Thermosetting resin composition, prepreg, resin-coated metal foil, laminate, printed wiring board, and semiconductor package
A thermosetting resin composition with a phenolic resin and aliphatic hydrocarbon group addresses the challenges of adhesive strength and crack resistance in printed wiring boards, enhancing performance under harsh environments.
Patent Information
- Application Number
- JP2020511118
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-03-30
- Filing Date
- 2019-03-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-03-29
AI Technical Summary
Conventional resin compositions used in printed wiring boards face challenges in ensuring high adhesive strength, particularly under harsh environments, while maintaining low elasticity, high heat resistance, and high elongation, leading to issues such as cracking and poor electrical insulation reliability.
A thermosetting resin composition containing a phenolic resin with an aliphatic hydrocarbon group of 10 to 25 carbon atoms, combined with other thermosetting resins, to enhance adhesive strength, crack resistance, and electrical insulation reliability, while maintaining low elasticity and high heat resistance.
The composition achieves high adhesive strength with metal foils, excellent crack resistance, and improved electrical insulation reliability, even under harsh conditions, with low tackiness and flexibility, suitable for forming prepregs and laminates in printed wiring boards.
Smart Images

Figure 0007563175000001 
Figure 0007563175000002 
Figure 0007563175000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, a prepreg, a resin-coated metal foil, a laminate, a printed wiring board, and a semiconductor package. [Background technology]
[0002] Everyday items used in daily life are becoming increasingly electronic in order to make them more convenient, efficient, and labor-saving, and there is a demand for the electronic components used in electronic devices to be even lighter and smaller in size in order to improve usability, etc. As a result, there is an increasing demand for higher density and higher functionality in the printed wiring boards used in these devices. Since the densification of printed wiring boards can be more effectively achieved by making the glass cloth base material thinner (for example, 30 μm or less), prepregs including such thin glass cloth have been developed and marketed in recent years. As a result, the densification of printed wiring boards is progressing more and more, but it is also becoming more difficult to sufficiently ensure the heat resistance, electrical insulation reliability, and adhesion between the wiring layer and the insulation layer in the printed wiring board.
[0003] Materials for wiring boards used in high-performance printed wiring boards are required to have heat resistance, electrical insulation reliability, long-term reliability, adhesion between wiring layers and insulating layers, etc. Furthermore, materials for flexible wiring boards, which are one type of high-performance printed wiring board, are required to have properties such as low elasticity and flexibility in addition to the above properties. Furthermore, in the case of substrates with ceramic components, the difference in thermal expansion coefficient between the ceramic components and the substrate, and the deterioration of component connection reliability caused by external impact are also major issues. As a solution to this problem, stress relaxation from the substrate side has been proposed. In order to solve these problems, resin compositions containing a thermosetting resin and a thermoplastic resin such as an acrylic polymer and a terminally modified polyethersulfone have been proposed (see, for example, Patent Documents 1 to 5). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-283535 [Patent Document 2] JP 2002-134907 A [Patent Document 3] JP 2002-371190 A [Patent Document 4] JP 2014-193994 A [Patent Document 5] JP 2016-047921 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, although a resin composition containing a thermoplastic resin can ensure low elasticity, high heat resistance, and high elongation, there is a problem in that it is difficult to ensure sufficiently excellent adhesive strength with a metal foil due to the low mechanical strength inherent to thermoplastic resins. Moreover, in recent years, printed wiring boards have been increasingly used in harsh environments such as high temperature environments, and further investigations by the present inventors have revealed that with conventional printed wiring boards, it is difficult to suppress the occurrence of cracks in harsh environments and to ensure adhesive strength with metal foil in harsh environments.
[0006] Therefore, the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a thermosetting resin composition capable of forming a prepreg having low elasticity, high heat resistance, high elongation at room temperature and at high temperature, high electrical insulation reliability, high adhesive strength with metal foil, and excellent crack resistance, as well as a prepreg containing the thermosetting resin composition, a metal foil with resin formed by laminating the thermosetting resin composition and a metal foil, a laminate containing the prepreg or the metal foil with resin, a printed wiring board containing the laminate, and a semiconductor package containing the printed wiring board. [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that a thermosetting resin composition containing a phenolic resin having an aliphatic hydrocarbon group with a specific number of carbon atoms can solve the above problems, and have completed the present invention. The present invention has been completed based on this finding.
[0008] The present invention relates to the following [1] to
[15] . [1] (A) A thermosetting resin composition comprising a phenolic resin, The thermosetting resin composition, wherein the component (A) comprises (A-1) a phenolic resin having an aliphatic hydrocarbon group having 10 to 25 carbon atoms. [2] The thermosetting resin composition according to the above [1], wherein the component (A-1) has at least one structural unit selected from the group consisting of a structural unit (a1) represented by the following general formula (a1) and a structural unit (a2) represented by the following general formula (a2): [ka] (In the above general formula, R 1 represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 9 carbon atoms which may have a substituent, an aromatic hydrocarbon group having 5 to 15 ring atoms which may have a substituent, or a combination of the aliphatic hydrocarbon group and the aromatic hydrocarbon group; R 2 represents an aliphatic hydrocarbon group having 10 to 25 carbon atoms. X represents a hydrogen atom, a hydroxyl group, or a hydroxylmethyl group. m and n each independently represent 0 or 1. [3] The thermosetting resin composition according to the above [2], wherein a molar ratio of the structural unit (a1) to the structural unit (a2) (structural unit (a1) / structural unit (a2)) is 0 to 5.0. [4] The thermosetting resin composition according to any one of the above [1] to [3], wherein the weight average molecular weight (Mw) of the component (A-1) is 4,000 or less. [5] The thermosetting resin composition according to any one of the above [1] to [4], wherein the hydroxyl equivalent of the component (A-1) is 90 to 350 g / eq. [6] The thermosetting resin composition according to any one of the above [1] to [5], wherein the content of the (A-1) component is 0.1 to 40 parts by mass per 100 parts by mass of the total amount of resin components in the thermosetting resin composition. [7] The thermosetting resin composition according to any one of the above [1] to [6], wherein the component (A) further comprises (A-2) a phenol-based resin having no aliphatic hydrocarbon group having 10 to 25 carbon atoms. [8] The thermosetting resin composition according to the above [7], wherein the content of the component (A-1) relative to the total amount of the component (A-1) and the component (A-2) is 30 to 95 mass %. [9] The thermosetting resin composition according to any one of the above [1] to [8], further comprising (B) a thermosetting resin.
[10] The thermosetting resin composition according to the above [9], wherein the component (B) is at least one selected from the group consisting of an epoxy resin, a cyanate resin, a bismaleimide compound, an addition polymer of a bismaleimide compound and a diamine, an isocyanate resin, a triallyl isocyanurate resin, a triallyl cyanurate resin, and a vinyl group-containing polyolefin.
[11] A prepreg comprising the thermosetting resin composition according to any one of the above [1] to
[10] .
[12] A resin-coated metal foil obtained by laminating the thermosetting resin composition according to any one of the above [1] to
[10] and a metal foil.
[13] A laminate comprising the prepreg described in
[11] above or the resin-coated metal foil described in
[12] above.
[14] A printed wiring board comprising the laminate according to
[13] above.
[15] A semiconductor package comprising the printed wiring board described in
[14] above. Effect of the Invention
[0009] The present invention can provide a thermosetting resin composition capable of forming a prepreg having low elasticity, high heat resistance, high elongation at room temperature and at high temperature, high electrical insulation reliability, high adhesive strength with metal foil, and excellent crack resistance (particularly crack resistance in harsh environments); a prepreg containing the thermosetting resin composition; a metal foil with resin formed by laminating the thermosetting resin composition with a metal foil; a laminate containing the prepreg or the metal foil with resin; a printed wiring board containing the laminate; and a semiconductor package containing the printed wiring board. The thermosetting resin composition of the present invention can also be used to form a prepreg with low tackiness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the present invention will be described in detail, but the present invention is not limited to the following embodiment. In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with the values shown in the examples. In addition, the lower and upper limits of the numerical ranges may be arbitrarily combined with the lower and upper limits of other numerical ranges. In addition, each component and material exemplified in this specification may be used alone or in combination of two or more types, unless otherwise specified. In this specification, the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. Furthermore, when the examples and the aspects described as preferred are a collection of options, any number of options may be extracted from the collection, and the extracted options may be combined in any manner with aspects described elsewhere. The present invention also includes any combination of the features described in this specification.
[0011] [Thermosetting resin composition] The thermosetting resin composition of the present invention comprises: A thermosetting resin composition comprising (A) a phenolic resin, The component (A) is a thermosetting resin composition containing (A-1) a phenolic resin having an aliphatic hydrocarbon group having 10 to 25 carbon atoms. The thermosetting resin composition of the present invention can achieve low elasticity, high heat resistance, high elongation under normal temperature and high temperature environments (hereinafter, sometimes simply referred to as high elongation), high crack resistance (especially high crack resistance under harsh environments), high electrical insulation reliability, and high adhesive strength with metal foil. This effect is mainly obtained by including component (A) which is a thermosetting resin but has low elasticity (A-1). It is advantageous in that it has high heat resistance and high elongation, and in particular, low elasticity, which can suppress cracks that tend to occur in printed wiring boards under harsh environments, and in addition, it can achieve high electrical insulation reliability and high adhesive strength with metal foil. In particular, due to its excellent elongation in high temperature environments, it exhibits a stress relaxation effect in high temperature environments, and also exhibits sufficient recovery properties against thermal expansion when a temperature change occurs between a normal temperature environment (referring to a temperature range of approximately 15 to 45°C, the same applies below) and a high temperature environment (referring to a temperature range of approximately 80 to 160°C, the same applies below).
[0012] The thermosetting resin composition of the present invention having the above-mentioned effects is particularly useful for prepregs, laminates, and resin-coated metal foils used in printed wiring boards, etc. Therefore, the thermosetting resin composition of the present invention is also useful as a thermosetting resin composition for an interlayer insulating layer, more specifically, as a thermosetting resin composition for an interlayer insulating layer of a printed wiring board or a thermosetting resin composition for an interlayer insulating layer of a flexible printed wiring board. When the morphology of the cured product of the thermosetting resin composition of the present invention is observed with a scanning electron microscope (SEM) at a magnification of about 2,000 times, no phase separation structure is formed and the morphology appears uniform. The components of the thermosetting resin composition of the present invention will be described below.
[0013] [(A): Phenolic resin] The phenolic resin (A) [hereinafter, sometimes referred to as phenolic resin (A)] contains (A-1) a phenolic resin having an aliphatic hydrocarbon group having 10 to 25 carbon atoms [hereinafter, sometimes referred to as phenolic resin (A-1)]. By containing the phenolic resin (A-1), the phenolic resin (A) can obtain high adhesive strength with the metal foil while having low elasticity, high heat resistance, and high elongation. As the phenolic resin (A-1), one type may be used alone, or two or more types may be used in combination. The phenolic resin (A) can usually function as a curing agent for the thermosetting resin (B) described later, particularly as a curing agent for epoxy resins. The phenolic resin (A-1) contained in the phenolic resin (A) will be described in detail below.
[0014] ((A-1): Phenolic resin having an aliphatic hydrocarbon group having 10 to 25 carbon atoms) The aliphatic hydrocarbon group having 10 to 25 carbon atoms in the phenolic resin (A-1) may be any of chain (straight chain, branched chain), cyclic, and a combination of chain and cyclic, but from the viewpoint of low elasticity and low moisture absorption, chain or a combination of chain and cyclic is preferred, more preferably containing a cyclic group, and even more preferably a combination of chain and cyclic. The "chain" may be straight chain or branched chain, but is more preferably straight chain. The aliphatic hydrocarbon group in the phenolic resin (A-1) has a carbon number of 10 or more, so that a cured product having low elasticity and low moisture absorption can be obtained, and the aliphatic hydrocarbon group has a carbon number of 25 or less, so that high heat resistance can be maintained. From the same viewpoint, the aliphatic hydrocarbon group having 10 to 25 carbon atoms contained in the phenolic resin (A-1) is preferably an aliphatic hydrocarbon group having 10 to 20 carbon atoms, more preferably an aliphatic hydrocarbon group having 12 to 20 carbon atoms, more preferably an aliphatic hydrocarbon group having 12 to 18 carbon atoms, even more preferably an aliphatic hydrocarbon group having 14 to 18 carbon atoms, particularly preferably an aliphatic hydrocarbon group having 14 to 16 carbon atoms, and most preferably a carbon number of 15. On the other hand, in the case of an aliphatic hydrocarbon group other than a chain, it is preferably an aliphatic hydrocarbon group having 10 to 18 carbon atoms, more preferably an aliphatic hydrocarbon group having 10 to 15 carbon atoms, even more preferably an aliphatic hydrocarbon group having 10 to 13 carbon atoms, particularly preferably an aliphatic hydrocarbon group having 10 to 12 carbon atoms, and most preferably an aliphatic hydrocarbon group having 11 carbon atoms.
[0015] The aliphatic hydrocarbon group includes a saturated aliphatic hydrocarbon group having 10 to 25 carbon atoms and an unsaturated aliphatic hydrocarbon group having 10 to 25 carbon atoms. The saturated aliphatic hydrocarbon group and the unsaturated aliphatic hydrocarbon group may be any of a chain (straight chain or branched chain), a ring, or a combination of a chain and a ring, but from the viewpoint of low elasticity and low moisture absorption, a chain or a combination of a chain and a ring is preferable. The chain is more preferably a straight chain. The number of unsaturated bonds possessed by the unsaturated aliphatic hydrocarbon group may be one, two or more, and usually five or less, or three or less.
[0016] From the above, the aliphatic hydrocarbon group having 10 to 25 carbon atoms contained in the phenolic resin (A-1) is preferably a chain-like aliphatic hydrocarbon group having 10 to 25 carbon atoms, or an aliphatic hydrocarbon group having a combination of a chain-like and a cyclic structure, from the viewpoint of low elasticity and low moisture absorption. In the case of an aliphatic hydrocarbon group having a combination of a chain-like and a cyclic structure, the chain-like portion is preferably a straight chain having 4 or more carbon atoms, more preferably a straight chain having 5 or more carbon atoms, from the viewpoint of low elasticity. There is no particular limitation on the combination of the chain-like and the cyclic structure, and it may be -chain-cyclic, -cyclic-chain, or -chain-cyclic-chain, but -cyclic-chain is preferable. Specific examples of -cyclic-chain include 4-pentylcyclohexyl group (C11), 4-octylcyclohexyl group (C14), 4-decylcyclohexyl group (C16), 4-pentylcyclooctyl group (C13), 4-octylcyclooctyl group (C16), etc. Among these, the cyclic chain type is preferably 4-pentylcyclohexyl group (C11).
[0017] In addition, as the phenolic resin (A-1), it is also preferable to use in combination a phenolic resin having a saturated aliphatic hydrocarbon group having 10 to 25 carbon atoms and a phenolic resin having an unsaturated aliphatic hydrocarbon group having 10 to 25 carbon atoms. When a phenolic resin having a saturated aliphatic hydrocarbon group having 10 to 25 carbon atoms and a phenolic resin having an unsaturated aliphatic hydrocarbon group having 10 to 25 carbon atoms are used in combination, the mass ratio of the phenolic resin having an unsaturated aliphatic hydrocarbon group having 10 to 25 carbon atoms to the total of both may be 60 mass% or more, 80 mass% or more, or 90 mass% or more. In addition, there is no particular limit to the upper limit of the mass ratio, and it may be 98 mass% or less. An example of the phenolic resin (A-1) of such an embodiment is a phenolic resin having a structural unit derived from cardanol. In the phenolic resin (A-1), the aliphatic hydrocarbon group having 10 to 25 carbon atoms is preferably substituted at the meta position (3rd or 5th position) relative to the position (1st position) to which the hydroxyl group of the phenol moiety is bonded.
[0018] Examples of the saturated aliphatic hydrocarbon group having 10 to 25 carbon atoms include various decyl groups (the term "various" means all of linear, branched, and cyclic groups, and the same applies hereinafter), various undecyl groups (including, for example, 4-pentylcyclohexyl groups), various dodecyl groups, various tetradecyl groups, various pentadecyl groups, various hexadecyl groups, various octadecyl groups, and various eicosyl groups. Examples of the unsaturated aliphatic hydrocarbon group having 10 to 25 carbon atoms include the saturated aliphatic hydrocarbon group having 10 to 25 carbon atoms, at least a part of which is a carbon-carbon unsaturated bond. For example, when the carbon number is 15, examples thereof include an 8-pentadecen-1-yl group, an 8,11-pentadecadien-1-yl group, and an 8,11,14-pentadecatrien-1-yl group.
[0019] From the viewpoint of low elasticity and low moisture absorption, the phenolic resin (A-1) preferably has at least one structural unit selected from the group consisting of a structural unit (a1) represented by the following general formula (a1) and a structural unit (a2) represented by the following general formula (a2). It can be said that the phenolic resin (A-1) has at least one structural unit (a2). [ka] (In the above general formula, R 1 represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 9 carbon atoms which may have a substituent, an aromatic hydrocarbon group having 5 to 15 ring atoms which may have a substituent, or a combination of the aliphatic hydrocarbon group and the aromatic hydrocarbon group; R 2 represents an aliphatic hydrocarbon group having 10 to 25 carbon atoms. X represents a hydrogen atom, a hydroxyl group, or a hydroxylmethyl group. m and n each independently represent 0 or 1.
[0020] In the general formulae (a1) and (a2), "-*" indicates a bond. At least one of the three bonds in the general formula (a1) is bonded to another structural unit, and at least one of the three bonds in the general formula (a2) is bonded to another structural unit. Among the bonds in each formula, the bond that is not bonded to a bond of another structural unit is bonded to a hydrogen atom. However, the benzene ring in the structural unit (a1) and the benzene ring in the structural unit (a2) are bonded via a methylene group, not directly bonded. Also, when the same molecule contains two or more structural units (a1) and the structural units (a1) are bonded to each other, the benzene ring in each structural unit (a1) is bonded via a methylene group, not directly bonded. Similarly, when the same molecule contains two or more structural units (a2) and the structural units (a2) are bonded to each other, the benzene ring in each structural unit (a2) is bonded via a methylene group, not directly bonded.
[0021] That is, the bond extending from the benzene ring in general formula (a1) is bonded to another structural unit or to a hydrogen atom. When bonded to another structural unit, the bond is bonded to a methylene group of the other structural unit (another structural unit (a1), or a structural unit (a2) in which at least one of m and n is 1). The bond extending from the methylene group in general formula (a1) bonds to a benzene ring of another structural unit (structural unit (a2) or another structural unit (a1)).
[0022] The bond extending from the benzene ring in general formula (a2) is bonded to another structural unit or to a hydrogen atom. When bonded to another structural unit, the bond is bonded to a methylene group of the other structural unit (structural unit (a1) or another structural unit (a2) in which at least one of m and n is 1). When m in the general formula (a2) is 0 (or n is 0), -(CH2) m -*(or -(CH2) nThe bond (-*) represents a bond (-*) similar to the bond extending from the benzene ring. That is, it is bonded to another structural unit or to a hydrogen atom. When it is bonded to another structural unit, the bond is bonded to a methylene group of the other structural unit, similar to the bond extending from the benzene ring. When m in the general formula (a2) is 1 (or n is 1), -(CH2) m -*(or -(CH2) n -*) is a methylene group, and its bond is bonded to a benzene ring of another structural unit (structural unit (a1) or another structural unit (a2)).
[0023] In the general formula (a1), R in the benzene ring 1 The bonding position of is preferably the ortho position (2-position or 6-position) relative to the bonding position of the hydroxyl group (1-position) from the viewpoints of low cost and ease of liquefaction of the synthesized resin. In this case, it is represented by the following general formula (a1-1) or (a1-2), respectively. [ka] (In the above general formulae (a1-1) and (a1-2), R 1 is R in the general formula (a1). 1 is the same as In addition, * in general formulae (a1-1) and (a1-2) is explained in the same manner as the above explanation for * in general formula (a1). In this specification, the description of the structural unit (a1) can be interpreted as the structural unit (a1-1) or the structural unit (a1-2).
[0024] In the general formula (a1), the bonding positions of the single bond and the methylene group in the benzene ring are not particularly limited, and are typically either the ortho position (2- or 6-position) or the para position (4-position) relative to the bonding position of the hydroxyl group (1-position).
[0025] In the above formula, R 1The aliphatic hydrocarbon group represented by may be any of a chain (straight-chain or branched-chain), a cyclic group, or a combination of a chain and a cyclic group, but is preferably a chain group, and more preferably a straight-chain group. The aliphatic hydrocarbon group may be either a saturated aliphatic hydrocarbon group having 1 to 9 carbon atoms or an unsaturated aliphatic hydrocarbon group having 2 to 9 carbon atoms. The saturated aliphatic hydrocarbon group having 1 to 9 carbon atoms is preferably a saturated aliphatic hydrocarbon group having 1 to 6 carbon atoms, more preferably a saturated aliphatic hydrocarbon group having 1 to 5 carbon atoms, and even more preferably a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms. The unsaturated aliphatic hydrocarbon group having 2 to 9 carbon atoms is preferably an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms, more preferably an unsaturated aliphatic hydrocarbon group having 2 to 4 carbon atoms, and even more preferably an unsaturated aliphatic hydrocarbon group having 3 carbon atoms, and particularly preferably an allyl group. R 1 The aliphatic hydrocarbon group represented by may have a substituent, and examples of the substituent include a hydroxyl group, a halogen atom, an oxygen-containing hydrocarbon group, and a nitrogen-containing cyclic group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the oxygen-containing hydrocarbon group include an ether bond-containing hydrocarbon group. Examples of the nitrogen-containing cyclic group include a pyridyl group, a pyrimidinyl group, a quinolinyl group, and an imidazolyl group.
[0026] R 1 The aromatic hydrocarbon group represented by may be an aromatic hydrocarbon group (aryl group) that does not contain a heteroatom, or may be a heteroaromatic hydrocarbon group (heteroaryl group) that contains a heteroatom, but is preferably an aromatic hydrocarbon group (aryl group) that does not contain a heteroatom. The aromatic hydrocarbon group has 5 to 15 ring atoms. In this specification, the "number of ring atoms" refers to the number of atoms (e.g., carbon atoms, nitrogen atoms, oxygen atoms, etc.) that form an aromatic ring, and does not include the number of atoms (e.g., hydrogen atoms, etc.) that substitute for the aromatic ring. The aromatic hydrocarbon group is preferably an aromatic hydrocarbon group having 5 to 12 ring atoms, more preferably an aromatic hydrocarbon group having 6 to 12 ring atoms, and even more preferably an aromatic hydrocarbon group having 6 to 10 ring atoms. The aromatic hydrocarbon group may have a substituent, and examples of the substituent include an aliphatic hydrocarbon group having 1 to 5 carbon atoms, a hydroxyl group, a halogen atom, etc. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0027] R 1 Examples of the combination of the aliphatic hydrocarbon group and the aromatic hydrocarbon group represented by the formula (I) include -aliphatic hydrocarbon group-aromatic hydrocarbon group, -aromatic hydrocarbon group-aliphatic hydrocarbon group, -aliphatic hydrocarbon group-aromatic hydrocarbon group-aliphatic hydrocarbon group, etc. Among these, -aliphatic hydrocarbon group-aromatic hydrocarbon group, so-called aralkyl group, is preferred. The aromatic hydrocarbon group and the aliphatic hydrocarbon group are preferably selected from the group consisting of the above-mentioned R 1 The aliphatic hydrocarbon group and the aromatic hydrocarbon group represented by the formula (I) are similar to those represented by the formula (I).
[0028] X is a hydrogen atom, a hydroxyl group or a hydroxylmethyl group, and is preferably a hydrogen atom or a hydroxymethyl group.
[0029] R 2 The aliphatic hydrocarbon group having 10 to 25 carbon atoms represented by R is explained in the same manner as the aliphatic hydrocarbon group having 10 to 25 carbon atoms contained in the above-mentioned phenolic resin (A-1). 2 is preferably substituted at the meta position (3-position or 5-position) relative to the position (1-position) to which the hydroxyl group of the phenol moiety is bonded, and in this case, is represented by the following general formula (a2-1) or (a2-2), respectively. [ka] (In the above general formulae (a2-1) and (a2-2), X and R 2 represents X and R in the general formula (a2). 2 is the same as In addition, * in general formulae (a2-1) and (a2-2) is explained in the same manner as the above explanation for * in general formula (a2). In this specification, the description of the structural unit (a2) can be interpreted as the structural unit (a2-1) or the structural unit (a2-2).
[0030] When the phenolic resin (A-1) has a structural unit (a1), the structural unit (a1) may be one type or two or more types. When the phenolic resin (A-1) has a structural unit (a2), the structural unit (a2) may be one type or two or more types. In other words, the phenolic resin (A-1) has several types of R 1 or several kinds of R 2 However, it is preferable that each of them is one kind.
[0031] In the phenolic resin (A-1), the molar ratio of the structural unit (a1) to the structural unit (a2) (structural unit (a1) / structural unit (a2)) is preferably 0 to 5.0, more preferably 0.25 to 5.0, even more preferably 1.0 to 3.0, and particularly preferably 1.0 to 2.0, from the viewpoints of reactivity with the thermosetting resin (B) described below, as well as low elasticity and low moisture absorption.
[0032] (Physical properties of phenolic resin (A-1)) From the viewpoint of compatibility, the weight average molecular weight (Mw) of the phenolic resin (A-1) is preferably 4,000 or less, more preferably 1,000 to 3,500, and even more preferably 2,000 to 3,000. By making the weight average molecular weight of the phenolic resin (A-1) 1,000 or more, the reactivity with the thermosetting resin (B) described later tends to be excellent, the heat resistance is not impaired, and the melt viscosity can be maintained. In the present specification, the weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC) analysis using tetrahydrofuran (THF) as a dissolving solution, and is a standard polystyrene equivalent value. More specifically, the weight average molecular weight (Mw) is measured according to the method described in the Examples. From the viewpoint of improving the glass transition temperature and the electrical insulation reliability, the hydroxyl equivalent of the phenolic resin (A-1) is preferably 90 to 350 g / eq, more preferably 95 to 300 g / eq, still more preferably 100 to 250 g / eq, and particularly preferably 100 to 160 g / eq. The hydroxyl equivalent is measured according to the method described in the Examples.
[0033] (Production method of phenolic resin (A-1)) The method for producing the phenolic resin (A-1) is not particularly limited, and a known method for producing a phenolic resin can be adopted. For example, the method for producing a polyhydric hydroxyl resin described in JP 2015-89940 A can be referred to and applied. One preferred embodiment of the production method includes, for example, a method in which a phenolic compound represented by the following general formula (2) is reacted with formaldehyde in the presence of a basic catalyst, and the resulting product is reacted with a phenolic compound represented by the following general formula (1), preferably in the presence of an acidic catalyst. The phenolic compound represented by the following general formula (1) forms the structural unit (a1), and the phenolic compound represented by the following general formula (2) forms the structural unit (a2). [ka] (R in the above general formula (1) 1 R in the general formula (a1) 1 is the same as R in the above general formula (2). 2 and X is R in the general formula (a2). 2 and X.)
[0034] (Phenol resin (A-1) content) The content of the phenolic resin (A-1) is preferably 0.1 to 40 parts by mass relative to 100 parts by mass of the total amount of the resin components of the thermosetting resin composition of the present invention. By making the content of the phenolic resin (A-1) 0.1 parts by mass or more relative to 100 parts by mass of the total amount of the resin components of the thermosetting resin composition, it becomes easy to obtain low elasticity and high elongation, which are characteristics of the phenolic resin (A-1), and by making it 40 parts by mass or less, it tends to be possible to suppress a decrease in glass transition temperature (Tg), a decrease in flame retardancy, and an increase in tackiness. From the same viewpoint, the content of the phenolic resin (A-1) is more preferably 5 to 40 parts by mass, further preferably 5 to 25 parts by mass, and particularly preferably 5 to 15 parts by mass, based on 100 parts by mass of the total amount of the resin components in the thermosetting resin composition. In this specification, the "total amount of resin components" means the total amount of the filler (D) described below that can be contained as necessary and other components excluding organic solvents.
[0035] ((A-2): Phenolic resin having no aliphatic hydrocarbon group having 10 to 25 carbon atoms) The phenolic resin (A) may further contain (A-2) a phenolic resin having no aliphatic hydrocarbon group having 10 to 25 carbon atoms [hereinafter, sometimes referred to as phenolic resin (A-2)], and from the viewpoint of ensuring adhesive strength with the metal foil, it is preferable that the phenolic resin (A-2) is contained. The aliphatic hydrocarbon group having 10 to 25 carbon atoms is explained in the same manner as in the phenolic resin (A-1) above. The phenolic resin (A-2) may be a known phenolic resin that does not have an aliphatic hydrocarbon group having a carbon number of 10 to 25. Among them, from the viewpoint of low moisture absorption, phenol novolac resin, cresol novolac type phenolic resin, biphenyl novolac type phenolic resin, etc. are preferred, and cresol novolac type phenolic resin is more preferred.
[0036] (Physical properties of phenolic resin (A-2)) The hydroxyl equivalent of the phenolic resin (A-2) is preferably 80 to 300 g / eq, more preferably 80 to 200 g / eq, and even more preferably 80 to 150 g / eq, from the viewpoints of improving the glass transition temperature and improving the electrical insulation reliability.
[0037] As the phenolic resin (A-2), commercially available products may be used, such as a cresol novolac phenolic resin "KA-1165" (manufactured by DIC Corporation, product name) and a biphenyl novolac phenolic resin "MEH-7851" (manufactured by Meiwa Chemical Industry Co., Ltd., product name).
[0038] The content ratio of the phenolic resin (A-1) to the total amount of the phenolic resin (A-1) and the phenolic resin (A-2) is preferably 30 to 95% by mass. By setting it within this range, there is a tendency that high adhesive strength with the metal foil can be obtained while having low elasticity, high heat resistance, and high elongation. From the same viewpoint, it is more preferably 50 to 95% by mass, further preferably 60 to 95% by mass, and particularly preferably 70 to 90% by mass.
[0039] [(B): Thermosetting resin] The thermosetting resin composition of the present invention may further contain a thermosetting resin (sometimes referred to as thermosetting resin (B)) as component (B), and from the viewpoints of heat resistance, electrical insulation reliability, and high glass transition temperature, it is preferable that the thermosetting resin (B) is contained. However, the component (B) does not contain the component (A). As the thermosetting resin (B), a known thermosetting resin can be used, and is not particularly limited, but is preferably at least one selected from the group consisting of, for example, epoxy resins, cyanate resins, bismaleimide compounds, addition polymers of bismaleimide compounds and diamines, isocyanate resins, triallyl isocyanurate resins, triallyl cyanurate resins, and vinyl group-containing polyolefins. Among these, from the viewpoint of the balance of performance such as heat resistance and electrical insulation reliability, epoxy resins and cyanate resins are preferred, and epoxy resins are more preferred.
[0040] As the epoxy resin, from the viewpoint of improving heat resistance and glass transition temperature, it is preferable to use an epoxy resin having two or more epoxy groups in one molecule. Here, epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferable. As the epoxy resin, known ones can be used. Among them, it is preferable to use at least one selected from the group consisting of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, biphenyl type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, phosphorus-containing epoxy resin, naphthalene skeleton-containing epoxy resin, aralkylene skeleton-containing epoxy resin, phenol biphenyl aralkyl type epoxy resin, phenol salicylaldehyde novolac type epoxy resin, lower alkyl group-substituted phenol salicylaldehyde novolac type epoxy resin, dicyclopentadiene skeleton-containing epoxy resin, polyfunctional glycidylamine type epoxy resin, polyfunctional alicyclic epoxy resin, and tetrabromobisphenol A type epoxy resin.
[0041] The weight average molecular weight (Mw) of the epoxy resin is preferably 200 to 1,000, and more preferably 300 to 900. When the weight average molecular weight is 200 or more, heat resistance tends to be improved, and when it is 1,000 or less, compatibility with the (A) component tends to be good. From the viewpoint of compatibility, the epoxy equivalent of the epoxy resin is preferably 150 to 500 g / eq, more preferably 150 to 450 g / eq, and even more preferably 150 to 300 g / eq.
[0042] As the epoxy resin, a commercially available product may be used. Examples of commercially available products include bisphenol A type epoxy resin "jER1001" (manufactured by Mitsubishi Chemical Corporation, product name), phenol novolac type epoxy resin "N770" (manufactured by DIC Corporation, product name), phenol biphenyl aralkyl type epoxy resin "NC-3000H" (manufactured by Nippon Kayaku Co., Ltd., product name), cresol novolac type epoxy resin "EPICLON N-660" (manufactured by DIC Corporation, product name), phosphorus-containing epoxy resin "ZX-1548" (manufactured by Tohto Kasei Co., Ltd., product name), naphthalene skeleton-containing epoxy resin "HP-9900" (manufactured by DIC Corporation, product name), tetrabromobisphenol A type epoxy resin "EPICLON 153" (manufactured by DIC Corporation, product name), and the like.
[0043] The cyanate resin may be a known one. Examples of the cyanate resin include novolac type cyanate resin, bisphenol A type cyanate resin, bisphenol E type cyanate resin, bisphenol F type cyanate resin, tetramethylbisphenol F type cyanate resin, and dicyclopentadiene type cyanate resin. The cyanate resin may be used alone or in combination of two or more types. As for the thermosetting resins other than those exemplified as the thermosetting resin (B), known resins can also be used.
[0044] (B) Component Content When the thermosetting resin composition of the present invention contains the (B) component, the content of the (B) component is preferably 40 to 90 parts by mass, more preferably 50 to 90 parts by mass, and even more preferably 60 to 80 parts by mass, per 100 parts by mass of the total amount of the resin components in the thermosetting resin composition. Furthermore, although there are no particular limitations, it is preferable to adjust the number of phenolic hydroxyl groups in component (A) to 0.5 to 1.5 equivalents relative to the functional groups (eg, epoxy groups) in component (B). By ensuring that the content of component (B) is within the above range, there is a tendency for the adhesive strength with the metal foil to be maintained, and for the deterioration of the glass transition temperature and the electrical insulation reliability to be suppressed.
[0045] [(C): Curing accelerator] The thermosetting resin composition of the present invention may contain, and preferably contains, a curing accelerator (sometimes referred to as curing accelerator (C)) as component (C). The curing accelerator (C) may be appropriately selected depending on the type of thermosetting resin (B), and one type may be used alone, or two or more types may be used in combination. For example, when an epoxy resin is used as the thermosetting resin (B), although there are no particular limitations, it is preferable that the resin contains at least one selected from the group consisting of an amine compound and an imidazole compound, and it is more preferable that the resin contains an imidazole compound. Examples of the amine compound include dicyandiamide, diaminodiphenylethane, and guanylurea. Examples of the imidazole compound include 2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, and benzimidazole. When the thermosetting resin composition of the present invention contains a curing accelerator (C), the content of the curing accelerator (C) is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, further preferably 0.01 to 3 parts by mass, and particularly preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the total amount of the resin components of the thermosetting resin composition. When an epoxy resin is contained as the (B) thermosetting resin, the content of the (D) curing accelerator can also be determined depending on the total amount of oxirane rings in the thermosetting resin composition.
[0046] [(D): Filler] The thermosetting resin composition of the present invention can contain, and preferably contains, a filler (sometimes referred to as filler (D)) as component (D). The filler may be used alone or in combination of two or more kinds. The filler (D) is not particularly limited, and known fillers can be used. The filler (D) may be an organic filler or an inorganic filler. From the viewpoint of low thermal expansion coefficient and flame retardancy, it is preferable that the filler (D) contains an inorganic filler. The inorganic filler may be used alone or in combination of two or more kinds. Examples of inorganic fillers include silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (calcined clay, etc.), talc, aluminum borate, and silicon carbide. Among these, silica is more preferred from the viewpoint of low dielectric constant and low linear expansion coefficient. Examples of silica include precipitated silica produced by a wet method and having a high water content, and dry method silica produced by a dry method and containing almost no bound water, and examples of dry method silica include crushed silica, fumed silica, and fused silica (fused spherical silica) depending on the production method. Among these, fused silica (fused spherical silica) and crushed silica are more preferred as silica.
[0047] The shape and particle size of the filler (D) are not particularly limited, but for example, the average particle size is preferably 0.1 to 10 μm, more preferably 0.1 to 4.0 μm. When the average particle size is 0.1 μm or more, the dispersibility of the fillers is good, and the viscosity of the varnish is reduced, which tends to improve the handling property. In addition, when the average particle size is 10 μm or less, the filler (D) tends not to settle during varnish formation. Here, the average particle size refers to the particle size at the point corresponding to 50% volume when the cumulative frequency distribution curve of the particle size is calculated with the total volume of the particles being 100%, and can be measured by a particle size distribution measuring device using a laser diffraction scattering method, etc.
[0048] When the thermosetting resin composition of the present invention contains a filler (D), the content of the filler (D) is preferably 5 to 40 parts by mass, more preferably 10 to 40 parts by mass, and even more preferably 15 to 35 parts by mass, based on 100 parts by mass of the total amount of the resin components of the thermosetting resin composition. When the content of the filler (D) is 5 parts by mass or more, the linear expansion coefficient is low, sufficient heat resistance is obtained, and low tackiness tends to be obtained. When the content of the filler (D) is 40 parts by mass or less, the cured product of the resin composition is less likely to become brittle, and the effect of low elasticity of the phenolic resin (A-1) tends to be sufficiently obtained.
[0049] [Other ingredients] The thermosetting resin composition of the present invention may contain, as necessary, a curing agent (excluding the above-mentioned component (A)); a crosslinking agent such as isocyanate or melamine; a rubber-based elastomer; a flame retardant such as a phosphorus-based compound; conductive particles; a coupling agent; a flow control agent; an antioxidant; a pigment; a leveling agent; an antifoaming agent; an ion trapping agent, etc. Any of these may be used that are known in the art. The inclusion of a coupling agent is preferable because it improves the dispersibility of the filler (D) and improves the adhesion of the prepreg to the substrate and to the metal foil. As the coupling agent, a silane coupling agent is preferable, and examples of the silane coupling agent include an epoxy silane coupling agent, an amino silane coupling agent, a vinyl silane coupling agent, a phenyl silane coupling agent, an alkyl silane coupling agent, an alkenyl silane coupling agent, an alkynyl silane coupling agent, a haloalkyl silane coupling agent, a siloxane coupling agent, a hydrosilane coupling agent, a silazane coupling agent, an alkoxy silane coupling agent, a chlorosilane coupling agent, a (meth)acryl silane coupling agent, an isocyanurate silane coupling agent, a ureido silane coupling agent, a mercapto silane coupling agent, a sulfide silane coupling agent, and an isocyanate silane coupling agent. Among these, an epoxy silane coupling agent is preferable. The coupling agent may be used alone or in combination of two or more. When the thermosetting resin composition of the present invention contains a coupling agent, the content thereof is preferably 0.01 to 20 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.05 to 2 parts by mass, relative to 100 parts by mass of the total amount of the resin components of the thermosetting resin. In addition, when the thermosetting resin composition of the present invention contains components other than the coupling agent, the content thereof may be appropriately adjusted depending on the purpose.
[0050] [Organic Solvent] The thermosetting resin composition of the present invention may contain an organic solvent from the viewpoint of facilitating handling by dilution and from the viewpoint of facilitating production of the prepreg described below. A thermosetting resin composition containing an organic solvent may be called a varnish. The organic solvent may be the organic solvent used in producing the (A) component or the (B) component that is contained in the thermosetting resin composition of the present invention as it is, or may be a newly added organic solvent, and there is no particular limitation. The organic solvent is not particularly limited, but may be a ketone solvent, an aromatic hydrocarbon solvent, an ester solvent, an amide solvent, an alcohol solvent, or the like. Specifically, the ketone solvent may be acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, or the like. The aromatic hydrocarbon solvent may be toluene, xylene, or the like. The ester solvent may be methoxyethyl acetate, ethoxyethyl acetate, butoxyethyl acetate, or the like. The amide solvent may be N-methylpyrrolidone, formamide, N-methylformamide, or N,N-dimethylacetamide, or the like. The alcohol solvent may be methanol, ethanol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monopropyl ether, or the like. The organic solvents may be used alone or in combination of two or more kinds. Among these, ketone-based solvents are preferred from the viewpoint of solubility. From the viewpoints of handling, impregnation into the base material of the prepreg, and the appearance of the prepreg, the varnish preferably has a non-volatile content concentration of 25 to 65 mass %. In this specification, the term "non-volatile content" refers to components remaining when the organic solvent contained in the thermosetting resin composition is removed, and includes the filler (D).
[0051] [Prepreg] The present invention also provides a prepreg containing the thermosetting resin composition of the present invention. The prepreg of the present invention is obtained by impregnating a substrate with the thermosetting resin composition of the present invention and drying it. The substrate is not particularly limited as long as it is a substrate used in manufacturing a metal-clad laminate or a printed wiring board, but a fiber substrate such as a woven fabric or a nonwoven fabric is usually used. Examples of the material of the fiber substrate include inorganic fibers such as glass, alumina, asbestos, boron, silica alumina glass, silica glass, Tyranno, silicon carbide, silicon nitride, and zirconia, organic fibers such as aramid, polyether ether ketone, polyether imide, polyether sulfone, carbon, and cellulose, and fibers made by mixing these. As the fiber substrate, a glass cloth having a thickness of 160 μm or less (preferably 10 to 160 μm, more preferably 10 to 100 μm, and even more preferably 20 to 50 μm) is preferably used. Furthermore, it is more preferable to use a glass cloth having a thickness of 50 μm or less, since this makes it possible to obtain a printed wiring board that can be bent as desired and to reduce dimensional changes caused by temperature, moisture absorption, etc. during the manufacturing process.
[0052] There are no particular limitations on the manufacturing conditions for the prepreg, but it is preferable to obtain the prepreg by volatilizing 80% by mass or more of the organic solvent contained in the varnish. The drying temperature is preferably 80 to 180°C, more preferably 110 to 160°C, and the drying time is appropriately set in consideration of the gelling time of the varnish. It is preferable that the prepreg thus obtained has a non-volatile content of the varnish of 30 to 80% by mass relative to the total amount of the non-volatile content of the varnish and the substrate.
[0053] [Metal foil with resin] The present invention also provides a resin-attached metal foil obtained by laminating the thermosetting resin composition of the present invention and a metal foil. The resin-attached metal foil can be produced, for example, by coating the thermosetting resin composition (varnish) of the present invention on a metal foil and drying it. The drying conditions are not particularly limited, but the drying can be preferably performed at 80 to 180°C, more preferably 110 to 160°C. There is no particular limitation on the coating method, and any known coating machine such as a die coater, a comma coater, a bar coater, a kiss coater, or a roll coater can be used.
[0054] [Laminate] The present invention also provides a laminate comprising the prepreg of the present invention or the resin-coated metal foil of the present invention. The laminate of the present invention is produced by laminating a plurality of prepregs of the present invention and applying heat and pressure thereto. The laminate of the present invention may be a laminate of a laminate made of a plurality of prepregs different from the present invention and a laminate made of a plurality of prepregs of the present invention. An example of a laminate made of a plurality of prepregs different from the present invention is a laminate having a higher storage modulus than the laminate made of a plurality of prepregs of the present invention. Since the laminate made of a plurality of prepregs of the present invention provides a stress relaxation effect, this embodiment can suppress the occurrence of cracks in the printed wiring board that may occur when only a laminate made of a plurality of prepregs different from the present invention is used.
[0055] In particular, a metal-clad laminate can be produced, for example, by overlapping the adhesive surfaces on both sides of the laminate with metal foil, and then heating and press-molding under vacuum press conditions, preferably at 130 to 250°C, more preferably at 150 to 230°C, and preferably at 0.5 to 10 MPa, more preferably at 1 to 5 MPa. Alternatively, the metal-clad laminate can be produced by stacking the resin-coated metal foils of the present invention so that their resin surfaces face each other and pressing them under vacuum press conditions. The heating and pressing method is not particularly limited, and for example, a multi-stage press, a multi-stage vacuum press, a continuous molding machine, an autoclave molding machine, etc. can be used.
[0056] The metal foil used in the resin-coated metal foil and the metal-clad laminate of the present invention is not particularly limited, but for example, copper foil and aluminum foil are generally used. The thickness of the metal foil is also not particularly limited, and can be selected from 1 to 200 μm, which is the thickness of the metal foil usually used in the laminate, preferably 10 to 100 μm, more preferably 10 to 50 μm. In addition, for example, a three-layer composite foil can be used in which an intermediate layer is made of nickel, nickel-phosphorus, nickel-tin alloy, nickel-iron alloy, lead, lead-tin alloy, or the like, and a copper layer of 0.5 to 15 μm and a copper layer of 10 to 300 μm are provided on both sides of the intermediate layer, or a two-layer composite foil made of aluminum and copper foil can be used.
[0057] (Storage modulus) The storage modulus of the cured product (laminate) obtained from the resin composition of the present invention is preferably 4.0×10 9 Pa or less is preferable, and 2.0×10 9 Pa or less is more preferable, and 1.9×10 9 Pa or less is more preferable, and 1.8×10 9 The lower limit of the storage modulus is not particularly limited, and is preferably 1.0×10 Pa or less. 9 Pa, 1.1 x 10 9 Pa, 1.2 x 10 9 It may be Pa. (Tensile elongation) The tensile elongation of the cured product (laminate) obtained from the resin composition of the present invention at room temperature (here, 25° C.) is preferably 3.0% or more, more preferably 3.2% or more, and even more preferably 3.5% or more, from the viewpoint of exerting a stress relaxation effect. There is no particular upper limit, but it is usually 6.0% or less, and may be 5.0% or less. Moreover, the tensile elongation in a high-temperature environment (here, 125°C) is preferably 5.0% or more, more preferably 5.4% or more, even more preferably 5.7% or more, particularly preferably 6.0% or more, and most preferably 6.5% or more, from the viewpoint of exerting a stress relaxation effect in a high-temperature environment and of restoring ability against thermal expansion when a temperature change occurs between a normal temperature environment and a high-temperature environment. There is no particular upper limit, but it is usually 12.0% or less, and may be 11.0% or less. The storage modulus and tensile elongation can be measured by the method described in the examples.
[0058] (Adhesion to metal foil) In the cured product (metal-clad laminate) obtained from the resin composition of the present invention, the adhesion to a metal foil at 25° C. is preferably 0.80 kN / m or more, more preferably 1.0 kN / m or more, even more preferably 1.20 kN / m or more, and particularly preferably 1.30 kN / m or more, when measured according to the method described in the Examples. There is no particular upper limit, but it is usually 2.0 kN / m or less, and may be 1.80 kN / m or less. The adhesiveness to the metal foil at 125° C. is preferably 0.40 kN / m or more, more preferably 0.50 kN / m or more, even more preferably 0.60 kN / m or more, and particularly preferably 0.70 kN / m or more. There is no particular upper limit, but it is usually 1.50 kN / m or less, and may be 1.30 kN / m or less, or may be 1.0 kN / m or less.
[0059] [Printed wiring board] The present invention also provides a printed wiring board containing the laminate of the present invention. The printed wiring board of the present invention is obtained by forming a circuit on the laminate of the present invention. The method for producing the printed wiring board of the present invention is not particularly limited, but it can be produced, for example, by performing circuit (wiring) processing on the metal foil of the laminate (metal-clad laminate) of the present invention having metal foil on one or both sides. The printed wiring board of the present invention may be a flexible printed wiring board.
[0060] [Semiconductor package] The semiconductor package of the present invention contains the printed wiring board of the present invention, and more specifically, is a package in which a semiconductor is mounted on the printed wiring board of the present invention. The semiconductor package of the present invention can be manufactured by mounting a semiconductor chip, a memory, etc., at a predetermined position on the printed wiring board of the present invention. EXAMPLES
[0061] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0062] [Synthesis Example 1] Production of phenolic resin (A-1) (Synthesis of phenolic resin (A-1-a)) A 2L glass flask equipped with a thermometer, a stirrer and a cooling tube was charged with 300g (1.0mol) of cardanol, 150g of methanol and 120g (2.0mol) of 50% aqueous formaldehyde solution, and 30% aqueous sodium hydroxide solution was dropped into the mixture over 2 hours. The temperature was then raised to 45°C and reacted for 6 hours. Next, 35% hydrochloric acid was added to the resulting reaction solution to neutralize the sodium hydroxide, and then 1,342g (10mol) of o-allylphenol was added, and 1.34g (0.1% by mass relative to o-allylphenol) of oxalic acid was added to make the system acidic, and the temperature was raised to 100°C and the reaction was carried out for 5 hours. After that, the reaction solution was washed with water, and the excess o-allylphenol was distilled off to obtain a phenolic resin (A-1-a). The weight average molecular weight (Mw) of the obtained phenolic resin (A-1-a) was 1,412, and the hydroxyl equivalent was 214 g / eq.
[0063] Here, the weight average molecular weight was calculated from a calibration curve using standard polystyrene by gel permeation chromatography (GPC). The calibration curve was approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Type; A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by Tosoh Corporation, product name]. The measurement conditions for GPC are shown below. Device: Pump: L-6200 type [manufactured by Hitachi High-Technologies Corporation] Detector: L-3300 type RI [Hitachi High-Technologies Corporation] Column oven: L-655A-52 [Hitachi High-Technologies Corporation] Column: Guard column: TSK Guardcolumn HHR-L + column: TSKgel G4000HHR + TSKgel G2000HHR (all product names manufactured by Tosoh Corporation) Column size: 6.0mm x 40mm (guard column), 7.8mm x 300mm (column) Eluent: Tetrahydrofuran Sample concentration: 30mg / 5mL Injection volume: 20μL Flow rate: 1.00mL / min Measurement temperature: 40℃
[0064] The hydroxyl equivalent weight (g / eq) of the phenolic resin was determined by titration using an automatic titration device "COM-1700S" (Hiranuma Sangyo Co., Ltd.) by the acetylation method with acetic anhydride.
[0065] [Synthesis Example 2] Production of phenolic resin (A-1) (Synthesis of phenolic resin (A-1-b)) In a 2L glass flask equipped with a thermometer, a stirrer and a cooling tube, 248g (1.0mol) of p-(4-pentylcyclohexyl)phenol, 150g of methanol and 120g (2.0mol) of 50% aqueous formaldehyde solution were charged, and 30% aqueous sodium hydroxide solution was dropped into the mixture over 2 hours. The temperature was then raised to 45°C and reacted for 6 hours. Next, 35% hydrochloric acid was added to the resulting reaction solution to neutralize the sodium hydroxide, and then 1,342g (10mol) of o-allylphenol was added, and 1.34g (0.1% by mass relative to o-allylphenol) of oxalic acid was added to make the system acidic, and the temperature was raised to 100°C and the reaction was carried out for 5 hours. After that, the reaction solution was washed with water, and the excess o-allylphenol was distilled off to obtain a phenolic resin (A-1-b). The weight average molecular weight (Mw) of the obtained phenolic resin (A-1-b) was 1,738, and the hydroxyl equivalent was 238 g / eq. The methods for measuring the weight average molecular weight (Mw) and the hydroxyl equivalent were as described in Synthesis Example 1.
[0066] [Example 1] The phenolic resin (A-1-a) obtained in Synthesis Example 1 was used as component (A-1), a cresol novolac phenolic resin (manufactured by DIC Corporation, hydroxyl equivalent 119 g / eq) was used as component (A-2), a dicyclopentadiene epoxy resin (manufactured by DIC Corporation, epoxy equivalent 254 g / eq) was used as thermosetting resin (B), crushed silica (manufactured by Fukushima Ceramics Co., Ltd.) was used as filler (D), and "A-187" (manufactured by Momentive Performance Materials, Inc., product name) was used as coupling agent in the amounts shown in Table 1. The mixture was dissolved in methyl isobutyl ketone, and 2-methylimidazole was added as curing accelerator (C) according to Table 1 to obtain a varnish with a non-volatile content of 40 mass%.
[0067] [Example 2] The same procedure was carried out as in Example 1, except that the blending amounts of the (A-1) component and the (A-2) component were changed as shown in Table 1, to obtain a varnish having a non-volatile content of 40 mass %.
[0068] [Example 3] The same procedure was carried out as in Example 1, except that a tetrabromobisphenol A type epoxy resin (manufactured by DIC Corporation, epoxy equivalent: 400 g / eq) was used as the thermosetting resin (B) instead of the dicyclopentadiene type epoxy resin, to obtain a varnish having a non-volatile content of 40 mass%.
[0069] [Example 4] The same procedure was carried out as in Example 3, except that the blending amounts of components (A-1) and (A-2) were changed as shown in Table 1, to obtain a varnish with a non-volatile content of 40 mass %.
[0070] [Example 5] The same procedure was carried out as in Example 1, except that a naphthalene skeleton-containing novolac epoxy resin (manufactured by DIC Corporation) was used as the thermosetting resin (B) instead of the dicyclopentadiene epoxy resin, to obtain a varnish with a non-volatile content of 40 mass%.
[0071] [Example 6] The same procedure was carried out as in Example 5, except that the blending amounts of components (A-1) and (A-2) were changed as shown in Table 1, to obtain a varnish with a non-volatile content of 40 mass %.
[0072] [Example 7] The same procedure was carried out as in Example 1, except that a phenol novolac type epoxy resin (manufactured by DIC Corporation) was used as the thermosetting resin (B) instead of the dicyclopentadiene type epoxy resin, to obtain a varnish having a non-volatile content of 40 mass %.
[0073] [Example 8] The same procedure was carried out as in Example 7, except that the blending amounts of components (A-1) and (A-2) were changed as shown in Table 1, to obtain a varnish with a non-volatile content of 40 mass %.
[0074] [Example 9] The same procedure was carried out as in Example 1, except that a phenol biphenyl aralkyl type epoxy resin (manufactured by Nippon Kayaku Co., Ltd.) was used as the thermosetting resin (B) instead of the dicyclopentadiene type epoxy resin, to obtain a varnish having a non-volatile content of 40 mass%.
[0075] [Example 10] The same procedure was carried out as in Example 9, except that the blending amounts of components (A-1) and (A-2) were changed as shown in Table 1, to obtain a varnish with a non-volatile content of 40 mass %.
[0076] [Example 11] In Example 2, the same procedure was carried out except that the "phenolic resin (A-1-b) obtained in Synthesis Example 2" was used as the (A-1) component instead of the "phenolic resin (A-1-a) obtained in Synthesis Example 1," to obtain a varnish with a non-volatile content of 40 mass%.
[0077] [Example 12] In Example 4, the same procedure was performed as above except that the "phenolic resin (A-1-b) obtained in Synthesis Example 2" was used instead of the "phenolic resin (A-1-a) obtained in Synthesis Example 1" as the (A-1) component, to obtain a varnish with a non-volatile content of 40 mass%.
[0078] [Example 13] In Example 6, the same procedure was carried out except that the "phenolic resin (A-1-b) obtained in Synthesis Example 2" was used instead of the "phenolic resin (A-1-a) obtained in Synthesis Example 1" as the (A-1) component, to obtain a varnish with a non-volatile content of 40 mass%.
[0079] [Example 14] In Example 8, the same procedure was carried out except that the "phenolic resin (A-1-b) obtained in Synthesis Example 2" was used instead of the "phenolic resin (A-1-a) obtained in Synthesis Example 1" as the (A-1) component, to obtain a varnish with a non-volatile content of 40 mass%.
[0080] [Example 15] In Example 10, the same procedure was performed as above except that the "phenolic resin (A-1-b) obtained in Synthesis Example 2" was used instead of the "phenolic resin (A-1-a) obtained in Synthesis Example 1" as the (A-1) component, to obtain a varnish with a non-volatile content of 40 mass%.
[0081] [Example 16] The same procedure was carried out as in Example 15, except that the blending amounts of components (A-1) and (A-2) were changed as shown in Table 2, to obtain a varnish with a non-volatile content of 40 mass %.
[0082] [Examples 17 and 18] The same procedure was carried out as in Example 3, except that the amounts of the (A-1), (A-2) and (B) components were changed as shown in Table 2, to obtain a varnish with a non-volatile content of 40% by mass.
[0083] [Comparative Example 1] (A-1) No component A cresol novolac phenolic resin (manufactured by DIC Corporation, hydroxyl equivalent 119 g / eq) as component (A-2), a dicyclopentadiene epoxy resin (manufactured by DIC Corporation, epoxy equivalent 254 g / eq) as thermosetting resin (B), crushed silica (manufactured by Fukushima Ceramics Co., Ltd.) as filler (D), and "A-187" (manufactured by Momentive Performance Materials, Inc., product name) as coupling agent were mixed in the amounts shown in Table 2 and dissolved in methyl isobutyl ketone, and then 2-methylimidazole was added as curing accelerator (C) according to Table 2 to obtain a varnish with a non-volatile content of 40 mass%.
[0084] [Comparative Example 2] (A-1) No component The same procedure was carried out as in Comparative Example 1, except that a naphthalene skeleton-containing novolac epoxy resin (manufactured by DIC Corporation) was used as component (B) instead of the dicyclopentadiene epoxy resin, to obtain a varnish with a non-volatile content of 40 mass%.
[0085] [Comparative Example 3] (A-1) No component The same procedure was carried out as in Comparative Example 1, except that a phenol biphenyl aralkyl type epoxy resin (manufactured by Nippon Kayaku Co., Ltd.) was used as the component (B) instead of the dicyclopentadiene type epoxy resin, to obtain a varnish with a non-volatile content of 40 mass%.
[0086] Using the varnish prepared in each example, a prepreg, a resin-coated copper foil, and a copper-clad laminate were prepared by the following methods, and each was evaluated by the methods described below.
[0087] [Preparation of prepreg] The varnish prepared in each example was impregnated into a 0.028 mm thick glass cloth 1037 (trade name, manufactured by Asahi Schwebel Corporation), and then heated and dried at 140° C. for 10 minutes to obtain a prepreg.
[0088] [Preparation of resin-coated copper foil] The varnish prepared in each example was applied to a 35 μm thick electrolytic copper foil "YGP-35" (trade name, manufactured by Nippon Denkai Co., Ltd.) using a coater, and then dried with hot air at 140°C for approximately 6 minutes to prepare a resin-coated copper foil with a coating thickness of 50 μm.
[0089] [Preparation of copper-clad laminate] A 35 μm thick electrolytic copper foil “YGP-35” (product name, manufactured by Nippon Denkai Co., Ltd.) was placed on both sides of the four laminated prepregs so that the adhesive surfaces faced the prepregs, and a double-sided copper-clad laminate was produced under vacuum press conditions of 4 MPa at 200°C for 60 minutes. The resin-coated copper foils were stacked with the resin surfaces facing each other, and a double-sided copper-clad laminate was produced by vacuum pressing at 200° C. for 60 minutes at 4 MPa.
[0090] [Preparation of multilayer boards with core substrate] A circuit was formed by etching the copper foil of a 1.0 mm-thick glass epoxy copper-clad laminate "MCL-E-75G" (trade name, manufactured by Hitachi Chemical Co., Ltd.). Two layers of prepreg were sandwiched between the core board thus obtained and an 18 μm-thick electrolytic copper foil "YGP-18" (trade name, manufactured by Nippon Denkai Co., Ltd.), and a multilayer board was produced under vacuum press conditions of 4 MPa at 200°C for 60 minutes, and this was used as the multilayer board for evaluation.
[0091] [Evaluation methods for varnish, prepreg and copper-clad laminate] (1) Varnish properties (compatibility of each component) The prepared varnish was placed in a transparent container, and the appearance after 24 hours was visually observed to check for separation of the varnish and the presence or absence of sediment, and evaluated according to the following evaluation criteria. A indicates excellent varnish properties. The results are shown in Tables 1 and 2. A: The varnish color is uniform and not separated, and no sediment is visible. B: The varnish color is non-uniform and can be judged to have separated, or the accumulation of sediment can be visually confirmed.
[0092] (2) Varnish properties (viscosity) The prepared varnish was placed in a cup and the varnish temperature was adjusted to 30°C using a water bath, after which the viscosity of the varnish was calculated using a BL type viscometer (manufactured by Toki Sangyo Co., Ltd.). If the viscosity at 30°C is 800 mPa s or less, it can be determined that there are no problems with the production of prepregs. The results are shown in Tables 1 and 2.
[0093] (3) Appearance of prepreg (presence or absence of aggregates) The appearance of the prepreg was evaluated by observing the occurrence of agglomerates using a 20x magnifying glass and evaluating it according to the following evaluation criteria. The results are shown in Tables 1 and 2. A: No aggregates were observed. B: Aggregates are observed.
[0094] (4) Storage modulus The storage modulus was evaluated by stacking the resin-coated copper foils so that the resin surfaces faced each other to prepare a double-sided copper-clad laminate, which was then etched over the entire surface. The laminate was then cut into a width of 5 mm and a length of 30 mm, and the storage modulus was measured using a dynamic viscoelasticity measuring device (manufactured by UBM Co., Ltd.). The storage modulus at 25°C was 4.0×10 9 It was determined that if the elastic modulus is less than 2.0×10 Pa, the elastic modulus is sufficiently low, the stress relaxation effect can be achieved, and the occurrence of cracks in the printed wiring board can be suppressed. 9 From the same viewpoint as above, it is more preferable that the elastic modulus is not more than Pa. The results are shown in Tables 1 and 2.
[0095] (5) Tensile elongation (25℃ and 125℃) A double-sided copper-clad laminate was prepared by stacking resin-coated copper foils with the resin surfaces facing each other, and the laminate was then etched over the entire surface. The laminate was then cut to a width of 10 mm and a length of 100 mm, and the tensile elongation was measured at 25°C and 125°C using a thermostatic autograph (manufactured by Shimadzu Corporation). If the tensile elongation at 25°C is 3.0% or more and the tensile elongation at 125°C is 5.0% or more, the stress relaxation effect can be achieved, and the occurrence of cracks in the printed wiring board can be easily suppressed. The results are shown in Tables 1 and 2.
[0096] (6) Heat resistance A double-sided copper-clad laminate made from four layers of the prepreg was cut into a square of 50 mm on each side to obtain a test piece. The test piece was floated in a solder bath at 260°C, and the time elapsed from that point until the test piece was visually observed to bulge was measured and used as an index of heat resistance. The elapsed time was measured up to 300 seconds, and if 300 seconds or more had elapsed, it was determined that the heat resistance was sufficient. The results are shown in Tables 1 and 2.
[0097] (7) Adhesion to metal foil (25℃ and 125℃) The copper foil of the double-sided copper-clad laminate made from four layers of the prepreg was partially etched to form a 3 mm wide copper foil line. Next, a thermostatic chamber-mounted peel tester (manufactured by Shimadzu Corporation) was used to set the temperature at 25°C or 125°C, and the load when the copper foil line was peeled off at a speed of 50 mm / min in a 90° direction relative to the adhesive surface was measured and used as an index of copper foil peel strength. If the copper foil peel strength at 25°C was 0.80 kN / m or more and the copper foil peel strength at 125°C was 0.40 kN / m or more, it was determined that the adhesion to the metal foil was sufficient. The results are shown in Tables 1 and 2.
[0098] (8) Tackiness 50 sheets of prepregs cut into a square of 250 mm square were stacked and sandwiched between 270 mm square head plates. Furthermore, the same head plate was stacked on the upper head plate to produce a composition with a total weight of the upper head plate of 3 kg. Furthermore, this composition was sealed and packed in an aluminum moisture-proof bag, and then placed in a thermostatic chamber set at 30°C to investigate the number of days that elapsed until the prepregs began to adhere to each other, which was used as an index of the presence or absence of tackiness. The number of days that elapsed until the prepregs began to adhere to each other is preferably 2 days or more, and if it is 7 days or more (shown as >7 in the table), it was determined that the composition had sufficiently low tackiness. Low tackiness is preferable because it is easy to handle and can be stored in a state where the prepregs are stacked on each other. The results are shown in Tables 1 and 2.
[0099] (9) Crack resistance (solder crack resistance) The multilayer board for evaluation was etched to form a circuit, and electrodes for mounting chips were formed. Then, solder resist was formed, and flux was applied as a finishing process. Then, solder paste was applied to the electrodes, and a chip resistor (3226 size) was mounted on the electrodes, and the board was put into a reflow furnace to produce a mounting board. Next, the manufactured mounted board was placed in a temperature cycle tester and a heat cycle test was performed under a series of conditions in which -45°C and 125°C were held in air for 30 minutes each (however, the heating rate was 10°C / min and the cooling rate was 10°C / min), with one cycle being one cycle. The mounted board was removed every 500 cycles and the cross section was visually observed to check for the presence or absence of solder cracks. The evaluation was continued up to a maximum of 4,000 cycles, and the number of cycles until solder cracks occurred was investigated and used as an index of solder crack resistance. The criterion for determining whether solder cracks occurred was that a crack size of 50% or more of the connection length between the component and the solder was deemed to be a failure (i.e., solder cracks had occurred). The number of cycles is preferably 2,500 or more.
[0100] (10) Electrical insulation reliability A double-sided copper-clad laminate made from four layers of the prepreg was processed to have a through-hole wall spacing of 350 μm, and the insulation resistance of 400 holes for each sample was measured over time using a test pattern to determine the electrical insulation reliability. The measurement was performed under conditions of 85°C / 85%RH atmosphere with 100V applied, and the time until electrical breakdown occurred was measured. The measurement time was up to 2,000 hours, and it was determined that the electrical insulation reliability was sufficient if it was more than 2,000 hours.
[0101] [Table 1]
[0102] [Table 2]
[0103] As is clear from Tables 1 and 2, the examples exhibited excellent properties in all respects, including low elasticity, high heat resistance, high elongation, high electrical insulation reliability, high adhesive strength with metal foil, low tackiness, and no solder cracks. In addition, the resin compositions (varnishes) prepared in the examples had good varnish properties, and the appearance of the prepregs was also good. It is noted that in Examples 1 to 16 in which the content of the phenolic resin (A-1) was in the range of 0.1 to 40 parts by mass relative to 100 parts by mass of the total amount of the resin components, the low tackiness was even more excellent. On the other hand, in Comparative Examples 1 to 3, which used a thermosetting resin composition not containing the phenolic resin (A-1), none of them satisfied all of the requirements of low elasticity, high heat resistance, high elongation, high electrical insulation reliability, high adhesive strength with metal foil, and solder crack resistance. In particular, although they achieved high adhesive strength with metal foil, they were significantly lacking in low elasticity, high elongation, and solder crack resistance.
Claims
1. A thermosetting resin composition comprising (A) a phenolic resin and (B) a thermosetting resin, The component (A) is a thermosetting resin composition comprising (A-1) a phenolic resin having an aliphatic hydrocarbon group having 10 to 25 carbon atoms, the component (A-1) has a structural unit (a1) represented by the following general formula (a1) and a structural unit (a2) represented by the following general formula (a2), and the molar ratio of the structural unit (a1) to the structural unit (a2) (structural unit (a1) / structural unit (a2)) is 0.25 to 5.0, The content of the (A-1) component is 0.1 to 40 parts by mass relative to 100 parts by mass of the total amount of the resin components of the thermosetting resin composition; The thermosetting resin composition (B) is at least one selected from the group consisting of an epoxy resin, a cyanate resin, a bismaleimide compound, an addition polymer of a bismaleimide compound and a diamine, an isocyanate resin, a triallyl isocyanurate resin, a triallyl cyanurate resin, and a vinyl group-containing polyolefin. 【Chemistry 1】 (In the above general formula, R 1 represents an unsaturated aliphatic hydrocarbon group having 2 to 9 carbon atoms which may have a substituent, R 2 represents an aliphatic hydrocarbon group having 10 to 25 carbon atoms; X represents a hydrogen atom, a hydroxyl group, or a hydroxylmethyl group; m and n each independently represent 0 or 1.
2. In the general formula (a1), R 1 The thermosetting resin composition according to claim 1, wherein is an unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms which may have a substituent.
3. The thermosetting resin composition according to claim 1, wherein the molar ratio of the structural unit (a1) to the structural unit (a2) (structural unit (a1) / structural unit (a2)) is 1.0 to 3.
0.
4. The thermosetting resin composition according to any one of claims 1 to 3, wherein the weight average molecular weight (Mw) of the component (A-1) is 4,000 or less.
5. The thermosetting resin composition according to any one of claims 1 to 4, wherein the hydroxyl equivalent of the component (A-1) is 90 to 350 g / eq.
6. The thermosetting resin composition according to claim 1, wherein the structural unit (a1) is represented by the following general formula (a1-1) or (a1-2), and the structural unit (a2) is represented by the following general formula (a2-1) or (a2-2): 【Chemistry 2】 (In the above formula, R 1 , R 2 , X, m and n are as defined above.
7. The thermosetting resin composition according to any one of claims 1 to 6, wherein the component (A) further comprises (A-2) a phenolic resin having no aliphatic hydrocarbon group having 10 to 25 carbon atoms.
8. The thermosetting resin composition according to claim 7, wherein the content of the component (A-1) relative to the total amount of the component (A-1) and the component (A-2) is 30 to 95 mass%.
9. A prepreg comprising the thermosetting resin composition according to any one of claims 1 to 8.
10. A resin-coated metal foil, comprising the thermosetting resin composition according to any one of claims 1 to 8 laminated with a metal foil.
11. A laminate comprising the prepreg according to claim 9 or the resin-coated metal foil according to claim 10.
12. A printed wiring board comprising the laminate according to claim 11.
13. A semiconductor package comprising the printed wiring board according to claim 12.
Citation Information
Patent Citations
Adhesive composition for flexible printed circuit board
JP1996283535A
Production of resol resin
JP2000026563A
Flexible printed wiring board and copper-clad laminate therefor
JP2002134907A
Electrical insulating resin composition for multilayer printed wiring board, multilayer printed wiring board using the same, and method for producing the board using the same
JP2002371190A
Epoxy resin composition having improved low-temperature curability, and its manufacturing method and intermediate.
JP2011516662A