculated. The cumulative frequency distribution had a profile similar to that of the slurry composition.
[0184] Using the obtained negative electrode of this example, the input / output performance and cycle performance were measured in the same manner as in Example 1. The results are shown in Table 6.
[0185] [Table 4]
[0186] [Table 5]
[0187] [Table 6]
[0188] As shown in the results of Tables 4 to 6, even when the composition of the slurry is changed by changing the type of active material, conductive agent, or binder, or when the order of adding the raw materials is changed, it is possible to realize an electrode and a secondary battery with excellent input / output performance and cycle performance by satisfying a predetermined cumulative frequency distribution.
[0189] According to at least one of these embodiments or examples, the slurry composition contains niobium titanium-containing composite oxide particles, a conductive agent, a resin material, and water, and the cumulative frequency distribution of particle size on a volume basis based on the particle size distribution of the slurry composition by a laser diffraction scattering method has a peak position in the range of 0.8 μm or more and 3 μm or less, and the ratio of the cumulative frequency from the small particle size side to the particle size of 1 μm is in the range of 20% or more and 35% or less, so that it is possible to provide an electrode and a secondary battery that have both a long life and high input / output performance.
[0190] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. The invention as originally claimed in the present application is set forth below. [1] A slurry composition comprising an active material containing niobium titanium-containing composite oxide particles, a conductive agent, a resin material, and a solvent containing water, wherein the volume-based cumulative frequency distribution of particle diameters based on a particle size distribution of the slurry composition measured by a laser diffraction scattering method has a peak position in the range of 0.8 μm to 3 μm, and the ratio of the cumulative frequency from the smallest particle diameter to a particle diameter of 1 μm is in the range of 20% to 35%. [2] The slurry composition according to [1], wherein in the cumulative frequency distribution, the ratio of cumulative frequencies from the smallest particle size to a particle size of 2 μm is in the range of 50% or more and 70% or less. [3] The slurry composition according to [1] or [2], wherein in the cumulative frequency distribution, the ratio of cumulative frequencies from the smallest particle size to a particle size of 5 μm is in the range of 80% or more and 95% or less. [4] The slurry composition according to any one of [1] to [3], having a viscosity of 1.5 Pa·s or more and 5 Pa·s or less at 25°C and 100 rpm as measured with a Brookfield viscometer. [5] The slurry composition according to any one of [1] to [4], further comprising lithium ion conductive inorganic solid particles. [6] The niobium titanium-containing composite oxide particles are x Ti 1-y M1 y Nb 2-z M2 z O 7+δ (M1 is at least one selected from the group consisting of Zr, Si, and Sn, M2 is at least one selected from the group consisting of V, Ta, and Bi, and 0≦x≦5, 0≦y<1, 0≦z<2, -0.3≦δ≦0.3), or Li x Ti 1-y M3 y+z Nb 2-z O 7-δ (M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo, and 0≦x≦5, 0≦y<1, 0≦z<2, -0.3≦δ≦0.3). [7] A method for producing a current collector comprising the steps of: applying the slurry composition according to any one of [1] to [6] to a current collector; and drying the slurry composition applied to the current collector to form an active material-containing layer on the current collector. a step of pressing the active material-containing layer; A method for manufacturing an electrode, comprising: [8] An electrode comprising: an active material containing niobium titanium-containing composite oxide particles; an active material-containing layer containing a conductive agent and a resin material; and a current collector on which the active material-containing layer is formed, An electrode, in which a cumulative frequency distribution on a volume basis of particle size based on a particle size distribution by a laser diffraction scattering method of the active material-containing layer has a peak position in the range of 0.8 μm or more and 3 μm or less, and the ratio of the cumulative frequency from the smallest particle size to a particle size of 1 μm is in the range of 20% or more and 35% or less. [9] A positive electrode; [8] as a negative electrode; and Non-aqueous electrolyte A secondary battery comprising:
[10] A battery pack comprising one or more of the secondary batteries described in [9].
[11] An external terminal for supplying current; The battery pack according to
[10] , further comprising a protection circuit.
[12] A battery pack as described in
[10] or
[11] , comprising two or more of the secondary batteries, the two or more secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.
[13] A vehicle equipped with a battery pack described in any one of
[10] to
[12] .
[14] A vehicle as described in
[13] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy. [Explanation of symbols]
[0191] Reference Signs List 1...electrode group, 2...container (exterior member), 3...positive electrode, 3a...positive electrode current collector, 3b...positive electrode active material-containing layer, 4...negative electrode, 4a...negative electrode current collector, 4b...negative electrode active material-containing layer, 5...separator, 6...positive electrode lead, 7...negative electrode lead, 8...positive electrode current collector tab, 9...negative electrode current collector tab, 10...sealing plate, 11...insulating member, 12...exterior member, 13...negative electrode terminal, 14...positive electrode terminal, 50...battery pack, 51...unit cell, 53...battery assembly, 54...printed wiring board, 55...substrate -mistor, 56...protection circuit, 57...external terminal for current supply, 71...automobile, 72...battery pack, 300...vehicle, 301...vehicle power supply, 310...communication bus, 311...battery management device, 312a-c...battery packs, 313a-c...battery pack monitoring device, 314a-c...battery pack, 316...positive terminal, 317 negative terminal, 340...inverter, 345...drive motor, 370...external terminal, 380...vehicle ECU, L1, L2...connection lines, W...drive wheels.
Claims
1. A slurry composition comprising an active material containing niobium titanium-containing composite oxide particles, a conductive agent, a resin material, and a solvent containing water, wherein a cumulative frequency distribution of particle diameters on a volume basis based on a particle size distribution of the slurry composition by a laser diffraction scattering method has a peak position in the range of 0.8 μm or more and 3 μm or less, and a cumulative frequency ratio of particle diameters from a small particle diameter to a particle diameter of 1 μm is in the range of 20% or more and 35% or less, In the cumulative frequency distribution, the ratio of the cumulative frequency from the smallest particle size to a particle size of 2 μm is in the range of 50% to 70%. A slurry composition, wherein in the cumulative frequency distribution, the ratio of cumulative frequencies from the smallest particle size to a particle size of 5 μm is in the range of 80% or more and 95% or less.
2. 2. The slurry composition according to claim 1, having a viscosity of 1.5 Pa·s or more and 5 Pa·s or less at 25° C. and 100 rpm as measured by a Brookfield viscometer.
3. 3. The slurry composition of claim 1 or claim 2, further comprising lithium ion conductive inorganic solid particles.
4. The niobium titanium-containing composite oxide particles are x Ti 1-y M1 y Nb 2-z M2 z O 7+δ (M1 is at least one selected from the group consisting of Zr, Si, and Sn, M2 is at least one selected from the group consisting of V, Ta, and Bi, and 0≦x≦5, 0≦y<1, 0≦z<2, −0.3≦δ≦0.3), or Li x Ti 1-y M3 y+z Nb 2-z O 7-δ (M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo, and is 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3). The slurry composition according to any one of claims 1 to 3.
5. A slurry composition described in any one of claims 1 to 4, wherein the conductive agent includes at least one of a fibrous carbon material and a granular carbon material.
6. A step of applying the slurry composition according to any one of claims 1 to 5 to a current collector; forming an active material-containing layer on the current collector by drying the slurry composition applied to the current collector; a step of pressing the active material-containing layer; A method for manufacturing an electrode, comprising:
7. An electrode comprising: an active material containing niobium titanium-containing composite oxide particles; an active material-containing layer containing a conductive agent and a resin material; and a current collector on which the active material-containing layer is formed, a cumulative frequency distribution of particle diameters on a volume basis based on a particle size distribution by a laser diffraction scattering method of the active material-containing layer has a peak position in a range of 0.8 μm or more and 3 μm or less, and a ratio of a cumulative frequency from a small particle diameter to a particle diameter of 1 μm is in a range of 20% or more and 35% or less; In the cumulative frequency distribution, the ratio of the cumulative frequency from the smallest particle size to a particle size of 2 μm is in the range of 50% to 70%. An electrode, wherein in the cumulative frequency distribution, the ratio of cumulative frequencies from the smallest particle size to a particle size of 5 μm is in the range of 80% or more and 95% or less.
8. The electrode according to claim 7, wherein the niobium titanium-containing composite oxide particles are represented by Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ (M1 is at least one selected from the group consisting of Zr, Si and Sn, M2 is at least one selected from the group consisting of V, Ta and Bi, and 0≦x≦5, 0≦y<1, 0≦z<2, -0.3≦δ≦0.3) or Li x Ti 1-y M3 y+z Nb 2-z O 7-δ (M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta and Mo, and 0≦x≦5, 0≦y<1, 0≦z<2, -0.3≦δ≦0.3).
9. A positive electrode and The electrode according to claim 7 or 8 as a negative electrode; Non-aqueous electrolyte A secondary battery comprising:
10. A battery pack comprising one or more of the secondary batteries according to claim 9.
11. An external terminal for supplying electricity; The battery pack of claim 10 , further comprising a protection circuit.
12. The battery pack according to claim 10 or 11, comprising two or more of the secondary batteries, the two or more secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.
13. A vehicle equipped with the battery pack according to any one of claims 10 to 12.
14. The vehicle of claim 13 including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP2009158396A
Nonaqueous electrolyte battery
JP2015084322A
Positive electrode and nonaqueous electrolyte battery
JP2016048671A
Electrode, power storage device, and electronic device
JP2016219414A
Positive electrode
JP2019040890A