Printing ink composition, laminate, and packaging material
A printing ink composition with a binder resin, rosin derivative, and phosphate ester chelating agent addresses alkali releasability and yellowing resistance issues, enhancing the stability and physical properties of printed layers in packaging materials.
Patent Information
- Application Number
- JP2024052904
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing printing ink compositions used in packaging materials face challenges with insufficient alkali releasability, yellowing resistance when adhesive tapes are applied, and stability issues, particularly when recycled plastic films are reused, leading to deterioration in hue and physical properties.
A printing ink composition comprising a binder resin, a rosin derivative with a high acid value, and a chelating agent with a phosphate ester structure, along with optional components, is formulated to enhance alkali releasability, yellowing resistance, and stability, while maintaining adhesion, blocking resistance, and heat resistance.
The composition achieves high alkali releasability, excellent yellowing resistance, and improved stability, ensuring the printed layer meets the physical requirements for packaging materials, including adhesion, blocking resistance, and heat resistance.
Smart Images

Figure 0007562896000011 
Figure 0007562896000001 
Figure 0007562896000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a printing ink composition, a laminate, and a packaging material. [Background technology]
[0002] Packaging materials using a substrate such as a plastic film for packaging foods, daily necessities, etc. are printed on the substrate with printing inks such as gravure ink for the purpose of decoration and securing necessary physical properties. For example, a simple printed matter called a surface printing method, in which the substrate is printed on the front side and the back side of the substrate that comes into contact with the contents is not printed, is generally used. As the printing ink used for surface printing, a printing ink made of a mixture of polyamide resin and nitrocellulose resin is generally used to achieve the required design and various physical properties, and various additives are further blended into the printing ink as necessary.
[0003] As the additive, a chelating agent is generally and widely used. It is known that when a printing ink contains a chelating agent, the adhesion, heat resistance, and blocking resistance of the resulting printed layer to the substrate are improved. As a chelating agent, a compound containing titanium or zirconium, which is a transition metal belonging to Group 4 of the periodic table, is widely used. Among them, a chelating agent containing titanium is widely used in terms of cost, etc.
[0004] In recent years, there has been a demand for the reuse of plastic films as a measure against environmental problems, including the problem of microplastics. However, when plastic films used in packaging materials are reused, contamination with printing ink can cause deterioration of the color of the recycled plastic film and deterioration of its physical properties. Therefore, when the plastic films are reused, they must be treated with an alkaline solution to remove the printing ink from the plastic films in advance.
[0005] For example, Patent Document 1 discloses a printing ink composition for alkali release that contains a polyamide resin, a nitrocellulose resin, and a chelating agent having an acetylacetone structure. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2022-080724 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the alkali releasability of the printed layer formed using the printing ink composition for alkali releasability proposed in Patent Document 1 is not necessarily sufficient. Therefore, strict conditions are required for the alkali releasability, and further improvements are required to enable the alkali releasability easily under milder conditions.
[0008] As the titanium-containing chelating agent, chelating agents having an acetylacetone structure or an ethyl acetoacetate structure are widely used. These chelating agents react with components contained in adhesive tapes and the like to produce colored compounds, which cause the printed layer at the portion where the adhesive tape is applied to turn yellow, resulting in poor appearance. Since adhesive tapes are often applied to the printed layer of packaging materials, further improvements are required to improve the poor appearance. Furthermore, it has been found that there is also a problem that the stability of the printing ink composition is impaired depending on the type of chelating agent.
[0009] The present invention aims to provide a printing ink composition that has high alkali release properties, can provide a printed layer that has excellent yellowing resistance when an adhesive tape is applied, and is highly stable. In addition, the present invention aims to provide a printing ink composition that can provide a printed layer that satisfies various physical properties required for a packaging material. The physical properties are adhesion to a substrate, blocking resistance, heat resistance, and wet friction resistance. Another objective of the present invention is to provide a laminate having a printed layer formed using the printing ink composition, and a packaging material including the laminate. [Means for solving the problem]
[0010] The present invention has the following aspects. [1] A printing ink composition containing a binder resin (A), a rosin derivative (B), and a chelating agent (C), wherein the binder resin (A) contains a polyamide resin (A1) and a nitrocellulose resin (A2), the rosin derivative (B) has an acid value of 150 mgKOH / g or more, the chelating agent (C) has a phosphate ester structure, the content of the rosin derivative (B) in terms of solid content is 1 to 15 mass% relative to the total mass of the solid content of the printing ink composition, and the content of the chelating agent (C) in terms of solid content is 0.5 to 10 mass% relative to the total mass of the solid content of the printing ink composition. [2] The printing ink composition according to [1], wherein the content of the binder resin (A) in terms of solid content is 25 to 75 mass % based on the total mass of the solid content of the printing ink composition. [3] The printing ink composition according to [1] or [2], wherein a mass ratio of the solid content of the polyamide resin (A1) to the solid content of the nitrocellulose resin (A2) is 1.5 to 9. [4] The printing ink composition according to any one of [1] to [3], wherein the rosin derivative (B) has an acid value of 150 to 280 mg KOH / g. [5] The printing ink composition according to any one of [1] to [4], wherein the polyamide resin (A1) has a weight average molecular weight of 30,000 or less. [6] The printing ink composition according to any one of [1] to [5], wherein the type and viscosity symbol of the nitrocellulose resin (A2) as defined by a viscosity measurement in accordance with JIS K 6703:1995 are H1 / 4, H1 / 2, H1 or H2. [7] The printing ink composition according to any one of [1] to [6], further comprising a chlorinated polyolefin resin. [8] The printing ink composition according to any one of [1] to [7], which is for gravure printing. [9] A laminate comprising a plastic film and a printed layer formed on at least one surface of the plastic film using the printing ink composition described in any one of [1] to [8].
[10] A packaging material comprising the laminate described in [9]. Effect of the Invention
[0011] According to the present invention, a printing ink composition can be provided that has high alkali release properties, can provide a printed layer that exhibits excellent resistance to yellowing when an adhesive tape is applied, and is highly stable. Furthermore, a printing ink composition can be provided that can provide a printed layer that satisfies various physical properties required for a packaging material. The physical properties are adhesion to a substrate, blocking resistance, heat resistance, and wet friction resistance. Furthermore, a laminate having a printed layer formed using the printing ink composition, and a packaging material including the laminate can also be provided. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various forms without departing from the spirit of the present invention. In this specification, the contents of the binder resin (A) and the rosin derivative (B) are all calculated on a solid content basis. "Solid content" refers to the components contained in the printing ink composition excluding volatile media such as solvents, and is the components that will ultimately form the printed layer, and is specifically measured in accordance with JIS K 5601-1-2:2008. The weight average molecular weight of the resin is a weight average molecular weight converted into a standard polystyrene molecular weight and is measured by gel permeation chromatography (GPC).
[0014] <Printing ink composition> A printing ink composition according to one embodiment of the present invention contains a binder resin (A), a rosin derivative (B) having an acid value of 150 mgKOH / g or more, and a chelating agent (C) having a phosphate ester structure. The printing ink composition may further contain components (optional components) other than the binder resin (A), the rosin derivative (B) and the chelating agent (C) as necessary, as long as the effects of the present invention are not impaired.
[0015] <Binder resin (A)> The binder resin (A) used in the present invention contains a polyamide resin (A1) and a nitrocellulose resin (A2).
[0016] (Polyamide resin (A1)) The polyamide resin (A1) may be a thermoplastic polyamide which is a polycondensation product of a polybasic acid and a polyamine and is soluble in an organic solvent. Examples of polybasic acids include adipic acid, sebacic acid, azelaic acid, phthalic anhydride, isophthalic acid, suberic acid, glutaric acid, fumaric acid, pimelic acid, oxalic acid, malonic acid, succinic acid, maleic acid, terephthalic acid, 1,4-cyclohexyldicarboxylic acid, trimellitic acid, dimer acid, hydrogenated dimer acid, etc. In addition to these polybasic acids, monocarboxylic acids such as acetic acid, propionic acid, lauric acid, palmitic acid, benzoic acid, and cyclohexanecarboxylic acid can also be used in combination. Examples of the polyamine include polyamines. Examples of the polyamine include aliphatic diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, and methylaminopropylamine; aliphatic polyamines such as diethylenetriamine and triethylenetetramine; alicyclic polyamines such as cyclohexylenediamine and isophoronediamine; and aromatic polyamines such as xylylenediamine, phenylenediamine, and diaminodiphenylmethane. In addition to these polyamines, primary or secondary monoamines such as n-butylamine, octylamine, dielamine, monoethanolamine, monopropanolamine, diethanolamine, and dipropanolamine can also be used in combination.
[0017] Specific examples of polyamide resin (A1) include thermoplastic polyamide resins using fatty acids made from vegetable materials and polymerized fatty acids made from them. Representative examples of fatty acids made from vegetable materials include tall oil, soybean oil, coconut oil, palm oil, cashew nut oil, rice bran, and cacao beans. On the other hand, examples of polymerized fatty acids include dimer acids and hydrogenated dimer acids obtained by reducing dimer acids with hydrogen. These polyamide resins (A1) may be used alone or in combination of two or more.
[0018] The weight average molecular weight (hereinafter also referred to as "Mw") of the polyamide resin (A1) is preferably 30,000 or less, more preferably from 500 to 30,000, further preferably from 700 to 20,000, and particularly preferably from 1,000 to 15,000. When the Mw of the polyamide resin (A1) is equal to or greater than the lower limit, the abrasion resistance and heat resistance of the resulting printed layer are likely to be improved. When the Mw of the polyamide resin (A1) is equal to or less than the upper limit, the solubility is likely to be improved, and the adhesion to the substrate, alkali releasability, and gloss of the resulting printed layer are likely to be improved.
[0019] The acid value of the polyamide resin (A1) is preferably 30 mgKOH / g or less, more preferably 20 mgKOH / g or less, and particularly preferably 15 mgKOH / g or less. When the acid value of the polyamide resin (A1) is the above upper limit or less, the stability of the printing ink composition is likely to be improved. The acid value of the polyamide resin (A1) can be measured by a neutralization titration method in accordance with JIS K 0070:1992. The amine value of the polyamide resin (A1) is preferably 30 mgKOH / g or less, more preferably 20 mgKOH / g or less, particularly preferably 15 mgKOH / g or less. When the amine value of the polyamide resin (A1) is the above upper limit or less, printability is likely to be improved.
[0020] The softening point of the polyamide resin is preferably 80 to 160° C., more preferably 85 to 150° C., and particularly preferably 90 to 140° C. When the softening point of the polyamide resin is equal to or higher than the lower limit, the heat resistance and blocking resistance of the resulting printed layer are likely to be improved. When the softening point of the polyamide resin is equal to or lower than the upper limit, the adhesion to the substrate is likely to be improved. The softening point of the polyamide is a value measured in accordance with JIS K 2207:2006.
[0021] As the polyamide resin, commercially available products may be used. Commercially available examples of polyamide resins include the "Leomaide Series" manufactured by Kao Corporation, the "Newmide Series" manufactured by Harima Chemical Group, the "Tomide Series" manufactured by T&K Toka Corporation, the "Sunmide Series" manufactured by Air Products Japan Co., Ltd., and the "Vegichem Green Series" manufactured by Tsuno Foods Industry Co., Ltd.
[0022] (Nitrocellulose resin (A2)) The type and viscosity symbol of the nitrocellulose resin (A2) as defined by the viscosity measurement according to JIS K 6703:1995 are preferably H1 / 4, H1 / 2, H1, or H2, and more preferably H1 / 2, H1, or H2. If the viscosity symbol of the nitrocellulose resin (A2) is lower than H1 / 4, the abrasion resistance, heat resistance, and blocking resistance of the resulting printed layer are likely to decrease. If the viscosity symbol of the nitrocellulose resin (A2) is higher than H2, the adhesion to the substrate, kneading resistance, ink stability, and alkali release property of the resulting printed layer are likely to decrease. If the type of nitrocellulose resin is L, the compatibility with the printing ink composition is likely to decrease slightly. That is, if the type and viscosity symbol of the nitrocellulose resin (A2) are H1 / 4, H1 / 2, H1, or H2, the compatibility with the printing ink composition is likely to improve, and the stability of the printing ink composition is likely to improve. Furthermore, the resulting printed layer tends to have improved abrasion resistance, heat resistance, blocking resistance, adhesion to the substrate, kneading resistance, ink stability, and alkali release properties.
[0023] The types are defined according to the nitrogen content in the nitrocellulose. Nitrocellulose with a nitrogen content of 10.7% or more but less than 11.5% is classified as type L. Nitrocellulose, which has a nitrogen content between 11.5% and 12.2%, is classified as type H. The types and viscosity symbols are defined according to the time it takes for a specified steel ball to fall between the marked lines (fall time) in a nitrocellulose solution having a specified solid content concentration. In the case of nitrocellulose of the above type and viscosity symbol H1 / 8, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 25 mass % is 1.6 to 2.9 seconds. In the case of nitrocellulose of the above type and viscosity symbol H1 / 4, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 25% by mass is 3.0 to 8.9 seconds. In the case of nitrocellulose of the above type and viscosity symbol H1 / 2, the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 20% by mass is 3.0 to 4.9 seconds, or the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 25% by mass is 9.0 to 22.0 seconds. In the case of nitrocellulose of the above type and viscosity symbol H1, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 20 mass % is 5.1 to 9.0 seconds. In the case of nitrocellulose of the above type and viscosity symbol H2, the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 12.2% by mass is 1.5 to 2.5 seconds, or the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 20% by mass is 15.0 to 40.0 seconds. These nitrocelluloses (A2) may be used alone or in combination of two or more kinds.
[0024] As the nitrocellulose (A2), a commercially available product may be used. An example of a commercially available product of nitrocellulose (A2) is the nitrocellulose used in the Examples described below.
[0025] <Rosin derivative (B)> By including the rosin derivative (B) in the printing ink composition of this embodiment, detachment of the printed layer is easily promoted when the printed layer is detached with an alkaline solution or the like and the plastic film is reused. Examples of the rosin derivative (B) include rosin modified maleic acid resin, rosin modified fumaric acid resin, rosin modified phenolic resin, rosin ester, hydrogenated rosin, polymerized rosin, and terpene phenolic resin. These rosin derivatives (B) may be used alone or in combination of two or more.
[0026] The acid value of the rosin derivative (B) is 150 mgKOH / g or more, preferably 150 to 280 mgKOH / g, more preferably 160 to 270 mgKOH / g, and particularly preferably 170 to 260 mgKOH / g. When the acid value of the rosin derivative (B) is equal to or more than the lower limit, the alkali releasability is likely to be improved. When the acid value of the rosin derivative (B) is equal to or less than the upper limit, the ink stability of the printing ink composition and the water resistance of the resulting printed layer are likely to be improved. The acid value of the rosin derivative (B) can be measured by a neutralization titration method in accordance with JIS K 0070:1992. The printing ink composition of this embodiment may further contain a rosin derivative having an acid value less than the above lower limit for the purpose of further improving the adhesion and gloss of the resulting printed layer to the substrate.
[0027] The softening point of the rosin derivative (B) is preferably 80 to 150°C, more preferably 90 to 140°C, and particularly preferably 95 to 130°C. When the softening point of the rosin derivative (B) is equal to or higher than the lower limit, the blocking resistance and heat resistance of the resulting printed layer are likely to be improved. When the softening point of the rosin derivative (B) is equal to or lower than the upper limit, the adhesion of the resulting printed layer to the substrate is likely to be improved. The softening point of the rosin derivative (B) can be measured by the ring and ball method in accordance with JIS K 5601-2-2:1999.
[0028] As the rosin derivative (B), a commercially available product may be used. Commercially available rosin derivatives (B) include, for example, the "Harimac Series", "Hariphenol Series", "Hariestar Series", and "Haritac Series" manufactured by Harima Chemical Group Co., Ltd.; the "Pine Crystal Series", "Marquid Series", and "Tamanol Series" manufactured by Arakawa Chemical Industries Co., Ltd.; and the "Foral Series" manufactured by Eastman Chemical Company.
[0029] <Chelating Agent (C)> The chelating agent (C) is a chelating agent having a phosphate ester structure. The phosphate ester structure means a structure represented by O=P(OR)3. At least one of R is a metal atom, and the others may be a hydrocarbon group. The chelating agent having a phosphate ester structure is an organometallic compound having a structure in which a phosphate ester is bonded to a metal atom. By using a chelating agent having such a phosphate ester structure, it is possible to form a printing layer that has excellent alkali release properties and excellent resistance to yellowing when a pressure-sensitive adhesive tape is applied, compared with conventional chelating agents having an acetylacetone structure or an ethyl acetoacetate structure. As the metal atom, a metal atom of Group 4 of the periodic table, such as a titanium atom or a zirconium atom, is preferable. Among these, a chelating agent that is an organometallic compound having a structure in which a phosphate ester is bonded to a titanium atom is preferred, a chelating agent that is an organometallic compound having a structure in which a phosphate ester is bonded to two titanium atoms is more preferred, and n-butyl phosphate titanium is particularly preferred.
[0030] <Optional ingredients> Examples of the optional components include solvents, pigments, pigment derivatives, extender pigments, waxes, antiblocking agents, fatty acid amides, chelating agents, curing agents, antisettling agents, UV absorbers, antioxidants, antistatic agents, leveling agents, thickeners, defoamers, plasticizers, dispersants, flame retardants, stabilizers, etc. Examples of the optional components also include resins other than the polyamide resin (A1), the nitrocellulose resin (A2), and the rosin derivative (B). These optional components may be used alone or in combination of two or more.
[0031] (solvent) The solvent is preferably an organic solvent. Examples of the organic solvent include aromatic organic solvents such as toluene and xylene, aliphatic hydrocarbon organic solvents such as cyclohexane and methylcyclohexane, ketone organic solvents such as methyl ethyl ketone and methyl isobutyl ketone, ester organic solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, and isobutyl acetate, alcohol organic solvents such as methanol, ethanol, n-propanol, isopropanol, and n-butanol, and glycol ether organic solvents such as ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether.
[0032] Among them, organic solvents that do not substantially contain aromatic organic solvents such as toluene and xylene (non-toluene organic solvents) are preferred. That is, it is preferable from an environmental point of view that the organic solvent contained in the printing ink composition is a non-toluene organic solvent that does not substantially contain toluene. The organic solvent preferably contains an aliphatic hydrocarbon organic solvent, an ester organic solvent, and an alcohol organic solvent. The content of the aliphatic hydrocarbon organic solvent in the organic solvent is preferably 1 to 80 mass% based on the total organic solvent. The content of the ester organic solvent in the organic solvent is preferably 1 to 70 mass% based on the total organic solvent. The content of the alcohol organic solvent in the organic solvent is preferably 1 to 50 mass% based on the total organic solvent.
[0033] (wax) The wax is preferably a hydrocarbon wax. When the printing ink composition contains a hydrocarbon wax, the abrasion resistance of the resulting printed layer is likely to be improved. Examples of the hydrocarbon wax include polyethylene wax, Fischer-Tropsch wax, paraffin wax, microstalline wax, and polypropylene wax. Among them, polyethylene wax and Fischer-Tropsch wax are preferred. Examples of the polyethylene wax include high-density polymerized polyethylene, low-density polymerized polyethylene, oxidized polyethylene, acid-modified polyethylene, and special monomer-modified polyethylene. In addition, Fischer-Tropsch wax is a wax produced by the Fischer-Tropsch process using carbon monoxide and hydrogen as raw materials, and has a nearly saturated, unbranched, linear molecular structure. These hydrocarbon waxes may be used alone or in combination of two or more kinds.
[0034] The penetration (hardness) of the hydrocarbon wax at 25° C. as defined in JIS K 2207:2006 is preferably from 0.1 to 30, more preferably from 0.1 to 28, and particularly preferably from 0.1 to 25. When the penetration (hardness) of the hydrocarbon wax is equal to or less than the above upper limit, the abrasion resistance and printability of the resulting printed layer are likely to be improved.
[0035] (Chlorinated polyolefin resin) The printing ink composition of the present embodiment may contain other resins in addition to the polyamide resin (A1), the nitrocellulose resin (A2), and the rosin derivative (B). As the other resins, chlorinated polyolefin resins are preferred. When the printing ink composition contains a chlorinated polyolefin resin, the adhesion of the resulting printed layer to the substrate is likely to be improved. The chlorinated polyolefin resin is a resin in which at least a part of the hydrogen atoms in the polyolefin resin is replaced with a chlorine atom. As the polyolefin resin, a homopolymer or copolymer of an α-olefin-based unsaturated hydrocarbon such as polypropylene, poly-1-butene, or poly-4-methyl-1-pentene is preferred, and polypropylene is more preferred. The chlorinated polyolefin resin can be produced by polymerizing a monomer in which at least a part of the hydrogen atoms in the monomer for producing the polyolefin are replaced with a chlorine atom. These chlorinated polyolefin resins may be used alone or in combination of two or more kinds.
[0036] The Mw of the chlorinated polyolefin resin is preferably 3,000 to 100,000, more preferably 3,500 to 80,000, and particularly preferably 4,000 to 50,000. When the Mw of the chlorinated polyolefin resin is equal to or greater than the lower limit, the adhesion of the resulting printed layer to the substrate is likely to be improved. When the Mw of the chlorinated polyolefin resin is equal to or less than the upper limit, the compatibility in the printing ink composition is likely to be improved.
[0037] The chlorine content of the chlorinated polyolefin resin is preferably 15 to 60 mass%, more preferably 20 to 55 mass%, and particularly preferably 25 to 50 mass%. When the chlorine content of the chlorinated polyolefin resin is equal to or higher than the lower limit, the alkali release property and compatibility are likely to be improved. When the chlorine content of the chlorinated polyolefin resin is equal to or lower than the upper limit, the adhesion of the resulting printed layer to the substrate is likely to be improved. The chlorine content of the chlorinated polyolefin resin is the content of chlorine atoms relative to the total mass of the chlorinated polyolefin resin.
[0038] (Pigments) The printing ink composition of the present embodiment may contain a pigment. The printing ink composition may be a colorless printing ink composition that does not substantially contain a coloring material such as a pigment. In the case of a colorless printing ink composition, it can be used as a medium.
[0039] Examples of the pigment that can be used include extender pigments, inorganic pigments, and organic pigments. Examples of the extender pigments include silica, barium sulfate, kaolin, clay, calcium carbonate, and magnesium carbonate. Examples of the inorganic pigments include white pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, and silica; black pigments such as carbon black and iron black; and inorganic pigments of various colors such as aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine blue, Prussian blue, red iron oxide, yellow iron oxide, and zinc oxide.
[0040] Examples of organic pigments include soluble azo-based, insoluble azo-based, azo-based, phthalocyanine-based, halogenated phthalocyanine-based, anthraquinone-based, anthanthrone-based, dianthraquinonyl-based, anthrapyrimidine-based, perylene-based, perinone-based, quinacridone-based, thioindigo-based, dioxazine-based, isoindolinone-based, quinophthalone-based, azomethine azo-based, flavanthrone-based, diketopyrrolopyrrole-based, isoindoline-based, indanthrone-based, and other organic pigments.
[0041] <Content of each ingredient> The solid content of the binder resin (A) is preferably 20 to 80 mass%, more preferably 25 to 75 mass%, further preferably 28 to 72 mass%, and particularly preferably 30 to 70 mass%, based on the total mass of the solid contents of the printing ink composition. When the content of the binder resin (A) is equal to or more than the lower limit, the adhesion to the substrate, water resistance, abrasion resistance, and printability of the resulting printed layer are likely to be improved.When the content of the binder resin (A) is equal to or less than the upper limit, the heat resistance and blocking resistance of the resulting printed layer are likely to be improved.
[0042] The mass ratio of the solid content of the polyamide resin (A1) to the solid content of the nitrocellulose resin (A2) is preferably 1.3-10, more preferably 1.5-9, further preferably 1.6-5.7, and particularly preferably 1.9-4. When the mass ratio is equal to or greater than the lower limit, the stability of the printing ink composition and the adhesion and rubbing resistance of the resulting printed layer to the substrate tend to be improved.When the mass ratio is equal to or less than the upper limit, the blocking resistance, heat resistance, water resistance, and abrasion resistance of the resulting printed layer tend to be improved.
[0043] The solid content of the rosin derivative (B) is from 1 to 15 mass %, preferably from 1.5 to 12 mass %, particularly preferably from 2 to 10 mass %, based on the total mass of the solid contents of the printing ink composition. When the content of the rosin derivative (B) is equal to or more than the lower limit, the alkali releasability, adhesion to a substrate, and gloss of the resulting printed layer are likely to be improved.When the content of the rosin derivative (B) is equal to or less than the upper limit, the heat resistance, blocking resistance, and water resistance of the resulting printed layer are likely to be improved.
[0044] The solid content of the chelating agent (C) is from 0.5 to 10 mass %, preferably from 0.7 to 8 mass %, particularly preferably from 1 to 5 mass %, based on the total mass of the solid contents of the printing ink composition. When the content of the chelating agent (C) is equal to or more than the lower limit, the heat resistance, blocking resistance, and adhesion to the substrate of the resulting printed layer are likely to be improved. When the content of the chelating agent (C) is equal to or less than the upper limit, the stability of the printing ink composition, and the alkali release property and yellowing resistance of the resulting printed layer are likely to be improved.
[0045] The mass ratio of the solid content of the binder resin (A) to the solid content of the chelating agent (C) is preferably 6-45, more preferably 10-30, and further preferably 15-25. The mass ratio of the solid content of the rosin derivative (B) to the solid content of the chelating agent (C) is preferably 0.5-5, more preferably 1-4, and even more preferably 1.5-3. The mass ratio of the solid content of the binder resin (A) to the solid content of the rosin derivative (B) is preferably 3-30, more preferably 5-15, and even more preferably 8-10.
[0046] When the printing ink composition contains a hydrocarbon wax, the solid content of the hydrocarbon wax is preferably 0.5 to 3.5 mass%, more preferably 0.7 to 3 mass%, and particularly preferably 1 to 2.5 mass%, based on the total mass of the solid contents of the ink composition. When the content of the hydrocarbon wax is equal to or more than the above lower limit, the abrasion resistance of the resulting printed layer is likely to be improved.When the content of the hydrocarbon wax is equal to or less than the above upper limit, the printability and heat resistance of the resulting printed layer are likely to be improved.
[0047] When the printing ink composition contains a chlorinated polyolefin resin, the content of the chlorinated polyolefin resin is preferably 0.5 to 10 mass%, more preferably 1 to 7 mass%, and particularly preferably 2 to 5 mass%, based on the total mass of the solid content in the ink composition. When the content of the chlorinated polyolefin resin is equal to or more than the above lower limit, the adhesion of the resulting printed layer to the substrate is likely to be improved. When the content of the chlorinated polyolefin resin is equal to or less than the above upper limit, the alkali release property and blocking resistance of the resulting printed layer are likely to be improved.
[0048] The content of the solvent is preferably 10 to 90% by mass, more preferably 15 to 85% by mass, and even more preferably 20 to 82% by mass, based on the total mass of the printing ink composition. When the content of the solvent is equal to or more than the lower limit, the flowability of the printing ink composition is likely to be improved. When the content of the solvent is equal to or less than the upper limit, the printability is likely to be improved.
[0049] When the printing ink composition contains a pigment, the content of the pigment in the ink composition may be set to an amount sufficient to ensure the ink's coloring power, etc. Specifically, the content of the pigment in the printing ink composition may be 1 to 80% by mass relative to the total mass of the solid content in the ink composition.
[0050] The content of optional components other than the hydrocarbon wax, the chlorinated polyolefin resin, and the pigment is not particularly limited as long as it is within a range that does not impair the effects of the present invention. For example, the content is preferably 0 to 10 mass %, and more preferably 0 to 5 mass %, based on the total mass of the solid contents of the printing ink composition.
[0051] <Method for producing printing ink composition> The printing ink composition of this embodiment can be obtained, for example, by dissolving or dispersing the polyamide resin (A1), the nitrocellulose resin (A2), the rosin derivative (B), the chelating agent (C), and optional components as necessary in a solvent. The method for mixing the components is not particularly limited, and the components can be mixed by various methods. The method for dissolving or dispersing each component in a solvent is not particularly limited, and can be carried out using a known dispersing machine. Examples of dispersing machines include paint shakers, ball mills, attritors, sand mills, bead mills, dyno mills, roll mills, ultrasonic mills, and high-pressure collision dispersing machines. Dispersing treatment can be carried out once or multiple times using one type of dispersing machine, or dispersing treatment can be carried out multiple times using two or more types of dispersing machines in combination.
[0052] <Mechanism of action> The printing ink composition of the present invention contains a chelating agent (C) having a phosphoric acid ester structure. The rosin-based tackifier and phenol-based compounds contained in the adhesive component of the adhesive tape react with conventional chelating agents having an acetylacetone structure or an ethyl acetoacetate structure to produce colored compounds, whereas the reaction is unlikely to occur with a chelating agent having a phosphoric acid ester structure. In addition, the printing ink composition of the present invention contains a rosin derivative (B) having an acid value of 150 mg KOH / g or more, and therefore has excellent alkali releasability. The inventors of the present application have found that the alkali releasability is further improved by containing a chelating agent (C) having a phosphoric acid ester structure in addition to the rosin derivative (B). The following factors are considered to be the factors that contribute to the improvement of the alkali releasability by the chelating agent (C) having a phosphoric acid ester structure. First, the chelating agent is considered to be involved in crosslinking between the binder resins (A). In the case of the chelating agent (C) having a phosphoric acid ester structure, the crosslinking property is lower than that of the conventional chelating agents having an acetylacetone structure or an ethyl acetoacetate structure, and therefore the interaction due to the crosslinking of the binder resin (A) is weaker, which is considered to have improved the alkali releasability. Secondly, in the case of the chelating agent (C) having a phosphoric acid ester structure, the crosslinked structure of the binder resin (A) is more likely to be broken by hydrolysis than that of the conventional chelating agents having an acetylacetone structure or an ethyl acetoacetate structure. In other words, the crosslinked structure of the binder resin (A) is more likely to be broken, which is considered to have improved the alkali releasability.
[0053] <Laminate> An example of a laminate according to an embodiment of the present invention is shown in Fig. 1. Note that the dimensional ratio in Fig. 1 is different from the actual one for the sake of convenience of explanation. The laminate 10 in FIG. 1 is a printed matter comprising a plastic film 11 and a printed layer 12 provided on one surface of the plastic film 11. When the laminate is attached to a packaging container as a label, it is preferable that the plastic film 11 is attached on the inside (the side in contact with the packaging container) of the printed layer 12, that is, the printed layer 12 is attached on the outside.
[0054] <Plastic film> The type of plastic film 11 can be appropriately selected depending on the type of laminate 10, and is not particularly limited, but examples include polyolefin (e.g., polyethylene (PE), polypropylene (PP)), polyester (e.g., polyethylene terephthalate (PET)), polystyrene (PS), oriented polypropylene (OPP), polyamide (NY), etc. Plastic films made of these materials may be used alone or in combination of two or more types. At least one of the front surface (front side) and the back surface (back side) of the plastic film may be subjected to a surface treatment such as corona discharge treatment, plasma treatment, flame treatment, solvent treatment or the like, if necessary.
[0055] The plastic film 11 may have a single layer structure or a laminated structure. That is, the plastic film 11 may be a single layer film or a laminated film. When the plastic film 11 is a laminated film, it may be a structure in which two or more films of the same type are laminated, or a structure in which two or more films of different types are laminated.
[0056] The thickness of the plastic films 11, 21 is preferably from 5 to 100 μm, more preferably from 12 to 60 μm, and even more preferably from 12 to 50 μm.
[0057] <Print layer> In the laminate 10, the printed layer 12 is provided on one surface of the plastic film 11. The printed layer 12 is a printed layer formed using the printing ink composition of the present embodiment described above. The thickness of the printed layer 12 is preferably from 0.2 to 3.0 μm, more preferably from 0.3 to 2.0 μm, and even more preferably from 0.3 to 1.5 μm.
[0058] <Method of manufacturing laminate> The method for producing the laminate 10 in FIG. 1 includes a step of forming a printed layer 12 on one surface of a plastic film 11 using the printing ink composition of this embodiment. In the method for producing the laminate 10 in FIG. 1, for example, the printing ink composition of the present embodiment is applied onto one surface of a plastic film 11 and dried to form a printed layer 12. The printing ink composition may be applied onto one surface of the plastic film 11, dried to form the printed layer 12, and then further applied (overcoated) with the printing ink composition.
[0059] The method for applying the printing ink is not particularly limited, and any known application method can be used, such as gravure printing, flexographic printing, brush coating, gravure coater method, die coater method, bar coater method, spray coating method, flow coating method, dip coating method, spin coating method, curtain coating method, etc. Among these, gravure printing is preferred because of its high quality and productivity.
[0060] The drying method is not particularly limited as long as it can remove the solvent contained in the printing ink composition coated on one side of the plastic film 11, and examples thereof include reduced pressure drying, pressure drying, heat drying, and air drying. The heating temperature is preferably from 30 to 150°C, and more preferably from 40 to 120°C.
[0061] <Application> The laminate 10 is preferably used as a packaging material. As the packaging material, a packaging material for soft packaging is preferable. "Soft packaging" refers to a packaging material made of a material having flexibility, i.e., a flexible package, and is used for packaging food, daily necessities, etc. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0063] [Raw materials used] As the polyamide resin (A1), the compound shown below was used. A1-1: Kao Corporation, product name "Reomide S-8200", weight average molecular weight: 6,000. A1-2: Harima Chemical Group Co., Ltd., product name "Pneumide 872", weight average molecular weight: 1,500. A1-3: Kao Corporation, product name "Reomide S-6800", weight average molecular weight: 27,000. A1-4: Kao Corporation, product name "Reomaid SP-40N", weight average molecular weight: 31,000.
[0064] As the nitrocellulose resin (A2), the compound shown below was used. A2-1: Manufactured by Kimia, product name "RS1 / 2", type and viscosity code: H1 / 2. A2-2: Manufactured by Kimia, product name "RS2", type and viscosity code: H2. A2-3: Manufactured by Kimia, product name "RS1 / 8", type and viscosity code: H1 / 8. A2-4: Manufactured by Kimia, product name "RS7", type and viscosity code: H7.
[0065] As other binder resins (A3), the compounds shown below were used. A3-1: Urethane resin (manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., product name "Seikabond A-155").
[0066] As the rosin derivative (B), the compound shown below was used. B-1: Rosin modified special synthetic resin (Harima Chemicals, product name "Harimac AS-5", acid value 190mgKOH / g, softening point 160℃). B-2: Acid-modified ultra-light-colored rosin (manufactured by Arakawa Chemical Industries, product name "Pine Crystal KE-604", acid value 240 mg KOH / g, softening point 130°C). B-3: Maleated rosin (manufactured by Arakawa Chemical Industries, Ltd., product name "Marquid No. 33", acid value: 305 mg KOH / g, softening point: 145°C). B-4: Acid-modified ultra-light-colored rosin (manufactured by Arakawa Chemical Industries, Ltd., product name "Pine Crystal KR-120", acid value: 320 mg KOH / g, softening point: 120°C). B-5: Maleated rosin (manufactured by Arakawa Chemical Industries, Ltd., product name "Marquid 3002", acid value: 100 mg KOH / g, softening point: 175°C). B-6: Styrene-maleic acid half ester copolymer (Arakawa Chemical Industries, Ltd., product name "Alastar 700", acid value: 187 mg KOH / g, softening point: 112°C). Note that B-6 is a styrene-maleic acid half ester copolymer and is not a rosin derivative.
[0067] As the chelating agent (C), the compound shown below was used. C-1: A chelating agent in which the ligand is a phosphate ester (manufactured by Borica, product name "AP100", solid content: 65% by mass). C-2: A chelating agent in which the ligand is a phosphate ester (manufactured by Matsumoto Fine Chemical Co., Ltd., product name "Orgatics TC-1040", solid content: 75% by mass). C-3: A chelating agent in which the ligand is a phosphate ester (manufactured by Dorfketal, trade name "IAM", solid content: 70% by mass). C-4: A chelating agent whose ligand is acetylacetone (manufactured by Matsumoto Fine Chemical Co., Ltd., product name "Orgatics TC-100", solid content: 75% by mass). C-5: A chelating agent in which the ligand is acetylacetone (manufactured by Matsumoto Fine Chemical Co., Ltd., product name "Orgatics TC-401", solid content: 65% by mass). C-6: A chelating agent in which the ligand is ethyl acetoacetate (manufactured by Matsumoto Fine Chemical Co., Ltd., trade name "Orgatix TC-710", solid content: 63% by mass).
[0068] As optional components, the compounds shown below were used. Hydrocarbon wax (manufactured by Mitsui Chemicals, product name "Hiwax 220P", penetration: 13, melting point: 110℃). - Chlorinated polyolefin resin (manufactured by Nippon Paper Industries Co., Ltd., product name "Superchlorine 370M"). Fatty acid amide: Stearic acid amide (manufactured by Nippon Fine Chemicals, product name "Neutron S"). Pigment 1: Titanium oxide (manufactured by Teika Corporation, product name "Titanix JR-600A"). ·Pigment 2: CIPigment Blue 15:4 (manufactured by Dainichiseika Chemical Co., Ltd., product name "4933GN-EP"). Plasticizer (manufactured by Fuji Amido Chemical Co., Ltd., product name "Topsizer No. 3"). - Defoaming agent (manufactured by BYK Japan, product name "BYK-1751"). Solvent: A mixed solvent of methylcyclohexane:n-propyl acetate:isopropanol = 5:3:2 (mass ratio).
[0069] [Evaluation method] (Evaluation of alkali release properties) The prints obtained in the examples and comparative examples were cut to 3 cm x 3 cm, immersed in a 1.5% aqueous sodium hydroxide solution at 70°C, and stirred for 3 minutes. The prints were taken out of the aqueous sodium hydroxide solution, washed with water, and then visually observed, and the alkali release property was evaluated according to the following evaluation criteria. 3 to 5 was considered to be acceptable. 5: The ratio of the area of the detached printed layer to the total area of the printed layer is 95% or more. 4: The ratio of the area of the detached printed layer to the total area of the printed layer is 80% or more and less than 95%. 3: The ratio of the area of the detached printed layer to the total area of the printed layer is 50% or more and less than 80%. 2: The ratio of the area of the detached printed layer to the total area of the printed layer is 20% or more and less than 50%. 1: The ratio of the area of the detached printed layer to the total area of the printed layer is less than 20%.
[0070] (Evaluation of yellowing resistance) The printed surfaces of the prints obtained in the Examples and Comparative Examples were covered with cellophane tape (manufactured by Nichiban Co., Ltd.), and after one day at 20°C, the appearance was observed and the yellowing resistance of the printed layer was evaluated according to the following evaluation criteria. 3 to 5 was considered acceptable. 5: No yellowing was observed. 4: Slight yellowing was observed. 3: Slight yellowing was observed. 2: Yellowing was observed. 1: Severe yellowing was observed.
[0071] (Evaluation of Adhesion) After sticking cellophane tape (manufactured by Nichiban Co., Ltd.) to the printed surface of the prints obtained in the Examples and Comparative Examples, the cellophane tape was quickly peeled off, and the state of the printed layer remaining on the base film was visually confirmed and the adhesion was evaluated according to the following evaluation criteria: 3 to 5 is considered to be acceptable. 5: The ratio of the area of the peeled off printing layer to the total area of the printing layer is less than 5%. 4: The ratio of the area of the peeled off printing layer to the total area of the printing layer is 5% or more and less than 20%. 3: The ratio of the area of the peeled off printing layer to the total area of the printing layer is 20% or more and less than 50%. 2: The ratio of the area of the peeled off printing layer to the total area of the printing layer is 50% or more and less than 80%. 1: The ratio of the area of the peeled off printing layer to the total area of the printing layer is 80% or more.
[0072] (Evaluation of blocking resistance) The printed layer of the printed matter obtained in the Examples and Comparative Examples was superimposed on the unprinted surface of the same film as that used for the unprinted printed matter, and the resultant was subjected to a pressure of 4 kg / cm 2 A load of 10 ... 5: Ink absorption onto non-printed surfaces is less than 5% of the total area of the printed layer. 4: Ink absorption onto the non-printed surface is greater than 5% and less than 20% of the total area of the printed layer. 3: Ink absorption onto the non-printed surface is greater than 20% and less than 50% of the total area of the printed layer. 2: Ink absorption onto the non-printed surface is greater than 50% and less than 80% of the total area of the printed layer. 1: Ink absorption onto the non-printed surface is 80% or more of the total area of the printed layer.
[0073] (Evaluation of heat resistance) The printed surface of the printed matter obtained in the Examples and Comparative Examples was placed on a soft aluminum foil, and a heat seal tester (manufactured by Tester Sangyo, product name "TP-701-C Heat Seal Tester") was used to test the printed matter at 110 to 150°C and 2 kg / cm from the aluminum foil. 2 The printed layer was then peeled off, the state of the printed layer was checked, and the heat resistance was evaluated according to the following evaluation criteria. A score of 3 to 5 was considered acceptable. 5: The ink did not come off even when heated to 150℃. 4: When heated to 140°C, the ink did not come off, but when heated to 150°C, the ink did come off. 3: When heated to 130°C, the ink did not come off, but when heated to 140°C, the ink did come off. 2: When heated to 120°C, the ink did not come off, but when heated to 130°C, the ink did come off. 1: Ink removal occurred when heated below 120℃.
[0074] (Evaluation of wet friction resistance) The prints obtained in the examples and comparative examples were subjected to a wet rub resistance test using a Gakushin type rub fastness tester (manufactured by Tester Sangyo Co., Ltd., product name "AB-301"), in which the printed surface was rubbed back and forth 100 times with a black cloth (gold cloth No. 3) moistened with water and loaded with 200 gf. Thereafter, the appearance of the printed layer was visually confirmed, and the wet rub resistance was evaluated according to the following evaluation criteria. 3 to 5 was considered to be acceptable. 5: The area of the printed layer that has transferred to the black cloth (gold cloth No. 3) is less than 10%. 4: The percentage of the area of the printed layer that has transferred to the black cloth (gold cloth No. 3) is greater than 10% and less than 20%. 3: The percentage of the area of the printed layer that has transferred to the black cloth (gold cloth No. 3) is greater than 20% and less than 50%. 2: The area of the printed layer that has transferred to the black cloth (gold cloth No. 3) is 50% or more and less than 80%. 1: The area of the printed layer that has transferred to the black cloth (gold cloth No. 3) is 80% or more.
[0075] (Evaluation of ink stability) The printing ink compositions obtained in the Examples and Comparative Examples were allowed to stand at 20°C for one day, after which the state of the printing ink compositions was observed and the stability of the ink was evaluated according to the following evaluation criteria. 3 to 5 was considered acceptable. 5: No change. 4: Slightly thickened. 3: Thickened. 2: Significantly thickened and became creamy. 1: It solidified and became jelly-like.
[0076] [Examples 1 to 23, Comparative Examples 1 to 12] <Preparation of printing ink composition> According to the formulations shown in Tables 1, 3, 5, 7, and 9, polyamide resin (A1), nitrocellulose resin (A2), rosin derivative (B), chelating agent (C), solvent, and other optional components were mixed, and the resulting mixture was kneaded with a paint shaker to obtain a printing ink composition. The numbers in Tables 1, 3, 5, 7, and 9 indicate the amount of solid content except for the chelating agent (C). On the other hand, the amount of chelating agent (C) includes volatile content (the solid content concentration of chelating agent (C) is shown next to the type of chelating agent). A blank space means that the component was not mixed (amount mixed: 0 parts by mass). The ink stability of the obtained printing ink composition was evaluated. The results are shown in Tables 2, 4, 6, 8, and 10.
[0077] <Creating printed matter> The prepared printing ink composition was diluted with a mixed solvent of methylcyclohexane: n-propyl acetate: isopropanol = 5:3:2 (mass ratio) so that the viscosity at 25 ° C. measured using Zahn cup #3 was 16 seconds, and a printing ink was prepared. Using a gravure printing machine (manufactured by Matsuo Sangyo Co., Ltd., product name "K Printing Proofer") equipped with a Helio 175 line / inch gravure engraving plate, the prepared printing ink was applied to the treated surface of an OPP film (manufactured by Futamura Chemical Co., Ltd., product name "FOR", thickness: 25 μm) whose one side had been corona discharge treated. Thereafter, hot air drying was performed at 80 ° C. for 10 seconds to produce a printed matter. The obtained printed matter was evaluated for alkali release, yellowing resistance, adhesion, blocking resistance, heat resistance, and wet friction resistance. The results are shown in Tables 2, 4, 6, 8, and 10.
[0078] [Table 1]
[0079] [Table 2]
[0080] [Table 3]
[0081] [Table 4]
[0082] [Table 5]
[0083] [Table 6]
[0084] [Table 7]
[0085]
Table 8
[0086]
Table 9
[0087]
Table 10
[0088] As shown in Tables 2, 4, and 6, the printing ink compositions obtained in each Example were excellent in alkali release property and yellowing resistance. In addition, various physical properties such as adhesion to the substrate, blocking resistance, heat resistance, wet friction resistance, and ink stability were also excellent. As shown in Table 8, the printing ink composition of Comparative Example 1 containing the rosin derivative (B) with an acid value of 100 mgKOH / g had poor alkali release property of the printed layer. The printing ink composition of Comparative Example 2 containing a styrene-maleic acid half ester copolymer instead of the rosin derivative (B) also had poor alkali release property of the printed layer. The printing ink composition of Comparative Example 3, which contained a low content of rosin derivative (B) of 0.7 mass%, also had poor alkali release property of the printed layer. On the other hand, the printing ink composition of Comparative Example 4, which contained a high content of rosin derivative (B) of 18 mass%, had poor blocking resistance, heat resistance, and wet friction resistance of the printed layer. The printing ink composition of Comparative Example 5, which did not contain the rosin derivative (B), had poor alkali release property of the printed layer. As shown in Tables 8 and 10, the printing ink compositions of Comparative Examples 6 and 7, which contained a chelating agent whose ligand was acetylacetone, were inferior in the alkali release property and yellowing resistance of the printed layer. As shown in Table 10, the printing ink composition of Comparative Example 8, which contained a chelating agent whose ligand was ethyl acetoacetate, was inferior in ink stability and also in the alkali release property of the printed layer. The printing ink composition of Comparative Example 9, which contained a low content of chelating agent (C) of 0.3 mass%, was inferior in blocking resistance and heat resistance of the printed layer. The printing ink composition of Comparative Example 10, which contained a high content of chelating agent (C) of 12 mass%, was inferior in ink stability and also in the alkali release property of the printed layer. The printing ink composition of Comparative Example 11, which did not contain a chelating agent, was inferior in blocking resistance and heat resistance of the printed layer. The printing composition of Comparative Example 12, which used a urethane resin (A3) instead of a polyamide resin (A1) as the binder resin (A), was inferior in ink stability. [Industrial Applicability]
[0089] The ink composition of the present invention is a printing ink composition that has high alkali release properties, can provide a printed layer that is excellent in yellowing resistance when a pressure-sensitive adhesive tape is applied, and has high stability. Furthermore, a printed layer that satisfies various physical properties required for a packaging material can be obtained. Therefore, it is particularly useful as an ink for gravure printing. [Explanation of symbols]
[0090] 10 Laminate 11 Plastic Film 12 printing layer
Claims
1. A printing ink composition containing a binder resin (A), a rosin derivative (B), and a chelating agent (C), wherein the binder resin (A) contains a polyamide resin (A1) and a nitrocellulose resin (A2), the rosin derivative (B) has an acid value of 150 mgKOH / g or more, the chelating agent (C) has a phosphate ester structure, the content of the rosin derivative (B) in terms of solid content is 1 to 15 mass% relative to the total mass of the solid content of the printing ink composition, and the content of the chelating agent (C) in terms of solid content is 0.5 to 10 mass% relative to the total mass of the solid content of the printing ink composition.
2. A printing ink composition as described in claim 1, wherein, in the alkaline release property evaluated by the following evaluation method, the ratio of the area of the detached printed layer to the total area of the printed layer is 50% or more. [Evaluation method] The printing ink composition is diluted with a mixed solvent of methylcyclohexane: n-propyl acetate: isopropanol = 5:3:2 (mass ratio) so that the viscosity at 25 ° C. measured using Zahn cup #3 is 16 seconds, and the printing ink is prepared. The printing ink is applied to the treated surface of stretched polypropylene, one side of which has been corona discharge treated, using a gravure printing machine. Thereafter, the printing ink is dried with hot air at 80 ° C. for 10 seconds, and the resulting printed matter is cut to 3 cm x 3 cm, immersed in a 1.5% aqueous sodium hydroxide solution at 70 ° C., and stirred for 3 minutes. The printed matter is pulled out of the aqueous sodium hydroxide solution, washed with water, and then visually observed.
3. A printing ink composition as described in Claim 1, wherein the chelating agent (C) is an organometallic compound having a structure in which a phosphate ester is bonded to a titanium atom.
4. 2. The printing ink composition according to claim 1, wherein the content of the binder resin (A) in terms of solid content is 25 to 75 mass % based on the total mass of the solid content of the printing ink composition.
5. 2. The printing ink composition according to claim 1, wherein a mass ratio of the solid content of the polyamide resin (A1) to the solid content of the nitrocellulose resin (A2) is 1.5 to 9.
6. The printing ink composition according to claim 1, wherein the rosin derivative (B) has an acid value of 150 to 280 mg KOH / g.
7. 2. The printing ink composition according to claim 1, wherein the polyamide resin (A1) has a weight average molecular weight of 30,000 or less.
8. The printing ink composition according to claim 1, wherein the type and viscosity symbol of the nitrocellulose resin (A2) as defined by a viscosity measurement in accordance with JIS K 6703:1995 are H1 / 4, H1 / 2, H1 or H2.
9. The printing ink composition according to claim 1 , further comprising a chlorinated polyolefin resin.
10. The printing ink composition according to any one of claims 1 to 9, which is for gravure printing.
11. A laminate comprising a plastic film and a printed layer formed on at least one surface of the plastic film using the printing ink composition according to claim 10.
12. A packaging material comprising the laminate according to claim 11.
Citation Information
Patent Citations
Printing ink composition
JP1998067959A
Printing ink composition
JP2007246822A
Gravure printing ink composition for surface printing
JP2013234238A
Print ink composition for detachment, and detachment method
JP2022080724A
Recycled olefin substrate production method
JP2022101885A
Cited By
Sun-proof water-based ink for printing special paper and preparation method of sun-proof water-based ink
CN121801376A