Vertical-cavity surface-emitting laser

The vertical cavity surface emitting laser design addresses oxidation issues by using a cap layer with low aluminum composition and specific refractive index configurations to enhance reliability and performance.

JP7563186B2Active Publication Date: 2024-10-08SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021002687
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-12
Publication Date
2024-10-08
Estimated Expiration
2041-01-12

AI Technical Summary

Technical Problem

The AlAs layer in vertical cavity surface emitting lasers is susceptible to oxidation due to its large aluminum composition, which can lead to natural oxidation during manufacturing, affecting the reliability and performance of the device.

Method used

A vertical cavity surface emitting laser design that includes a first lower distributed Bragg reflector extending to the edge of the substrate, covered by a cap layer with a lower aluminum composition, and a III-V compound semiconductor layer with specific refractive index relationships to minimize oxidation and thermal resistance.

Benefits of technology

The design effectively prevents oxidation of the AlAs layer, enhances reliability, and reduces thermal resistance, allowing for expanded modulation bandwidth and maintained optical output even with increased current injection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563186000001
    Figure 0007563186000001
  • Figure 0007563186000002
    Figure 0007563186000002
  • Figure 0007563186000003
    Figure 0007563186000003
Patent Text Reader

Abstract

To provide a vertical resonance type surface emitting laser in which a layer having a relatively large aluminum composition is hard to be oxidized.SOLUTION: A vertical resonance type surface emitting laser 10 comprises: a substrate 12 including a principal surface; a first lower distribution Bragg reflector 14 extending to an edge of the principal surface; a group III-V compound semiconductor layer 16 provided on the first lower distribution Bragg reflector; a second lower distribution Bragg reflector 18 provided on the group III-V compound semiconductor layer; an active layer 20 provided on the second lower distribution Bragg reflector; and an upper distribution Bragg reflector 22 provided on the active layer. The first lower distribution Bragg reflector includes first layers 14a and second layers 14b which are alternately arrayed. The upper distribution Bragg reflector includes third layers 22a and fourth layers 22b which are alternately arrayed. The group III-V compound semiconductor layer does not contain aluminum or has an aluminum composition smaller than that of the third layer. The first layer has an aluminum composition larger than that of the third layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to vertical-cavity surface-emitting lasers. [Background technology]

[0002] Non-Patent Document 1 discloses a vertical-cavity surface-emitting laser provided on a GaAs substrate and having a lower distributed Bragg reflector including alternating AlAs and GaAs layers. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] M. Gbski, P.-S. Wong, M. Riaziat, and JA Lott, “30 GHz bandwidthtemperature stable 980 nm vertical-cavity surface-emitting lasers withAlAs / GaAs bottom distributed Bragg reflectors for optical data communication,”J. Phys. Photonics, vol. 2, no. 3, p. 035008, Jul. 2020, doi:10.1088 / 2515-7647 / ab9420. Summary of the Invention [Problem to be solved by the invention]

[0004] The AlAs layer is easily oxidized due to its large aluminum content. In the vertical-cavity surface-emitting laser, the end faces of the AlAs layer are exposed during the manufacturing process, and the AlAs layer may be naturally oxidized near the end faces.

[0005] The present disclosure provides a vertical-cavity surface-emitting laser in which layers having a relatively large aluminum composition are less susceptible to oxidation. [Means for solving the problem]

[0006] A vertical-cavity surface-emitting laser according to one aspect of the present disclosure includes a substrate having a main surface including a first area and a second area surrounding the first area, a first lower distributed Bragg reflector provided on the first area and the second area and extending to an edge of the main surface, a III-V compound semiconductor layer provided on the first lower distributed Bragg reflector, a second lower distributed Bragg reflector provided on the III-V compound semiconductor layer, an active layer provided on the second lower distributed Bragg reflector, and an upper distributed Bragg reflector provided on the active layer, wherein the III-V compound semiconductor layer is provided on the first area and the second area, the second lower distributed Bragg reflector is provided on the first area, and the first lower distributed Bragg reflector is provided on the active layer. the reflector comprises alternating first and second layers, the first layer having a refractive index lower than that of the second layer and the first layer comprising a III-V compound semiconductor containing aluminum; the upper distributed Bragg reflector comprises alternating third and fourth layers, the third layer having a refractive index lower than that of the fourth layer and the third layer comprising a III-V compound semiconductor containing aluminum; the III-V compound semiconductor layer does not contain aluminum or has an aluminum composition lower than that of the third layer, the first layer has an aluminum composition higher than that of the third layer, and the III-V compound semiconductor layer has a thickness greater than that of the second layer. Effect of the Invention

[0007] According to the present disclosure, a vertical-cavity surface-emitting laser is provided in which a layer having a relatively large aluminum composition is less susceptible to oxidation. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a plan view illustrating a vertical-cavity surface-emitting laser according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] 3A to 3C are cross-sectional views each showing a schematic diagram of each process of a method for manufacturing a vertical-cavity surface-emitting laser according to an embodiment. [Figure 4] 4A to 4C are cross-sectional views each showing a schematic process of a method for manufacturing a vertical-cavity surface-emitting laser according to an embodiment. [Diagram 5] FIG. 5 is a diagram showing the materials and dopant concentrations of the members constituting the vertical-cavity surface-emitting laser of the first experimental example. [Figure 6] FIG. 6 is a graph showing the simulation results of the characteristics of the vertical-cavity surface-emitting lasers of the first and second experimental examples. [Figure 7] FIG. 7 is a plan view diagrammatically illustrating an example of a vertical-cavity surface-emitting laser. [Figure 8] 8A to 8C are cross-sectional views each showing a schematic process of a method for manufacturing the vertical-cavity surface-emitting laser shown in FIG. [Figure 9] 9A to 9C are cross-sectional views each showing a schematic process of a method for manufacturing the vertical-cavity surface-emitting laser shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Description of the embodiments of the present disclosure] A vertical cavity surface emitting laser according to one embodiment includes a substrate having a main surface including a first area and a second area surrounding the first area, a first lower distributed Bragg reflector provided on the first area and the second area and extending to an edge of the main surface, a III-V compound semiconductor layer provided on the first lower distributed Bragg reflector, a second lower distributed Bragg reflector provided on the III-V compound semiconductor layer, an active layer provided on the second lower distributed Bragg reflector, and an upper distributed Bragg reflector provided on the active layer, wherein the III-V compound semiconductor layer is provided on the first area and the second area, the second lower distributed Bragg reflector is provided on the first area, and the first lower distributed Bragg reflector is provided on the active layer. the upper distributed Bragg reflector comprises alternating first and second layers, the first layer having a refractive index lower than that of the second layer and the first layer comprising a III-V compound semiconductor containing aluminum; the upper distributed Bragg reflector comprises alternating third and fourth layers, the third layer having a refractive index lower than that of the fourth layer and the third layer comprising a III-V compound semiconductor containing aluminum; the III-V compound semiconductor layer does not contain aluminum or has an aluminum composition lower than that of the third layer, the first layer has an aluminum composition higher than that of the third layer, and the III-V compound semiconductor layer has a thickness greater than that of the second layer.

[0010] In the vertical-cavity surface-emitting laser, the first lower distributed Bragg reflector extends to an edge of the main surface of the substrate, and the III-V compound semiconductor layer is provided on the first lower distributed Bragg reflector, so that even if the first lower distributed Bragg reflector includes a first layer having a relatively large aluminum composition, the first layer is unlikely to be oxidized.

[0011] The upper distributed Bragg reflector may include a current confinement structure, the current confinement structure including a current aperture portion including an aluminum-containing III-V compound semiconductor and an insulator portion, the insulator portion surrounding the current aperture portion, and the first layer may have an aluminum composition equal to or greater than the aluminum composition of the current aperture portion. In this case, the aluminum composition of the first layer is large. Even in such a case, the first layer is unlikely to be oxidized according to the vertical-cavity surface-emitting laser.

[0012] The second layer may be aluminum-free or may have an aluminum composition smaller than the aluminum composition of the III-V compound semiconductor layer, in which case the aluminum composition of the second layer is smaller.

[0013] The first layer may contain AlAs, and the second layer may contain GaAs, whereby the thermal resistance of the vertical-cavity surface-emitting laser can be reduced compared to a case where each of the first layer and the second layer contains a ternary III-V compound semiconductor.

[0014] Where T is the thickness of the III-V compound semiconductor layer, N is the refractive index of the III-V compound semiconductor layer, λ is the oscillation wavelength of the vertical-cavity surface-emitting laser, and m is an integer equal to or greater than 1, T=(m×λ / 2+λ / 4) / N may be satisfied. In this case, it is possible to suppress a decrease in the periodicity of the first lower distributed Bragg reflector and the second lower distributed Bragg reflector. In addition, λ / 4 in the above formula makes it possible to suppress the confinement of light in the III-V compound semiconductor layer.

[0015] The second lower distributed Bragg reflector may include fifth and sixth layers alternately arranged, the fifth layer having a refractive index lower than that of the sixth layer, and the number of pairs each consisting of the fifth and sixth layers may be equal to or greater than 8 and equal to or less than 25. In this case, the first lower distributed Bragg reflector may be spaced an appropriate distance from the active layer.

[0016] The vertical cavity surface emitting laser may further include a third lower distributed Bragg reflector provided between the active layer and the second lower distributed Bragg reflector, and a contact layer provided between the second lower distributed Bragg reflector and the third lower distributed Bragg reflector, in which case a current can be injected into the active layer through the contact layer and the third lower distributed Bragg reflector.

[0017] [Details of the embodiment of the present disclosure] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In the description of the drawings, the same or equivalent elements are designated by the same reference numerals, and duplicated descriptions will be omitted.

[0018] FIG. 1 is a plan view showing a vertical cavity surface emitting laser according to an embodiment. FIG. 2 is a cross-sectional view taken along line II-II in FIG. 1. A vertical cavity surface emitting laser (VCSEL) 10 shown in FIG. 1 and FIG. 2 is, for example, a laser for communication. The vertical cavity surface emitting laser 10 emits laser light L along an axis Ax. The oscillation wavelength of the laser light L is, for example, 840 nm or more and 860 nm or less. As shown in FIG. 2, the vertical cavity surface emitting laser 10 includes a substrate 12, a first lower DBR (DBR: Distributed Bragg Reflector) portion 14 (first lower distributed Bragg reflector), a cap layer 16 (III-V compound semiconductor layer), a second lower DBR portion 18 (second lower distributed Bragg reflector), an active layer 20, and an upper DBR portion 22 (upper distributed Bragg reflector). The vertical-cavity surface-emitting laser 10 may further include a third lower DBR section 24 (third lower distributed Bragg reflector), a contact layer 28, and a contact layer 29.

[0019] The substrate 12 may be a semi-insulating substrate. The substrate 12 has a main surface 12a that intersects with the axis Ax. The main surface 12a includes a first area 12a1 and a second area 12a2 that surrounds the first area 12a1. The second area 12a2 is located at an edge 12ae of the main surface 12a. The second area 12a2 may be an annular area that extends along the edge 12ae of the main surface 12a. The carrier concentration of the substrate 12 is, for example, 1×10 15 cm -3 The substrate 12 may be, for example, a III-V compound semiconductor substrate such as GaAs.

[0020] The first lower DBR portion 14 is provided on the first area 12a1 and the second area 12a2. The first lower DBR portion 14 extends to an edge 12ae of the main surface 12a of the substrate 12. The first lower DBR portion 14 may cover the entire main surface 12a of the substrate 12. The first lower DBR portion 14 includes first layers 14a and second layers 14b arranged alternately along the axis Ax. The number of pairs each consisting of the first layer 14a and the second layer 14b may be 20 or more and 40 or less. The first layer 14a has a refractive index lower than that of the second layer 14b. The first layer 14a includes a III-V compound semiconductor containing aluminum. The first layer 14a has an aluminum composition x. The first layer 14a is made of AlAs or Al. x Ga 1-x The first layer 14a may contain As. x may be greater than 0.9, greater than 0.98, or may be 1. The higher the aluminum composition, the lower the refractive index. In one embodiment, the first layer 14a is an AlAs layer. The second layer 14b includes a III-V compound semiconductor. The second layer 14b may be aluminum-free or have a low aluminum composition. The second layer 14b may be GaAs or Al x1 Ga 1-x1The second layer 14a may include As. x1 may be less than x, may be less than 0.3, or may be 0. In one embodiment, the second layer 14b is a GaAs layer. The first lower DBR portion 14 may be undoped or of a first conductivity type (e.g., p-type). Examples of p-type dopants include carbon. The undoped first lower DBR portion 14 includes the first lower DBR portion 14 that is unintentionally doped. The first layer 14a may have a thickness of 50 nm to 100 nm. The second layer 14b may have a thickness T1 of 50 nm to 100 nm.

[0021] The cap layer 16 is provided on the first lower DBR portion 14. The cap layer 16 is provided on the first area 12a1 and the second area 12a2. The cap layer 16 may extend to an edge 12ae of the main surface 12a of the substrate 12. The cap layer 16 may cover the entire upper surface of the first lower DBR portion 14. The cap layer 16 includes a III-V compound semiconductor. The cap layer 16 does not include aluminum or has a small aluminum composition y. The cap layer 16 includes Al y Ga 1-y It may include As or GaAs. y may be 0.3 or less, 0.2 or less, or 0. In one embodiment, the cap layer 16 is Al y Ga 1-y As (y=0.12) layer. The cap layer 16 may be undoped or of a second conductivity type (e.g., n-type). Examples of n-type dopants include silicon. An undoped cap layer 16 includes a cap layer 16 that is unintentionally doped.

[0022] The thickness T of the cap layer 16 is greater than the thickness T1 of the second layer 14b. The cap layer 16 may be greater than the thickness of the first layer 14a. The thickness T may be 100 nm or more, or 200 nm or more. The thickness T may be 400 nm or less. In one embodiment, the thickness T is 240 nm. When T is the thickness of the cap layer 16, N is the refractive index of the cap layer 16, λ is the oscillation wavelength of the vertical-cavity surface-emitting laser 10, and m is an integer greater than or equal to 1, the following formula (1) may be satisfied. T = (m × λ / 2 + λ / 4) / N … (1)

[0023] As an example, when λ is 853.7 nm, the refractive index of GaAs is 3.663, and that of Al y Ga 1-y The refractive index of As (y=0.12) is 3.522, and that of Al y Ga 1-y The refractive index of Al As (y=0.2) is 3.452. As the aluminum composition y increases, y Ga 1-y The refractive index of As decreases monotonically.

[0024] The second lower DBR portion 18 is provided on the cap layer 16. The second lower DBR portion 18 is provided on the first area 12a1 and is not provided on the second area 12a2. The second lower DBR portion 18 includes a fifth layer 18a and a sixth layer 18b arranged alternately along the axis Ax. The number of pairs each consisting of the fifth layer 18a and the sixth layer 18b may be 8 or more and 25 or less. The second lower DBR portion 18 may have a thickness of 0.5 μm or more. The fifth layer 18a has a refractive index lower than that of the sixth layer 18b. Each of the fifth layer 18a and the sixth layer 18b includes a III-V compound semiconductor including aluminum. The fifth layer 18a has an aluminum composition higher than that of the sixth layer 18b. Each of the fifth layer 18a and the sixth layer 18b may include AlGaAs. The second lower DBR portion 18 may be of a second conductivity type (e.g., n-type).

[0025] The active layer 20 is provided on the second lower DBR portion 18. The active layer 20 includes a quantum well structure 20a, an upper spacer 20b, and a lower spacer 20c. The lower spacer 20c is provided on the second lower DBR portion 18. The quantum well structure 20a is provided on the lower spacer 20c. The upper spacer 20b is provided on the quantum well structure 20a. The quantum well structure 20a may include an InGaAs layer and an AlGaAs layer alternately arranged along the axis Ax. Each of the upper spacer 20b and the lower spacer 20c may be an AlGaAs layer.

[0026] The upper DBR section 22 is provided on the active layer 20. The upper DBR section 22 includes third layers 22a and fourth layers 22b arranged alternately along the axis Ax. The number of pairs each consisting of the third layer 22a and the fourth layer 22b may be 20 or more and 30 or less. The third layer 22a has a refractive index lower than that of the fourth layer 22b. Each of the third layer 22a and the fourth layer 22b includes an aluminum-containing III-V compound semiconductor. The third layer 22a has an aluminum composition z larger than that of the fourth layer 22b. The third layer 22a includes Al z Ga 1-z The fourth layer 22b may contain As. z may be 0.7 or more, or may be 0.9 or more. In one embodiment, z is 0.9. The aluminum composition x of the first layer 14a of the first lower DBR portion 14 is greater than the aluminum composition z of the third layer 22a. The aluminum composition y of the cap layer 16 is less than the aluminum composition z of the third layer 22a. The fourth layer 22b contains Al z1 Ga 1-z1 It may contain As. z1 may be equal to or less than 0.3. The upper DBR portion 22 may be of a first conductivity type (eg, p-type).

[0027] The upper DBR portion 22 may include a current confinement structure 26. The current confinement structure 26 includes a current aperture portion 26a including an aluminum-containing III-V compound semiconductor, and an insulator portion 26b. The insulator portion 26b surrounds the current aperture portion 26a. The axis Ax passes through the current aperture portion 26a. The current aperture portion 26a is, for example, cylindrical. The current aperture portion 26a has an aluminum composition s. The current aperture portion 26a is made of Al. s Ga 1-s The insulator portion 26b may include As. s may be 0.95 or more, or may be 0.98 or more. In one embodiment, s is 0.98. The aluminum composition x of the first layer 14a of the first lower DBR portion 14 may be equal to or greater than the aluminum composition s of the current aperture portion 26a. The current aperture portion 26a may be of the first conductivity type (e.g., p-type). The insulator portion 26b may include aluminum oxide.

[0028] The third lower DBR section 24 is provided between the active layer 20 and the second lower DBR section 18. The third lower DBR section 24 includes seventh layers 24a and eighth layers 24b arranged alternately along the axis Ax. The number of pairs each including the seventh layer 24a and the eighth layer 24b may be 8 or more and 25 or less. The seventh layer 24a has a refractive index lower than that of the eighth layer 24b. Each of the seventh layer 24a and the eighth layer 24b includes a III-V compound semiconductor including aluminum. The seventh layer 24a has an aluminum composition higher than that of the eighth layer 24b. Each of the seventh layer 24a and the eighth layer 24b may include AlGaAs. The third lower DBR section 24 may be of the second conductivity type (e.g., n-type).

[0029] The contact layer 28 is provided between the second lower DBR portion 18 and the third lower DBR portion 24. The contact layer 28 may be of the second conductivity type (e.g., n-type). The contact layer 28 includes a III-V compound semiconductor such as AlGaAs. The dopant concentration of the contact layer 28 is higher than the dopant concentration of the second lower DBR portion 18. The dopant concentration of the second lower DBR portion 18 is higher than the dopant concentration of the cap layer 16.

[0030] The contact layer 29 is provided on the upper DBR portion 22. The contact layer 29 may be of a first conductivity type (e.g., p-type). The contact layer 29 includes a III-V compound semiconductor such as AlGaAs. The dopant concentration of the contact layer 29 is higher than the dopant concentration of the upper DBR portion 22.

[0031] The first area 12a1 of the main surface 12a of the substrate 12 may include a first region 12a11, an annular second region 12a12 surrounding the first region 12a11, and a third region 12a13 surrounding the second region 12a12. The axis Ax passes through the first region 12a11. The first region 12a11 has, for example, a circular shape centered on the axis Ax. A post PS including a third lower DBR portion 24, an active layer 20, an upper DBR portion 22, and a contact layer 29 is provided on the first region 12a11. A trench TR surrounding the post PS is provided on the second region 12a12. The bottom of the trench TR reaches the contact layer 28. A mesa MS having the same layer structure as the post PS is provided on the third region 12a13. A recess RS is provided on the second area 12a2 of the main surface 12a. The recess RS is a cutout portion. The bottom of the recess RS reaches the cap layer 16 .

[0032] An insulating layer 50 is provided on the post PS, the trench TR, the mesa MS, and the recess RS. The insulating layer 50 is used as a protective film. The insulating layer 50 has a first opening 50a provided on the upper surface of the post PS and a second opening 50b provided at the bottom of the trench TR. A first electrode 30 connected to the contact layer 29 is provided in the first opening 50a. The first electrode 30 may be an annular electrode surrounding the axis Ax. The first electrode 30 is, for example, an anode electrode. The first electrode 30 is connected to the pad electrode 34 by a wiring conductor 32. A second electrode 40 connected to the contact layer 28 is provided in the second opening 50b. The second electrode 40 is, for example, a cathode electrode. The second electrode 40 is connected to the pad electrode 44 by a wiring conductor 42.

[0033] According to the vertical-cavity surface-emitting laser 10 of this embodiment, the first lower DBR 14 extends to the edge 12ae of the main surface 12a of the substrate 12, and the cap layer 16 is provided on the first lower DBR 14. Therefore, even if the first lower DBR 14 includes the first layer 14a having a relatively large aluminum composition, the first layer 14a is not easily oxidized. Furthermore, even if the barrier property of the insulating layer 50 is low, the first layer 14a is not easily oxidized because the first lower DBR 14 is covered by the cap layer 16. Therefore, it is possible to suppress distortion caused by a density difference or a thermal expansion coefficient difference between a portion including a III-V compound semiconductor and a portion including an oxide. Therefore, the vertical-cavity surface-emitting laser 10 has high reliability even after a long period of use.

[0034] When the first layer 14a has an aluminum composition x equal to or greater than the aluminum composition s of the current aperture portion 26a, the aluminum composition x of the first layer 14a becomes large. Even in such a case, according to the vertical-cavity surface-emitting laser 10, the first layer 14a is unlikely to be oxidized.

[0035] When the first layer 14a contains AlAs and the second layer 14b contains GaAs, the thermal resistance of the vertical-cavity surface-emitting laser 10 can be reduced compared to when each of the first layer 14a and the second layer 14b contains a ternary III-V compound semiconductor. This makes it possible to suppress an increase in self-heating even if the current injected into the vertical-cavity surface-emitting laser 10 is increased. Therefore, it is possible to widen the modulation band of the vertical-cavity surface-emitting laser 10 while maintaining the desired optical output of the vertical-cavity surface-emitting laser 10.

[0036] When the above formula (1) is satisfied, it is possible to suppress a decrease in the periodicity in the first lower DBR portion 14 and the second lower DBR portion 18. In addition, λ / 4 in the above formula (1) makes it difficult for a parasitic cavity to be formed, so that it is possible to suppress the confinement of light in the cap layer 16.

[0037] When the number of pairs each formed of the fifth layer 18a and the sixth layer 18b is equal to or greater than 8 and equal to or less than 25, the first lower DBR 14 can be separated by an appropriate distance from the active layer 20. This makes it possible to suppress light absorption by the first lower DBR 14.

[0038] 3 and 4 are cross-sectional views each showing a schematic diagram of each step of a method for manufacturing a vertical-cavity surface-emitting laser according to an embodiment. The vertical-cavity surface-emitting laser 10 described above may be manufactured as follows.

[0039] (Formation of Semiconductor Laminate) First, as shown in FIG. 3(a), a semiconductor laminate SL is formed on the main surface 12a of the substrate 12. Specifically, the first lower DBR 14, the cap layer 16, the second lower DBR 18, the contact layer 28, the semiconductor laminate 124 to become the third lower DBR 24, the active layer 20, the semiconductor laminate 122 to become the upper DBR 22, and the contact layer 29 are formed in this order on the main surface 12a. The semiconductor laminate 122 includes a semiconductor layer 122a and a semiconductor layer 122b to become the third layer 22a and the fourth layer 22b, respectively, and a semiconductor layer 126 to become the current confinement structure 26. The semiconductor laminate 124 includes a semiconductor layer 124a and a semiconductor layer 124b to become the seventh layer 24a and the eighth layer 24b, respectively. Each layer constituting the semiconductor laminate SL is formed by, for example, metalorganic vapor phase epitaxy or molecular beam epitaxy.

[0040] (Trench formation) 3(b), a trench TR is formed in the semiconductor laminate SL on the second region 12a12 in the first area 12a1 of the main surface 12a. This forms a post PS surrounded by the trench TR. The trench TR is formed by, for example, dry etching.

[0041] (Oxidation) 3(c), the periphery of the post PS is oxidized by exposing the post PS to an oxygen-containing gas such as water vapor, thereby forming the upper DBR portion 22 and the third lower DBR portion 24.

[0042] (Formation of recess) Next, as shown in FIG. 4(a), a recess RS is formed on the second area 12a2 of the main surface 12a. As a result, a mesa MS is formed between the recess RS and the trench TR. The recess RS is formed by, for example, dry etching. The recess RS is formed to electrically isolate adjacent elements from each other. The recess RS may be a lattice-shaped groove extending along the main surface 12a. After the recess RS is formed, the portion of the fifth layer 18a of the second lower DBR portion 18 exposed on the side wall of the recess RS may be naturally oxidized. On the other hand, the first layer 14a of the first lower DBR portion 14 is not naturally oxidized because it is covered by the cap layer 16.

[0043] (Formation of insulating layer) Next, as shown in FIG. 4(b), an insulating layer 50 is formed on the post PS, the trench TR, the mesa MS and the recess RS.

[0044] (Electrode formation) 4(c), a first opening 50a and a second opening 50b are formed in the insulating layer 50. Next, a first electrode 30 is formed in the first opening 50a, and a second electrode 40 is formed in the second opening 50b.

[0045] (Disconnect) Next, the substrate 12, the first lower DBR portion 14, and the cap layer 16 are cut at the bottom of the recess RS by, for example, cleaving or dicing, thereby completing the manufacture of the vertical-cavity surface-emitting laser 10 shown in FIGS.

[0046] Fig. 5 is a diagram showing the materials and dopant concentrations of the members constituting the vertical-cavity surface-emitting laser of the first experimental example. The vertical-cavity surface-emitting laser of the first experimental example is an example of the vertical-cavity surface-emitting laser 10 of Fig. 2. The oscillation wavelength of the vertical-cavity surface-emitting laser of the first experimental example is 850 nm.

[0047] In the vertical-cavity surface-emitting laser of the second experimental example, the first lower DBR portion 14 is made of 25 pairs of Al 0.12 Ga0.88 As / Al 0.9 Ga 0.1 Other than the replacement with As, the vertical-cavity surface-emitting laser has the same configuration as the vertical-cavity surface-emitting laser of the first experimental example.

[0048] Simulations were performed on the characteristics of the vertical-cavity surface-emitting lasers of Experimental Examples 1 and 2. The simulation results are shown below. The threshold current I th The threshold current I of the vertical-cavity surface-emitting laser of Experimental Example 2 was 0.7009 mA. th The slope efficiency of the vertical-cavity surface-emitting laser of Experimental Example 1 was 0.7215 W / A. The slope efficiency of the vertical-cavity surface-emitting laser of Experimental Example 2 was 0.7256 W / A. The thermal resistance R th The thermal resistance R of the vertical-cavity surface-emitting laser of Experimental Example 2 was 2.08 K / mW. th The vertical-cavity surface-emitting laser of Experimental Example 1 had a threshold current I th and slope efficiency, and the thermal resistance R is about 20% smaller than that of the vertical-cavity surface-emitting laser of Experimental Example 2. th had the following characteristics:

[0049] 6 is a graph showing the simulation results of the characteristics of the vertical-cavity surface-emitting lasers of the first and second experimental examples. The horizontal axis represents the threshold current I from the current I (mA) injected into each vertical-cavity surface-emitting laser. th The vertical axis shows the relaxation oscillation frequency f r (GHz) is shown. Relaxation oscillation frequency f r is a measure of the performance of the modulation bandwidth of the optical response.

[0050] From FIG. 6, when the current I is relatively large, the vertical-cavity surface-emitting laser of Experimental Example 1 has a relaxation oscillation frequency f rIn the vertical-cavity surface-emitting laser of Experimental Example 1, the thermal resistance is reduced compared to the vertical-cavity surface-emitting laser of Experimental Example 2, and therefore the modulation band can be expanded.

[0051] FIG. 7 is a plan view showing an example of a vertical-cavity surface-emitting laser. The vertical-cavity surface-emitting laser 210 shown in FIG. 7 has the same configuration as the vertical-cavity surface-emitting laser 10, except that it includes a lower DBR 214 instead of the first lower DBR 14, the cap layer 16, and the second lower DBR 18. The lower DBR 214 includes a ninth layer 214a and a tenth layer 214b arranged alternately along the axis Ax. The number of pairs including the ninth layer 214a and the tenth layer 214b is, for example, 33. The ninth layer 214a includes a semiconductor portion 214a1 and an insulator portion 214a2 surrounding the semiconductor portion 214a1. The semiconductor portion 214a1 is, for example, an AlAs layer. The insulator portion 214a2 includes aluminum oxide. The tenth layer 214b is, for example, a GaAs layer.

[0052] A recess RS1, instead of the recess RS, is provided on the second area 12a2 of the main surface 12a of the substrate 12. The bottom of the recess RS1 reaches the main surface 12a of the substrate 12.

[0053] Fig. 8 and Fig. 9 are cross-sectional views each showing a schematic diagram of each step of the method for manufacturing the vertical-cavity surface-emitting laser shown in Fig. 7. The vertical-cavity surface-emitting laser 210 in Fig. 7 may be manufactured as follows.

[0054] (Formation of Semiconductor Laminate) 8(a), a semiconductor stack SL1 is formed on the primary surface 12a of the substrate 12. Specifically, a semiconductor stack 314 to become the lower DBR 214, a contact layer 28, a semiconductor stack 124 to become the third lower DBR 24, an active layer 20, a semiconductor stack 122 to become the upper DBR 22, and a contact layer 29 are formed in this order on the primary surface 12a. The semiconductor stack 314 includes a semiconductor layer 314a and a semiconductor layer 314b to become the ninth layer 214a and the tenth layer 214b, respectively.

[0055] (Trench formation) 8(b), a trench TR is formed in the semiconductor laminate SL1 on the second region 12a12 in the first area 12a1 of the main surface 12a, thereby forming a post PS surrounded by the trench TR.

[0056] (Oxidation) 8(c), the periphery of the post PS is oxidized by exposing the post PS to an oxygen-containing gas such as water vapor, thereby forming the upper DBR portion 22 and the third lower DBR portion 24.

[0057] (Formation of recess) Next, as shown in FIG. 9(a), a recess RS1 is formed on the second area 12a2 of the main surface 12a. As a result, a mesa MS is formed between the recess RS1 and the trench TR. The recess RS1 is formed to electrically isolate adjacent elements from each other. After the recess RS1 is formed, the end face of the semiconductor layer 314a is exposed on the side wall of the recess RS1 and is naturally oxidized. As a result, a ninth layer 214a is formed. In addition, a tenth layer 214b is formed from the semiconductor layer 314b.

[0058] (Formation of insulating layer) Next, as shown in FIG. 9(b), an insulating layer 50 is formed on the post PS, the trench TR, the mesa MS and the recess RS1.

[0059] (Electrode formation) 9(c), a first opening 50a and a second opening 50b are formed in the insulating layer 50. Thereafter, a first electrode 30 is formed in the first opening 50a, and a second electrode 40 is formed in the second opening 50b.

[0060] (Disconnect) Next, the substrate 12 is cut at the bottom of the recess RS1. In this manner, the vertical-cavity surface-emitting laser 210 is manufactured.

[0061] Although the preferred embodiments of the present disclosure have been described in detail above, the present disclosure is not limited to the above embodiments.

[0062] For example, the vertical-cavity surface-emitting laser 10 does not need to include the contact layer 28. In this case, the second electrode 40 contacts the second lower DBR portion 18.

[0063] For example, each of the first to eighth layers included in the DBR portion may have a compositionally graded layer in which the Al composition changes toward the adjacent layer. The thickness of the compositionally graded layer is, for example, 10 to 30 nm. In the compositionally graded layer, the Al composition changes linearly so as to approach the Al composition of the adjacent layer.

[0064] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not by the above meaning, and is intended to include all modifications within the scope and meaning equivalent to the claims. [Explanation of symbols]

[0065] 10...Vertical-cavity surface-emitting laser 12...Substrate 12a…main surface 12a1…Area 1 12a2…Second Area 12a11…First area 12a12…Second area 12a13…Third area 12ae…Fate 14…First lower DBR section 14a…1st layer 14b…Second layer 16…Cap layer 18…Second lower DBR section 18a…5th layer 18b…6th layer 20…Active layer 20a...Quantum well structure 20b...Upper spacer 20c…Lower spacer 22...Upper DBR section 22a...Third layer 22b…4th layer 24…Third lower DBR section 24a…7th layer 24b…8th layer 26…Current confinement structure 26a…Current aperture part 26b…Insulator part 28…Contact layer 29…Contact layer 30...1st electrode 32...Wiring conductor 34...Pad electrode 40…Second electrode 42...Wiring conductor 44…Pad electrode 50…Insulating layer 50a…First opening 50b…Second opening 122...Semiconductor laminate 122a...semiconductor layer 122b...semiconductor layer 124...Semiconductor laminate 124a...semiconductor layer 124b...semiconductor layer 126...Semiconductor layer 210... Vertical-cavity surface-emitting laser 214…Lower DBR section 214a…9th layer 214a1...Semiconductor part 214a2...Insulating part 214b…10th layer 314...Semiconductor laminate 314a...semiconductor layer 314b...semiconductor layer Ax…Axis L: Laser light MS…Mesa PS…Post RS…Concave RS1…Concave SL: Semiconductor laminate SL1: Semiconductor laminate TR…Trench

Claims

1. A vertical-cavity surface-emitting laser, comprising: A substrate having a main surface including a first area and a second area surrounding the first area; a first lower distributed Bragg reflector disposed on the first area and the second area and extending to an edge of the major surface; a III-V compound semiconductor layer disposed on the first lower distributed Bragg reflector; a second lower distributed Bragg reflector disposed on the III-V compound semiconductor layer; an active layer disposed on the second lower distributed Bragg reflector; an upper distributed Bragg reflector disposed on the active layer; Equipped with the III-V compound semiconductor layer is provided on the first area and the second area, the second lower distributed Bragg reflector is disposed on the first area; the first lower distributed Bragg reflector comprises alternating first and second layers; the first layer has a refractive index lower than the refractive index of the second layer; the first layer includes a III-V compound semiconductor including aluminum; the upper distributed Bragg reflector comprises alternating third and fourth layers; the third layer has a refractive index lower than the refractive index of the fourth layer; the third layer includes a III-V compound semiconductor including aluminum; the III-V compound semiconductor layer is free of aluminum or has an aluminum composition smaller than the aluminum composition of the third layer; the first layer has an aluminum composition greater than an aluminum composition of the third layer; the III-V compound semiconductor layer has a thickness greater than a thickness of the second layer; a vertical-cavity surface-emitting laser, wherein T=(m×λ / 2+λ / 4) / N is satisfied, where T is a thickness of the III-V compound semiconductor layer, N is a refractive index of the III-V compound semiconductor layer, λ is an oscillation wavelength of the vertical-cavity surface-emitting laser, and m is an integer of 1 or more.

2. A substrate having a main surface including a first area and a second area surrounding the first area; a first lower distributed Bragg reflector disposed on the first area and the second area and extending to an edge of the major surface; a III-V compound semiconductor layer disposed on the first lower distributed Bragg reflector; a second lower distributed Bragg reflector disposed on the III-V compound semiconductor layer; an active layer disposed on the second lower distributed Bragg reflector; an upper distributed Bragg reflector disposed on the active layer; a third lower distributed Bragg reflector disposed between the active layer and the second lower distributed Bragg reflector; a contact layer provided between the second lower distributed Bragg reflector and the third lower distributed Bragg reflector; Equipped with the III-V compound semiconductor layer is provided on the first area and the second area, the second lower distributed Bragg reflector is disposed on the first area; the first lower distributed Bragg reflector comprises alternating first and second layers; the first layer has a refractive index lower than the refractive index of the second layer; the first layer includes a III-V compound semiconductor including aluminum; the upper distributed Bragg reflector comprises alternating third and fourth layers; the third layer has a refractive index lower than the refractive index of the fourth layer; the third layer includes a III-V compound semiconductor including aluminum; the III-V compound semiconductor layer is free of aluminum or has an aluminum composition smaller than the aluminum composition of the third layer; the first layer has an aluminum composition greater than an aluminum composition of the third layer; The III-V compound semiconductor layer has a thickness greater than a thickness of the second layer.

3. The vertical-cavity surface-emitting laser as described in claim 2, wherein T = (m × λ / 2 + λ / 4) / N is satisfied when T is a thickness of the III-V compound semiconductor layer, N is a refractive index of the III-V compound semiconductor layer, λ is an oscillation wavelength of the vertical-cavity surface-emitting laser, and m is an integer of 1 or more.

4. the upper distributed Bragg reflector includes a current confinement structure; the current confinement structure includes a current aperture portion including an aluminum-containing III-V compound semiconductor, and an insulator portion; the insulator portion surrounds the current aperture portion; 4. The vertical-cavity surface-emitting laser according to claim 1, wherein the first layer has an aluminum composition equal to or greater than an aluminum composition of the current aperture portion.

5. 5. The vertical-cavity surface-emitting laser according to claim 1, wherein the second layer does not contain aluminum or has an aluminum composition smaller than an aluminum composition of the III-V compound semiconductor layer.

6. 6. The vertical-cavity surface-emitting laser according to claim 1, wherein the first layer comprises AlAs and the second layer comprises GaAs.

7. the second lower distributed Bragg reflector comprises alternating fifth and sixth layers; the fifth layer has a refractive index lower than the refractive index of the sixth layer; 7. The vertical-cavity surface-emitting laser according to claim 1, wherein the number of pairs each composed of the fifth layer and the sixth layer is 8 to 25.

Citation Information

Patent Citations

  • Vertical cavity surface emitting laser, manufacturing method thereof, and optical transmission system

    JP2005191343A

  • Surface light-emitting laser element, surface light-emitting laser array, optical scanning device, image forming device, and optical communication system

    JP2008060322A

  • Plane emission laser element, plane emission laser array, optical scanner, and image forming apparatus

    JP2012190869A

  • Surface-emitting laser array and method for manufacturing surface-emitting laser array

    JP2015015386A

  • Vertical resonance type surface emitting laser, and method for manufacturing the same

    JP2019040953A