Multiple Containers
The multi-layer container addresses thermal contraction issues by using higher intrinsic viscosity resin for the outer container and an air introduction system to prevent cooling water ingress, ensuring effective product integrity.
Patent Information
- Application Number
- JP2020040734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-03-10
AI Technical Summary
In existing multi-layer containers, high-temperature filling leads to thermal contraction differences between the inner and outer containers, creating voids where cooling water can enter during the cooling process, resulting in defective products.
The multi-layer container design includes an outer container with a higher intrinsic viscosity resin than the inner container, coupled with an outside air introduction system to equalize thermal shrinkage, preventing water ingress into the gap.
This design reduces thermal shrinkage differences, minimizing void formation and preventing cooling water entry, thus reducing defective products.
Smart Images

Figure 0007562964000001 
Figure 0007562964000002 
Figure 0007562964000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-container. [Background technology]
[0002] 2. Description of the Related Art Multi-layer containers, also known as freshness-preserving containers, airless bottles, or peelable laminated containers, are known as containers for storing contents such as liquid seasonings or liquid cosmetics and preserving the freshness of the contents (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-186059 A Summary of the Invention [Problem to be solved by the invention]
[0004] Meanwhile, methods of filling contents into multi-layer containers include a room temperature filling method in which the contents are filled at room temperature, and a high temperature filling method in which hot contents heated to a predetermined temperature above room temperature are filled. In the room temperature filling method, the room temperature contents are filled, and then a cap is attached to finish the filling process. On the other hand, in the high temperature filling method, after the filling process in which hot contents are filled into the blow-molded container by the high temperature filling process, a cooling process is performed in which cooling water is sprayed over the entire container with the cap attached and sealed to cool the contents to room temperature.
[0005] In general multi-layer containers, including the multi-layer container of Patent Document 1, the inner container undergoes thermal shrinkage due to high-temperature filling, causing the gap (hereinafter simply referred to as "gap") formed between the outer container and the inner container to be in a decompressed state. As a result, cooling water sprayed after high-temperature filling may be sucked through the gap between the cap and the mouth, and into the gap through an outside air inlet hole provided in the mouth. It is difficult to remove the cooling water that has entered the gap, and depending on the amount of water that has entered, it may be necessary to dispose of the product as a defective product.
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a multi-layer container capable of preventing water from entering a gap between an inner container and an outer container that occurs after hot filling. [Means for solving the problem]
[0007] The multi-layer container according to the present invention is a multi-layer container including a container body in which an inner container for accommodating contents and an outer container which contains the inner container and has an outside air introduction hole for introducing outside air into a gap formed between the inner container and the outer container are peelably laminated, the outer container and the inner container are formed into a bottle shape by stretch blow molding using a polyester-based resin, an outside air introduction path is provided for guiding the outside air introduced from the outside air introduction hole to the gap, and the difference between the shrinkage rate of the inner container and the shrinkage rate of the outer container due to thermal shrinkage after filling the inner container with high temperatures equal to or higher than room temperature is 2.5% or less, In a cooling step after the hot filling of the contents, the contents are cooled by spraying cooling water. When the gap is brought into a negative pressure state due to the thermal contraction, the outside air is introduced from the outside air introduction hole through the outside air introduction path into the gap, while the outside air is introduced from the outside air introduction hole to the gap. The cooling Water ingress Prevent do.
[0008] Preferably, in the multiple container, the intrinsic viscosity of the resin of the outer container is greater than the intrinsic viscosity of the resin of the inner container.
[0009] Preferably, in the multi-layer container, the intrinsic viscosity of the resin used to mold the outer container is 0.78 or more and 0.88 or less, and the intrinsic viscosity of the resin used to mold the inner container is 0.68 or more and 0.78 or less.
[0010] Preferably, in the multi-layer container, the intrinsic viscosity of the resin of the molded outer container is 0.75 or more and 0.85 or less, and the intrinsic viscosity of the resin of the molded inner container is 0.65 or more and 0.75 or less.
[0011] Preferably, in the multi-layer container, the outer container bends inward and deforms when pressed by a squeeze operation, and restores to its original shape before pressing when the pressure is released by stopping the squeeze operation, and the inner container shrinks as the contents decrease when the contents are poured out by squeezing the outer container.
[0013] Preferably, in the multi-layer container, the container body has heat resistance against the contents filled therein at a temperature equal to or higher than room temperature.
[0014] Preferably, in the multi-layer container, the outside air introduction hole is provided in the mouth of the container body, and the mouth of the container body is thermally crystallized. Effect of the Invention
[0015] The multi-layer container according to the present invention can prevent water from entering the gap between the inner container and the outer container that occurs after hot filling. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a schematic diagram showing a vertical cross section of the multi-layer container according to the present embodiment. [Diagram 2] 1 is a table showing various characteristics of the outer container and inner container of the multi-layer container according to the present embodiment and various characteristics of the outer container and inner container of a conventional multi-layer container. [Diagram 3] 1 is a table showing various characteristics and evaluation results of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0018] In this embodiment, the direction along the central axis Z of the bottle-shaped multi-container 1 is also referred to as the "axial direction", the direction rotating around the central axis Z of the multi-container 1 as the rotation axis is also referred to as the "circumferential direction", and the direction perpendicular to the central axis Z of the multi-container 1 is also referred to as the "radial direction". In this embodiment, the axial direction from the mouth 3 to the bottom 6 of the multi-container 1 is also referred to as the "downward", and the axial direction from the bottom 6 to the mouth 3 of the multi-container 1 is also referred to as the "upward". In this embodiment, the cross section of the multi-container 1 cut along a plane along the central axis Z of the multi-container 1 is also referred to as the "longitudinal cross section", and the cross section of the multi-container 1 cut along a plane perpendicular to the central axis Z of the multi-container 1 is also referred to as the "transverse cross section".
[0019] Fig. 1 is a schematic diagram showing a vertical cross section of a multi-layer container 1 according to this embodiment. Note that Fig. 1 shows the multi-layer container 1 in a state after the inner surface of the outer container 10 and the outer surface of the inner container 20 have been peeled off, such as the state after the multi-layer container 1 is filled with the contents.
[0020] The multi-layer container 1 is a bottle-shaped container. As shown in Fig. 1, the multi-layer container 1 includes a mouth 3 which is one end of a container body 2 and has a pouring outlet 21 for the contents, a bottom 6 which is the other end of the container body 2 and has a grounding surface, a shoulder 4 which extends downward while spreading outward in the radial direction from the mouth 3, and a body 5 which extends downward from the shoulder 4 and is connected to the bottom 6.
[0021] The multi-layer container 1 comprises a bottle-shaped outer container 10 that constitutes the outer shell of the multi-layer container 1 and encloses an inner container 20, and the inner container 20 that contains the contents and has a shape that conforms to the inner surface of the outer container 10. The multi-layer container 1 is a freshness-preserving container (also called an airless bottle) in which the inner surface of the outer container 10 and the outer surface of the inner container 20 are laminated in a peelable manner.
[0022] The multi-layer container 1 has an outside air introduction hole 11 capable of introducing outside air between the outer container 10 and the inner container 20. Specifically, the outside air introduction hole 11 is provided in the mouth 3 of the outer container 10 and communicates with the gap A, as shown in FIG. 1. Alternatively, the outside air introduction hole 11 can be provided as a slit in the portion where the mouth 3 of the outer container 10 and the mouth 3 of the inner container 20 are fixed. Furthermore, the multi-layer container 1 is provided with an outside air introduction path A1 between the mouth 3 of the outer container 10 and the mouth 3 of the inner container 20, which introduces outside air introduced from the outside air introduction hole 11 into the gap A. When the gap A is in a negative pressure state, the outside air is introduced from the outside air introduction hole 11 and introduced into the gap A via the outside air introduction path A1.
[0023] The outer container 10 and the inner container 20 are containers made of thermoplastic resin and are manufactured by blow molding. Preferably, the outer container 10 and the inner container 20 are manufactured by biaxial stretch blow molding using a tubular preform such as a test tube shape. Specifically, the outer container 10 and the inner container 20 are manufactured by simultaneously stretch blow molding the preform of the outer container 10 and the preform of the inner container 20 in a state where the preform of the inner container 20 is inserted into the preform of the outer container 10 and stacked. Alternatively, the outer container 10 and the inner container 20 may be manufactured by stretch blow molding the preform of the outer container 10 and then stretch blow molding the preform of the inner container 20 inside the outer container 10. In the blow molding, the mouth portion 3 of the outer container 10 and the inner container 20 become a non-stretched portion, and the shoulder portion 4, the body portion 5, and the bottom portion 6 become stretched portions.
[0024] The outer container 10 and the inner container 20 are molded using a polyester-based resin. Examples of the polyester-based resin include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and copolymer polyesters thereof. Preferably, the outer container 10 and the inner container 20 are molded using a polyethylene terephthalate resin.
[0025] As an example of a method for peeling the inner container 20 from the outer container 10, the inner container 20 is thermally shrunk by a high-temperature filling process to promote peeling. In the high-temperature filling process, the content liquid is filled at a high temperature, so the mouth portion 3 may be heat-treated at the preform stage to thermally crystallize and suppress deformation of the mouth portion 3. The content of the multi-layer container 1 may be, for example, a beverage heated to a high temperature (either a hot beverage or a cold beverage) or a liquid seasoning heated to a high temperature. Here, "high temperature" refers to a temperature at which the content is heated to a temperature higher than room temperature, and refers to, for example, about 65°C to 85°C.
[0026] In the blow molding process for the multi-layer container 1, blow air is blown into the preform inside the heated blow mold, and at the same time, a stretch rod is stretched and pressed against the blow mold, and cooled air is blown in to mold an outer container 10 and an inner container 20 in a shape that matches the blow mold.
[0027] During this process, distortion occurs in each of the outer container 10 and the inner container 20 due to stretching, etc. This distortion is alleviated by heat setting of the blow mold, but is not completely removed and remains in the outer container 10 and the inner container 20 after molding. For this reason, when the multi-layer container 1 is heated after molding, the residual distortion present in the outer container 10 and the inner container 20 is alleviated and thermal shrinkage occurs. In particular, in the filling process of the contents that is carried out after molding, the container is subjected to heat sterilization treatment and high-temperature filling in which the contents are filled at a high temperature is carried out, so that the multi-layer container 1 is heated after molding and thermal shrinkage occurs.
[0028] FIG. 2 is a table showing various characteristics of the outer container 10 and the inner container 20 of the multi-layer container 1 according to this embodiment and various characteristics of the outer container and the inner container of a conventional multi-layer container. As shown in FIG. 2, in the conventional multi-layer container, the resins used are the same from the viewpoint of recyclability and production efficiency, and are manufactured using a resin with a relatively low intrinsic viscosity (IV) so that it can withstand high-temperature filling. Therefore, the amount of heat shrinkage occurring after molding of the conventional multi-layer container is likely to be larger in the inner container than in the outer container. This is because the inner container may have a larger residual strain than the outer container. One factor that causes the residual strain of the inner container to be larger than that of the outer container is that the inner container has a geometrically higher stretch ratio than the outer container. Another factor that causes this is that when the residual strain is relieved by heat setting, the outer container is in contact with the blow mold while the inner container is not in contact with the blow mold, so the effect of relieving the residual strain by heat setting is smaller than that of the outer container. Another factor that causes this is that the thermal crystallization of the inner container is more difficult to promote than that of the outer container during heat setting, so the inner container has a lower crystallization degree and lower heat resistance.
[0029] Thus, in conventional multi-layer containers, the amount of thermal shrinkage of the inner container is relatively larger than that of the outer container, so that the outer surface of the inner container that was in close contact with the inner surface of the outer container may peel off from the inner surface of the outer container, forming a gap between the outer container and the inner container. That is, the gap is a space formed between the outer container and the inner container by the peeling off of the outer container and the inner container. In general, the mouth of a multi-layer container is a non-stretched portion that is not stretched, and the bottom can be configured not to peel off, so the gap is at least a space formed by the peeling off of the body of the inner container and the body of the outer container due to thermal shrinkage after molding.
[0030] However, conventional multi-layer containers are manufactured using a resin with a relatively low intrinsic viscosity, and so large voids are easily formed due to the difference in the amount of thermal shrinkage between the inner container and the outer container. As a result, when the inner container thermally shrinks, the pressure in the voids is reduced to a negative pressure, and the cooling water sprayed during the cooling process is sucked in through the outside air inlet and enters the voids, which is a problem.
[0031] Therefore, in the multi-layer container 1 of this embodiment, in order to reduce the difference in the amount of thermal shrinkage between the outer container 10 and the inner container 20, the intrinsic viscosities of the outer container 10 and the inner container 20 are configured as shown in FIG.
[0032] 2, the multi-layer container 1 of this embodiment is configured so that the intrinsic viscosity of the resin of the outer container 10 is greater than the intrinsic viscosity of the resin of the inner container 20. The intrinsic viscosity of a resin is correlated with the molecular weight of the resin, and a resin with a small intrinsic viscosity is often a low molecular weight resin, while a resin with a large intrinsic viscosity is often a high molecular weight resin.
[0033] The outer container 10, which is molded from a resin with a relatively high intrinsic viscosity, has relatively long molecular chains that tend to tangle when stretched during blow molding, and many of the molecular chains are difficult to move and solidify while tangled, so that residual distortion is likely to be large. The residual distortion of the outer container 10 is easily alleviated during heat setting, but since a resin with a relatively high intrinsic viscosity is used, thermal crystallization due to heat setting is less likely to occur than in the outer container of a conventional multi-layer container, and distortion is also less likely to be alleviated, so the residual distortion is also large. For this reason, when the outer container 10 is heated after molding, the amount of thermal shrinkage is greater than that of the outer container of a conventional multi-layer container.
[0034] On the other hand, the inner container 20 made of a resin with a relatively low intrinsic viscosity has relatively short molecular chains, similar to the inner containers of conventional multi-layer containers, and therefore the molecular chains are less likely to become entangled during stretching in blow molding, and the residual distortion is relatively small. The inner container 20 uses a resin with a relatively low intrinsic viscosity, so the residual distortion is relatively small, but like conventional inner containers, the residual distortion is difficult to relieve during heat setting.
[0035] In this way, in the multi-layer container 1 of this embodiment, the resins of each container are set so that the intrinsic viscosity of the resin used in molding the outer container 10 is relatively higher than that of the resin used in molding the inner container 20. As a result, the amount of thermal shrinkage of the outer container 10 approaches that of the inner container 20, and the difference between the amounts of thermal shrinkage of the outer container 10 and the inner container 20 due to thermal shrinkage after molding is reduced to a level that is approximately equal or slightly smaller than that of the inner container 20, so that the amount of space A formed is reduced to a level at which the outer container 10 and the inner container 20 are peeled off. Therefore, even if the pressure of the space A is reduced by thermal shrinkage after the high-temperature filling process, cooling water will not enter the space A through the outside air introduction hole 11.
[0036] In particular, in the multi-layer container 1, the resin (pellets) used to mold the outer container 10 has an intrinsic viscosity of 0.78 or more and 0.88 or less, and the resin (pellets) used to mold the inner container 20 has an intrinsic viscosity of 0.68 or more and 0.78 or less, so that the molded outer container 10 has an intrinsic viscosity of 0.75 or more and 0.85 or less, and the molded inner container 20 has an intrinsic viscosity of 0.65 or more and 0.75 or less. The reason why the intrinsic viscosity of the resin (pellets) used to mold the outer container 10 and the inner container 20 is made slightly higher than the intrinsic viscosity of the molded outer container 10 and the inner container 20 is that when the outer container 10 and the inner container 20 are molded using a polyester-based resin, the intrinsic viscosity value becomes smaller due to injection molding caused by the hydrolysis reaction of the polyester-based resin.
[0037] Here, the resin used to mold the inner container 20 may be polyethylene terephthalate resin used to mold so-called heat-resistant PET bottles. Furthermore, the resin used to mold the outer container 10 may be polyethylene terephthalate resin used to mold general non-heat-resistant PET bottles. In the multi-layer container 1, the difference between the amount of thermal shrinkage of the outer container 10 and the amount of thermal shrinkage of the inner container 20 due to thermal shrinkage after molding is reduced to be equal or slightly smaller, thereby making it possible to reduce the amount of space A to an extent that the outer container 10 and the inner container 20 can be peeled off.
[0038] Furthermore, in order to reduce the amount of void A, it is preferable to set the difference in shrinkage rate between the outer container 10 and the inner container 20 before and after high-temperature filling to 2.5% or less. This difference in shrinkage rate is the difference in the rate (shrinkage rate) of change in the respective volumes of the outer container 10 and the inner container 20 due to thermal shrinkage before and after high-temperature filling. By making the intrinsic viscosity of the outer container 10 relatively higher than that of the inner container 20, the difference between the amount of thermal shrinkage of the outer container 10 and the amount of thermal shrinkage of the inner container 20 can be reduced.
[0039] In a conventional multi-layer container, the difference in the amount of thermal shrinkage between the outer container and the inner container is relatively large as shown in Fig. 2, so the amount of void (porosity) of gap A is naturally large. In contrast, in the multi-layer container 1 of the present embodiment, the amount of thermal shrinkage of the outer container 10 is larger than that of the conventional multi-layer container, so the difference with the amount of thermal shrinkage of the inner container 20 is reduced, and the amount of void A formed after thermal shrinkage can be reduced.
[0040] [Effects] As described above, in the multi-layer container 1 according to the present embodiment, the outer container 10 and the inner container 20 are molded using the same type of resin and are configured to have the characteristics shown in FIG. 2. As a result, in the multi-layer container 1 according to the present embodiment, the difference between the thermal shrinkage amount of the outer container 10 and the thermal shrinkage amount of the inner container 20 can be reduced so that they are substantially equal or the inner container 20 is slightly smaller. Therefore, in the multi-layer container 1 according to the present embodiment, the difference in the thermal shrinkage amount between the outer container 10 and the inner container 20 is reduced, so that the amount of void A formed by thermal shrinkage after high-temperature filling is reduced. This means that when the void A is in a negative pressure state, the amount of outside air introduced can be controlled to a small amount. Therefore, the multi-layer container 1 according to the present embodiment 1 can prevent the cooling water sprayed in the cooling process after the high-temperature filling process from being sucked into the void A, and can suppress the occurrence of defective products in which water has entered the void A.
[0041] [others] In the above-described embodiment, the multi-layer container 1 is a container in which the outer container 10 forms the outer shell of the multi-layer container 1 and the inner container 20 contains the contents. However, the multi-layer container 1 is not limited to a container in which the outer container 10 forms the outer shell of the multi-layer container 1 and the inner container 20 contains the contents. In other words, the multi-layer container 1 may have a container forming the outer shell of the multi-layer container 1 provided further outside the outer container 10, or a container that contains the contents provided further inside the inner container 20. In this way, the multi-layer container 1 only needs to function as a laminate in which the outer container 10 and the inner container 20 are peelably stacked adjacent to each other and form a gap A between them, and may naturally be a container having a triple or more multi-layer structure capable of forming a plurality of gaps A.
[0042] In the above-described embodiment, the multi-layer container 1 corresponds to an example of a "multi-layer container" as described in the claims. The container body 2 corresponds to an example of a "container body" as described in the claims. The mouth portion 3 corresponds to an example of a "mouth portion" as described in the claims. The outer container 10 corresponds to an example of an "outer container" as described in the claims. The inner container 20 corresponds to an example of an "inner container" as described in the claims. The outside air introduction hole 11 corresponds to an example of an "outside air introduction hole" as described in the claims. The gap A corresponds to an example of a "gap" as described in the claims. The outside air introduction path A1 corresponds to an example of an "outside air introduction path" as described in the claims.
[0043] The terms used in the above embodiments and claims should be interpreted as open-ended terms. For example, the term "including" should be interpreted as "not limited to what is described as including." The term "comprises" should be interpreted as "not limited to what is described as comprising." The term "has" should be interpreted as "not limited to what is described as having." EXAMPLES
[0044] The present invention will be described in more detail below using examples, but the present invention is not limited thereto.
[0045] [1. Creation of multi-container] - Preform molding - The preforms for the outer container and the inner container were produced by injection molding using an existing injection molding machine using the PET resin used in Example 1. Similarly, the preforms for the outer container and the inner container were each produced by injection molding using the PET resin used in Comparative Examples 1 to 3. - Molding of multi-layer containers - The preform to become the inner container was inserted into the preform to become the outer container of Example 1, and heated to 100-110°C in this stacked state, after which the preform to become the outer container and the preform to become the inner container were simultaneously stretch-blow molded to obtain a multi-layer container 1. Similarly, the preform to become the outer container and the preform to become the inner container were simultaneously stretch-blow molded to obtain a multi-layer container for Comparative Examples 1-3. The multi-layer containers produced in Example 1 and Comparative Examples 1-3 each had a full capacity (maximum amount of liquid that can be accommodated in the container) of about 460 ml.
[0046] [2. Heat shrink method for multi-layer containers] The multi-layer container thus prepared was filled with 400 g of hot water heated to 75°C as the content, and after sealing the opening with a cap, it was kept in an upright position for 5 minutes. The cap used was a cap equipped with an outside air inlet that can introduce outside air into the outside air inlet hole, and a check valve that opens the outside air inlet when introducing outside air and closes the outside air inlet after introducing outside air. Next, the multi-layer container filled with warm water was cooled for 3 minutes by spraying 20°C cooling water from a shower onto the top of the container. The amount of cooling water sprayed from the shower was set so that the temperature of the contents (water) after cooling would be 50°C. After this point, no thermal shrinkage of the multi-layer container was observed even though the temperature of the contents dropped.
[0047] [3. Measurement of multi-container characteristics] 3 is a table showing the various properties, measurement results, and evaluation results of the multi-layer containers of Example 1 and Comparative Examples 1 to 3. The properties (intrinsic viscosity, shrinkage rate, shrinkage amount, porosity, and void volume) of Example 1 and Comparative Examples 1 to 3 were measured and calculated by the following methods.
[0048] -Intrinsic viscosity- Of the multi-walled containers after blow molding, a portion near the mouth, which is a non-stretched portion that has not been thermally crystallized, was cut out and dried at 150°C for 4 hours, and then 0.3 g was weighed out. A mixed solvent of 1,1,2,2-tetrachloroethane and phenol in a weight ratio of 50:50 was added to this to adjust the concentration to 1.00 g / dl, and the mixture was stirred at 120°C for 20 minutes to completely dissolve it. After cooling the dissolved solution to room temperature, the relative viscosity was measured using a relative viscometer (Y501, manufactured by Viscotek) adjusted to 30°C, and the intrinsic viscosity was calculated.
[0049] As shown in FIG. 3, the intrinsic viscosity of the polyester resin pellets (PET resin) of the outer container and the intrinsic viscosity of the polyester resin pellets (PET resin) of the inner container used in the multi-layer container of this embodiment (Example 1) were as follows. Intrinsic viscosity of PET resin pellets in outer container: 0.85 Intrinsic viscosity of PET resin pellets in inner container: 0.74 As shown in FIG. 3, the intrinsic viscosities of the polyester resin pellets (PET resin) of the outer container and the polyester resin pellets (PET resin) of the inner container used in Comparative Examples 1 to 3 were as follows. Comparative Example 1 Intrinsic viscosity of PET resin pellets in outer container: 0.85 Intrinsic viscosity of PET resin pellets in the container: 0.85 Comparative Example 2 Intrinsic viscosity of PET resin pellets in outer container: 0.74 Intrinsic viscosity of PET resin pellets in inner container: 0.74 Comparative Example 3 Intrinsic viscosity of PET resin pellets in outer container: 0.74 Intrinsic viscosity of PET resin pellets in the container: 0.85
[0050] The intrinsic viscosity of the outer container 10 and the inner container 20 of the multi-layer container 1 molded from PET resin pellets were as follows. Example 1 Intrinsic viscosity of outer container: 0.75 Intrinsic viscosity of inner container: 0.65 Comparative Example 1 Intrinsic viscosity of outer container: 0.75 Intrinsic viscosity of inner container: 0.75 Comparative Example 2 Intrinsic viscosity of outer container: 0.65 Intrinsic viscosity of inner container: 0.65 Comparative Example 3 Intrinsic viscosity of outer container: 0.65 Intrinsic viscosity of inner container: 0.75
[0051] - Shrinkage rate - (Shrinkage rate of inner container) A full volume (g) of water at 20°C was poured into the inner container of the multi-layer container after blow molding (hereinafter referred to as the "container before shrinkage") and the multi-layer container after heat shrinkage by the heat shrinking method (hereinafter referred to as the "container after shrinkage"), and the volumes before and after heat shrinkage were measured. The measured content volume (g) was converted to volume (cc), and the shrinkage rate (%) of the inner container was calculated from the change in volume before and after heat shrinkage. For the container after shrinkage, the full volume (g) was measured after removing the cap used during filling. Example 1 Container shrinkage rate: 5% Comparative Example 1 Container shrinkage rate 10% Comparative Example 2 Container shrinkage rate: 4% Comparative Example 3 Container shrinkage rate: 9% (Outer container shrinkage rate) For the container before shrinkage, 400g of water at 20°C was poured in as the content, and the container was capped. In this state, the container was immersed in a container containing a specified amount of water as the immersion liquid, and the volume (cc) was measured by Archimedes' method. At the time of measurement, water was poured into the container, and since the outer container has a specified thickness, shrinkage due to water pressure was considered to be negligible. In addition, since the container thickness is about 300 μm, which is thin enough to be negligible in volume, the volume including the container thickness was substituted for the content (g) of the outer container. For the shrunken container, the container filled with hot water by the above-mentioned heat shrinking method was cooled to room temperature, and in the same manner as for the unshrunken container, it was immersed in a container with a capped state into a container containing a predetermined amount of water as an immersion liquid, and the volume (cc) was measured by the Archimedes method. The shrinkage rate (%) of the outer container was calculated from the volume change of the outer container before and after the shrinkage. Example 1 Outer container shrinkage rate: 3% Comparative Example 1 Outer container shrinkage rate: 4% Comparative Example 2 Outer container shrinkage rate 0% Comparative Example 3 Outer container shrinkage rate 0%
[0052] -Difference in shrinkage rate- The difference in shrinkage rate between the outer container and the inner container was calculated from the shrinkage rate of the inner container and the shrinkage rate of the outer container using the following formula 1. Formula 1: "Difference in shrinkage rate (%)" = "Shrinkage rate of inner container (%)" - "Shrinkage rate of outer container (%)" Example 1 Shrinkage rate difference: 2% Comparative Example 1 Shrinkage rate difference: 6% Comparative Example 2 Shrinkage rate difference: 4% Comparative Example 3 Shrinkage rate difference: 9%
[0053] -Void volume / porosity- The void volume (cc) was calculated from the following formula 2. Formula 2: "Void volume (cc)" = "Inner container shrinkage volume (cc)" - "Outer container shrinkage volume (cc)" The porosity (%) of the multi-layer container was calculated from the following formula 3. Formula 3: "Void ratio (%)" = "Void volume (cc)" / "Full capacity of inner container before shrinkage (cc)" x 100 Example 1 Vacancy amount: 9cc, porosity: 1.95% Comparative Example 1 Void amount: 26cc, porosity: 5.65% Comparative Example 2 Void amount: 18cc, porosity: 3.91% Comparative Example 3 Void amount: 40cc, porosity: 8.96%
[0054] [5. Evaluation Results] The presence or absence of water infiltration into the gaps of the multi-layer container of Example 1 and the multi-layer containers of Comparative Examples 1 to 3 was evaluated. The evaluation method was a visual sensory evaluation of the multi-layer containers that had been subjected to the high-temperature filling process and the cooling process by the above-mentioned heat shrinkage method. The evaluation results are shown in Figure 3. -Judgment criteria- ○: No cooling water infiltration was confirmed in the gap (good enough to be used as a product) ×: Cooling water was found to have entered the gap (defective product that cannot be used as a product)
[0055] In Example 1, as shown in Fig. 3, no infiltration of water into the gap was confirmed, and good results were obtained. In Example 1, as shown in Fig. 3, a resin was selected so that the intrinsic viscosity of the outer container was higher than that of the inner container, and as a result, the amount of thermal shrinkage of the outer container approached the amount of thermal shrinkage of the inner container, and the difference in the shrinkage rates of the outer container and the inner container was reduced, and it was confirmed that the gaps formed after thermal shrinkage were reduced. Therefore, the multi-layer container of Example 1 was proven to be useful as a container for products that store high-temperature contents in a high-temperature filling process, as it prevents water sprayed during the cooling process after high-temperature filling from infiltrating into the gaps.
[0056] On the other hand, ingress of water into the gap was confirmed in all of Comparative Examples 1 to 3, as shown in Fig. 3. The reason for water ingress into the gap is presumably that the difference between the amount of thermal shrinkage of the outer container and the amount of thermal shrinkage of the inner container was relatively large compared to Example 1 due to the use of containers in which the intrinsic viscosity of the outer container and the intrinsic viscosity of the inner container were equivalent (Comparative Examples 1 and 2) or a container in which the intrinsic viscosity of the outer container was lower than that of the inner container (Comparative Example 3), resulting in a larger void volume of the resulting gap. [Explanation of symbols]
[0057] 1 multiple containers 2 Container body 3 Mouth 4 Shoulder 5. Torso 6 Bottom 10 Outer container 11. Outside air intake 20 Inner container 21 Spout A void A1 Outside air intake S Storage space Z center axis
Claims
1. A multi-layer container including an inner container for accommodating a content, and an outer container for containing the inner container and having an outside air introduction hole for introducing outside air into a space formed between the inner container and the outer container, the multi-layer container including a container body that is peelably stacked, The outer container and the inner container are formed into a bottle shape by stretch blow molding using a polyester resin, an outside air introduction path is provided to introduce the outside air introduced through the outside air introduction hole into the gap; The difference between the shrinkage rate of the inner container and the shrinkage rate of the outer container due to thermal shrinkage after filling the contents at a temperature equal to or higher than room temperature is 2.5% or less; In a cooling step after the hot filling of the contents, the contents are cooled by spraying cooling water, When the gap is put into a negative pressure state due to the thermal contraction of the contents after the high-temperature filling, the outside air is introduced into the gap from the outside air introduction hole through the outside air introduction path. preventing the cooling water from entering the gap through the outside air introduction hole; Multiple containers.
2. The intrinsic viscosity of the resin of the outer container is greater than the intrinsic viscosity of the resin of the inner container. The multi-container of claim 1.
3. The intrinsic viscosity of the resin used for molding the outer container is 0.78 or more and 0.88 or less, The intrinsic viscosity of the resin used to mold the inner container is 0.68 or more and 0.78 or less. The multi-container of claim 2.
4. The intrinsic viscosity of the resin of the molded outer container is 0.75 or more and 0.85 or less, The intrinsic viscosity of the resin of the molded inner container is 0.65 or more and 0.75 or less. The multi-container according to claim 2 or 3.
5. When the outer container is pressed by a squeezing operation, it bends inward and deforms, and when the pressure is released by stopping the squeezing operation, it returns to its original shape before the pressure was applied. When the contents are poured out by squeezing the outer container, the inner container shrinks as the contents decrease. The multi-layer container according to any one of claims 1 to 4.
6. The container body has heat resistance against the contents to be filled at a temperature equal to or higher than room temperature. The multi-layer container according to any one of claims 1 to 5.
7. The outside air introduction hole is provided at the mouth of the container body, The mouth of the container body is thermally crystallized. The multi-layer container according to any one of claims 1 to 6.
Citation Information
Patent Citations
Manufacture of heat insulating container
JP1993031800A
Synthetic resin double container
JP2010126207A
Polyester expanded foam container
JP2012076751A
Biaxial stretch blow-molded container
JP2014046966A
Blow-molded multiple bottle made of polyester resin, release agent used for the same, and coating method and coating equipment thereof
JP2017186059A