POLARIZING FILM WITH ADHESIVE LAYER, ADHESIVE SHEET, LAMINATED MEMBER, AND IMAGE DISPLAY DEVICE
By employing an adhesive layer with an intramolecular hydrogen abstraction type initiator, the issue of polarizing film discoloration due to iodine ion concentration is mitigated, ensuring the film's stability and appearance in humid environments.
Patent Information
- Application Number
- JP2020163236
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-01
- Filing Date
- 2020-09-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Polarizing films in image display devices, particularly those containing polyvinyl alcohol (PVA) layers, tend to discolor due to an increase in iodine ion concentration when exposed to high humidity, especially when bonded with adhesive layers containing intermolecular hydrogen abstraction type initiators.
The use of an adhesive layer formed from a composition containing an intramolecular hydrogen abstraction type initiator, such as methyl phenylglyoxylate, which minimizes the reaction with the PVA layer, thereby suppressing iodine ion concentration and preventing discoloration.
The adhesive layer effectively prevents discoloration of the polarizing film even under high humidity conditions, maintaining the film's integrity and appearance.
Smart Images

Figure 0007563081000003 
Figure 0007563081000004 
Figure 0007563081000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive sheet that can be suitably used as a component of image display devices such as personal computers, mobile terminals (PDAs), game consoles, televisions (TVs), car navigation systems, touch panels, pen tablets, and the like. [Background technology]
[0002] In recent years, in order to improve the visibility of image display devices, the gap between an image display panel such as a liquid crystal display (LCD), a plasma display panel (PDP), or an electroluminescence display (ELD) and a protective panel or touch panel member placed on the front side (viewing side) of the image display panel has been filled with an adhesive to suppress reflection of incident light and outgoing light from a displayed image at the air layer interface.
[0003] As a method for filling such gaps between components of an image display device with an adhesive, a method for filling the gaps between components of an image display device with an adhesive sheet is known. For example, Patent Document 1 discloses an adhesive sheet obtained by curing with ultraviolet light.
[0004] The above-mentioned photocuring with ultraviolet light or the like is easier to control than heat curing, and therefore has excellent handling properties in the pressure-sensitive adhesive sheet production process.
[0005] Patent Document 2 discloses a method in which an adhesive sheet that has been primarily crosslinked by ultraviolet light is attached to a component of an image display device, and then the adhesive sheet is irradiated with ultraviolet light through the component of the image display device for secondary curing.
[0006] Furthermore, Patent Document 3 discloses a photocurable composition containing a (meth)acrylic copolymer containing a macromonomer as a constituent unit, a crosslinking agent, and a crosslinking initiator, and the half-width X1 (nm) of a one-dimensional scattering profile in small-angle X-ray scattering measurement is -1) A photocurable composition is disclosed, which is characterized in that 0.05 < X1 < 0.30. According to such a composition, it can exhibit self-adhesiveness while maintaining a sheet shape at room temperature. When heated in an uncured state, it softens or flows, for example, by heating to a temperature above the glass transition temperature of the macromonomer, it can soften or flow and fill every corner following the unevenness of the bonding surface. Furthermore, it is also disclosed that by photocuring, excellent cohesive force can be exerted.
[0007] In addition, Patent Document 4 discloses an adhesive composition containing a hydroxyl group-containing acrylic resin, an ethylenically unsaturated compound having one ethylenically unsaturated group, a crosslinking agent, and a photopolymerization initiator. The adhesive composition is characterized in that the photopolymerization initiator contains an intramolecular hydrogen abstraction type photopolymerization initiator having a specific structural site. According to such a composition, excellent step followability and blister resistance can be achieved in a well-balanced manner. Furthermore, it is disclosed that an adhesive sheet having high-level reliability, excellent in adhesive physical properties (adhesive force, holding force), wet heat resistance, and optical properties (transparency) can be obtained.
Prior Art Documents
Patent Documents
[0008]
Patent Document 1
Patent Document 2
Patent Document 3
Patent Document 4
Summary of the Invention
Problems to be Solved by the Invention
[0009] By the way, in recent years, with the progress of thinning of polarizing films accompanying the weight reduction and thinning of image display devices such as liquid crystal display devices, there may occur a polarizing film that causes discoloration. The inventors have investigated the cause of such discoloration and found that the polarizing film discolors when the concentration of specific iodine ions in the internal polyvinyl alcohol (PVA) layer (polarizer) becomes high.
[0010] The problem to be solved by the present invention is to provide a polarizing film and a pressure-sensitive adhesive sheet with a pressure-sensitive adhesive layer that do not discolor the polarizing film, more specifically, to provide a polarizing film and a pressure-sensitive adhesive sheet with a pressure-sensitive adhesive layer that do not discolor the polarizing film even when exposed to high humidity after the pressure-sensitive adhesive layer and the polarizing film are bonded together. [Means for solving the problem]
[0011] The polarizing film with an adhesive layer provided by the present invention is a polarizing film with an adhesive layer, which has a polarizing film and an adhesive layer on at least one surface of the polarizing film, wherein the adhesive layer is formed from an adhesive composition containing an intramolecular hydrogen abstraction initiator (A), and the polarizing film has an absorbance of 3.5 or more at a wavelength of 300 to 400 nm, measured after adhering an adhesive layer formed from an adhesive composition containing an intermolecular hydrogen abstraction initiator to the polarizing film and leaving the film at 25°C and 90% RH for 2 days. Effect of the Invention
[0012] In the polarized film with an adhesive layer according to one embodiment of the present invention, the adhesive layer has discoloration resistance to the polarized film, particularly the PVA layer that constitutes the polarized film, and therefore discoloration can be suppressed even when a polarized film that is sensitive to heat, humidity, materials, etc., and in particular that reacts with a specific adhesive component to increase the concentration of specific iodine ions, is used.
[0013] Furthermore, the pressure-sensitive adhesive sheet according to another embodiment of the present invention can have excellent anti-foaming reliability, even when applied to a polarized film that reacts with a specific pressure-sensitive adhesive component to increase a specific iodine ion concentration, while suppressing discoloration of the polarized film due to an increase in the specific iodine ion concentration caused by the reaction of the pressure-sensitive adhesive component. [Brief description of the drawings]
[0014] [Figure 1] 1 shows a cross-sectional view of a sample used in a test method for evaluating yellowing resistance reliability performed in Examples. [Diagram 2] FIG. 2 is a diagram for explaining a method for evaluating anti-foaming reliability performed in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] An embodiment of the present invention will be described in detail below, although the present invention is not limited to the following embodiment.
[0016] <Polarizing film with adhesive layer> The pressure-sensitive adhesive layer-attached polarizing film of the present invention (hereinafter also referred to as "the present polarizing film") comprises a polarizing film and a pressure-sensitive adhesive layer on at least one surface of the polarizing film. The pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition containing an intramolecular hydrogen abstraction initiator (A). The adhesive layer formed from such an adhesive composition can suppress discoloration because the polarizer of the polarizing film, i.e., the PVA layer, does not react with the intramolecular hydrogen abstraction initiator (A) to increase the iodine ion concentration.
[0017] [Polarizing film] A "polarizing film" is a film that has the function of converting natural light into linearly polarized light. Examples of such films include those in which iodine or a dichroic dye is adsorbed and oriented on a PVA-based resin, polyvinyl acetate resin, ethylene / vinyl acetate (EVA) resin, polyamide resin, polyester-based resin, or the like, and a typical example is a PVA-based resin film dyed with iodine.
[0018] The discoloration mechanism of polarizing film is caused by the concentration of iodine ions (I5 -More specifically, when a pressure-sensitive adhesive component containing an intermolecular hydrogen abstraction initiator is used, the initiator migrates to the polarizer and acts on the iodine complex in the PVA layer, increasing the specific iodine ion concentration (I5 - ) increases, which increases the absorbance of the PVA layer at wavelengths of 300 to 400 nm, causing discoloration of the polarizing film. Therefore, the present invention can be suitably used for polarizing films that undergo yellowing due to pressure-sensitive adhesives containing intermolecular hydrogen abstraction initiators. From this viewpoint, the polarizing film used in the present polarizing film is prepared by adhering a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an intermolecular hydrogen abstraction initiator as described in the "Examples" section below, more specifically, by adhering a pressure-sensitive adhesive sheet formed from the pressure-sensitive adhesive composition of Comparative Example 1 described below, and leaving the film to stand at 25°C and 90% RH for two days, and then measuring the absorbance of the polarizer at a wavelength of 300 to 400 nm using an ultraviolet-visible-near-infrared spectrophotometer of 3.5 or more, and preferably 4 or more. Incidentally, the absorbance of the polarizer at wavelengths of 300 to 400 nm measured under the above conditions being 3.5 or more indicates that the polarizing film has yellowed as shown in Comparative Example 1 described below.
[0019] In addition, since discoloration of a polarizing film caused by using an adhesive containing an intermolecular hydrogen abstraction initiator is particularly noticeable at the edges, the edges of the polarizing film used in the present polarizing film are, as described above, attached with an adhesive layer formed from an adhesive composition containing an intermolecular hydrogen abstraction initiator, more specifically, with an adhesive sheet formed from the adhesive composition of Comparative Example 1 described below, and allowed to stand for two days at 25°C and 90% RH, and the absorbance of the polarizer at a wavelength of 300 to 400 nm, as measured using an ultraviolet-visible-near infrared spectrophotometer, is 3.5 or more, and preferably 4 or more. The term "edge" refers to an edge in the width direction of the polarizing film, and indicates a position at 5% or 95% of the total width of the polarizing film, and the term "center" refers to a position at 50% of the total width of the polarizing film.
[0020] [Intramolecular Hydrogen Abstraction Initiator (A)] Examples of the intramolecular hydrogen abstraction initiator (A) include benzoylformate-based photopolymerization initiators such as methyl phenylglyoxylate, and oxyphenyl-based photopolymerization initiators such as methyl benzoylformate, a mixture of oxyphenylacetic acid 2-[2-oxo-2-phenylacetoxyethoxy]ethyl ester and oxyphenylacetic acid 2-(2-hydroxy-ethoxy)ethyl ester, and among these, benzoylformate-based photopolymerization initiators are preferred. These may be used alone or in combination of two or more kinds.
[0021] Commercially available products of the intramolecular hydrogen abstraction initiator (A) include, for example, "Omnirad MBF" and "Omnirad 754" manufactured by IGM RESINS BV.
[0022] Although the mechanism of action is not necessarily clear, it is presumed that the intramolecular hydrogen abstraction initiator (A) has a weaker ability to retain its active state than the intermolecular hydrogen abstraction initiator, and therefore cannot migrate to the polarizer, thereby suppressing discoloration. In other words, in the present invention, it is preferable to use the intramolecular hydrogen abstraction initiator (A) without using an intermolecular hydrogen abstraction initiator.
[0023] Among the above, methyl phenylglyoxylate represented by the following structural formula is particularly preferred from the viewpoint of yellowing resistance reliability for a polarizing film containing moisture. In addition, since methyl phenylglyoxylate is in a liquid state at room temperature (23°C), it has excellent dispersibility when mixed into a pressure-sensitive adhesive composition, and can be mixed uniformly. It also has other excellent advantages, such as being easily made into a masterbatch.
[0024] For example, JP 2013-40256 A describes that methyl phenylglyoxylate can be used as an example of a photopolymerization initiator. However, JP2013-40256A only describes that the photopolymerization initiator is used solely for curing by irradiation with radiation, and makes no mention at all of the fact that discoloration of the polarizing film can be suppressed by selecting an intramolecular hydrogen abstraction initiator (A) as in the present invention. In this respect, the present invention is a more useful invention than JP 2013-40256 A.
[0025] [ka]
[0026] The amount of the intramolecular hydrogen abstraction initiator (A) to be added is not particularly limited, and is typically adjusted to 0.1 to 10 parts by mass, particularly 0.2 to 5 parts by mass, and particularly 0.5 to 3 parts by mass, per 100 parts by mass of the adhesive component (B) described below (base polymer (b1) when used, total amount of the mixture (b2) of monomer components constituting the base polymer when used instead of the base polymer, total amount of unreacted monomer and the partial polymer (b3) of the mixture when used). However, it may exceed this range in balance with other factors.
[0027] <Adhesive layer> The pressure-sensitive adhesive layer in the present invention (hereinafter also referred to as "the pressure-sensitive adhesive layer" for short) is formed from a pressure-sensitive adhesive composition containing the intramolecular hydrogen abstraction initiator (A). The pressure-sensitive adhesive composition preferably contains at least one pressure-sensitive adhesive component (B) selected from the group consisting of a base polymer (b1), a mixture of monomer components constituting the base polymer (b2), and a partial polymer (b3) thereof. This pressure-sensitive adhesive layer may be a single layer or a multilayer. In the case of a multilayer, it is preferable that the surface layer is a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition.
[0028] <Adhesive composition> The pressure-sensitive adhesive composition (hereinafter also referred to as "the composition") contains the intramolecular hydrogen abstraction initiator (A). The composition preferably contains at least one pressure-sensitive adhesive component (B) selected from the group consisting of a base polymer (b1), a mixture of monomer components constituting the base polymer (b2), and a partial polymer (b3) thereof.
[0029] The term "base polymer" refers to the polymer component that is contained in the largest proportion in the pressure-sensitive adhesive composition, and more preferably refers to a polymer component that is the main component in the composition or a polymer component that is contained in the composition at more than 50 mass %.
[0030] The content of the base polymer (b1) is preferably 60 mass % or more, more preferably 80 mass % or more, and most preferably 90 mass % or more, based on the total mass of the pressure-sensitive adhesive composition. The upper limit is preferably 99.9% by mass or less.
[0031] In addition, as the pressure-sensitive adhesive component (B), at least one of a mixture (b2) of monomer components for forming the base polymer (b1) and a partial polymer (b3) of the mixture may be used in place of the base polymer (b1).
[0032] The partially polymerized product (b3) refers to a resultant product obtained by polymerizing a portion of the mixture of the monomer components, and more specifically, includes a polymer or oligomer obtained by partially polymerizing the monomer components and unreacted monomer components.
[0033] In addition, from the viewpoint of increasing the reliability of lamination in the present polarizing film, the present composition is preferably a photocurable pressure-sensitive adhesive composition that is cured by irradiation with ultraviolet light.
[0034] Examples of the base polymer (b1) include (meth)acrylic acid ester (co)polymers, rubber polymers, silicone polymers, polyester polymers, urethane polymers, polyamide polymers, epoxy polymers, and fluorine polymers. These may be used alone or in combination of two or more. Among these, (meth)acrylic acid ester (co)polymers are preferred.
[0035] Examples of the (meth)acrylic acid ester (co)polymer include a homopolymer of an alkyl (meth)acrylate, as well as a copolymer obtained by copolymerizing the homopolymer with a monomer component having copolymerizability. Further, a more preferred example of the (meth)acrylic acid ester (co)polymer is a copolymer containing, as a monomer component, an alkyl (meth)acrylate and at least one monomer selected from the group consisting of a carboxyl group-containing monomer, a hydroxyl group-containing monomer, an amino group-containing monomer, an epoxy group-containing monomer, an amide group-containing monomer, and other vinyl monomers that are copolymerizable therewith. Additionally, the term "(meth)acrylate" encompasses both acrylate and methacrylate. In the present invention, the term "(co)polymer" encompasses polymers and copolymers, and the term "(meth)acrylic" encompasses acrylic and methacrylic.
[0036] [Details of adhesive component (B)] More specifically, the above (b1) to (b3) include a copolymer (b1) composed of at least one monomer component selected from the group consisting of a straight-chain or branched alkyl (meth)acrylate having 4 to 18 carbon atoms in the side chain (hereinafter also referred to as "copolymerizable monomer a") and a carboxyl group-containing monomer copolymerizable therewith (hereinafter also referred to as "copolymerizable monomer b"), a vinyl monomer (hereinafter also referred to as "copolymerizable monomer c"), a (meth)acrylate having 1 to 3 carbon atoms in the side chain (hereinafter also referred to as "copolymerizable monomer d"), and a hydroxyl group-containing monomer (hereinafter also referred to as "copolymerizable monomer e"); a mixture (b2) of these monomer components, or a partial polymer (b3) thereof.
[0037] Furthermore, among the (meth)acrylic acid ester (co)polymers, mixtures of monomer components constituting the (meth)acrylic acid ester (co)polymers, or partial polymers thereof, suitable examples include (α) a copolymer composed of monomer components containing copolymerizable monomer a, and copolymerizable monomer b and / or copolymerizable monomer c, a mixture of these monomer components, or a partial polymer thereof, and (β) a copolymer composed of monomer components containing copolymerizable monomer a, copolymerizable monomer b and / or copolymerizable monomer c, and copolymerizable monomer d and / or copolymerizable monomer e, a mixture of these monomer components, or a partial polymer thereof. Of these, (α) is preferred, and a copolymer composed of monomer components including copolymerizable monomer a, copolymerizable monomer b and copolymerizable monomer c, a mixture of these monomer components or a partial polymer thereof is particularly preferred.
[0038] Examples of the linear or branched alkyl(meth)acrylate having 4 to 18 carbon atoms in the side chain (copolymerizable monomer a) include n-butyl(meth)acrylate, isobutyl(meth)acrylate, sec-butyl(meth)acrylate, t-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, neopentyl(meth)acrylate, hexyl(meth)acrylate, cyclohexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, nonyl(meth)acrylate, isononyl(meth)acrylate, acrylate, t-butylcyclohexyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, isobornyl (meth)acrylate, 3,5,5-trimethylcyclohexane (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0039] The copolymerizable monomer a is contained in the total monomer components of the copolymer in an amount of preferably 30% by mass or more and 90% by mass or less, more preferably 35% by mass or more and 88% by mass or less, even more preferably 40% by mass or more and 85% by mass or less, and even more preferably 55% by mass or more and 85% by mass or less.
[0040] Examples of the carboxy group-containing monomer (copolymerizable monomer b) include (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, and itaconic acid, among which (meth)acrylic acid is preferred. These may be used alone or in combination of two or more. In addition, "(meth)acryloyl" is meant to encompass acryloyl and methacryloyl.
[0041] The copolymerizable monomer b is contained in the total monomer components of the copolymer in an amount of 1.2% by mass or more and 15% by mass or less, and from the viewpoint of obtaining excellent adhesive properties, it is preferable that the content be in the range of 1.5% by mass or more and 10% by mass or less, and even more preferable that the content be in the range of 2% by mass or more and 8% by mass or less.
[0042] The vinyl monomer (copolymerizable monomer c) may be a compound having a vinyl group in the molecule. Examples of such compounds include (meth)acrylic acid alkyl esters having an alkyl group with 1 to 12 carbon atoms, functional monomers having functional groups such as a hydroxyl group, an amide group, and an alkoxyl alkyl group in the molecule, polyalkylene glycol di(meth)acrylates, vinyl acetate, vinyl propionate, vinyl laurate, and other vinyl ester monomers, as well as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes, and aromatic vinyl monomers, among which vinyl ester monomers are preferred. These may be used alone or in combination of two or more.
[0043] The copolymerizable monomer c is preferably contained in the total monomer components of the copolymer in an amount of 1.2% by mass or more and 40% by mass or less, and more preferably 1.5% by mass or more and 35% by mass or less, and even more preferably 2% by mass or more and 30% by mass or less, from the viewpoint of obtaining excellent adhesive properties.
[0044] Examples of the (meth)acrylate having 1 to 3 carbon atoms in the side chain (copolymerizable monomer d) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0045] The copolymerizable monomer d is preferably contained in the total monomer components of the copolymer in an amount ranging from 0% by mass to 70% by mass, more preferably from 3% by mass to 65% by mass, and even more preferably from 5% by mass to 60% by mass.
[0046] Examples of the hydroxyl group-containing monomer (copolymerizable monomer e) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0047] The copolymerizable monomer e is preferably contained in the total monomer components of the copolymer in an amount ranging from 0% by mass to 30% by mass, more preferably from 0% by mass to 25% by mass, and even more preferably from 0% by mass to 20% by mass.
[0048] In addition to the above, acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride, epoxy group-containing monomers such as glycidyl (meth)acrylate, α-ethyl glycidyl acrylate, and 3,4-epoxybutyl (meth)acrylate, amino group-containing (meth)acrylic acid ester monomers such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate, amide group-containing monomers such as (meth)acrylamide, Nt-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, diacetone (meth)acrylamide, maleic acid amide, and maleimide, and heterocyclic basic monomers such as vinyl pyrrolidone, vinyl pyridine, and vinyl carbazole can also be used as necessary.
[0049] The most typical specific examples of the (meth)acrylic acid ester (co)polymer, the mixture of monomer components constituting the (meth)acrylic acid ester (co)polymer, or the partial polymer thereof are, for example, a copolymerizable monomer a such as 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, isostearyl (meth)acrylate, butyl (meth)acrylate, ethyl (meth)acrylate, or methyl (meth)acrylate, and (meth)acrylic acid, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxypropylhexahydrophthalic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxypropylphthalic acid, 2-(meth)acryloyloxyethylmale ... Examples of the copolymerizable monomer include (meth)acrylic acid ester copolymers obtained by copolymerizing a copolymerizable monomer b such as 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, etc., with a copolymerizable monomer c having an organic functional group or the like such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, glycerol (meth)acrylate, monomethyl maleate, monomethyl itaconate, vinyl acetate, glycidyl (meth)acrylate, (meth)acrylamide, (meth)acrylonitrile, fluorinated (meth)acrylate, silicone (meth)acrylate, etc., and a mixture of these monomer components or a partial polymer thereof.
[0050] The (meth)acrylic acid ester (co)polymer can be obtained by polymerizing the above-mentioned copolymerizable monomers according to a conventionally known method such as solution radical polymerization, suspension polymerization, bulk polymerization, or emulsion polymerization. In the present invention, in place of the (meth)acrylic acid ester (co)polymer, at least one of the mixture of the copolymerizable monomer components and a partial polymer of the mixture may be used.
[0051] The mass average molecular weight of the (meth)acrylic acid ester (co)polymer is preferably from 50,000 to 1,500,000, more preferably from 70,000 to 1,300,000, and even more preferably from 100,000 to 1,200,000.
[0052] Here, the mass average molecular weight is measured by the following method. A measurement sample is prepared by dissolving 4 mg of the (meth)acrylic acid ester (co)polymer (A) in 12 mL of tetrahydrofuran (THF). A molecular weight distribution curve is measured under the following conditions using a gel permeation chromatography (GPC) analyzer (apparatus name: Tosoh Corporation HLC-8320GPC) to determine the mass average molecular weight (Mm). Guard column: TSKguardcolumnHXL Separation column: TSKgelGMHXL (4 columns) ·Temperature: 40℃ ·Injection volume: 100μL Polystyrene equivalent Solvent: THF ·Flow rate: 1.0mL / min
[0053] When a pressure-sensitive adhesive composition with high cohesive strength is to be obtained, the mass average molecular weight of the (meth)acrylic acid ester (co)polymer is preferably 700,000 or more and 1,500,000 or less, particularly 800,000 or more and 1,300,000 or less, from the viewpoint that the larger the molecular weight, the greater the cohesive strength obtained due to entanglement of molecular chains. On the other hand, when it is desired to obtain a pressure-sensitive adhesive composition having high fluidity and stress relaxation properties, the mass average molecular weight of the (meth)acrylic acid ester (co)polymer is preferably 100,000 or more and 700,000 or less, particularly 150,000 or more and 600,000 or less. Furthermore, when no solvent is used in forming an adhesive sheet or the like, it is difficult to use a polymer with a large molecular weight, and therefore the mass average molecular weight of the (meth)acrylic acid ester (co)polymer is preferably from 100,000 to 700,000, particularly from 150,000 to 600,000, and of these, particularly from 200,000 to 500,000.
[0054] [Compound (C)] In order to impart excellent resistance to foaming and yellowing to polarized films, it is preferable to use a compound having a radical polymerizable functional group having a carbon-carbon double bond and a radical generating group in the molecule [compound (C)] in combination with the intramolecular hydrogen abstraction initiator (A) in the present composition.
[0055] Here, examples of the "radically polymerizable functional group having a carbon-carbon double bond" include functional groups having an unsaturated double bond, such as a (meth)acryloyl group and a vinyl group. On the other hand, in the compound (C), the "radical generating group" means a group that generates a radical that initiates a polymerization reaction when excited by active energy rays such as ultraviolet rays.
[0056] As described above, since the compound (C) has a radically polymerizable functional group having a carbon-carbon double bond in the molecule, it polymerizes by itself when irradiated with ultraviolet light, and therefore tends not to migrate to the polarizing film, thereby reducing the risk of discoloring the polarizing film.
[0057] The "radical generating group" is preferably a group having a structure that is excited by irradiation with active energy rays and generates a radical by causing a hydrogen abstraction reaction. Since the compound (C) has a radical generating group, for example, the compounds (C) can be polymerized with each other or a crosslinked structure can be formed between molecules of the base polymer (b1), thereby improving the cohesive strength of the adhesive resin composition.
[0058] The compound (C) may be any compound as long as it has a radically polymerizable functional group having a carbon-carbon double bond in the molecule and also has a radical generating group, i.e., a functional group that generates radicals when irradiated with active energy rays. In particular, those having a structure capable of abstracting hydrogen from molecules of the base polymer (b1) and the like to generate radicals are preferred.
[0059] Examples of the compound (C) include compounds having a (meth)acryloyl group and at least one structure selected from the group consisting of a benzophenone structure, a benzyl structure, an o-benzoylbenzoic acid ester structure, a thioxanthone structure, a 3-ketocoumarin structure, a 2-ethylanthraquinone structure, and a camphorquinone structure.
[0060] Among the above, compound (C) is preferably a compound having a (meth)acryloyl group and a benzophenone structure. More specifically, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and mixtures thereof can be mentioned. Among them, 4-methacryloyloxybenzophenone is preferred.
[0061] The lower limit of the content of the compound (C) is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and most preferably 0.5 parts by mass or more, per 100 parts by mass of the adhesive component (B) (the base polymer when a base polymer (b1) is used, the total amount of the mixture when a mixture (b2) of monomer components constituting the base polymer is used instead of the base polymer, and the total amount of unreacted monomers and the partial polymer (b3) of the mixture when a partial polymer (b3) of the mixture is used).
[0062] The upper limit is preferably 5 parts by mass or less, more preferably 2 parts by mass or less, and most preferably 1 part by mass or less, per 100 parts by mass of the pressure-sensitive adhesive component (B).
[0063] The blending ratio of the intramolecular hydrogen abstraction initiator (A) to the compound (C) [intramolecular hydrogen abstraction initiator (A) / compound (C)] is usually 99 / 1 to 1 / 99, preferably 90 / 10 to 40 / 60, and more preferably 85 / 15 to 60 / 40, by mass.
[0064] [Crosslinking agents other than compound (C)] The composition may contain a crosslinking agent other than the compound (C) as required. For example, when crosslinking the (meth)acrylic acid ester (co)polymer as the pressure-sensitive adhesive component (B), a method of adding a crosslinking agent capable of chemically bonding with reactive groups such as hydroxyl groups and carboxyl groups introduced into the (meth)acrylic acid ester (co)polymer and reacting by heating or curing, or a method of adding a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups as a crosslinking agent and a reaction initiator such as a photopolymerization initiator and crosslinking by ultraviolet irradiation or the like can be mentioned. Among these, a crosslinking method using light irradiation such as ultraviolet light is preferred, from the viewpoint of not consuming polar functional groups such as carboxyl groups in the present composition through reaction and maintaining the high cohesive strength and adhesive properties derived from the polar components.
[0065] Examples of the crosslinking agent include crosslinking agents having at least one crosslinkable functional group selected from (meth)acryloyl group, epoxy group, isocyanate group, carboxy group, hydroxy group, carbodiimide group, oxazoline group, aziridine group, vinyl group, amino group, imino group, and amide group, and one or more of them may be used in combination. Among them, polyfunctional (meth)acrylates having two or more (meth)acryloyl groups are preferred. The crosslinkable functional group may be protected with a protecting group which can be removed.
[0066] From the viewpoint of balancing the flexibility and cohesive strength of the composition, the content of the crosslinking agent is preferably from 0.01 to 10 parts by mass per 100 parts by mass of the adhesive component (B) (the base polymer when a base polymer (b1) is used, the total amount of the mixture when a mixture (b2) of monomer components constituting the base polymer is used instead of the base polymer, and the total amount of unreacted monomers and the partial polymer (b3) of the mixture when a partial polymer (b3) of the mixture is used), and more preferably from 0.05 to 8 parts by mass, and even more preferably from 0.1 to 5 parts by mass.
[0067] [Antioxidants] In addition to the above, the composition may contain an antioxidant as necessary. Examples of the antioxidant include 2,2'-methylenebis(4-methyl-6-t-butylphenol), hexamethylene glycol-bis(3,5-di-t-butyl-4-hydroxyhydrocinnamate), tetrakis[methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate)]methane, triethylene glycol-bis-3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate, 1,3,5-trimethylphenyl ... Examples of antioxidants include hindered phenol-based antioxidants such as n-octadecyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenol)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), and 4,4'-butylidene-bis-(6-t-butyl-3-methyl-phenol), as well as various types of antioxidants such as sulfur-based and amine-based antioxidants.
[0068] [Other compounding agents] Furthermore, the composition may appropriately contain known components that are blended in normal pressure-sensitive adhesive compositions, such as light stabilizers, ultraviolet absorbers, metal deactivators, rust inhibitors, anti-aging agents, moisture absorbers, foaming agents, defoamers, inorganic particles, viscosity adjusters, tackifier resins, photosensitizers, fluorescent agents, and reaction catalysts (tertiary amine compounds, quaternary ammonium compounds, tin laurate compounds, and the like).
[0069] (Preparation of Pressure-Sensitive Adhesive Composition) The composition can be obtained, for example, by mixing predetermined amounts of the intramolecular hydrogen abstraction initiator (A), the pressure-sensitive adhesive component (B), and, if necessary, other components. In addition, the present composition may use, as the pressure-sensitive adhesive component (B), at least one of a mixture (b2) of monomer components constituting the base polymer and a partial polymer (b3) of the mixture, instead of the base polymer (b1). There is no particular limitation on the mixing method, and there is no particular limitation on the mixing order of each component. A heat treatment step may be included in the production of the present composition. In this case, it is desirable to previously mix the components of the present composition and then carry out the heat treatment. In the above mixing, various mixed components may be concentrated and used in the form of a master batch.
[0070] As described above, the mixing method is not particularly limited, and for example, a universal kneader, a planetary mixer, a Banbury mixer, a kneader, a gate mixer, a pressure kneader, a three-roll mill, a two-roll mill, etc. can be used. When mixing the components of the present composition, a solvent may be used as necessary. The present composition can also be used as a solventless system that does not contain a solvent. By using the composition as a solventless system, the solvent does not remain, and the heat resistance and light resistance can be improved.
[0071] <Adhesive sheet> The pressure-sensitive adhesive sheet of the present invention (hereinafter also referred to as "the pressure-sensitive adhesive sheet") has a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition containing an intramolecular hydrogen abstraction initiator (A) and a compound (C) having, in its molecule, a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group.
[0072] In addition, the pressure-sensitive adhesive composition preferably contains at least one pressure-sensitive adhesive component (B) selected from the group consisting of a base polymer (b1), a mixture of monomer components constituting the base polymer (b2), and a partial polymer (b3) thereof.
[0073] The specific details of the intramolecular hydrogen abstraction initiator (A), the pressure-sensitive adhesive component (B) and the compound (C) are as described above, and the preferred embodiments are also the same.
[0074] In particular, the pressure-sensitive adhesive layer is preferably photocurable. More specifically, the pressure-sensitive adhesive layer is preferably formed from a photocurable pressure-sensitive adhesive composition that is cured by irradiation with ultraviolet light.
[0075] In particular, the pressure-sensitive adhesive composition preferably contains an intramolecular hydrogen abstraction initiator (A), a pressure-sensitive adhesive component (B), and a compound (C) having, in its molecule, a radical polymerizable functional group having a carbon-carbon double bond and a radical generating group. Furthermore, in the above-mentioned configuration, it is more preferable to use at least one of a benzoylmethylformate photopolymerization initiator and an oxyphenyl photopolymerization initiator as the intramolecular hydrogen abstraction initiator (A).
[0076] <Form of adhesive sheet> The present adhesive sheet is usually used as an adhesive sheet with a release film, in which the present composition is formed into a single-layer or multi-layer sheet on a release film, but the present composition may also be directly applied to an adherend and formed into a sheet for use. Examples of the material of such a release film include polyester resin, polyolefin resin, polycarbonate resin, polystyrene resin, acrylic resin, triacetyl cellulose resin, fluororesin, etc. Among these, polyester resin and polyolefin resin are particularly preferred.
[0077] The pressure-sensitive adhesive sheet may be in the form of a roll or sheets. Among these, adhesive sheets processed into various shapes are particularly preferred, and an adhesive sheet with release film is preferred in which a release film is laminated to sandwich the adhesive sheet, the outer edge of the release film forming the outer layer protruding outward beyond the outer edge of the adhesive layer of the adhesive sheet, and the adhesive sheet is cut into sheets (for example, the adhesive layer and release film have a rectangular planar shape such as a rectangle). Moreover, a pressure-sensitive adhesive sheet with a release film having such a shape is particularly preferably used as a repair part. Adhesive sheets used as repair parts are required to be applicable to image display devices equipped with various types of polarizing films, and the present adhesive sheet is highly useful because it can suppress discoloration of the polarizing film regardless of the type of polarizing film used in the image display device.
[0078] (Multi-layer structure) When the present pressure-sensitive adhesive sheet is made multilayered, i.e., when it has a laminated structure with an intermediate layer and an outermost layer, it is preferable that the outermost layer combines unevenness-following ability and foaming resistance reliability, as in the case of the above-mentioned single layer, and therefore it is preferable that the outermost layer is formed using the above-mentioned pressure-sensitive adhesive composition. On the other hand, since the intermediate layer does not contribute to adhesion to the components of the image display device, it is preferable that the intermediate layer has light transmittance to an extent that does not impair transparency and does not inhibit the curing reaction of the outermost layer, and has properties that enhance cuttability and handleability.
[0079] The type of adhesive component (e.g., base polymer) forming the intermediate layer is not particularly limited as long as it is a transparent resin, but it is preferable to use the same adhesive component (B) as described above. In this case, from the viewpoint of ensuring transparency and ease of preparation, it is preferable to use the same resin as the adhesive component (B) (e.g., base polymer (b1)) of the outermost layer.
[0080] The intermediate layer may be formed so as to be cured by ultraviolet crosslinking, or may be formed so as to be cured by heat. Also, the intermediate layer may be formed so as not to be post-cured. However, in consideration of adhesion to the outermost layer, it is preferable to form the intermediate layer so as to be post-cured, and it is particularly preferable to form the intermediate layer so as to be crosslinked by ultraviolet light. In this case, since the light transmittance decreases when the content of the photopolymerization initiator increases, it is preferable to contain the photopolymerization initiator in a lower content in the intermediate layer than in the outer layer.
[0081] In addition, the pressure-sensitive adhesive sheet is preferably cured primarily by crosslinking the pressure-sensitive adhesive layer with ultraviolet light so that it has latent ultraviolet reactivity, in other words, so that it retains ultraviolet reactivity. In the case of the primary curing, the pressure-sensitive adhesive layer may be crosslinked with ultraviolet light by irradiating the layer with ultraviolet light through the release film. In this case, the degree of ultraviolet crosslinking can be adjusted by controlling the amount of ultraviolet light irradiation, but as described above, the degree of ultraviolet crosslinking can also be adjusted by irradiating the layer with ultraviolet light through the release film to block part of the ultraviolet light.
[0082] The present pressure-sensitive adhesive sheet is preferably an optically transparent pressure-sensitive adhesive sheet. Here, the term "optically transparent" means that the total light transmittance is 80% or more, preferably 85% or more, and more preferably 90% or more.
[0083] The thickness of the pressure-sensitive adhesive sheet is preferably from 10 μm to 500 μm in terms of practicality, more preferably from 15 μm to 400 μm, and even more preferably from 20 μm to 350 μm.
[0084] <Laminated materials> The laminated member of the present invention (hereinafter also referred to as "the member" for short) has a configuration in which the pressure-sensitive adhesive sheet is bonded to a component of an image display device. Here, examples of the image display device constituent members include a touch panel, an image display panel, a surface protection panel, and a polarizing film, and the image display device may be a laminate of any one of these or a combination of two or more of these. The component of an image display device to which the pressure-sensitive adhesive sheet of the present invention is adhered is preferably a polarizing film, that is, it is preferable to form a laminated member having a configuration in which the pressure-sensitive adhesive sheet of the present invention is adhered to a polarizing film. The PVA layer that constitutes the polarizing film has become thinner in recent years, and as a result, the iodine density has increased, making it more susceptible to reaction with moisture and adhesives, which makes it more susceptible to discoloration. This adhesive sheet can suppress discoloration of the PVA layer even when exposed to high humidity after being laminated with a polarizing film to form a laminated member.
[0085] <Image display device> The image display device of the present invention (hereinafter also referred to as "the device") has the present member or the present polarizing film. More specifically, examples of the device include a surface protection panel / the present pressure-sensitive adhesive sheet / touch panel, a touch panel / the present pressure-sensitive adhesive sheet, the present polarizing film / image display panel, etc.
[0086] <Methods of manufacturing pressure-sensitive adhesive sheets, laminated members, and image display devices> The following describes a method for producing the pressure-sensitive adhesive sheet, laminated member, and image display device of the present invention, but is not limited to this method. Typically, the sheet, laminated member, and image display device are preferably obtained by the following steps (1) and (2), but the first curing step (1) may be omitted.
[0087] [Step (1)] In step (1), for example, the composition is heated and melted (hot melt), and then coated on a transparent release resin sheet to form a single-layer or multi-layer sheet to form a sheet-like pressure-sensitive adhesive layer. The sheet-like pressure-sensitive adhesive layer may be crosslinked with ultraviolet light and primarily cured so that it has latent ultraviolet reactivity, in other words, so that it retains ultraviolet reactivity. In the case of the primary curing, the sheet-shaped pressure-sensitive adhesive layer may be crosslinked by irradiating it with ultraviolet light through the transparent release resin sheet.
[0088] In this case, it is possible to adjust the degree of ultraviolet crosslinking by controlling the amount of ultraviolet radiation. However, as described above, it is also possible to adjust the degree of ultraviolet crosslinking by irradiating ultraviolet radiation through a transparent release resin sheet to block part of the ultraviolet radiation.
[0089] Examples of transparent release resin sheets include cast films or stretched films of polyester resins, polypropylene resins, or polyethylene resins that have been coated with silicone resin to give a release treatment, and release paper, etc., which can be appropriately selected and used. In particular, it is preferable to use transparent release resin sheets with different peel strengths or transparent release resin sheets with different thicknesses.
[0090] The thickness of the "sheet-like pressure-sensitive adhesive layer", i.e., the pressure-sensitive adhesive sheet before secondary curing described below, the amount of ultraviolet light irradiated, the irradiating wavelength, the irradiating device, etc. may be adjusted as appropriate.
[0091] [Step (2)] In step (2), two image display device components are laminated via the "sheet-like adhesive layer" obtained in step (1), and then ultraviolet light is irradiated from at least one of the image display device components to crosslink the "sheet-like adhesive layer" with ultraviolet light via this member, thereby causing secondary curing.
[0092] In order to cause an ultraviolet crosslinking reaction in the "sheet-like adhesive layer" via the above-mentioned image display device constituent member, a sufficient amount of light with an effective wavelength for exciting the photopolymerization initiator in the "sheet-like adhesive layer" and generating radicals must reach the image display device constituent member, and therefore it is preferable that one of the image display device constituent members has an ultraviolet transmittance of a certain level or higher. Specifically, for example, when a glass plate is laminated on the side of the "sheet-like adhesive layer" that is irradiated with ultraviolet light, it is preferable that the ultraviolet transmittance of the glass plate is at a certain level or higher, and, for example, when a glass plate, an adhesive, and a protective sheet are laminated, it is preferable that the ultraviolet transmittance of the laminate of the glass plate, the adhesive, and the protective sheet is at a certain level or higher. Therefore, it is preferable that the ultraviolet transmittance, i.e., the light transmittance in the UV-A wavelength range of 315 to 400 nm, of the image display device component laminated to the ultraviolet ray irradiation side of the "sheet-like pressure-sensitive adhesive layer" is 20% or more, particularly 30% or more, and even more preferably 40% or more.
[0093] Examples of members that can have such light transmittance include those made of polycarbonate resin, acrylic resin, polyvinyl chloride resin, polyester resin, cellulose resin such as triacetyl cellulose resin (TAC) and diacetyl cellulose resin, styrene resin, etc. Among these, polycarbonate resin, acrylic resin, triacetyl cellulose resin, etc. have high hygroscopicity, and moisture absorbed by the resin during storage is easily released as outgas from the resin when used at high temperatures. According to the image display device of the present invention, foaming caused by the release of such outgas can be suppressed, so that it is possible to use resin members made of the polycarbonate resin, acrylic resin, triacetyl cellulose resin, etc. as resin members constituting the image display device.
[0094] (Explanation of terms, etc.) In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it encompasses a plate, a sheet, and a film.
[0095] In this specification, when it is written "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" and "preferably smaller than Y". In addition, when it is stated that "X or more" (X is any number), unless otherwise specified, it includes the meaning of "X or more" as well as "preferably larger than X", and when it is stated that "Y or less" (Y is any number), it includes the meaning of "Y or less" as well as "preferably smaller than Y", unless otherwise specified. Furthermore, "at least one of x and y (x and y are any constitution or component)" means three combinations: x only, y only, and x and y. EXAMPLES
[0096] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.
[0097] Example 1 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 30 g of methyl phenylglyoxylate (A-1, manufactured by Sanyo Trading Co., Ltd., SBPI-716) was added as an intramolecular hydrogen abstraction initiator and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0098] The obtained pressure-sensitive adhesive composition was sandwiched between two release-treated polyethylene terephthalate films (Diafoil MRV, 100 μm thick, manufactured by Mitsubishi Chemical Corporation / Diafoil MRQ, 75 μm thick, manufactured by Mitsubishi Chemical Corporation) and shaped into a sheet having a thickness of 150 μm to produce transparent double-sided pressure-sensitive adhesive sheet 1. The transparent double-sided pressure-sensitive adhesive sheet 1 was subjected to various evaluations described below. The results are shown in Table 1.
[0099] Example 2 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 27 g of methyl phenylglyoxylate (A-1, SBPI-716 manufactured by Sanyo Trading Co., Ltd.) and 3 g of 4-methacryloyloxybenzophenone (C-1, MBP manufactured by MCC Unitech Co., Ltd.) were added as intramolecular hydrogen abstraction initiators and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0100] The obtained pressure-sensitive adhesive composition was sandwiched between two release-treated polyethylene terephthalate films (Diafoil MRV, 100 μm thick, manufactured by Mitsubishi Chemical Corporation / Diafoil MRQ, 75 μm thick, manufactured by Mitsubishi Chemical Corporation) and shaped into a sheet having a thickness of 150 μm to produce transparent double-sided pressure-sensitive adhesive sheet 2. The transparent double-sided pressure-sensitive adhesive sheet 2 was subjected to various evaluations described below. The results are shown in Table 1.
[0101] Example 3 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 24 g of methyl phenylglyoxylate (A-1, manufactured by Sanyo Trading Co., Ltd., SBPI-716) and 6 g of 4-methacryloyloxybenzophenone (C-1, manufactured by MCC Unitech Co., Ltd., MBP) were added as intramolecular hydrogen abstraction initiators and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0102] The obtained pressure-sensitive adhesive composition was sandwiched between two release-treated polyethylene terephthalate films (Diafoil MRV, 100 μm thick, manufactured by Mitsubishi Chemical Corporation / Diafoil MRQ, 75 μm thick, manufactured by Mitsubishi Chemical Corporation) and shaped into a sheet having a thickness of 150 μm to produce transparent double-sided pressure-sensitive adhesive sheet 3. The transparent double-sided pressure-sensitive adhesive sheet 3 was subjected to various evaluations described below. The results are shown in Table 1.
[0103] Example 4 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 21 g of methyl phenylglyoxylate (A-1, manufactured by Sanyo Trading Co., Ltd., SBPI-716) and 9 g of 4-methacryloyloxybenzophenone (C-1, manufactured by MCC Unitech Co., Ltd., MBP) were added as intramolecular hydrogen abstraction initiators and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0104] The obtained pressure-sensitive adhesive composition was sandwiched between two release-treated polyethylene terephthalate films (Diafoil MRV, 100 μm thick, manufactured by Mitsubishi Chemical Corporation / Diafoil MRQ, 75 μm thick, manufactured by Mitsubishi Chemical Corporation) and shaped into a sheet having a thickness of 150 μm to produce transparent double-sided pressure-sensitive adhesive sheet 4. The transparent double-sided pressure-sensitive adhesive sheet 4 was subjected to various evaluations described below. The results are shown in Table 1.
[0105] Example 5 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 200 g of an ultraviolet curing resin propoxylated pentaerythritol triacrylate (ATM-4PL, manufactured by Shin-Nakamura Chemical Co., Ltd.) as a crosslinking agent and 30 g of methyl phenylglyoxylate (A-1, manufactured by Sanyo Trading Co., Ltd., SBPI-716) as an intramolecular hydrogen abstraction initiator were added and mixed uniformly to obtain a resin composition for the adhesive layer.
[0106] The obtained pressure-sensitive adhesive composition was sandwiched between two release-treated polyethylene terephthalate films (Diafoil MRV, 100 μm thick, manufactured by Mitsubishi Chemical Corporation / Diafoil MRQ, 75 μm thick, manufactured by Mitsubishi Chemical Corporation) and shaped into a sheet having a thickness of 150 μm to produce transparent double-sided pressure-sensitive adhesive sheet 5. The transparent double-sided pressure-sensitive adhesive sheet 5 was subjected to various evaluations described below. The results are shown in Table 1.
[0107] Example 6 To 1 kg of a copolymer (B-2, mass average molecular weight 120,000) consisting of 40 parts by mass of 2-ethylhexyl acrylate, 44 parts by mass of lauryl acrylate, 3 parts by mass of acrylamide, 6.5 parts by mass of methyl methacrylate, and 6.5 parts by mass of isobornyl methacrylate, 15 g of methyl phenylglyoxylate (A-1, manufactured by Sanyo Trading Co., Ltd., SBPI-716) as an intramolecular hydrogen abstraction initiator was added and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0108] The obtained pressure-sensitive adhesive composition was sandwiched between two release-treated polyethylene terephthalate films (Diafoil MRV, 100 μm thick, manufactured by Mitsubishi Chemical Corporation / Diafoil MRQ, 75 μm thick, manufactured by Mitsubishi Chemical Corporation) and shaped into a sheet having a thickness of 150 μm to produce transparent double-sided pressure-sensitive adhesive sheet 6. The transparent double-sided pressure-sensitive adhesive sheet 6 was subjected to various evaluations described below. The results are shown in Table 1.
[0109] Comparative Example 1 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 15 g of a mixture of 4-methylbenzophenone and 2,4,6-trimethylbenzophenone (A'-1, manufactured by IGM, ESACURE TZT) as an intermolecular hydrogen abstraction initiator was added and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0110] Next, the pressure-sensitive adhesive composition was formed into a sheet having a thickness of 150 μm on a release-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, Diafoil MRV, thickness 100 μm), and then covered with a release-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, Diafoil MRQ, thickness 75 μm) to produce pressure-sensitive adhesive sheet 7. The pressure-sensitive adhesive sheet 7 was subjected to various evaluations described below. The results are shown in Table 1.
[0111] Comparative Example 2 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 15 g of a diester of carboxymethoxybenzophenone and polytetramethylene glycol (A'-2, IGM, Omnipol BP) as an intermolecular hydrogen abstraction initiator was added and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0112] Next, the pressure-sensitive adhesive composition was formed into a sheet having a thickness of 150 μm on a release-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, Diafoil MRV, thickness 100 μm), and then covered with a release-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, Diafoil MRQ, thickness 75 μm) to produce pressure-sensitive adhesive sheet 8. The pressure-sensitive adhesive sheet 8 was subjected to various evaluations described below. The results are shown in Table 1.
[0113] Comparative Example 3 To 1 kg of a copolymer (B-1, mass average molecular weight 400,000) consisting of 76 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of vinyl acetate, and 4 parts by mass of acrylic acid, 15 g of a diester of carboxymethoxybenzophenone and polyethylene glycol 200 (A'-3, manufactured by LGM, Omnipol 682) as an intermolecular hydrogen abstraction initiator was added and mixed uniformly to obtain a pressure-sensitive adhesive composition.
[0114] Next, the pressure-sensitive adhesive composition was formed into a sheet having a thickness of 150 μm on a release-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, Diafoil MRV, thickness 100 μm), and then covered with a release-treated polyethylene terephthalate film (manufactured by Mitsubishi Chemical Corporation, Diafoil MRQ, thickness 75 μm) to produce pressure-sensitive adhesive sheet 9. The pressure-sensitive adhesive sheet 9 was subjected to various evaluations described below. The results are shown in Table 1.
[0115] <Various evaluations> (1) Yellowing resistance reliability The protective film of a commercially available polarizing film (layer structure: TAC layer / PVA layer / TAC layer, POL in FIG. 1) was peeled off in advance, and the film was left to stand for 2 days in an environment of 25°C and 90% RH. After leaving it for 2 days, the release film on one side of each of the adhesive sheets 1 to 9 (adhesive sheet thickness 150 μm, OCA in Figure 1) prepared in the above Examples and Comparative Examples was peeled off, and a PET film (Toyobo Co., Ltd., Cosmoshine A4100, 100 μm) was attached to the exposed surface using a hand roller. Next, the adhesive sheet with the PET film was cut into a size of 30 mm x 30 mm, the remaining release film was peeled off, and a polarizing film was attached with a hand roller so as to have the layer structure shown in Figure 1. The laminate was autoclaved for 20 minutes under an environment of 60 °C x 0.2 MPa. Furthermore, the integrated light intensity of 8000 mJ / cm at a wavelength of 365 nm was applied through the PET film. 2 A sample for evaluating the yellowing resistance reliability was prepared by irradiating the sample with ultraviolet light from a high-pressure mercury lamp so as to crosslink the sample (see Figure 1).
[0116] This sample for evaluating yellowing resistance reliability was allowed to stand at 25°C and 90% RH for two days, after which acetone was used to separate only the PVA layer used in the polarizing film from the sample for evaluating yellowing resistance reliability, and the PVA layer was visually inspected to see whether it had yellowed.
[0117] Regarding the yellowing resistance reliability, the PVA layer was judged as "poor" when its appearance turned yellow, and as "good" when it showed no discoloration. The results are shown in Table 1.
[0118] As shown in the Comparative Examples described below, the commercially available polarized film yellows due to the pressure-sensitive adhesive containing an intermolecular hydrogen abstraction initiator, but in order to quantify the degree of yellowing, the absorbance of the polarizer at the discolored portion (edge) of the sample for evaluating yellowing resistance reliability in Comparative Example 1 was measured as follows and found to be 3.5 or more. This shows that the absorbance of Comparative Example 1, which was rated x in the yellowing resistance reliability test, is 3.5 or more, and therefore the absorbance of the Examples, which were rated ◯ in the yellowing resistance reliability test, is lower than this.
[0119] (Absorbance of polarizer) The measurement device used was an ultraviolet-visible-near infrared spectrophotometer (Shimadzu Corporation's SolidSpec-3700DUV). Based on the measurement conditions below, light from the spectrometer was directly introduced and two polarizing films (one was a blank polarizing film and the other was the above-mentioned sample for evaluating yellowing resistance reliability) were crossed and stacked to measure the absorbance.
[0120] <Measurement conditions> Slit width: 5 nm ·Measurement speed slow Light source: Deuterium lamp 310nm or less, halogen lamp 310nm or more Detector: PMT (870nm or less) · Accessory equipment Large sample chamber Integrating sphere (60mmφ) Spectralon ·Incidence angle 0° (transmission measurement)
[0121] (2) Bubble-proof reliability The release film on one side of the transparent double-sided pressure-sensitive adhesive sheets 3 and 4 (thickness 150 μm) produced in Examples 3 and 4 was peeled off, and the sheets were attached to a soda-lime glass plate (54 × 82 mm, thickness 0.55 mm) with a hand roll (Figure 2 (a)). After that, stamp marks of 1 mm and 2 mm were made from the film side as shown in Figure 2 (b) and (c). Furthermore, the remaining release film was peeled off, and the sheets were attached to a chemically strengthened glass plate (54 × 82 mm, thickness 0.55 mm) with a polarizing film by hand rolling while bending the glass as shown in Figure 2 (d). Next, the laminated product was autoclaved for 20 minutes under an environment of 60°C and 0.2 MPa. This sample was then irradiated with an integrated light dose of 3000 mJ / cm2 at a wavelength of 365 nm through a PET film. 2 The samples were irradiated with ultraviolet light from a high-pressure mercury lamp and left to stand for 6 hours in an environment of 85°C, after which the appearance was visually inspected. As a result, no air bubbles were observed in any of the samples.
[0122] (3) Overall evaluation Based on the evaluation results of the above yellowing resistance reliability and bubbling resistance reliability, a comprehensive evaluation was made according to the following evaluation criteria. ◎ There are two "〇"s 〇···There is one "〇" ×...There is no "〇"
[0123] [Table 1]
[0124] (Evaluation Results) The pressure-sensitive adhesive sheets of Examples 1 to 6 contained an intramolecular hydrogen abstraction initiator (A) as a photopolymerization initiator, and thus had excellent reliability in terms of resistance to yellowing of the polarizing film.
[0125] On the other hand, it was found that the samples of Comparative Examples 1 to 3, which have a benzophenone structure, which is an intermolecular hydrogen abstraction type photopolymerization initiator, cause yellowing of the polarizing film.
[0126] Moreover, it was confirmed that those containing the above compound (C) as in Examples 3 and 4 could have both high yellowing resistance and high bubbling resistance.
[0127] In addition, in order to confirm that yellowing occurs depending on the type of polarizing film, i.e., that there are polarizing films that do not yellow even when a pressure-sensitive adhesive composition containing an intermolecular hydrogen abstraction initiator is used, a commercially available polarizing film other than the polarizing film described above was prepared. The polarizing film was used to carry out the same test as the above-mentioned yellowing resistance reliability test, and the polarizing film did not yellow even when the pressure-sensitive adhesive of Comparative Example 1 was used. From the above, although the mechanism is unclear, it was found that the yellowing of polarizing films depends on the type of polarizing film and is affected by the hydrogen abstraction initiator, and in particular, for polarizing films that discolor when using an adhesive containing an intermolecular hydrogen abstraction initiator, it is effective to use an intramolecular hydrogen abstraction initiator (A) instead of the initiator. [Industrial Applicability]
[0128] The pressure-sensitive adhesive layer-attached polarizing film of the present invention is suitable for bonding various members, since the pressure-sensitive adhesive layer has reliable yellowing resistance to the polarizing film. In particular, it can be suitably used for an image display device having a touch panel.
Claims
1. A polarizing film with a pressure-sensitive adhesive layer, comprising a polarizing film and a pressure-sensitive adhesive layer on at least one surface of the polarizing film, the pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition containing an intramolecular hydrogen abstraction initiator (A) and a compound (C) having, in its molecule, a radical polymerizable functional group having a carbon-carbon double bond and a radical generating group, and a blending ratio of the intramolecular hydrogen abstraction initiator (A) to the compound (C) [(A) / (C)] is 85 / 15 to 60 / 40 by mass; The polarizing film has an absorbance of a polarizer at a wavelength of 300 to 400 nm of 3.5 or more, the absorbance being measured after adhering a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an intermolecular hydrogen abstraction initiator and leaving the film at rest at 25°C and 90% RH for 2 days. Polarizing film with adhesive layer.
2. The pressure-sensitive adhesive composition further comprises at least one pressure-sensitive adhesive component (B) selected from the group consisting of a base polymer (b1), a mixture of monomer components constituting the base polymer (b2), and a partial polymer (b3) thereof.
3. The pressure-sensitive adhesive layer-attached polarizing film according to claim 1 or 2, wherein the compound (C) having in its molecule a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group has a (meth)acryloyl group, and at least one structure selected from the group consisting of a benzophenone structure, a benzyl structure, an o-benzoylbenzoic acid ester structure, a thioxanthone structure, a 3-ketocoumarin structure, a 2-ethylanthraquinone structure, and a camphorquinone structure.
4. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 3, wherein the intramolecular hydrogen abstraction initiator (A) is at least one of a benzoylmethylformate-based photopolymerization initiator and an oxyphenyl-based photopolymerization initiator.
5. The pressure-sensitive adhesive layer-attached polarizing film according to claim 4 , wherein the methyl benzoylformate-based photopolymerization initiator is methyl phenylglyoxylate.
6. The pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 5, wherein the pressure-sensitive adhesive composition further contains a crosslinking agent other than the compound (C).
7. The pressure-sensitive adhesive layer-attached polarizing film according to claim 6 , wherein the crosslinking agent other than the compound (C) is a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups.
8. 3. The polarized film with a pressure-sensitive adhesive layer according to claim 2, wherein the intramolecular hydrogen abstraction initiator (A) is contained in a range of 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the pressure-sensitive adhesive component (B).
9. The polarizing film with the pressure-sensitive adhesive layer according to any one of claims 1 to 8, wherein the pressure-sensitive adhesive layer is a photocurable layer.
10. The pressure-sensitive adhesive sheet has a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an intramolecular hydrogen abstraction initiator (A) and a compound (C) having, in its molecule, a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group, and the blending ratio of the intramolecular hydrogen abstraction initiator (A) to the compound (C) [(A) / (C)] is 85 / 15 to 60 / 40 by mass.
11. The pressure-sensitive adhesive sheet according to claim 10, wherein the pressure-sensitive adhesive composition further comprises at least one pressure-sensitive adhesive component (B) selected from the group consisting of a base polymer (b1), a mixture of monomer components constituting the base polymer (b2), and a partial polymer (b3) thereof.
12. The pressure-sensitive adhesive sheet according to claim 10 or 11, wherein the compound (C) having a radically polymerizable functional group having a carbon-carbon double bond and a radical generating group in the molecule has a (meth)acryloyl group and at least one structure selected from the group consisting of a benzophenone structure, a benzyl structure, an o-benzoylbenzoic acid ester structure, a thioxanthone structure, a 3-ketocoumarin structure, a 2-ethylanthraquinone structure and a camphorquinone structure.
13. The pressure-sensitive adhesive sheet according to any one of claims 10 to 12, wherein the intramolecular hydrogen abstraction initiator (A) is at least one of a benzoylmethylformate photopolymerization initiator and an oxyphenyl photopolymerization initiator.
14. The pressure-sensitive adhesive sheet according to claim 13 , wherein the methyl benzoylformate-based photopolymerization initiator is methyl phenylglyoxylate.
15. The pressure-sensitive adhesive sheet according to any one of claims 10 to 14, wherein the pressure-sensitive adhesive composition further comprises a crosslinking agent other than the compound (C).
16. The pressure-sensitive adhesive sheet according to claim 15 , wherein the crosslinking agent other than the compound (C) is a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups.
17. The pressure-sensitive adhesive sheet according to any one of claims 10 to 16, wherein the pressure-sensitive adhesive layer is a photocurable layer.
18. The pressure-sensitive adhesive sheet according to claim 11, wherein the intramolecular hydrogen abstraction initiator (A) is contained in an amount of 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the pressure-sensitive adhesive component (B).
19. The pressure-sensitive adhesive sheet according to any one of claims 10 to 18, wherein the pressure-sensitive adhesive sheet has a thickness of 10 µm or more and 500 µm or less.
20. A laminated member having a configuration in which the pressure-sensitive adhesive sheet according to any one of claims 10 to 19 is laminated to a component of an image display device.
21. The laminate member according to claim 20 , wherein the image display device component is a polarizing film.
22. An image display device comprising the laminated member according to claim 20 or 21.
23. An image display device comprising the pressure-sensitive adhesive layer-attached polarizing film according to any one of claims 1 to 9.
Citation Information
Patent Citations
Adhesive agent of polaroid and preparation method for polaroid by using adhesive agent
CN102212317A
Antistatic agent, adhesive composition applying same, display device and polarizer
CN107903355A
JP1974071529A
Pressure-sensitive adhesive sheet for bonding of optical element
JP2006169438A
Optical functional film with adhesive composition layer for liquid crystal display and liquid crystal display including the same
JP2007156066A