Resin composition and optical film using same

The combination of a fumaric acid ester polymer and silicone resin in a resin composition addresses manufacturing complexities and stability issues, resulting in optical films with stable retardation, low wavelength dependence, and enhanced dimensional stability for liquid crystal displays.

JP7562939B2Active Publication Date: 2024-10-08TOSOH CORP
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2019019383
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-02-06
Publication Date
2024-10-08
Estimated Expiration
2039-02-06

AI Technical Summary

Technical Problem

Existing optical compensation films face issues with complex manufacturing processes, poor productivity, difficulty in controlling uniformity of phase difference, instability due to high photoelastic constants, large wavelength dependence, and poor dimensional stability, especially when used with polarizing plates at high temperatures.

Method used

A resin composition containing a fumaric acid ester polymer and a silicone resin, with specific molecular structures and ratios, which is molded into films to achieve negative birefringence, high heat resistance, and excellent dimensional stability.

Benefits of technology

The resin composition provides films with stable retardation characteristics, low wavelength dependence, and improved dimensional stability, suitable for high-temperature applications, enhancing optical performance in liquid crystal displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562939000001
    Figure 0007562939000001
  • Figure 0007562939000002
    Figure 0007562939000002
  • Figure 0007562939000003
    Figure 0007562939000003
Patent Text Reader

Abstract

To provide an optical film having excellent phase difference characteristics and wavelength dependence.SOLUTION: Provided is a resin composition containing 80 wt.% or more of a fumarate-based polymer represented by the following formula (1) and 0.1 wt.% to 20 wt.% of a silicone resin (in the formula, Rand Reach independently represent a C1-12 linear or branched alkyl group, or a C3-6 cyclic alkyl group).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition suitable as an optical material, and more specifically to a resin composition and an optical film excellent in retardation properties, wavelength dependency and dimensional stability.

[0002] The present invention relates to an optical film having negative birefringence and excellent dimensional stability such as retardation characteristics and wavelength dependency, and more particularly to an optical film for use in a liquid crystal display device. [Background technology]

[0003] Liquid crystal displays (LCDs) are the most important display devices in our multimedia society, and are used in a wide range of applications, from smartphones and computer monitors to laptops and televisions.

[0004] Many optical films are used in liquid crystal displays to improve display characteristics, and retardation films in particular play an important role in improving contrast when viewed from the front or at an angle, compensating for color tones, etc. Conventional retardation films are made of polycarbonate or cyclic polyolefin, both of which are polymers with positive birefringence. Here, the positive and negative birefringence are defined as follows:

[0005] The optical anisotropy of a polymer film that has been molecularly oriented by stretching or other means can be represented by an index ellipsoid, where nx is the refractive index in the fast axis direction in the film plane when the film is stretched, ny is the refractive index in the in-plane direction perpendicular to nx, and nz is the refractive index in the thickness direction of the film.

[0006] In other words, when a polymer with negative birefringence is uniaxially stretched, the refractive index is small in the direction of the stretching axis (fast axis: stretching direction), and when a polymer with positive birefringence is uniaxially stretched, the refractive index is small in the direction perpendicular to the stretching axis (fast axis: direction perpendicular to the stretching direction).

[0007] The in-plane retardation (Re) is expressed as the value obtained by multiplying the refractive index in the direction perpendicular to the fast axis (ny) minus the refractive index in the fast axis direction (nx) by the thickness of the film.

[0008] Many polymers have positive birefringence. Polymers with negative birefringence include acrylic resin and polystyrene, but acrylic resin has low retardation and is not sufficient for optical compensation film. Polystyrene is not currently used due to problems with retardation stability, such as a large photoelastic coefficient at room temperature that causes the retardation to change with even a slight stress, optical properties such as a large wavelength dependency of retardation, and practical problems such as low heat resistance.

[0009] Here, the wavelength dependence of retardation means that the retardation changes depending on the measurement wavelength, and can be expressed as the ratio R450 / R550, which is the ratio of the retardation measured at a wavelength of 450 nm (R450) to the retardation measured at a wavelength of 550 nm (R550). In general, polymers with aromatic structures tend to have a large R450 / R550, which reduces the contrast and viewing angle characteristics in the low wavelength region.

[0010] Stretched polymer films that exhibit negative birefringence have a high refractive index in the thickness direction of the film, making them unprecedented optical compensation films. They are useful, for example, as optical compensation films for compensating for the viewing angle characteristics of displays such as super twisted nematic liquid crystal displays (STN-LCDs), vertically aligned liquid crystal displays (VA-LCDs), in-plane aligned liquid crystal displays (IPS-LCDs), reflective liquid crystal displays, and semi-transmissive liquid crystal displays, as well as optical compensation films for compensating for the viewing angle of polarizing plates, and there is strong market demand for optical compensation films with negative birefringence.

[0011] Methods for producing a film in which a refractive index in the thickness direction of the film is increased by using a polymer having positive birefringence have been proposed. One method is a treatment method in which a heat-shrinkable film is adhered to one or both sides of a polymer film, and the laminate is heat-stretched to apply a shrinking force in the thickness direction of the polymer film (see, for example, Patent Documents 1 to 3). Another method has been proposed in which an electric field is applied to the polymer film while the film is uniaxially stretched in-plane (see, for example, Patent Document 4).

[0012] Also, an optical compensation film made of fine particles having negative optical anisotropy and a transparent polymer has been proposed (see, for example, Patent Document 5).

[0013] Also, optical compensation films or optical compensation layers have been proposed in which a liquid crystalline polymer film is coated and homeotropically aligned (see, for example, Patent Document 6). Furthermore, optical compensation films have been proposed in which aromatic polymers such as polyvinylnaphthalene and polyvinylbiphenyl are coated (see, for example, Patent Document 7 and Non-Patent Document 1). Furthermore, optical films using polyvinylcarbazole-based polymers have been proposed (see, for example, Patent Document 8).

[0014] Also, optical films made of fumaric acid ester resins have been proposed (see, for example, Patent Document 9). [Prior art documents] [Patent documents]

[0015] [Patent Document 1] Patent No. 2818983 [Patent Document 2] Japanese Patent Application Publication No. 05-297223 [Patent Document 3] Japanese Patent Application Publication No. 05-323120 [Patent Document 4] Japanese Patent Application Publication No. 06-088909 [Patent Document 5] JP 2005-156862 A [Patent Document 6] JP 2002-333524 A [Patent Document 7] JP 2006-221116 A [Patent Document 8] JP 2001-91746 A [Patent Document 9] JP 2008-64817 A [Non-patent literature]

[0016] [Non-Patent Document 1] Journal of the Japanese Society of Rheology Vol.22, No.2, 129-134(1994) Summary of the Invention [Problem to be solved by the invention]

[0017] However, the methods proposed in Patent Documents 1 to 4 have problems such as poor productivity due to the extremely complicated manufacturing process. In addition, control of the uniformity of the phase difference is significantly more difficult than control by conventional stretching. In addition, when polycarbonate is used as the base film, the photoelastic constant at room temperature is large, and the phase difference changes due to a slight stress, so there is also a problem with the stability of the phase difference. In addition, there are problems such as the large wavelength dependency of the phase difference.

[0018] In addition, the optical compensation film obtained in Patent Document 5 is an optical compensation film having negative birefringence by adding fine particles having negative optical anisotropy, and from the viewpoint of simplifying the manufacturing method and economic efficiency, an optical compensation film that does not require the addition of fine particles is required. The method described in Patent Document 6 has a problem that it is difficult to uniformly align the liquid crystal polymer in a homeotropic manner. In addition, the methods described in Patent Documents 7 and 8 have problems that the obtained film is easily cracked and the wavelength dependency of the retardation is large. In addition, as described in Non-Patent Document 1, there is a problem that the photoelastic coefficient of the glass region is high and the retardation is not stable.

[0019] The retardation film obtained in Patent Document 9 has excellent optical properties such as retardation characteristics and wavelength dependency, but when used with a polarizing plate that requires durability at high temperatures, there is a problem with dimensional stability during heating, and improvement of the dimensional stability has been desired.

[0020] The present invention has been made in view of the above problems, and its object is to provide a resin composition that is excellent in retardation properties, wavelength dependency and dimensional stability when used as an optical film. Another object of the present invention is to provide an additive that can impart dimensional stability to a raw material resin when molded into a film. [Means for solving the problem]

[0021] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and discovered that a resin composition containing a specific polymer and a specific silicone resin solves the above problems, thereby completing the present invention.

[0022] That is, the present invention relates to a resin composition containing 80% by weight or more and 99.9% by weight or less of a fumaric acid ester-based polymer containing a fumaric acid diester residue represented by the following general formula (1) and 0.1% by weight or more and 20% by weight or less of a silicone resin represented by the following general formula (2).

[0023] [ka]

[0024] (In the formula, R1 and R2 each independently represent one type of a linear or branched alkyl group having 1 to 12 carbon atoms or a cyclic alkyl group having 3 to 6 carbon atoms.)

[0025] [ka]

[0026] (In the formula, R3, R4, R5, R6, R7, and R8 each independently represent one of the group consisting of hydrogen, a hydroxyl group, a phenyl group, or an alkyl group, an acyloxy group, or an alkoxy group having 1 to 12 carbon atoms. Here, a+b+c+d=1.)

[0027] Another embodiment of the present invention is a dimensional stabilizer containing a silicone resin represented by the general formula (2).

[0028] The present invention will be described in detail below.

[0029] The resin composition of the present invention contains 80% by weight or more and 99.9% by weight or less of a fumarate ester-based polymer containing a fumarate diester residue represented by the following general formula (1), and 0.1% by weight or more and 20% by weight or less of a silicone resin represented by the following general formula (2).

[0030] [ka]

[0031] (In the formula, R1 and R2 each independently represent one type of a linear or branched alkyl group having 1 to 12 carbon atoms or a cyclic alkyl group having 3 to 6 carbon atoms.)

[0032] [ka]

[0033] (In the formula, R3, R4, R5, R6, R7, and R8 each independently represent one of the group consisting of hydrogen, a hydroxyl group, a phenyl group, or an alkyl group, an acyloxy group, or an alkoxy group having 1 to 12 carbon atoms, where a+b+c+d=1.)

[0034] Here, R1 and R2, which are ester substituents of the fumaric acid ester residue unit in general formula (1), are each independently an alkyl group having 1 to 12 carbon atoms, which may be substituted with a halogen group such as fluorine or chlorine; an ether group; an ester group or an amino group. Examples of such groups include one or more of ethyl group, isopropyl group, n-butyl group, s-butyl group, t-butyl group, s-pentyl group, t-pentyl group, s-hexyl group, t-hexyl group, cyclopropyl group, cyclopentyl group, cyclohexyl group, 2-ethylhexyl group, n-octyl group, etc., and are preferably isopropyl group, ethyl group, n-butyl group, 2-ethylhexyl group, n-octyl group, etc., since they provide an optical compensation film having excellent heat resistance and mechanical properties, and are preferably isopropyl group, since they provide an optical compensation film having excellent balance between heat resistance and mechanical properties.

[0035] The fumarate ester polymer in the present invention may be a copolymer containing a residue unit other than the residue unit represented by general formula (1), or may be a polymer having only the residue unit represented by general formula (1). Preferably, the fumarate ester polymer is a polymer having only the residue unit represented by general formula (1).

[0036] Specific examples of the fumarate residue unit represented by the general formula (1) include dimethyl fumarate residue, diethyl fumarate residue, diisopropyl fumarate residue, di-tert-butyl fumarate residue, di-n-butyl fumarate residue, di-sec-butyl fumarate residue, isobutyl fumarate residue, dipentyl fumarate residue, diisopentyl fumarate residue, di-sec-isoamyl fumarate residue, dineopentyl fumarate residue, di-tert-pentyl fumarate residue, Examples of the fumarate residue include one or more of diethyl fumarate residue, di-2-ethylhexyl fumarate residue, dicyclopropyl fumarate residue, dicyclobutyl fumarate residue, dicyclopentyl fumarate residue and dicyclohexyl fumarate residue. Among these, diethyl fumarate residue, diisopropyl fumarate residue, di-n-butyl fumarate residue, di-2-ethylhexyl fumarate residue, di-n-octyl fumarate residue and the like are preferred, and diisopropyl fumarate residue is particularly preferred.

[0037] When the fumaric acid ester polymer used in the present invention is a copolymer, the ratio of the fumaric acid ester residues represented by the general formula (1) is preferably 30 mol% or more, and more preferably 50 mol% or more, and more preferably 70 mol% or more, since the obtained optical compensation film is particularly excellent in heat resistance and mechanical properties. Also, the ratio of the fumaric acid ester residues represented by the general formula (1) is preferably 100% or less.

[0038] Specific examples of the fumarate polymer used in the present invention include diisopropyl fumarate polymer, di-n-butyl fumarate polymer, diisopropyl fumarate-dimethyl fumarate copolymer, diisopropyl fumarate-diethyl fumarate copolymer, diisopropyl fumarate-di-n-butyl fumarate copolymer, diisopropyl fumarate-bis(2-ethylhexyl) fumarate copolymer, diisopropyl fumarate-di-n-octyl fumarate copolymer, and the like. Among these, diisopropyl fumarate polymer, diisopropyl fumarate-diethyl fumarate copolymer, diisopropyl fumarate-bis(2-ethylhexyl) fumarate copolymer, and diisopropyl fumarate-di-n-octyl fumarate copolymer are particularly preferred.

[0039] In the present invention, the fumarate ester polymer is preferably a copolymer having at least diisopropyl fumarate as a residue unit. In this case, the constituent ratio of diisopropyl fumarate residue units is preferably 70 mol % or more, more preferably 80 mol % or more. This results in an optical compensation film with excellent heat resistance and retardation properties.

[0040] Furthermore, the fumarate polymer constituting the resin composition of the present invention may contain other monomer residues as long as the purpose of the present invention is not deviated from. Examples of the other monomer residues include styrene residues such as styrene residues and α-methylstyrene residues; acrylic acid residues; acrylic acid ester residues such as methyl acrylate residues, ethyl acrylate residues, butyl acrylate residues, 3-ethyl-3-oxetanylmethyl acrylate residues, tetrahydrofurfuryl acrylate residues; methacrylic acid residues; methacrylic acid ester residues such as methyl methacrylate residues, ethyl methacrylate residues, butyl methacrylate residues, 3-ethyl-3-oxetanylmethyl methacrylate residues, and tetrahydrofurfuryl methacrylate residues; vinyl ester residues such as vinyl acetate residues and vinyl propionate residues; vinyl ether residues such as methyl vinyl ether residues, ethyl vinyl ether residues, and butyl vinyl ether residues; acrylonitrile residues; methacrylonitrile residues; olefin residues such as ethylene residues and propylene residues; and the like.

[0041] Fumaric acid ester polymers have particularly excellent mechanical properties and excellent processability during film formation. Therefore, they are used in applications where the number average molecular weight (Mn) calculated as standard polystyrene from the elution curve measured by gel permeation chromatography (GPC) is 1×10 3 ~5×10 6 and more preferably 5×10 4 ~5×10 5 And more preferably 8×10 4 ~5×10 5 It is.

[0042] The method for producing the fumaric acid ester polymer constituting the resin composition of the present invention is not particularly limited as long as a fumaric acid ester polymer can be obtained. For example, the fumaric acid ester polymer can be produced by radical polymerization of fumaric acid esters.

[0043] The radical polymerization method used can be any known polymerization method, such as bulk polymerization, solution polymerization, suspension polymerization, precipitation polymerization, emulsion polymerization, and the like.

[0044] Examples of polymerization initiators for carrying out radical polymerization include organic peroxides such as benzoyl peroxide, lauryl peroxide, octanoyl peroxide, acetyl peroxide, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, and t-butyl peroxypivalate; and azo initiators such as 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-butyronitrile), 2,2'-azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, and 1,1'-azobis(cyclohexane-1-carbonitrile).

[0045] Solvents that can be used in the solution polymerization method, suspension polymerization method, precipitation polymerization method, and emulsion polymerization method are not particularly limited, and examples thereof include aromatic solvents such as benzene, toluene, and xylene; alcohol solvents such as methanol, ethanol, propyl alcohol, and butyl alcohol; cyclohexane; dioxane; tetrahydrofuran (THF); acetone; methyl ethyl ketone; dimethylformamide; isopropyl acetate; water; and mixed solvents of these.

[0046] The polymerization temperature during radical polymerization can be appropriately set depending on the decomposition temperature of the polymerization initiator, and is generally preferably in the range of 40° C. or higher and 150° C. or lower.

[0047] The suspension polymerization method in the present invention may be a known radical suspension polymerization method, and is not particularly limited as long as an aqueous medium is used. The aqueous medium is not particularly limited, and examples thereof include water, industrial water, ion-exchanged water, and distilled water.

[0048] A dispersant that is generally used in the suspension polymerization reaction of the present invention can be used, and there is no particular limitation on the dispersant, and any known dispersant can be used. Examples of such dispersants include polyvinyl alcohol-based dispersants such as polyvinyl alcohol; cellulose-based dispersants such as methyl cellulose, ethyl cellulose, propyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, and carboxyethyl cellulose; and inorganic compounds such as calcium phosphate. Among these, cellulose-based dispersants are preferred because they provide more stable suspension polymerization, and hydroxypropyl methyl cellulose is more preferred.

[0049] The blending ratios of the aqueous medium, monomer, dispersant, and oil-soluble radical polymerization initiator in the method for producing a fumaric acid ester polymer of the present invention can be appropriately selected depending on the desired quality of the fumaric acid ester polymer. In particular, it is preferable to use 50 to 150 parts by weight of the monomer, 0.01 to 20 parts by weight of the dispersant, and 0.001 to 5 parts by weight of the oil-soluble radical polymerization initiator per 100 parts by weight of the aqueous medium, in order to obtain a method for producing a fumaric acid ester polymer with excellent production efficiency.

[0050] The suspension polymerization reaction apparatus in the present invention is not particularly limited, and known apparatuses can be used, such as a glass-lined (GL) or stainless steel (SUS) reaction vessel equipped with an agitating blade, a temperature control device, etc. Examples of the agitating blade include a paddle blade, a four-blade paddle blade, an anchor blade, a three-blade swept-back blade, a six-blade turbine blade, and a blue margin blade.

[0051] The resin composition according to the present invention is characterized in that, by containing the silicone resin represented by general formula (2), when formed into a film for use, it has excellent dimensional stability even at high temperatures.

[0052] In the present invention, the silicone resin represented by the general formula (2) can be used as a dimensional stabilizer.

[0053] The silicone resin represented by the general formula (2) is characterized by satisfying the condition a+b+c+d=1. In the silicone resin, since the retardation characteristics are excellent, (c+d) is preferably 0.2 or more and 1.0 or less, and particularly preferably 0.4 or more and 1.0 or less. Furthermore, it is preferable that the silicone resin has (a+b) of 0.8 or less and (c+d) of 0.2 or more and 1.0 or less.

[0054] In the present invention, a, b, c, and d of the silicone resin are 29 It can be quantitatively determined by Si-NMR spectroscopy.

[0055] In the present invention, R3, R4, R5, R6, R7, and R8 of the silicone resin each independently represent one of the group consisting of hydrogen, a hydroxyl group, a phenyl group, or an alkyl group, an acyloxy group, or an alkoxy group having 1 to 12 carbon atoms. Among these, because of excellent moisture resistance, one of the group consisting of hydrogen, a hydroxyl group, a phenyl group, a methyl group, an ethyl group, an isopropyl group, an n-propyl group, and a methoxy group is preferred, and one of the group consisting of a hydroxyl group, a phenyl group, a methyl group, an isopropyl group, and a methoxy group is more preferred.

[0056] In the present invention, specific examples of silicone resins include RSN-249 (Dow Corning Corporation, solid flake hydroxyl functional silicone resin having Si-bonded methyl and phenyl groups, Si-bonded OH group content of 5 wt%, molar ratio Ph / Me: 0.7 / 1, Mw: 5,696 g / mol, a: 0.02, b: 0.56, c: 0.44, d: 0), RSN-217 (Dow Corning Corporation, liquid hydroxyl functional silicone resin having Si-bonded phenyl groups, Si-bonded OH group content of 6 wt%, Mw: 1,426 g / mol, a: 0, b: 0.48, c: 0.52, d: 0), YR-3370 (Momentive Performance Materials Holdings Corporation, solid flake hydroxyl functional silicone resin having Si-bonded methyl groups, Si-bonded OH group content of 2 wt%, Mw: 8,250 g / mol, a: 0, b: 0.08, c: 0.92, d: 0), and KR-220L (Shin-Etsu Chemical Co., Ltd., solid flake hydroxyl functional silicone resin with Si-bonded methyl groups, Si-bonded OH group content 6 wt%, Mw: 3,234 g / mol, a: 0.00, b: 0.27, c: 0.73, d: 0). The structural parameters (a, b, c, and d) of these silicone resins are as follows: 29 Quantitatively determined by Si-NMR.

[0057] From the viewpoints of improving dimensional stability, improving mechanical properties, and retardation stability, the silicone resin of the present invention preferably has a weight average molecular weight, in terms of standard polystyrene, of 100 to 40,000, more preferably 100 to 10,000, and particularly preferably 100 to 5,000.

[0058] The silicone resins of the present invention can be prepared by hydrolytic polycondensation according to methods well known in the art, and have the general formula SiX q R' 4-qHere, X represents a hydrolyzable substituent, for example, halogen, preferably chlorine, an alkoxy group, an acyloxy group, etc. q represents a number defining the functionality of the precursor, and is an integer ranging from 1 to 4. R' is a non-hydrolyzable substituent. Details of polycondensation by hydrolysis are described, for example, in "Ullmanns Encyklopadieder technischen Chemie, Verlag Chemie, 4th ed., vol. 21, pp. 511-541".

[0059] The proportion of silicone resin in the resin composition of the present invention is 0.01% by weight or more and 20% by weight or less relative to 100 parts by weight of fumaric acid ester polymer, and is preferably 0.1% by weight or more and 15% by weight or less, more preferably 0.3% by weight or more and 10% by weight or less, because it has excellent dimensional stability and retardation properties. In the present invention, when the proportion of silicone resin is 0.01% by weight or more, dimensional stability is improved in a high temperature environment. In addition, when the proportion is 20% by weight or less, an optical film having excellent retardation properties, which is a feature of the present invention, can be obtained.

[0060] These silicone resins may be used alone or in combination of two or more.

[0061] The method for producing the optical film of the present invention is not particularly limited. For example, the optical film can be produced by forming the film into a film by a solution casting method, a melt casting method or the like, and stretching the film at least uniaxially.

[0062] The solution casting method is a method in which a solution (hereinafter referred to as "dope") in which a fumaric acid ester polymer is dissolved in a solvent is cast onto a support substrate, and the solvent is removed by heating or the like to obtain a film. In this case, the method of casting the dope onto the support substrate includes, for example, the T-die method, the doctor blade method, the bar coater method, the roll coater method, and the lip coater method. In particular, the most common method is to continuously extrude the dope from a die onto a belt-shaped or drum-shaped support substrate industrially. Examples of the support substrate that can be used include glass substrates; metal substrates such as stainless steel and ferrotype; and plastic substrates such as polyethylene terephthalate (PET) and triacetyl cellulose (TAC). In the solution casting method, when a film having high transparency and excellent thickness accuracy and surface smoothness is formed, the solution viscosity of the dope is an extremely important factor, and is preferably 700 to 30,000 cps, and particularly preferably 1,000 to 10,000 cps. The melt casting method is a molding method in which a fumaric acid ester polymer is melted in an extruder, extruded from a slit in a T-die into a film, and then taken up while being cooled by a roll or air.

[0063] The obtained film can be stretched uniaxially or biaxially to produce an optical film with controlled retardation. Examples of the uniaxial stretching method include free width uniaxial stretching, stretching with a tenter, and stretching between rolls, while examples of the biaxial stretching method include stretching with a tenter and stretching by expanding into a tube shape.

[0064] The thickness of the optical film when stretched is preferably from 10 μm to 200 μm, more preferably from 30 μm to 180 μm, and particularly preferably from 30 μm to 150 μm, from the viewpoints of suitability for thinning optical members and ease of stretching treatment.

[0065] As the stretching conditions, since it is difficult for thickness unevenness to occur and it becomes an optical film excellent in mechanical properties and optical properties, the stretching temperature is preferably 50°C or higher and 200°C or lower, particularly preferably 80°C or higher and 180°C or lower, and the stretching ratio is preferably 1.01 to 3 times, particularly preferably 1.01 to 2 times.

[0066] For the optical film using the resin composition of the present invention, when the refractive index in the in-plane slow axis direction of the film surface is nx, the refractive index in the direction perpendicular thereto is ny, and the refractive index in the film thickness direction is nz, there is a relationship of nx ≦ ny < nz, and the ratio (R450 / R550) of the retardation measured with light of 450 nm and the retardation measured with light of 550 nm is 1.1 or less. It is an optical film characterized by this, and by satisfying the relationship of nx ≦ ny < nz, it becomes an optical film excellent in viewing angle compensation performance such as an IPS-LCD.

[0067] In addition, since the optical film using the resin composition of the present invention becomes a film having more excellent optical properties, the in-plane retardation (Re) measured at a wavelength of 550 nm represented by the following formula (1) is preferably 0 to 300 nm, more preferably 0 to 290 nm, and particularly preferably 0 to 280 nm. Re = (ny - nx) × d (1) (Here, d represents the film thickness.)

[0068] In addition, the in-plane retardation (Re) when used as a circularly polarized film formed by laminating and integrating an optical film and a polarizing plate is preferably 0 to 280 nm. The circularly polarized film is useful not only as a compensation film for a reflective liquid crystal display but also as an antireflection film, a brightness enhancement film, etc. for an organic EL display.

[0069] In addition, for the optical film of the present invention, the out-of-plane retardation (Rth) measured at a wavelength of 550 nm represented by the following formula (2) is preferably -30 to -300 nm, more preferably -50 to -300 nm, and particularly preferably -80 to -300 nm. Rth = 〔(nx + ny) / 2 - nz〕× d (2)

[0070] The resin composition of the present invention has excellent dimensional stability due to the inclusion of a silicone resin, and is useful for polarizing plate applications that require high dimensional stability even under high heat environments. The linear expansion coefficient of an optical film using the resin composition of the present invention at 40 to 85°C is 15.0 x 10 -5 / ° C. or less. The linear expansion coefficient here is a value measured as the average linear expansion coefficient of a test piece in a given temperature range in accordance with JIS K 7197, but in the present invention, it is a value in the temperature range of 40° C. to 85° C.

[0071] The thickness of the optical film obtained by stretching is preferably from 5 μm to 100 μm, more preferably from 10 μm to 80 μm, and particularly preferably from 10 μm to 60 μm.

[0072] The optical film of the present invention is preferably blended with an antioxidant to enhance the thermal stability during film molding or of the film itself. Examples of the antioxidant include hindered phenol-based antioxidants, phosphorus-based antioxidants, and other antioxidants, and these antioxidants may be used alone or in combination. It is preferable to use a hindered phenol-based antioxidant and a phosphorus-based antioxidant in combination because the antioxidant action is synergistically improved, and in this case, it is particularly preferable to mix 100 to 500 parts by weight of the phosphorus-based antioxidant with 100 parts by weight of the hindered phenol-based antioxidant. The amount of the antioxidant to be added is preferably 0.01 to 10 parts by weight, particularly preferably 0.5 to 1 part by weight, with respect to 100 parts by weight of the fumaric acid ester polymer of the present invention.

[0073] Furthermore, as an ultraviolet absorbing agent, for example, benzotriazole, benzophenone, triazine, benzoate, or the like may be blended as required.

[0074] The optical film of the present invention may contain other additives such as polymers, surfactants, polymer electrolytes, conductive complexes, inorganic fillers, pigments, dyes, antistatic agents, antiblocking agents, and lubricants, within the scope of the gist of the invention.

[0075] The optical film of the present invention can be laminated with a polarizing plate to be used as a circular or elliptical polarizing plate, or can be laminated with a polarizer made of polyvinyl alcohol / iodine, etc. to form a polarizing plate. The optical film of the present invention can also be laminated with another optical film or with another optical film.

[0076] An optical film using the resin composition of the present invention is useful as an antireflection film or a compensation film for the contrast or viewing angle characteristics of a liquid crystal display. EXAMPLES

[0077] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, the reagents used were commercially available products.

[0078] The physical properties shown in the examples were measured by the following methods.

[0079] <Measurement of number average molecular weight> Gel permeation chromatography (GPC) apparatus (Tosoh Corporation, product name: C0-8011 (column GMH HR The measurements were performed at 40°C using a 100% sintered body (equipped with a -H) and tetrahydrofuran as a solvent, and the values ​​were calculated in terms of standard polystyrene.

[0080] <Polymer analysis> The polymer structure was analyzed using a nuclear magnetic resonance measuring device (manufactured by JEOL, product name: JNM-GX270) and proton nuclear magnetic resonance spectroscopy ( 1 H-NMR spectroscopy was used to determine the molecular weight.

[0081] <Structural analysis of silicone resin> The a, b, c, and d in general formula (2) were quantitatively determined by 29Si-NMR spectroscopy. The NMR experiments were carried out using a JEOL (JNM-ECZ400S / KI). The sample was dissolved in deuterated chloroform and loaded into a Teflon NMR sample tube (NORELL, TL-5-7) with 5 mM chromium acetylacetonate added as a relaxation reagent. NMR data were acquired at room temperature (22°C) with a 29Si resonance frequency of 79.4 MHz. 29Si measurements were performed with a 90° excitation pulse of 10 μs, a waiting time (time between scans) of 10 seconds, and proton decoupling at 400 MHz during acquisition. Each spectrum was acquired with 4000 scans. Chemical shifts (δ) were calibrated with tetramethylsilane as a standard (δ=0 ppm). Peak assignments were performed according to the description of JP 2015-523434 A.

[0082] <Measurement of light transmittance and haze of optical films> The light transmittance and haze of the prepared films were measured using a haze meter (manufactured by Nippon Denshoku Industries, product name: NDH2000). The light transmittance was measured in accordance with JIS K 7361-1 (1997 edition), and the haze was measured in accordance with JIS-K 7136 (2000 edition).

[0083] <Measurement of phase difference characteristics> The retardation characteristics of the optical compensation film were measured using a sample tilt type automatic birefringence meter (manufactured by Oji Scientific Instruments, product name: KOBRA-WR) with light having a wavelength of 589 nm.

[0084] <Measurement of wavelength dispersion characteristics> The wavelength dispersion characteristics of the optical film were measured using a tilt-type automatic birefringence meter (manufactured by Oji Scientific Instruments, product name: KOBRA-WR) as the ratio of the phase difference Re(450) due to light with a wavelength of 450 nm to the phase difference Re(550) due to light with a wavelength of 550 nm.

[0085] <Measurement of linear expansion coefficient> Using a linear expansion coefficient measuring device (manufactured in-house), the test film was heated from room temperature to 115° C. at a rate of 2° C. / min, and the deformation amount at each temperature was measured. The linear expansion coefficient of the film was then calculated from the deformation amount in the temperature range of 40° C. to 85° C.

[0086] Synthesis Example 1 In a 1-liter reactor equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 600 g of distilled water, 3.4 g of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name Metolose 60SH-50) as a dispersant, 400.0 g of diisopropyl fumarate, and 8.3 g of t-butyl peroxypivalate as an oil-soluble radical initiator were placed, and after nitrogen bubbling for 1 hour, radical suspension polymerization was carried out by holding at 50°C for 24 hours while stirring at 400 rpm. After the polymerization reaction was completed, the contents were recovered from the reactor, the polymerized product was filtered, washed twice with distilled water and twice with methanol, and then dried under reduced pressure at 80°C (yield: 77%). The number average molecular weight of the obtained diisopropyl fumarate polymer was 129,000.

[0087] Synthesis Example 2 In a 1-liter reactor equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 600 g of distilled water, 3.4 g of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name Metolose 60SH-50) as a dispersant, 350.9 g of diisopropyl fumarate, 49.1 g of diethyl fumarate (14.0 parts by weight per 100 parts by weight of diisopropyl fumarate), and 8.3 g of t-butyl peroxypivalate as an oil-soluble radical initiator were placed, and after nitrogen bubbling for 1 hour, radical suspension polymerization was carried out by maintaining the mixture at 50°C for 28 hours while stirring at 400 rpm. After the polymerization reaction was completed, the contents were recovered from the reactor, the polymerized product was filtered, washed twice with distilled water and twice with methanol, and then dried under reduced pressure at 80°C (yield: 75%).

[0088] The number average molecular weight of the resulting fumaric acid ester polymer was 138,000. 1 H-NMR measurements showed that the polymer particles consisted of diisopropyl fumarate units / fumarate. The copolymer was confirmed to be a diisopropyl fumarate / diethyl fumarate copolymer with a diethyl fumarate / diisopropyl fumarate moiety ratio of 86.7 / 13.3 (mol%).

[0089] Synthesis Example 3 In a 1-liter reactor equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 600 g of distilled water, 3.4 g of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name Metolose 60SH-50) as a dispersant, 340.5 g of diisopropyl fumarate, 59.5 g of di-n-butyl fumarate (17.6 parts by weight per 100 parts by weight of diisopropyl fumarate), and 8.3 g of t-butyl peroxypivalate as an oil-soluble radical initiator were placed, and after nitrogen bubbling for 1 hour, the mixture was stirred at 400 rpm and held at 50°C for 28 hours to carry out radical suspension polymerization. After the polymerization reaction was completed, the contents were recovered from the reactor, the polymerized product was filtered, washed twice with distilled water and twice with methanol, and then dried under reduced pressure at 80°C (yield: 76%).

[0090] The number average molecular weight of the resulting fumaric acid ester polymer was 117,000. 1 H-NMR measurements showed that the polymer particles consisted of diisopropyl fumarate units / fumarate. The copolymer was confirmed to be a diisopropyl fumarate / di-n-butyl fumarate copolymer with a di-n-butyl fumarate / di-n-butyl fumarate moiety ratio of 88.5 / 11.5 (mol%).

[0091] Synthesis Example 4 In a 1-liter reactor equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 600 g of distilled water, 3.4 g of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name Metolose 60SH-50) as a dispersant, 332.2 g of diisopropyl fumarate, 67.8 g of bis(2-ethylhexyl) fumarate (20.4 parts by weight per 100 parts by weight of diisopropyl fumarate), and 8.3 g of t-butyl peroxypivalate as an oil-soluble radical initiator were placed, and after nitrogen bubbling for 1 hour, the mixture was stirred at 400 rpm and held at 50°C for 28 hours to carry out radical suspension polymerization. After the polymerization reaction was completed, the contents were recovered from the reactor, the polymerized product was filtered, washed twice with distilled water and twice with methanol, and then dried under reduced pressure at 80°C (yield: 73%).

[0092] The number average molecular weight of the resulting fumaric acid ester polymer was 140,000. 1 H-NMR measurements showed that the polymer particles consisted of diisopropyl fumarate units / fumarate. The copolymer was confirmed to be a diisopropyl fumarate / bis(2-ethylhexyl fumarate) copolymer with a bis(2-ethylhexyl) fumarate moiety ratio of 87.4 / 12.6 (mol%).

[0093] Synthesis Example 5 Into a 1-liter reactor equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 600 g of distilled water, 3.4 g of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical Co., Ltd., trade name: Metolose 60SH-50) as a dispersant, 350.9 g of diisopropyl fumarate, and 67.8 g of di-n-octyl fumarate (per 100 parts by weight of diisopropyl fumarate, 19.3 Parts by weight of 100 parts by weight of 100 parts by weight of tert-butyl peroxypivalate, an oil-soluble radical initiator, were added, and after nitrogen bubbling for 1 hour, the mixture was stirred at 400 rpm and held at 50°C for 28 hours to carry out radical suspension polymerization. After the polymerization reaction was completed, the contents were recovered from the reactor, and the polymerized product was filtered, washed twice with distilled water and twice with methanol, and then dried under reduced pressure at 80°C (yield: 77%).

[0094] The number average molecular weight of the obtained fumaric acid ester polymer was 125,000. 1 By 1H-NMR measurement, it was confirmed that the polymer particles were a diisopropyl fumarate·di-n-octyl fumarate copolymer with a diisopropyl fumarate residue unit / di-n-octyl fumarate residue unit = 87.2 / 12.8 (mol%).

[0095] Example 1 To 100 parts by weight of the diisopropyl fumarate polymer obtained in Synthesis Example 1, 3 parts by weight of silicone resin RSN-217 (Dow Corning) was added, dissolved in a toluene·methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto a support substrate of a solution casting apparatus by the T-die method, dried at 80 °C and 130 °C for 4 minutes each, and a film with a width of 250 mm and a thickness of 50 μm was obtained.

[0096] From the results of the three-dimensional refractive index measurement of the film (nx = 1.4787, ny = 1.4788, nz = 1.4825), the obtained film had a refractive index in the film thickness direction of nx ≤ ny < nz. The in-plane retardation Re = (ny - nx) × d was 5.0 nm, the out-of-plane retardation Rth = [((nx + ny) / 2 - nz)] × d was -188 nm, the ratio of retardations (R450 / R550) (wavelength dependence) was 1.01, and the linear expansion coefficient at 40 °C to 85 °C was 14.5×10 -5 / °C.

[0097] From these results, the obtained film had negative birefringence, a large refractive index in the thickness direction, low wavelength dependence, and excellent dimensional stability, and was thus suitable for an optical film.

[0098] Example 2 To 100 parts by weight of the diisopropyl fumarate - diethyl fumarate copolymer obtained in Synthesis Example 2, 3 parts by weight of silicone resin YR - 3370 (Momentive Performance Materials Holdings Inc.) was blended, dissolved in a toluene - methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto a support substrate of a solution casting apparatus by the T - die method, dried at 80 °C and 130 °C for 4 minutes each, and a film with a width of 250 mm and a thickness of 40 μm was obtained.

[0099] From the results of measuring the three - dimensional refractive index of the film (nx = 1.4812, ny = 1.4813, nz = 1.4856), the refractive index in the film thickness direction of the obtained film was nx ≤ ny < nz. The in - plane retardation Re=(ny - nx)×d was 4.0 nm, the out - of - plane retardation Rth = 〔(nx + ny) / 2 - nz〕×d was - 174 nm, the ratio of retardations (R450 / R550) (wavelength dependence) was 1.01, and the linear expansion coefficient at 40 °C to 85 °C was 14.0×10 -5 / °C.

[0100] From these results, the obtained film had negative birefringence, a large refractive index in the thickness direction, small wavelength dependence, and excellent dimensional stability, so it was suitable for an optical film.

[0101] Example 3 To 100 parts by weight of the diisopropyl fumarate - di - n - butyl fumarate copolymer obtained in Synthesis Example 3, 3 parts by weight of silicone resin KR - 220L (Shin - Etsu Chemical Co., Ltd.) was blended, dissolved in a toluene - methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto a support substrate of a solution casting apparatus by the T - die method, dried at 80 °C and 130 °C for 4 minutes each, and a film with a width of 250 mm and a thickness of 45 μm was obtained.

[0102] From the results of the three-dimensional refractive index measurement of the film (nx = 1.4798, ny = 1.4799, nz = 1.4838), the obtained film had a refractive index in the film thickness direction of nx ≦ ny < nz. The in-plane retardation Re = (ny - nx) × d was 4.5 nm, the out-of-plane retardation Rth = 〔(nx + ny) / 2 - nz〕× d was -178 nm, the ratio of retardations (R450 / R550) (wavelength dependence) was 1.01, and the linear expansion coefficient at 40°C to 85°C was 13.8×10 -5 / °C.

[0103] From these results, the obtained film had negative birefringence, a large refractive index in the thickness direction, low wavelength dependence, and excellent dimensional stability, making it suitable for an optical film.

[0104] Example 4 To 100 parts by weight of the diisopropyl fumarate·bis(2-ethylhexyl) fumarate copolymer obtained in Synthesis Example 4, 10 parts by weight of silicone resin RSN-217 (Dow Corning) was blended, dissolved in a toluene·methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto a support substrate of a solution casting apparatus by the T-die method, dried at 80°C and 130°C for 4 minutes each, and a film with a width of 250 mm and a thickness of 40 μm was obtained.

[0105] From the results of the three-dimensional refractive index measurement of the film (nx = 1.4798, ny = 1.4799, nz = 1.4838), the obtained film had a refractive index in the film thickness direction of nx ≦ ny < nz. The in-plane retardation Re = (ny - nx) × d was 4.0 nm, the out-of-plane retardation Rth = 〔(nx + ny) / 2 - nz〕× d was -158nm , the ratio of retardations (R450 / R550) (wavelength dependence) was 1.01, and the linear expansion coefficient at 40°C to 85°C was 14.2×10 -5 / °C.

[0106] From these results, the obtained film had negative birefringence, a large refractive index in the thickness direction, low wavelength dependence, and excellent dimensional stability, making it suitable for an optical film.

[0107] Example 5 Diisopropyl fumarate - di - n - octyl fumarate copolymer obtained in Synthesis Example 5 100 weight units To this, 3 parts by weight of silicone resin RSN - 217 (Dow Corning) was added, dissolved in a toluene - methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto the support substrate of a solution casting apparatus by the T - die method, dried at 80 °C and 130 °C for 4 minutes each, and a film with a width of 250 mm and a thickness of 50 μm was obtained. The obtained film was cut into 50 mm - square pieces and biaxially stretched by a biaxial stretching apparatus (manufactured by Imoto Seisakusho) under the conditions of a temperature of 150 °C and a stretching rate of 10 mm / min. to a 1.25 - fold stretch.

[0108] From the results of measuring the three - dimensional refractive index of the film (nx = 1.4670, ny = 1.4705, nz = 1.4725), the refractive index in the film thickness direction of the obtained film was nx ≦ ny < nz and was large. The in - plane retardation Re=(ny - nx)×d was 157 nm, the out - of - plane retardation Rth = 〔(nx + ny) / 2 - nz〕×d was - 168 nm, the ratio of retardations (R450 / R550) (wavelength dependence) was 1.02, and the linear expansion coefficient at 40 °C to 85 °C was 13.2×10 -5 / °C.

[0109] From these results, the obtained film had negative birefringence, a large refractive index in the thickness direction, small wavelength dependence, and excellent dimensional stability, and was thus suitable for an optical film.

[0110] Comparative Example 1 The diisopropyl fumarate polymer obtained in Synthesis Example 1 was dissolved in a toluene - methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto the support substrate of a solution casting apparatus by the T - die method, dried at 80 °C and 130 °C for 4 minutes each, and a film with a width of 250 mm and a thickness of 50 μm was obtained.

[0111] From the results of the three-dimensional refractive index measurement of the film (nx = 1.4779, ny = 1.4780, nz = 1.4823), the refractive index in the film thickness direction of the obtained film was nx ≦ ny < nz and was large. The in-plane retardation Re = (ny - nx) × d was 5.0 nm, the out-of-plane retardation Rth = 〔(nx + ny) / 2 - nz〕× d was -218 nm, the ratio of retardations (R450 / R550) (wavelength dependence) was 1.01, and the linear expansion coefficient at 40°C to 85°C was 18.0×10 -5 / °C.

[0112] From these results, the obtained film had problems with dimensional stability.

[0113] Comparative Example 2 To 100 parts by weight of the diisopropyl fumarate polymer obtained in Synthesis Example 1, 30 parts by weight of silicone resin RSN-217 (Dow Corning) was blended, dissolved in a toluene / methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone = 50 wt% / 50 wt%) to form a 20% solution, cast onto a support substrate of a solution casting apparatus by the T-die method, dried at 80°C and 130°C for 4 minutes each, and a film having a width of 250 mm and a thickness of 50 μm was obtained.

[0114] The appearance of the obtained film was opaque and not suitable for an optical film.

Claims

1. A resin composition containing no spherical inorganic particles, and containing 80% by weight or more and 99.9% by weight or less of a fumaric acid ester-based polymer containing a fumaric acid diester residue represented by the following general formula (1), and 0.1% by weight or more and 20% by weight or less of a silicone resin represented by the following general formula (2) and having a weight average molecular weight of 1,426 to 10,000: 【Chemistry 1】 (In the formula, R 1 and R 2 each independently represents one of the group consisting of a linear or branched alkyl group having 1 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms. 【Chemistry 2】 (In the formula, R 3 , R 4 , R 5 , R 6 , R 7 , R 8 each independently represents one of the group consisting of hydrogen, a hydroxyl group, a phenyl group, a methyl group, an ethyl group, an isopropyl group, an n-propyl group, and a methoxy group, and at least a methyl group and / or a phenyl group are present, and a hydroxyl group is also present. Here, a+b+c+d=1, a≧0, b>0, c>0, d≧0, and (c+d) is 0.4 or more and less than 1.

0.

2. 2. The resin composition according to claim 1, wherein the fumaric acid ester polymer is a copolymer containing 30 mol % or more of the fumaric acid diester residue unit represented by the general formula (1).

3. The resin composition according to claim 1 or 2, characterized in that the fumaric acid diester residue represented by the general formula (1) is at least one kind of fumaric acid diester residue selected from dimethyl fumarate residue, diethyl fumarate residue, diisopropyl fumarate residue, di-tert-butyl fumarate residue, di-n-butyl fumarate residue, di-sec-butyl fumarate residue, isobutyl fumarate residue, dipentyl fumarate residue, diisopentyl fumarate residue, di-sec-isoamyl fumarate residue, dineopentyl fumarate residue, di-tert-pentyl fumarate residue, di-2-ethylhexyl fumarate residue, dicyclopropyl fumarate residue, dicyclobutyl fumarate residue, dicyclopentyl fumarate residue and dicyclohexyl fumarate residue.

4. 4. An optical film comprising the resin composition according to claim 1, wherein the refractive index in the fast axis direction in the film plane is nx, the refractive index in the direction perpendicular thereto is ny, and the refractive index in the thickness direction of the film is nz, the relationship being nx≦ny<nz, and the ratio (R450 / R550) of the retardation measured with light having a wavelength of 450 nm to the retardation measured with light having a wavelength of 550 nm is 1.1 or less.

Citation Information

Patent Citations

  • Composite membrane for separating gas

    JP1987282620A

  • Manufacturing method of birefringent film, retardation plate and liquid crystal display device using the same

    JP1993297223A

  • Production of double refraction film, phase shifter and liquid crystal display device

    JP1993323120A

  • Production of double refraction film and liquid crystal display device using the double refraction film

    JP1994088909A

  • Optical film and liquid crystal display device

    JP2001091746A