Magnetic compact and inductor
By controlling the area ratio and standard deviation of magnetic particles in a magnetic molded body, the issue of low permeability is addressed, resulting in improved magnetic performance.
Patent Information
- Application Number
- JP2020166445
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Conventional magnetic molded bodies face issues with poor dispersibility and uneven distribution of particles with different average sizes, leading to low magnetic permeability due to insufficient arrangement of small particles in gaps between large particles.
A magnetic molded body comprising first and second magnetic particles with controlled area ratio and standard deviation, where the area ratio standard deviation is 0.40 or less, ensuring even distribution and improved magnetic permeability.
The solution achieves a magnetic molded body with high magnetic permeability by uniformly arranging first and second magnetic particles, enhancing the magnetic properties.
Smart Images

Figure 0007563087000003 
Figure 0007563087000004 
Figure 0007563087000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a magnetic compact and an inductor. [Background technology]
[0002] Patent Document 1 describes a core (magnetic compact) manufactured using a metal powder having a particle size distribution obtained by blending two particle groups with different average particle sizes, and an inductor manufactured using this core. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-113436 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors realized that there were problems to be overcome with conventional magnetic compacts and found it necessary to take measures to address these problems. Specifically, the present inventors discovered the following problems:
[0005] The core described in Patent Document 1 is a mixture of particle groups with different average particle sizes, and when the particle groups are mixed by a commonly known method, the dispersibility and flowability of the particles with a large average particle size and the particles with a small average particle size are reduced. Therefore, in the resin, the particles with a small average particle size are not sufficiently arranged in the gaps between the particles with a large average particle size, and the arrangement of the particles with a large average particle size and the particles with a small average particle size is biased, resulting in a low filling rate and making it difficult to increase the magnetic permeability. As a result, the core described in Patent Document 1 could not obtain a high magnetic permeability.
[0006] The present invention has been made in view of the above problems. That is, a main object of the present invention is to provide a magnetic green body and an inductor that can obtain high magnetic permeability. [Means for solving the problem]
[0007] The inventors of the present application attempted to solve the above problems by taking a new approach, rather than simply extending the conventional technology, and as a result arrived at an invention that achieves the above-mentioned main object.
[0008] The magnetic molding according to the present invention is A magnetic molding comprising first magnetic particles, second magnetic particles having a particle size larger than that of the first magnetic particles, and a resin, In the following area ratios calculated for a plurality of regions of the magnetic compact, Area ratio=(total area of the first magnetic particles) / (total area of the second magnetic particles) The standard deviation of the area ratio is 0.40 or less.
[0009] An inductor according to the present invention has the above-mentioned magnetic compact disposed on a winding core of a coil conductor. Effect of the Invention
[0010] The magnetic molding of the present invention has an area ratio (sum of the area of the first magnetic particles) / (sum of the area of the second magnetic particles) calculated for multiple regions, and the standard deviation of the area ratio is 0.40 or less, so that a magnetic molding with high magnetic permeability can be obtained. [Brief description of the drawings]
[0011] [Figure 1] 1(a) and 1(b) are process diagrams that diagrammatically show the method for producing a magnetic green compact according to this embodiment. [Diagram 2] 2A, 2B, and 2C are views showing the magnetic green body according to the present embodiment, in which FIG. 2A is a perspective view, FIG. 2B is a plan view, and FIG. 2C is a cross-sectional view taken along the line a-a' of FIG. 2A. [Diagram 3] FIG. 3 is a schematic diagram of a cross-sectional SEM image of the magnetic green compact according to this embodiment. [Figure 4] FIG. 4 is a graph showing the correlation between the frequency of magnetic particles and particle size. [Diagram 5] FIG. 5 is an explanatory diagram for explaining a method for calculating the area ratio from a cross-sectional SEM image. [Figure 6] FIG. 6 is a schematic perspective view showing the steps of a method for manufacturing an inductor according to this embodiment. [Figure 7] FIG. 7 is a perspective view of the inductor according to the present embodiment. [Figure 8] FIG. 8 is a front perspective view of the inductor according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. However, the embodiment described below is for illustrative purposes only, and the present invention is not limited to the embodiment described below.
[0013] [About magnetic compacts] The magnetic green body according to the embodiment of the present invention will be described. In the broad sense, the term "magnetic green body" refers to a material used to enhance a magnetic field in a device that generates a magnetic field, such as an inductor, and in the narrow sense, refers to a material used as a coating for a coil (conductor) in an inductor or a core for a coil (conductor).
[0014] First, the raw materials used to manufacture the magnetic green body will be described. The raw materials used to manufacture the magnetic green body may include first magnetic raw particles, second magnetic raw particles, resin, solvent and / or hardener. In addition, they may include additives such as lubricants.
[0015] The first magnetic raw particle may be a conventionally used Fe-based metal magnetic particle, for example, Fe (pure iron) or an Fe alloy. An example of an Fe alloy may be one or more metal magnetic material particles selected from the group consisting of an alloy containing Fe and Ni, an alloy containing Fe and Co, an alloy containing Fe and Si, an alloy containing Fe, Si and Cr, an alloy containing Fe, Si and Al, an alloy containing Fe, Si, B and Cr, and an alloy containing Fe, P, Cr, Si, B, Nb and C. Furthermore, the first magnetic raw particle may have a surface that has been subjected to an insulation treatment. For example, the first magnetic raw particle may have an insulating coating on its surface. The insulating coating may be one or more insulating coatings selected from the group consisting of an inorganic glass coating, an organic-inorganic hybrid coating, and an inorganic insulating coating formed by a sol-gel reaction of a metal alkoxide.
[0016] The second magnetic raw particle may be a conventionally used Fe-based metal magnetic particle, for example, Fe (pure iron) or an Fe alloy. An example of an Fe alloy may be one or more metal magnetic material particles selected from the group consisting of an alloy containing Fe and Ni, an alloy containing Fe and Co, an alloy containing Fe and Si, an alloy containing Fe, Si and Cr, an alloy containing Fe, Si and Al, an alloy containing Fe, Si, B and Cr, and an alloy containing Fe, P, Cr, Si, B, Nb and C. The composition of the second magnetic raw particle may be the same as or different from the composition of the first magnetic raw particle. Furthermore, the second magnetic raw particle may have a surface that has been subjected to an insulation treatment. For example, the second magnetic raw particle may have an insulating coating on its surface. The insulating coating may be one or more insulating coatings selected from the group consisting of an inorganic glass coating, an organic-inorganic hybrid coating, and an inorganic insulating coating formed by a sol-gel reaction of a metal alkoxide.
[0017] The resin may contain a functional group that contributes to the curing reaction. In other words, the resin may be cured by the curing reaction to enable the production of a magnetic molding. Therefore, the "resin" in this specification may include not only a completely cured resin, but also a resin in an uncured state before the curing reaction. An example of the resin may be at least one selected from the group consisting of epoxy resin, phenolic resin, polyester resin, polyimide resin, polyolefin resin, and silicone resin. In particular, when an epoxy resin is used as the resin, a magnetic molding having high electrical insulation and / or mechanical strength can be obtained. Alternatively, a thermoplastic resin such as polyamideimide, polyphenylene sulfide, and / or liquid crystal polymer may be used. The curing reaction is preferably caused by heat. In other words, the resin is preferably a thermosetting resin. One example is a thermoplastic epoxy resin. If such a resin is used, the curing reaction can be caused by a simple method.
[0018] The solvent is used to mix the raw materials to obtain a slurry, and is preferably an organic solvent. For example, the solvent may include any of aromatic hydrocarbons such as toluene or xylene, ketones such as acetone, methyl ethyl ketone, or methyl isobutyl ketone, alcohols such as methanol, ethanol, or isopropyl alcohol, and glycol ethers such as propylene glycol monomethyl ether or propylene glycol monomethyl ether acetate.
[0019] The hardener may be used to harden the resin, and may include, by way of example only, an imidazole-based hardener, an amine-based hardener, or a guanidine-based hardener (e.g., dicyandiamide).
[0020] The lubricant may be used to improve the lubricity of the second magnetic raw particles and the first magnetic raw particles and to improve the filling rate. Furthermore, the lubricant may be used to facilitate release from a mold during molding. The lubricant may include, for example, nanosilica, barium sulfate, or a stearic acid compound (lithium stearate, magnesium stearate, zinc stearate, potassium stearate, etc.).
[0021] The weight ratio of each raw material used in the manufacturing method of the magnetic compact may be such that the first magnetic raw material particles and the second magnetic raw material particles are 94% to 98% by weight based on the total, the resin and the hardener are 1% to 5% by weight based on the total, and the remainder is the lubricant and the solvent. The ratio of the first magnetic raw material particles and the second magnetic raw material particles is preferably such that the weight of the first magnetic raw material particles: the weight of the second magnetic raw material particles is 10:90 to 50:50. The ratio of the resin and the hardener is preferably such that the weight of the resin: the weight of the hardener is 95:5 to 98:2.
[0022] -Method of manufacturing magnetic compact- Next, a method for producing a magnetic green body according to an embodiment of the present invention will be described with reference to Fig. 1 and Fig. 2. Fig. 1(a) and Fig. 1(b) are process diagrams that typically show the method for producing a magnetic green body according to the present embodiment. Fig. 2 shows the magnetic green body according to the present embodiment, with Fig. 2(a) being a perspective view, Fig. 2(b) being a plan view, and Fig. 2(c) being a cross-sectional view taken along line a-a' of Fig. 2(a). The method described below is merely an example, and the method for producing a magnetic green body according to the present embodiment is not limited to the following method.
[0023] First, a first magnetic raw particle having a small particle size and a second magnetic raw particle having a large particle size are prepared. Here, the first magnetic raw particle and the second magnetic raw particle may form an insulating film on the particle surface. The method of forming the insulating film is not particularly limited, and may be formed by, for example, a mechanochemical method or a sol-gel method. Among them, the mechanochemical method is a low-cost method that is particularly suitable for forming a relatively thick insulating film on particles having a large particle size. In addition, when forming an insulating film using the mechanochemical method, the thickness of the insulating film can be controlled by controlling the amount of insulating material added. On the other hand, the sol-gel method is applicable to particle sizes of a wide range of compositions and sizes, and can form an insulating film with a relatively thin thickness. In addition, an insulating film with a relatively high melting point can be formed. When forming an insulating film using the sol-gel method, the thickness of the insulating film can be controlled by, for example, adjusting the time of the sol-gel reaction, the amount of metal alkoxide and solvent added, and the like. Of the prepared first magnetic raw material particles and second magnetic raw material particles, the second magnetic raw material particles are placed in a stirring vessel and stirred in the vessel.
[0024] Next, a particle raw material containing a first magnetic raw material particle having a small particle size, a resin, a solvent, and a hardener is mixed to obtain a slurry. Then, this slurry is stored in a spraying device. An example of the spraying device is a device capable of spraying in a mist form. More specifically, a spraying device is included. The above-mentioned raw material may contain a lubricant. In other words, the lubricant is not an essential component of the raw material. In the particle raw material stored in the spraying device, the weight ratio of the solvent may be 1.0% by weight or more and 5.0% by weight or less based on the weight of the entire material used (first magnetic raw material particle, second magnetic raw material particle, resin, hardener, solvent, and / or lubricant).
[0025] Next, a particle raw material containing the first magnetic raw particles is sprayed onto the second magnetic raw particles being stirred in the stirring vessel using a spraying device. In this specification, "spraying" means ejecting a liquid in a mist form. The spraying is performed at a temperature of 30°C to 80°C in the air or in N2. 2It is preferable that the heating is performed under a 1000 rpm atmosphere. By spraying the first magnetic raw particles onto the second magnetic raw particles under such a temperature, the solvent in the raw material may be volatilized. In this way, by spraying the particle raw material containing the first magnetic raw particles onto the second magnetic raw particles using a spraying device, the first magnetic raw particles are evenly dispersed around the second magnetic raw particles. Therefore, when the magnetic compact is produced, the first magnetic raw particles and the second magnetic raw particles are easily arranged evenly, and the first magnetic raw particles are filled into the gaps between the second magnetic raw particles, making it difficult for cavities to occur, and the filling rate between the first magnetic raw particles and the second magnetic raw particles can be increased. Then, the precursor containing the first magnetic raw particles and the second magnetic raw particles is stirred in the stirring vessel and evenly dispersed.
[0026] After that, the precursor from which the solvent has evaporated is shaken with a sieve shaker (mesh size: 160 μm or more and 300 μm or less) to remove the coarse particles, thereby obtaining a magnetic powder. Here, in the magnetic powder of this embodiment, the resin undergoes almost no hardening reaction. In other words, the resin is in an unhardened or semi-hardened state. In this specification, the term "magnetic powder" refers to a particulate material used to manufacture a "magnetic molding". In this way, a magnetic powder is obtained in which a plurality of first magnetic raw particles are bonded to the periphery of a second magnetic raw particle with a resin. In this embodiment, the embodiment contains the first magnetic raw particle and the second magnetic raw particle, but third magnetic raw particle, fourth magnetic raw particle, etc., which have different compositions and / or average particle diameters from these, may be used in addition.
[0027] Next, the manufactured magnetic powder 100 is filled into a mold K (see FIG. 1). In this embodiment, the mold K is described as a mold for manufacturing an E-shaped core that is E-shaped in cross section, but the mold is not limited thereto and may be, for example, a mold for manufacturing at least one selected from the group consisting of an I-shaped core, a T-shaped core, a plate-shaped core, and a toroidal ring-shaped core. The mold K filled with the magnetic powder 100 is introduced into a pressure molding machine (see FIG. 1(a)), and pressure may be applied under an environment of 20°C to 40°C, 50 MPa to 150 MPa, and 30 s or less (see FIG. 1(b)). Here, the magnetic powder 100 contains a thermosetting resin as described above, but since the temperature during pressure application is relatively low, 20°C to 40°C, the curing reaction does not proceed and the magnetic powder may be in an uncured or semi-cured state. After pressure application is completed, the magnetic compact may be removed from the mold.
[0028] In this way, the magnetic green body 10 of this embodiment may be stored with the resin in an uncured or semi-cured state. In other words, when it becomes necessary to manufacture a magnetic green body that is almost completely cured as a product, the semi-cured magnetic green body 10 may be filled into a mold different from the mold K, and the resin may be cured under the curing conditions of 150°C to 200°C, 5 MPa to 50 MPa, and 60 s to 1800 s to manufacture the magnetic green body (see Figs. 2(a) to (c)). The magnetic green body may be produced by molding a sheet containing magnetic powder, stacking, pressing, and thermally curing a plurality of sheets.
[0029] -Analysis method for magnetic compacts- Next, an analysis method of the magnetic green body manufactured by the above-mentioned manufacturing method will be described with reference to Figures 3 to 5. Figure 3 is a schematic diagram of a cross-sectional SEM image of the magnetic green body according to this embodiment, Figure 4 is a graph showing the correlation between the particle size and frequency of the magnetic particles in the magnetic green body according to this embodiment, and Figure 5 is an explanatory diagram for explaining a calculation method of the area ratio of the magnetic particles in the magnetic green body according to this embodiment. In Figures 3 and 5, the symbol J indicates resin.
[0030] The manufactured magnetic green bodies are mainly analyzed using a SEM (scanning electron microscope). To obtain cross-sectional SEM images, the fracture surface near the center of the magnetic green body is cross-sectionally processed using an ion milling device, and the processed magnetic green body sample is introduced into the SEM. Cross-sectional observation is performed at a magnification of 500 to 2000 times. A schematic diagram of the obtained cross-sectional SEM image is shown in Figure 3.
[0031] Furthermore, the obtained cross-sectional SEM image is subjected to image analysis using image analysis software (WinROOF2018 manufactured by Mitani Shoji), and the particle size distribution of the magnetic powder is obtained from the image analysis. Specifically, the particle size (circle equivalent diameter) of each particle is calculated by binarizing the obtained cross-sectional SEM image, and the shape of each particle is assumed to be a sphere having the calculated circle equivalent diameter. The frequency of each particle is counted, and the correlation between the particle size and the particle frequency on a volume basis is graphed, and the particle size distribution is obtained. The graph obtained by the image analysis is shown in FIG. 4. According to the graph in FIG. 4, the manufactured magnetic powder has a first peak value and a second peak value having a higher particle frequency than the first peak value. In addition, the magnetic powder has a bottom value between the first peak value and the second peak value. The particle size corresponding to the bottom value is calculated as D. Note that the number of peak values is not limited to two, and may be three or more. In addition, there may be multiple bottom values corresponding to this. When there are multiple bottom values, the particle size corresponding to the smallest bottom value is taken as D. In the obtained particle size distribution, particles having a particle size (circle equivalent diameter) smaller than the particle size D are defined as first magnetic particles, and particles having a particle size (circle equivalent diameter) larger than the particle size D are defined as second magnetic particles. In this embodiment, the particle size D1 corresponding to the first peak value corresponds to the most frequent particle size of the first magnetic particles, and the particle size D2 corresponding to the second peak value corresponds to the most frequent particle size of the second magnetic particles. Furthermore, the particle size corresponding to the bottom value between the first peak value and the second peak value is defined as D.
[0032] Here, in this specification, the "first magnetic particles" refer to particles having a particle size (equivalent circle diameter) smaller than the particle size D corresponding to the bottom value, and the "second magnetic particles" refer to particles having a particle size (equivalent circle diameter) larger than the particle size D corresponding to the bottom value. Furthermore, in this specification, the "mode particle size of the first magnetic particles" refers to the particle size at which the particle frequency is highest in the region of particle sizes smaller than the particle size D in a graph showing the correlation between the particle size and frequency of magnetic particles in a magnetic powder, and the "mode particle size of the second magnetic particles" refers to the particle size at which the particle frequency is highest in the region of particle sizes larger than the particle size D in a graph showing the correlation between the particle size and frequency of magnetic particles in a magnetic powder.
[0033] The first magnetic particles in this embodiment may have a mode particle size of 0.5 μm or more and 8 μm or less, preferably 1 μm or more and 5 μm or less. The second magnetic particles are particles having a particle size larger than the first magnetic particles. The mode particle size of the second magnetic particles is preferably 10 μm or more and 50 μm or less. When the mode particle size of the second magnetic particles is 50 μm or less, the eddy current loss can be reduced. The mode particle size of the second magnetic particles is more preferably 20 μm or more and 40 μm or less. Also, (mode particle size of the first magnetic particles) / (mode particle size of the second magnetic particles)=0.02 or more and 0.5 or less. In this case, the filling rate of the magnetic particles can be increased. Also, in the magnetic compact, the filling rate of the magnetic particles is preferably 0.75 or more.
[0034] The area ratio of the first magnetic particles and the second magnetic particles is calculated using the cross-sectional SEM image of the magnetic compact (see FIG. 3) and the particle size distribution of the magnetic particles in the magnetic compact (see FIG. 4). The calculation method of the area ratio is explained below. In FIG. 3 and FIG. 5, the second magnetic particles L as large particles are vertically hatched, the first magnetic particles S as small particles are horizontally hatched, and the resin J is hatched with dots.
[0035] First, an analysis area A for analyzing the area ratio of the first magnetic particles S and the second magnetic particles L is set (see FIG. 5). The analysis area A is an area of 10×D horizontally and 7.5×D vertically, utilizing particle size D. Note that the analysis area A is not limited to this size, and a larger area may be analyzed. The total area of the first magnetic particles S and the total area of the second magnetic particles L within this analysis area A are calculated. The area calculation can be performed using the image analysis software described above. The area ratio is then calculated as (sum of the areas of the first magnetic particles S) / (sum of the areas of the second magnetic particles L).
[0036] The calculation of the area ratio is performed at 10 randomly selected locations in the magnetic compact, and the standard deviation is calculated. In the magnetic compact according to the present embodiment, the standard deviation is 0.40 or less. More preferably, the standard deviation is 0.34 or less. In this specification, the "standard deviation" is an index showing the variation of data, and the smaller the standard deviation value, the smaller the variation.
[0037] Furthermore, it is also possible to measure the filling rate of the magnetic particles from the above-mentioned cross-sectional SEM image. Specifically, a cross-sectional SEM image is obtained in the same manner as in the measurement of the coverage rate in the above-mentioned magnetic compact. The ratio of the occupied area of the magnetic particles to the area of the observation region is obtained by binarizing the acquired cross-sectional SEM image. The ratio of the occupied area of the magnetic particles to the area of the observation region is obtained at 10 randomly selected locations, and the average value is taken as the filling rate of the magnetic particles. This makes it possible to measure the filling rate of the magnetic particles. In this embodiment, the aspect of obtaining the particle size distribution from the cross-sectional SEM image has been described, but when obtaining the particle size distribution of powdered magnetic particles as a raw material, it can be measured by a laser diffraction method or a scattering method.
[0038] [About inductors] Next, an inductor using the above-mentioned magnetic molded body will be described. First, a method for manufacturing an inductor will be described with reference to Figs. 6 to 8. Fig. 6 is a perspective view of steps that typically show a method for manufacturing an inductor according to this embodiment, Fig. 7 is a perspective view of the inductor according to this embodiment, and Fig. 8 is a front perspective view of the inductor according to this embodiment.
[0039] -Inductor manufacturing method- First, the conductor 20 to be wound around the magnetic compact is prepared. The conductor 20 is preferably configured by covering a metal wire (e.g., a rectangular copper wire) with a resin or the like. In this case, the conductor 20 can be firmly molded in cooperation with the resin contained in the magnetic compact. The conductor 20 is preferably wound by alpha winding, in which the start and end of the winding are wound outward at the same time. By winding the conductor 20 by alpha winding, the end of the winding is positioned on the outside, making it easy to handle the lead-out portion.
[0040] Next, the magnetic green compact 10 in which the resin is uncured or semi-cured is prepared. The alpha-wound conductive wire 20 is accommodated in the magnetic green compact 10. That is, the magnetic green compact 10 is placed in the winding core of the coil conductor. At this time, a part of the E-shaped core is inserted in the winding core of the conductive wire 20 (see FIG. 6). Furthermore, the magnetic powder may be further used to cover the conductive wire 20. The conductive wire 20, the magnetic green compact 10 and the magnetic powder are accommodated in a mold and then introduced into a pressure molding machine. Then, the resin contained in the magnetic green compact 10 is cured in an environment of 150° C. to 200° C., 5 MPa to 50 MPa, and 60 s to 1800 s to form an inductor element.
[0041] Next, the element body may be barrel polished to round off the edges of the element body. Rounding the edges can prevent breakage of the external electrodes that will be formed later. Then, the external electrodes 30 are formed on the element body. The external electrodes 30 may be formed by plating, by applying a conductive paste to the element body and baking it, or by sputtering (see FIGS. 7 and 8). Examples of the external electrodes 30 include those made by thermally curing a conductive resin paste containing Ag powder, Ni plating, Sn plating, and the like. The external electrodes 30 may also have a structure in which multiple layers of these are laminated.
[0042] In this way, an inductor can be manufactured using the magnetic powder and magnetic compact described above. Note that, although in Fig. 7 the cross section of the conductor 20 intersecting with the extension direction of the conductor 20 is exposed on the surface of the element body and connected to the external electrode 30, both ends of the conductor 20 may be bent so that the side of the conductor 20 parallel to the extension direction of the conductor 20 is exposed on the surface of the element body and connected to the external electrode 30. EXAMPLES
[0043] -Example of magnetic compact- Next, examples related to the present invention will be described. Magnetic compacts of the following examples and comparative examples were manufactured and subjected to verification tests.
[0044] The raw materials used in the manufacture of the magnetic green body in Examples 1 and 2 and Comparative Examples 1 and 2 are shown below. As for the manufacturing method of the magnetic green body, in Examples 1 and 2, as in the manufacturing method of the magnetic green body according to the present embodiment, first, a particle raw material containing the first magnetic raw particles was sprayed on the second magnetic raw particles in an environment of 60 ° C to manufacture the magnetic powder. On the other hand, in Comparative Examples 1 and 2, a resin and a solvent were added to the first magnetic raw particles and the second magnetic raw particles being stirred in a stirring vessel, and then a hardener and a lubricant were added to obtain a granulated powder. The granulated powder was dried at 60 ° C to volatilize the solvent. At this stage, since one granulated powder contains a plurality of second magnetic raw particles, the second magnetic raw particles were pulverized with a pulverizer so that the second magnetic raw particles were separated from each other, and the magnetic powder was obtained by removing the coarse particles with a sieve as in the examples. In Examples 1 and 2 and Comparative Examples 1 and 2, the mesh size of the sieve for removing the coarse particles was set to 180 μm.
[0045] Next, a toroidal ring-shaped magnetic green body was manufactured using the magnetic powders of the above-mentioned Examples 1 and 2 and Comparative Examples 1 and 2. The manufacturing method of the magnetic green body was the same as that described in the above "-Method of manufacturing magnetic green body-" for both the Examples and Comparative Examples. First, pressure was applied for 10 seconds in a first mold at 30°C and 100 MPa. Next, pressure was applied for 600 seconds in a second mold at 180°C and 20 MPa to harden the resin and manufacture the magnetic green body.
[0046] The raw materials used for the magnetic powders of Examples 1 and 2 and Comparative Examples 1 and 2 are as follows. First magnetic particle: D50 particle size 4.0μm Fe-6.7Si-2.5Cr amorphous alloy (Fe:Si:Cr=90.8:6.7:2.5 (weight ratio)) Second magnetic particle: D50 particle size 28μm Fe-6.7Si-2.5Cr amorphous alloy (Fe:Si:Cr=90.8:6.7:2.5 (weight ratio)) Resin: Thermosetting epoxy resin Solvent: Acetone Hardener: Imidazole Lubricant: Nano-silica (diameter 50 nmφ) particle shape
[0047] For the magnetic powder after production in Example 1, the weight ratio of the first magnetic particles and the second magnetic particles was 96.0% by weight based on the total magnetic powder, the weight ratio of the resin and the hardener was 3.6% by weight based on the total magnetic powder, and the lubricant was 0.4% by weight based on the total magnetic powder. Note that the solvent was used at 4.6% by weight based on the weight of the total raw materials (first magnetic particles, second magnetic particles, resin, solvent, hardener, and lubricant), but was volatilized during the production of the magnetic powder.
[0048] Furthermore, for the magnetic powder after production in Example 1, the weight ratio of the first magnetic particles:the weight ratio of the second magnetic particles was 25:75, and the weight ratio of the resin:the weight ratio of the curing agent was 97.4:2.6.
[0049] In the magnetic powder after production in Example 2, the weight ratio of the first magnetic particles and the second magnetic particles was 96.5% by weight based on the total magnetic powder, the weight ratio of the resin and the hardener was 3.1% by weight based on the total magnetic powder, and the lubricant was 0.4% by weight based on the total magnetic powder. Note that the solvent was used at 4.1% by weight based on the total weight of the raw materials, but was volatilized during the production of the magnetic powder.
[0050] In addition, for the magnetic powder after production in Example 2, the weight ratio of the first magnetic particles:the weight ratio of the second magnetic particles was 25:75, and the weight ratio of the resin:the weight ratio of the curing agent was 97.4:2.6.
[0051] In the magnetic powder after production in Comparative Example 1, the weight ratio of the first magnetic particles and the second magnetic particles was 96.0% by weight based on the total magnetic powder, the weight ratio of the resin and the hardener was 3.6% by weight based on the total magnetic powder, and the lubricant was 0.4% by weight based on the total magnetic powder. Note that the solvent was used at 4.6% by weight based on the total weight of the raw materials, but was volatilized during the production of the magnetic powder.
[0052] In addition, for the magnetic powder after production in Comparative Example 1, the weight ratio of the first magnetic particles:the weight ratio of the second magnetic particles was 25:75, and the weight ratio of the resin:the weight ratio of the curing agent was 97.4:2.6.
[0053] In the magnetic powder after production in Comparative Example 2, the weight ratio of the first magnetic particles and the second magnetic particles was 96.5% by weight based on the total magnetic powder, the weight ratio of the resin and the hardener was 3.1% by weight based on the total magnetic powder, and the lubricant was 0.4% by weight based on the total magnetic powder. Note that the solvent was used at 4.1% by weight based on the total weight of the raw materials, but was volatilized during the production of the magnetic powder.
[0054] In addition, for the magnetic powder after production in Comparative Example 2, the weight ratio of the first magnetic particles:the weight ratio of the second magnetic particles was 25:75, and the weight ratio of the resin:the weight ratio of the curing agent was 97.4:2.6.
[0055] Next, for Examples 1 and 2 and Comparative Examples 1 and 2, cross-sectional SEM images were obtained in multiple regions of the magnetic compact to determine the area ratio, and the standard deviation was calculated. The standard deviation results are shown in Table 1. The method for calculating the standard deviation was the method described in the above "Analysis method of magnetic compact". The standard deviation was measured in 10 regions of the magnetic compact.
[0056] [Table 1]
[0057] From the results in Table 1 above, it was found that Examples 1 and 2 had smaller standard deviations than Comparative Examples 1 and 2. That is, the standard deviations of the magnetic compacts of Comparative Examples 1 and 2 were higher than 0.40, whereas the standard deviations of the magnetic compacts of Examples 1 and 2 were 0.40 or less.
[0058] Next, the relative magnetic permeability was measured for the magnetic compacts of Examples 1 and 2 and Comparative Examples 1 and 2. The relative magnetic permeability was measured using an impedance analyzer (E4294A manufactured by Keysight Corporation) at a measurement frequency of 1 MHz. The results of the relative magnetic permeability are shown in Table 2. Note that the "relative magnetic permeability" in this specification refers to the ratio of the magnetic permeability μ of a material to the magnetic permeability μ of a vacuum. 0 The ratio μs = μ / μ 0 means.
[0059] [Table 2]
[0060] From the results of Table 2 above, it was found that Examples 1 and 2 had higher relative magnetic permeability than Comparative Examples 1 and 2. That is, the relative magnetic permeability of the magnetic compacts of Comparative Examples 1 and 2 was less than 23.5, whereas the relative magnetic permeability of the magnetic compacts of Examples 1 and 2 was 23.5 or more. More specifically, the relative magnetic permeability of the inductors of Examples 1 and 2 was 24 or more.
[0061] It should be noted that the embodiments disclosed herein are illustrative in all respects and are not intended to be limiting. Therefore, the technical scope of the present invention is not interpreted solely by the above-described embodiments, but is defined by the claims. The technical scope of the present invention includes all modifications within the scope and meaning equivalent to the claims. [Industrial Applicability]
[0062] The magnetic molded body and inductor according to the present invention can achieve high magnetic permeability and can therefore be suitably used in electronic components that require high magnetic properties. [Explanation of symbols]
[0063] 1 Inductor 10 Magnetic molded body 100 magnetic powder 20 conductors 30 External electrode D1 Most frequent particle size of the first magnetic particle D2: Most frequent particle size of the second magnetic particle D The bottom value with the smallest particle frequency among multiple peak values S 1st magnetic particle L Second magnetic particle J Resin K mold
Claims
1. A magnetic molding comprising first magnetic particles having a first peak value, second magnetic particles having a second peak value and a particle size larger than that of the first magnetic particles, and a resin, When the minimum bottom value between the first peak value and the second peak value is D, the following area ratios of 10 randomly selected points calculated from a plurality of regions of 10×D horizontally and 7.5×D vertically of the magnetic molding are obtained: Area ratio=(total area of the first magnetic particles) / (total area of the second magnetic particles) A magnetic molding, wherein the standard deviation of the area ratio is 0.40 or less.
2. 2. The magnetic molding according to claim 1, wherein the standard deviation is 0.34 or less.
3. the magnetic molding has a bottom value at which the particle frequency is minimum between any of a plurality of peak values in a particle size distribution showing a correlation between particle frequency and particle size, the particle size of the first magnetic particles is smaller than the bottom value, The magnetic green compact according to claim 1 , wherein the particle diameter of the second magnetic particles is greater than the bottom value.
4. The magnetic compact according to claim 1, wherein the first magnetic particles and the second magnetic particles are metal magnetic particles.
5. 5. The magnetic molding according to claim 4, wherein the metal magnetic particles comprise at least one selected from the group consisting of an alloy containing Fe, Fe, and Ni, an alloy containing Fe and Co, an alloy containing Fe and Si, an alloy containing Fe, Si, and Cr, an alloy containing Fe, Si, B, and Cr, and an alloy containing Fe, P, Cr, Si, B, Nb, and C.
6. The magnetic molding according to any one of claims 1 to 5, wherein the resin is a thermosetting resin.
7. An inductor, comprising the magnetic compact according to any one of claims 1 to 6 disposed on a winding core of a coil conductor.
Citation Information
Patent Citations
inductor
JP2014013803A
Composite particle, powder magnetic core, magnetic element and portable electronic apparatus
JP2014103265A
Soft magnetic material, core and inductor
JP2018113436A
Dust core
JP2020095988A