Glass laminate and optical imaging member
A glass substrate with an Al alloy reflective film and a dielectric film addresses the issues of weather resistance and protrusions in Al films, enhancing productivity and enabling high-resolution imaging.
Patent Information
- Application Number
- JP2020209879
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Aluminum (Al) films used in reflective films have low weather resistance and can develop protrusions, which are defects in optical imaging members, and require a protective film, increasing costs.
A glass substrate with a reflective film made of an Al alloy and a dielectric film, such as silicon oxide, is used to suppress the reaction between the glass substrate's alkaline components and the reflective film, preventing protrusion defects and enhancing weather resistance without the need for a protective film.
The solution provides a reflective film with improved weather resistance and productivity by suppressing protrusion defects, reducing costs, and enabling high-resolution imaging.
Smart Images

Figure 0007563158000002 
Figure 0007563158000003 
Figure 0007563158000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass substrate with a reflective film, a glass laminate, and an optical imaging member. [Background technology]
[0002] In recent years, technological developments have been progressing for forming an image in the air from light emitted from a flat panel display. Specifically, for example, a technology has been developed in which light emitted from a flat panel display is reflected by and transmitted through an optical imaging member and then enters the eye, so that an image displayed on the flat panel display appears to be displayed in the air.
[0003] The following Patent Document 1 discloses an example of an optical imaging member and a glass laminate used therein. The glass laminate described in Patent Document 1 is formed by laminating a plurality of glass substrates with a reflective film. It is described that Al or Ag is used for the reflective film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-094794 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the Al film has a problem in that it has low weather resistance, and in order to maintain a suitable reflectivity, it is necessary to provide a protective film on the surface of the Al film, which increases costs.
[0006] Furthermore, when an Al film is used as a reflective film, protrusions with a width of about several tens of μm to a hundred μm may occur on the surface of the Al film. Such protrusions become unacceptable defects when used in display-related members, particularly when used in optical imaging members. After extensive research, the present inventors have found that the cause of these defects is gases such as H2 that are generated by the reaction of the Al film with alkaline components of a detergent remaining on the surface of the glass substrate.
[0007] An object of the present invention is to provide a glass substrate with a reflective film, a glass laminate, and an optical imaging member that can reflect light favorably and increase productivity. [Means for solving the problem]
[0008] The glass substrate with a reflective film according to the present invention comprises a glass substrate having first and second main surfaces facing each other, and a reflective film provided on the first main surface of the glass substrate, the reflective film being made of an alloy containing Al, and further comprising a dielectric film provided between the glass substrate and the reflective film.
[0009] Preferably, the dielectric film is a silicon oxide film.
[0010] The glass substrate is preferably made of non-alkali glass.
[0011] It is preferable that the tolerance of the thickness of the glass substrate is within ±5 μm.
[0012] A glass laminate according to the present invention comprises a plurality of rectangular glass substrates with a reflective film which are stacked together, each of the plurality of glass substrates with a reflective film being the above-mentioned glass substrate with a reflective film.
[0013] The optical imaging member of the present invention comprises a pair of glass laminates, each of which is the above-mentioned glass laminate, each of the pair of glass laminates having a lamination end face in which surfaces connected to first main surfaces and second main surfaces of a plurality of glass substrates with reflective film are continuous, the lamination end face of one glass laminate is disposed on the lamination end face of the other glass laminate, and the first main surface of the glass substrate with reflective film in one glass laminate and the first main surface of the glass substrate with reflective film in the other glass laminate are perpendicular to each other. Effect of the Invention
[0014] According to the present invention, it is possible to provide a glass substrate with a reflective film, a glass laminate, and an optical imaging member that can reflect light favorably and increase productivity. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic cross-sectional view showing a glass substrate with a reflective film according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic perspective view of a glass substrate with a reflective film according to a modified example of the first embodiment of the present invention. [Diagram 3] FIG. 5 is a schematic perspective view of a glass laminate according to a second embodiment of the present invention. [Figure 4] FIG. 13 is a schematic, partially cut-away perspective view illustrating an optical imaging member according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in each drawing, components having substantially the same functions may be referred to by the same reference numerals.
[0017] (Glass substrate with reflective coating) (First embodiment) 1 is a schematic cross-sectional view showing a glass substrate with a reflective film according to a first embodiment of the present invention. The glass substrate with a reflective film 1 is used, for example, as an optical imaging member. The glass substrate with a reflective film 1 includes a glass substrate 2, a dielectric film 3, and a reflective film 4. The glass substrate 2 has a first main surface 2a and a second main surface 2b. The dielectric film 3 is provided on the first main surface 2a. The reflective film 4 is provided on the dielectric film 3.
[0018] The reflective film 4 is made of an alloy containing Al. The reflective film 4 is preferably made of an alloy containing Al and Mg. This can effectively increase both the reflectance and the weather resistance.
[0019] More specifically, the composition of the alloy constituting the reflective film 4 is preferably, in mass %, 90.6% to 98.7% Al, 0.45% to 5.6% Mg, 0% to 0.8% Si, 0% to 0.7% Fe, 0% to 0.4% Cu, 0% to 1% Mn, 0% to 0.35% Cr, 0% to 0.25% Zn, 1% to 0.2% Ti, and 0% to 0.06% B.
[0020] The feature of this embodiment is that the reflective film 4 is made of an alloy containing Al, and the dielectric film 3 is provided between the glass substrate 2 and the reflective film 4. As described above, in the past, when manufacturing a glass substrate with a reflective film, protrusions having a width of about several tens of μm to a hundred μm were sometimes generated on the reflective film. Here, the present inventors found that the cause of this is gas such as H2 generated by the reaction between the alkaline component of the detergent remaining on the glass substrate and the reflective film. It is considered that the generated gas pushes up a part of the reflective film, causing the protruding defect. In contrast, in the glass substrate with a reflective film 1 of this embodiment, the dielectric film 3 is provided between the glass substrate 2 and the reflective film 4. This makes it possible to suppress the reaction between the alkaline component on the glass substrate 2 and the reflective film 4, and to suppress the generation of gas. Therefore, it is possible to suppress the generation of protruding defects in the reflective film 4, and to increase productivity. In addition, since the reflective film 4 is made of an alloy containing Al, it is possible to increase weather resistance, and it is not necessary to provide a protective film on the reflective film 4. Therefore, it is possible to reduce costs, effectively increase productivity, and favorably reflect light.
[0021] In this embodiment, the dielectric film 3 is a silicon oxide film. More specifically, the dielectric film 3 is a SiO2 film. However, the material of the dielectric film 3 is not limited to the above, and for example, silicon nitride or aluminum oxide can be used. Specifically, the dielectric film 3 can be made of Si3N4 or Al2O3. It is more preferable to use SiO2 for the dielectric film 3. This allows the refractive indexes of the glass substrate 2 and the dielectric film 3 to be close to each other, and the reflection of light at the interface between the glass substrate 2 and the dielectric film 3 can be suppressed. This makes it possible to suppress the occurrence of so-called ghosts when used in an optical imaging member.
[0022] The thickness of the dielectric film 3 is preferably 1 nm or more, which can more reliably suppress the reaction between the alkaline component and the reflective film 4. The upper limit of the thickness of the dielectric film 3 is not particularly limited, but may be, for example, 50 nm or less.
[0023] The glass substrate 2 is preferably made of non-alkali glass, which can more reliably suppress the reaction between the alkaline component and the reflective film 4. An example of the non-alkali glass is "OA-11" manufactured by Nippon Electric Glass Co., Ltd.
[0024] Incidentally, a glass laminate is used for the optical imaging member. The glass laminate is a laminate of a plurality of rectangular glass substrates with a reflective film. The glass substrate 1 with a reflective film of this embodiment shown in Fig. 1 is a rectangular plate. Fig. 2 shows a rectangular glass substrate with a reflective film, which is a modified example of this embodiment.
[0025] FIG. 2 is a schematic perspective view of a glass substrate with a reflective film according to a modified example of the first embodiment. A rectangular glass substrate with a reflective film 1A has a first surface 2c, a second surface 2d, a third surface 2e, and a fourth surface 2f. The first surface 2c, the second surface 2d, the third surface 2e, and the fourth surface 2f are connected to the first main surface 2a and the second main surface 2b, respectively. The first surface 2c and the third surface 2e face each other. The first surface 2c and the third surface 2e extend in the longitudinal direction. On the other hand, the second surface 2d and the fourth surface 2f face each other. The second surface 2d and the fourth surface 2f extend in the lateral direction.
[0026] When the dimension along the longitudinal direction of the rectangular glass substrate 1A with a reflective film is L, the dimension along the lateral direction is W, and the aspect ratio is L / W, L / W is preferably 5 or more, more preferably 10 or more, even more preferably 20 or more, even more preferably 30 or more, still more preferably 40 or more, even more preferably 50 or more, still more preferably 60 or more, and particularly preferably 100 to 2000. If the aspect ratio is too small, the production efficiency of the optical imaging member is likely to decrease.
[0027] For example, a laminate of a plurality of rectangular glass substrates 1A with a reflective film may be obtained by cutting a laminate of the glass substrate 1 with a reflective film of the first embodiment. Alternatively, a plurality of rectangular glass substrates 1A with a reflective film may be obtained by cutting one glass substrate 1 with a reflective film. Then, the glass substrates 1A with a reflective film may be laminated to obtain one glass laminate.
[0028] In the glass laminate, the interval between the multiple reflective films 4 is equal to the thickness of the reflective film-coated glass substrate 1. Here, the thickness of the glass substrate 2 is preferably 3000 μm or less, more preferably 2500 μm or less, even more preferably 1500 μm or less, and even more preferably 1000 μm or less. The thinner the glass substrate 2, the narrower the interval between the reflective films 4, making it easier to obtain a high-resolution image.
[0029] On the other hand, the thickness of the glass substrate 2 is preferably 50 μm or more, more preferably 100 μm or more, even more preferably 300 μm or more, even more preferably 400 μm or more, and particularly preferably 500 μm or more, so that the glass substrate 2 is less likely to be damaged during the transportation process or the like.
[0030] The arithmetic mean roughness Ra of at least one of the first main surface 2a and the second main surface 2b of the glass substrate 2 is preferably 10 nm or less, more preferably 5 nm or less, even more preferably 1 nm or less, even more preferably 0.8 nm or less, even more preferably 0.4 nm or less, even more preferably 0.3 nm or less, and particularly preferably 0.001 nm to 0.2 nm. If the arithmetic mean roughness Ra of the first main surface 2a and the second main surface 2b of the glass substrate 2 is too large, the intervals of the reflective films 4 are likely to vary. Therefore, especially when the glass substrates 1 with the reflective films are laminated, the variation in the intervals of the reflective films 4 is amplified, making it difficult to obtain a high-resolution image. Furthermore, when the glass substrates 1 with the reflective films are laminated, air is likely to be entrained, and optical bonding is difficult. The arithmetic mean roughness Ra in this specification complies with JIS B 0601:2001.
[0031] The waviness of the glass substrate 2 is preferably 1 μm or less, more preferably 0.08 μm or less, even more preferably 0.05 μm or less, even more preferably 0.03 μm or less, even more preferably 0.02 μm or less, and particularly preferably 0.01 μm or less. If the waviness of the glass substrate 2 is too large, the intervals of the reflective films 4 tend to vary. Therefore, particularly when the glass substrates 1 with the reflective films are laminated, the variation in the intervals of the reflective films 4 is amplified, making it difficult to obtain a high-resolution image. Furthermore, when the glass substrates 1 with the reflective films are laminated, air tends to be entrained and optical bonding becomes difficult. It should be noted that "waviness" refers to the value measured using a stylus-type surface shape measuring device to measure the WCA (filtered centerline waviness) as described in JIS B 0610:2001, and this measurement is performed in accordance with a method conforming to SEMI STD D15-1296 "Method for measuring surface waviness of FPD protective glass substrates", with a cutoff of 0.8 mm to 8 mm during measurement, and refers to the value measured over a length of 300 mm in a direction perpendicular to the withdrawal direction of glass substrate 2.
[0032] The dimension of one side of the glass substrate 2 as viewed from the first main surface 2a is preferably 500 mm or more, more preferably 600 mm or more, even more preferably 800 mm or more, even more preferably 1000 mm or more, even more preferably 1200 mm or more, even more preferably 1500 mm or more, and particularly preferably 2000 mm or more. In this way, it becomes easier to increase the size of the optical imaging member. Furthermore, since a large number of rectangular glass substrates 1A with a reflective film can be obtained from one glass substrate 1 with a reflective film, the productivity can be increased. Note that if the glass substrate 2 is made large, it may become more difficult to completely remove the alkaline component of the detergent. In contrast, in this embodiment, a dielectric film 3 is provided between the glass substrate 2 and the reflective film 4. This makes it possible to suppress the reaction between the alkaline component and the reflective film 4, and to suppress the occurrence of defects. In this way, the present invention is also suitable for the case where the glass substrate 1 with a reflective film is made large.
[0033] On the other hand, if the dimension of one side of the glass substrate 2 is too large, it becomes difficult to cut the reflective film-coated glass substrate 1 when obtaining the rectangular reflective film-coated glass substrate 1A. Therefore, the dimension of one side of the glass substrate 2 is preferably 3500 mm or less, more preferably 3200 mm or less, and particularly preferably 3000 mm or less.
[0034] The transmittance of the glass substrate 2 at a wavelength of 300 nm, calculated as a thickness of 500 μm, is preferably 30% or more, more preferably 50% or more, even more preferably 70% or more, even more preferably 80% or more, even more preferably 85% or more, and particularly preferably 89% to 99%. The transmittance of the glass substrate 2 at a wavelength of 350 nm, calculated as a thickness of 500 μm, is preferably 50% or more, more preferably 70% or more, even more preferably 80% or more, even more preferably 85% or more, even more preferably 89% or more, even more preferably 90% or more, and particularly preferably 91% or more. The transmittance of the glass substrate 2 at a wavelength of 550 nm, calculated as a thickness of 500 μm, is preferably 85% or more, more preferably 89% or more, even more preferably 90% or more, and particularly preferably 91% to 99%. In this way, when the glass substrate 1 with a reflective film is applied to an optical imaging member or the like, the loss of light is reduced when the light is transmitted while being repeatedly reflected, making it easier to obtain a high-resolution image.
[0035] The tolerance of the thickness of the glass substrate 1 with a reflective film is preferably within the range of ±5 μm. If the tolerance is too large, the intervals of the reflective films 4 are likely to vary. Therefore, particularly when the glass substrates 1 with a reflective film are stacked, the variation in the intervals of the reflective films 4 is amplified, making it difficult to obtain a high-resolution image. Furthermore, when the glass substrates 1 with a reflective film are stacked, air is likely to be entrapped, and optical bonding becomes difficult.
[0036] The effects of the present invention will be described in more detail below by comparing examples and comparative examples.
[0037] (Example) A SiO2 film was formed on the first main surface of a glass substrate ("OA-11" manufactured by Nippon Electric Glass Co., Ltd.) that had been cleaned with a batch cleaner using an alkaline detergent. The thickness of the SiO2 film was 50 nm. The SiO2 film was formed by introducing 150 sccm of Ar gas and using 3 kW of power, and was oxidized in the oxidation source by introducing 150 sccm of O2 gas and using 2.5 kW of power.
[0038] Next, a reflective film was formed on the SiO2 film. The reflective film was an Al-Mg alloy film. The thickness of the reflective film was 100 nm. The reflective film was formed by introducing 300 sccm of Ar gas and using 5 kW of power. Using the above method, 20 glass substrates with reflective film were produced.
[0039] (Comparative Example) Twenty glass substrates with a reflective film were produced in the same manner as in the example, except that a SiO 2 film was not formed on the first main surface of the glass substrate, but a reflective film was formed thereon.
[0040] (evaluation) The incidence of protrusion-like defects on the surfaces of the glass substrates with a reflective film of the examples and comparative examples was investigated.
[0041] [Table 1]
[0042] As shown in Table 1, in the comparative example, the incidence rate of protrusions is 40%. In contrast, in the example, the incidence rate of protrusions is 0%. In this way, in the present invention, it is possible to suppress the occurrence of defects due to protrusions and to increase productivity.
[0043] (Glass laminate) Second embodiment 3 is a schematic perspective view of a glass laminate according to a second embodiment of the present invention. The glass laminate 15 includes a plurality of rectangular glass substrates 1A with a reflective film. The glass laminate 15 is formed by stacking a plurality of glass substrates 1A with a reflective film. Specifically, a configuration in which the second main surface 2b of the glass substrate 2 in one glass substrate 1A with a reflective film and the reflective film 4 of the other glass substrate 1A with a reflective film are bonded together is repeated.
[0044] The glass laminate 15 has a pair of lamination end faces 16 and 17. The lamination end face 16 is formed by continuing the first surfaces 2c of the plurality of reflective film-coated glass substrates 1A. The lamination end face 17 is formed by continuing the third surfaces 2e of the plurality of reflective film-coated glass substrates 1A. The lamination end face 16 or the lamination end face 17 is a surface that is joined to the lamination end face 16 or the lamination end face 17 of another glass laminate 15 when obtaining an optical imaging member.
[0045] Of lamination end faces 16 and 17, the arithmetic mean roughness Ra of the surface to be joined to another glass laminate 15 is preferably 3 μm or less, more preferably 2 μm or less, even more preferably 1.5 μm or less, even more preferably 1.2 μm or less, and particularly preferably 1 μm or less. This makes it possible to prevent air from being entrapped when a pair of glass laminates 15 are joined together.
[0046] On the other hand, the arithmetic mean roughness Ra of the lamination end surface 16 and the lamination end surface 17 is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, even more preferably 0.2 μm or more, even more preferably 0.4 μm or more, and particularly preferably 0.7 μm or more. In this case, the need to polish the lamination end surface 16 is reduced. Therefore, by setting it to be equal to or less than any of the above upper limits and equal to or more than any of the above lower limits, the bondability between the glass laminates 15 can be improved and the productivity can be increased.
[0047] In the glass laminate 15, the number of laminated glass substrates 1A with a reflective film is preferably 100 or more, more preferably 200 or more, even more preferably 300 or more, even more preferably 400 or more, still more preferably 500 or more, even more preferably 600 or more, and particularly preferably 700 or more. The greater the number of laminated glass substrates 1A with a reflective film, the easier it is to produce a large optical imaging member.
[0048] The glass substrates 1A with a reflective film are preferably bonded together by an adhesive layer. In this way, the glass substrates 1A with a reflective film can be firmly integrated together. The thickness of the adhesive layer is preferably 100 μm or less, more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and particularly preferably 30 μm or less. In this way, it becomes easier to narrow the gap between the reflective films 4. Note that, as the adhesive used for the adhesive layer, a transparent adhesive such as OCA (Optical Clear Adhesive) or Cemedine is preferable from the viewpoint of optical properties. Alternatively, an adhesive made of a UV-curable resin is preferable from the viewpoint of manufacturing efficiency.
[0049] The adhesive layer may be made of, for example, EVA resin (ethylene-vinyl acetate copolymer resin). The thickness of the adhesive layer made of EVA resin is preferably 0.5 mm or less, more preferably 0.4 mm or less, even more preferably 0.3 mm or less, even more preferably 0.2 mm or less, even more preferably 0.1 mm or less, even more preferably 0.05 mm or less, and particularly preferably 0.005 mm to 0.03 mm. This makes it easier to obtain a high-resolution image.
[0050] (Optical imaging components) (Third embodiment) 4 is a schematic partially cutaway perspective view showing an optical imaging member according to a third embodiment of the present invention. The optical imaging member 20 includes a pair of glass laminates 15. A lamination end face 17 of one glass laminate 15 is disposed on a lamination end face 16 of the other glass laminate 15. Each first main surface 2a of the glass substrate 1A with a reflective film in one glass laminate 15 and each first main surface 2a of the glass substrate 1A with a reflective film in the other glass laminate 15 are perpendicular to each other.
[0051] The lamination end surface 16 and the lamination end surface 17 of the pair of glass laminates 15 are preferably joined by an adhesive layer. In this way, the pair of glass laminates 15 can be firmly bonded and fixed. The thickness of the adhesive layer is preferably 100 μm or less, more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and particularly preferably 1 μm to 30 μm. This can reduce the optical effect of the adhesive layer. Note that the adhesive used for the adhesive layer is preferably a transparent adhesive such as OCA.
[0052] In this embodiment, the first cover glass 22 and the second cover glass 23 are disposed on the outermost layer side of the pair of glass laminates 15. The first cover glass 22 and the second cover glass 23 are preferably bonded to the glass laminate 15 by an adhesive layer. Specifically, the first cover glass 22, the adhesive layer, one glass laminate 15, the adhesive layer, the other glass laminate 15, the adhesive layer, and the second cover glass 23 are laminated in this order. This eliminates the need to polish the lamination end surface 16 or the lamination end surface 17 of the pair of glass laminates 15 with high precision. Therefore, the productivity of the optical imaging member 20 can be significantly improved. However, the optical imaging member 20 does not necessarily have to have the first cover glass 22 and the second cover glass 23. [Explanation of symbols]
[0053] 1,1A…Glass substrate with reflective film 2. Glass substrate 2a, 2b...First and second principal surfaces 2c~2f: 1st to 4th sides 3...Dielectric film 4…Reflection film 15...Glass laminate 16,17…Laminated end face 20...Optical imaging member 22, 23…First and second cover glasses
Claims
1. A display device comprising a plurality of laminated rectangular glass substrates with a reflective film, Each of the plurality of glass substrates with a reflective film includes a glass substrate having a first main surface and a second main surface facing each other; a reflective film provided on the first main surface of the glass substrate; Equipped with the reflective film is made of an alloy containing Al, The reflective film is not provided on the second main surface of the glass substrate, Each of the plurality of glass substrates with a reflective film further includes a dielectric film provided between the glass substrate and the reflective film, The glass laminate, wherein the first main surface and the second main surface of the glass substrate have an arithmetic mean roughness Ra of 10 nm or less.
2. A display device comprising a plurality of laminated rectangular glass substrates with a reflective film, Each of the plurality of glass substrates with a reflective film includes a glass substrate having a first main surface and a second main surface facing each other; a reflective film provided on the first main surface of the glass substrate; Equipped with the reflective film is made of an alloy containing Al, The reflective film is not provided on the second main surface of the glass substrate, Each of the plurality of glass substrates with a reflective film further includes a dielectric film provided between the glass substrate and the reflective film, The glass laminate, wherein the dielectric film has a thickness of 50 nm or less.
3. 3. The glass laminate according to claim 1, wherein the dielectric film is a silicon oxide film.
4. The glass laminate according to any one of claims 1 to 3, wherein the glass substrate is made of alkali-free glass.
5. The glass laminate according to any one of claims 1 to 4, wherein the thickness tolerance is within ±5 µm.
6. A pair of glass laminates, The pair of glass laminates are each the glass laminate according to any one of claims 1 to 5, each of the pair of glass laminates has a lamination end surface in which surfaces connected to the first main surfaces and the second main surfaces of the plurality of reflective film-coated glass substrates are continuous; the lamination end surface of one of the glass laminates is disposed on the lamination end surface of the other glass laminate, An optical imaging member, wherein the first main surface of the glass substrate with a reflective film in one of the glass laminates and the first main surface of the glass substrate with a reflective film in the other of the glass laminates are perpendicular to each other.
Citation Information
Patent Citations
Reflection mirror for automobile
JP1986133902A
Production of reflecting mirror
JP1991126644A
Surface mirror having optical catalyst layer and its manufacturing method
JP2003131018A
Mirror for vehicle and its manufacturing method
JP2006151203A
Glass laminate with protective glass substrate and manufacturing method therefor
JP2015094794A