Method for manufacturing light-reflecting substrate

By laminating and thermally curing a resin composition with a white inorganic pigment under controlled conditions, the method addresses poor adhesion issues in light reflective substrates, achieving high reflectance and strong bonding.

JP7563064B2Active Publication Date: 2024-10-08AJINOMOTO CO INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020152864
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-11
Publication Date
2024-10-08
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

The adhesion between the cured resin composition containing a white inorganic pigment and the conductor layer of the substrate is poor in existing light reflective substrates, leading to inadequate bonding.

Method used

A method involving laminating a resin composition containing a white inorganic pigment on a base substrate and thermally curing it under specific conditions, including a heat treatment at controlled temperatures and rates, to enhance adhesion.

Benefits of technology

The method produces a light-reflecting substrate with excellent adhesion to the base, maintaining high reflectance and ensuring strong bonding between the cured resin composition layer and the conductor layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563064000003
    Figure 0007563064000003
  • Figure 0007563064000001
    Figure 0007563064000001
  • Figure 0007563064000002
    Figure 0007563064000002
Patent Text Reader

Abstract

To provide a manufacturing method for a light reflection substrate that exhibits good substrate adhesion.SOLUTION: The manufacturing method of a light reflection substrate 1 includes the steps of laminating a resin sheet (reflection sheet) 3 including a support body and a resin composition layer containing a white inorganic pigment provided on the support body onto a substrate 2 provided with a conductor layer at least partially on the surface, so that the resin composition layer is bonded to the conductor layer of the substrate and thermally curing the resin composition layer under conditions satisfying at least one of the following (i) and (ii), in this order. (i) the resin composition layer is subjected to heat treatment to hold at a temperature T1 followed by heat treatment to hold at a temperature T2 higher than T1. (ii) the resin composition layer is heated up to the temperature T2 at a temperature increase rate of 0.5 to 30°C / minute, followed by heat treatment to hold at temperature T2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a light reflective substrate. [Background technology]

[0002] Light-emitting diodes (LEDs), which emit light with low power, are increasingly being mounted on printed wiring boards for use as backlights for liquid crystal displays in mobile devices, computers, televisions, etc., and as light sources for lighting fixtures. LEDs have become increasingly miniaturized in recent years, and there are LEDs known as mini LEDs and micro LEDs.

[0003] A reflective sheet is formed on the outermost layer of such a printed wiring board to reflect light in order to improve the efficiency of extracting light emitted from a light source. A printed wiring board provided with such a reflective sheet is also called a "light reflective substrate."

[0004] As a material for the reflective sheet of such a light-reflective substrate, for example, Patent Document 1 discloses a resin composition containing a binder polymer and crosslinked polymer particles containing a white inorganic pigment. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5797279 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the inventors have conducted research and found that when a resin composition containing a white inorganic pigment is thermally cured to form a cured body (reflective sheet), the resulting light-reflecting substrate may have poor adhesion between the cured body and the conductor layer of the base substrate (hereinafter simply referred to as "base adhesion").

[0007] An object of the present invention is to provide a method for producing a light reflective substrate that exhibits good adhesion to a substrate. [Means for solving the problem]

[0008] Means for Solving the Problems The inventors of the present invention conducted intensive research to solve the above problems and discovered that a light-reflecting substrate exhibiting good adhesion to the substrate can be produced by laminating a resin composition containing a white inorganic pigment onto a base substrate and then thermally curing the resin composition under specific conditions, thereby completing the present invention.

[0009] That is, the present invention includes the following. [1] A method for producing a light reflective substrate, comprising the following steps (A) and (B) in this order: (A) A step of laminating a resin sheet including a support and a resin composition layer containing a white inorganic pigment provided on a substrate (hereinafter referred to as a "base substrate") having a conductor layer on at least a portion of the surface thereof, such that the resin composition layer is bonded to the conductor layer of the base substrate. (B) a step of thermally curing the resin composition layer under conditions that satisfy at least one of the following (i) and (ii): (i) After the heat treatment at temperature T1, the material is subjected to a heat treatment at temperature T2 higher than temperature T1. (ii) The temperature is raised to a temperature T2 at a rate of 0.5 to 30° C. / min, and then the temperature is maintained at T2 for a heat treatment. [2] The method according to [1], wherein the support is peeled off between the step (A) and the step (B). [3] The method according to [1] or [2], wherein the resin composition layer further contains a thermosetting resin. [4] The method according to any one of [1] to [3], wherein the content of the white inorganic pigment is 20 to 60 mass % when the non-volatile components in the resin composition layer are taken as 100 mass %. [5] The method according to [3] or [4], wherein the thermosetting resin comprises an epoxy resin. [6] The method according to [5], wherein the content of the epoxy resin in the resin composition layer is 1 to 50 mass % when the non-volatile components in the resin composition layer are taken as 100 mass %. [7] The method according to any one of [1] to [6], wherein the white inorganic pigment is one or more selected from aluminum oxide, titanium oxide, zirconium oxide, magnesium oxide, barium titanate, zinc oxide, cerium oxide, and calcium carbonate. [8] The method according to any one of [1] to [7], wherein the light reflective substrate exhibits a reflectance of 85% or more for light with a wavelength of 460 nm. [9] The method according to any one of [1] to [8], wherein the adhesive strength between the cured product of the resin composition layer in the light reflective substrate and the conductor layer of the base substrate is 0.3 kgf / cm or more. Effect of the Invention

[0010] According to the present invention, it is possible to provide a method for producing a light reflective substrate that exhibits good adhesion to the underlying layer. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a light reflecting substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Before describing in detail the method for producing a light reflective substrate of the present invention (hereinafter also simply referred to as the "method of the present invention"), the resin sheet used in the method of the present invention will be described.

[0013] <Resin sheet> The resin sheet used in the method of the present invention includes a support and a resin composition layer containing a white inorganic pigment provided on the support.

[0014] (Resin composition layer) The resin composition layer contains a white inorganic pigment. This allows a cured body obtained by curing the resin composition layer to exhibit light reflecting properties. In one embodiment of the present invention, the "white inorganic pigment" refers to an inorganic compound or inorganic filler having a reflectance of 90% or more for light with a wavelength of 500 nm.

[0015] -White inorganic pigment- Examples of white inorganic pigment materials include white metal oxides such as aluminum oxide (alumina), titanium oxide, zirconium oxide, magnesium oxide, zinc oxide, cerium oxide, antimony oxide, tin oxide, barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, barium titanate zirconate, barium zirconate, and calcium zirconate; white metal sulfides such as zinc sulfide and strontium sulfide; white metal hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide; white metal nitrides such as boron nitride, aluminum nitride, and manganese nitride; white metal carbonates such as calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, and lead carbonate; white metal sulfates such as barium sulfate, calcium sulfate, and lead sulfate; white metal phosphates such as zinc phosphate, titanium phosphate, zirconium phosphate, and zirconium tungstate phosphate; white metal borates such as aluminum borate; and white minerals such as cordierite, talc, clay, mica, hydrotalcite, and boehmite.

[0016] Among these, the white inorganic pigment is preferably selected from aluminum oxide, titanium oxide, zirconium oxide, magnesium oxide, barium titanate, zinc oxide, cerium oxide, and calcium carbonate, and titanium oxide is particularly suitable. As the titanium oxide, any of rutile type, anatase type, and brookite type may be used, but rutile type is preferable from the viewpoint of further improving the reflectance. As the titanium oxide, those obtained by a method such as a sulfuric acid method or a chlorine method can be used. The material of the white inorganic pigment may be one type alone or a mixture of two or more types. The shape of the white inorganic pigment may be, for example, any of an irregular shape, a crushed shape, a scaly shape, and a spherical shape.

[0017] Examples of commercially available white inorganic pigments include "PX3788" manufactured by Sakai Chemical Industry Co., Ltd.; Typec "CR-50", "CR-57", "CR-80", "CR-90", "CR-93", "CR-95", "CR-97", "CR-60", "CR-63", "CR-67", "CR-58", "CR-85", and "UT771" manufactured by Ishihara Sangyo Kaisha; Typepure "R-100", "R-101", "R-102", "R-103", "R-104", "R-105", "R-108", "R-900", "R-902", "R-960", "R-706", and "R-931" manufactured by DuPont; "AHP300" manufactured by Nippon Light Metal Co., Ltd.; and Alnabeads "CB-P05" and "CB-A30S" manufactured by Showa Denko KK.

[0018] The specific surface area of ​​the white inorganic pigment is preferably 0.5 m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 2m 2 / g or more. There is no particular upper limit, but it is preferably 80m 2 / g or less, 70m 2 / g or less or 60m 2 The specific surface area is determined by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0019] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of the white inorganic pigment is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 2 μm or less or 1 μm or less.

[0020] The average particle size of the white inorganic pigment can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the white inorganic pigment is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the white inorganic pigment and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light source wavelengths used and a flow cell method to measure the particle size distribution of the white inorganic pigment on a volume basis, and the average particle size can be calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0021] From the viewpoint of improving moisture resistance and dispersibility, the white inorganic pigment is preferably treated with a surface treatment agent. The surface treatment agent may be used alone or in any combination of two or more. Examples of the surface treatment agent include silane coupling agents such as vinyl silane coupling agents, epoxy silane coupling agents, styryl silane coupling agents, (meth)acrylic silane coupling agents, amino silane coupling agents, isocyanurate silane coupling agents, ureido silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, acid anhydride silane coupling agents, alkyl silane coupling agents, and phenyl silane coupling agents. In the method of the present invention using specific curing conditions, from the viewpoint of easily realizing a light reflective substrate that exhibits higher reflectance and has better adhesion to the base, the surface treatment agent is preferably a surface treatment agent that does not contain a nitrogen atom (containing no nitrogen atoms), and more preferably a silane coupling agent that does not contain a nitrogen atom (containing no nitrogen atoms). Examples of the silane coupling agent that does not contain a nitrogen atom (containing no nitrogen atom) include silane coupling agents selected from phenyl silane coupling agents, alkyl silane coupling agents, epoxy-based silane coupling agents, vinyl-based silane coupling agents, (meth)acrylic-based silane coupling agents, and styryl-based silane coupling agents.

[0022] Examples of phenyl silane coupling agents include phenyl trimethoxy silane and phenyl triethoxy silane. Examples of alkyl silane coupling agents include methyl trimethoxy silane, dimethyl dimethoxy silane, methyl triethoxy silane, dimethyl diethoxy silane, n-propyl trimethoxy silane, n-propyl triethoxy silane, hexyl trimethoxy silane, hexyl triethoxy silane, octyl triethoxy silane, decyl trimethoxy silane, and 1,6-bis (trimethoxy silyl) hexane. Examples of epoxy silane coupling agents include 2- (3,4-epoxy cyclohexyl) ethyl trimethoxy silane, 3-glycidoxy propyl methyl dimethoxy silane, 3-glycidoxy propyl trimethoxy silane, 3-glycidoxy propyl methyl diethoxy silane, and 3-glycidoxy propyl triethoxy silane.

[0023] Examples of vinyl-based silane coupling agents include vinyltrimethoxysilane and vinyltriethoxysilane. Examples of (meth)acrylic-based silane coupling agents include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane. Examples of styryl-based silane coupling agents include p-styryltrimethoxysilane.

[0024] Commercially available surface treatment agents include, for example, "KBM-103" and "KBE-103" (phenyl silane coupling agents) manufactured by Shin-Etsu Chemical Co., Ltd.; "KBM-13", "KBM-22", "KBE-13", "KBE-22", "KBM-3033", "KBE-3033", "KBM-3063", "KBE-3063", "KBE-3083", "KBM-3103C", "KBM-3066", and "KBM-7103" (alkyl silane coupling agents); -1003", "KBE-1003" (vinyl silane coupling agent); "KBM-303", "KBM-402", "KBM-403", "KBE-402", "KBE-403" (epoxy silane coupling agent); "KBM-1403" (styryl silane coupling agent); "KBM-502", "KBM-503", "KBE-502", "KBE-503", "KBM-5103" ((meth)acrylic silane coupling agent).

[0025] From the viewpoint of improving the dispersibility of the white inorganic pigment, the degree of surface treatment with the surface treatment agent is preferably within a predetermined range. Specifically, 100 parts by mass of the white inorganic pigment is preferably surface-treated with 0.2 parts by mass to 5 parts by mass of the surface treatment agent, more preferably 0.2 parts by mass to 3 parts by mass, and even more preferably 0.3 parts by mass to 2 parts by mass.

[0026] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the white inorganic pigment. From the viewpoint of improving the dispersibility of the white inorganic pigment, the amount of carbon per unit surface area of ​​the white inorganic pigment is 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0027] The carbon amount per unit surface area of ​​the white inorganic pigment can be measured after the surface-treated white inorganic pigment is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the white inorganic pigment that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solids, the carbon amount per unit surface area of ​​the white inorganic pigment can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.

[0028] From the viewpoint of realizing a light-reflecting substrate exhibiting high light reflectance, the content of the white inorganic pigment in the resin composition layer is preferably 20% by mass or more, more preferably 22% by mass or more, and even more preferably 24% by mass or more or 25% by mass or more, when the non-volatile components in the resin composition layer are taken as 100% by mass.

[0029] In the prior art, when a resin composition layer with a high content of white inorganic pigment is used, the resulting light reflecting substrate tends to have poor adhesion to the substrate, but according to the method of the present invention employing specific curing conditions, the content of the white inorganic pigment can be further increased without decreasing the adhesion to the substrate. For example, the content of the white inorganic pigment in the resin composition layer may be increased to 26% by mass or more, 28% by mass or more, 30% by mass or more, 32% by mass or more, 34% by mass or more, 36% by mass or more, 38% by mass or more, or 40% by mass or more.

[0030] The upper limit of the content of the white inorganic pigment in the resin composition layer is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 60% by mass or less or 55% by mass or less, from the viewpoint of realizing good adhesion to the base.

[0031] In a preferred embodiment, the content of the white inorganic pigment is 20 to 60 mass % when the non-volatile components in the resin composition layer are taken as 100 mass %.

[0032] -Other inorganic fillers- The resin composition layer may contain other inorganic fillers as long as it contains at least a white inorganic pigment. Such other inorganic fillers are not particularly limited as long as they are inorganic fillers different from the white inorganic pigment, and for example, an inorganic filler having a reflectance of less than 90% for light with a wavelength of 500 nm may be used.

[0033] Among them, in the method of the present invention employing specific curing conditions, silica is suitable as the other inorganic filler from the viewpoint of easily realizing a light-reflecting substrate exhibiting higher reflectance and having better adhesion to the base. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Moreover, as the silica, spherical silica is preferred. The specific surface area and average particle size of silica are the same as those of the white inorganic pigment. Silica may be used alone or in combination of two or more types.

[0034] Examples of commercially available silica products include "UFP-30" manufactured by Denka; "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; and "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs.

[0035] In order to improve moisture resistance and dispersibility, it is preferable that the other inorganic fillers such as silica are treated with a surface treatment agent. Examples of the surface treatment agent include the same surface treatment agents as those for the white inorganic pigment. The degree of surface treatment of the other inorganic fillers with the surface treatment agent is the same as that of the white inorganic pigment.

[0036] From the viewpoint of obtaining the effects of the present invention remarkably, the content of the other inorganic filler in the resin composition layer is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more, when the non-volatile components in the resin composition layer are 100% by mass. The upper limit of the content of the other inorganic filler is preferably 70% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, and particularly preferably 35% by mass or less.

[0037] From the viewpoint of realizing a light-reflective substrate that exhibits high light reflectance and good adhesion to the base, the total content of the white inorganic pigment and other inorganic filler, i.e., the total content of the inorganic filler components, is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, particularly preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 75% by mass or less, and particularly preferably 70% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass.

[0038] The mass ratio of other inorganic fillers such as silica to the white inorganic pigment (mass of other inorganic fillers / mass of white inorganic pigment) is, from the viewpoint of realizing a light-reflecting substrate that exhibits high light reflectance and good adhesion to the base, preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.5 or more, particularly preferably 0.8 or more, and is preferably 4 or less, more preferably 4 or less, even more preferably 2 or less, particularly preferably 1.5 or less.

[0039] The resin composition layer contains a thermosetting resin as a resin. As the thermosetting resin, a conventionally known thermosetting resin used when forming an insulating layer of a printed wiring board can be used, and among them, in the method of the present invention using specific curing conditions, an epoxy resin is preferred from the viewpoint of easily realizing a light reflective substrate that exhibits a higher reflectance and has better adhesion to the base. Therefore, in one embodiment, the resin composition contains a thermosetting resin, and in a preferred embodiment, the thermosetting resin contains an epoxy resin.

[0040] -Epoxy resin- The epoxy resin means a curable resin having an epoxy group. The epoxy resin may be used alone or in combination of two or more kinds.

[0041] Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, hydrogenated bisphenol A type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl esters, and the like. Examples of epoxy resins that can be used include aryl epoxy resins, cresol novolac epoxy resins, phenol aralkyl epoxy resins, biphenyl epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane epoxy resins, cyclohexane dimethanol epoxy resins, naphthylene ether epoxy resins, trimethylol epoxy resins, tetraphenylethane epoxy resins, isocyanurate epoxy resins, phenolphthalimidine epoxy resins, and phenolphthalein epoxy resins.

[0042] The resin composition layer preferably contains, as an epoxy resin, an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0043] Epoxy resins include epoxy resins that are solid at a temperature of 25° C. (hereinafter also referred to as "solid epoxy resins") and epoxy resins that are liquid at a temperature of 25° C. (hereinafter also referred to as "liquid epoxy resins"). In the resin sheet used in the method of the present invention, the resin composition layer may contain, as the epoxy resin, only a solid epoxy resin, or only a liquid epoxy resin, or may contain a combination of a solid epoxy resin and a liquid epoxy resin.

[0044] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0045] Preferred solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, and phenolphthalein type epoxy resins.

[0046] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; and "EXA-73" manufactured by DIC Corporation. 11", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN475V" manufactured by Nippon Steel Chemical & Material Co., Ltd. (Naphthalene type epoxy resin); "ESN485" (Naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (Dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (Bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (Biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (Anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX77" manufactured by Mitsubishi Chemical Co., Ltd. Examples of epoxy resins include "PG-100" (phenol aralkyl type epoxy resin), "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals, "YX7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical, "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical, "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical, "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical, and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. These may be used alone or in combination of two or more types.

[0047] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0048] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, hydrogenated bisphenol A type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, and epoxy resins having a butadiene structure.

[0049] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", and "825" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycilol type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L" and "EP-3980S" (glycidylamine type epoxy resins) manufactured by ADEKA Corporation; and "EP-4088S" (glycidylamine type epoxy resins) manufactured by ADEKA Corporation. Examples of such epoxy resins include: "ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd. (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); "EX-721" manufactured by Nagase Chemtex Corporation (glycidyl ester type epoxy resin); "Celloxide 2021P" manufactured by Daicel Corporation (alicyclic epoxy resin having an ester skeleton); "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" manufactured by Nippon Soda Co., Ltd. (epoxy resin having a butadiene structure); "ZX1658" and "ZX1658GS" manufactured by Nippon Steel Chemical & Material Co., Ltd. (1,4-glycidylcyclohexane type epoxy resin), "YX8000" manufactured by Mitsubishi Chemical Corporation (hydrogenated bisphenol A type epoxy resin), and "KF-101" manufactured by Shin-Etsu Chemical Co., Ltd. (epoxy modified silicone resin). These may be used alone or in combination of two or more types.

[0050] The epoxy resin may be any one of a solid epoxy resin, a liquid epoxy resin, or a combination thereof. However, from the viewpoint of easily realizing a light-reflecting substrate exhibiting a higher reflectance and having even better adhesion to the base in the method of the present invention employing specific curing conditions, it is preferable for the epoxy resin to contain a solid epoxy resin, and it is particularly preferable for the epoxy resin to be a combination of a solid epoxy resin and a liquid epoxy resin.

[0051] When a solid epoxy resin and a liquid epoxy resin are used in combination as the epoxy resin, the mass ratio thereof (solid epoxy resin:liquid epoxy resin) is preferably 20:1 to 1:20, more preferably 10:1 to 1:10, and particularly preferably 3:1 to 1:3.

[0052] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 1,000 g / eq., even more preferably 80 g / eq. to 500 g / eq., and even more preferably 100 g / eq. to 300 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0053] The weight average molecular weight (Mw) of the epoxy resin is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0054] From the viewpoint of obtaining the remarkable effect of the present invention, the content of the epoxy resin is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, even more preferably 10% by mass or more or 15% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less, and particularly preferably 30% by mass or less, when the non-volatile components in the resin composition layer are taken as 100% by mass. Therefore, in a preferred embodiment, the content of the epoxy resin is 1 to 50% by mass, when the non-volatile components in the resin composition layer are taken as 100% by mass.

[0055] In the resin sheet used in the method of the present invention, the resin composition layer may further contain other components. Such other components include, for example, a curing agent, a thermoplastic resin, a curing accelerator, and other additives. Each component will be described in detail below.

[0056] - Hardener - The resin composition layer may contain a curing agent. The curing agent has a function of reacting with the epoxy resin to cure the resin composition. The curing agent may be used alone or in combination of two or more kinds.

[0057] The curing agent is not particularly limited, and examples thereof include phenol-based curing agents, carbodiimide-based curing agents, acid anhydride-based curing agents, amine-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, thiol-based curing agents, etc. In the method of the present invention employing specific curing conditions, the curing agent preferably contains a phenol-based curing agent, from the viewpoint of easily realizing a light-reflecting substrate that exhibits higher reflectance and is more excellent in adhesion to the base.

[0058] The phenol-based curing agent is a curing agent having two or more phenolic hydroxyl groups in one molecule, and examples thereof include bisphenol-based curing agents, biphenyl-type phenol-based curing agents, naphthalene-type phenol-based curing agents, phenol novolac-type phenol-based curing agents, naphthylene ether-type phenol-based curing agents, triazine skeleton-containing phenol-based curing agents, polyphenylene ether-type phenol-based curing agents, phenol aralkyl-type phenol-based curing agents, cresol novolac-type phenol-based curing agents, bisphenol-type phenol-based curing agents, etc. From the viewpoint of easily realizing a light-reflecting substrate exhibiting a higher reflectance and having even better adhesion to the base, a bisphenol-based curing agent is preferable, more preferably a bisphenol-based curing agent selected from a bisphenol compound having a fluorine atom, a bisphenol compound having an alicyclic structure, and a bisphenol compound having a fluorene skeleton, further preferably a bisphenol compound having a fluorine atom, and particularly preferably bisphenol AF.

[0059] Commercially available phenolic hardeners include "BIS-AF" and "BIS-Z" manufactured by Central Glass Co., Ltd., "BisE" and "BisP-TMC" manufactured by Honshu Chemical Industry Co., Ltd., "BisA", "BisF", and "BisP-M" manufactured by Mitsui Fine Chemicals Co., Ltd., "BisP-AP", "BisP-MIBK", "BisP-B", "Bis-Z", "BisP-CP", "o,o'-BPF", "BisP-IOTD", "BisP-IBTD", "BisP-DED", and "BisP-BA" manufactured by Honshu Chemical Industry Co., Ltd. Kagaku Kogyo Co., Ltd. "Bis-C", "Bis26X-A", "BisOPP-A", "BisOTBP-A", "BisOCHP-A", "BisOFP-A", "BisOC-Z", "BisOC-FL", "BisOFP-A", "BisOC-CP" ", "BisOCHP-Z", "methylenebisP-CR", "TM-BPF", "BisOC-F", "Bis3M6B-IBTD", "BisOC-IST", "BisP-IST", "BisP-PRM", "BisP-LV", etc.

[0060] The carbodiimide-based curing agent is a curing agent having two or more carbodiimide structures in one molecule, and examples of the curing agent include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(methylenediphenylenecarbodiimide), poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide].

[0061] Commercially available carbodiimide curing agents include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0062] The acid anhydride curing agent is a curing agent having one or more carboxylic acid anhydride groups (-CO-O-CO-) in one molecule, and examples thereof include phthalic anhydride, pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, methylene-4,4' aromatic acid anhydride-based hardeners such as tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, cyclopentanetetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, and the like; and polymeric anhydride-based hardeners such as styrene / maleic anhydride copolymer, and alkyl (meth)acrylate / styrene / maleic anhydride copolymer. Commercially available acid anhydride curing agents include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd., "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation, and "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.

[0063] The amine-based curing agent is a curing agent having two or more amino groups, and examples thereof include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines. Among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or a secondary amine, and more preferably a primary amine. Specific examples of the amine-based curing agent include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propane, and the like. propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. As the amine-based curing agent, commercially available products may be used, and examples thereof include "SEIKACURE-S" manufactured by Seika Corporation, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.

[0064] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0065] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0066] The thiol-based curing agent is a curing agent having two or more mercapto groups, and examples thereof include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.

[0067] The reactive group equivalent of the curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The reactive group equivalent is the mass of the curing agent per equivalent of reactive group. For example, in the case of a phenol-based curing agent, the reactive group is a phenolic hydroxyl group. In the case of an acid anhydride-based curing agent, one equivalent of a carboxylic anhydride group (-CO-O-CO-) corresponds to two equivalents of reactive group.

[0068] From the viewpoint of obtaining the effects of the present invention prominently, the content of the curing agent is, when the non-volatile components in the resin composition layer are taken as 100% by mass, preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less, for example, 0% by mass or more, 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 1% by mass or more, and particularly preferably 3% by mass or more.

[0069] -Thermoplastic resin- The resin composition layer may contain a thermoplastic resin. The thermoplastic resin may be used alone or in combination of two or more kinds.

[0070] Examples of thermoplastic resins include phenoxy resins, polyvinyl acetal resins, acrylic resins, polyolefin resins, polybutadiene resins, polyimide resins, polyamideimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polyetherimide resins, polycarbonate resins, polyetheretherketone resins, and polyester resins. Of these, resins selected from phenoxy resins, acrylic resins, and polyphenylene ether resins are preferred.

[0071] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation, "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "YX7200B35", "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.

[0072] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0073] The acrylic resin refers to a polymer obtained by polymerizing a monomer component including a (meth)acrylic acid ester monomer. The monomer components constituting the acrylic resin may contain, in addition to the (meth)acrylic acid ester monomer, a (meth)acrylamide monomer, a styrene monomer, a functional group-containing monomer, or the like as copolymerization components. Specific examples of acrylic resins include "ARUFON UP-1000", "ARUFON UP-1010", "ARUFON UP-1020", "ARUFON UP-1021", "ARUFON UP-1061", "ARUFON UP-1080", "ARUFON UP-1110", "ARUFON UP-1170", "ARUFON UP-1190", "ARUFON UP-1500", "ARUFON UH-2000", "ARUFON UH-2041", "ARUFON UH-2190", "ARUFON UHE-2012", "ARUFON UC-3510", "ARUFON UG-4010", "ARUFON US-6100", and "ARUFON US-6170", all manufactured by Toagosei Co., Ltd. These may be used alone or in combination of two or more.

[0074] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin-based elastomers such as polypropylene and ethylene-propylene block copolymer.

[0075] Examples of polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxy group-containing polybutadiene resins, phenolic hydroxy group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, isocyanate group-containing polybutadiene resins, urethane group-containing polybutadiene resins, polyphenylene ether-polybutadiene resins, and the like.

[0076] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).

[0077] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.

[0078] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0079] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0080] Specific examples of polyphenylene ether resins include oligophenylene ether-styrene resins "OPE-2St1200" and "OPE-2St2200" manufactured by Mitsubishi Gas Chemical Company, Inc., and "Noryl (registered trademark) SA90" manufactured by SABIC, etc. Specific examples of polyetherimide resins include "Ultem" manufactured by GE, etc.

[0081] Examples of polycarbonate resins include hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxyl group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, and urethane group-containing carbonate resins. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002" and "T6001" (polycarbonate diol) manufactured by Asahi Kasei Chemicals Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diol) manufactured by Kuraray Co., Ltd. Specific examples of polyether ether ketone resins include "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd. Examples of polyester resins include polyethylene terephthalate resins.

[0082] The weight average molecular weight of the thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more, and is preferably 100,000 or less, more preferably 70,000 or less, and even more preferably 60,000 or less. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0083] The thermoplastic resin is preferably one that, when formed into a film having a thickness of 20 μm, has a transmittance of 80% or more for light having a wavelength of 450 nm that is incident perpendicularly to the film surface.

[0084] The content of the thermoplastic resin, when the non-volatile components in the resin composition layer are taken as 100% by mass, is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less, for example, 0% by mass or more, 0.1% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, and particularly preferably 10% by mass or more.

[0085] -Curing accelerator- The resin composition layer may contain a curing accelerator. The curing accelerator has a function of accelerating the curing reaction of the thermosetting resin. The curing accelerator may be used alone or in combination of two or more.

[0086] Examples of the curing accelerator include phosphorus-based curing accelerators, imidazole-based curing accelerators, amine-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, etc. Among them, from the viewpoint of achieving a higher light reflectance, phosphorus-based curing accelerators and imidazole-based curing accelerators are preferred, and phosphorus-based curing accelerators are more preferred.

[0087] From the viewpoint of achieving a higher light reflectance, the phosphorus-based curing accelerator preferably contains one or more members selected from the group consisting of phosphonium salts and phosphines.

[0088] Examples of the phosphonium salt include aliphatic phosphonium salts such as tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitate, tetrabutylphosphonium hydrogenhexahydrophthalate, tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butylmethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, and the like. Examples of aromatic phosphonium salts include aromatic phosphonium salts such as phenylphosphonium bromide, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate.

[0089] Examples of phosphines include aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine; dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, and tris(2,5-dimethylphenyl)phosphine. tris(2,6-dimethylphenyl)phosphine, tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2- Examples of aromatic phosphines include bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; and aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct.

[0090] As the phosphorus-based curing accelerator, commercially available products may be used, for example, "TBP-DA" manufactured by Hokko Chemical Industry Co., Ltd.

[0091] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.

[0092] As the imidazole-based curing accelerator, commercially available products may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation, and "1B2PZ-10M" manufactured by Shikoku Kasei Co., Ltd.

[0093] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.

[0094] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.

[0095] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0096] From the viewpoint of obtaining the effects of the present invention prominently, the content of the curing accelerator is, when the non-volatile components in the resin composition layer are taken as 100% by mass, preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.8% by mass or less, for example, 0% by mass or more, 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more.

[0097] -Other additives- The resin composition layer may further contain other additives. Examples of the other additives include photocurable components such as (meth)acrylic resins and radical polymerizable compounds, as well as diluents and photopolymerization initiators as auxiliary agents; organic fillers such as rubber particles; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, and salicylic acid-based ultraviolet absorbers; adhesion improvers such as urea silane; adhesion imparters such as triazole-based adhesion imparters, tetrazole-based adhesion imparters, and triazine-based adhesion imparters; and hindered phenol-based antioxidants. antioxidants such as fluorine-based surfactants, silicone-based surfactants, etc.; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. One type of other additive may be used alone, or two or more types may be used in combination at any ratio. The content of other additives can be appropriately set by those skilled in the art.

[0098] From the viewpoint of making the light reflecting substrate thinner, and because the light reflecting substrate produced by the method of the present invention has excellent light reflectance even when the reflective sheet (cured product of the resin composition layer) is a thin film, the thickness of the resin composition layer is preferably 200 μm or less, more preferably 150 μm or less or 100 μm or less, and even more preferably 80 μm or less, 60 μm or less, or 50 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, but may usually be 10 μm or more, 15 μm or more, 20 μm or more, etc.

[0099] In the method of the present invention employing specific curing conditions, from the viewpoint of easily realizing a light-reflecting substrate that exhibits higher reflectivity and has even better adhesion to the base, the resin composition layer preferably has a minimum melt viscosity of 5,000 poise or less, more preferably 2,000 poise or less, even more preferably 1,000 poise or less, and particularly preferably 500 poise or less.

[0100] -Support- Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0101] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate (PC), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0102] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0103] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0104] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "PET501010", "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0105] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0106] The support may also be a metal foil with a support substrate, which is a thin metal foil with a peelable support substrate attached thereto. In one embodiment, the metal foil with a support substrate includes a support substrate, a release layer provided on the support substrate, and a metal foil provided on the release layer. When a metal foil with a support substrate is used as the support, the resin composition layer is provided on the metal foil.

[0107] In the metal foil with a supporting substrate, the material of the supporting substrate is not particularly limited, and examples thereof include copper foil, aluminum foil, stainless steel foil, titanium foil, copper alloy foil, etc. When copper foil is used as the supporting substrate, it may be electrolytic copper foil or rolled copper foil. In addition, the release layer is not particularly limited as long as it can release the metal foil from the supporting substrate, and examples thereof include an alloy layer of an element selected from the group consisting of Cr, Ni, Co, Fe, Mo, Ti, W, and P; an organic coating, etc.

[0108] In the metal foil with a supporting substrate, the material of the metal foil is preferably, for example, copper foil or copper alloy foil.

[0109] In the metal foil with a supporting substrate, the thickness of the supporting substrate is not particularly limited, but is preferably in the range of 10 μm to 150 μm, more preferably in the range of 10 μm to 100 μm, and the thickness of the metal foil may be, for example, in the range of 0.1 μm to 10 μm.

[0110] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0111] The resin sheet can be produced, for example, by preparing a liquid resin composition as is or a resin varnish by dissolving the resin composition in an organic solvent, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.

[0112] As the organic solvent, a known one can be appropriately used, and the type is not particularly limited. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, and diphenyl ether; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of the organic solvent include ether ester solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in combination of two or more in any ratio.

[0113] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin composition (resin varnish), for example, when a resin composition (resin varnish) containing 30 mass % to 60 mass % of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0114] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0115] The method for producing a light reflecting substrate of the present invention (hereinafter, simply referred to as the "method of the present invention") will be described in detail below based on preferred embodiments. However, the present invention is not limited to the following embodiments, and can be modified as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.

[0116] [Method of manufacturing light-reflecting substrate] The method for producing a light reflective substrate of the present invention is characterized by comprising the following steps (A) and (B) in this order: (A) A step of laminating a resin sheet including a support and a resin composition layer containing a white inorganic pigment provided on a substrate having a conductor layer on at least a part of the surface thereof such that the resin composition layer is bonded to the conductor layer of the substrate. (B) a step of thermally curing the resin composition layer under conditions that satisfy at least one of the following (i) and (ii): (i) After the heat treatment at temperature T1, the material is subjected to a heat treatment at temperature T2 higher than temperature T1. (ii) The temperature is raised to a temperature T2 at a rate of 0.5 to 30° C. / min, and then the temperature is maintained at T2 for a heat treatment.

[0117] In the present invention, the phrase "including steps (A) and (B) in this order" does not preclude the inclusion of other steps, so long as steps (A) and (B) are included and are performed in this order. The same applies to "including in this order" when referring to steps or processes hereinafter.

[0118] -Process (A)- In step (A), a resin sheet including a support and a resin composition layer containing a white inorganic pigment provided on the support is laminated on a substrate having a conductor layer on at least a portion of its surface such that the resin composition layer is bonded to the conductor layer of the substrate.

[0119] The structure of the resin sheet is as described above.

[0120] The substrate used in step (A) is not particularly limited as long as it has a conductor layer on at least a part of its surface, and examples thereof include glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates, etc., on one or both sides of which a conductor layer is formed. The conductor layer may be patterned. A substrate on which a conductor layer (circuit) is formed on one or both sides may be called an "inner layer circuit substrate". In addition, when manufacturing a printed wiring board (light reflecting substrate), an intermediate product on which an insulating layer and / or a conductor layer is to be further formed is also included in the "substrate" of the present invention. When the light reflecting substrate is a circuit board with built-in components, a circuit board with built-in components may be used.

[0121] In the present invention, the substrate having a conductor layer on at least a part of its surface, which is the target onto which the resin sheet is laminated in step (A), is also simply referred to as a "base substrate".

[0122] The substrate and the resin sheet can be laminated, for example, by thermocompression bonding the resin sheet to the substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression bonding member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate.

[0123] The substrate and the resin sheet may be laminated by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably carried out under reduced pressure conditions of 26.7hPa or less.

[0124] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0125] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0126] The support may be peeled off (removed) between step (A) and step (B), or may be peeled off after step (B). In the method of the present invention employing specific curing conditions, it is preferable to peel off the support between step (A) and step (B) from the viewpoint of easily realizing a light reflective substrate that exhibits higher reflectance and is more excellent in adhesion to the base. Therefore, in a preferred embodiment, the support is peeled off between step (A) and step (B).

[0127] In addition, when the reflective sheet (cured body) formed by curing the resin composition layer is used as an interlayer insulating layer, and when a metal foil is used as the support, the conductor layer may be formed using the metal foil without peeling off the support. In addition, when a metal foil with a support substrate is used as the support, the support substrate (and the peel layer) may be peeled off. Then, the conductor layer can be formed using the metal foil.

[0128] -Process (B)- In step (B), the resin composition layer is thermally cured, thereby forming a reflective sheet (cured product) on the base substrate.

[0129] In order to realize a light reflective substrate having good adhesion to the underlying layer, it is important to thermally cure the resin composition layer under conditions that satisfy at least one of the following (i) and (ii). (i) After the heat treatment at temperature T1, the material is subjected to a heat treatment at temperature T2 higher than temperature T1. (ii) The temperature is raised to a temperature T2 at a rate of 0.5 to 30° C. / min, and then the temperature is maintained at T2 for a heat treatment.

[0130] According to the method of the present invention, which employs such specific curing conditions, a light-reflecting substrate exhibiting high reflectance and good adhesion to the substrate can be realized. When the composition of the cured body formed from the resin composition layer of the light-reflecting substrate manufactured by the method of the present invention was examined, the inventors confirmed that a phase rich in inorganic filler components exists on the surface on the side not in contact with the substrate, but the proportion of inorganic filler components decreases at a certain distance from the surface in the thickness direction. Here, the "thickness direction" refers to the thickness direction of the cured body, and indicates the direction perpendicular to the main surface of the cured body.

[0131] It is presumed that the inorganic filler component-rich phase present in a limited region near the surface on the side not in contact with the base substrate realizes a light reflectance that is significantly higher than would be expected from the bulk inorganic filler concentration, and that the resin component-rich phase present in the region near the main surface in contact with the base substrate provides excellent adhesion to the base substrate.

[0132] -Thermosetting conditions (i)- Thermal curing of the resin composition layer under conditions that satisfy (i) may be referred to as a "step cure", a heat treatment in which the resin composition layer is maintained at a temperature T1 may be referred to as a "precure", and a heat treatment in which the resin composition layer is maintained at a temperature T2 higher than the temperature T1 may be referred to as a "postcure".

[0133] Regarding the thermal curing condition (i), the temperature T1, although depending on the composition of the resin composition layer, can usually be 50°C≦T1<150°C, preferably 60°C≦T1≦140°C, more preferably 70°C≦T1≦130°C, even more preferably 80°C≦T1≦120°C, and particularly preferably 80°C≦T1≦110°C.

[0134] The time for which the temperature T1 is maintained varies depending on the value of the temperature T1, but is preferably 10 to 150 minutes, more preferably 15 to 120 minutes, and even more preferably 20 to 120 minutes.

[0135] The heat treatment held at temperature T1 may be carried out under normal pressure or under reduced pressure, but from the viewpoint of easily realizing a light-reflecting substrate that exhibits higher reflectivity and has even better adhesion to the base, it is preferable to carry out the treatment at an air pressure in the range of 0.075 mmHg to 3751 mmHg (0.1 hPa to 5000 hPa), more preferably in the range of 1 mmHg to 1875 mmHg (1.3 hPa to 2500 hPa).

[0136] The temperature T2 varies depending on the composition of the resin composition layer, but can usually be 150°C≦T2≦250°C, preferably 155°C≦T2≦230°C, more preferably 160°C≦T2≦220°C, even more preferably 170°C≦T2≦210°C, and particularly preferably 180°C≦T2≦200°C.

[0137] The temperatures T1 and T2 preferably satisfy the relationship 20°C≦T2-T1≦150°C, more preferably 30°C≦T2-T1≦140°C, further preferably 40°C≦T2-T1≦130°C, and particularly preferably 50°C≦T2-T1≦120°C.

[0138] The time for which the temperature T2 is maintained varies depending on the value of the temperature T2, but is preferably 10 to 150 minutes, more preferably 15 to 120 minutes, and even more preferably 20 to 120 minutes.

[0139] The heat treatment at temperature T2 may be carried out under normal pressure or reduced pressure, and is preferably carried out under the same air pressure as that for the heat treatment at temperature T1.

[0140] After the heat treatment at temperature T1, the resin composition layer may be cooled once and then subjected to heat treatment at temperature T2. Alternatively, after the heat treatment at temperature T1, the resin composition layer may be subjected to heat treatment at temperature T2 without being cooled. The heat treatment at temperature T1 and the heat treatment at temperature T2 may be performed using the same heat treatment device, or the heat treatment at temperature T1 may be performed using a first heat treatment device, and the heat treatment at temperature T2 may be performed using a second heat treatment device different from the first heat treatment device. The heat treatment device is not particularly limited as long as it can thermally cure the resin composition layer on the base substrate to form a cured body, and a conventionally known device may be used. For example, an oven, a hot press, or the like may be used as the heat treatment device. For example, after the heat treatment at temperature T1 is performed using an oven adjusted to temperature T1, the object to be heated may be transferred to an oven adjusted to temperature T2 and heat treatment at temperature T2 may be performed. Alternatively, a heat treatment at temperature T1 may be performed using a heat treatment device capable of temperature programming, followed by increasing the temperature from T1 to T2, and then performing a heat treatment at temperature T2. In this case, the rate of temperature increase from T1 to T2 is not particularly limited and may be any value, and may be within the same range as the rate of temperature increase in the thermal curing condition (ii) described later.

[0141] Regarding the thermal curing condition (i), as long as it includes a heat treatment at temperature T1 and a heat treatment at temperature T2 higher than temperature T1 in this order, it may be subjected to a heat treatment at another temperature. In other words, the step cure of the thermal curing condition (i) is not limited to a two-step heat treatment, and may include three or more steps of heat treatment.

[0142] -Thermosetting conditions (ii)- Heat curing of the resin composition layer under the condition (ii) is sometimes referred to as "(programmed) temperature rise cure".

[0143] The value of temperature T2 and the time for which it is held at temperature T2 may be the same as those described for the thermal curing condition (i).

[0144] Regarding the thermal curing condition (ii), the rate of temperature rise when raising the temperature to T2 is in the range of 0.5 to 30° C. / min, from the viewpoint of realizing a light reflective substrate exhibiting high reflectance and having good adhesion to the base, and is preferably 1° C. / min or more, more preferably 1.5° C. / min or more, 2° C. / min or more, or 2.5° C. / min or more, and is preferably 25° C. / min or less, more preferably 20° C. / min or less, 15° C. / min or less, 10° C. / min or less, 8° C. / min or less, or 6° C. / min or less.

[0145] The heating rate does not need to be constant from the heating start temperature T0 to the temperature T2, and may be changed within the above-mentioned preferred range. The heating start temperature T0 is not particularly limited, and may be the environmental temperature (room temperature, etc.) when the method of the present invention is carried out.

[0146] The temperature rise cure may be carried out under normal pressure or under reduced pressure, and is preferably carried out under the same air pressure as that described for the step cure.

[0147] The heat treatment device used for the temperature rise cure is not particularly limited as long as it can raise the temperature of the resin composition layer on the base substrate at a predetermined temperature rise rate and can heat the layer to a temperature T2, and any conventionally known device may be used. For example, an oven, a hot press, etc. may be used as the heat treatment device.

[0148] By the step (B), a reflective sheet consisting of a cured product of the resin composition layer is formed on the base substrate. In the light reflective substrate produced, the reflective sheet may be included as an interlayer insulating layer or a solder resist. When the reflective sheet is included as an interlayer insulating layer, the method of the present invention may also include a step of forming a conductor layer on the reflective sheet. Such a step can be carried out according to various methods used in the production of printed wiring boards that are known to those skilled in the art.

[0149] The method of the present invention may also include a step of arranging a light source on the reflective sheet (C) (the cured product of the resin composition layer). Examples of the light source include a light emitting diode (LED), a mini LED, a micro LED, and the like.

[0150] As shown in an example in Fig. 1, the light reflective substrate 1 has a reflective sheet 3 formed on a substrate 2, and a light source 4 such as a light emitting diode (LED) is disposed on a surface 31 of the reflective sheet 3. The substrate 2 corresponds to the above-mentioned "base substrate" (the conductor layer is not shown in Fig. 1), and the surface 31 of the reflective sheet 3 corresponds to the above-mentioned "surface not in contact with the base substrate."

[0151] In order to increase the efficiency of extracting light emitted from the light source, the surface of the reflective sheet facing the light source may have a recess in addition to being flat as shown in Fig. 1. When the surface of the reflective sheet has a recess, it is preferable to place the light source in the recess.

[0152] If necessary, after electrically connecting the light source, the light source may be fixed by performing a sealing process or the like on the light source.

[0153] The light reflecting substrate produced by the method of the present invention has a phase rich in inorganic filler components in the region near the surface of the reflecting sheet (cured product of the resin composition layer) on the side not in contact with the base substrate, and therefore exhibits high light reflectance, for example, preferably exhibits a reflectance of 85% or more, more preferably 86% or more or 88% or more, and even more preferably 90% or more, 92% or more, 94% or more, or 95% or more, with respect to light having a wavelength of 460 nm. The upper limit of such light reflectance may be 100% or less. Therefore, in a preferred embodiment, the light reflecting substrate exhibits a reflectance of 85% or more with respect to light having a wavelength of 460 nm. The light reflectance of the cured product can be measured, for example, using a multichannel spectrometer (MCPD-7700, manufactured by Otsuka Electronics Co., Ltd.).

[0154] The light reflecting substrate manufactured by the method of the present invention can achieve such a high light reflectance without a decrease in the adhesion to the substrate. For example, in the light reflecting substrate manufactured by the method of the present invention, the reflecting sheet (cured resin composition layer) exhibits an adhesion strength to the conductor layer of the substrate of preferably 0.3 kgf / cm or more, more preferably 0.32 kgf / cm or more, 0.34 kgf / cm or more, 0.35 kgf / cm or more, 0.36 kgf / cm or more, 0.38 kgf / cm or more, or 0.4 kgf / cm or more. The upper limit of such adhesion strength may be 1 kgf / cm or less, 0.9 kgf / cm or less, etc. Therefore, in a preferred embodiment, the adhesion strength between the reflecting sheet in the light reflecting substrate and the conductor layer of the substrate is 0.3 kgf / cm or more.

[0155] [Semiconductor Devices] A semiconductor device can be manufactured by using the light reflecting substrate manufactured by the method of the present invention. The semiconductor device can be manufactured by mounting a component (semiconductor chip) on the conductive portion of the light reflecting substrate. For example, a semiconductor device mounted with a light emitting diode (LED) that emits light with low power, such as a backlight for a liquid crystal display of a mobile terminal, a computer, a television, etc., or a light source for a lighting fixture, can be mentioned. EXAMPLES

[0156] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (25°C) and atmospheric pressure (1 atm).

[0157] <Preparation Example 1> Preparation of resin sheet 1 (1) Preparation of resin composition Five parts of liquid bisphenol A type epoxy resin ("jER828EL" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 180 g / eq.), five parts of solid fluorine atom-containing epoxy resin ("YX7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 245 g / eq.), and 20 parts of biphenyl skeleton and cyclohexane skeleton-containing phenoxy resin ("YX7200B35" manufactured by Mitsubishi Chemical Corporation, weight average molecular weight 30,000, 20 μm film light transmittance (450 nm) 88%, MEK solution with solid content of 35 mass%) were dissolved in 10 parts of MEK with stirring. Titanium oxide ("PX3788" manufactured by Sakai Chemical Industry Co., Ltd., treated with a phenyl silane coupling agent ("KBM-103" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size 0.26 μm, specific surface area 13.2 m) was added thereto. 2 A resin composition (varnish) was prepared by mixing 10 parts of spherical silica ("SO-C2" manufactured by Admatechs, treated with a methacrylic silane coupling agent ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size 0.5 μm, reflectance to light with a wavelength of 500 nm of approximately 80%), 10 parts of bisphenol AF (a solution of "BIS-AF" manufactured by Central Glass Co., Ltd. adjusted to 50% non-volatile content with MEK), and 0.2 parts of a phosphorus-based curing accelerator ("TBP-DA" manufactured by Hokko Chemical Industry Co., Ltd.). The mixture was uniformly dispersed using a high-speed rotating mixer to prepare a resin composition (varnish).

[0158] (2) Preparation of resin sheet A PET film with a release layer ("PET501010" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. The resin composition prepared in (1) above was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying would be 50 μm. Thereafter, the resin composition 1 was heated at 80° C. for 4 minutes to obtain a resin sheet 1 including a resin composition layer having a thickness of 50 μm.

[0159] <Preparation Example 2> Preparation of Resin Sheet 1-RCC Resin sheet 1-RCC was produced in the same manner as in Production Example 1, except that an electrolytic copper foil ("3EC-III" manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 35 μm) was used as the support instead of a PET film with a release layer ("PET501010" manufactured by Lintec Corporation, thickness 38 μm). The resin composition was applied onto the glossy surface of the electrolytic copper foil.

[0160] <Preparation Example 3> Preparation of resin sheet 2 Resin sheet 2 was produced in the same manner as in Production Example 1, except that 5 parts of a hydrogenated liquid epoxy resin ("YX8000" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 205 g / eq.) and 5 parts of a biphenyl type epoxy resin ("YX4000H" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 195 g / eq.) were used instead of 5 parts of a liquid bisphenol A type epoxy resin ("jER828EL" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 180 g / eq.) and 5 parts of a solid fluorine atom-containing epoxy resin ("YX7760" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 245 g / eq.).

[0161] <Preparation Example 4> Preparation of resin sheet 3 Resin sheet 3 was prepared in the same manner as in Preparation Example 1, except that (1) the amount of titanium oxide ("PX3788" manufactured by Sakai Chemical Industry Co., Ltd., treated with a phenyl silane coupling agent) was changed from 10 parts to 20 parts, and (2) spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., treated with a methacrylic silane coupling agent) was not added.

[0162] <Preparation Example 5> Preparation of resin sheet 4 (1) Preparation of resin composition Three parts of biphenyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 272 g / eq.), two parts of tetrakishydroxyphenylethane type epoxy resin ("jER1031S" manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent of about 200 g / eq.), 10 parts of bisphenol A type epoxy acrylate ("ZAR-2000" manufactured by Nippon Kayaku Co., Ltd., acid value 99 mg KOH / g, non-volatile content 70%), and one part of diluent ("DPHA" manufactured by Nippon Kayaku Co., Ltd., dipentaerythritol hexaacrylate, acrylic equivalent of about 96 g / eq.) were dissolved in 6 parts of MEK and 10 parts of ethyl diglycol acetate under heating while stirring. Titanium oxide ("PX3788" manufactured by Sakai Chemical Industry Co., Ltd., treated with a phenyl silane coupling agent ("KBM-103" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size 0.26 μm, specific surface area 13.2 m 2 A resin composition was prepared by mixing 8 parts of spherical silica ("SO-C2" manufactured by Admatechs, treated with a methacrylic silane coupling agent ("KBM-503" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size 0.5 μm, reflectance to light with a wavelength of 500 nm of approximately 80%), and 0.04 parts of a photopolymerization initiator ("Irgacure819" manufactured by BASF, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) and dispersing the mixture uniformly using a high-speed rotating mixer.

[0163] (2) Preparation of resin sheet Using the resin composition prepared in (1) above, a resin sheet 4 was produced in the same manner as in Production Example 1. The resin sheet 4 includes a support and a photosensitive resin composition layer provided on the support.

[0164] The composition of the resin composition layer and the support for each of the produced resin sheets are shown in Table 1.

[0165] [Table 1]

[0166] <Example 1> (A) Fabrication of Substrate A (A1) Surface preparation for circuit boards A circuit pattern was formed by etching on both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.8 mm, Matsushita Electric Works "R5715ES") to produce an inner layer circuit board with an in-plane copper area of ​​30%. The copper circuit of the obtained inner layer circuit board was roughened with a micro-etching agent (Mec Co., Ltd. "CZ8100") and then dried at 190°C for 30 minutes.

[0167] (A2) Lamination of resin sheet The resin sheet 1 obtained in the above-mentioned preparation example was laminated on both sides of the substrate-treated inner layer circuit board using a batch-type vacuum pressure laminator ("MVLP-500" manufactured by Meiki Seisakusho Co., Ltd.) so that the resin composition layer was bonded to the inner layer circuit board. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 120°C for 30 seconds at a pressure of 0.74 MPa.

[0168] (A3) Smoothing of resin sheet The laminated resin sheet was then smoothed by heat pressing at atmospheric pressure at 100° C. and a pressure of 0.5 MPa for 60 seconds, thus obtaining a laminate with a support having a layer structure of support / resin composition layer / inner layer circuit board / resin composition layer / support.

[0169] (A4) Thermal curing of the resin composition layer The support was peeled off from the laminate with support obtained in (A3) above to obtain a laminate having a layer structure of resin composition layer / inner layer circuit board / resin composition layer.The laminate was then heated in an oven at 100°C for 30 minutes (pre-cure), and then heated in an oven at 180°C for 90 minutes (post-cure) to thermally cure the resin composition layer.As a result, a substrate A having a layer structure of cured body / inner layer circuit board / cured body was obtained.

[0170] (B) Manufacturing of Substrate B (B1) Copper foil preparation The shiny side of electrolytic copper foil (Mitsui Mining & Metals "3EC-III", thickness 35μm) was immersed in a micro-etching agent (Mec Etch Bond "CZ-8101" manufactured by Mec Co., Ltd.) to roughen the copper surface (Ra value = 1μm) and apply anti-rust treatment (CL8300). Then, it was heated in an oven at 130°C for 30 minutes. The obtained copper foil is hereinafter referred to as CZ copper foil.

[0171] (B2) Lamination of resin sheet The resin sheet 1 obtained in the above Preparation Example was laminated on one side of a CZ copper foil to prepare a resin sheet with a copper foil having a layer structure of support / resin composition layer / CZ copper foil. The lamination conditions were the same as those in (A2) above.

[0172] (B3) Thermal curing of the resin composition layer The support was peeled off from the resin sheet with copper foil prepared in (B2) above to obtain a laminate having a layer structure of resin composition layer / CZ copper foil.Then, the laminate was heated under the same curing conditions as in (A4) above to thermally cure the resin composition layer.As a result, a cured body with copper foil having a layer structure of cured body / CZ copper foil was obtained.

[0173] (B4) Fixing to the circuit board The cured product with the copper foil obtained in (B3) above was attached to both sides of a substrate-treated circuit board using an adhesive (Aron Alpha EX) so that the cured product was in contact with the circuit board. The substrate-treated circuit board was the same as that prepared in (A1) above. Next, the cured body with the copper foil was laminated to a circuit board under the same conditions as in (A2) above, thereby obtaining a substrate B having a layer structure of CZ copper foil / cured body / circuit board / cured body / CZ copper foil.

[0174] <Example 2> Substrates A and B were obtained in the same manner as in Example 1, except that when the resin composition layer was thermally cured, the support was not peeled off, but the resin composition layer was thermally cured with the support attached, and then the support was peeled off.

[0175] <Example 3> Substrates A and B were obtained in the same manner as in Example 1, except that (1) when the resin composition layer was thermally cured, the support was not peeled off, but the resin composition layer was thermally cured with the support attached, and then the support was peeled off, and (2) the temperature was raised from 25°C to 180°C at a heating rate of 2.6°C / min in an oven, and then the resin composition layer was thermally cured by heating at 180°C for 90 minutes.

[0176] <Example 4> Substrates A and B were obtained in the same manner as in Example 1, except that (1) when the resin composition layer was thermally cured, the support was not peeled off, but the resin composition layer was thermally cured with the support attached, and then the support was peeled off, and (2) the temperature was raised from 25°C to 180°C at a heating rate of 2.6°C / min in a hot press, and then the resin composition layer was thermally cured by heating at 180°C for 90 minutes.

[0177] <Example 5> Substrates A and B were obtained in the same manner as in Example 1, except that (1) resin sheet 1-RCC was used instead of resin sheet 1, and (2) when the resin composition layer was thermally cured, the support was not peeled off, but the resin composition layer was thermally cured with the support still attached, and then the support was peeled off.

[0178] <Example 6> Substrates A and B were obtained in the same manner as in Example 1, except that Resin sheet 2 was used in place of Resin sheet 1.

[0179] <Example 7> Substrates A and B were obtained in the same manner as in Example 1, except that resin sheet 3 was used in place of resin sheet 1.

[0180] <Comparative Example 1> Substrates A and B were obtained in the same manner as in Example 1, except that (1) when the resin composition layer was thermally cured, the support was not peeled off, but the resin composition layer was thermally cured with the support attached, and then the support was peeled off, and (2) the object to be heated was placed in an oven heated to 180°C, and heated at 180°C for 90 minutes to thermally cure the resin composition layer.

[0181] <Comparative Example 2> Substrates A and B were obtained in the same manner as in Example 1, except that (1) resin sheet 4 (a resin sheet including a photosensitive resin composition layer) was used instead of resin sheet 1, and (2) the resin composition layer was photocured by the following procedure. (Photocuring procedure): 100 mJ / cm2 on the photosensitive resin composition layer 2 The photosensitive resin composition layer was then exposed to ultraviolet light of 1 J / cm2 for photocuring. Thereafter, a 1% by mass aqueous solution of sodium carbonate at 30°C was used as a developer and spray-developed on the entire surface of the photosensitive resin composition layer at a spray pressure of 0.2 MPa for 2 minutes. After the spray development, 2 The photosensitive resin composition layer was then cured by heating at 190° C. for 90 minutes.

[0182] The various measurement and evaluation methods are explained below.

[0183] <Measurement of light reflectance> Substrate A produced in the examples and comparative examples was cut into a piece 50 mm wide and 50 mm long, and the reflectance (%) for light with a wavelength of 460 nm was measured using a multichannel spectrometer (Otsuka Electronics Co., Ltd., MCPD-7700) and evaluated according to the following criteria.

[0184] Light reflectance rating criteria: ◎: Reflectance is 95% or more ○: Reflectance is 90% or more and less than 95% △: Reflectance is 85% or more but less than 90% ×: Reflectance is less than 85%

[0185] <Measurement of adhesion to substrate> The substrate B obtained in the examples and comparative examples was cut into small pieces of 150 x 30 mm. A cutter was used to make a 10 mm wide and 100 mm long cut in the copper foil part of the small piece, and one end of the copper foil was peeled off and held with a gripper (TSE Autocom type testing machine "AC-50C-SL"), and the load at which 35 mm was peeled off vertically at room temperature at a speed of 50 mm / min was measured in accordance with JIS C6481 using an Instron universal testing machine, and the results were evaluated according to the following criteria.

[0186] Evaluation criteria for substrate adhesion: ◎: Adhesion strength is 0.5kgf / cm or more 〇: Adhesion strength is 0.3kgf / cm or more and less than 0.5kgf / cm ×: Adhesion strength is less than 0.3kgf / cm

[0187] The thermal curing conditions of the resin composition layer in the examples and comparative examples and the evaluation results of the produced substrates are shown in Table 2. It was confirmed that in the substrates produced in the examples, a phase rich in inorganic filler components was present in the region near the surface of the cured product of the resin composition layer (reflective sheet) on the side not in contact with the base substrate, and a phase rich in resin components was present in the region near the main surface of the reflective sheet in contact with the base substrate.

[0188] [Table 2] [Explanation of symbols]

[0189] 1 Light reflecting substrate 2. Board 3 Reflective sheet 31 Reflective sheet surface 4 light source

Claims

1. A method for producing a light reflective substrate, comprising the following steps (A) and (B) in this order: (A) A step of laminating a resin sheet including a support and a resin composition layer containing a white inorganic pigment provided on a substrate (hereinafter referred to as a "base substrate") having a conductor layer on at least a portion of the surface thereof, such that the resin composition layer is bonded to the conductor layer of the base substrate. (B) a step of thermally curing the resin composition layer under conditions that satisfy at least one of the following (i) and (ii): (i) Temperature T 1 After the heat treatment at temperature T 1 Higher temperature T 2 The mixture is subjected to a heat treatment in which the mixture is held at a temperature T 1 and temperature T 2 50°C≦T 1 < 150 ° C and 20 ° C ≦ T 2 -T 1 ≦150°C. (ii) At a temperature rise rate of 0.5 to 30° C. / min, the temperature T 2 After heating to temperature T 2 The mixture is subjected to a heat treatment in which the mixture is held at a temperature T 2 150°C≦T 2 ≦250°C.

2. Under condition (i), the temperature T 1 and temperature T 2 60°C≦T 1 ≦140° C. and 30° C.≦T 2 -T 1 The method of claim 1, wherein the temperature is ≦140° C.

3. Under condition (ii), the temperature T 2 160°C≦T 2 The method according to claim 1 or 2, wherein the temperature is ≦220° C.

4. The method according to any one of claims 1 to 3, wherein the support is peeled off between the step (A) and the step (B).

5. The method according to any one of claims 1 to 4, wherein the resin composition layer further comprises a thermosetting resin.

6. The method according to any one of claims 1 to 5, wherein the content of the white inorganic pigment is 20 to 60 mass% when the non-volatile components in the resin composition layer are taken as 100 mass%.

7. The method of claim 5 or 6, wherein the thermosetting resin comprises an epoxy resin.

8. The method according to claim 7, wherein the content of the epoxy resin is 1 to 50% by mass when the non-volatile components in the resin composition layer are taken as 100% by mass.

9. The method according to any one of claims 1 to 8, wherein the white inorganic pigment is at least one selected from the group consisting of aluminum oxide, titanium oxide, zirconium oxide, magnesium oxide, barium titanate, zinc oxide, cerium oxide, and calcium carbonate.

10. The method according to claim 1, wherein the white inorganic pigment is surface-treated with a silane coupling agent not containing a nitrogen atom.

11. A method according to any one of claims 1 to 10, wherein the resin composition layer further contains another inorganic filler different from the white inorganic pigment.

12. The method described in claim 11, wherein the mass ratio of the other inorganic fillers to the white inorganic pigment (mass of the other inorganic fillers / mass of the white inorganic pigment) is 0.1 or more and 4 or less.

13. The method described in claim 7 or 8, wherein the epoxy resin comprises one or more selected from bisphenol A type epoxy resins and bisphenol AF type epoxy resins.

14. The method according to any one of claims 1 to 13, wherein the light-reflecting substrate exhibits a reflectance of 85% or more for light having a wavelength of 460 nm.

15. The method according to any one of claims 1 to 14, wherein the adhesive strength between the cured resin composition layer in the light reflecting substrate and the conductor layer of the base substrate is 0.3 kgf / cm or more.

16. A method described in any one of claims 1 to 15, further comprising the step of (C) placing a light source on the cured body of the resin composition layer.

Citation Information

Patent Citations

  • Signal switching device

    JP1982097279A

  • Manufacture of multilayered copper clad circuit board having internal layer circuit

    JP2000349444A

  • Cover ray film

    JP2009302110A

  • Method of producing cured material of resin sheet, cured material of resin sheet, metal foil with resin, metal substrate, LED substrate and power module

    JP2012067225A

  • Curable resin composition, and flexible substrate and reflection sheet having film of curable resin composition