Solid electrolyte, method for producing solid electrolyte, and all-solid-state battery

A solid electrolyte with a pyrrolidinium-based organic cation and boron cluster anion, optimized through quenching, enhances ionic conductivity, improving battery performance in all-solid-state batteries.

JP7563373B2Active Publication Date: 2024-10-08TOYOTA JIDOSHA KK
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021214182
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-10-08
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The ionic conductivity of existing solid electrolytes in all-solid-state batteries is inadequate, which significantly affects battery performance.

Method used

A solid electrolyte composed of a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion, with specific peak intensities in X-ray diffraction measurements, and a manufacturing method involving quenching to enhance ionic conductivity.

Benefits of technology

The proposed solid electrolyte achieves improved ionic conductivity, leading to better input and output characteristics in all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563373000003
    Figure 0007563373000003
  • Figure 0007563373000004
    Figure 0007563373000004
  • Figure 0007563373000005
    Figure 0007563373000005
Patent Text Reader

Abstract

To provide a solid electrolyte having preferable ion conductivity.SOLUTION: The disclosure relates to a solid electrolyte comprising: a matrix including, pyrrolidinium based organic cation, and a boron cluster anion; and a metal salt including a metal cation and anion. The solid electrolyte has a prescribed peak A which exists in a position of 2θ=15.7°±0.5° in an X-ray diffraction measurement using a CuKα ray, and a prescribed peak B which exists in a position of 2θ=18.2°±0.5°.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid electrolyte, a method for producing a solid electrolyte, and an all-solid-state battery. [Background technology]

[0002] An all-solid-state battery is a battery having a solid electrolyte layer between a positive electrode layer and a negative electrode layer, and has the advantage that it is easier to simplify safety devices compared to liquid batteries having an electrolyte solution containing a flammable organic solvent. Organic solid electrolytes and inorganic solid electrolytes are known as solid electrolytes used in the solid electrolyte layer.

[0003] For example, Patent Document 1 discloses an electrolyte composition that contains, as a solid electrolyte, a matrix containing an organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-194777 A Summary of the Invention [Problem to be solved by the invention]

[0005] The battery performance of an all-solid-state battery is greatly affected by the ionic conductivity of the solid electrolyte. Therefore, a solid electrolyte having good ionic conductivity is desired. The present disclosure has been made in view of the above-mentioned circumstances, and has as its main object to provide a solid electrolyte having good ionic conductivity. [Means for solving the problem]

[0006] In order to solve the above problems, the present disclosure provides a solid electrolyte having a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion, wherein the solid electrolyte has, in X-ray diffraction measurement using CuKα radiation, peak A appearing at 2θ=15.7°±0.5° and peak B appearing at 2θ=18.2°±0.5°, and the intensity of peak A or peak B is the largest among all peaks observed in the X-ray diffraction measurement.

[0007] The present disclosure also provides a solid electrolyte having a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion, the solid electrolyte having a peak A appearing at a position of 2θ=15.7°±0.5° and a peak B appearing at a position of 2θ=18.2°±0.5° in an X-ray diffraction measurement using CuKα radiation, and an intensity of the peak A being within a range of I A The intensity of the above peak B is I B Let the intensity at the reference position be I S The present invention provides a solid electrolyte that satisfies at least one of the following conditions (i) and (ii): Condition (i): A -I S ) / I S But it is greater than 2.69. Condition (ii): B -I S ) / I S is greater than 0.73.

[0008] According to the present disclosure, since it has the predetermined peak A and peak B, it becomes a solid electrolyte with good ion conductivity.

[0009] In the above disclosure, the intensity of the peak A or the intensity of the peak B may be the greatest among all peaks observed in the above X-ray diffraction measurement.

[0010] In the above disclosure,A -I S ) / I S However, it may be 7.74 or more.

[0011] In the above disclosure, B -I S ) / I S However, it may be 3.16 or more.

[0012] In the above disclosure, the anion in the metal salt may be a boron cluster anion.

[0013] The present disclosure also provides a method for producing the above-mentioned solid electrolyte, the method including: a preparation step of preparing a precursor containing the matrix containing the pyrrolidinium-based organic cation and the boron cluster anion, and the metal salt containing the metal cation and the anion; a heating step of heating the precursor at a temperature equal to or higher than the melting temperature of the matrix to obtain a melt of the precursor; and a quenching step of quenching and solidifying the melt to obtain the solid electrolyte.

[0014] According to the present disclosure, by including the quenching step, a solid electrolyte having good ion conductivity can be produced.

[0015] The present disclosure also provides an all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, wherein at least one of the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer contains the above-mentioned solid electrolyte.

[0016] According to the present disclosure, at least one of the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer contains the above-mentioned solid electrolyte, resulting in an all-solid-state battery with good input and output characteristics. Effect of the Invention

[0017] The present disclosure has an effect of providing a solid electrolyte having good ion conductivity. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a flow diagram showing an example of a method for producing a solid electrolyte according to the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. [Diagram 3] 1 shows the results of X-ray diffraction measurements in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The solid electrolyte, the method for producing the solid electrolyte, and the all-solid-state battery according to the present disclosure will be described in detail below.

[0020] A. Solid electrolyte The solid electrolyte of the present disclosure has a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion, and the solid electrolyte has peak A appearing at 2θ=15.7°±0.5° and peak B appearing at 2θ=18.2°±0.5° in X-ray diffraction measurement using CuKα radiation. In addition, the solid electrolyte of the present disclosure preferably has the intensity of peak A or the intensity of peak B greatest among all peaks observed in the X-ray diffraction measurement. In addition, the solid electrolyte of the present disclosure preferably has the intensity of peak A greatest than I A The intensity of the above peak B is I B Let the intensity at the reference position be I S In this case, it is preferable that a predetermined condition is satisfied.

[0021] According to the present disclosure, since it has the predetermined peak A and peak B, it becomes a solid electrolyte with good ion conductivity.

[0022] As described above, a solid electrolyte having good ion conductivity is desired. The present inventors have conducted extensive research into an electrolyte composition (solid electrolyte) containing a matrix containing an organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion, and have found that a solid electrolyte having a novel crystal phase can be obtained by a specific manufacturing method, and that this solid electrolyte has good ion conductivity.

[0023] In an X-ray diffraction measurement using CuKα radiation, the solid electrolyte of the present disclosure has a peak A appearing at 2θ=15.7°±0.5° and a peak B appearing at 2θ=18.2°±0.5°. The positions of peak A and peak B may vary within a range of ±0.3° or ±0.1°, respectively.

[0024] In the present disclosure, it is preferred that the intensity of peak A or the intensity of peak B is the greatest among all peaks observed in X-ray diffraction measurement.

[0025] In addition, in this disclosure, the intensity of peak A is I A and the intensity of peak B is I B Let the intensity at the reference position be I S In this case, it is preferable that at least one of the following conditions (i) and (ii) is satisfied. Condition (i): A -I S ) / I S But it is greater than 2.69. Condition (ii): B -I S ) / I S is greater than 0.73. In this disclosure, A -I S ) / I S The value calculated by is the standard value 1, (I B -I S ) / I S The value calculated in the above is sometimes referred to as standard value 2.

[0026] In this disclosure, the "reference position" refers to a position where no peak is observed in X-ray diffraction measurement. The reference position is preferably a position that is at least -2° away from the position of the peak observed at the lowest angle side, or a position that is at least +2° away from the position of the peak observed at the highest angle side. A specific example of the reference position is 2θ=12.0°.

[0027] (I A -I S ) / I S may be 3.00 or more, 5.00 or more, 7.00 or more, or 7.74 or more. A -I S ) / I S The upper limit of is not particularly limited, but is, for example, 13.00 or less. B -I S ) / I S may be 1.00 or more, 2.00 or more, 3.00 or more, or 3.16 or more. B -I S ) / I S The upper limit of is not particularly limited, but is, for example, 8.00 or less.

[0028] Also, I A and I B and may be the same or different. A and I B The "same" is A I B The ratio (I B / I A ) is 0.95 or more and 1.05 or less. A and I B If different from I B / I A is, for example, 0.5 or more, may be 0.7 or more, or may be 0.9 or more. B / I A is, for example, 1.5 or less, may be 1.3 or less, or may be 1.1 or less.

[0029] In addition, the solid electrolyte in the present disclosure may have only peak A and peak B in X-ray diffraction measurement using CuKα radiation, or may have peaks other than peak A and peak B. In the latter case, the position of the peak other than peak A and peak B may be, for example, at least one of 2θ=15.0±0.5°, 16.8°±0.5°, and 17.4°±0.5°. These peak positions may vary within a range of ±0.3°. In the present disclosure, the peak obtained at the above position may be referred to as peak X.

[0030] In addition, the solid electrolyte of the present disclosure preferably does not have a peak Y at 2θ=16.1±0.5° in X-ray diffraction measurement. Peak Y is a peak other than the above-mentioned peaks A, B, and X. "Does not have a peak Y" means that the intensity of the peaks other than peaks A, B, and X at 2θ=16.1±0.5° is less than I Y In this case, I Y / I A is less than or equal to 0.1, or I Y / I B is less than or equal to 0.1.

[0031] 1. Matrix The matrix in the present disclosure contains a pyrrolidinium-based organic cation and a boron cluster anion. The solid electrolyte may contain one type of matrix or may contain two or more types of matrices.

[0032] The pyrrolidinium-based organic cation is usually an organic cation having a pyrrolidinium skeleton, and is preferably represented by the following structure.

[0033] [ka]

[0034] In the formula, R and R′ each independently represent a substituent belonging to any one of the following groups: Group (i): linear, branched or cyclic alkyl or fluoroalkyl groups having 1 to 8 carbon atoms. Group (ii): an aryl group or a fluoroaryl group having 6 to 9 carbon atoms. Group (iii): linear, branched or cyclic alkoxy or fluoroalkoxy groups having 1 to 8 carbon atoms. Group (iV): an aryloxy group or a fluoroaryloxy group having 6 to 9 carbon atoms. Group (v): amino group. Group (vi): Substituents having two or more moieties defined by any two or more of groups (i) to (v).

[0035] Specific examples of pyrrolidinium-based organic cations include N-methyl-N-propylpyrrolidinium (Pyr13), N-methyl-N-(2-methoxyethyl)-pyrrolidinium (Pyr12ol), N-methyl-N-ethylpyrrolidinium (Pyr12) and N-methyl-N-butylpyrrolidinium (Pyr14).

[0036] Boron cluster anions refer to any of the following anionic forms: boranes, which have 6 to 12 boron atoms and a net charge of -2; carboranes, which have 1 carbon atom and 5 to 11 boron atoms in the cluster structure and a net charge of -1; and carboranes, which have 2 carbon atoms and 4 to 10 boron atoms in the cluster structure and a net charge of -1 or -2.

[0037] The boron cluster anion may be unsubstituted, and may have only hydrogen atoms in addition to boron atoms and carbon atoms. The boron cluster anion may also have hydrogen atoms substituted. In this case, the hydrogen atoms may be replaced by at least one of a halogen atom and an organic substituent. The number of substituted hydrogen atoms may be one or more. The types of the halogen atoms and the organic substituents may each be one or more than one.

[0038] The boron cluster anion can be represented, for example, by any one of the following general formulas (i) to (v). General formula (i):[B y H (y-z-i) R 1 z X i ] 2- General formula (ii): [CB (y-1) H (y-z-i) R 1 z X i ] - General formula (iii): [C2B (y-2) H (y-t-j-1) R 1 t X j ] - General formula (iv):[C2B (y-3) H (y-t-j) R 1 t X j ] - General formula (v):[C2B (y-3) H (y-t-j-1) R 1 t X j ] 2- In the formula, y is an integer satisfying 6≦y≦12, z+i is an integer satisfying 0≦z+i≦y, t+j is an integer satisfying 0≦t+j≦y-1, and X is at least one of F, Cl, Br, and I. 1 is an organic substituent or hydrogen.

[0039] Examples of boron cluster anions include [B6H6] 2- , [B 12 H 12 ] 2- , [CB9H 10 ] - , [CB 11 H 12 ] - , [C2B 10 H 11 ] -The boron cluster anion may have a so-called closo structure.

[0040] 2. Metal salts The metal salt in the present disclosure contains a metal cation and an anion. The solid electrolyte may contain one type of metal salt or may contain two or more types of metal salts.

[0041] The metal cation is, for example, Li + and Na + Alkali metal cations such as Mg 2+ and Ca 2+ and the like alkaline earth metal cations.

[0042] The anion in the metal salt may or may not be a boron cluster anion, such as (fluorosulfonyl)imide (FSI), bis(trifluoromethanesulfonyl)imide (TFSI), hexafluorophosphate (PF6), and tetrafluoroborate (BF4).

[0043] 3.Solid electrolyte The solid electrolyte in the present disclosure has a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion.

[0044] The solid electrolyte has a pyrrolidinium-based organic cation and a boron cluster anion as cations. The ratio of the pyrrolidinium-based organic cation to the total of the pyrrolidinium-based organic cation and the metal cation is, for example, 1 mol% to 50 mol%, and may be 5 mol% to 30 mol%. The solid electrolyte preferably contains at least N-methyl-N-butylpyrrolidinium (Pyr14) and Li as cations. That is, it is preferable to use a matrix containing Pyr14 as a pyrrolidinium-based organic cation in combination with a metal salt containing Li as a metal cation.

[0045] The solid electrolyte has at least a boron cluster anion as an anion. The anion in the solid electrolyte may be only a boron cluster anion. The solid electrolyte may have one, two, or three or more kinds of boron cluster anions as an anion. The solid electrolyte may have, as an anion, [B6H6] 2- , [B 12 H 12 ] 2- , [CB9H 10 ] - , [CB 11 H 12 ] - , [C2B 10 H 11 ] - Among them, the solid electrolyte preferably contains at least one of the following anions: [CB9H 10 ] - and [CB 11 H 12 ] - For example, the solid electrolyte preferably contains at least one anion selected from the group consisting of [CB9H 10 ] - and [CB 11 H 12 ] - If it contains, [CB9H 10 ] - and [CB 11 H 12 ] - [CB9H 10] - The ratio is, for example, 30 mol % or more and 90 mol % or less, alternatively 40 mol % or more and 80 mol % or less, or may be 50 mol % or more and 70 mol % or less.

[0046] The solid electrolyte in the present disclosure preferably has high ionic conductivity. The ionic conductivity at 25° C. is, for example, 0.3 mS / cm or more, may be 0.6 mS / cm or more, or may be 0.9 mS / cm or more. On the other hand, the ionic conductivity at 25° C. is, for example, 7 mS / cm or less, may be 5 mS / cm or less, 3 mS / cm or less, 2 mS / cm or less, or may be 1.2 mS / cm or less.

[0047] The shape of the solid electrolyte may be, for example, particulate. The particle diameter (D50) of the solid electrolyte is, for example, 0.1 μm or more and 50 μm or less. The particle diameter D50 refers to the cumulative 50% particle diameter in the volume-based particle diameter distribution measured by a laser diffraction particle size distribution measuring device. The elastic modulus of the solid electrolyte is preferably low. The elastic modulus is, for example, less than 10 GPa, and may be less than 1 GPa or less than 0.5 GPa. The solid electrolyte may be a single-phase material having a single crystal phase, or a multi-phase material having multiple crystal phases.

[0048] B. Manufacturing method of solid electrolyte Fig. 1 is a flow diagram showing an example of a method for producing a solid electrolyte according to the present disclosure. As shown in Fig. 1, the method for producing a solid electrolyte according to the present disclosure includes a preparation step of preparing a precursor containing a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion and a metal salt containing a metal cation and an anion, a heating step of heating the precursor at a temperature equal to or higher than the melting temperature of the matrix to obtain a melt of the precursor, and a quenching step of quenching and solidifying the melt to obtain the solid electrolyte.

[0049] According to the present disclosure, by including the quenching step, a solid electrolyte having good ion conductivity can be produced.

[0050] 1. Preparation process The preparation step is a step of preparing a precursor containing a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion, and a metal salt containing a metal cation and an anion.

[0051] In the preparation step, the precursors may be purchased or prepared by oneself. In the latter case, for example, the above-mentioned matrix material and metal salt material can be mixed and prepared. The ratio of each material is preferably adjusted appropriately in consideration of the composition of the target solid electrolyte.

[0052] 2.Heating process The heating step is a step of heating the precursor to a temperature equal to or higher than the melting temperature of the matrix to obtain a molten precursor.

[0053] The heating temperature in the heating step is not limited as long as it is equal to or higher than the melting point of the matrix, and can be, for example, 150°C or higher and 200°C or lower. In addition, it is preferable that the time of the heating step (heating time) is short. The heating time is, for example, 12 hours or less, may be 9 hours or less, or may be 6 hours or less. On the other hand, the heating time is, for example, 2 hours or more, and may be 4 hours or more.

[0054] 3.Quenching process The quenching step is a step of rapidly cooling the molten material to solidify it, thereby obtaining the above-mentioned solid electrolyte.

[0055] In the quenching method, a method is usually used in which the molten material is directly or indirectly brought into contact with a refrigerant. The difference between the temperature of the molten material and the temperature of the refrigerant is, for example, 80° C. or more, may be 100° C. or more, or may be 120° C. or more. For example, when the temperature of the molten material is 160° C. and the molten material is exposed to room temperature (refrigerant temperature 25° C.), the temperature difference between the two is 135° C.

[0056] The cooling rate in the quenching step is, for example, 3°C / min or more, may be 10°C / min or more, or may be 100°C / min or more. Here, the cooling rate refers to an average cooling rate obtained by dividing the difference between the temperature of the melt before quenching and the temperature of the solid electrolyte after quenching (for example, 50°C) by the quenching time (for example, the time until it reaches 50°C). If the cooling rate is too slow, it is presumed that a crystalline phase that cannot contribute to ion conduction will be formed. In addition, the quenching may be performed at a temperature at which the melt solidifies, but may be, for example, cooled to 50°C or less, or may be cooled to room temperature (25°C). The quenching time in the quenching step is, for example, 1 second or more and 45 minutes or less. Specific quenching methods include, for example, a method of exposing the melt to room temperature, a method of contacting a container containing the melt with a liquid such as water or ice water, and a method of contacting the melt with a rotating metal roll.

[0057] C. All-solid-state battery Fig. 2 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. The all-solid-state battery 10 shown in Fig. 2 has a positive electrode active material layer 1, a negative electrode active material layer 2, and a solid electrolyte layer 3 disposed between the positive electrode active material layer 1 and the negative electrode active material layer 2, and at least one of the positive electrode active material layer 1, the negative electrode active material layer 2, and the solid electrolyte layer 3 contains the above-mentioned solid electrolyte. The all-solid-state battery 10 also has a positive electrode current collector 4 that collects current from the positive electrode active material layer 1, and a negative electrode current collector 5 that collects current from the negative electrode active material layer 2.

[0058] According to the present disclosure, at least one of the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer contains the above-mentioned solid electrolyte, resulting in an all-solid-state battery with good input and output characteristics.

[0059] 1.Cathode active material layer The positive electrode active material layer in the present disclosure contains at least a positive electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary.

[0060] The positive electrode active material may be, for example, an oxide active material. Examples of the oxide active material include LiCoO2, LiNi1 / 3 Co 1 / 3 Mn 1 / 3 Examples of such active materials include rock salt layered active materials such as O2, spinel type active materials such as LiMn2O4, and olivine type active materials such as LiFePO4.

[0061] The solid electrolyte may be a conventional solid electrolyte used in a solid-state battery, but is preferably the solid electrolyte of the present disclosure. The conductive material may be, for example, a carbon material such as acetylene black (AB). The binder may be, for example, a rubber-based binder or a fluoride-based binder. The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0062] 2.Negative electrode active material layer The negative electrode active material layer contains at least a negative electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary.

[0063] Examples of the negative electrode active material include metal active materials (simple substances or alloys) such as Si, Sn, Li, In, and Al, carbon active materials such as graphite, and oxide active materials such as lithium titanate.

[0064] As the solid electrolyte, a conventionally known solid electrolyte used in an all-solid-state battery can be used, but the above-mentioned solid electrolyte in the present disclosure is preferable. The conductive material and binder are the same as those described in "1. Positive electrode active material layer", so the description here is omitted. The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0065] 3.Solid electrolyte layer The solid electrolyte layer contains at least a solid electrolyte, and may contain a binder as necessary.

[0066] As the solid electrolyte, a conventionally known solid electrolyte used in an all-solid-state battery can be used, but the solid electrolyte in the present disclosure described above is preferable. The binder is the same as that described in "1. Positive electrode active material layer", so the description here is omitted. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.

[0067] 4. Positive and negative electrode current collectors The all-solid-state battery in the present disclosure usually has a positive electrode current collector that collects the positive electrode active material layer and a negative electrode current collector that collects the negative electrode active material layer. The positive electrode current collector and the negative electrode current collector are not particularly limited, and may be conventionally known positive electrode current collectors and negative electrode current collectors used in all-solid-state batteries. Examples of the positive electrode current collector include Al and SUS. Examples of the negative electrode current collector include Cu and Ni. The thickness and shape of the positive electrode current collector and the negative electrode current collector can be appropriately selected depending on the application of the all-solid-state battery.

[0068] 5.All-solid-state battery The all-solid-state battery in the present disclosure is typically an all-solid-state lithium-ion secondary battery. The use of the all-solid-state battery is not particularly limited, but examples thereof include power sources for vehicles such as hybrid electric vehicles (HEVs), electric vehicles (BEVs), gasoline-powered vehicles, and diesel-powered vehicles. In particular, it is preferable to use the all-solid-state battery as a driving power source for hybrid electric vehicles or electric vehicles. In addition, the all-solid-state battery in the present disclosure may be used as a power source for moving objects other than vehicles (for example, railways, ships, and aircraft), and may be used as a power source for electrical products such as information processing devices.

[0069] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0070] [Example 1] (Synthesis of solid electrolyte) Pyr14CB9H is a matrix containing organic cations and boron cluster anions. 10 As a metal salt, LiCB9H 10 and LiCB 11 H 12 These were prepared as Pyr14CB9H 10 : LiCB9H 10 :LiCB 11 H 12 The mixture was weighed and mixed so as to have a molar ratio of 2:4:4. Next, the mixture was heated and mixed at 160°C for 6 hours. After 30 minutes, the melt was removed from the heating device and rapidly cooled to room temperature. Thus, a solid electrolyte was synthesized.

[0071] (Preparation of evaluation cells) The synthesized solid electrolyte was formed into a pellet using a press pressure of 20 kN, which was then sandwiched between Al foils to prepare an evaluation cell.

[0072] [Comparative Example 1] A solid electrolyte and an evaluation cell were prepared in the same manner as in Example 1, except that the heating and mixing time was 15 hours, after which the heating device was turned off and the mixture was gradually cooled to room temperature on the heating device over a period of 2 hours.

[0073] [evaluation] (X-ray diffraction measurement) The solid electrolytes obtained in Example 1 and Comparative Example 1 were subjected to X-ray diffraction (XRD) measurement using CuKα radiation. The results of the XRD measurement are shown in FIG. 3. In addition, from the results of the XRD measurement, the standard value 1((I A -I S ) / I S ) and standard value 2 ((I B -I S ) / I S The results are shown in Table 1. S The intensity at 2θ=12.0° was used.

[0074] (Ionic conductivity measurement) The ionic conductivity at 25° C. was calculated by an AC impedance method for the evaluation cells obtained in Example 1 and Comparative Example 1. The results are shown in Table 1.

[0075] [Table 1]

[0076] As shown in Table 1, the ion conductivity of Example 1 was higher than that of Comparative Example 1. Also, as shown in Table 1 and FIG. 3, in Example 1, both the standard value 1 and the standard value 2 were larger than those of Comparative Example 1. Also, as shown in FIG. 3, in Example 1, the intensity of the peak A obtained at 2θ=15.7° was the largest, and the intensity of the peak B obtained at 2θ=18.2° was the next largest. On the other hand, in Comparative Example 1, the intensity of the peak obtained at 2θ=17.4° was the largest. Also, in Comparative Example 1, a peak that was not observed in Example 1 was confirmed near 2θ=16.1°. From this result, it was confirmed that the solid electrolyte of Example 1 has a crystal phase different from that of the solid electrolyte of Comparative Example 1. [Explanation of symbols]

[0077] 1...Cathode active material layer 2...Negative electrode active material layer 3...Solid electrolyte layer 4...Positive electrode current collector 5...Negative electrode current collector 10...All-solid-state battery

Claims

1. a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion; and a metal salt containing a metal cation and an anion, In an X-ray diffraction measurement using CuKα radiation, the solid electrolyte has a peak A appearing at a position of 2θ=15.7°±0.5° and a peak B appearing at a position of 2θ=18.2°±0.5°, A solid electrolyte, wherein, among all peaks observed in the X-ray diffraction measurement, the intensity of the peak A is the largest and the intensity of the peak B is the second largest.

2. a matrix containing a pyrrolidinium-based organic cation and a boron cluster anion; and a metal salt containing a metal cation and an anion, In an X-ray diffraction measurement using CuKα radiation, the solid electrolyte has a peak A appearing at a position of 2θ=15.7°±0.5° and a peak B appearing at a position of 2θ=18.2°±0.5°, The intensity of the peak A is I A and the intensity of the peak B is I B and the intensity at the reference position is I S A solid electrolyte, which satisfies the following conditions (i) and (ii): Condition (i): (I A -I S ) / I S is greater than 2.

69. Condition (ii): (I B -I S ) / I S is greater than 0.

73.

3. 3. The solid electrolyte according to claim 2, wherein, among all peaks observed in the X-ray diffraction measurement, the intensity of the peak A is the largest and the intensity of the peak B is the second largest.

4. The above (I A -I S ) / I SThe solid electrolyte according to claim 2 or 3, wherein the σ is 7.74 or more.

5. The above (I B -I S ) / I S The solid electrolyte according to any one of claims 2 to 4, wherein the σ is 3.16 or more.

6. 6. The solid electrolyte according to claim 1, wherein the anion in the metal salt is a boron cluster anion.

7. A method for producing a solid electrolyte according to any one of claims 1 to 6, comprising the steps of: a preparation step of preparing a precursor containing the matrix containing the pyrrolidinium-based organic cation and the boron cluster anion, and the metal salt containing the metal cation and the anion; a heating step of heating the precursor at a temperature equal to or higher than the melting temperature of the matrix to obtain a melt of the precursor; and a quenching step of quenching the molten material to solidify it, thereby obtaining the solid electrolyte.

8. An all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, An all-solid-state battery, wherein at least one of the positive electrode active material layer, the negative electrode active material layer and the solid electrolyte layer contains the solid electrolyte according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Solid electrolyte material and molded body thereof

    JP2020064832A

  • Batteries with soft materials based on boron compounds

    JP2020194769A

  • Method for synthesizing and optimizing novel soft materials on the basis of boron compounds

    JP2020194772A

  • Novel soft materials on the basis of boron compounds

    JP2020194777A

  • All-solid battery

    JP2021086720A