Method for smelting nickel oxide ore

The use of a horizontal hole-type sample container with a rod-shaped jig for nickel oxide ore smelting addresses mixing and unloading challenges, ensuring uniform reduction and high-quality ferronickel production by maintaining temperature and composition uniformity.

JP7563249B2Active Publication Date: 2024-10-08SUMITOMO METAL MINING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021038479
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-10
Publication Date
2024-10-08
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

Existing methods for smelting nickel oxide ore face challenges in uniformly mixing and reducing the ore, leading to non-uniform composition, difficulty in separating ferronickel from slag, and issues with charging and unloading high-temperature pellets, which can cause furnace damage and quality deterioration.

Method used

A method involving a horizontal hole-type sample container with through holes for inserting a rod-shaped loading/unloading jig to facilitate smooth charging and unloading of the mixture into and out of a reduction furnace, ensuring uniform reduction and preventing quality deterioration.

Benefits of technology

Enables accurate, efficient, and stable charging and unloading of nickel oxide ore mixtures, preventing oxidation and ensuring high-quality ferronickel production by maintaining uniform temperature and composition during the reduction process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563249000005
    Figure 0007563249000005
  • Figure 0007563249000006
    Figure 0007563249000006
  • Figure 0007563249000007
    Figure 0007563249000007
Patent Text Reader

Abstract

To provide a method capable of performing accurate and efficient charging of a mixture into a reduction furnace or extracting thereof from the reduction furnace while preventing an obtained metal from degradation, in a technique of manufacturing ferronickel by heating and reducing the mixture containing nickel oxide ore inside the reduction furnace.SOLUTION: A smelting method reduces a mixture containing nickel oxide ore and carbonaceous reducer to manufacture ferronickel. The smelting method includes: a mixture treatment step of mixing the nickel oxide ore and the carbonaceous reducer; and a reduction step of charging the mixture into a reduction furnace to apply a reduction treatment. In the reduction step, the mixture is housed in a horizontal hole type specimen container with a through hole formed in two side faces to apply the reduction treatment. The operation of the charging into the reduction furnace or an extraction from the reduction furnace of the mixture housed in the horizontal hole type specimen container is performed by inserting a rod-like specimen charging-extracting jig having a square cross section into the through hole of the horizontal hole type specimen container and carrying thereof.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for smelting nickel oxide ore, in which ferronickel is produced by reducing a mixture of nickel oxide ore, which is a raw material ore, and a carbonaceous reducing agent. [Background technology]

[0002] Known methods for smelting nickel oxide ores called limonite or saprolite include a pyrometallurgical method for producing nickel matte using a smelting furnace, a pyrometallurgical method for producing ferronickel using a rotary kiln or a moving hearth furnace, and a hydrometallurgical method for producing mixed sulfide using an autoclave.

[0003] When smelting nickel oxide ore, the raw material ore is first treated to form agglomerates, slurry, etc. ("pretreatment" prior to reduction treatment). Specifically, in the pretreatment, nickel oxide ore is agglomerated, that is, converted from a powder or fine particle form into agglomerates, by first mixing the nickel oxide ore with components other than the nickel oxide ore, such as a binder and a reducing agent, to form a mixture, which is then subjected to moisture adjustment and the like, and then charged into an agglomeration machine to form agglomerates (referring to pellets, briquettes, etc., hereinafter simply referred to as "pellets") of, for example, about 10 mm to 30 mm in size.

[0004] Pellets need to have a certain degree of breathability, for example, to allow moisture to evaporate. Also, if reduction is not uniform within the pellets, the composition will be non-uniform, and metals may become dispersed and unevenly distributed. Therefore, it is important to mix the mixture uniformly and to maintain as uniform a temperature as possible during pellet reduction.

[0005] In addition, it is also important to coarsen the ferronickel produced by reduction. If the produced ferronickel has a size of, for example, about several tens of μm to several hundreds of μm, it becomes difficult to separate it from the slag, and the yield of ferronickel is significantly reduced. For this reason, a technology is required to effectively coarsen the ferronickel produced after reduction.

[0006] For example, a small amount of pellets is charged into a reduction furnace, a reduction test is performed, and the resulting reduced product is taken out to examine various properties. However, the treatment temperature is as high as 1000°C to 1500°C, and it is not easy to charge and take out the pellets. Conventionally, the operation of charging the pellets into the furnace and taking out the reduced product obtained by reduction was performed using a special ladle made of a metal that can withstand relatively high temperatures, but the ladle bends due to the high treatment temperature, and there are cases where the ladle gets caught on the inner wall of the furnace when taking out the pellets, making it difficult to take out the pellets smoothly.

[0007] As such, many challenges remain in the technology of mixing and reducing nickel oxide ore to produce metal, and a particularly important technical challenge is being able to carry out various experiments accurately and efficiently. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2018-178252 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been proposed in view of the above circumstances, and has an object to provide a method for producing ferronickel by heating and reducing a mixture containing nickel oxide ore in a reduction furnace, which can accurately and efficiently charge and unload the mixture to be treated into and from the reduction furnace, and can prevent deterioration in the quality of the obtained metal. [Means for solving the problem]

[0010] As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by carrying the mixture in a horizontal-hole type sample container having a through hole for reduction treatment, and by inserting a rod-shaped sample loading / removal tool into the through hole of the horizontal-hole type sample container when loading the mixture into a reduction furnace or removing it from the furnace, thereby completing the present invention.

[0011] (1) A first aspect of the present invention is a method for smelting nickel oxide ore, which produces ferronickel by reducing a mixture containing nickel oxide ore as a raw material ore and a carbonaceous reducing agent, the method comprising: a mixing step of mixing the nickel oxide ore with the carbonaceous reducing agent; and a reduction step of charging the mixture into a reduction furnace and heating the mixture to perform a reduction treatment, the reduction step being performed by accommodating the mixture in a side-hole-type sample container having through holes formed on two opposing side surfaces, and the operation of charging the mixture accommodated in the side-hole-type sample container into the reduction furnace and removing the reduced product obtained by the reduction treatment from the reduction furnace is performed by inserting a rod-shaped sample loading / removal jig having a square cross section into the through holes on the two side surfaces of the side-hole-type sample container and carrying it.

[0012] (2) A second aspect of the present invention is a method for smelting nickel oxide ore according to claim 1, wherein in the first aspect, the through hole formed in the side surface of the horizontal-hole-type sample container is a rectangular hole.

[0013] (3) A third aspect of the present invention is a method for smelting nickel oxide ore according to the first or second aspect of the present invention, wherein in the reduction step, reduction treatment is performed in the reduction furnace at a reduction temperature of 1200° C. or more and 1500° C. or less. Effect of the Invention

[0014] According to the present invention, in a technique for producing ferronickel by heating and reducing a mixture containing nickel oxide ore in a reduction furnace, a method can be provided that can accurately and efficiently charge and unload the mixture into and from the reduction furnace and prevent deterioration in the quality of the obtained metal. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a process diagram showing an example of the flow of a method for smelting nickel oxide ore. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of a reduction furnace. [Diagram 3] FIG. 2 is a diagram showing the configuration of a sample container, (A) being a perspective view, and (B) being a side view showing the side of the container. [Figure 4] FIG. 13 is a diagram showing an example of the configuration of a sample loading / unloading jig. [Diagram 5] 1A to 1C are diagrams showing examples of the shape of the tip of a sample loading and unloading jig. [Figure 6] 1 is a diagram showing the state when a sample loading / unloading jig is inserted into a through hole of a horizontal-hole type sample container. FIG. [Figure 7] FIG. 2 is a diagram showing the schematic configuration of a sample container (A) provided with a handle and a ladle (B) used in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] A specific embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention. In addition, in this specification, the expression "X to Y" (X and Y are arbitrary numerical values) means "X or more and Y or less."

[0017] ≪1. Nickel oxide ore smelting method≫ In the method for smelting nickel oxide ore according to the present embodiment, nickel oxide ore, which is a raw material ore, is mixed with a carbonaceous reducing agent, and the mixture is subjected to a reduction treatment in a smelting furnace (reduction furnace) to generate ferronickel metal and slag.

[0018] Specifically, the method for smelting nickel oxide ore includes at least a mixing step of mixing nickel oxide ore with a carbonaceous reducing agent, and a reduction step of charging the resulting mixture into a reduction furnace and heating the mixture to perform a reduction treatment.

[0019] In this case, in the smelting method according to the present embodiment, in the reduction step, the mixture to be reduced is placed in a horizontal-hole type sample container with through holes formed on two opposing side surfaces, and the reduction process is carried out. The operation of loading the mixture placed in the horizontal-hole type sample container into a reduction furnace and removing the reduced product obtained by the reduction process from the reduction furnace is performed by inserting a rod-shaped sample loading / unloading tool with a square cross section into the through hole of the horizontal-hole type sample container and carrying it.

[0020] According to this method, the mixture to be reduced and the reduced product after reduction can be charged and discharged stably and smoothly, and it is possible to prevent the deterioration of workability due to the deformation of the ladle as in the conventional method, and as a result, it is possible to effectively suppress the deterioration of the quality of the obtained reduced product due to oxidation, etc.

[0021] ≪2. About the smelting process≫ As described above, the method for smelting nickel oxide ore involves heating a mixture of nickel oxide ore, which is a raw material ore, and a carbonaceous reducing agent in a reduction furnace to reduce nickel (nickel oxide) and iron (iron oxide), thereby producing metal of an iron-nickel alloy (ferronickel).Ferronickel can be obtained by separating the metal from the reduction product obtained by the reduction process (separating the metal from the slag).

[0022] Specifically, as shown in FIG. 1, the method for smelting nickel oxide ore according to the present embodiment includes a mixing process S1 in which a raw material containing nickel oxide ore is mixed with a carbonaceous reducing agent, a mixture forming process S2 in which the obtained mixture is formed into a predetermined shape, a reduction process S3 in which the formed mixture is reduced and heated at a predetermined reduction temperature in a reduction furnace, and a recovery process S4 in which the metal and slag generated in the reduction process S3 are separated and the metal is recovered.

[0023] [Mixing process] The mixing process S1 is a process for mixing raw material powders including nickel oxide ore to obtain a mixture. Specifically, the raw material ore, nickel oxide ore, is mixed with a carbonaceous reducing agent, and powders having a particle size of, for example, about 0.2 mm to 0.8 mm, such as iron ore, flux components, and binders, are mixed as optional additives to obtain a mixture. The mixing process can be performed using a mixer or the like.

[0024] In the mixing process S1, kneading may be performed to improve mixability. For example, by kneading the mixture with a twin-screw kneader or the like, shear force is applied to the mixture, which breaks down aggregates of the carbonaceous reducing agent, raw material powder, etc., and allows for more uniform mixing. In addition, the adhesion of each particle can be increased, making it easier to perform a uniform reduction process on the resulting mixture.

[0025] The nickel oxide ore, which is the raw material ore, is not particularly limited, and limonite ore, saprolite ore, etc. can be used. Nickel oxide ore contains nickel oxide (NiO) and iron oxide (Fe2O3) as constituents.

[0026] As described above, in the mixing process S1, a specific amount of carbonaceous reducing agent is added to nickel oxide ore and mixed to obtain a mixture. The carbonaceous reducing agent is not particularly limited, but examples thereof include coal powder and coke powder. It is preferable that the carbonaceous reducing agent has the same particle size as the nickel oxide ore, which is the raw material ore. If the particle sizes of the carbonaceous reducing agent and the nickel oxide ore are the same, they can be easily mixed uniformly, and as a result, the reduction reaction can be caused uniformly, which is preferable.

[0027] The amount of the carbonaceous reducing agent is not particularly limited, but is preferably 50.0% or less, more preferably 40.0% or less, when the amount of the carbonaceous reducing agent required to reduce nickel oxide and iron oxide constituting the nickel oxide ore without excess or deficiency is taken as 100%. Here, the amount of the carbonaceous reducing agent required to reduce nickel oxide and iron oxide without excess or deficiency can be rephrased as the total value of the chemical equivalent required to reduce the entire amount of nickel oxide to nickel metal and the chemical equivalent required to reduce iron oxide to iron metal (hereinafter also referred to as the "total value of chemical equivalents"). In this way, by setting the amount of the carbonaceous reducing agent to a ratio of 50.0% or less, when the total value of the chemical equivalents is taken as 100%, the reduction reaction can be efficiently progressed. The lower limit of the amount of the carbonaceous reducing agent is not particularly limited, but is preferably 10.0% or more, more preferably 15.0% or more, when the total value of the chemical equivalents is taken as 100%.

[0028] In addition to the nickel oxide ore and the carbonaceous reducing agent, the iron ore added as an optional component is not particularly limited, and examples of the iron ore that can be used include iron ore with an iron content of about 50% or more, and hematite obtained by hydrometallurgy of nickel oxide ore. Examples of the binder include bentonite, polysaccharides, resins, water glass, and dehydrated cake. Examples of the flux component include calcium oxide, calcium hydroxide, calcium carbonate, and silicon dioxide.

[0029] Table 1 below shows an example of the composition (wt%) of some of the raw material powders mixed in the mixing process S1, but the composition of the raw material powders is not limited to this.

[0030] [Table 1]

[0031] [Mixture forming process] The mixture forming step S2 is a step of forming the mixture obtained in the mixing treatment step S1. Specifically, the mixture obtained by mixing the raw material powders is formed into a lump of a certain size or more so that the mixture can be, for example, stacked and charged into a reduction furnace during the reduction treatment in the next reduction step S3.

[0032] The shape of the agglomerated material (also called pellets) obtained by molding the mixture can be a rectangular parallelepiped, cylindrical, spherical, etc. Such a shape makes it easy to mold the mixture and reduces the cost of molding. In addition, since these shapes are not complicated, there are almost no defective products and the yield of molding is extremely high. In addition, if the shape is a rectangular parallelepiped, cylindrical, or spherical shape, it is easy to stack the pellets in a reduction furnace, making it possible to increase the amount of pellets to be processed during reduction. Furthermore, the amount of pellets to be processed during reduction can be increased without making each pellet huge, and they are easy to handle. In addition, they do not collapse when being charged into a reduction furnace, making it difficult for defects to occur.

[0033] The volume of the pellets of the molded (agglomerated) mixture is not particularly limited, and may be, for example, 8000 mm 3 If the pellet volume is too small, the molding cost will be high, and it may take time to load the pellets into the reduction furnace. Furthermore, if the pellet volume is small, the ratio of the surface area to the entire pellet will be high, which may cause a difference in reduction between the surface and the inside to appear, and may affect the quality of the ferronickel. 3 By doing so, the molding cost can be reduced, the handling is easy, and it is preferable. Furthermore, it is possible to produce high-quality ferric nickel.

[0034] After the mixture is molded, it may be subjected to a drying process. Depending on the moisture in the mixture, the rapid temperature rise in the reduction process may cause the moisture in the mixture to evaporate and expand all at once, causing the mixture to break into pieces. For this reason, a drying process may be provided after the mixture molding process to dry the mixture. For example, in the drying process, the mixture may be dried so that the solid content is about 70% by weight and the moisture content is about 30% by weight.

[0035] The method of drying the mixture is not particularly limited, and for example, hot air at 150°C to 400°C can be blown onto the lumps to dry them. In the case of a mixture in the form of a relatively large lump, the mixture may have cracks or fractures before or after drying. In the case of a large lump, even if the surface area increases due to cracks or the like, the effect is minimal.

[0036] An example of the composition (parts by weight) of the solid content in the mixture (after drying treatment) is shown in the following Table 2. Note that the composition of the mixture is not limited to this.

[0037] [Table 2]

[0038] [Reduction process] In the reduction step S3, the mixture (molded product) obtained in the mixture molding step S2 is reduced and heated to a predetermined reduction temperature in a reduction furnace. This reduction process causes a smelting reaction (reduction reaction) of the mixture containing nickel oxide ore to proceed, producing metal and slag.

[0039] The temperature of the reduction treatment (reduction temperature) is preferably 1200° C. or higher and 1500° C. or lower, and more preferably 1250° C. or higher and 1450° C. or lower. By setting the reduction temperature within such a range, the reduction reaction can be efficiently and reliably progressed, and ferronickel having the desired properties can be obtained.

[0040] In the reduction process, the slag in the mixture is semi-melted and the liquid and solid phases are mixed, but the metal and slag that have already been separated do not mix, and the mixture becomes a mixture of metal solid phase and slag solid phase as separate phases by subsequent cooling. The volume of this mixture has shrunk to about 50% to 60% of the volume of the mixture to be charged.

[0041] In this embodiment, the mixture to be reduced is placed in a side-hole type sample container having through holes formed on two opposing side surfaces, and the reduction process is carried out by inserting a rod-shaped sample loading / unloading tool having a rectangular cross section into the through holes of the side-hole type sample container and carrying it in the operation of loading the mixture placed in the side-hole type sample container into a reduction furnace and unloading the reduced product obtained by the reduction process from the reduction furnace.

[0042] First, the configuration of the reduction furnace used in the reduction process in the reduction step S3 will be described. Fig. 2 is a schematic diagram showing an example of the configuration of the reduction furnace.

[0043] As shown in FIG. 2, the reducing furnace 1 may be a box furnace in which the furnace body 11 has a box shape (rectangular parallelepiped shape). The reducing furnace 1 may be, but is not limited to, a burner furnace in which a burner 12 is provided at a predetermined position and the reduction process is performed by heating with the burner. By adopting burner heating (burner furnace) as the heating method of the reducing furnace 1, the inside of the furnace can be heated with excellent combustibility, which is preferable. The fuel for the burner is not particularly limited and may be any of gas fuel such as LPG, liquid fuel such as heavy oil, and solid fuel such as coal and coke, but among them, LPG is preferable in terms of its excellent combustibility.

[0044] The reducing furnace 1 is provided with a sample stage 13 inside the box-shaped furnace body 11. The sample stage 13 is a stage for placing a mixture to be reduced. A reducing agent such as a carbonaceous reducing agent may be laid on the upper surface of the sample stage 13.

[0045] The reduction furnace 1 also has an exhaust port 14 for exhausting gas from within the furnace, for example, on its upper surface (ceiling surface).

[0046] A sample loading / unloading port 15 is provided on a predetermined side of the reduction furnace 1 for loading a sample mixture into the reduction furnace and for unloading the reduced product obtained by reduction treatment from the reduction furnace. The height position of the sample loading / unloading port 15 corresponds approximately to the height of the mounting surface of the sample stage 13 inside the furnace body 11. Therefore, when a mixture is loaded from the sample loading / unloading port 15, it can be appropriately mounted on the mounting surface of the sample stage 13. Also, when unloading the reduced product, it can be easily unloaded from the sample loading / unloading port 15 provided at the same height as the sample stage 13.

[0047] Although not shown, the sample inlet / outlet 15 is provided with an opening / closing door, which can be opened when the mixture is introduced or the reduced product is removed, and closed when the reduction treatment is performed. This allows the inside of the reduction furnace 1 to be an airtight space during the reduction treatment.

[0048] Next, a horizontal-hole type sample container for containing a mixture to be subjected to reduction treatment will be described. Fig. 3 shows the configuration of a horizontal-hole type sample container, (A) being a perspective view, and (B) being a side view showing the side of the container.

[0049] As shown in Fig. 3, the side-hole type sample container 2 is, for example, a box-shaped container having side surfaces 21 to 24 on all four sides. The mixture is contained inside the side-hole type sample container 2, and in this state, is loaded into a reduction furnace 1 and subjected to reduction treatment. The side-hole type sample container 2 has an open ceiling surface at the top, and the reduced material is placed inside the container from above.

[0050] As shown in FIG. 3, the horizontal-hole type container for samples 2 has through holes 21h, 23h formed in two opposing side surfaces 21, 23. The two through holes 21h, 23h are formed at approximately the same height position from the bottom of the container on each side surface 21, 23. That is, they are arranged in a straight line at the same height position. As will be described in detail later, a rod-shaped sample loading and unloading jig 3 (see FIG. 4) is inserted into the through holes 21h, 23h from one through hole 21h to the other through hole 23h. The horizontal-hole type container for samples 2 is then carried in a lifted state like a balance, whereby the horizontal-hole type container for samples 2 containing the mixture is loaded into and unloaded from the reduction furnace 1.

[0051] The through holes 21h, 23h are not particularly limited, but are preferably rectangular holes. By having the through holes 21h, 23h be rectangular holes, when a rod-shaped sample loading / removal jig 3 having a rectangular cross section is inserted as described below, the sides constituting the holes and the sides of the rectangular shape of the sample loading / removal jig 3 come into line contact with each other, so that the horizontal-hole type sample container 2 can be stably held and carried by the sample loading / removal jig 3. The size of the hole is preferably sufficiently larger than the cross-sectional size of the sample loading / removal jig 3 to be inserted into the through hole.

[0052] The through-holes are not limited to being formed only on two side surfaces of the horizontal-hole-type container for specimens 2, but may be formed on all four side surfaces, for example. Even in this case, it is preferable that the height positions of the through-holes from the bottom of the container are approximately the same.

[0053] Next, the sample loading / unloading jig will be described. Fig. 4 is a side view showing an example of the configuration of the sample loading / unloading jig.

[0054] The sample loading / unloading jig 3 is a jig used for loading a mixture into the reduction furnace 1 and unloading the reduced product obtained by the reduction treatment from the reduction furnace 1. As shown in Fig. 4, the sample loading / unloading jig 3 is made of a long rod-like body and has a rectangular cross section.

[0055] In addition, the sample loading / removal jig 3 may have a tip that is slightly sharper than the central portion, as shown in Figs. 5(A) and (B), for example. This makes it easier to insert the sample loading / removal jig 3 into the through holes 21h, 23h of the horizontal-hole-type sample container 2, and allows for more accurate insertion into the through holes, improving workability. The size of the sample loading / removal jig 3 is made smaller than the size of the through holes 21h, 23h of the horizontal-hole-type sample container 2. It is preferable to set the size appropriately, taking into account thermal expansion and distortion of the horizontal-hole-type sample container 2.

[0056] In the operation of loading and unloading a mixture, the sample loading / unloading jig 3 is inserted into the through holes 21h, 23h formed in the side surfaces 21, 23 of the above-mentioned side-hole-type container for samples 2. Specifically, for example, from the outside of the side-hole-type container for samples 2, the tip of the sample loading / unloading jig 3 is inserted into the through hole 21h formed in the side surface 21, and then passed through the inside of the side-hole-type container for samples 2 and inserted into the through hole 23h formed in the opposing side surface 23.

[0057] 6, the sample loading / removal jig 3 is attached from the through hole 21h to the through hole 23h. In other words, the horizontal-hole-type sample container 2 is held in a hooked state on the sample loading / removal jig 3. In this state, for example, an operator can hold the end of the sample loading / removal jig 3 and lift it up like a balance, allowing the horizontal-hole-type sample container 2 to be carried.

[0058] In this embodiment, the rod-shaped sample loading / removal jig 3 is inserted into the through-holes 21h, 23h on the two side surfaces 21, 23 of the horizontal-hole type sample container 2 and carried around to load the mixture contained in the horizontal-hole type sample container 2 into the reduction furnace 1 and remove the reduced product obtained by the reduction treatment from the reduction furnace 1. In particular, since the sample loading / removal jig 3 is a rectangular rod with a rectangular cross section, it is difficult to slip and can be stably held in the through-holes 21h, 23h, improving workability. Furthermore, since the through-holes 21h, 23h of the horizontal-hole type sample container 2 are preferably rectangular, the sides constituting the through-holes 21h, 23h and the sides of the square shape of the sample loading / removal jig 3 are in line contact with each other, thereby further improving stability.

[0059] More specifically, the operation of charging the mixture as a sample into the reduction furnace 1 in the reduction treatment and the operation of removing the reduced product obtained by the treatment from the reduction furnace 1 will be described.

[0060] First, a mixture, which is a sample to be subjected to reduction treatment, is placed inside the horizontal-hole type sample container 2. Next, the sample loading / removal jig 3 is prepared, and the sample loading / removal jig is inserted from its tip into the through-hole 21h formed in the side surface 21 of the horizontal-hole type sample container 2 containing the mixture, and after passing through the inside of the container, its tip is taken out from the through-hole 23h formed in the opposing side surface 23. This results in the horizontal-hole type sample container 2 being hooked and held by the sample loading / removal jig 3 from the through-hole 21h to the through-hole 23h (see FIG. 6). In this state, an operator can hold the end of the rod-shaped sample loading / removal jig 3 and lift it up to carry the horizontal-hole type sample container 2 containing the mixture.

[0061] Next, with the horizontal-hole type sample container 2 held by the sample loading / unloading jig 3, the door of the sample loading / unloading port 15 provided on the side of the reduction furnace 1 is opened, and an operator holds the end of the sample loading / unloading jig 3 and loads the horizontal-hole type sample container 2 into the reduction furnace 1 through the sample loading / unloading port 15. Then, while still holding the end of the sample loading / unloading jig 3, the operator moves the horizontal-hole type sample container 2 close to the sample stage 13 provided in the furnace body 11 and gently places it on the sample stage 13.

[0062] Thereafter, the sample loading / unloading jig 3 is removed from the through holes 21h, 23h of the horizontal-hole-type sample container 2, and only the sample loading / unloading jig 3 is taken out of the reduction furnace 1 through the sample loading / unloading port 15. Then, the door provided at the sample loading / unloading port 15 is closed, heating of the reduction furnace 1 by the burner 12 is started, and the reduction process is performed on the mixture in the horizontal-hole-type sample container 2 placed on the sample stage 13. At this time, the sample loading / unloading jig 3 used to load the mixture has been removed from the reduction furnace 1, so that it is outside the furnace during the reduction process and the load due to high temperature heat can be avoided.

[0063] After the reduction process is completed, a reduced product is generated by heating and reducing the mixture inside the side-hole-type sample container 3 placed on the sample stage 13 of the reduction furnace 1. The operation of removing the reduced product from the reduction furnace 1 is performed in the reverse order of the operation of loading. That is, the door of the sample loading / unloading port 15 provided in the reduction furnace 1 is opened, and the sample loading / unloading jig 3 is inserted into the through holes 21h and 23h of the side-hole-type sample container 2 placed on the sample stage 13, and the side-hole-type sample container 2 is held by the sample loading / unloading jig 3 in the same state as when it was loaded into the reduction furnace 1 (see FIG. 6).

[0064] In this state, by gripping the end of the sample loading / unloading jig 3 and pulling it out, the horizontal-hole-type sample container 2 containing the reduced material can be easily removed from the reduction furnace 1.

[0065] In addition, when the reduction treatment is started, the sample loading / unloading jig 3 may not be taken out of the furnace. That is, after the horizontal-hole type sample container 2 held by the sample loading / unloading jig 3 is loaded into the reduction furnace 1 and placed on the sample stage 13, the opening / closing door provided at the sample loading / unloading port 15 may be closed and heating of the reduction furnace 1 may be started with the sample loading / unloading jig 3 still inserted into the through holes 21h and 23h of the horizontal-hole type sample container 2. Even in this case, since the sample loading / unloading jig 3 is inserted into the horizontal-hole type sample container 2 through the through holes 21h and 23h, even if the sample loading / unloading jig 3 is deformed by high-temperature heat, the horizontal-hole type sample container 2 can be smoothly taken out of the reduction furnace 1 by gripping the end of the sample loading / unloading jig 3 after the reduction treatment is completed.

[0066] In this manner, according to the present embodiment, the mixture is accommodated in the horizontal-hole type sample container 2 having the through-holes 21h, 23h formed in the two opposing side surfaces 21, 23, and in the operation of loading the mixture into the reduction furnace 1 and removing the reduced product obtained by the reduction treatment from the reduction furnace 1, the rod-shaped sample loading / removal jig 3 is inserted into the through-holes 21h, 23h of the horizontal-hole type sample container 2 and is carried in a hooked state, so that the transportation can be performed stably and smoothly. In addition, it is possible to prevent the deterioration of the workability due to the deformation of the ladle as in the conventional case. As a result, it is possible to effectively suppress the deterioration of the quality of the reduced product obtained due to oxidation, etc.

[0067] Furthermore, for example, in the case of charging samples of various compositions and conducting a test to search for effective reaction conditions for a predetermined reaction time, it is also important to consider the position (inside the furnace) at which the mixture is placed in the reducing furnace 1. In this regard, by charging the mixture through the above-mentioned operation, the mixture can be accurately placed in the reducing furnace, and the test to search for reaction conditions can be conducted more effectively.

[0068] By carrying out the reduction treatment in the reduction step S3 as described above, ferronickel can be produced accurately, reliably, and efficiently.

[0069] [Recovery process] In the recovery step S4, the metal and slag generated in the reduction step S3 are separated and the metal is recovered. Specifically, the metal phase is separated and recovered from a mixture (mixture) containing a metal phase (metal solid phase) and a slag phase (slag solid phase) obtained by subjecting the mixture filled in a container to a reduction heat treatment.

[0070] Methods for separating the metal phase and the slag phase from the mixture of the metal phase and the slag phase obtained as a solid include, for example, sieving to remove unnecessary materials, as well as separation by specific gravity or magnetic force.

[0071] Furthermore, the obtained metal phase and slag phase have poor wettability and can be easily separated. For example, by dropping the large mixture obtained by the treatment in the reduction step S3 described above from a predetermined drop or by applying a predetermined vibration during sieving, the metal phase and slag phase can be easily separated from the mixture.

[0072] In this manner, the metal phase and the slag phase are separated, and the metal phase, i.e., ferronickel, is recovered. EXAMPLES

[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0074] [Examples and Comparative Examples] A method for smelting nickel oxide ore was carried out to produce ferronickel by reducing a mixture of nickel oxide ore, which is a raw material ore, and a carbonaceous reductant under the conditions shown below.

[0075] (Mixing process) A mixture was obtained by mixing nickel oxide ore as raw material ore, iron ore, silica sand and limestone as flux components, binder, and carbonaceous reducing agent (coal powder, carbon content: 78% by weight, average particle size: about 83 μm) using a mixer while adding an appropriate amount of water. The carbonaceous reducing agent was included in an amount that was 37.0% when the amount required to reduce nickel oxide and iron oxide (Fe2O3) contained in the nickel oxide ore as raw material ore without excess or deficiency was taken as 100%.

[0076] (Mixture forming process) Next, the obtained mixture was granulated using a pan-type granulator and sieved to a size of φ15.0±0.5 mm. After that, the sample was dried by blowing hot air at 170°C to 250°C onto it so that the solid content was about 70% by weight and the moisture content was about 30% by weight before reduction. The solid content composition (excluding carbon) of the sample after drying is shown in Table 3 below.

[0077] [Table 3]

[0078] (Reduction process) Next, the sieved sample (mixture sample) was divided into 12 pieces (Examples 1 to 9, Comparative Examples 1 to 3), and was subjected to a reduction treatment by heating in a reduction furnace (burner furnace).

[0079] In this embodiment, a horizontal-hole type sample container as shown in the schematic diagram of Fig. 3 was used, and the mixture was placed in the container and subjected to reduction treatment. The mixture was charged into the reduction furnace and the resulting reduced product was removed from the reduction furnace using a rod-shaped sample loading / removal tool with a square cross section as shown in Fig. 4, which was inserted into through holes formed in two side surfaces of the horizontal-hole type sample container and carried as shown in Fig. 6. Ash (mainly SiO2, with small amounts of oxides such as Al2O3 and MgO as other components) was spread over the upper surface of the horizontal-hole type sample container on which the sample was placed, and the mixture sample was placed on top of it.

[0080] The reduction furnace used was a box-shaped burner furnace with an internal sample stage and a sample loading / unloading port on a predetermined side at a position corresponding to the height position of the sample stage mounting surface (see FIG. 2). The reduction furnace was equipped with a burner, and pulverized coal, LPG, heavy oil, and coke were used as fuel.

[0081] Specifically, in the examples, when loading the horizontal-hole type sample container into the reduction furnace, a sample loading / unloading jig was inserted into the through-holes formed on the two sides of the horizontal-hole type sample container containing the mixture, and the end of the sample loading / unloading jig was grasped and lifted to load the sample through the sample loading / unloading port provided on the side of the reduction furnace. The horizontal-hole type sample container was inserted near the top of the sample stage provided in the reduction furnace, and the horizontal-hole type sample container was gently placed on the sample stage.

[0082] Then, the sample loading / unloading jig inserted into the through hole of the side-hole type sample container was removed, and only the sample loading / unloading jig was taken out from the sample loading / unloading port. The door at the sample loading / unloading port was closed, and heating of the reduction furnace was started by the burner to carry out the reduction treatment of the mixture in the side-hole type sample container placed on the sample stage.

[0083] Next, after the reduction treatment was completed, the door of the sample loading / unloading port provided in the reduction furnace was opened, and the sample loading / unloading jig was inserted near the side-hole type sample container. Then, the sample loading / unloading jig was inserted into the through hole of the side-hole type sample container, and in this state, the end of the sample loading / unloading jig was grasped and lifted, thereby removing the reduced material contained in the side-hole type sample container from the reduction furnace.

[0084] The reduced product was cooled and then the nickel metallization rate and nickel content in the metal were measured, as shown below.

[0085] On the other hand, in the comparative example, a sample container with a handle as shown in the side view of Fig. 7(A) and a ladle as shown in Fig. 7(B) were used, and the mixture sample was placed in the sample container, and the ladle was hooked on the handle of the sample container to load it into the reduction furnace. After the reduction treatment was completed, the ladle was similarly hooked on the handle of the sample container to remove it from the reduction furnace. The reduction treatment was performed with the opening and closing door of the sample loading and unloading port closed.

[0086] [evaluation] After cooling each sample, the nickel metallization rate and the nickel content in the metal, defined by the following formula, were analyzed and calculated using an ICP emission spectrometer (SHIMAZU S-8100). Nickel metal ratio = amount of metalized Ni in the mixture ÷ (total amount of Ni in the mixture) × 100 (%) ··· [1] Formula Nickel content in metal = amount of metalized Ni in the mixture ÷ (total amount of metalized Ni and Fe in the mixture) × 100 (%) ··· [2]

[0087] The removal of the reduced material from the reduction furnace was also evaluated. In other words, the case where the removal was performed without any problems was evaluated as "○", and the case where the sample container was tilted or shifted and the removal took more than 30 seconds was evaluated as "△".

[0088] Table 4 below shows the reduction treatment conditions, the workability in removing the material, the nickel metal ratio, and the calculated nickel content in the metal.

[0089] [Table 4]

[0090] As shown in Table 4, in Examples 1 to 9, the workability of sample removal was excellent, and both the nickel metallization rate and metal content were good. This is believed to be because the mixture was placed in a horizontal-hole type sample container and then charged into and removed from the reduction furnace, enabling stable and smooth operation without tilting or shifting.

[0091] On the other hand, in Comparative Examples 1 to 3, the stability of the work was reduced, and tilting and shifting occurred, which required a lot of work time, and as a result, the quality of the obtained reduced product was also reduced. [Explanation of symbols]

[0092] 1. Reduction furnace 11 Furnace body 12 Burner 13 Sample stage 14 Exhaust port 15 Sample loading / unloading port 2. Horizontal hole type sample container 21~24 Side 21h,23h through hole 3. Sample loading and unloading tool

Claims

1. A method for smelting nickel oxide ore to produce ferronickel by reducing a mixture containing nickel oxide ore as a raw material ore and a carbonaceous reductant, comprising the steps of: a mixing step of mixing the nickel oxide ore with the carbonaceous reductant; a reduction step of charging the mixture into a box-shaped reduction furnace and heating the mixture to perform a reduction treatment; having In the reduction step, the mixture is placed in a horizontal-hole type sample container having through holes formed on two opposing side surfaces, and the reduction treatment is performed thereon; In the operation of loading the mixture contained in the side-hole type sample container into the reduction furnace and removing the reduced product obtained by the reduction treatment from the reduction furnace, the side-hole type sample container is carried by inserting rod-shaped sample loading / removal jigs having a square cross section into the through holes on two side surfaces of the side-hole type sample container, and the side-hole type sample container is loaded into and removed from the reduction furnace through a sample loading / removal port provided on the side surface of the reduction furnace. A method for smelting nickel oxide ores.

2. The through hole formed in the side surface of the horizontal hole-type sample container is a rectangular hole.

2. The method for smelting nickel oxide ore according to claim 1.

3. In the reduction step, In the reduction furnace, a reduction treatment is performed at a reduction temperature of 1200° C. or more and 1500° C. or less.

3. A method for smelting nickel oxide ore according to claim 1 or 2.

Citation Information

Patent Citations

  • Container for transport

    JP2003104354A

  • Manufacturing method of reduced iron using rotary hearth furnace, and rotary hearth furnace

    JP2018178252A

  • Method for smelting oxide ore and reduction furnace

    JP2019035127A

  • Method for smelting oxide ore

    JP2020045542A

  • Smelting method of oxide ore

    JP2020084268A