Method for separating impurities from silicon carbide, and temperature treated and purified silicon carbide powder
The method addresses the inefficiencies in SiC purification by combining temperature and mechanical treatments to achieve high-purity SiC powder, overcoming economic and environmental challenges of existing methods.
Patent Information
- Application Number
- JP2022546696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-31
- Filing Date
- 2021-01-29
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2041-01-29
AI Technical Summary
The existing methods for purifying silicon carbide (SiC) are costly, environmentally unfriendly, and inefficient in removing a wide variety of impurities, leading to a shortage of high-quality SiC granules needed for high-tech applications, with current production methods being economically unviable and environmentally harmful.
A method involving temperature treatment of SiC waste under vacuum or non-oxidizing atmosphere, followed by mechanical separation, to remove impurities effectively, resulting in a purified SiC powder suitable for high-tech applications.
The method achieves a high-purity SiC powder with at least 98% purity, economically viable and environmentally friendly, suitable for industrial reuse, by effectively separating impurities through temperature and mechanical treatment.
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of technical ceramics and relates to a method for separating impurities from silicon carbide, which can be applied, for example, to SiC powder of grinding sludge or silicon carbide waste resulting from production or so-called SiC sinter scrap, and to a temperature-treated and then purified silicon carbide powder.
[0002] Silicon carbide (SiC) is an industrial synthetic mineral that is used in many industrial sectors due to its excellent properties (hardness, high temperature properties, chemical resistance). Of particular importance is its use in the form of specific ultrafine powders (0.5 to about 250 μm) of high purity and rigorously fractionated as an abrasive for high-quality surface treatment in microelectronics / photovoltaics (wafer sawing), ceramics production, bulletproof ceramics production for military technology, automotive / environmental technology (diesel particulate filters) and mechanical engineering in general.
[0003] SiC powder is produced by crushing, refining and separating specific raw SiC, a process that produces large and constant quantities of low-value and low-utilization SiC.
[0004] Therefore, an increase in the demand for granules always requires an increase in the production of raw SiC. To this extent, an increase in the amount of raw material is not advantageous for the producers, but leads to structural shortages and inflexible prices.
[0005] The production of raw SiC by electrolytic synthesis, the so-called Acheson process (DE 76629 A, DE 85197 A), which has been in use for about 120 years, is associated with high electricity and oil (raw petroleum coke) prices, as well as environmental costs (due to high dust, CO / CO2 and SO2 emissions). Alternative production methods have not been successful, mainly for economic reasons, despite many attempts, and are not available for the time being.
[0006] Although SiC is considered a globally available bulk material, strategically important high quality (HQ) granules have already been experiencing shortages and price increases for the past few years. In 2008, a shortage of 40,000-60,000 tonnes of HQ SiC raw material was estimated in Europe (Silicon Carbide & More #24, 2008, S. 3). But a bigger problem with these specific granules is the large demand for individual particle size bands for high-tech applications. All this, in conjunction with the previously mentioned inflexible price, leads to price increases and supply shortages of these specific HQ granules.
[0007] SiC powder for abrasive applications is worn down in terms of cutting performance and particle size. Much of the SiC is lost during dissipation. Where waste containing SiC can be recovered, material separation is technically very difficult and reprocessing is not economically viable.
[0008] Overall, there are large amounts of SiC powder contaminated with a wide variety of substances. The impurities are very diverse according to their origin and consist of organic and inorganic non-metallic impurities and inorganic metallic impurities. Organic impurities include organic polymer residues (mainly hydrocarbon compounds) such as liquid oils, polyethylene glycols (PEG), solvents, lubricants, as well as solid polymers such as plastic wear products.
[0009] Inorganic non-metallic impurities include, among others, free carbon and silicon oxides (mainly SiO2), and Ca-Al-Si-O compounds.Metallic impurities include iron and iron alloys, boron, vanadium, aluminum, titanium, copper, manganese, tungsten, chromium, nickel and their compounds.
[0010] In addition, the so-called free silicon (Si 遊離 ), which is understood to mean metal or alloy silicon that is not bonded in SiC or SiO2. SiC waste occurs, for example, during the production of SiC in the Acheson process or as scrap from SiC mouldings and cannot be industrially processed without further reprocessing steps.
[0011] Impurities are, for example, classified according to DIN EN ISO 9286, DIN EN ISO 21068 Part 1-3 and C according to FEPA standard 45-1:2011. 遊離 , Si 遊離 , SiO2 and iron. Spectroscopic methods, in particular DIN EN 15991, are also used to analyze impurities.
[0012] There are already many known methods for separating impurities and purifying, i.e., increasing the SiC content of contaminated SiC. These can be divided into physical and chemical processes.
[0013] Physical processes exploit the differences in density, particle size and other physical properties of some impurities, such as magnetic properties and wettability. For example, iron impurities, which are magnetic, are removed by magnetic separation. Impurities with different particle sizes and densities are separated by cyclone and hydrocyclone processes. Impurities with different densities and wettability are separated by flotation processes.
[0014] Chemical processes essentially rely on the solubility of each impurity in chemicals such as solvents, acids or alkalis. As SiC is very stable to such chemicals, even very aggressive chemicals such as hydrofluoric acid can be used to dissolve the impurities.
[0015] It is also possible to remove impurities using thermal processes; for example, free carbon can be oxidized at temperatures of 400-800 °C in air. It is also known that by partially adding NaCl during the synthesis of SiC, unwanted impurities react with chlorine at high temperatures to form easily volatile chlorides, which can then be removed from the SiC. However, post-treatment of contaminated powders by this method is not known because it is very costly, chlorine gas acts aggressively on plant equipment, and is not environmentally friendly.
[0016] A disadvantage of the known methods is that the removal of impurities from SiC requires a high level of effort, since a specific process must be used to remove each particular impurity, and thus a combination of processes is always required to obtain the highest possible purity of SiC in high concentration.
[0017] The object of the present invention is to provide a method for separating impurities from silicon carbide, which allows the various impurities to be substantially completely removed in a simple and economical manner, or to be removed to such an extent that the purified silicon carbide powder can be industrially reused, to provide a temperature-treated SiC powder that can be easily purified in a simple and low-cost manner, and a purified silicon carbide powder for industrial applications, in particular high-tech applications.
[0018] This problem is solved by the invention as set forth in the claims. Advantageous embodiments are the subject matter of the dependent claims, the invention also comprising combinations of the individual claims in the sense of an AND conjunction, insofar as they are not mutually exclusive.
[0019] In the method for separating impurities from silicon carbide according to the present invention, the average particle size d 50 Powdered SiC waste containing at least 50% by mass of SiC with a size of 0.5-1000 μm and having a minimum content of 0.1% by mass of iron and 0.1% by mass of metallic silicon is subjected to a temperature treatment at a temperature of 1400-2600°C under vacuum or a non-oxidizing atmosphere, cooled and then mechanically processed to physically separate, and then the physically separated SiC powder is divided into two fractions, in one of which the mass of impurities is at least twice that of the other fraction.
[0020] Advantageously, in one fraction the mass of impurities is at least 10 times, advantageously at least 20 times, that of the other fraction.
[0021] More preferably, the powdered SiC waste comprises at least 75% by weight of SiC, advantageously 80% by weight of SiC, even more advantageously 85% by weight of SiC, even more advantageously 90% by weight of SiC.
[0022] Also preferably, the average particle size d 50 Powdered SiC waste containing at least 50 mass % of SiC having a particle size of 0.5 to 500 μm is used.
[0023] Also advantageously, the average particle size d 50 Powdered SiC waste containing at least 50 mass % of SiC having a particle size of >500-1000 μm is used.
[0024] The average particle size d measured by the laser diffraction method 50 Advantageously, powdered SiC waste containing at least 50% by mass of SiC with a diameter of >500-1000 μm is subjected to a temperature treatment at a temperature of 1400-<2000° C.
[0025] Similarly, the average particle size d measured by the laser diffraction method 50 It is advantageous when powdered SiC waste is used which contains at least 50% by mass of SiC with a size of 0.5 to 1000 μm and has a content of 0.5 to 5.0% by mass of iron and 0.5 to 5.0% by mass of metallic silicon.
[0026] Furthermore, it is advantageous if the thermal treatment of the SiC waste is carried out at temperatures between 1400 and <2000°C.
[0027] It is also advantageous when the temperature treatment of the SiC waste is carried out at a temperature of 2000 to 2600°C.
[0028] It is also advantageous if the temperature treatment in vacuum or in a non-oxidizing atmosphere during the heating stage is carried out at a heating rate of 8 K / min or less in the temperature ranges 1200° C. to <1400° C. and 1400° C. to 1800° C.
[0029] Furthermore, it is advantageous if the temperature treatment in vacuum or in a non-oxidizing atmosphere during the heating step is carried out above 1800° C. with a heating rate of 5 K / min or less.
[0030] Likewise, it is advantageous if the temperature treatment is carried out in a vacuum or in a non-oxidizing atmosphere with a holding time at the maximum temperature of 10 minutes to 300 minutes.
[0031] It is also advantageous if the temperature treatment in a non-oxidizing atmosphere is carried out with an amount of non-oxidizing gas of 0.5 to 30 l / h.
[0032] Advantageously, the temperature treatment in vacuum or in a non-oxidizing atmosphere is carried out with the discharge of gaseous reaction products.
[0033] Also advantageously, the powdered SiC is cooled at a cooling rate of 0.1 to 100 K / min.
[0034] More preferably, the powdered SiC is cooled in the temperature range of 1200° C. to 800° C. at a cooling rate of 0.5 to 10 K / min.
[0035] Also advantageously, the mechanical treatment of the regenerated powdered SiC is carried out by application of mechanical shocks, advantageously by mixing, grinding, more advantageously by autogenous grinding, or by using eddy currents and / or ultrasound.
[0036] It is also advantageous when the mechanical treatment is carried out with an energy input of 0.1 to 5 MJ / kg.
[0037] Furthermore, it is advantageous if the physical separation of the regenerated powdered SiC is performed according to particle size, particle shape, particle density and / or physical and / or chemical surface properties of the particles.
[0038] Likewise, it is advantageous if separation according to particle size and / or particle shape is carried out by sieving, screening and / or cyclone processes.
[0039] It is also advantageous if the separation is carried out by the action of gravity on the particle density, using flotation, sedimentation, screening, centrifugation and / or cyclone processes, or by flotation and / or cyclone processes depending on the particle density.
[0040] It is also advantageous if the fraction contains at least 95% by weight, advantageously at least 98% by weight, and even more advantageously at least 99% by weight, of silicon carbide.
[0041] Furthermore, it is advantageous if, as impurities, substantially metallic impurities are separated.
[0042] Likewise, it is advantageous if carbon, advantageously carbon black, graphite and / or coke powder, and / or silicon and / or silicon dioxide (SiO2), are added during the temperature treatment in order to remove impurities in the form of Si and / or C, so as to obtain a composition of SiC that is as stoichiometric as possible.
[0043] The temperature treated silicon carbide powder according to the present invention comprises SiC powder particles and substantially metallic impurities in the form of a metallic interphase, and has the metallic impurities on the flat and / or convex surfaces of the silicon carbide powder particles, the metallic impurities being arranged in islands or in the gaps or seams between the silicon carbide powder particles and being firmly bonded to one or more silicon carbide powder particles, and the contact angle of the impurities being between 10° and 90°.
[0044] Further, the purified silicon carbide powder according to the present invention comprises at least 98% by weight of SiC and up to 2% by weight of substantially metallic impurities, the impurities being substantially located on the surface of the silicon carbide powder particles.
[0045] Advantageously, the refined silicon carbide powder comprises at least 99% by weight SiC.
[0046] Likewise, advantageously, in the purified SiC powder, the impurities are present on the surface of the silicon carbide powder particles in the form of metal interphase melt islands, which are firmly bonded to the surface of the particles after mechanical processing of the silicon carbide powder particles.
[0047] More preferably, the metallic impurities are located on the surface in the case of primary silicon carbide particles and on the surface and / or at the junctions of the particles in the case of secondary silicon carbide particles.
[0048] Also advantageously, the impurities on the surfaces of the silicon carbide powder particles are substantially located in convex shaped portions of the surfaces of the silicon carbide powder particles.
[0049] The solution according to the invention makes it possible for the first time to remove various impurities from silicon carbide in a simple and economical manner, essentially completely, or to such an extent that the purified silicon carbide powder can be industrially reused. Likewise, the solution according to the invention makes it possible for the first time to present a temperature-treated SiC powder which can be easily purified in a simple and low-cost manner, and to provide a purified silicon carbide powder which can be industrially reused, in particular for high-tech applications.
[0050] This is a method for separating impurities from silicon carbide, the method comprising the steps of: 50 This is achieved by subjecting powdered SiC waste, containing at least 50% by mass of SiC with a diameter of 0.5-1000 μm and having a minimum content of 0.1% by mass of iron and 0.1% by mass of metallic silicon, to a temperature treatment at a temperature of 1400-2600 °C under vacuum or in a non-oxidizing atmosphere, and after cooling, mechanically processing and physically separating the same, in one fraction (the "contaminated fraction") the mass of impurities is at least twice that of the other fraction (the "clean fraction").
[0051] Thus, according to the present invention, there is a "clean fraction" and a "contaminated fraction".
[0052] In the present invention, fractions are understood to mean parts of the SiC powder produced by physical separation according to their impurity content, where the physical separation can be carried out according to various physical properties, such as particle size, density, mass, concentration, etc.
[0053] For example, after physical separation of powdered SiC waste according to particle size, powder groups with, for example, three, four or five different particle sizes can be obtained. Then, depending on the subdivision and composition of the powder groups with respect to impurities, they are assigned to two fractions, namely clean and contaminated. The separation of each powder group with respect to impurities into two fractions according to the invention can be easily performed by a person skilled in the art by several fractionation experiments and content analysis, thereby achieving a separation into a "clean" fraction and a "contaminated" fraction with parameters according to the invention.
[0054] Advantageously, the mass of impurities in one fraction, the "contaminated" fraction, is 10 times, and even more advantageously 20 times, that of the other fraction, the "clean" fraction. Advantageously, relative to the total mass of the two fractions, the "clean" fraction has a mass fraction of at least 60% by mass, advantageously at least 70% by mass, and even more advantageously at least 80% by mass.
[0055] Furthermore, in the present invention, the mass of impurities in a fraction is understood to mean the mass concentration of all components other than SiC.
[0056] As a quality characteristic of SiC powder, the concentration of SiC is used first, which is determined according to FEPA standard 45-1:2011. The remainder to 100% is the impurity content. Not considered as impurities in the present invention are doping elements, such as Al and boron, incorporated into the SiC lattice. These impurities are not disadvantageous or disruptive in most applications of SiC.
[0057] According to the invention, by separating the impurities, an increase in the SiC concentration is achieved in the "clean" fraction compared to the starting SiC powder. Advantageously, an increase in the SiC concentration from 85% in the starting powder to 95% in the "clean" fraction, or from a SiC concentration of 96% in the starting powder to a SiC concentration of at least 99% in the "clean" fraction, is achieved. The mass of the impurities in the starting material is at least 3 to 100 times the mass of the impurities in the "clean" fraction.
[0058] In the method for separating impurities from silicon carbide according to the present invention, the average particle size d 50 Powdered SiC waste containing at least 50% by mass of SiC with a size of 0.5-1000 μm and having a minimum content of 0.1% by mass of iron and 0.1% by mass of metallic silicon is used as starting material.
[0059] Here, it is advantageous if the powdered SiC waste contains at least 75% by weight of SiC, better still 80% by weight of SiC, even better still 85% by weight of SiC or 90% by weight of SiC. In the powdered SiC waste, the proportion of SiC is usually not very high, but before the powdered SiC waste is used in the method according to the invention, it may be subjected to known reprocessing and homogenization processes in order to remove impurities which can already be separated in these processes. Thus, the mass of the starting material for the method according to the invention can be reduced overall and limited to powdered SiC waste from which separation of impurities is not possible.
[0060] Furthermore, according to the present invention, the average particle size d 50 It may be advantageous to use powdered SiC waste containing at least 50% by mass of SiC with a size of 0.5-500 μm, or >500-1000 μm.
[0061] According to the solution according to the invention, the average particle size d 50Powdered SiC waste is used, which contains at least 50% by weight of SiC with a diameter of 0.5-1000 μm and has a minimum content of 0.1% by weight of iron and 0.1% by weight of metallic silicon, and which advantageously has a content of 0.5-5.0% by weight of iron and 0.5-5.0% by weight of metallic silicon. According to the invention, the SiC waste must have a content of at least 0.1% by weight of iron, which may be present in the form of iron, iron alloys or iron compounds. The at least 0.1% by weight of metallic silicon present according to the invention may be in the form of free silicon. If the SiC waste used according to the invention does not initially have such a content of at least 0.1% by weight of iron and 0.1% by weight of metallic silicon, these contents must be achieved by the addition of iron, iron alloys, iron compounds and / or metallic silicon.
[0062] It is therefore advantageous to analyze the material composition of the SiC waste before it is used in the method according to the invention and to add silicon, SiO2, iron, iron-containing compounds and / or carbon during the subsequent temperature treatment in order to obtain as completely regenerated powdered SiC as possible as the final product of the temperature treatment. As carbon, carbon black and / or coke powder can advantageously be added. SiO2 may also be present due to the oxidation of SiC.
[0063] It is particularly advantageous if the amounts of free carbon, SiO2, free silicon and iron are adjusted before the heat treatment so that the free carbon can react stoichiometrically with SiO2 and free silicon during the heat treatment to form SiC, with the amount of free silicon being adjusted so that it is far in excess of the free silicon and iron for this reaction, in a mass ratio of 60:40 to 20:80. As a result, chemical compounds, in particular iron silicides, can be formed during the heat treatment, which have a mass ratio of >6×10 -6 It has a high coefficient of linear thermal expansion of 1 / K, which is extremely important for subsequent purification.
[0064] It is also particularly advantageous if the free silicon and iron are present in a mass ratio of 35:65 to 20:80, since in this case mainly metastable iron silicide Fe5Si3 is formed during heat treatment, which has a very high expansion coefficient and therefore provides very good refinability during subsequent reprocessing.
[0065] The powdered SiC waste as starting material for the production of regenerated powdered silicon carbide can be used as loose bulk powder. Also, powders with a low degree of compaction, which may be present due to the production technique and / or due to powder storage, can be used as starting material as well. It is advantageous if the powdered SiC waste is not used in loose bulk form, but is subjected to a slight compaction force before being used in the method according to the invention. It is particularly advantageous if the powder is compacted by applying a compaction force of 0.002 to 100 MPa.
[0066] The bulk density is measured by weighing and measuring the volume of the bulk. The pure density of a powder is measured, for example, by gas pycnometry, and can be calculated from the known pure densities of the components if the composition is known. For silicon carbide, the pure density is 3.21 g / cm 3 It is.
[0067] These powdered SiC wastes for producing regenerated powdered silicon carbide are then subjected to a temperature treatment in a vacuum or in a non-oxidizing atmosphere at a temperature of 1400-2600° C., where the temperature is advantageously between 2000° C. and 2600° C. In the heat treatment of the powdered SiC wastes, a lower heating rate of 8 K / min or less is advantageously applied when heating in the temperature ranges from 1200° C. to <1400° C. and from 1400° C. to 1800° C., and a heating rate of 5 K / min or less is advantageously applied at temperatures above 1800° C.
[0068] In the present invention, a heating rate is understood to mean the temperature difference between the beginning and the end of a temperature range divided by the total time of heating in this temperature range. However, it is also possible to set different heating rates and even different holding times in each temperature range. In the present invention, a holding time is understood to mean that the heating rate during this time is 0 K / min.
[0069] The holding time is advantageously between 10 and 300 minutes at the maximum temperature of the method according to the invention, but this also depends on the powder volume and the temperature to be treated. Furthermore, the lower the maximum temperature, the longer the holding time at each maximum temperature.
[0070] Temperatures in the range of 1400 to <2000 ° C. are advantageously used to obtain a mean grain size d 50 It is also suitable for powdered SiC waste containing at least 50 mass % of SiC having a particle size of >500 to 1000 μm.
[0071] In the temperature treatment under a non-oxidizing atmosphere, the throughput of the non-oxidizing flowing gas during heating is set to an average flow rate of 0.5 to 30 l / min. It is particularly advantageous when the throughput of the non-oxidizing flowing gas during heating is set to an average flow rate of 0.5 to 30 l / min in the temperature range of 1200 to 2000°C. In the present invention, the average flow rate is understood to be the total amount of gas flowed from the beginning to the end of the mentioned temperature range divided by the total time of heating in this temperature range. Here, it is also possible to set the flow rate of the flowing non-oxidizing gas variously in each temperature range. The flowing gas atmosphere can be set to positive or negative pressure, and here, the negative pressure is preferably, for example, 70000 to 90000 Pa.
[0072] Depending on the device for carrying out the temperature treatment of the powdered SiC waste according to the invention, the method can be carried out in different ways. Usually, the temperature treatment is carried out in a closed furnace body, into which the powdered SiC waste in refractory containers (crucibles) is introduced. A vacuum or a non-oxidizing gas atmosphere is applied to such a closed furnace body. In the case of a non-oxidizing gas atmosphere, a flowing gas is preferably guided to the furnace body so that it flows as completely as possible around the container and the powder. This can be achieved, for example, in such a way that the gas flows in on one side of the furnace body and out on the other side, with the container being arranged between the inlet and the outlet. This gas induction or vacuum is possible both in so-called batch furnaces for discontinuous temperature treatment and in continuous furnaces for continuous temperature treatment.
[0073] As non-oxidizing atmospheres, industrial protective gas atmospheres with a residual oxygen content of <100 ppm, such as argon or nitrogen atmospheres, can be used. However, mixtures with, for example, CO can also be used, as they do not cause oxidation of the SiC. The temperature treatment can be carried out under slight positive pressure or under negative pressure up to vacuum. Advantageously, the heat treatment is carried out under an argon atmosphere. The heat treatment can be carried out in batch furnaces or in continuous operation.
[0074] The temperature treatment of the powdered SiC waste in a vacuum or in a non-oxidizing atmosphere can be carried out with the discharge of gaseous reaction products. In this case, advantageously, carbon monoxide (CO) and silicon monoxide (SiO) are discharged. Advantageously, the discharge of gaseous reaction products during the heating stage is preferably carried out in the temperature range from 1200°C to 2000°C, particularly preferably in the temperature range from 1350°C to 1800°C.
[0075] The method according to the invention provides for the separation of impurities from regenerated powdered silicon carbide.
[0076] When the SiC waste is heat-treated to produce regenerated powdered silicon carbide, the substantially powder-like structure of the product is maintained, where the silicon carbide powder particles are present either as individualized primary crystals and primary crystallites, i.e. not bonded to one another, or in a slightly interpenetrated state as secondary crystallites, i.e. as an association of interpenetrating individual primary crystals or primary crystallites. By crystallites is meant single particles that are homogeneous in crystal structure and whose external form does not or only partially has a crystal structure.
[0077] After heat treatment, the regenerated powdered silicon carbide is cooled.
[0078] Cooling is advantageously carried out at a cooling rate of 0.1-100 K / min, particularly advantageously until a temperature of 200 ° C is reached. Usually, in industrial processes, the furnace is opened at temperatures above 200 ° C and the powder can be further cooled in air. Particularly advantageous for temperature treatments with final temperatures of 2000-2600 ° C is rapid cooling from the respective final temperature to 1800 ° C at a cooling rate of 10-50 K / min. Similarly, cooling is advantageously carried out in the temperature range of 1200 ° C to 800 ° C at a cooling rate of 5-25 K / min. Such cooling rates can be achieved industrially by using rapid cooling devices, for example by introducing and circulating a low-temperature non-oxidizing gas into the furnace and passing it through a heat exchanger.
[0079] The subsequent mechanical treatment according to the invention is preferably carried out by applying mechanical impacts, preferably by mixing or grinding or by using eddy currents and / or ultrasound. Grinding can preferably be carried out by autogenous grinding (interparticle motion) under negative pressure.
[0080] More advantageously, the mechanical treatment is carried out with an energy input of between 0.1 and 5 MJ / kg.
[0081] The mechanically treated SiC powder is then physically separated, whereby the separation of the regenerated powdered SiC can be carried out according to particle size, particle shape, particle density and / or physical and / or chemical surface and / or solid properties of the particles. Separation according to particle size and / or particle shape can advantageously be carried out by sieving, sorting and / or cyclone processes.
[0082] Separation can be performed using flotation, settling, screening, centrifugation and / or cyclone processes due to the action of gravity on particle density, or separation can be performed by flotation and / or cyclone processes depending on particle density. Separation processes that use separation by electric field strength, etc. can use surface properties. Separation processes that use electrical material properties, e.g., magnetism, can use solid properties.
[0083] After physical separation, the SiC powder obtained is divided into two fractions, this division being carried out according to the mass of impurities, which, according to the invention, in one fraction the mass of impurities is at least twice that of the other fraction.
[0084] By dividing into two fractions according to the invention, it has surprisingly been found that one fraction has a SiC powder with less than 5% by weight, preferably less than 2% by weight, more preferably less than 1% by weight of impurities, and the other fraction contains substantially all the remaining impurities. Here, the division into at least one "clean" fraction and at least one "contaminated" fraction with a higher impurity content is carried out by one or more classical separation processes, preferably dry fractionation processes such as sieving, screening or magnetic separation. Here, depending on the number of separation cuts in the process, several purified clean and contaminated fractions may be produced, which are combined at the end of the division / fractionation to form the two fractions according to the invention.
[0085] By dividing / fractionating into several fractions before combining, a purification factor can be determined for each fraction, and by combining the fractions, the difference in purification factors of two fractions according to the invention can be adjusted at the end of the method according to the invention.
[0086] Thus, by the method according to the invention, at least 95% by weight, preferably at least 98% by weight, more preferably at least 99% by weight, of silicon carbide is achieved in at least one fraction.
[0087] It has surprisingly been found that the metallic impurities melt during the temperature treatment and are therefore able to at least partially wet the SiC particles, so that after cooling the metallic impurities are able to form strong bonds with the SiC particles at the joints between adjacent SiC particles and between multiple SiC particles, the metallic impurities being present, for example, as metal silicides or ternary metal-Si-C compounds or ternary metal-Si-C alloys or mixtures thereof, so-called metallic interphases.
[0088] Surprisingly, the mechanical treatment achieves spalling or flaking of the metallic impurities, so that they can be separated from the SiC and, if necessary, further broken down during further mechanical treatment, thereby achieving a concentration of these metallic impurities in the mechanically treated, regenerated powdered silicon carbide fraction.
[0089] If the SiC waste as starting material for the production of purified silicon carbide powder does not contain carbon, it is advantageous to add carbon particles, for example in the form of carbon black, graphite powder or coke powder. Such addition can advantageously be such that the mass proportion of carbon is 0.3 to 0.5 times the free Si content and / or the Si content of SiO2.
[0090] The method according to the invention produces purified SiC powder which is industrially reusable, in particular for high-tech applications, and which can be produced in a simple and economical manner with high yields.
[0091] The SiC powder purified by the method according to the invention can then be fed to chemical refining.
[0092] According to the invention, the regenerated powdered silicon carbide is separated into two fractions, the regenerated silicon carbide powder in one fraction having a maximum of 5% by weight, preferably a maximum of 2% by weight, more preferably less than 1% by weight of impurities, and the remaining impurities being contained in the other fraction.
[0093] An advantage of the method according to the invention is that the mechanical treatment and fractionation of the powder can be carried out in known conventional processes which are known and in any case used, for example for the reprocessing of SiC powder used as an abrasive.
[0094] The purified silicon carbide powder according to the invention, which contains at least 98% by weight of SiC, preferably 99% by weight of SiC, and a maximum of 2% by weight of impurities, still has adhering residues of metal impurities on the surface of the silicon carbide powder particles. Surprisingly, after the method according to the invention, only a maximum of 2% by weight of impurities remains on the surface of the SiC powder particles.
[0095] After the temperature treatment according to the invention, surprisingly, SiC particles are formed with a unique structure for separating materials during the mechanical treatment according to the invention. The feature of these structures is that the metal impurities can be present in the form of metal interphases, which are concentrated and deposited on the surface of the silicon carbide powder particles and are usually very tightly bound to the surface of the SiC powder particles, so that mechanical separation of the majority of impurities, especially metal impurities, from the SiC powder particles into two or more fractions can be easily achieved. Such adhesion of impurities to the surface of SiC powder particles has not been observed so far. Similarly, it is surprising that the impurity structures attached to the surface of these SiC powder particles can be removed to a very high extent by relatively simple mechanical separation and / or physical treatment, so that high-purity to ultra-high-purity SiC powders can be produced with at least 98% by weight of SiC in one fraction.
[0096] Here, the impurities are essentially present in the form of islands of metal interphase deposited on the surface of the silicon carbide powder particles, mostly in the form of molten droplets. After the mechanical treatment and physical separation according to the present invention, the impurities that still remain are firmly bound to the surface of the SiC powder particles.
[0097] Advantageously, according to the invention, these impurities on the surface of the individual silicon carbide powder particles after the temperature treatment are substantially located on the flat and / or convex shaped parts of the surface of the silicon carbide powder particles. In this case, the contact angle of these impurities on the surface of the silicon carbide powder particles varies widely, but is usually in the range of 10 ° to 90 °.
[0098] Furthermore, it is also possible that impurities are arranged between the SiC powder particles as metallic interphases, which on the one hand are firmly bonded to the flat and / or convex morphology of the surface of the individual SiC powder particles and on the other hand are bonded to each other as metallic interphases, so that the gaps between the SiC powder particles or the joints between the SiC powder particles are filled. At these locations and / or grain boundaries, the metallic interphases form shapes that visually resemble weld seams in the shape of a fillet weld (flat weld seam, concave weld seam, convex weld seam).
[0099] The metallic interphases formed as impurities during the temperature treatment of the method according to the invention are characterized in that they are in particular silicides or carbides of the metals present. In particular, the method is directed to the production of the iron silicides Fe3Si (α2 phase), FeSi (ε phase), FeSi2 (ζ2 phase or Fe3Si7) and in particular the metastable Fe5Si3 (η phase). These silicides have a linear thermal expansion coefficient >6×10 in the range from 20 to 1400 °C. -6 It is generally 1 / K, which can be relatively easily separated from the particle surface of the silicon carbide powder and therefore forms the basis of the separation method according to the invention.
[0100] Besides the silicides mentioned above, ternary Fe-Si-C compounds may also be formed in small amounts. Other metallic impurities such as Ti, V, and Al may also be present in solution in the silicides and carbides, or may form solid solutions.
[0101] Surprisingly, mechanical processing of the temperature-treated SiC waste material results in relatively clean spalling of impurities from the SiC powder particles, both on the surface of the SiC powder particles and between the SiC powder particles, leaving essentially only the droplet-like melts deposited as islands of the metal interphase as impurities on the flat and / or convex surfaces of the silicon carbide powder particles. When the melts deposited as islands also spall completely or partially, fragments of these melts remain firmly attached to the flat and / or convex surfaces of the silicon carbide powder particles. The fracture of the firmly attached fragments has a typical shell-like fracture.
[0102] The SiC powder heat-treated according to the present invention contains SiC powder particles and substantially metallic impurities, and the proportion of secondary crystallites interpenetrating and bonded by metallic impurities is significantly higher in these SiC powders before the mechanical treatment according to the present invention than after the mechanical treatment. During the mechanical treatment, such interpenetrating secondary crystallites are individualized to become primary crystallites, and most of the attached metallic impurities are peeled off. According to the method according to the present invention, the impurities deposited in islands on the surface of the silicon carbide powder particles are firmly bonded to the SiC powder particles, and the contact angle of these metallic mixed phases with the flat and / or convex SiC powder particle surfaces is 10 to 90°. In the present invention, the contact angle of the metallic mixed phase with the SiC particle surface means the angle that is generated by the interfacial tension (Young's equation) at the phase boundary between the solid surface of the SiC particle, the molten liquid metallic mixed phase, and the surrounding gas atmosphere during the temperature treatment, and that is maintained even after the melt is solidified. Even when the metallic interphase is arranged as a joint and in the form of a seam between the SiC particles, there is a contact angle at the phase boundary between the SiC particle surface, the metallic interphase and the surrounding atmosphere, which is preferably measured by microscopic images, particularly preferably by image evaluation on images produced by scanning electron microscopy of ceramographically / metallographically prepared polished pieces of the heat-treated powder particles producing a cross section through the phase boundary.
[0103] The contact angle of the impurities that remain on the SiC particle surface in the form of the metal mixture and its fragments and are firmly attached can also be measured for the SiC powder mechanically treated and purified according to the present invention. From the fracture pattern, it is possible to easily distinguish the surface of the metal mixture and the fragments of the refined SiC powder that are fractured during mechanical treatment from the surface of the metal mixture of the temperature-treated SiC powder that is melted during heat treatment. In the case of the mechanically treated and purified SiC powder, only the contact angle at the phase boundary between the melted mixture and the surface of the SiC particle and the surrounding atmosphere is used when measuring the contact angle, and the angle between the fracture surface of the metal mixture fragments that is mechanically treated and the SiC particle and the surrounding surface is not used.
[0104] Such purified silicon carbide powders therefore differ from known regenerated SiC powders in which the impurities are primarily present separate from the SiC particles.
[0105] Thus, the purified silicon carbide powder according to the present invention can be distinguished from known reclaimed powders by optical and electron microscopy such as SEM, TEM or SEM-EDX.
[0106] Similarly, after the mechanical treatment of the SiC particles after the temperature treatment, in particular the crushing, according to the invention, characteristic fracture points and fracture surfaces are formed in the SiC powder particles treated according to the invention, which can be easily detected by the above-mentioned inspection method. These typical fracture points and fracture surfaces of the impurities formed according to the invention are unique characteristics according to the invention of the purified silicon carbide powder.
[0107] Since the silicon carbide powder particles present by the method according to the invention are mostly broken down at the grain boundaries of the individual SiC particles, particle individualization is also possible.
[0108] A particular advantage of the solution according to the invention is that the higher the amount of impurities in the SiC waste, the better the removal and clear separation of the molten impurities can be achieved.
[0109] The present invention will now be described in more detail with reference to some examples.
[0110] Example 1 SiC powder as a by-product of primary crushing of SiC, comprising 91.8% by mass of SiC and 1.0% by mass of C. 遊離 10 kg of SiC powder containing 1.3% by weight of C, 1.8% by weight of Si, 3.7% by weight of SiO2, 0.4% by weight of Fe, and impurities including Al, V, Ti and Ca in the range of >300 ppm each, are mixed with 180 g of coke powder, 100 g of Si and 40 g of Fe. The powder mixture has an average grain size of 9.5 μm as measured by laser diffraction. The bulk density of the powder mixture is 0.6 g / cm. 3The powder mixture is filled into a graphite crucible and compressed at 50 MPa using a pressure plunger. The crucible is heated in a protective gas furnace under argon atmosphere at 8 K / min up to 2500 °C and held there for 60 min at 2500 °C, with the heating rate reduced to 3 K / min from 1200 °C to 2000 °C. During the entire temperature treatment, a 20 l / h Ar gas flow is passed around the graphite crucible. Furthermore, carbon monoxide (CO) and silicon monoxide (SiO) emanating from the protective gas furnace are evacuated.
[0111] Cooling is carried out at a rate of 2.5 K / min overall. After cooling, the powdered crucible contents are treated in an air mill with 0.1 MJ / kg and, after a sorting step, are divided into three powders with particle sizes <10 μm, 10-60 μm and >60 μm. The SiC powder before mechanical treatment has a SiC content of 97.8% by mass, and in particular the metallic impurities are present in concentrations of the same order of magnitude as in the starting powder. After mechanical treatment in the air mill, the powder with a particle size >60 μm has a SiC content of 99.1% by mass. The Si and SiO2 contents are each 0.22% by mass and C 遊離 The content of Cu was 0.12 wt%, the content of Fe was 0.16 wt%, and the contents of other metallic impurities were all clearly <100 ppm, respectively. In the other two combined powders, 8.6 times the amount of impurities was detected.
[0112] The average particle size of the "clean" fraction after heat treatment and mechanical refining is 92.7 μm. These particles are therefore on average 9.75 times larger than the starting material introduced into the protective gas furnace.
[0113] As a result of the process according to the invention, the "clean" fraction has a mass fraction of 81% by weight.
[0114] Before mechanical treatment, the heat-treated powder contains a large number of secondary particles, with impurities accumulating at the junctions of the secondary particles. After mechanical treatment, the "clean" fraction contains almost exclusively primary particles. These particles have islands or fragmentary islands of metal melt, mainly composed of Fe5Si3, present on the convex parts of the particle surface and in the places where the secondary particles have reverted back to primary particles due to the applied mechanical force. The remaining secondary particles have impurities at the junctions of the interpenetrating interparticle aggregates. These impurities were detected by SEM to be present firmly attached to the SiC particles. In the contaminated fraction, the impurities are present in the form described herein as well as in powder form.
[0115] Example 2 A SiC powder as a by-product of SiC processing, containing 95.8% SiC and 1.5% C. 遊離 10 kg of SiC powder containing 0.2%, 1.2% Si, 1.2% SiO2, 1.4% Fe and impurities including Al, V, Ti and Ca in the range of >100 ppm are mixed with 80 g of coke powder. The powder mixture has an average grain size of 41.5 μm as measured by laser diffraction. The powder mixture introduced into the crucible has a mass of 1.3 g / cm after the compaction step. 3 The crucible is heated in a protective gas furnace under argon atmosphere at a negative pressure of 70000 Pa at 5 K / min to 2000 ° C, then at 6 K / min to 2300 ° C and held at this temperature for 180 min. During the entire temperature treatment, a 0.5 l / h Ar gas flow is passed around the graphite crucible. In addition, carbon monoxide (CO) and silicon monoxide (SiO) generated from the protective gas furnace in the temperature range of 1200 ° C - 2000 ° C are evacuated.
[0116] Cool to room temperature at 2 K / min. In the range of 1200°C to 800°C, cool at a rate of 8 K / min.
[0117] After cooling and before mechanical treatment, the SiC powder has a SiC content of 96.1% by weight. There is no change in the amount of metallic impurities present.
[0118] The powdered crucible contents are milled at 0.3 MJ / kg and, after sieving, divided into five powders with particle sizes <40 μm, 40-63 μm, 63-125 μm, 125-250 μm and >250 μm. The powders with particle sizes <40 and 40-63 μm are then mixed into one fraction, and the powders with particle sizes 63-125 μm, 125-250 and >250 μm are mixed into a second fraction. The "clean" fractions are the fractions with particle sizes 63-125 μm, 125-250 μm and >250 μm and have a SiC content of 98.8% SiC. The Si and SiO2 contents are each 0.2% and the C 遊離 The content of Ca was 0.14%, the content of Fe was 0.25%, and the contents of all other metallic impurities could be significantly reduced to <50 ppm. The "contaminated" fractions with particle sizes <40 μm and 40-63 μm contained 13.8 times more impurities than the "clean" fraction.
[0119] The average particle size of the "clean" fraction after heat treatment and mechanical refining is 100.4 μm. These particles are therefore on average 2.4 times larger than the starting material introduced into the protective gas furnace.
[0120] As a result of the process according to the invention, the "clean" fraction has a mass fraction of 82.5% by weight.
[0121] Before mechanical treatment, the heat-treated powder contains many secondary particles, with impurities accumulating at the junctions of the secondary particles. After mechanical treatment, the "clean" fraction contains almost only primary particles. In these particles, fragments of the metal melt consisting of Fe3Si and Fe5Si3 are present on the flat and convex parts of the particle surface and in the places where the secondary particles have reverted back to primary particles due to the applied mechanical force. The remaining secondary particles contain impurities with the same silicides at the junctions of the interpenetrating interparticle aggregates. These impurities are detected by SEM-EDX to be present firmly attached to the SiC particles. In the "contaminated" fraction, the impurities are present in the form described here as well as in powder form.
[0122] Example 3 10 kg of dust-like SiC powder as a by-product of SiC processing, which is composed of 98.5% by mass of SiC and 10 kg of dust-like SiC powder as a by-product of SiC processing 遊離 The powder contains 0.3% by weight of Na, 0.6% by weight of Si, 0.4% by weight of SiO2, 0.1% by weight of Fe, and impurities including Al, V, Ti, and Ca in the range of >100 ppm. 20 g of Fe is mixed into the powder. The powder mixture has an average particle size of 16.4 μm as measured by laser diffraction. The powder bulk is placed in a crucible and heated to >1.2 g / cm using a vibrating plate. 3 The crucible is heated in a furnace under nitrogen atmosphere at 5 K / min under a negative pressure of 0.9 bar with a nitrogen flow rate of 10 l / min to 1800 °C and from there at 3 K / min to 2400 °C. It is kept at 2400 °C for 100 min.
[0123] Cooling is carried out at a rate of 10 K / min.
[0124] After cooling, the powdered contents of the crucible were milled at 1 MJ / kg and then precipitated to a density of 2.5-3.9 g / cm. 3 It is divided into three types of powder.
[0125] The SiC powder before mechanical treatment has a SiC content of 99.5 mass %, and metal impurities in particular are present at concentrations on the same order as in the starting powder.
[0126] After mechanical processing in a mill, the density is 3.2 g / cm 3 The powder of this embodiment has 99.8% by weight of SiC and therefore forms a "clean" fraction. The content of Si is 0.03% by weight, the content of SiO2 is 0.02% by weight and the content of C is 0.02% by weight. 遊離 The content of A was 0.11 mass%, the content of Fe was 0.02 mass%, and the contents of other metal impurities were all obviously reduced to <20 ppm.
[0127] Density is 2.5g / cm 3 of powder and density is 3.9g / cm 3 This powder is combined with the "contaminated" fraction, which contains 10.4 times the amount of impurities as the "clean" fraction.
[0128] The average particle size of the clean fraction after heat treatment and mechanical refining is 59.7 μm. These particles are therefore on average 3.6 times larger than the starting material introduced into the protective gas furnace.
[0129] As a result of the process according to the invention, the "clean" fraction has a mass fraction of 84% by weight.
[0130] Before mechanical treatment, the heat-treated powder contains a large number of secondary particles, with impurities accumulating at the junctions of the secondary particles. After mechanical treatment, the "clean" fraction contains almost exclusively primary particles. In these particles, islands of metallic melt consisting of Fe5Si3 are present in the convex parts of the particle surface and in the places where the secondary particles have reverted to primary particles due to the applied mechanical force. The remaining secondary particles contain impurities at the junctions of the interpenetrating interparticle aggregates. These impurities were detected by SEM to be present in a state of being firmly attached to the SiC particles. The metallic impurities have a contact angle of 30-75° with the SiC particle surface, as revealed by image analysis evaluation of polished sections of the powder particles. In the "contaminated" fraction, the impurities are present in the form described herein as well as in powder form.
[0131] Example 4 A dust-like SiC powder as a by-product of SiC processing, comprising 97.5% by mass of SiC and 1.5% by mass of C. 遊離 10 kg of SiC powder containing 0.4% by weight of SiC, 0.6% by weight of Si, 0.5% by weight of SiO2, 0.2% by weight of Fe, and impurities including Al, V, Ti, and Ca in the range of >100 ppm are mixed with 100 g of iron powder and 60 g of Si powder. The powder mixture has an average grain size of 16.4 μm as measured by laser diffraction. The bulk density of the powder mixture is 1 g / cm. 3 The powder mixture is loosely packed into a graphite crucible, which is heated in a furnace under vacuum at 7.5 K / min to 2050°C and held there for 270 min at 2050°C.
[0132] Cooling is carried out at a rate of 10 K / min.
[0133] After cooling, the powdered crucible contents are milled at 0.2 MJ / kg and split into two fractions due to the difference in surface potential in an electric field.
[0134] The SiC powder before mechanical treatment has a SiC content of 98.3%, and metal impurities in particular are present at concentrations on the same order as in the starting powder.
[0135] After mechanical processing in a mill, the "clean" fraction has 99.2% by weight of SiC. In the clean fraction, the contents of Si and SiO2 are 0.3% and 0.2% by weight, respectively, and C 遊離 The content of 0.2 wt.%, the content of Fe was 0.1 wt.%, and the contents of all other metallic impurities could be clearly reduced to <100 ppm. The "contaminated" fraction contained 9.6 times more impurities than the "clean" fraction.
[0136] The average particle size of the "clean" fraction after heat treatment and mechanical refining is 33 μm. These particles are therefore on average twice as large as the starting material introduced into the protective gas furnace.
[0137] As a result of the process according to the invention, the "clean" fraction has a mass fraction of 87% by weight.
[0138] Before mechanical treatment, the heat-treated powder contains many secondary particles, with impurities accumulated at the junctions of the secondary particles. After mechanical treatment, the "clean" fraction contains almost exclusively primary particles. These particles have islands of metallic melt consisting of Fe5Si3, FeSi, and FeSi2 at the convex portions of the particle surface and at the points where the secondary particles have reverted back to primary particles due to the applied mechanical force. The remaining secondary particles have impurities at the junctions of the interpenetrating interparticle aggregates. These impurities were detected by TEM to be present firmly attached to the SiC particles. In the "contaminated" fraction, the impurities are present in the form described herein as well as in powder form.
[0139] Example 5 A powdered SiC powder as a by-product of SiC raw material production, comprising 92.6% by mass of SiC and 1.0% by mass of C. 遊離 10 kg of SiC powder containing 2.75% by weight of SiC, 0.1% by weight of Si, 3.5% by weight of SiO2, 0.2% by weight of Fe, and impurities including Al, V, Ti, and Ca in the range of >400 ppm are mixed with 150 g of sand and 25 g of graphite powder. The powder mixture has an average grain size of 100 μm as measured by laser diffraction. The powder mixture is loosely packed into a graphite crucible and then packed in a 100 g / cm3 powder. 3 The crucible is heated in a protective gas furnace under argon at 5 K / min to 1900 °C, adjusting the pressure to a negative pressure of 70000 Pa. At 1900 °C, this temperature is maintained for 180 min.
[0140] Cooling is carried out at a rate of 25 K / min.
[0141] After cooling, the powdered contents of the crucible are milled at 0.1 MJ / kg and separated into three powders with particle sizes of <20 μm, 20-70 μm, and >70 μm using cyclones connected in series.
[0142] The SiC powder before mechanical treatment had a SiC content of 98.3 mass %, and metal impurities in particular were present at concentrations on the same order as in the starting powder.
[0143] After mechanical processing in a mill, the powder as the "clean" fraction with a particle size of >70 μm has a SiC content of 98.5% by mass. The Si and SiO2 contents are 0.1% and 0.1% by mass, respectively, and C 遊離 The content of was 1 mass%, the content of Fe was 0.1 mass%, and the contents of other metal impurities were all obviously reduced to <200 ppm.
[0144] Powders with particle sizes <20 μm and those with particle sizes between 20 and 70 μm were combined to form the "contaminated" fraction, which contained 2.3 times the amount of impurities as the "clean" fraction.
[0145] The average particle size of the "clean" fraction after heat treatment and mechanical refining is 125 μm. These particles are therefore on average 1.25 times larger than the starting material introduced into the protective gas furnace.
[0146] As a result of the process according to the invention, the "clean" fraction has a mass fraction of 90% by weight.
[0147] Before mechanical treatment, the heat-treated powder contains many secondary particles, with impurities accumulating at the junctions of the secondary particles. After mechanical treatment, the "clean" fraction contains almost exclusively primary particles. These particles have islands of metallic melt composed of silicon and vanadium carbides and silicides on the convex parts of the particle surface and in the places where the secondary particles have reverted back to primary particles due to the applied mechanical force. The remaining secondary particles have impurities at the junctions of the interpenetrating interparticle aggregates. These impurities were detected by SEM-EDX to be present firmly attached to the SiC particles. In the "contaminated" fraction, the impurities are present in the form described herein as well as in powder form.
Claims
1. A method for separating impurities from silicon carbide, comprising the steps of: 50 % of SiC powder, the SiC powder comprising at least 50% by weight of SiC with a particle size of 0.5-1000 μm and having a minimum content of 0.1% by weight of iron and 0.1% by weight of metallic silicon, is subjected to a temperature treatment at a temperature of 1400-2600° C. under vacuum or a non-oxidizing atmosphere, cooled, mechanically treated by application of mechanical shocks and physically separated according to particle size, particle shape, particle density and / or physical and / or chemical surface properties of the particles, and then the physically separated SiC powder is divided into two fractions, in one of which the mass of impurities is at least twice that of the other fraction.
2. 2. The process according to claim 1, wherein in one fraction the mass of impurities is at least 10 times, preferably at least 20 times, that in the other fraction.
3. The method of claim 1 , wherein the powdered SiC waste comprises at least 75% by weight of SiC, advantageously 80% by weight of SiC, even more advantageously 85% by weight of SiC, even more advantageously 90% by weight of SiC.
4. Average particle size d measured by laser diffraction method 50 2. The method according to claim 1, wherein a powdered SiC waste material is used, the powdered SiC waste material containing at least 50% by weight of SiC having a diameter of 0.5 to 500 μm.
5. Average particle size d measured by laser diffraction method 50 2. The method according to claim 1, wherein a powdered SiC waste is used, the powdered SiC waste containing at least 50% by weight of SiC having a diameter of >500-1000 μm.
6. Average particle size d measured by laser diffraction method 50 2. The method according to claim 1, wherein the powdered SiC waste, which contains at least 50% by weight of SiC with a size >500-1000 μm, is subjected to a temperature treatment at a temperature of 1400-<2000° C.
7. Average particle size d measured by laser diffraction method 50 2. The method according to claim 1, wherein a powdered SiC waste is used, which contains at least 50% by weight of SiC having a size of 0.5 to 1000 μm and has a content of 0.5 to 5.0% by weight of iron and 0.5 to 5.0% by weight of metallic silicon.
8. The method of claim 1, wherein the temperature treatment of the SiC waste is carried out at a temperature of 1400 to less than 2000°C.
9. The method of claim 1, wherein the temperature treatment of the SiC waste is carried out at a temperature between 2000 and 2600°C.
10. 2. The method according to claim 1, wherein the temperature treatment in vacuum or in a non-oxidizing atmosphere in the heating step is carried out in the temperature range from 1200° C. to less than 1400° C. and from 1400° C. to 1800° C. with a heating rate of 8 K / min or less.
11. 2. The method of claim 1, wherein the temperature treatment in vacuum or in a non-oxidizing atmosphere in the heating step is carried out above 1800° C. with a heating rate of up to 5 K / min.
12. 2. The method according to claim 1, wherein the temperature treatment in a vacuum or in a non-oxidizing atmosphere is carried out with a holding time at the maximum temperature of 10 to 300 minutes.
13. 11. The method according to claim 1 or 10, wherein the temperature treatment in a non-oxidizing atmosphere is carried out with an amount of non-oxidizing gas of 0.5 to 30 l / h.
14. 2. The method according to claim 1, wherein the temperature treatment in a vacuum or in a non-oxidizing atmosphere is carried out with discharge of gaseous reaction products.
15. The method of claim 1, wherein the powdered SiC is cooled at a cooling rate of 0.1 to 100 K / min.
16. 2. The method of claim 1, wherein the powdered SiC is cooled in the temperature range of 1200° C. to 800° C. at a cooling rate of 0.5 to 10 K / min.
17. 2. The method according to claim 1, wherein the mechanical treatment of the regenerated powdered SiC is carried out by mixing, grinding, preferably also by autogenous grinding, or by using eddy currents and / or ultrasound.
18. 18. The method according to claim 17, wherein the mechanical treatment is carried out with an energy input of 0.1 to 5 MJ / kg.
19. 2. The method of claim 1, wherein the separation according to particle size and / or particle shape is carried out by sieving, screening and / or cyclone processes.
20. 2. The method of claim 1, wherein the separation is performed using flotation, sedimentation, screening, centrifugation and / or cyclone processes due to the action of gravity on the particle density, or the separation is performed by flotation and / or cyclone processes depending on the particle density.
21. 2. The method of claim 1, further comprising separating a fraction containing at least 95% by weight of silicon carbide.
22. 22. The method of claim 21, further comprising separating into a fraction containing at least 98% by weight silicon carbide.
23. 22. The method of claim 21, further comprising separating into a fraction containing at least 99% by weight silicon carbide.
24. 2. The method of claim 1, wherein the impurities are substantially metallic impurities.
25. To remove impurities in the form of Si and / or C, carbon, preferably carbon black, graphite and / or coke powder, and / or silicon and / or silicon dioxide (SiO 2 2. The method of claim 1, further comprising adding, during said temperature treatment, a substantially stoichiometric composition of SiC.
26. 1. A silicon carbide powder comprising SiC powder particles and substantially metallic impurities in the form of a metal interphase, the powder having metallic impurities on flat and / or convex surfaces of the silicon carbide powder particles, the metallic impurities being located in islands or in interstices or junctions between silicon carbide powder particles and firmly bonded to one or more silicon carbide powder particles, the contact angle of the impurities being between 10° and 90°.
Citation Information
Patent Citations
Preparation of sic in high purity
JP1983009807A
Production of fine power of high purity silicon carbide
JP1987027316A
Silicon carbide sintered compact
JP2000169246A
Silicon carbide powder and its production
JP2000351614A
Method of manufacturing silicon carbide from silicon waste
JP2010173916A