Cured film and laminate, and methods for producing the same
A cured film with a wrinkle-like uneven structure, formed by irradiating an active energy ray-curable composition, addresses the limitations of existing methods by providing durable matte and antistatic properties for architectural materials and display members.
Patent Information
- Application Number
- JP2020128536
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing methods for imparting matte properties to architectural materials and display members fail to achieve sufficient matting effects and often result in surface irregularities that compromise scratch resistance and antistatic properties, with inorganic particles tending to fall off and affect visibility.
A cured film with a wrinkle-like uneven structure is formed by irradiating an active energy ray-curable composition containing a polymer with active groups that generate radicals, using excimer light to create a durable and matte surface with enhanced scratch resistance and antistatic properties.
The cured film and laminate exhibit excellent matte properties, improved scratch resistance, and maintain antistatic properties without particle fallout, ensuring enhanced visibility and durability.
Smart Images

Figure 0007563023000001 
Figure 0007563023000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cured film and a laminate, and to a method for producing the same. [Background technology]
[0002] In order to impart a matte finish to building materials such as wallpaper, display members, decorative films, and other members, fine irregularities are sometimes imparted to the surface of a substrate. In addition, these members are sometimes required to have antistatic properties. Patent Document 1 discloses a method for forming fine projections and recesses by irradiating the surface of a biaxially oriented thermoplastic resin film used in a magnetic recording medium with excimer laser light. Patent Document 2 discloses a method for forming irregularities on the surface of a film having a hard coat layer used in an antireflection film, in which a film having a hard coat layer containing a hard coat resin and inorganic fine particles is irradiated with excimer light to decompose the hard coat resin portion of the surface layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 4-305430 [Patent Document 2] JP 2014-224920 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the method described in Patent Document 1 can only obtain a specific uneven structure that does not provide a sufficient matte effect. In addition, since the unevenness is formed directly on the biaxially oriented thermoplastic resin film, it is difficult to apply the film to display applications that require various surface properties such as scratch resistance and antistatic properties. In the method described in Patent Document 2, only the hard coat resin of the hard coat layer is decomposed to expose inorganic fine particles on the surface, so the particles tend to fall off, which may impair visibility when used in displays, etc. In addition, there is a problem that the surface uneven structure is limited by the shape and distribution of the particles. An object of the present invention is to provide a cured film and a laminate having excellent matte properties, and a method for producing such a cured film and a laminate. [Means for solving the problem]
[0005] The present invention has the following aspects. [1] A cured film obtained by irradiating an active energy ray-curable composition with active energy rays, the cured film having a wrinkled uneven surface structure, and the curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays. [2] The cured film according to [1] above, wherein the active group is at least one group selected from the group consisting of a benzophenone group, an acetophenone group, a benzoin group, an α-hydroxyketone group, an α-aminoketone group, an α-diketone group, an α-diketone dialkyl acetal group, an anthraquinone group, a thioxanthone group, and a phosphine oxide group. [3] The cured film according to [1] or [2] above, wherein the curable composition contains a (meth)acrylate. [4] The cured film according to any one of [1] to [3] above, wherein the uneven structure has a mean length of roughness curve elements (RSm) according to JIS B0601:2013 of 1 μm or more. [5] The cured film according to any one of the above [1] to [4], wherein the uneven structure has an arithmetic mean height (Sa) defined by ISO 25178 of 0.1 μm or more. [6] The cured film according to any one of the above [1] to [5], wherein the average value (θa) of the local tilt angle of the uneven structure is 2° or more. [7] The cured film according to any one of the above [1] to [6], wherein the 60° gloss of the surface is 50 or less. [8] The method for producing a cured film according to any one of the above [1] to [7], wherein an active energy ray-curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays is cured by irradiating it with excimer light. [9] A laminate comprising the cured film according to any one of the above [1] to [7] laminated on a substrate.
[10] The laminate according to [9] above, wherein the substrate is a film.
[11] A method for producing a laminate according to [9] or
[10] above, comprising laminating an active energy ray-curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays on a substrate, and curing the composition by irradiating with excimer light. Effect of the Invention
[0006] The cured film and laminate of the present invention have excellent matt properties. According to the method for producing the cured film and laminate of the present invention, a cured film and laminate having excellent matt properties can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment of the present invention will be described in detail. In the present invention, "(meth)acrylate" is a general term for acrylate or methacrylate. "(meth)acrylic" is a general term for acrylic and methacrylic. "~" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit.
[0008] [Cured film] The cured film of the present invention (hereinafter simply referred to as "cured film") is obtained by irradiating an active energy ray-curable composition with active energy rays, and has a wrinkled uneven structure (non-smooth structure) on the surface. The curable composition contains a polymer having an active group that generates radicals upon irradiation with active energy rays. The cured film of the present invention is suitable as an anti-glare film because of its excellent matte properties.
[0009] (average length of roughness curve element) The average length of the roughness curve element in the uneven structure of the cured film is the average length of the roughness curve element (RSm, hereinafter also simply referred to as "RSm") according to JIS B0601:2013. The evaluation length when calculating RSm is 236.87 μm. The preferred range of RSm is 1 μm or more, more preferably 5 to 120 μm, even more preferably 7 to 80 μm, particularly preferably 10 to 60 μm, and most preferably 15 to 40 μm. When within the above range, excellent matte properties are achieved, and excellent visibility when used in displays, etc.
[0010] (arithmetic mean height) The arithmetic mean height of the uneven structure of the cured film is the arithmetic mean height (Sa, hereinafter simply referred to as "Sa") defined by ISO25178. The evaluation length for calculating Sa is 236.87 μm. Sa is preferably 0.1 μm or more, more preferably 0.15 to 20 μm, even more preferably 0.2 to 10 μm, particularly preferably 0.3 to 5 μm, and most preferably in the range of 0.4 to 3 μm. When within the above range, excellent matte properties are achieved, and excellent visibility is achieved when used in displays, etc.
[0011] (Average value of the inclination angle of the uneven structure) The average value of the local inclination angle (θa, hereinafter also simply referred to as "θa") in the concave-convex structure of the cured film can be measured by the method described in the Examples described later. The evaluation length for calculating θa was 236.87 μm. θa is preferably 2° or more, more preferably 2.5° or more, even more preferably 3° or more, particularly preferably 3.5° or more, and most preferably 4° or more, and the upper limit may be 90°. When it is in this range, it has good matte properties.
[0012] (Thickness) From the viewpoint of improving the matte property, the thickness of the cured film (concave-convex layer) is preferably in the range of 0.1 to 100 μm, more preferably 0.2 to 20 μm, further preferably 0.3 to 10 μm, and particularly preferably 0.3 to 7 μm. The thickness of the cured film indicates the maximum thickness of the concave-convex layer, and is determined by cross-sectional observation using an electron microscope.
[0013] (Hayes) The haze of the cured film measured by the method described in the Examples below is preferably 1% or more, more preferably 3% or more, even more preferably 5% or more, particularly preferably 10% or more, and most preferably 20% or more, with the upper limit being, for example, 99%. The higher the haze, the better the matte properties tend to be. In particular, when used for anti-glare applications in various displays, the range is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more, with the upper limit being, for example, 99%. Depending on the application, the higher the range, the more preferable it is.
[0014] (Gross) The 60° gloss (60° specular gloss) of the surface of the cured film measured by the method described in the Examples below is preferably 50 or less, more preferably 40 or less, even more preferably 30 or less, particularly preferably 25 or less, and most preferably 20 or less, with the lower the better. The smaller the 60° gloss value, the better the matte property. Similarly, the 20° gloss is preferably 30 or less, more preferably 20 or less, even more preferably 15 or less, particularly preferably 10 or less, and most preferably 8 or less, with the lower the better. The smaller the 20° gloss value, the better the matte property.
[0015] (Pencil hardness) The pencil hardness of the cured film measured by the method described in the Examples below is preferably F or more, more preferably H or more, and further preferably 2H or more. When the hardness is in the above range, the film has excellent scratch resistance and is suitable for applications where visibility is important, such as displays. The present inventors have found that by using an active energy ray-curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays, not only the matte properties of the cured film are improved, but also the pencil hardness is improved. This is presumably because, compared to a typical monomolecular activator, the incorporation of an active group in the polymer improves compatibility with other components in the curable composition, accelerating the curing of the cured film.
[0016] [Method for producing cured film and laminate] The cured film of the present invention and the laminate of the present invention having the same (hereinafter simply referred to as "laminate") can be produced, for example, by a method of laminating a coating film of a curable composition on a substrate, and irradiating the surface side of the coating film (the side opposite to the substrate) with active energy rays to form a cured film on the surface of the substrate. By irradiating the surface side of the coating film of the curable composition with active energy rays, the surface side of the coating film is cured first to form a cured coating. When the inside of the coating film subsequently cures, the cured coating on the surface side that has cured first buckles, forming a cured film having a wrinkled uneven structure on the surface.
[0017] (Curable composition) The curable composition used for forming the cured film contains a polymer having an active group that generates radicals upon irradiation with active energy rays. The curable composition may further contain an active energy ray-curable compound other than the polymer having an active group that generates radicals upon irradiation with active energy rays, an organic solvent, and other components, as necessary.
[0018] The present inventors have found that by including a polymer having an active group that generates radicals by irradiation with active energy rays in a curable composition, it is possible to easily impart an uneven structure to a cured film. That is, by including a polymer having an active group that generates radicals by irradiation with active energy rays in a curable composition, it is possible to easily form an uneven structure and to widen the composition range of the curable composition that can form an uneven structure. In addition, it has also been found that the cured film can be made harder.
[0019] (Polymers having active groups that generate radicals upon irradiation with active energy rays) The polymer having an active group that generates radicals upon irradiation with active energy rays (hereinafter also referred to as "polymer (X)") may be any polymer having a structure that generates radicals upon irradiation with active energy rays (hereinafter also referred to as "structure having photopolymerization initiation ability"). As the structure having photopolymerization initiation ability, various known structures can be used, for example, hydrogen abstraction type, electron transfer type, and intramolecular cleavage type. Examples of the active group include benzophenone group, acetophenone group, benzoin group, α-hydroxyketone group, α-aminoketone group, α-diketone group, α-diketone dialkylacetal group, anthraquinone group, thioxanthone group, and phosphine oxide group. Examples of the α-hydroxyketone group include a group in which one hydrogen atom is removed from the "hydroxyl group in 2-hydroxyethoxy" of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone. As the active group, a benzophenone group, an acetophenone group, and an α-hydroxyketone group are preferred in that they are less susceptible to oxygen inhibition during curing and have good surface curing properties when forming a concave-convex layer. The active group may be present at the terminal of the main chain of the polymer (X), or may be present in a unit based on a monomer constituting the polymer (X). The polymer (X) preferably has a plurality of active groups in the molecule, which can increase the concentration of active groups near the coating surface, making the coating less susceptible to oxygen inhibition, improving curability, and facilitating the development of unevenness such as wrinkled structures on the cured surface.
[0020] As the polymer (X), from the viewpoint of introducing a plurality of active groups into the molecule, a polymer having a unit based on a monomer having an active group is preferred. The monomer having an active group may be a compound having an active group and a radically polymerizable group. The radically polymerizable group may be the same as those mentioned above. As the monomer having an active group, from the viewpoint of ease of synthesis of the polymer (X) and ease of adjustment of the amount of the active group to be introduced, a (meth)acrylic acid ester having an active group is preferable. Examples of the monomer having an active group include 4-methacryloyloxybenzophenone and 2-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenoxy]ethyl methacrylate.
[0021] The polymer (X) preferably has a unit based on a monomer having an alkyl group having 4 or more carbon atoms in addition to a unit based on a monomer having an active group. If the polymer (X) has this unit, when a coating film of the curable polymer composition is formed, the polymer (X) is likely to segregate to the surface side of the coating film. If the polymer (X) segregates to the surface side of the coating film, the curing reaction inside the coating film (substrate layer side) is less susceptible to oxygen inhibition, and the curability is improved. For example, it can be cured with a low exposure dose, and even a thin film that tends to be easily inhibited by oxygen can be cured well. The alkyl group having 4 or more carbon atoms may be linear, branched, or cyclic. The cyclic alkyl group may be monocyclic or polycyclic. From the viewpoint of more effectively segregating the polymer (X) on the surface of the coating film, the alkyl group is preferably linear. The carbon number of the alkyl group having 4 or more carbon atoms is preferably in the range of 4 to 30, more preferably in the range of 6 to 20, and even more preferably in the range of 12 to 18, from the viewpoint of more effectively segregating the polymer (X) on the surface of the coating film.
[0022] Examples of monomers having an alkyl group having 4 or more carbon atoms include compounds having an alkyl group having 4 or more carbon atoms and a radical polymerizable group. From the viewpoints of ease of synthesis of the compound and ease of adjusting the amount of the alkyl group having 4 or more carbon atoms introduced, (meth)acrylic acid esters having an alkyl group having 4 or more carbon atoms are preferred. Examples of monomers having an alkyl group having 4 or more carbon atoms include butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, and isodecyl (meth). ) acrylate, dodecyl (meth)acrylate, myristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, tridecyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, tricyclodecane (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, and the like. Among these, it is preferable to include a (meth)acrylic acid ester having a linear alkyl group having 4 or more carbon atoms. As the (meth)acrylic acid ester having a linear alkyl group having 4 or more carbon atoms, it is preferable that the number of carbon atoms in the alkyl group is within the above-mentioned preferred range, and taking into consideration ease of production, etc., 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate are more preferable, and stearyl (meth)acrylate is particularly preferable. These (meth)acrylic acid esters may be used alone or in combination of two or more kinds.
[0023] From the viewpoint of more effectively segregating the polymer (X) on the surface of the coating film, the polymer (X) may have units based on a monomer containing a fluorine atom or a silicon atom in addition to or instead of units based on a monomer having an alkyl group having 4 or more carbon atoms. The fluorine atom-containing monomer is preferably a (meth)acrylic acid ester containing a fluorine atom, more preferably a (meth)acrylic acid ester having a perfluoroalkyl group, the number of carbon atoms of which is preferably 4 or more. The silicon atom-containing monomer is preferably a (meth)acrylic acid ester having a polydimethylsiloxane chain.
[0024] The polymer (X) may further have a unit based on a monomer having a hydrogen donor functional group, if necessary. In particular, when the active group contains a hydrogen abstraction type, it is preferable to have a unit based on a monomer having a hydrogen donor functional group. If the polymer (X) has this unit, the curing of the coating film of the curable polymer composition can be effectively performed from the surface, and the curability can be improved and unevenness can be easily formed. Examples of the hydrogen donating functional group include a hydroxyl group, an amino group, a mercapto group, an amide group, etc. Among these, a hydroxyl group, an amino group, or an amide group is preferred from the viewpoint of efficiently proceeding with the curing reaction, improving the curability, or facilitating the formation of unevenness. Examples of the monomer having a hydrogen donor functional group include a compound having a hydrogen donor functional group and a radical polymerizable group. From the viewpoints of ease of synthesis of the compound and ease of adjustment of the amount of hydrogen donor functional group to be introduced, a (meth)acrylic acid ester having a hydrogen donor functional group is preferred. Examples of monomers having a hydrogen donating functional group include hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, monobutyl hydroxyl fumarate, and monobutyl hydroxy itaconate; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-vinyl caprolactam, N-vinyl pyrrolidone, and N-isopropyl (meth)acrylamide. Examples of the monomers include amino group- or amide group-containing monomers such as N,N-dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, 2-[(butylamino)carbonyl]oxy]ethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, N,N-diethylaminopropyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, N,N-diethylaminopropyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylamide, (meth)acryloylmorpholine, and vinylacetamide. Among these, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, (N,N-dimethylacrylamide, N,N-dimethylaminoethyl (meth)acrylate, and N,N-diethylaminoethyl (meth)acrylate are preferred because they have an excellent curing acceleration effect when used in combination with an active group, and N,N-diethylaminoethyl (meth)acrylate is more preferred because it is easy to increase the unevenness. These compounds may be used alone or in combination of two or more.
[0025] The polymer (X) may further contain units based on other monomers other than those mentioned above, if necessary. Examples of the other monomers include compounds having a radical polymerizable group but not having an active group, an alkyl group having 4 or more carbon atoms, a fluorine atom, or a hydrogen donor functional group. Examples of other monomers include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, citraconic acid, and salts thereof; (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and propyl (meth)acrylate; nitrogen-containing monomers such as (meth)acrylonitrile; styrene-based compounds such as styrene, α-methylstyrene, divinylbenzene, and vinyl toluene, and vinyl esters such as vinyl propionate and vinyl acetate; silicon-containing monomers such as γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane; phosphorus-containing vinyl monomers; vinyl halides such as vinyl chloride and vinylidene chloride; and conjugated dienes such as butadiene.
[0026] The content of active groups per gram of polymer (X) is preferably in the range of 0.1 to 3.5 mmol / g, more preferably 0.3 to 3.0 mmol / g, further preferably 0.5 to 2.7 mmol / g, and particularly preferably 1.0 to 2.5 mmol / g. When the content of active groups is within the above range, curability is excellent and unevenness can be formed more effectively. The ratio of units based on monomers having active groups to the total mass of all units constituting the polymer (X) is preferably in the range of 1 to 90 mass%, more preferably 10 to 80 mass%, further preferably 20 to 70 mass%, and particularly preferably 30 to 60 mass%. If the ratio of units based on monomers having active groups is within the above range, curability can be improved and unevenness can be formed more effectively.
[0027] The ratio of units based on monomers having an alkyl group with 4 or more carbon atoms to the total mass of all units constituting the polymer (X) is preferably 80 mass% or less, more preferably 1 to 70 mass%, further preferably 5 to 60 mass%, and particularly preferably 8 to 50 mass%. If the ratio of units based on monomers having an alkyl group with 4 or more carbon atoms is within the above range, curability can be improved and unevenness can be formed more effectively.
[0028] The ratio of units based on a monomer having a hydrogen donor functional group to the total mass of all units constituting the polymer (X) is preferably 80 mass% or less, more preferably 1 to 60 mass%, further preferably 3 to 50 mass%, and particularly preferably 5 to 40 mass%. If the ratio of units based on a monomer having a hydrogen donor functional group is within the above range, curability can be improved and unevenness can be formed more effectively.
[0029] The weight average molecular weight (Mw) of the polymer (X) is preferably in the range of 1000 to 100000, more preferably 3000 to 50000, and further preferably 5000 to 30000. When Mw is within the above range, the coatability and curability of the curable polymer composition are improved, and the ease of forming unevenness is improved. The Mw of the polymer (X) is a value calculated in terms of standard polystyrene as measured by gel permeation chromatography (GPC). The detailed measurement conditions are as described in the Examples below.
[0030] The glass transition temperature (Tg) of the polymer (X) is preferably in the range of −30 to 150° C., more preferably 0 to 120° C., and further preferably 25 to 100° C. If Tg is within the above range, the curability can be improved, and the ease of forming unevenness can also be improved. The polymer (X) can be obtained, for example, by polymerizing a monomer component containing a monomer having an active group. The monomer component may further contain, as necessary, one or more of a monomer having an alkyl group having 4 or more carbon atoms, a monomer containing a fluorine atom, a monomer having a hydrogen donor functional group, and other monomers.
[0031] The polymerization is typically carried out in the presence of a polymerization initiator. If necessary, a chain transfer agent may be used in combination during the polymerization. The polymerization method includes known methods such as solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization, and among them, solution polymerization is preferred because of its simple operation and high productivity.
[0032] The content of the polymer (X) in the curable composition is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 1.0% by mass or more, particularly preferably 2.0% by mass or more, and most preferably 3.0% by mass or more, based on the non-volatile content (all components excluding the solvent). There is no particular upper limit and it may be 100% by mass, but in consideration of the hardness of the cured film, it is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, particularly preferably 15% by mass or less, and most preferably 10% by mass or less. The higher this content, the better the surface unevenness of the cured film is formed. The non-volatile content of the curable composition is the total mass of components other than the solvent such as the organic solvent. The non-volatile content of the curable composition can be measured by a conventionally known method, for example, by measuring the change in weight when 1 g of the composition is spread and heated at 100° C. for 1 hour to volatilize the organic solvent.
[0033] (Active energy ray-curable compound other than polymer (X)) In order to facilitate the formation of an uneven structure in the cured film, improve scratch resistance, and improve hardness, the active energy ray curable composition is also preferably blended with an active energy ray curable compound (hereinafter also referred to as "compound (Y)") other than the polymer (X). Examples of the compound (Y) include (meth)acrylate. There is no particular limitation on the (meth)acrylate, and it is possible to use monofunctional (meth)acrylate, bifunctional (meth)acrylate, trifunctional or higher polyfunctional (meth)acrylate, or a commercially available active energy ray curable resin material, or a material further containing other components within a range that does not impair the purpose of this embodiment. As the (meth)acrylate, a monofunctional or bifunctional (meth)acrylate is preferred from the viewpoint of easily forming a wrinkled uneven structure. In order to increase the hardness and scratch resistance of the cured film, a trifunctional or higher polyfunctional (meth)acrylate is generally preferred. However, according to the study by the present inventor, it was found that depending on the type of trifunctional or higher polyfunctional (meth)acrylate, it may be difficult to form a wrinkled uneven structure. However, it was found that when used in combination with the polymer (X), an uneven structure can be easily formed even when a trifunctional or higher polyfunctional (meth)acrylate is used. Therefore, according to the present invention, by using a trifunctional or higher polyfunctional (meth)acrylate, it is easy to achieve both the formation of an uneven structure and the hardness of the cured film.
[0034] Examples of the trifunctional or higher polyfunctional (meth)acrylate include ethylene oxide-modified (meth)acrylates such as dipentaerythritol hexa(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and ethylene oxide-modified pentaerythritol tetra(meth)acrylate. Examples of suitable urethane acrylates include isocyanuric acid modified tri(meth)acrylates such as ethylene oxide-modified isocyanuric acid tri(meth)acrylate, ε-caprolactone-modified tris(acryloxyethyl)isocyanurate, and urethane acrylates such as pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer. Among these, ethylene oxide-modified types and trifunctional (meth)acrylates are preferred in consideration of the ease of forming a wrinkled uneven structure. In addition, in consideration of the hardness and scratch resistance of the cured film, it is preferable to contain a (meth)acrylate having 6 or more functionalities, such as dipentaerythritol hexa(meth)acrylate and ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and modified dipentaerythritol hexa(meth)acrylate such as ethylene oxide-modified is even more preferable because it is easier to form unevenness.
[0035] Examples of the bifunctional polyfunctional (meth)acrylate include alkanediol di(meth)acrylates such as 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, tricyclodecanedimethylol di(meth)acrylate, bisphenol-modified di(meth)acrylates such as bisphenol A ethylene oxide-modified di(meth)acrylate and bisphenol F ethylene oxide-modified di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, urethane di(meth)acrylate, and epoxy di(meth)acrylate. Among these, in consideration of the ease of forming a wrinkled uneven structure, a structure without a branch is preferable, and alkyl diol di(meth)acrylate is more preferable, and alkyl diol di(meth)acrylate having 4 to 18 carbon atoms is even more preferable.
[0036] Examples of the active energy ray-curable monofunctional (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and methoxypropyl (meth)acrylate. alkoxyalkyl (meth)acrylates such as ethoxypropyl (meth)acrylate, aromatic (meth)acrylates such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate, amino group-containing (meth)acrylates such as diaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate, ethylene oxide-modified (meth)acrylates such as methoxyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and phenylphenol ethylene oxide-modified (meth)acrylate, glycidyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.
[0037] The curable composition may contain an active energy ray-curable compound other than (meth)acrylate. Examples of such compounds include vinyl compounds such as (meth)acrylic acid, styrene, vinyl halides, and vinyl acetate, and diene compounds such as vinylidene halides, 1,3-butadiene, isoprene, and chloroprene.
[0038] When compound (Y) is blended in the curable composition, the content thereof is preferably 5 to 99.99 mass%, more preferably 30 to 99.9 mass%, further preferably 40 to 99 mass%, particularly preferably 50 to 98 mass%, and most preferably 60 to 97 mass%, based on the non-volatile content. When in the above range, a wrinkled uneven structure is easily formed, and a cured film having excellent hardness can be formed. In particular, in applications requiring improved hardness and scratch resistance of the cured film, it is preferable that the content of tri- or higher functional polyfunctional (meth)acrylate is high, and the content of tri- or higher functional polyfunctional (meth)acrylate is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 60% by mass or more, and particularly preferably 80% by mass or more, with the upper limit being in the range of 99.99% by mass, based on the non-volatile content. In applications where hardness is more important, it is preferable to incorporate a 6- or higher functional (meth)acrylate, and in that case, the content of this compound relative to the non-volatile content is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, with the upper limit being in the range of 99.99% by mass.
[0039] (resin) In order to improve adhesion to a substrate, the curable composition may further contain various resins other than the polymer (X), such as conventionally known resins such as acrylic resins, polyester resins, polyurethane resins, polyvinyl resins, etc. Among these, acrylic resins are preferred in terms of their excellent transparency and affinity with the polymer (X) and the compound (Y). When the curable composition contains a resin, the content of the resin is preferably 50% by mass or less, more preferably 30% by mass or less, further preferably 20% by mass or less, and particularly preferably 10% by mass or less, based on the non-volatile content. The lower the content, the higher the hardness of the cured film tends to be.
[0040] (particle) In order to further improve the matte property due to the wrinkled uneven structure of the cured film, it is also possible to blend particles into the curable composition. The particles are not particularly limited, and examples thereof include inorganic particles such as silica, hollow silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, zirconium oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin. The inorganic particles may be particles surface-modified with a silane coupling agent having a reactive group such as a (meth)acryloyl group. The organic particles are preferably of a crosslinked type in order to maintain their shape, and crosslinked acrylic resin particles and crosslinked styrene resin particles are more preferable. Two or more of these particles may be used in combination. The average primary particle size of the particles is preferably in the range of 0.01 to 30 μm, more preferably 0.05 to 10 μm, further preferably 0.1 to 5 μm, and particularly preferably 0.5 to 3 μm. When within this range, the matte properties are excellently improved. When particles are blended, the content thereof is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less, based on the non-volatile content in the curable composition, from the viewpoint of improving matte properties.
[0041] (Photopolymerization initiator) A photopolymerization initiator may be added to promote the curing of the curable composition. The molecular weight of the photopolymerization initiator is preferably 1000 or less. Specific examples include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin phenyl ether, benzyl diphenyl disulfide, dibenzyl, diacetyl, anthraquinone, naphthoquinone, 3,3'-dimethyl-4-methoxybenzophenone, benzophenone, p,p'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, pivaloin ethyl ether, benzyl dimethyl ketal, 1,1-dichloroacetophenone, pt-butyl dichloroacetophenone, etc. phenone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-diethylthioxanthone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-dichloro-4-phenoxyacetophenone, phenyl glyoxylate, α-hydroxyisobutylphenone, dibenzosparone, 1-(4-isopropylphenyl)-2-hydroxy-2-methyl-1-propanone, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, tribromophenylsulfone, and tribromomethylphenylsulfone. These photopolymerization initiators may be used alone or in combination of two or more. When a photopolymerization initiator is added, the content thereof is preferably 20% by mass or less, more preferably 10% by mass or less, further preferably 8% by mass or less, and particularly preferably 5% by mass or less, based on the non-volatile content, from the viewpoints of promoting curing and hardness of the cured film.
[0042] (Leveling agent) In order to improve the appearance of the cured film, a leveling agent can be added to the curable composition. Examples of the leveling agent include acrylic leveling agents, silicone leveling agents, and fluorine leveling agents. These leveling agents may be used alone or in combination of two or more. When a leveling agent is added, the content thereof is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the nonvolatile content, from the viewpoint of improving the appearance of the cured film.
[0043] (Various additives) The curable composition may contain various additives, such as a polymerization accelerator such as a compound containing a thiol group, an antifouling agent, a plasticizer, a surfactant, an antioxidant, and an ultraviolet absorber, as long as the effects of the present invention are not impaired.
[0044] (Organic solvent) For the purpose of improving the workability when applying the curable composition to a substrate, an organic solvent may be added to the curable composition as necessary. Examples of organic solvents include aromatic solvents such as toluene and xylene; ketone-based solvents such as methyl ethyl ketone, acetone, methyl isobutyl ketone, and cyclohexanone; ether-based solvents such as diethyl ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, anisole, and phenetole; ester-based solvents such as ethyl acetate, butyl acetate, isopropyl acetate, and ethylene glycol diacetate; amide-based solvents such as dimethylformamide, diethylformamide, and N-methylpyrrolidone; cellosolve-based solvents such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; alcohol-based solvents such as methanol, ethanol, propanol, isopropanol, and butanol; and halogen-based solvents such as dichloromethane and chloroform. These organic solvents may be used alone or in combination of two or more. Among these organic solvents, ester-based solvents, ether-based solvents, alcohol-based solvents and ketone-based solvents are preferred in that they can easily improve workability during coating. When an organic solvent is blended in the curable composition, the content thereof is preferably from 10 parts by mass to 1,900 parts by mass, and more preferably from 40 parts by mass to 400 parts by mass, per 100 parts by mass of nonvolatile matter, from the viewpoint of improving operability in a coating operation.
[0045] (Formation of coating film) Examples of the method for forming a coating film of the curable composition include a method in which the curable composition is applied onto a surface of a substrate or an article to form a coating film, and then dried as necessary. The coating method is not particularly limited, and examples thereof include known methods such as dip coating, air knife coating, curtain coating, spin coating, roller coating, bar coating, wire bar coating, gravure coating, and spray coating. When the curable composition contains an organic solvent, it is preferable to heat-dry the composition before irradiating it with active energy rays. By heating and drying the composition beforehand, the solvent in the coating film can be effectively removed. The drying temperature for the heat-drying is preferably 30°C or higher and 200°C or lower, more preferably 40°C or higher and 150°C or lower. The drying time is preferably 0.01 minutes or higher and 30 minutes or lower, more preferably 0.1 minutes or higher and 10 minutes or lower.
[0046] (Irradiation with active energy rays) The coating film of the curable composition formed on the surface of the substrate or article is irradiated with active energy rays to form a cured film, and a laminate is formed in which the cured film is laminated on the substrate or article. As the active energy rays, those with high energy (short wavelength) capable of effectively curing the surface of the coating film are preferable, and vacuum ultraviolet rays (ultraviolet rays with a wavelength of 200 nm or less) are more preferable. Among the vacuum ultraviolet rays, excimer light with a half-width of 50 nm or less is optimal. Examples of excimer light include argon excimer light (126 nm), krypton excimer light (146 nm), xenon excimer light (172 nm), and argon-fluorine excimer light (193 nm). Among these, xenon excimer light is preferable in consideration of ease of use, the ability to form an effective uneven structure in the cured film, and the curability of the curable composition.
[0047] When using vacuum ultraviolet light, the cumulative amount of light to be irradiated is preferably 1 to 3000 mJ / cm. 2 , more preferably 3 to 1000 mJ / cm 2 , and more preferably 5 to 500 mJ / cm 2 , particularly preferably 10 to 100 mJ / cm 2 The illuminance is preferably in the range of 1 to 500 mW / cm 2 , more preferably 2 to 300 mW / cm 2 , and more preferably 3 to 100 mW / cm 2 The range is. In addition, the vacuum ultraviolet irradiation is preferably performed in an environment with a low oxygen content, such as a nitrogen atmosphere. The oxygen concentration in the atmosphere is preferably 10% or less, more preferably 5% or less, further preferably 3% or less, and particularly preferably 1% or less.
[0048] After the vacuum ultraviolet irradiation, it is preferable to irradiate the cured film with active energy rays other than vacuum ultraviolet rays in order to cure the film to a deep portion. Examples of active energy rays include ultraviolet rays and electron beams. Examples of ultraviolet rays include ultraviolet rays with a wavelength of 200 nm or more irradiated from high pressure mercury lamps, low pressure mercury lamps, metal halide lamps, UV-LED lamps, etc. Examples of electron beams include electron beams irradiated from EB irradiators, etc. As active energy rays other than vacuum ultraviolet rays, ultraviolet rays are more preferable in consideration of the curability of the curable composition.
[0049] The cumulative amount of ultraviolet light to be irradiated is preferably 1 to 5000 mJ / cm 2 , more preferably 50 to 3000 mJ / cm 2 , and more preferably 100 to 1000 mJ / cm 2 , particularly preferably 200 to 700 mJ / cm 2 The illuminance is preferably in the range of 1 to 1000 mW / cm 2 , more preferably 50 to 500 mW / cm 2 , and more preferably 80 to 300 mW / cm 2 The range is.
[0050] [Laminate] The laminate of the present invention has a layer made of a substrate and a layer (uneven layer) made of a cured film of a curable composition. The laminate may further have a primer layer between the substrate and the cured film. In addition, the laminate may have a back functional layer on the surface of the substrate opposite to the cured film side. As long as it does not impair the effects of the present invention, the cured film may have a surface functional layer on the surface opposite to the substrate.
[0051] (base material) The substrate may be a known one, for example, a resin substrate, a metal substrate, or a paper substrate. Among these, a resin substrate is preferred from the viewpoint of processability. The resin substrate may be a single-layer structure or a multi-layer structure of two or more layers, and is not particularly limited. It is preferred that the resin substrate be a multi-layer structure of two or more layers, each layer having its own characteristics, and multi-functional. As the resin substrate, various resin films (sheets) can be used, for example, polyester film, poly(meth)acrylate film, polyolefin film, polycarbonate film, polyimide film, triacetyl cellulose film, polystyrene film, polyvinyl chloride film, polyvinyl alcohol film, and nylon film. When the laminate is used for a display, polyester film, poly(meth)acrylate film, polyolefin film, polycarbonate film, polyimide film, and triacetyl cellulose film are preferred. Among these, polyester film, poly(meth)acrylate film, and polyolefin film are preferred for anti-glare applications, and polyester film is more preferred in terms of transparency, moldability, and versatility.
[0052] The polyester film may be a non-stretched film or a stretched film, and a stretched film is preferable. Among them, a uniaxially stretched film stretched in one direction or a biaxially stretched film stretched in two directions is preferable, and a biaxially stretched film is more preferable from the viewpoint of excellent balance of mechanical properties and flatness. The polyester constituting the polyester film that can be used as the substrate may be either a homopolyester or a copolymer polyester. The homopolyester is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid. Examples of the aliphatic glycol include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol. The aromatic dicarboxylic acid and the aliphatic glycol may each be used alone or in combination of two or more. Examples of the dicarboxylic acid component of the copolymer polyester include isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, and oxycarboxylic acid. Examples of the glycol component include ethylene glycol, diethylene glycol, propylene glycol, butanediol, 4-cyclohexanedimethanol, and neopentyl glycol. The dicarboxylic acid component and the glycol component may each be used alone or in combination of two or more. Representative examples of polyester include polyethylene terephthalate and polyethylene naphthalate. As the polyester film, from among the above, films formed from polyethylene terephthalate and polyethylene naphthalate are more preferable in consideration of mechanical strength and heat resistance, and from the viewpoint of ease of production and handleability for applications such as surface protection films, films formed from polyethylene terephthalate are particularly preferable.
[0053] The poly(meth)acrylate constituting the poly(meth)acrylate film that can be used as the substrate may be any one having a unit based on (meth)acrylate, and various acrylic resins can be used. Examples of the (meth)acrylate include alkyl (meth)acrylates having an alkyl group with 1 to 4 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, and alkyl (meth)acrylates having an alkyl group with a larger number of carbon atoms. In consideration of transparency, processability, and chemical resistance, the poly(meth)acrylate preferably contains as a main component a unit based on an alkyl(meth)acrylate having 1 to 4 carbon atoms, more preferably contains as a main component at least one selected from the group consisting of units based on methyl(meth)acrylate and units based on ethyl(meth)acrylate, and particularly preferably contains as a main component a unit based on methyl(meth)acrylate. It is also possible to impart properties such as flexibility to the poly(meth)acrylate by incorporating units based on (meth)acrylates other than alkyl (meth)acrylates or units based on other monomers. The proportion of units based on alkyl (meth)acrylate having 1 to 4 carbon atoms relative to the total mass of the poly(meth)acrylate is preferably 50% by mass or more, and more preferably 80% by mass or more.
[0054] The substrate may contain particles for the purposes of imparting slipperiness, preventing scratches during each process, and improving blocking resistance. The type of particles can be appropriately selected according to the purpose, and is not particularly limited. Specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, zirconium oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin. Furthermore, when the base layer includes a polyester film, precipitated particles obtained by precipitating a part of a metal compound such as a catalyst during the polyester manufacturing process can also be used. Among these, silica particles and calcium carbonate particles are preferred because they are particularly effective in small amounts. The shape of the particles is not particularly limited, and any of spherical, block, rod-like, flat, etc. is acceptable. In addition, there is no particular limit to the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination, if necessary. The average primary particle size of the particles is preferably 10 μm or less, more preferably 0.01 to 5 μm, and further preferably in the range of 0.01 to 3 μm. If the average primary particle size is 10 μm or less, problems due to a decrease in the transparency of the substrate are unlikely to occur. The average primary particle size of the particles is the cumulative 50% (mass basis) value in the equivalent sphericity distribution measured by a centrifugal sedimentation type particle size distribution measuring device. When the substrate contains particles, the content of the particles is not necessarily limited since it depends on the average primary particle diameter of the particles, but is preferably 5% by mass or less, more preferably in the range of 0.0003 to 3% by mass, and even more preferably in the range of 0.0005 to 1% by mass, based on the total mass of the substrate (total mass of the layers containing the particles when the substrate is composed of multiple layers). If the particle content is 5% by mass or less, defects such as particle dropout and reduced transparency of the substrate are unlikely to occur.
[0055] The substrate may contain additives other than the above-mentioned particles as necessary. Examples of the additives that can be used include known additives such as ultraviolet absorbers, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, and pigments. When the substrate is a film, the thickness is not particularly limited as long as it is within a range that allows film formation, but is preferably in the range of 2 to 350 μm, more preferably 5 to 250 μm, and even more preferably 10 to 100 μm.
[0056] (Primer layer) The primer layer is appropriately provided between the substrate and the cured film (concave-convex layer) in order to impart various functions. The primer layer may be a single layer having a single or multiple functions, or may be composed of multiple layers. In a preferred embodiment, the primer layer is an adhesion improving layer. If the adhesion between the substrate and the uneven layer is insufficient, the laminate may not be usable depending on the application. By having the adhesion improving layer, the adhesion between the substrate and the uneven layer is improved, and the laminate can be used for various applications. From the viewpoint of improving adhesion, it is preferable that the adhesion improving layer contains either one or both of a resin and a compound derived from a crosslinking agent. In another preferred embodiment, the primer layer is an antistatic layer. When the primer layer is an antistatic layer, adhesion of dust and the like due to peeling electrification or frictional electrification can be reduced to the outermost surface of the laminate, particularly to the outermost surface on the side where the uneven layer is present relative to the substrate. In order to make the primer layer an antistatic layer, for example, an antistatic agent may be contained in the primer layer.
[0057] The resin contained in the primer layer may be a conventionally known resin. Specific examples of the resin include polyester resin, acrylic resin, urethane resin, polyvinyl resin (polyvinyl alcohol, vinyl chloride-vinyl acetate copolymer, etc.), etc. Among them, polyester resin, acrylic resin, and urethane resin are preferred in terms of adhesion performance and coating properties. When the substrate is a resin film, the resin contained in the primer layer is preferably the same type of resin as that of the resin film from the viewpoint of affinity with the substrate. For example, when the substrate is a polyester film, the primer layer preferably contains a polyester resin. When the substrate is a poly(meth)acrylate film, the primer layer preferably contains an acrylic resin.
[0058] The polyester resin may be one whose main components are a polyvalent carboxylic acid and a polyvalent hydroxy compound. Examples of polyvalent carboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, trimellitic acid monopotassium salt, and ester-forming derivatives thereof. Examples of polyhydric hydroxy compounds include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of these compounds may be appropriately selected and subjected to a conventional polycondensation reaction to synthesize a polyester resin.
[0059] The acrylic resin is a polymer of a polymerizable monomer including a (meth)acrylic monomer. Examples of the acrylic resin include a homopolymer or copolymer of a (meth)acrylic monomer, and a copolymer of a (meth)acrylic monomer and a polymerizable monomer other than a (meth)acrylic monomer. The acrylic resin may be a copolymer of such a polymer with another polymer (e.g., polyester, polyurethane, etc.). Such a copolymer is, for example, a block copolymer or a graft copolymer. Alternatively, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a solution or dispersion of a polyester. Similarly, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a solution or dispersion of a polyurethane. Similarly, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a solution or dispersion of another polymer. The polymerizable monomer is not particularly limited, but particularly representative compounds include, for example, carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, and citraconic acid, and salts thereof; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, monobutyl hydroxyl fumarate, and monobutyl hydroxy itaconate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethyl Examples of suitable monomers include alkyl (meth)acrylates such as dihexyl (meth)acrylate and lauryl (meth)acrylate; nitrogen-containing monomers such as (meth)acrylamide, diacetone acrylamide, N-methylol acrylamide and (meth)acrylonitrile; styrene-based compounds such as styrene, α-methylstyrene, divinylbenzene and vinyl toluene, vinyl esters such as vinyl propionate and vinyl acetate; silicon-containing monomers such as γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane; phosphorus-containing vinyl monomers; vinyl halides such as vinyl chloride and vinylidene chloride; and conjugated dienes such as butadiene.
[0060] The urethane resin is a polymeric compound having a urethane bond in the molecule, and is typically synthesized by the reaction of a polyol with a polyisocyanate compound. A chain extender may be used when synthesizing the urethane resin. Examples of polyols used to obtain the urethane resin include polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, and acrylic polyols. These compounds may be used alone or in combination of two or more.
[0061] Polycarbonate polyol is obtained by the reaction (dealcoholization reaction) of polyhydric alcohol with carbonate compound. Examples of polyhydric alcohol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and 3,3-dimethylolheptane. Examples of carbonate compounds include dimethyl carbonate, diethyl carbonate, diphenyl carbonate, and ethylene carbonate. Specific examples of polycarbonate polyols include poly(1,6-hexylene) carbonate and poly(3-methyl-1,5-pentylene) carbonate.
[0062] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene ether glycol, and polyhexamethylene ether glycol.
[0063] Examples of polyester polyols include those obtained by reacting a polyvalent carboxylic acid or an acid anhydride thereof with a polyhydric alcohol, and those having a derivative unit of a lactone compound such as polycaprolactone. Examples of polyvalent carboxylic acids include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, fumaric acid, maleic acid, terephthalic acid, and isophthalic acid. Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, and 2-methyl-2-propyl-1,3-propanediol. , 1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-2-hexyl-1,3-propanediol, cyclohexanediol, bishydroxymethylcyclohexane, dimethanolbenzene, bishydroxyethoxybenzene, alkyl dialkanolamines, and lactone diols.
[0064] As the polyol, in consideration of adhesion performance, polyester polyol and polycarbonate polyol are preferred, and polyester polyol is particularly preferred.
[0065] Examples of polyisocyanate compounds used to obtain urethane resins include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate; aliphatic diisocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate; aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic diisocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and isopropylidenedicyclohexyl diisocyanate. These may be used alone or in combination of two or more. There are no particular limitations on the chain extender as long as it has two or more active groups that react with an isocyanate group, and generally, a chain extender having two hydroxyl groups or two amino groups can be mainly used. Examples of chain extenders having two hydroxyl groups include glycol compounds such as aliphatic glycols such as ethylene glycol, propylene glycol, and butanediol; aromatic glycols such as xylylene glycol and bishydroxyethoxybenzene; and ester glycols such as neopentyl glycol hydroxypivalate. Examples of chain extenders having two amino groups include aromatic diamines such as tolylenediamine, xylylenediamine, and diphenylmethanediamine; aliphatic diamines such as ethylenediamine, propylenediamine, hexanediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-1,5-pentanediamine, trimethylhexanediamine, 2-butyl-2-ethyl-1,5-pentanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine; and alicyclic diamines such as 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, dicyclohexylmethanediamine, isopropylidincyclohexyl-4,4'-diamine, 1,4-diaminocyclohexane, and 1,3-bisaminomethylcyclohexane.
[0066] The urethane resin is typically used in the form of a dispersion or solution. The medium for the dispersion or solution may be a solvent, but is preferably water. The aqueous dispersion or solution of the urethane resin may be a forced emulsification type using an emulsifier, a self-emulsification type in which a hydrophilic group is introduced into the structure of the urethane resin, or a water-soluble type, etc. In particular, a self-emulsification type in which an ionic group is introduced into the structure of the urethane resin to form an ionomer is preferred, since it has excellent storage stability of the liquid and excellent water resistance and transparency of the resulting primer layer. Examples of the ionic group to be introduced into the structure of the urethane resin include a variety of groups such as a carboxyl group, a sulfonic acid group, a phosphoric acid group, a phosphonic acid group, and a quaternary ammonium salt group, with the carboxyl group being preferred. The carboxyl group is preferably in the form of a salt neutralized with a neutralizing agent such as ammonia, amines, alkali metals, inorganic alkalis, etc. Particularly preferred neutralizing agents are ammonia, trimethylamine, and triethylamine. In the urethane resin having a carboxyl group neutralized with a neutralizing agent, the carboxyl group from which the neutralizing agent is removed in the drying process after application can be used as a crosslinking reaction point with a crosslinking agent. This makes it possible to provide excellent stability in the liquid state before coating, and to improve the durability, solvent resistance, water resistance, blocking resistance, etc. of the obtained primer layer. As a method for introducing carboxyl groups into urethane resin, various methods can be used in each stage of polymerization reaction. For example, a method using a resin having carboxyl groups as a copolymerization component during prepolymer synthesis, or a method using a component having carboxyl groups as one component of polyol, polyisocyanate compound, chain extender, etc. is mentioned. In particular, a method using a carboxyl group-containing diol and introducing a desired amount of carboxyl groups by the amount of this component is preferred. For example, a carboxyl group-containing diol can be copolymerized with the diol used in synthesizing the urethane resin. Examples of the carboxyl group-containing diol include dimethylolpropionic acid, dimethylolbutanoic acid, bis-(2-hydroxyethyl)propionic acid, bis-(2-hydroxyethyl)butanoic acid, and salts of these acids in which the carboxyl group has been neutralized with a neutralizing agent.
[0067] In order to make the primer layer stronger and improve its performance such as adhesion, the primer layer preferably contains a compound derived from a crosslinking agent. As the crosslinking agent, a known material can be used, for example, a melamine compound, an isocyanate compound, an oxazoline compound, an epoxy compound, a carbodiimide compound, a silane coupling compound, a hydrazide compound, and an aziridine compound. Among them, a melamine compound, an isocyanate compound, an epoxy compound, an oxazoline compound, a carbodiimide compound, and a silane coupling compound are preferred, and from the viewpoint of further improving adhesion and durability, a melamine compound, an oxazoline compound, an isocyanate compound, and an epoxy compound are more preferred, and a melamine compound, an oxazoline compound, and an isocyanate compound are particularly preferred. These crosslinking agents may be used alone or in combination of two or more. By using two or more types in combination, adhesion and durability may be further improved.
[0068] The melamine compound is a compound having a melamine skeleton in the compound, and examples thereof include alkylolated melamine derivatives, compounds obtained by reacting an alkylolated melamine derivative with an alcohol to partially or completely etherify the same, and mixtures thereof. Examples of alcohols used for etherification include methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, and isobutanol. The melamine compound may be either a monomer or a dimer or higher polymer, or a mixture thereof. Furthermore, a melamine compound obtained by co-condensing a part of the melamine with urea or the like may be used, and a catalyst may be used to increase the reactivity of the melamine compound. In consideration of reactivity with various compounds, a melamine compound having a hydroxyl group is preferable.
[0069] The isocyanate compound refers to a compound having an isocyanate derivative structure, such as an isocyanate compound or a blocked isocyanate compound. Examples of the isocyanate compound include aromatic isocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate; aliphatic isocyanate compounds having an aromatic ring such as α,α,α',α'-tetramethylxylylene diisocyanate; aliphatic isocyanate compounds such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic isocyanate compounds such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), and isopropylidenedicyclohexyl diisocyanate. Also included are polymers and derivatives such as biuretized products, isocyanurate products, uretdione products, and carbodiimide modified products of these isocyanate compounds. These may be used alone or in combination of two or more. Among the above isocyanate compounds, aliphatic isocyanate compounds or alicyclic isocyanate compounds are preferred over aromatic isocyanate compounds from the viewpoint of avoiding yellowing due to ultraviolet rays. Examples of the blocked isocyanate compound include compounds in which the isocyanate group of the isocyanate compound is blocked with a blocking agent. Examples of the blocking agent include bisulfites, phenol-based compounds such as phenol, cresol, and ethylphenol, alcohol-based compounds such as propylene glycol monomethyl ether, ethylene glycol, benzyl alcohol, methanol, and ethanol, active methylene-based compounds such as dimethyl malonate, diethyl malonate, isobutanoyl methyl acetate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone, mercaptan-based compounds such as butyl mercaptan and dodecyl mercaptan, lactam-based compounds such as ε-caprolactam and δ-valerolactam, amine-based compounds such as diphenylaniline, aniline, and ethyleneimine, acid amide compounds such as acetanilide and acetic acid amide, and oxime-based compounds such as formaldehyde, acetaldoxime, acetoneoxime, methyl ethyl ketoneoxime, and cyclohexanoneoxime. These may be used alone or in combination of two or more. As the blocked isocyanate compound, an isocyanate compound blocked with an active methylene compound is preferred from the viewpoint that the primer layer is less likely to be destroyed. The isocyanate compound may be used alone or as a mixture or bond with various polymers. In terms of improving the dispersibility and crosslinking property of the isocyanate compound, it is preferable to use a mixture or bond with a polyester resin or a urethane resin.
[0070] The oxazoline compound is a compound having an oxazoline group in the molecule. The oxazoline compound is preferably a polymer containing an oxazoline group. The polymer containing an oxazoline group is obtained by polymerization of an addition polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition-polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. These may be used alone or in combination of two or more. Among these, 2-isopropenyl-2-oxazoline is suitable because it is easily available industrially. The other monomer is not particularly limited as long as it is a monomer that can be copolymerized with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylates such as alkyl (meth)acrylates (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salts, potassium salts, ammonium salts, tertiary amine salts, and the like); unsaturated nitriles such as acrylonitrile and methacrylonitrile; (meth)acrylonitrile; Examples of such unsaturated amides include acrylamide, N-alkyl(meth)acrylamide, and N,N-dialkyl(meth)acrylamide (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); vinyl esters include vinyl acetate and vinyl propionate; vinyl ethers include methyl vinyl ether and ethyl vinyl ether; α-olefins include ethylene and propylene; halogen-containing α,β-unsaturated monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. These may be used alone or in combination of two or more. The amount of oxazoline groups per 1 g of the oxazoline compound is preferably in the range of 0.5 to 10 mmol / g, more preferably 1 to 9 mmol / g, further preferably 3 to 8 mmol / g, and particularly preferably 4 to 6 mmol / g. If the amount of oxazoline groups is within the above range, the durability of the coating film is improved and the adhesion can be easily adjusted.
[0071] An epoxy compound is a compound having an epoxy group in the molecule. Examples of epoxy compounds include condensates of epichlorohydrin and compounds having a hydroxyl group or an amino group (ethylene glycol, polyethylene glycol, glycerin, polyglycerin, bisphenol A, etc.), and include polyepoxy compounds, diepoxy compounds, monoepoxy compounds, and glycidylamine compounds. Examples of polyepoxy compounds include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, and trimethylolpropane polyglycidyl ether. Examples of diepoxy compounds include neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and polytetramethylene glycol diglycidyl ether. Examples of monoepoxy compounds include allyl glycidyl ether, 2-ethylhexyl glycidyl ether, and phenyl glycidyl ether. Examples of glycidylamine compounds include N,N,N',N'-tetraglycidyl-m-xylylenediamine and 1,3-bis(N,N-diglycidylamino)cyclohexane.
[0072] The carbodiimide compound is a compound having one or more carbodiimide structures or carbodiimide derivative structures in the molecule. From the viewpoint of the strength of the primer layer, the carbodiimide compound is preferably a polycarbodiimide compound having two or more carbodiimide structures or carbodiimide derivative structures in the molecule. Carbodiimide compounds can be synthesized by known methods, and generally, condensation reaction of diisocyanate compounds is used. The diisocyanate compounds are not particularly limited, and both aromatic and aliphatic compounds can be used, such as tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexyl diisocyanate, and dicyclohexylmethane diisocyanate. In order to improve the water solubility or water dispersibility of the polycarbodiimide compound, a surfactant may be added, or a hydrophilic monomer such as a polyalkylene oxide, a quaternary ammonium salt of a dialkylamino alcohol, or a hydroxyalkylsulfonate may be added, within a range that does not impair the effects of the present invention.
[0073] A silane coupling compound is an organosilicon compound that has an organic functional group and a hydrolyzable group such as an alkoxy group in one molecule. Examples of the silane coupling compound include epoxy group-containing compounds such as 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; vinyl group-containing compounds such as vinyltrimethoxysilane and vinyltriethoxysilane; styryl group-containing compounds such as p-styryltrimethoxysilane and p-styryltriethoxysilane; (meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; (meth)acryloyl group-containing compounds such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2 -(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane and other amino group-containing compounds; tris(trimethoxysilylpropyl)isocyanurate, tris(triethoxysilylpropyl)isocyanurate and other isocyanurate group-containing compounds; 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane and other mercapto group-containing compounds. Among the above-mentioned compounds, from the viewpoint of the strength of the primer layer, preferred silane coupling compounds are epoxy group-containing silane coupling compounds, double bond-containing silane coupling compounds such as vinyl groups and (meth)acrylic groups, and amino group-containing silane coupling compounds.
[0074] In addition, these crosslinking agents react during the drying process and film formation process to improve the performance of the primer layer. It is assumed that the crosslinking agent-derived compounds present in the formed primer layer include unreacted crosslinking agents, reacted compounds, or mixtures thereof.
[0075] The antistatic agent contained in the primer layer is not particularly limited, and any known antistatic agent can be used. Examples of the antistatic agent include compounds having an ammonium group, polyether compounds, compounds having a sulfonic acid group, betaine compounds, and conductive organic polymers. The primer layer may contain particles to improve blocking and slip properties. The primer layer may contain additives such as antifoaming agents, coatability improvers, thickeners, organic lubricants, ultraviolet absorbers, antioxidants, foaming agents, dyes, and pigments, as necessary, within the scope of the present invention.
[0076] The proportion of the resin in 100% by mass of the primer layer is, for example, 5% by mass or more, preferably 10 to 99% by mass, more preferably 20 to 95% by mass, and even more preferably 30 to 90% by mass. If the proportion of the resin is within the above range, the adhesion performance and the appearance of the primer layer are more excellent. The proportion of the compound derived from the crosslinking agent in 100% by mass of the primer layer is, for example, 80% by mass or less, preferably 0.5 to 65% by mass, more preferably 3 to 50% by mass, and further preferably 5 to 40% by mass. If the proportion of the compound derived from the crosslinking agent is within the above range, the adhesion performance and strength of the primer layer are more excellent. The thickness of the primer layer depends on the material used in the primer layer and the performance to be achieved, so cannot be generalized, but is preferably in the range of 0.001 to 10 μm, more preferably 0.01 to 4 μm, and even more preferably 0.02 to 1 μm. The primer layer can be formed by a known method.
[0077] (Surface functional layer) The surface functional layer is a layer provided on the surface of the cured film (uneven layer) opposite to the substrate layer to impart various functions. Examples of the surface functional layer include an antifouling layer, an antistatic layer, a refractive index adjustment layer (antireflection layer, low reflection layer, etc.), an infrared absorbing layer, an ultraviolet absorbing layer, and a color correction layer. The surface functional layer may be a single layer having a single or multiple functions, or may be composed of multiple layers.
[0078] The antifouling layer is provided to improve the antifouling performance by imparting water repellency and oil repellency to the cured film. As the material used for the antifouling layer, conventionally known materials such as silicone compounds, fluorine compounds, and long-chain alkyl group-containing compounds can be used. Among these, silicone compounds and fluorine compounds are preferred for exhibiting stronger antifouling performance, and fluorine compounds and long-chain alkyl group-containing compounds are preferred from the viewpoint of not contaminating the other party with which the antifouling layer comes into contact.
[0079] The silicone compound is a compound having a silicone structure in the molecule, and examples thereof include alkyl silicones such as dimethyl silicone and diethyl silicone, and phenyl silicone and methylphenyl silicone having a phenyl group. Silicones having various functional groups can also be used, and examples thereof include ether groups, hydroxyl groups, amino groups, epoxy groups, carboxylic acid groups, halogen groups such as fluorine, perfluoroalkyl groups, various alkyl groups, and various aromatic groups and other hydrocarbon groups. As other functional groups, silicones having vinyl groups and hydrogen silicones in which hydrogen atoms are directly bonded to silicon atoms are also common, and it is also possible to use both in combination as addition type silicones (types obtained by the addition reaction of vinyl groups and hydrogen silane). In addition, a method of introducing a double bond such as an acryloyl group and reacting at the double bond is also preferred. In addition, as the silicone compound, modified silicones such as acrylic grafted silicone, silicone grafted acrylic, amino modified silicone, perfluoroalkyl modified silicone, etc. are also usable. In consideration of heat resistance and contamination, it is preferable to use a curable silicone resin, and as the type of curable type, any curing reaction type such as condensation type, addition type, active energy ray curable type, etc. can be used.
[0080] The fluorine compound is a compound containing fluorine atoms. As the fluorine compound, an organic fluorine compound is preferably used, for example, a perfluoroalkyl group-containing compound, a polymer of an olefin compound containing a fluorine atom, an aromatic fluorine compound such as fluorobenzene, etc. From the viewpoint of mold releasability, a compound having a perfluoroalkyl group is preferable. Furthermore, the fluorine compound can also be a compound containing a long chain alkyl compound as described later. Examples of the compound having a perfluoroalkyl group include perfluoroalkyl group-containing (meth)acrylates such as perfluoroalkyl (meth)acrylate, perfluoroalkyl methyl (meth)acrylate, 2-perfluoroalkyl ethyl (meth)acrylate, 3-perfluoroalkyl propyl (meth)acrylate, 3-perfluoroalkyl-1-methylpropyl (meth)acrylate, and 3-perfluoroalkyl-2-propenyl (meth)acrylate, and polymers thereof; and perfluoroalkyl group-containing vinyl ethers such as perfluoroalkyl methyl vinyl ether, 2-perfluoroalkyl ethyl vinyl ether, 3-perfluoropropyl vinyl ether, 3-perfluoroalkyl-1-methylpropyl vinyl ether, and 3-perfluoroalkyl-2-propenyl vinyl ether, and polymers thereof. In consideration of heat resistance and staining resistance, a polymer is preferable. The polymer may be a single compound or a polymer of multiple compounds. In addition, from the viewpoint of stain resistance, the perfluoroalkyl group preferably has 3 to 11 carbon atoms. Furthermore, it may be a polymer with a compound containing a long-chain alkyl compound as described below.
[0081] The long-chain alkyl compound is a compound having a straight-chain or branched alkyl group having usually 6 or more, preferably 8 or more, more preferably 12 or more carbon atoms. Examples of the alkyl group include a hexyl group, an octyl group, a decyl group, a lauryl group, an octadecyl group, and a behenyl group. Examples of the compound having an alkyl group include various long-chain alkyl group-containing polymer compounds, long-chain alkyl group-containing amine compounds, long-chain alkyl group-containing ether compounds, and long-chain alkyl group-containing quaternary ammonium salts. Considering heat resistance and stain resistance, a polymer compound is preferable. In addition, from the viewpoint of effectively obtaining antifouling properties, a polymer compound having a long-chain alkyl group in the side chain is more preferable. A polymer compound having a long-chain alkyl group in the side chain can be obtained by reacting a polymer having a reactive group with a compound having an alkyl group capable of reacting with the reactive group. Examples of the reactive group include a hydroxyl group, an amino group, a carboxyl group, and an acid anhydride group. Examples of compounds having these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, a polyester resin containing a reactive group, and a poly(meth)acrylic resin containing a reactive group. Among these, polyvinyl alcohol is preferred in terms of antifouling properties and ease of handling. Examples of compounds having an alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, and behenyl isocyanate, long-chain alkyl group-containing acid chlorides such as hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, and behenyl chloride, long-chain alkyl group-containing amines, and long-chain alkyl group-containing alcohols. Among these, in consideration of releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred. Furthermore, polymeric compounds having a long-chain alkyl group in the side chain can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of long-chain alkyl (meth)acrylates include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.
[0082] The content of the above-mentioned antifouling material for expressing the antifouling performance in the surface functional layer depends on the material used, so it cannot be generally stated, but in the case of silicone compounds and fluorine compounds, it is usually 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.2 mass% or more, and the upper limit may be 100 mass%. In addition, in the case of using a long-chain alkyl group-containing compound, it is usually 0.1 mass% or more, preferably 1 mass% or more, and even more preferably 3 mass% or more, and the upper limit may be 100 mass%. By using it in the above range, it is possible to obtain effective antifouling performance.
[0083] As the antistatic agent used when forming the antistatic layer as the surface functional layer, various conventionally known antistatic agents can be used. In addition, for example, a method of introducing a double bond such as an acryloyl group into a compound having an ammonium group and reacting at the double bond is also preferred.
[0084] Examples of the refractive index adjusting layer include a high refractive index layer, a low refractive index layer, and a laminate thereof. When the objective is to increase the refractive index, materials that have been conventionally known can be used as the material for the refractive index adjusting layer. Examples of such materials include aromatic-containing compounds such as a benzene structure, a bisphenol A structure, a melamine structure, and a fluorene structure, condensed polycyclic aromatic compounds such as naphthalene, anthracene, phenanthrene, naphthacene, benzo[a]anthracene, benzo[a]phenanthrene, pyrene, benzo[c]phenanthrene, and perylene structures, which are considered to have high refractive indexes among aromatic compounds, metal oxides such as zirconium oxide, titanium oxide, zinc oxide, tin oxide, antimony oxide, yttrium oxide, indium oxide, cerium oxide, ATO (antimony tin oxide), and ITO (indium tin oxide), metal-containing compounds such as metal chelate compounds such as titanium chelate and zirconium chelate, compounds containing a sulfur element, and compounds containing a halogen element. Metal oxides are preferably used in the form of particles since there is a concern that their adhesion may decrease depending on the form of use, and the average primary particle diameter is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 25 nm or less, from the viewpoint of coating appearance, etc. When the refractive index adjustment layer is intended to have a low refractive index, the material of the refractive index adjustment layer can be a conventionally known material, for example, low refractive index acrylic resin or urethane resin.In addition, in particular, compounds in which fluorine atoms are incorporated in the resin, for example, fluorine resin, compounds containing fluorine resin in the main skeleton, and compounds containing perfluoroalkyl groups in the side chain, can be mentioned.In addition, inorganic materials can be, for example, hollow silica particles, fluorine atom-containing inorganic compounds such as magnesium fluoride and calcium fluoride, and hollow particles or nanoporous particles thereof.
[0085] The thickness of the surface functional layer is preferably 5 times or less, more preferably 2 times or less, the height from the concave to the convex of the uneven structure of the cured film. The smaller this ratio is, the less likely the matte performance of the cured film is to decrease. The thickness of the surface functional layer depends on the height from the concave to the convex of the uneven structure of the cured film, so it cannot be generalized, but it is usually in the range of 0.001 to 3 μm, preferably 0.005 to 2 μm, more preferably 0.01 to 1 μm, even more preferably 0.02 to 0.5 μm, and particularly preferably 0.03 to 0.2 μm. By using within the above range, it is possible to achieve both the expression of the function of the surface functional layer and the matte property of the cured film. The surface functional layer can be formed by a known method.
[0086] (Back functional layer) The back functional layer is a layer provided on the surface opposite to the cured film (uneven layer) of the base layer to impart various functions. Examples of the back functional layer include an adhesive layer, an antistatic layer, a refractive index adjustment layer, and an antiblocking layer. The back functional layer may be a single layer having a single or multiple functions, or may be composed of multiple layers.
[0087] The adhesive layer is provided to bond the laminate to various adherends. The antistatic layer is provided to prevent adhesion of dust and the like due to peeling charge or frictional charge on the outermost surface of the laminate, particularly on the outermost surface opposite to the uneven layer side of the base layer, and to prevent defects and the like caused thereby. The refractive index adjustment layer is provided, for example, to improve the total light transmittance of the laminate. The antiblocking layer is provided to reduce blocking of the laminate. Examples of the adhesive that forms the adhesive layer include known adhesives such as acrylic, polyester, urethane and rubber adhesives. Among these, acrylic adhesives are preferred in view of versatility. The components forming the antistatic layer and the refractive index adjusting layer are the same as those explained for the surface functional layer.
[0088] The thickness of the back functional layer depends on the material used in the back functional layer and the performance to be achieved, so it cannot be generally stated, but is, for example, 0.001 to 30 μm. When the back functional layer is an adhesive layer, the thickness is preferably 0.01 to 30 μm, more preferably 0.1 to 20 μm. When the back functional layer is an antistatic layer, the thickness is preferably 0.001 to 10 μm, more preferably 0.01 to 5 μm. The back surface functional layer can be formed by a known method.
[0089] (Formation of surface functional layer and back functional layer) The front surface functional layer and the back surface functional layer can be formed, for example, by coating a liquid prepared by dispersing the above-mentioned components in a solution or solvent so that the solid content is approximately 0.1 to 80% by mass onto a specified surface, followed by drying and curing. Examples of the coating method include conventionally known coating methods such as gravure coating, reverse roll coating, die coating, air doctor coating, blade coating, rod coating, bar coating, curtain coating, knife coating, transfer roll coating, squeeze coating, impregnation coating, kiss coating, spray coating, calendar coating, and extrusion coating. The drying and curing conditions when forming the front functional layer and the back functional layer are not particularly limited, but the drying temperature of the solvent such as water used in the coating liquid is usually in the range of 50 to 150 ° C, preferably 80 to 130 ° C, and more preferably 90 to 120 ° C. The drying time is generally in the range of 3 to 200 seconds, preferably 5 to 120 seconds. In addition, in order to improve the strength of the front functional layer and the back functional layer, it is preferable to perform a heat treatment after drying at a temperature of usually 150 to 270 ° C, preferably 170 to 230 ° C, and more preferably 180 to 210 ° C. The heat treatment time is generally in the range of 3 to 200 seconds, preferably 5 to 120 seconds. Such a heat treatment is suitable when the laminate is a film.
[0090] (Total light transmittance) The laminate preferably has transparency. The total light transmittance measured by the method described in the Examples below is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, particularly preferably 80% or more, and most preferably 90% or more, and the higher the transmittance the better (the upper limit is 100%). EXAMPLES
[0091] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. The measurement and evaluation methods used in the present invention are as follows.
[0092] (1) Intrinsic viscosity of polyester 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (weight ratio), and measured at 30°C.
[0093] (2) Average primary particle diameter (d50:μm) The cumulative 50% value (by weight) in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device SA-CP3 manufactured by Shimadzu Corporation was taken as the average primary particle size.
[0094] (3) Weight average molecular weight (Mw) of polymer (X) The weight average molecular weight (Mw) of the acrylic polymer was measured using a gel permeation chromatography (GPC) "HLC-8120" (manufactured by Tosoh Corporation). As the column, TSKgel G5000HXL*GMHXL-L (manufactured by Tosoh Corporation) was used. In addition, a calibration curve was created using F288 / F80 / F40 / F10 / F4 / F1 / A5000 / A1000 / A500 (manufactured by Tosoh Corporation) and styrene as standard polystyrene. The measurement was performed at a column oven temperature of 40°C using 100 μl of a solution in which the polymer was dissolved in tetrahydrofuran to a concentration of 0.4%. The weight average molecular weight (Mw) was calculated in terms of standard polystyrene.
[0095] (4) Measurement of glass transition temperature (Tg) 5 mg of the sample was sealed in an aluminum pan, and the temperature was increased and decreased from -100°C to 250°C, 250°C to -100°C, and -100°C to 250°C at a rate of 10°C per minute under a nitrogen atmosphere using a differential scanning calorimeter (Seiko Instruments Inc., EXSTAR DSC6200). The inflection point at the second temperature increase was taken as the glass transition temperature (Tg).
[0096] (5) RSm, Sa and inclination angle (θa) Using a surface profile measurement system (Hitachi High-Tech Science Corporation's scanning white light interference microscope "VS1330"), the surface profile was measured by optical interference over an area of 177.60 μm × 236.87 μm on the surface of the cured film, and the data was analyzed. The evaluation length used to calculate RSm and θa was 236.87 μm. The objective lens magnification during measurement was set to 20 times. The presence or absence of a wrinkled uneven structure was also confirmed in this evaluation. The processing conditions used for data analysis are as follows. Surface correction: 4th order Interpolation: Full Interpolation Filter: Median 3x3 pixels Boundary processing: Symmetrical expansion and edge interpolation Trimming: None
[0097] (6) Total light transmittance / haze The laminate in which the cured film was formed on the substrate was used as the measurement subject. The total light transmittance and haze were measured using a Nippon Denshoku Industries haze meter "SH7000" in accordance with JIS Z8722:2009 (geometric conditions of irradiation and reception of a transmitting object), JIS K7361-1:1997 (test method for total light transmittance of plastic transparent materials), and JIS K7136:2000 (method of determining haze of plastic transparent materials).
[0098] (7) 20° and 60° gloss and matte The laminate having a cured film formed on a substrate was used as the measurement subject. The 20° and 60° gloss (20° and 60° specular gloss) was measured using a gloss meter "VG2000" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS Z 8741-1997. The lower the gloss value, the better the matte property.
[0099] (8)Pencil hardness The pencil hardness of the cured film was measured according to JIS K5600-5-4:1999 General testing methods for paints - Part 5: Mechanical properties of coatings - Section 4: Scratch hardness (pencil method).
[0100] (9) Matte finish The laminate was placed in a room illuminated by a linear white fluorescent lamp, and the distance between the fluorescent lamp and the laminate was set at 2.5 m. The matte finish on the uneven layer side (reflection of the fluorescent lamp) was evaluated by visual inspection according to the following evaluation criteria A to D. Evaluations A to C are judgments that confirm the matte finish. A: The reflected image of the fluorescent light is very blurry and the outline of the fluorescent light cannot be seen. B: The reflected image of the fluorescent light is blurred, but you can faintly see its outline. C: The reflected image of the fluorescent light is slightly blurred, and although the outline can be seen, it appears wavy and appears dark white. D: The reflected image of the fluorescent light is clear, the contours can be clearly seen, and it appears linear and white.
[0101] The materials used in the examples and comparative examples are as follows. (base material) Polyester (S1): Polyethylene terephthalate homopolymer with an intrinsic viscosity of 0.63 dl / g obtained using magnesium acetate tetrahydrate and tetrabutyl titanate as polymerization catalysts. Polyester (S2): Polyethylene terephthalate homopolymer with an intrinsic viscosity of 0.64 dl / g obtained using magnesium acetate tetrahydrate, orthophosphoric acid and germanium dioxide as polymerization catalysts. · Polyester (S3): Polyethylene terephthalate homopolymer containing 0.3 mass% silica particles with an average primary particle diameter of 2 μm.
[0102] (Synthesis of (meth)acrylic acid esters having active groups) (Synthesis Example 1) Synthesis of 2-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenoxy]ethyl methacrylate Methacrylic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) was distilled under reduced pressure, and a fraction with a purity of 99.8% or more was collected to obtain a distillate of methacrylic anhydride. The reduced pressure distillation was carried out by gradually increasing the temperature from room temperature to 90° C. under a pressure of 30 Pa. Separately, 22.4 g (0.1 mol) of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone (manufactured by Tokyo Chemical Industry Co., Ltd.) and 30.4 g (0.3 mol) of triethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 500 mL of methylene chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) to which 23.1 g (0.15 mol) of the above-mentioned distillate of methacrylic anhydride was added dropwise at room temperature and stirred for 12 hours. The reaction solution was washed three times with 500 mL of ion-exchanged water, and then the organic phase was concentrated to remove the solvent. The residue was purified by column chromatography (ethyl acetate / hexane = 10 / 90 (volume ratio)) to obtain 21.6 g of the target compound (yield 74%). 1H-NMR analysis confirmed that the compound obtained was 2-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenoxy]ethyl methacrylate. 1 H NMR (300MHz, chloroform-d): δ8.06(d,J=9.0Hz,2H),6.96(d,J=9.0Hz,2H),6.13(d,J=0.6Hz,1H),5.5 9(s,1H),4.50(d,J=5.1Hz,2H),4.29(dd,J=5.5,4.1Hz,3H),1.94(dd,J=1.6,1.0Hz,3H),1.61(s,6H).
[0103] (Production of Polymer (X)) (Production Example 1) Production of polymer (X1) having active groups that generate radicals upon irradiation with active energy rays Methyl isobutyl ketone (hereinafter referred to as MIBK) (78 parts by mass) was placed in a flask equipped with a stirrer, a cooling tube, and a thermometer, and then the flask was replaced with nitrogen and heated to 65°C, and a mixed solution of 4-methacryloyloxybenzophenone (40 parts by mass), stearyl methacrylate (10 parts by mass), 2-ethylhexyl methacrylate (30 parts by mass), hydroxyethyl methacrylate (10 parts by mass), diethylaminoethyl methacrylate (10 parts by mass), 2,2'-azobis(2,4-dimethylvaleronitrile) (0.8 parts by mass), and MIBK (78 parts by mass) was added dropwise over 2 hours. After another 2 hours, a mixed solution of azobis(2,4-dimethylvaleronitrile) (0.5 parts by mass) and MIBK (0.6 parts by mass) was added in order to increase the polymerization rate, and the mixture was maintained for 5 hours. Thereafter, the reaction solution was cooled to 40° C. to obtain an MIBK solution of a polymer having an active group (X1). The nonvolatile content of (X1) was 40% by mass, and the weight average molecular weight (Mw) of the polymer in (X1) was 17,200, the glass transition temperature was 48° C., and the content of active groups was 1.5 mmol / g.
[0104] (Production Example 2) Production of polymer (X2) having active groups that generate radicals upon irradiation with active energy rays An MIBK solution of a polymer having active groups (X2) was obtained under the same conditions as in Production Example 1, except that the composition of the mixed solution in Production Example 1 was changed to 2-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenoxy]ethyl methacrylate (25 parts by mass), 4-methacryloyloxybenzophenone (25 parts by mass), stearyl methacrylate (10 parts by mass), 2-ethylhexyl methacrylate (30 parts by mass), diethylaminoethyl methacrylate (10 parts by mass), 2,2'-azobis(2,4-dimethylvaleronitrile) (0.8 parts by mass), and MIBK (78 parts by mass). The non-volatile content of (X2) was 40% by mass, the weight average molecular weight (Mw) of the polymer in (X2) was 19,800, and the content of active groups was 1.8 mmol / g.
[0105] (Curable composition) The materials shown below were mixed in the amounts (parts by mass, calculated as non-volatile content) shown in Table 1. Next, a mixed solvent of propylene glycol monomethyl ether (hereinafter, PGM) and methyl ethyl ketone (hereinafter, MEK) (PGM:MEK (mass ratio) 7:3) was added so that the solid content concentration was 30 mass %, and the mixture was stirred until uniform, to obtain a curable composition (coating liquid) used in each of the Examples and Comparative Examples. (Meth)acrylate (B1): A mixture of pentaerythritol triacrylate (trifunctional) and pentaerythritol tetraacrylate (tetrafunctional) (Viscoat #300, manufactured by Osaka Organic Chemical Industry Co., Ltd.) (Meth)acrylate (B2): Ethoxylated dipentaerythritol hexa(meth)acrylate (hexafunctional) (A-DPH-12E, manufactured by Shin-Nakamura Chemical Co., Ltd.) Photoinitiator (E): Omnirad 184 manufactured by IGM Resins BV
[0106] [Table 1]
[0107] (Composition for forming primer layer) The polyester resin (P1), urethane resin (P2), melamine compound (P3), and particles (P4) shown below were mixed in a ratio of polyester resin (P1) / urethane resin (P2) / melamine compound (P3) / particles (P4) (solid content mass ratio) = 60 / 25 / 10 / 5 to obtain a composition for forming a primer layer. Polyester resin (P1): Water dispersion of polyester resin having the following composition Monomer composition: (acid component) terephthalic acid / isophthalic acid / 5-sodium sulfoisophthalic acid / / (diol component) ethylene glycol / 1,4-butanediol / diethylene glycol = 56 / 40 / 4 / / 70 / 20 / 10 (mol%) · Urethane resin (P2): Water dispersion of polyester-based urethane resin with the following composition Isophorone diisocyanate: terephthalic acid: isophthalic acid: ethylene glycol: diethylene glycol: dimethylolpropanoic acid = 12: 19: 18: 21: 25: 5 (mol%) Melamine compound (P3): Hexamethoxymethylolmelamine Particles: (P4): Silica particles with an average primary particle size of 0.07 μm
[0108] (Polyester film base) The raw material for the outermost layer (surface layer) was a mixture of polyesters (S1), (S2), and (S3) in proportions of 91%, 3%, and 6% by mass, respectively, and the raw material for the intermediate layer was a mixture of polyesters (S1) and (S2) in proportions of 97% and 3% by mass, respectively. Each of these raw materials was supplied to two extruders and melted at 285°C. After that, they were co-extruded onto a cooling roll set at 40°C in a layer structure of two types and three layers (surface layer / intermediate layer / surface layer = extrusion amount 1:8:1), and then cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.1 times in the longitudinal direction at a film temperature of 85°C using the difference in roll peripheral speed, and then a composition for forming a primer layer was applied to one side of this longitudinally stretched film, which was then introduced into a tenter and dried at 95°C for 10 seconds.Then, the film was stretched 4.2 times in the transverse direction at 120°C, heat-treated at 230°C for 10 seconds, and then relaxed by 2% in the transverse direction to obtain a polyester film substrate 50 μm thick (after drying) and having a 0.1 μm thick primer layer on one side.
[0109] [Examples 1 to 6] The coating solution shown in Table 1 below was applied onto the primer layer of the polyester film, dried at 70°C for 1 minute, and irradiated with excimer light (half width 14 nm) from xenon (wavelength 172 nm) at a dose of 15 mJ / cm 2 , illuminance 5mW / cm 2 The coating film made of the coating solution in Table 1 was irradiated with a 172 nm xenon excimer light irradiator (Ushio Inc., lamp unit type: SUS05 (lamp house type: H0011, lighting power supply type: B0005), nitrogen flow (oxygen concentration 1% or less)) and then irradiated with a high-pressure mercury lamp in an air atmosphere with an accumulated light dose of 400 mJ / cm. 2 , illuminance 200mW / cm 2 The layer was irradiated with ultraviolet light using a UV conveyor of a high-output UV device (model: US5-X1802-X1202) manufactured by Eye Graphics Co., Ltd., to obtain a laminate having a cured film with a thickness (after drying) of 5 μm. The cured film of this laminate had a wrinkled uneven structure, and had good matte properties and good pencil hardness. The evaluation results for this laminate are shown in Table 2 below. It should be noted that Examples 3 and 6 are reference examples.
[0110] [Comparative Examples 1 to 3] A laminate having a cured film was obtained in the same manner as in Example 1, except that the composition of the coating liquid in Example 1 was changed to the composition shown in Table 1. The obtained laminate was evaluated, and as shown in Table 2 below, no wrinkle-like irregularities were formed and the laminate did not have a matte finish.
[0111] [Comparative Examples 4 and 5] A laminate having a cured film was obtained by manufacturing in the same manner as in Example 1, except that the composition of the coating solution in Example 1 was changed to the composition shown in Table 1, and curing was performed only by irradiation with ultraviolet light from a high-pressure mercury lamp without using excimer light. When the obtained laminate was evaluated, as shown in Table 2 below, slight wrinkle-like irregularities were formed, but the matte property was weak.
[0112] [Table 2]
Claims
1. A cured film made of an active energy ray-curable composition, the film having a wrinkled uneven structure on the surface, The wrinkled uneven structure is an uneven structure formed by buckling the cured coating film, the cured coating film being formed by curing the surface side of a coating film of an active energy ray-curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays, a trifunctional (meth)acrylate, and a tetrafunctional (meth)acrylate by irradiating the surface side with excimer light, and then curing the inside of the coating film by irradiating with active energy rays other than vacuum ultraviolet rays, The arithmetic mean height (Sa) of the uneven structure defined by ISO 25178 is 0.15 μm or more, The average length (RSm) of the roughness curve element of the uneven structure according to JIS B0601:2013 is 21 μm or more, The cured film, wherein the active group is at least one group selected from the group consisting of a benzophenone group, an acetophenone group, a benzoin group, an α-hydroxyketone group, an α-aminoketone group, an α-diketone group, an α-diketone dialkyl acetal group, an anthraquinone group, a thioxanthone group, and a phosphine oxide group.
2. The cured film according to claim 1 , wherein the average value (θa) of the local inclination angle of the concave-convex structure is 2° or more.
3. 3. The cured film according to claim 1, wherein the 60° gloss of the surface is 50 or less.
4. The method for producing a cured film according to any one of claims 1 to 3, comprising irradiating a coating film of an active energy ray-curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays, a trifunctional (meth)acrylate, and a tetrafunctional (meth)acrylate with excimer light to cure a surface side of the coating film to form a cured coating film, and then irradiating the coating film with active energy rays other than vacuum ultraviolet rays to cure the inside of the coating film to form a cured film.
5. A laminate comprising the cured film according to any one of claims 1 to 3 laminated on a substrate.
6. The laminate according to claim 5 , wherein the substrate is a film.
7. 7. The method for producing a laminate according to claim 5 or 6, comprising laminating an active energy ray-curable composition containing a polymer having an active group that generates radicals upon irradiation with active energy rays, a trifunctional (meth)acrylate, and a tetrafunctional (meth)acrylate on a substrate to form a coating film, irradiating the surface side of the coating film with excimer light to cure the surface side to form a cured coating film, and then irradiating the coating film with active energy rays other than vacuum ultraviolet light to cure the interior of the coating film to form a cured film.
Citation Information
Patent Citations
Biaxially oriented thermoplastic resin film
JP1992305430A
Ultraviolet-curable resin composition
JP1993070535A
Production method of antireflection film
JP2014224920A
Cured product
JP2020111715A
JPP7156204B