Release Film
The release film with a smooth and solvent-resistant release layer effectively prevents defects and ensures easy peeling of ultra-thin ceramic green sheets by combining (meth)acrylic acid ester and silicone components, addressing the issues of pinholes and breakage in existing technologies.
Patent Information
- Application Number
- JP2023174544
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2037-10-12
AI Technical Summary
Existing release films fail to effectively prevent defects such as pinholes and thickness unevenness in ultra-thin ceramic green sheets, and the peeling process often results in breakage due to insufficient solvent resistance and elastic modulus.
A release film with a release layer having a surface area average roughness of 7 nm or less, a maximum protrusion height of 50 nm or less, and an elastic modulus of 4.0 GPa or more, composed of a (meth)acrylic acid ester and silicone-based components, ensuring compatibility and resistance to solvents.
The film prevents defects in ceramic green sheets and allows for smooth peeling without breakage, maintaining consistent peeling force throughout the manufacturing process.
Smart Images

Figure 0007563550000003 
Figure 0007563550000001 
Figure 0007563550000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a release film used for producing a ceramic green sheet. [Background technology]
[0002] Conventionally, multilayer ceramic products such as multilayer ceramic capacitors and multilayer ceramic substrates have been produced by forming ceramic green sheets, stacking a plurality of the resulting ceramic green sheets, and firing the stacked sheets.
[0003] The ceramic green sheet is formed by coating a ceramic slurry containing a ceramic material such as barium titanate or titanium oxide on a release film. The release film used is a film substrate that has been subjected to a release treatment with a silicone compound such as polysiloxane. This release film is required to have releasability that allows the thin ceramic green sheet formed on the release film to be peeled off from the release film without breaking.
[0004] In recent years, with the miniaturization and high performance of electronic devices, multilayer ceramic capacitors and multilayer ceramic substrates have become smaller and more multilayered, and ceramic green sheets have become ultra-thin. When a ceramic green sheet becomes ultra-thin and its thickness after drying is, for example, 1 μm or less, defects such as pinholes and uneven thickness tend to occur in the ceramic green sheet when a ceramic slurry is applied and dried. In addition, when the molded ceramic green sheet is peeled off from the release film, defects such as breakage due to a decrease in the strength of the ceramic green sheet tend to occur.
[0005] In order to solve the former problem, Patent Document 1 proposes the use of a carrier film (release film) having a surface with a maximum height Rmax of 0.2 μm or less on the surface to which the ceramic slurry is applied, as defined by JIS B0601. However, even if a release film with a specified maximum height Rmax is used as in Patent Document 1, it is not possible to effectively prevent defects such as pinholes and uneven thickness from occurring in the thinned ceramic green sheet. In addition, there are still problems such as breakage of the ceramic green sheet when the thinned ceramic green sheet is peeled off from the release film.
[0006] It has also been proposed that the surface of the release layer becomes highly smooth, mainly due to the cured product of the active energy ray-curable component, and that the occurrence of defects such as pinholes and uneven thickness in the ceramic green sheet can be effectively prevented or suppressed. It has also been proposed that when the release layer contains a silicone-based component or its cured product and has an elastic modulus of 4.0 GPa or more, the ceramic green sheet can be normally peeled off from the release film (see Patent Document 2).
[0007] However, even if a release film with the surface properties and elastic modulus as in Patent Document 2 is used, problems still exist, such as the release layer being eroded by the solvent in the slurry when applying the green sheet and then forming electrodes thereon, causing the peeling force of the green sheet to become too strong, resulting in the green sheet breaking or not being able to be peeled off. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2003-203822 A [Patent Document 2] International Publication No. 2013 / 145865 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a release film for producing ceramic green sheets, which prevents or suppresses the occurrence of defects such as pinholes and uneven thickness in ceramic green sheets, and has excellent solvent resistance to solvents such as those used in ceramic slurry when molding ceramic green sheets and those used in electrode slurry when forming electrodes, thereby providing excellent peelability even when producing ultra-thin ceramic green sheets. [Means for solving the problem]
[0010] That is, the present invention comprises the following: 1. A release film for producing ceramic green sheets, comprising a release layer on at least one surface of a film substrate, wherein the surface of the release layer has an area average surface roughness (Sa) of 7 nm or less, and the absolute value of the difference (θ1-θ2) between the diiodomethane contact angle θ1 of the surface of the release layer and the diiodomethane contact angle θ2 of the surface of the release layer after the release film is immersed in toluene is 3.0° or less, and the elastic modulus of the surface of the release layer measured by a nanoindentation test is 4.0 GPa or more. 2. A release film for producing ceramic green sheets, as described in claim 1, wherein the release layer is a cured product of a release agent composition containing a (meth)acrylic ester and a silicone-based component, the maximum projection height (Rp) of the surface of the release layer is 50 nm or less, the area surface average roughness (Sa) of the surface of the film substrate opposite to the release layer is 5 to 50 nm, and the maximum projection height (Rp) is 30 to 1000 nm. 3. The release film for producing a ceramic green sheet according to the above item 2, wherein the mass ratio of the silicone-based component in the release agent composition to the total mass of the (meth)acrylic acid ester and the silicone-based component is 0.2 to 5 mass %. 4. The release film for producing a ceramic green sheet according to claim 2 or 3, wherein the silicone component is a polyorganosiloxane having a reactive functional group. 5. A release film for producing a ceramic green sheet according to any one of the above items 2 to 4, wherein the (meth)acrylic acid ester is a (meth)acrylate compound having three or more functional (meth)acryloyl groups. 6. The release film for producing a ceramic green sheet according to any one of the above 1 to 5, wherein the release layer has a thickness of 0.2 to 2 μm. 7. A release film for producing a ceramic green sheet, according to any one of claims 1 to 6, wherein the film substrate has a first layer substantially free of inorganic particles and a second layer containing inorganic particles, a release layer is provided on the first layer, the second layer forms the opposite surface of the film substrate, the inorganic particles contained in the second layer are silica particles and / or calcium carbonate particles, and the total amount of the inorganic particles contained in the second layer is 5,000 to 15,000 ppm. Effect of the Invention
[0011] According to the present invention, the surface of the release layer is highly smooth mainly due to the cured product of the (meth)acrylic acid ester, and the occurrence of defects such as pinholes and uneven thickness in the ceramic green sheet can be effectively prevented and suppressed. In addition, the release layer at the time of forming the ceramic green sheet contains a silicone-based component or its cured product, and the difference (θ1-θ2) between the diiodomethane contact angle θ1 of the release layer surface and the diiodomethane contact angle θ2 of the release layer surface after the release film is immersed in toluene is 3.0° or less in absolute value, so that the release layer is not eroded by the solvent of the slurry used in the ceramic green sheet manufacturing process, and the elastic modulus of the release layer is specified as above, so that the ceramic green sheet can always be normally peeled off from the release film for producing the ceramic green sheet.
[0012] Therefore, according to the release film for producing a ceramic green sheet of the present invention, the surface of the release layer becomes highly smooth, and the occurrence of defects such as pinholes and uneven thickness in the ceramic green sheet can be effectively prevented or suppressed, and further, the release film has excellent releasability from the ceramic green sheet. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view of a release film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described. As shown in Fig. 1, a release film for producing a ceramic green sheet (hereinafter, may be simply referred to as "release film") 1 according to one embodiment of the present invention is configured to include a film substrate 13 and a release layer 14 laminated on a surface 111 (upper surface in Fig. 1) of a first layer 11 of the film substrate 13. It is preferable that the substrate film 13 has a second layer 12 that forms a surface opposite to the surface 111 of the first layer 11 of the substrate film 13.
[0015] The film substrate 13 in the release film 1 according to the present embodiment is not particularly limited, and any one of the conventionally known ones can be appropriately selected and used. Examples of such a film substrate 13 include films made of plastics such as polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polypropylene and polymethylpentene, polycarbonate, and ethylene-vinyl acetate copolymers, and may be a single layer or a multilayer of two or more layers of the same or different kinds. Among these, polyester films are preferred, polyethylene terephthalate films are particularly preferred, and biaxially stretched polyethylene terephthalate films are even more preferred. Polyethylene terephthalate films are less likely to generate dust during processing, use, etc., and therefore, for example, ceramic slurry coating defects due to dust, etc. can be effectively prevented.
[0016] In addition, in this film substrate 13, the surface 111 of the first layer 11 can be subjected to a surface treatment such as an oxidation method or a primer treatment in order to improve adhesion to the release layer 14 provided on the surface 111 of the first layer 11. Examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromium oxidation treatment (wet), flame treatment, hot air treatment, ozone, and ultraviolet irradiation treatment. These surface treatment methods are appropriately selected depending on the type of substrate film, but generally, corona discharge treatment is preferably used in terms of effectiveness and operability.
[0017] The thickness of the film substrate 13 may usually be 10 to 250 μm, preferably 15 to 100 μm, and particularly preferably 20 to 50 μm.
[0018] The area surface average roughness (Sa) of the surface 111 of the first layer 11 of the film substrate 13 is preferably 2 to 40 nm, and more preferably 5 to 30 nm. The maximum projection height (Rp) of the surface 111 of the first layer 11 of the film substrate 13 is preferably 10 to 500 nm, and more preferably 30 to 300 nm. By setting the area surface average roughness (Sa) and maximum projection height (Rp) of the surface 111 of the first layer 11 of the film substrate 13 in the above ranges, it becomes easy to keep the area surface average roughness (Sa) and maximum projection height (Rp) of the surface of the release layer 14 within the ranges described below.
[0019] Meanwhile, the regional surface average roughness (Sa) of surface 112 (the surface opposite to the surface of the first layer; the lower surface in FIG. 1; sometimes referred to as the "rear surface") of second layer 12 of film substrate 13 is 5 to 50 nm, and preferably 10 to 30 nm. Also, the maximum projection height (Rp) of surface 112 of second layer 12 of film substrate 13 is 30 to 1000 nm, and preferably 50 to 300 nm.
[0020] It is preferable that the area surface average roughness (Sa) of the surface 112 of the second layer 12 of the film substrate 13 is 5 nm or more, since the surface of the second layer is not too smooth and there is no risk of blocking between the surface 112 of the second layer 12 of the film substrate 13 and the highly smooth release layer 14 when the release film 1 is wound up. On the other hand, it is preferable that the area surface average roughness (Sa) of the surface 112 of the second layer 12 of the film substrate 13 is 50 nm or less, since it is easy to keep the maximum projection height (Rp) of the surface 112 of the second layer 12 of the substrate 13 within the above-mentioned preferable low range.
[0021] When the maximum protrusion height (Rp) on the surface 112 of the second layer 12 of the film substrate 13 is 1000 nm or less, when the ceramic green sheet is formed and wound up, the protrusion shape on the surface 112 of the second layer 12 of the film substrate 13 that is in close contact with the ceramic green sheet is not transferred to the ceramic green sheet, the ceramic green sheet does not become thin in parts, and when the ceramic green sheets are laminated to produce a capacitor, there is no risk of a defect due to a short circuit, which is preferable. On the other hand, when the maximum protrusion height (Rp) on the surface 112 of the second layer 12 of the film substrate 13 is 30 nm or more, the unevenness on the surface 112 of the second layer 12 of the film substrate 13 is not too uniform, and the surface 112 of the second layer 12 does not become too flat, so that the surface of the film substrate 13 that contacts the roll is likely to entrain air in the process of forming the release layer 14, etc. As a result, the film substrate 13 does not meander during transportation, and also does not slip when wound into a roll, which is preferable.
[0022] Furthermore, by setting the regional surface average roughness (Sa) and maximum protrusion height (Rp) of the surface 112 of the second layer 12 of the film substrate 13 within the above-mentioned ranges, winding slippage during winding can be effectively suppressed, making it unnecessary to increase the winding tension, and thereby making it possible to suppress deformation of the winding core portion caused by the winding tension.
[0023] In addition, a layer the same as the release layer 14 described below, or a layer different from the release layer 14, may be provided on the side opposite to the surface 111 of the first layer 11 of the film substrate 13 (surface 112 of the second layer 12).
[0024] In order to obtain a film in which the maximum projection height (Rp) of the surface 111 of the first layer 11 of the film substrate 13 and the maximum projection height (Rp) of the surface 112 of the second layer 12 are both within the above-mentioned preferred range, a film substrate 13 may be used in which the maximum projection height (Rp) of the surface of the first layer 13 and the maximum projection height (Rp) of the surface 112 of the second layer 12 are different, i.e., the front and back have different roughnesses, or a film substrate 13 in which the maximum projection height (Rp) of the surface 111 of the first layer 11 and the maximum projection height (Rp) of the surface 112 of the second layer 12 are substantially the same, i.e., the front and back have the same roughnesses.
[0025] The film substrate may be a single layer or a multilayer of two or more layers, but preferably has a first layer that does not substantially contain inorganic particles on at least one side. In the case of a laminated film consisting of a multilayer structure of two or more layers, it is preferable to have a second layer that can contain particles, etc. on the opposite side of the release layer of the first layer that does not substantially contain inorganic particles. As for the laminate structure, if the layer on the side where the release layer is applied is the first layer, the layer on the opposite side is the second layer, and the core layer other than these is the third layer, the layer structure in the thickness direction can be a laminate structure such as release layer / first layer / second layer, or release layer / first layer / third layer / second layer. Of course, the third layer may have a multi-layer structure. In addition, the second layer may not contain particles. In that case, it is preferable to provide a coat layer containing particles and a binder on the second layer in order to impart slip properties for winding the film into a roll.
[0026] In the film substrate of the present invention, the first layer forming the surface to which the release layer is applied is preferably substantially free of inorganic particles. Here, when an anchor coat layer or the like described below is provided on the first layer, it is preferable that the coat layer is substantially free of inorganic particles, and it is preferable that the area surface average roughness (Sa) after lamination of the coat layer is within the above range. In the present invention, "substantially free of inorganic particles" means that the content of inorganic elements is 50 ppm or less, preferably 10 ppm or less, and most preferably below the detection limit when the inorganic elements are quantified by fluorescent X-ray analysis. This is because even if inorganic particles are not actively added to the film, contaminants derived from foreign matter or dirt attached to the raw material resin or the line or equipment in the film manufacturing process may peel off and be mixed into the film.
[0027] In the film substrate of the present invention, the second layer forming the surface opposite to the surface to which the release layer is applied preferably contains particles from the viewpoint of the slipperiness of the film and the ease of air escape, and it is particularly preferable to use silica particles and / or calcium carbonate particles. The particle content contained is preferably 5000 to 15000 ppm in total of particles in the second layer. When the total of silica particles and / or calcium carbonate particles is 5000 ppm or more, air can be uniformly escaped when the film is wound up into a roll, and the rolled shape and flatness are good, making it suitable for the production of ultra-thin ceramic green sheets. In addition, when the total of silica particles and / or calcium carbonate particles is 15000 ppm or less, the lubricant is less likely to aggregate and coarse protrusions are not formed, which is preferable because the quality is stable when producing ultra-thin ceramic green sheets.
[0028] As the particles contained in the second layer, in addition to silica and / or calcium carbonate, inactive inorganic particles and / or heat-resistant organic particles can be used. From the viewpoint of transparency and cost, it is more preferable to use silica particles and / or calcium carbonate particles, but other inorganic particles that can be used include alumina-silica composite oxide particles and hydroxyapatite particles. In addition, examples of heat-resistant organic particles include crosslinked polyacrylic particles, crosslinked polystyrene particles, and benzoguanamine particles. In addition, when silica particles are used, porous colloidal silica is preferred, and when calcium carbonate particles are used, light calcium carbonate that has been surface-treated with a polyacrylic acid-based polymer compound is preferred from the viewpoint of preventing the lubricant from falling off.
[0029] The average particle size of the particles added to the second layer is preferably 0.1 μm or more and 2.0 μm or less, and particularly preferably 0.5 μm or more and 1.0 μm or less. If the average particle size of the particles is 0.1 μm or more, the slipperiness of the release film is good, which is preferable. In addition, if the average particle size is 2.0 μm or less, there is no risk of pinholes being generated in the ceramic green sheet due to coarse particles on the surface of the release layer, which is preferable.
[0030] The second layer may contain two or more types of particles made of different materials, or may contain the same type of particles having different average particle sizes.
[0031] The average particle size of the particles is measured by observing the particles on the cross section of the processed film with a transmission electron microscope or a scanning electron microscope, observing 100 non-aggregated particles, taking the maximum diameter of each particle as the particle size, and averaging these to determine the average particle size.
[0032] When the second layer does not contain particles, it is preferable to provide the second layer with a coating layer containing particles to provide easy slipping. This coating layer is not particularly limited, but is preferably provided by in-line coating during film production. When the second layer does not contain particles and has a coating layer containing particles on the second layer, the surface of the coating layer preferably has a regional surface average roughness (Sa) in the range of 5 to 50 nm for the same reason as the regional surface average roughness (Sa) of the second layer described above.
[0033] From the viewpoint of reducing pinholes, it is preferable that the first layer, which is the layer on which the release layer is to be formed, does not use recycled materials or the like in order to prevent contamination with particles of lubricants or the like.
[0034] The thickness ratio of the first layer, which is the layer on which the release layer is provided, is preferably 20% to 50% of the total thickness of the base film. If it is 20% or more, the film is less susceptible to the effects of particles contained in the second layer, etc. from the inside, and it is easy for the area surface average roughness Sa to satisfy the above range, which is preferable. If it is 50% or less of the total thickness of the base film, the usage ratio of recycled raw materials in the second layer can be increased, which is preferable because it reduces the environmental load.
[0035] From the viewpoint of economic efficiency, the layers other than the first layer (the second layer or the third layer) may be made of 50 to 90% by mass of recycled raw materials such as film scraps and PET bottles. Even in this case, it is preferable that the type and amount of the lubricant contained in the second layer, the particle size, and the area surface average roughness (Sa) satisfy the above ranges.
[0036] In addition, in order to improve the adhesion of a release layer or the like that will be applied later, or to prevent static electricity, a coating layer may be provided on the surface of the first layer and / or the second layer before stretching or after uniaxial stretching in the film-forming process, and corona treatment, etc. may also be performed.
[0037] The release layer 14 in the release film 1 according to this embodiment is a cured product obtained by curing a release agent composition (hereinafter referred to as "release agent composition") containing a (meth)acrylic acid ester and a silicone-based component. According to such a release agent composition, the concave portions between the protrusions present on the surface 111 of the first layer 11 of the film substrate 13 can be effectively filled mainly by the cured product of the (meth)acrylic acid ester, and the surface of the obtained release layer 14 can be made highly smooth, and the silicone-based component or its cured product can impart appropriate releasability to the surface of the release layer 14. Furthermore, since the coating of the release agent composition can be cured by irradiation with active energy rays during the production of the release film 1, the occurrence of damage such as shrinkage or deformation of the substrate can be suppressed compared to the case where a thermosetting release agent composition is used.
[0038] Incidentally, conventional silicone resin-based release agents tend to conform to the surface shape of the film substrate 13, and do not provide a smoothing effect like that of the release agent composition. Conventionally, in certain resin films, particularly polyester-based films, the addition of a filler is essential to impart surface slipperiness and mechanical strength, but there is a limit to reducing the density of high protrusions caused by such fillers through improvements in film production methods. In contrast, by highly smoothing the surface of the release layer 14 with the cured product of (meth)acrylic acid ester as described above, the density of high protrusions on the surface of the release layer 14 can be reduced, and a release film 1 having a highly smooth surface can be obtained. In addition, the release layer formed by the conventional silicone resin-based release agent has a low elastic modulus and is easily deformed, so that when the molded ceramic green sheet is peeled off, the release layer deforms and conforms to the ceramic green sheet, which increases the peeling force, and the ceramic green sheet may not be peeled off normally.
[0039] The (meth)acrylic acid ester of the release agent composition is not particularly limited as long as it is a component that is cured by irradiation with active energy rays without impeding the effects of the present invention, and may be any of a monomer, an oligomer, or a polymer, or a mixture thereof. This (meth)acrylic acid ester is preferably a (meth)acrylate-based compound. In this specification, the (meth)acrylate-based compound means both an acrylate-based compound and a methacrylate-based compound. The same applies to other similar terms. If the main component of the release layer 14 is a cured product of a (meth)acrylic acid ester-based component, the release layer 14 is less likely to repel the ceramic slurry.
[0040] The (meth)acrylate compound is preferably at least one selected from polyfunctional (meth)acrylate monomers and (meth)acrylate oligomers, particularly preferably at least one selected from trifunctional or higher (meth)acrylate monomers and (meth)acrylate oligomers, and more preferably a trifunctional or higher (meth)acrylate monomer. By being trifunctional or higher, the curability of the release agent composition is excellent, and the surface of the resulting release layer 14 has better releasability. More preferably, it is 6-functional or higher, particularly preferably 7-functional or higher, and most preferably 9-functional or higher. There is no particular upper limit to the number of functional groups, but it is preferably 20 or less. By making it 20 or less, intramolecular reactions tend to proceed more easily than intermolecular crosslinking reactions, and there is no risk of not being able to obtain the effect of improving the crosslink density, which is preferable.
[0041] Examples of polyfunctional (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tris((meth)acryloxyethyl)isocyanurate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, etc. These may be used alone or in combination of two or more.
[0042] Examples of the polyfunctional (meth)acrylate oligomer include polyester acrylate oligomers, epoxy acrylate oligomers, urethane acrylate oligomers, polyether acrylate oligomers, polybutadiene acrylate oligomers, and silicone acrylate oligomers.
[0043] The polyester acrylate oligomer can be obtained, for example, by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends, which is obtained by condensation of a polycarboxylic acid and a polyhydric alcohol, with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an alkylene oxide to a polycarboxylic acid, with (meth)acrylic acid.
[0044] The epoxy acrylate oligomer can be obtained, for example, by reacting (meth)acrylic acid with the oxirane ring of a relatively low molecular weight bisphenol epoxy resin or novolac epoxy resin to esterify it. In addition, a carboxyl-modified epoxy acrylate oligomer obtained by partially modifying an epoxy acrylate oligomer with a dibasic carboxylic acid anhydride can also be used.
[0045] The urethane acrylate oligomer can be obtained, for example, by esterifying a polyurethane oligomer obtained by reacting a polyether polyol or polyester polyol with a polyisocyanate with (meth)acrylic acid.
[0046] The polyether acrylate oligomer can be obtained by esterifying the hydroxyl groups of a polyether polyol with (meth)acrylic acid.
[0047] The above-mentioned polyfunctional (meth)acrylate monomers and polyfunctional (meth)acrylate oligomers can be used alone or in combination of two or more. Also, the polyfunctional (meth)acrylate monomers and polyfunctional (meth)acrylate oligomers can be used in combination.
[0048] In the release agent composition, the (meth)acrylic acid ester may be used alone or in combination of two or more kinds.
[0049] The silicone-based component of the release agent composition is not particularly limited as long as it can impart the desired releasability to the surface of the release layer 14 without impeding the effects of the present invention, and polyorganosiloxane, preferably polyorganosiloxane having a reactive functional group, particularly preferably polydimethylsiloxane having a reactive functional group, is used, but it can be said that a combination of polydimethylsiloxane compatible with (meth)acrylic acid ester is preferable. In the case of a combination with poor compatibility, the polyorganosiloxane is liberated on the surface of the release layer and the reactivity with the active energy curable component is reduced, so that it appears to show excellent release properties, but when used in the ceramic capacitor green sheet manufacturing process and the electrode printing process, the polyorganosiloxane is eroded by the dilution solvent of the slurry, and when the release film for manufacturing the ceramic capacitor green sheet is peeled off, it becomes difficult to peel or cannot be peeled off. On the other hand, when it is completely compatible, the amount of polyorganosiloxane liberated on the surface is extremely reduced, and the peeling force is not reduced. With the appropriate compatibility, the reactive functional group of the polyorganosiloxane reacts with the active energy ray curable resin, and the polyorganosiloxane (silicone-based component) is incorporated into the crosslinked structure and fixed. This prevents the silicone-based component in the release layer 14 from transferring to the ceramic green sheet molded on the release layer 14.
[0050] As a method for adjusting the compatibility between the polyorganosiloxane as the silicone component of the release agent composition and the (meth)acrylic acid ester as the binder, a method of selecting a type in which polydimethylsiloxane is added to the side chain of the acrylic main chain, which has better compatibility with the (meth)acrylic acid ester as the binder, compared to the polydimethylsiloxane with the silicone main chain, can be mentioned. In addition, even if the main chain is polydimethylsiloxane of silicone, it is possible to achieve moderate compatibility with the binder by selecting a polyorganosiloxane with appropriate polarity. The polarity of polyorganosiloxane can be referred to, for example, the BYK Coating and Ink Additives Catalog (2016.06 (44th edition)).
[0051] When the main chain of the silicone-based component of the release agent composition is polyorganosiloxane, the reactive functional group may be introduced at one end of the polyorganosiloxane, at both ends, or at the side chain. Examples of the reactive functional group include (meth)acryloyl group, vinyl group, maleimide group, epoxy group, carboxyl group, isocyanate group, and hydroxyl group. Among them, (meth)acryloyl group, vinyl group, and maleimide group, which can be cured at the same time when the (meth)acrylic acid ester is cured (when irradiated with active energy rays), are preferred. It is preferred that at least two or more of these reactive functional groups are introduced into one molecule of polyorganosiloxane. In addition, two or more types of these reactive functional groups may be introduced into one molecule of polyorganosiloxane.
[0052] The release agent having a polyorganosiloxane main chain used in the present invention may be a commercially available product. Examples of commercially available products include BYK-UV3505, BYK-UV3575, and BYK-UV3500 (manufactured by BYK). In the present invention, it is preferable to select an appropriate polyorganosiloxane type to improve compatibility depending on the type of binder used.
[0053] When the main chain of the silicone-based component of the release agent composition is acrylic, it is preferable to use an ultraviolet-curable acrylic copolymer having a (meth)acryloyl group and a polyorganosiloxane group in one molecule.
[0054] When an ultraviolet ray curable acrylic copolymer having a (meth)acryloyl group and a polyorganosiloxane group in one molecule is used as a release agent, it has more acrylic moieties than silicone-based oils such as polydimethylsiloxane, and therefore has improved compatibility with the binder component, and the curing property of the binder component and the release agent is improved in the release layer processing step, and the amount of unreacted release agent is reduced, which is preferable. Furthermore, by using an ultraviolet ray curable acrylic copolymer having a (meth)acryloyl group and a polyorganosiloxane group in one molecule, not only a crosslinked structure is formed between the binder component and the release agent, but also intermolecular interactions such as hydrogen bonds and van der Waals forces are formed, so that there is no risk of the release layer being eroded by organic solvents, which is preferable. In this specification, an ultraviolet ray curable acrylic copolymer having a (meth)acryloyl group and a polyorganosiloxane group in one molecule may be referred to as a (meth)acryloyl group-containing copolymerized acrylic silicone.
[0055] The ultraviolet-curable acrylic copolymer used in the present invention may be a commercially available product, such as GL-02R, GL-04R (manufactured by Kyoeisha Chemical Co., Ltd.), 8SS-723 (manufactured by Taisei Fine Chemical Co., Ltd.), and TA37-400A (manufactured by Hitachi Chemical Co., Ltd.).
[0056] In the release agent composition, the silicone-based component may be used alone or in combination of two or more kinds.
[0057] The mass ratio of the silicone-based component in the release agent composition to the total mass of the (meth)acrylic acid ester and the silicone-based component is preferably 0.2 to 5 mass%, and particularly preferably 1.0 to 2.5 mass%. In addition, by setting the composition and the mass ratio of the silicone-based component in the above range so that the difference (θ1-θ2) between the diiodomethane contact angle θ1 on the release layer surface and the diiodomethane contact angle θ2 on the release layer surface after the release film is immersed in toluene is 3.0° or less in absolute value, the ceramic slurry can be applied to the surface of the release layer 14 without being repelled, and the formed ceramic green sheet can be easily peeled off without breaking, and the release layer 14 has excellent peelability. If the mass ratio of the silicone-based component is 0.2 mass% or more, the release layer 14 can exhibit sufficient peeling performance, which is preferable. On the other hand, if the mass ratio of the silicone-based component is 5 mass% or less, the release layer 14 is easily cured and the elastic modulus of the release layer 14 is high, which is preferable. Furthermore, when ceramic slurry is applied to the surface of the release layer 14, the ceramic slurry is less likely to be repelled, which is preferable. Also, the release layer 14 becomes easier to harden, which is preferable in terms of peelability.
[0058] The mass ratio of the total mass of the (meth)acrylic acid ester and the silicone-based component to the total mass of the solid content contained in the release agent composition is preferably 85 mass% or more, and particularly preferably 90 mass% or more. When the mass ratio of the total mass of the (meth)acrylic acid ester and the silicone-based component is within the above range, the surface of the release layer 14 to be formed is made highly smooth, and it becomes easier to obtain sufficient curability of the release agent composition.
[0059] Here, when ultraviolet rays are used as the active energy rays to be irradiated to the release agent composition, it is preferable that the release agent composition further contains a photopolymerization initiator. By containing the photopolymerization initiator in this way, the (meth)acrylic acid ester (and the silicone-based component) can be cured efficiently, and the polymerization curing time and the amount of light irradiation can be reduced.
[0060] Specific examples of the photopolymerization initiator include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzyl, dibenzyl, diacetyl, β-chloroanthraquinone, (2,4,6-trimethylbenzyldiphenyl)phosphine oxide, and 2-benzothiazole-N,N-diethyldithiocarbamate. In particular, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methylpropan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, which are considered to have excellent surface curing properties, are preferred, and among these, 2-hydroxy-2-methyl-1-phenyl-propan-1-one and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one are particularly preferred. These may be used alone or in combination of two or more.
[0061] The photopolymerization initiator is preferably used in an amount of 1 to 20 parts by mass, particularly 3 to 15 parts by mass, per 100 parts by mass in total of the (meth)acrylic acid ester and the active energy ray-curable silicone component (e.g., polyorganosiloxane having a (meth)acryloyl group, a vinyl group, or a maleimide group as a reactive functional group).
[0062] The release agent (including the release agent composition) constituting the release layer 14 may contain silica, an antistatic agent, a dye, a pigment, and other additives as necessary. These additives are preferably used in an amount of 0.1 to 50 parts by mass relative to 100 parts by mass in total of the (meth)acrylic acid ester and the silicone component.
[0063] The thickness of the release layer 14 is preferably 0.2 to 2 μm, and particularly preferably 0.5 to 1.5 μm. If the thickness of the release layer 14 is less than 0.5 μm, oxygen inhibition occurs during curing of the release layer, and sufficient elastic modulus cannot be obtained, so it is preferable to cure the layer in an inert gas environment. On the other hand, if the thickness of the release layer 14 exceeds 2 μm, the release film 1 may be easily curled due to the cure shrinkage of the release layer 14. In addition, when the release film 1 is wound into a roll, blocking with the surface of the second layer of the substrate 13 is likely to occur, which may cause poor winding or increase the amount of charge when unwinding, making it easier for foreign matter to adhere.
[0064] The release layer 14 can be formed by applying a release agent solution containing a release agent and, if desired, a diluent, etc., to the surface of the first layer of the substrate 13, drying it as necessary, and curing it by irradiation with active energy rays. If the reactive functional group of the silicone-based component is one that reacts with heat, the reaction can be caused by drying at this time, and the silicone-based component can be incorporated into a crosslinked structure. Examples of methods that can be used to apply the release agent solution include gravure coating, bar coating, spray coating, spin coating, knife coating, roll coating, and die coating.
[0065] As the active energy ray, ultraviolet rays, electron beams, etc. are usually used. The irradiation amount of the active energy ray varies depending on the type of energy ray. For example, in the case of ultraviolet rays, the light amount is 50 to 1000 mJ / cm. 2 is preferable, and particularly 100 to 500 mJ / cm 2 In the case of electron beams, the dose is preferably about 10 to 500 kGy.
[0066] The (meth)acrylic acid ester in the release agent composition is cured by the irradiation of the active energy rays. In addition, when the silicone-based component in the release agent composition has a reactive group that is curable by active energy rays, the silicone-based component is also cured. As a result, a release layer 14 is formed that is highly smooth, does not easily repel ceramic slurry, and has excellent releasability for the ceramic green sheet.
[0067] In the release film 1 according to this embodiment, the surface of the release layer 14 (the upper surface in FIG. 1) on which the ceramic slurry is molded has an area surface average roughness (Sa) of 8 nm or less and a maximum projection height (Rp) of 50 nm or less. The area surface average roughness (Sa) and maximum projection height (Rp) in this specification are values measured using a non-contact surface shape measurement system (VertScan R550H-M100, manufactured by Ryoka Systems Co., Ltd.).
[0068] By setting the area surface average roughness (Sa) and maximum projection height (Rp) of the surface of the release layer 14 within the above ranges, the surface of the release layer 14 can be made sufficiently smooth, and even when a thin ceramic green sheet having a thickness of less than 1 μm is molded on the surface of the release layer 14, defects such as pinholes and thickness unevenness are unlikely to occur in the thin ceramic green sheet, and good sheet moldability is shown. In addition, by setting the area surface average roughness (Sa) and maximum projection height (Rp) of the surface of the release layer 14 within the above ranges, the peelability of the ceramic green sheet is also excellent, and even when a thin ceramic green sheet having a thickness of less than 1 μm is peeled off from the release layer 14, the ceramic green sheet is unlikely to break. These excellent effects cannot be obtained by simply specifying the maximum height (Rmax) of the release layer 14 as in Patent Document 1.
[0069] The surface characteristics of the release layer 14 are fixed by being incorporated into the crosslinked structure of the cured product of the (meth)acrylic acid ester when the polyorganosiloxane and the (meth)acrylic acid ester are cured by ultraviolet irradiation, but if the compatibility with the (meth)acrylic acid ester is poor, the surface characteristics are not sufficiently fixed, and problems such as heavy peeling occur when applying ceramic slurry or after the electrode printing process. Therefore, it is necessary that the absolute value of the difference (θ1-θ2) between the diiodomethane contact angle θ1 of the surface 121 of the release layer and the diiodomethane contact angle θ2 of the surface 121 of the release layer after the release film is immersed in toluene is 3.0° or less. If the compatibility between the (meth)acrylic acid ester and the silicone-based component is good, the absolute value of the difference (θ1-θ2) between the diiodomethane contact angle θ2 is 3.0 or less, which is preferable because a constant peeling force can be obtained regardless of the ceramic green sheet manufacturing process.
[0070] The surface average roughness (Sa) of the surface of the release layer 14 is preferably 7 nm or less, and more preferably 5 nm or less. The surface maximum protrusion height (Rp) of the release layer 14 is preferably 50 nm or less, and more preferably 30 nm or less.
[0071] The elastic modulus of the release layer 14 measured by a nanoindentation test is 4.0 GPa or more, preferably 4.2 GPa or more. When the elastic modulus of the release layer 14 is 4.0 GPa or more, the release layer 14 is less likely to deform, and therefore, when the ceramic green sheet is peeled off from the release layer 14, the release layer 14 is less likely to follow the ceramic green sheet, and therefore, the ceramic green sheet can be peeled off normally. On the other hand, when the elastic modulus of the release layer 14 is 4.0 GPa or more, when the ceramic green sheet is peeled off from the release layer 14, the release layer 14 is less likely to deform and to follow the ceramic green sheet, and therefore, the peeling force is reduced, and the ceramic green sheet can be peeled off normally, which is preferable. The high elastic modulus as described above can be preferably achieved by using a release agent composition for forming the release layer 14 and appropriately selecting and setting the type and amount of the (meth)acrylic acid ester.
[0072] In this specification, the elastic modulus of the release layer is measured by a nanoindentation test in an atmosphere of 23° C. Specifically, the back side of the substrate of the release film 1 cut to a size of 10 mm×10 mm is fixed with a two-liquid epoxy adhesive onto a glass plate attached to an aluminum base, and a microhardness evaluation device (in the test example, "NanoIndenter SA2" manufactured by MTS Corporation) is used to perform the measurement.
[0073] By using the release film 1 as described above in the manufacturing process of the ceramic green sheet, it is possible to effectively prevent or suppress the occurrence of defects such as pinholes and uneven thickness in the obtained ceramic green sheet, and also to effectively prevent or suppress the occurrence of problems such as breakage of the ceramic green sheet when peeling the ceramic green sheet from the release film 1.
[0074] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.
[0075] For example, as described above, other layers may be present between the substrate 13 and the release layer 14 or on the surface 112 of the second layer 12 of the substrate 13 . EXAMPLES
[0076] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.
[0077] (Laminated film x1) A biaxially oriented polyester film having a thickness of 31 μm, which contained substantially no inorganic particles, was used for surface 111 of first layer 11 of substrate 13. The area average surface roughness (Sa) of the surface of the first layer was 2 nm and the maximum projection height (Rp) was 25 nm, and the area average surface roughness (Sa) of the surface of the second layer was 28 nm and the maximum projection height (Rp) was 740 nm.
[0078] (Laminated film x2) A polyester film (Toyobo Ester (registered trademark) film E5101, manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was used. E5101 is a film containing inorganic particles. The area average surface roughness (Sa) of the surface of the first layer of the laminated film X2 was 24 nm, and the maximum projection height (Rp) was 770 nm, and the area average surface roughness (Sa) of the surface of the second layer was 24 nm, and the maximum projection height (Rp) was 770 nm.
[0079] Example 1 A coating solution having the composition shown below was applied to the surface 111 of the first layer of the laminated film X1 using a wire bar so that the release layer thickness after drying would be 0.8 μm. The coating solution was then dried at 90° C. for 15 seconds, and then irradiated with an ultraviolet ray irradiator (Heraeus, LC6B, H bulb) with an integrated light dose of 70 mJ / cm 2 . 2 A release film for producing ceramic green sheets was obtained by irradiating the film with ultraviolet rays of 1000 nm. The obtained release film was coated with ceramic slurry, and the surface roughness of the release layer, elastic modulus, change in contact angle before and after immersion in toluene, curling, blocking property, slurry coatability, peelability, etc. were evaluated, and good evaluation results were obtained. Isopropyl alcohol 59.40 parts by weight Methyl ethyl ketone 19.80 parts by mass Dipentaerythritol hexaacrylate 19.00 parts by mass (Product name: A-DPH, manufactured by Shin Nakamura Chemical Industry Co., Ltd., solid content 100% by mass) (Meth)acryloyl group-containing copolymer acrylic silicone 1.00 parts by mass (Product name: GL-04R, Kyoeisha Chemical Co., Ltd., solid content 20%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0080] Example 2 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the (meth)acryloyl group-containing copolymerized acrylic silicone was changed to an acryloyl group-containing polydimethylsiloxane (product name: BYK-UV3505, manufactured by BYK-Chemie Japan).
[0081] Example 3 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the (meth)acryloyl group-containing copolymerized acrylic silicone was changed to an acryloyl group-containing modified polydimethylsiloxane (product name: BYK-UV3575, manufactured by BYK-Chemie Japan).
[0082] Example 4 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the (meth)acryloyl group-containing copolymerized acrylic silicone was changed to a silicone-modified UV-curable release agent (product name: TA37-400A, manufactured by Hitachi Chemical Co., Ltd.).
[0083] Example 5 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the coating solution was changed to the composition shown below and applied to a film thickness of 2 μm. Isopropyl alcohol 60.00 parts by weight Methyl ethyl ketone 20.00 parts by mass Trifunctional acrylate 19.00 parts by mass (Product name: A-TMMT-3, manufactured by Shin-Nakamura Chemical Industry Co., Ltd., solid content 100% by mass) Acryloyl group-containing polyether-modified polydimethylsiloxane 0.20 parts by mass (Product name: BYK-UV3500, manufactured by BYK Japan, solid content 100%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0084] Example 6 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the coating liquid was changed to have the composition shown below. Isopropyl alcohol 60.00 parts by weight Methyl ethyl ketone 20.00 parts by mass 10-functional urethane acrylate 19.00 parts by weight (Product name: UV1700B, manufactured by Nippon Gosei Kagaku Kogyo Co., Ltd., solid content 100% by mass) Acryloyl group-containing polyether-modified polydimethylsiloxane 0.20 parts by mass (Product name: BYK-UV3500, manufactured by BYK Japan, solid content 100%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0085] Example 7 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the coating liquid was changed to have the composition shown below. Isopropyl alcohol 59.40 parts by weight Methyl ethyl ketone 19.80 parts by mass 10-functional urethane acrylate 19.00 parts by weight (Product name: UV1700B, manufactured by Nippon Gosei Kagaku Kogyo Co., Ltd., solid content 100% by mass) (Meth)acryloyl group-containing copolymer acrylic silicone 1.00 parts by mass (Product name: GL-04R, Kyoeisha Chemical Co., Ltd., solid content 20%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0086] Example 8 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the coating liquid was changed to have the composition shown below. Isopropyl alcohol 59.85 parts by weight Methyl ethyl ketone 19.95 parts by mass 10-functional urethane acrylate 19.00 parts by weight (Product name: UV1700B, manufactured by Nippon Gosei Kagaku Kogyo Co., Ltd., solid content 100% by mass) Acryloyl group-containing copolymerized acrylic silicone: 0.40 parts by mass (Product name: 8SS-723, Taisei Fine Chemical Co., Ltd., solid content 50%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0087] Example 9 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the coating liquid was changed to have the composition shown below. Isopropyl alcohol 59.40 parts by weight Methyl ethyl ketone 19.80 parts by mass 15-functional urethane acrylate 19.00 parts by weight (Product name: 8UX-015A, Taisei Fine Chemical Co., Ltd., solid content 100% by mass) (Meth)acryloyl group-containing copolymer acrylic silicone 1.00 parts by mass (Product name: GL-04R, Kyoeisha Chemical Co., Ltd., solid content 20%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0088] Example 10 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 7, except that coating was performed so that the release layer had a thickness of 0.5 μm.
[0089] Example 11 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 7, except that coating was performed so that the release layer had a thickness of 0.2 μm.
[0090] Example 12 A release film for producing a ceramic green sheet was obtained in the same manner as in Example 1, except that the laminate film X2 was used as the substrate 13.
[0091] Comparative Example 1 Except for changing the coating solution to the composition shown below, a release film for producing an ultrathin ceramic green sheet was obtained in the same manner as in Example 1. In Comparative Example 1, the solvent resistance near the surface of the release layer was poor, possibly due to poor compatibility between dipentaerythritol hexaacrylate and acryloyl group-containing polyether-modified polydimethylsiloxane used as the binder. Isopropyl alcohol 60.00 parts by weight Methyl ethyl ketone 20.00 parts by mass Dipentaerythritol hexaacrylate 19.00 parts by mass (Product name: A-DPH, manufactured by Shin Nakamura Chemical Industry Co., Ltd., solid content 100% by mass) Acryloyl group-containing polyether-modified polydimethylsiloxane 0.20 parts by mass (Product name: BYK-UV3500, manufactured by BYK Japan, solid content 100%) α-Aminoalkylphenone 0.80 parts by mass (Product name: IRGACURE907, manufactured by BASF, 100% active ingredient)
[0092] Comparative Example 2 A release film was prepared in the same manner as in Example 1, except that the thickness of the release agent layer was changed as shown in Table 1. In Comparative Example 2, the release layer was thin, and the surface curing inhibition specific to radical polymerization occurred significantly, which resulted in a low elastic modulus of the release layer. As a result, the peeling force became heavy.
[0093] Comparative Example 3 A release film was produced in the same manner as in Example 1, except that the mass ratio of the (meth)acrylic acid ester and the silicone-based component in the release agent composition C was changed as shown in Table 1. In Comparative Example 3, the mass ratio of the silicone-based component was high, so that the elastic modulus of the release layer was reduced and the solvent resistance of the release layer surface was also deteriorated. As a result, the peeling force became heavy.
[0094] Comparative Example 4 100 parts by mass of heat-curing addition reaction type silicone (product name: KS-847H, manufactured by Shin-Etsu Chemical Co., Ltd., solid content concentration 30%) was diluted with toluene, and 2 parts by mass of platinum catalyst (manufactured by Shin-Etsu Chemical Co., Ltd., CAT-PL-50T) was mixed therewith to prepare a release agent solution with a solid content of 5.0% by mass. The obtained release agent solution was uniformly applied to one side (surface of the first layer) of the same substrate as in Example 1 so that the thickness of the release agent layer formed after drying was 0.3 μm, and the solution was dried at 140° C. for 1 minute to form a release agent layer, which was used as a release film. In Comparative Example 4, since the silicone-based component was the main component, the elastic modulus of the release layer was significantly low and the solvent resistance was also significantly deteriorated. Therefore, the peeling force was too strong and the release was not possible.
[0095] [Test Example 1] (Release layer thickness measurement) The thickness (μm) of the release layer of the release film obtained in the examples and comparative examples was measured using a reflection type film thickness meter (F20, manufactured by Filmetrics). Specifically, the release film obtained in the examples and comparative examples was cut to 100×100 mm, and then the release film was placed on the film thickness meter so that the opposite side to the side to be measured was the suction stage side, and the film thickness was measured at 10 points on the surface of the release layer, and the average value was taken as the thickness of the release layer. The results are shown in Table 1.
[0096] [Test Example 2] (Measurement of surface roughness) The values were measured under the following conditions using a non-contact surface shape measurement system (VertScan R550H-M100, manufactured by Ryoka Systems Co., Ltd.). The area surface average roughness (Sa) was calculated by averaging five measurements, and the maximum protrusion height (Rp) was calculated by measuring seven times and using the maximum of the five measurements excluding the maximum and minimum values. (Measurement conditions) Measurement mode: WAVE mode Objective lens: 10x 0.5×Tube lens ·Measurement area 936μm×702μm (Analysis conditions) Area correction: 4th order correction Interpolation: Fully interpolated
[0097] [Test Example 3] (Elasticity measurement) The release films obtained in the examples and comparative examples were cut into 10 mm x 10 mm size, and then the back surface of the substrate of the cut release film was fixed with a two-liquid epoxy adhesive on a glass plate attached to an aluminum base. Then, using a microhardness evaluation device (MTS, NanoIndenter SA2), a nanoindentation test was performed under the following conditions: maximum indentation depth of the indenter 100 nm, strain rate of 0.05 sec-1, displacement amplitude of 2 nm, vibration frequency of 45 Hz, and an atmosphere of 23°C, to measure the elastic modulus of the release layer of the release film. The results are shown in Table 1.
[0098] [Test Example 4] (Evaluation of change in contact angle of release layer) For the release films obtained in the examples and comparative examples, a droplet of diiodomethane (droplet volume 0.9 μL) was created on the release layer surface of the release film that was left stationary using a contact angle meter (Kyowa Interface Science Co., Ltd., fully automatic contact angle meter DM-701) under conditions of 25°C and 50% RH, and the contact angle was measured. The contact angle was measured 30 seconds after the drop on the release film, and the average value of the values measured five times was used. Next, the release film to be used for measurement was cut into a size of 5 cm x 5 cm, and immersed for 5 minutes with the release layer surface facing down in a glass tray containing 30 mL of toluene at a liquid temperature of 25 ° C. The immersed release film was taken out, air-dried for 15 minutes with the release layer surface facing up, and then vacuum-dried overnight at 25 ° C. The release film thus obtained after immersion in toluene was measured by the same method as the above-mentioned method for measuring the contact angle. The initial contact angle of diiodomethane on the release layer surface before immersion in toluene measured by the above method was θ1, and the contact angle of diiodomethane on the release layer surface after immersion in toluene was θ2. The absolute value of θ1-θ2 was used as the change in contact angle before and after immersion in toluene. The change in contact angle was evaluated according to the following criteria. ◎: |θ1-θ2| < 1.0° ○:1.0°≦ |θ1−θ2| < 2.0° △:2.0°≦ |θ1−θ2| ≦ 3.0° ×: |θ1-θ2|> 3.0°
[0099] [Test Example 5] (Curl Evaluation) The release films obtained in the examples and comparative examples were cut to 200 x 200 mm, and then placed on a flat glass plate so that the substrate was on the glass plate side. Next, a 100 x 100 mm glass plate was placed in the center of the release layer of the release film, and the height from the upper surface of the lower glass plate to the apex of each corner of the release film was measured, and the curl was evaluated according to the following criteria. The results are shown in Table 1. ○…The total height of each corner is less than 50 mm △: The total height of each corner is 50mm or more and less than 100mm ×…The total height of each corner is 100mm or more
[0100] [Test Example 6] (Evaluation of blocking properties) The release films obtained in the Examples and Comparative Examples were wound up into a roll with a width of 400 mm and a length of 5000 m. The release film roll was stored for 30 days in an environment of 40°C and humidity of 50% or less, and the appearance of the release film roll in its original state was visually observed, and the blocking property was evaluated according to the following criteria. The results are shown in Table 1. ○…No change from when rolled up (no blocking) △: Color change due to adhesion between films was observed in less than half of the width direction (slight blocking) ×: A change in color due to adhesion between films was observed over the majority of the width direction (blocking occurred)
[0101] [Test Example 7] (Slurry Coating Property Evaluation (Pinhole Evaluation)) A composition consisting of the materials listed below was stirred and mixed, and dispersed for 30 minutes using a bead mill with zirconia beads having a diameter of 0.5 mm as a dispersoid, to obtain a ceramic slurry. Toluene 76.3 parts by mass Ethanol 76.3 parts by mass Barium titanate (HPBT-1, manufactured by Fuji Titanium Co., Ltd.) 35.0 parts by mass Polyvinyl butyral 3.5 parts by weight (Sekisui Chemical Co., Ltd. S-LEC (registered trademark) BM-S) DOP (dioctyl phthalate) 1.8 parts by mass Next, the slurry was applied to the release surface of the obtained release film sample using an applicator so that the dried thickness would be 0.8 μm, and after drying at 90° C. for 1 minute, the release film was peeled off to obtain a ceramic green sheet. The obtained ceramic green sheet was cut at a widthwise center region of 25 cm 2 The surface opposite to the ceramic slurry coating was irradiated with light within the range of 100 mm, and the occurrence of pinholes through which light was visible was observed and visually evaluated according to the following criteria. The measurement was carried out five times, and the average value was used. ◎: No pinholes ○: Almost no pinholes (guideline: 2 or less pinholes per measurement area) △: Pinholes have occurred (Guideline: 5 or fewer pinholes per measurement area) ×: Many pinholes were generated
[0102] [Test Example 8] (Evaluation of peelability) A composition consisting of the materials listed below was stirred and mixed, and dispersed for 60 minutes using a bead mill with zirconia beads having a diameter of 0.5 mm as a dispersoid, to obtain a ceramic slurry. Toluene 38.3 parts by mass Ethanol 38.3 parts by mass Barium titanate (HPBT-1, manufactured by Fuji Titanium Co., Ltd.) 64.8 parts by weight Polyvinyl butyral 6.5 parts by weight (Sekisui Chemical Co., Ltd. S-LEC (registered trademark) BM-S) DOP (dioctyl phthalate) 3.3 parts by mass Next, the release surface of the obtained release film sample was coated with an applicator so that the dried slurry would be 10 μm thick, and then dried at 90° C. for 2 minutes to form a ceramic green sheet on the release film. The obtained release film with the ceramic green sheet was de-electrified using a static eliminator (Keyence Corporation, SJ-F020), and then peeled off at a width of 30 mm, a peeling angle of 90 degrees, and a peeling speed of 10 m / min using a peeling tester (Kyowa Interface Science Co., Ltd., VPA-3). The ceramic green sheet surface was fixed, and the release film surface was peeled off in the direction of pulling. The stress applied during peeling was measured and taken as the peeling force. The releasability of the ceramic green sheet was evaluated according to the following criteria. ◎: Peeling force is 2.0mN / mm 2 It was possible to peel it off with the following very light force. ○: Peel strength is 2.0mN / mm 2 Greater than 3.0mN / mm 2 It was possible to peel it off with the following relatively light force. △: Peeling force is 3.0mN / mm 2 Greater than 4.0mN / mm 2 It was possible to peel it off with the following light force. ×: Peeling force is 4.0mN / mm 2 needed a greater force than
[0103] [Table 1]
[0104] [Table 2]
[0105] As is clear from Tables 1 and 2, the release films obtained in the examples had no defects due to the surface of the release layer or the back surface of the substrate, and also had excellent releasability of the ceramic green sheet.
[0106] As shown in Tables 1 and 2, the contact angle change |θ1-θ2| of diiodomethane before and after immersion in toluene differed depending on the combination of (meth)acrylic acid ester and silicone-based component. In Examples 1 to 12, the contact angle change |θ1-θ2| of diiodomethane before and after immersion in toluene was 3.0° or less, and the release layer was not eroded by the organic solvent during ceramic green sheet processing, and peeling was possible with low force. On the other hand, the elastic modulus of the release layer surface was low in Comparative Examples 2 to 4. Moreover, in Comparative Examples 1, 3, and 4, the contact angle change |θ1-θ2| of diiodomethane before and after immersion in toluene was greater than 3.0°, and the release layer was eroded by the organic solvent during ceramic green sheet processing, increasing the peeling force.
[0107] When internal electrodes were printed on the ceramic green sheets, no change was observed in the force required to peel off the ceramic green sheets with internal electrodes in Examples 1 to 12. On the other hand, in Comparative Examples 1 to 4, the ceramic green sheets with internal electrodes could not be satisfactorily peeled off or the force required to peel off increased. [Industrial Applicability]
[0108] The release film for producing a ceramic green sheet of the present invention is particularly suitable for forming a thin ceramic green sheet having a thickness of 1 μm or less. [Explanation of symbols]
[0109] 1: Release film 11: First layer 12: Second layer 13: Film base 14: Release layer 111: Surface of the first layer 112: Surface of the second layer 121: Surface of release layer
Claims
1. A release film having a release layer provided on at least one surface of a film substrate, The surface average roughness (Sa) of the release layer is 7 nm or less; The maximum protrusion height (Rp) of the surface of the release layer is 50 nm or less, the difference (θ1-θ2) between the diiodomethane contact angle θ1 on the surface of the release layer and the diiodomethane contact angle θ2 on the surface of the release layer after the release film is immersed in toluene is 3.0° or less as an absolute value, and the elastic modulus of the surface of the release layer measured by a nanoindentation test is 4.0 GPa or more; The release layer is a cured product of a release agent composition, The release agent composition contains a hexa- or higher functional urethane acrylate and a silicone-based component, the mass ratio of the silicone-based component in the release agent composition to the total mass of the hexa- or higher functional urethane acrylate and the silicone-based component is 0.2 to 5 mass %, The silicone-based component is a polyorganosiloxane having a reactive functional group, The reactive functional group is at least one selected from a (meth)acryloyl group, a vinyl group, a maleimide group, an epoxy group, a carboxyl group, an isocyanate group, and a hydroxyl group. Release film for manufacturing ceramic green sheets.
2. the release layer is a cured product of a release agent composition, the release agent composition contains a hexa- or higher functional urethane acrylate and a silicone-based component, the area surface average roughness (Sa) of the surface of the film substrate opposite to the release layer is 5 to 50 nm, and the maximum projection height (Rp) is 30 to 1000 nm, The thickness of the film substrate is 10 to 250 μm. The release film for producing a ceramic green sheet according to claim 1.
3. 2. The release film for producing a ceramic green sheet according to claim 1, wherein the reactive functional group in the polyorganosiloxane having a reactive functional group is a (meth)acryloyl group.
4. 2. The release film for producing a ceramic green sheet according to claim 1, wherein the total height of each corner is less than 50 mm in a curl evaluation calculated by the following measurement method: Curl Rating After cutting the release film to 200 x 200 mm, the release film is placed on a flat glass plate so that the substrate faces the glass plate. Next, a 100 x 100 mm glass plate is placed in the center of the release layer of the release film, and then the height from the upper surface of the lower glass plate to the apex of each corner of the release film is measured.
5. 2. The release film for producing a ceramic green sheet according to claim 1, wherein the release layer has a thickness of 0.2 to 2 μm.
6. 2. The release film for producing a ceramic green sheet according to claim 1, wherein the film substrate has a first layer that is substantially free of inorganic particles and a second layer that contains inorganic particles, a release layer is provided on the first layer, the second layer forms an opposite surface of the film substrate, the inorganic particles contained in the second layer are silica particles and / or calcium carbonate particles, and the total amount of the inorganic particles contained in the second layer is 5,000 to 15,000 ppm.
Citation Information
Patent Citations
Method of manufacturing laminated ceramic electronic component
JP2003203822A
Exfoliation film for manufacturing green sheet, and method for manufacturing exfoliation film for manufacturing green sheet
JP2014082500A
Release film for molding ceramic sheet
JP2015033811A
Release laminate film
JP2017177678A
High-energy radiation-curable acryloxy-functional silicone composition for release film for dielectric ceramic forming material and release film for dielectric ceramic forming material using the same
JP2017505250A