Superconducting device, manufacturing method for superconducting device, and laminate
The superconducting device employs a through electrode with a high melting point metal outer layer and low melting point metal inner layer, separated by high melting point partitions, to mitigate stress and volume fluctuations, ensuring structural integrity during temperature changes.
Patent Information
- Application Number
- JP2023508173
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-03-22
AI Technical Summary
Superconducting devices experience significant stress due to volume fluctuations and thermal expansion when exposed to temperature changes during the reflow process, particularly in high-density packaging where through electrodes and bonding electrodes are integrated, leading to potential damage such as cracks.
The superconducting device incorporates a through electrode with a high melting point metal outer portion and a low melting point metal inner portion, separated by a high melting point metal cap and base films, which act as partition walls to mitigate stress and volume fluctuations.
This configuration effectively suppresses stress and volume fluctuations in the superconducting device by isolating the through electrode and bonding electrode, maintaining structural integrity and reducing the risk of damage.
Smart Images

Figure 0007563578000001 
Figure 0007563578000002 
Figure 0007563578000003
Abstract
Description
[Technical field]
[0001] The disclosed technology relates to a superconducting device, a method for manufacturing a superconducting device, and a laminate. [Background technology]
[0002] The following techniques are known as techniques related to superconducting devices having structural portions that exhibit superconductivity. For example, a semiconductor device including a base substrate, a carrier substrate, and an embedded metallization layer interposed between the base substrate and the carrier substrate is known. A method for manufacturing the semiconductor device includes the following steps: forming an upper metallization layer of a first conductive metal material on an upper surface of the carrier substrate; then forming an unfilled through-substrate via in the carrier substrate to the embedded metallization layer; then forming an under-bump metallization layer of a second conductive metal material on a surface that defines the unfilled through-substrate via and a periphery surrounding the unfilled through-substrate via on the carrier substrate and on the first conductive metal material layer; the under-bump metallization layer is bonded to the embedded metallization layer and the upper metallization layer; the first conductive metal material and the second conductive metal material are different; then depositing and patterning a sacrificial layer to form an opening that exposes the unfilled through-substrate via and a periphery surrounding the unfilled through-substrate via on the carrier substrate and on the upper metallization layer. The opening is then filled with a third conductive metal material to form a filled through-substrate via, and the sacrificial layer is then removed to form a cylindrically shaped solder bump that is self-aligned with the filled through-substrate via. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2020-520090 Summary of the Invention [Problem to be solved by the invention]
[0004] The disclosed technique aims to suppress stress caused by temperature changes in superconducting devices. [Means for solving the problem]
[0005] The superconducting device according to the disclosed technology includes a substrate, a through hole provided in the substrate, and a through electrode provided in the through hole. The through electrode has a first portion and a second portion provided between the first portion and an inner wall surface of the through hole, and the second portion is formed of a material containing a first metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The superconducting device includes an electrode electrically connected to the through electrode, at least a portion of which is provided outside the through hole and formed of a material containing a second metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature, and a partition portion provided between the through electrode and the joining electrode and formed of a material containing the first metal. The melting point of the first metal is higher than the melting point of the second metal. Effect of the Invention
[0006] According to the disclosed technique, it is possible to suppress stress caused by temperature changes in a superconducting device. [Brief description of the drawings]
[0007] [Figure 1] 1 is a cross-sectional view showing an example of a configuration of a superconducting device according to an embodiment of the disclosed technique. [Diagram 2] FIG. 1 is a diagram illustrating an example of a configuration of a superconducting quantum bit device according to an embodiment of the disclosed technique. [Figure 3A] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3B] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3C] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3D]1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3E] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3F] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3G] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3H] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3I] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3J] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3K] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3L] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 3M] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4A] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4B] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4C] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4D] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4E] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4F] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4G] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4H] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4I] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4J] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Figure 4K] 1 is a cross-sectional view showing an example of a method for manufacturing a superconducting device according to an embodiment of the disclosed technique. [Diagram 5] 1 is a cross-sectional view showing an example of a configuration of a superconducting device according to an embodiment of the disclosed technique. [Figure 6] 1 is a cross-sectional view showing an example of a configuration of a superconducting device according to an embodiment of the disclosed technique. [Figure 7] 1 is a cross-sectional view showing an example of a configuration of a superconducting device according to an embodiment of the disclosed technique. [Figure 8] 1 is a cross-sectional view showing an example of a configuration of a laminate according to an embodiment of the disclosed technique. [Figure 9] 1 is a cross-sectional view showing an example of a configuration of a laminate according to an embodiment of the disclosed technique. [Figure 10] 1 is a cross-sectional view showing an example of a configuration of a laminate according to an embodiment of the disclosed technique. [Figure 11] 1 is a cross-sectional view showing an example of a configuration of a laminate according to an embodiment of the disclosed technique. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Quantum computers are said to have overwhelming processing power compared to conventional computers by using quantum mechanical phenomena such as superposition and quantum entanglement. As a device for realizing a quantum computer, for example, a superconducting device using a Josephson element containing a superconducting material has been proposed. A Josephson element is a switching element that utilizes the tunneling effect of electric current in a superconducting state. Superconducting devices are usually used in extremely low temperature environments such as a few mK because they exhibit superconductivity in such environments.
[0009] On the other hand, it is considered that high density packaging is possible by stacking superconducting devices together or stacking a superconducting device with another device. In a superconducting device, it is considered that a through electrode is used as a means for realizing three-dimensional packaging. Specifically, a superconducting device having a substrate, a through electrode penetrating the substrate, and a bonding electrode electrically connected to the through electrode is assumed. The superconducting device is stacked on another device via the bonding electrode by a reflow process. In this reflow process, the superconducting device is exposed to a temperature equal to or higher than the melting point of the bonding electrode. When the bonding electrode contains, for example, Sn, Pb, or an alloy thereof, its melting point is 200°C or higher, and the reflow temperature is set to about 300°C. That is, in a superconducting device, the temperature difference between the temperature during packaging and the temperature during use is 500°C or higher. Therefore, in a superconducting device used in an extremely low temperature environment, the volume fluctuation due to the expansion and contraction of the through electrode and the bonding electrode becomes large compared to a general device used in a normal temperature environment, and there is a high risk of damage such as cracks occurring in these electrodes. In particular, in a structure in which the through electrode and the bonding electrode are integrally formed as described in Patent Document 1, the volume of the structure in which the through electrode and the bonding electrode are integrated becomes large, and the volume fluctuation and the associated stress become more pronounced.
[0010] Hereinafter, an example of an embodiment of the disclosure will be described with reference to the drawings. In each drawing, the same or equivalent components and parts are given the same reference numerals, and duplicated descriptions will be omitted as appropriate.
[0011] [First embodiment] 1 is a cross-sectional view showing an example of the configuration of a superconducting device 10 according to a first embodiment of the disclosed technique. The superconducting device 10 includes a substrate 20, a superconducting quantum bit element 30, a through electrode 40, and a bonding electrode 50.
[0012] The substrate 20 is made of an insulator or a semiconductor. By using a semiconductor such as silicon as the substrate 20, it becomes easy to apply existing semiconductor processing techniques.
[0013] The superconducting quantum bit element 30 is provided on the surface S1 side of the substrate 20. The superconducting quantum bit element 30 is an element that forms a coherent two-level system using superconductivity. In this embodiment, the superconducting quantum bit element 30 is configured to include a Josephson element shown in FIG. 2. The Josephson element is configured to include a pair of superconductors 31 that exhibit superconductivity at a temperature equal to or lower than a predetermined critical temperature, and an extremely thin insulator 32 having a thickness of about several nm sandwiched between the pair of superconductors 31. The superconductor 31 may be, for example, aluminum, and the insulator 32 may be, for example, aluminum oxide. The superconducting quantum bit element 30 is connected to a wiring 60 through a via 61. The via 61 and the wiring 60 are each made of a high-melting point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The high-melting point metal will be described in detail later. Surface S1 of substrate 20 is covered with insulator layer 90 made of an insulator such as SiO 2 , and superconducting quantum bit element 30, via 61, and wiring 60 are embedded in insulator layer 90.
[0014] The through electrode 40 penetrates the substrate 20. One end of the through electrode 40 is connected to a wiring 60 provided on the surface S1 side of the substrate 20, and the other end is connected to a bonding electrode 50 via a cap film 70 provided on the surface S2 side of the substrate 20 opposite to the surface S1. In other words, the through electrode 40 functions as a transmission path that transmits a quantum bit output from the superconducting quantum bit element 30 provided on the surface S1 side of the substrate 20 to the bonding electrode 50 provided on the surface S2 side of the substrate 20.
[0015] The through electrode 40 includes an outer portion 41 and an inner portion 42. The outer portion 41 is made of a high-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature, and surrounds the inner portion 42. The inner portion 42 is made of a low-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. That is, the inside of the through electrode 40 is filled with a low-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The low-melting-point metal will be described in detail later. The end of the through electrode 40 on the surface S2 side of the substrate 20 is blocked by a cap film 70. The cap film 70 is made of a high-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The cap film 70 functions as a partition wall that separates the through electrode 40 and the joining electrode 50. The low-melting-point metal that constitutes the inner portion 42 of the through electrode 40 is completely surrounded (sealed) by the high-melting-point metal that constitutes the through electrode 40 and the high-melting-point metal that constitutes the cap film 70. Between the substrate 20 and the through electrode 40, an insulating film 93 made of an insulator such as SiO2 is provided. That is, the substrate 20 and the through electrode 40 are electrically isolated from each other. The surface S2 of the substrate 20 is covered with an insulator layer 92. The cap film 70 is embedded in the insulator layer 92, and the end of the through electrode 40 on the S2 side of the substrate 20 reaches inside the insulator layer 92.
[0016] The bonding electrode 50 has a so-called bump shape and functions as an external connection terminal for bonding the superconducting device 10 to another device. The bonding electrode 50 is provided on the surface S2 side of the substrate 20, and is connected to the through electrode 40 via the cap film 70 and the undercoat film 80. In this embodiment, the bonding electrode 50 is provided directly below the through electrode 40. The bonding electrode 50 is made of a low-melting point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The bonding electrode 50 has a portion embedded in the insulator layer 92 and a portion exposed from the surface of the insulator layer 92. The undercoat film 80 is interposed between the bonding electrode 50 and the insulator layer 92. The undercoat film 80 functions as a so-called under-bump metal, and has a function of suppressing the diffusion of the low-melting point metal constituting the bonding electrode 50 into the insulator layer 92 and a function of increasing the adhesion between the bonding electrode 50 and the insulator layer 92. Moreover, the base film 80 functions as a partition wall that separates the through electrode 40 and the joining electrode 50. The base film 80 is made of a high-melting point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature.
[0017] Dummy wiring 62 that is not electrically connected to the superconducting quantum bit element 30 is provided in the insulating layer 92. The potential of the dummy wiring 62 may be, for example, a ground potential or may be floating. The dummy wiring 62 is provided as necessary to balance the wiring density on the surface S1 side of the substrate 20 and the wiring density on the surface S2 side of the substrate 20. If the wiring density on the surface S1 side of the substrate 20 and the wiring density on the surface S2 side of the substrate 20 are not uniform, warping of the substrate 20 becomes significant. By appropriately providing the dummy wiring 62 on the surface S2 side of the substrate 20 and balancing the wiring densities on both sides of the substrate 20, it is possible to suppress warping of the substrate 20. Note that wiring electrically connected to the superconducting quantum bit element 30 or wiring having a specific electrical function may be provided on the surface S2 side of the substrate 20. Also, dummy wiring and wiring having a specific electrical function may be provided so as to be mixed on the surface S2 side of the substrate 20.
[0018] As described above, the via 61, the wiring 60, the outer portion 41 of the through electrode 40, the cap film 70, and the undercoat film 80 are each made of a high-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The high-melting-point metals that respectively constitute the via 61, the wiring 60, the outer portion 41 of the through electrode 40, the cap film 70, and the undercoat film 80 are preferably the same metal. Also, as described above, the inner portion 42 of the through electrode 40 and the joining electrode 50 are each made of a low-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. The low-melting-point metals that respectively constitute the inner portion 42 of the through electrode 40 and the joining electrode 50 are preferably the same metal.
[0019] In this specification, a high melting point metal is a metal with a melting point of 800°C or more, and a low melting point metal is a metal with a melting point of 300°C or less. Examples of high melting point metals that exhibit superconductivity at a temperature below a predetermined temperature include Ta, Nb, V, Mo, or alloys containing these as main components, or nitrides of these. Examples of low melting point metals that exhibit superconductivity at a temperature below a predetermined temperature include Sn, Pb, In, Ga, or alloys containing these as main components. The high melting point metal is an example of the first metal in the disclosed technology. The low melting point metal is an example of the low melting point metal in the disclosed technology.
[0020] The high-melting point metal and the low-melting point metal that exhibit superconductivity at a temperature equal to or lower than a predetermined temperature preferably have a small difference in thermal expansion coefficient from the substrate 20. For example, when the substrate 20 is a Si substrate, it is preferable to use Mo or Ta as the high-melting point metal, and Ga or Sn as the low-melting point metal.
[0021] Furthermore, by using Ga (melting point: 29.8°C) or In (melting point: 156.6°C), which has a relatively low melting point, as a low-melting-point metal that exhibits superconductivity at temperatures below a predetermined temperature, the difference between the temperature when the superconducting device 10 is mounted and the temperature when it is in use can be reduced, and volumetric changes due to temperature fluctuations and the associated stress can be suppressed.
[0022] In addition, metals used as high-melting-point metals and low-melting-point metals that exhibit superconductivity at a temperature equal to or lower than a predetermined temperature may be selected from the viewpoint of ease of processing. For example, both Ta, which is a high-melting-point metal, and Sn, which is a low-melting-point metal, can be patterned by chlorine-based reactive dry etching.
[0023] The following describes a method for manufacturing the superconducting device 10. Figures 3A to 3M are cross-sectional views showing an example of a method for manufacturing the superconducting device 10.
[0024] First, the superconducting quantum bit element 30 is formed on the surface S1 of the substrate 20 made of a semiconductor such as Si. Next, an insulator film made of an insulator such as SiO2 that constitutes the insulator layer 90 is formed on the surface S1 of the substrate 20 by, for example, a chemical vapor deposition (CVD) method. The superconducting quantum bit element 30 is embedded in the insulator layer 90 (FIG. 3A).
[0025] Next, after forming vias 61 connected to superconducting quantum bit elements 30, a high-melting-point metal (e.g., Ta) that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature is deposited on the surface of insulator layer 90 by, for example, sputtering. This high-melting-point metal is then patterned to form wiring 60. Wiring 60 is covered with an insulating film made of an insulator such as SiO2 that constitutes insulator layer 90 (FIG. 3B). Vias 61 are made of the same high-melting-point metal (e.g., Ta) as wiring 60.
[0026] Next, the surface S2 side of the substrate 20 is ground to thin the substrate 20. Chemical Mechanical Polishing (CMP) and chemical treatment are performed as a finishing step of the thinning process of the substrate 20. Next, an insulator layer 92 made of an insulator such as SiO2 is formed on the surface S2 of the substrate 20 by, for example, a CVD method (FIG. 3C).
[0027] Next, by reactive ion etching using, for example, the Bosch process, through-holes 45 are formed from the surface of the insulator layer 92 through the substrate 20 to reach the wiring 60. The Bosch process is a dry etching technique that realizes vertical deep digging of the substrate 20 at high speed and with a high aspect ratio by repeating three steps: isotropic etching of the substrate 20, deposition of a protective film (not shown), and anisotropic etching of the substrate 20 (removal of the protective film on the bottom surface). Etching stops when the through-holes 45 reach the wiring 60 (FIG. 3D).
[0028] Next, an insulating film 93 made of an insulator such as SiO2 is formed on the side of the through hole 45 by, for example, a CVD method. Next, a high-melting point metal M1 (for example, Ta) that is the same as the wiring 60 is deposited on the surface S2 side of the substrate 20 by, for example, a sputtering method. The surface of the insulator layer 92 and the side and bottom of the through hole 45 are covered with the high-melting point metal M1. The part of the high-melting point metal M1 covering the side and bottom of the through hole 45 becomes the outer part 41 of the through electrode 40, and the part of the high-melting point metal M1 covering the surface of the insulator layer 92 becomes a part of the dummy wiring 62. The outer part 41 of the through electrode 40 is connected to the wiring 60 at the bottom of the through hole 45 (FIG. 3E).
[0029] Next, a seed layer (not shown) is formed on the surface of the high melting point metal M1 by, for example, a sputtering method, and then a low melting point metal M2 (for example, Sn) that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature is deposited on the high melting point metal M1 by a plating method. The low melting point metal M2 fills the through hole 45, thereby forming the inner portion 42 of the through electrode 40 (FIG. 3F).
[0030] Next, the excess low-melting-point metal M2 deposited on the insulator layer 92 is removed by, for example, CMP. Thereafter, the same high-melting-point metal M1 (for example, Ta) as that used for the wiring 60 and the outer portion 41 of the through electrode 40 is further deposited on the surface S2 side of the substrate 20 by, for example, a sputtering method (FIG. 3G).
[0031] Next, the high melting point metal M1 is patterned, thereby forming dummy wirings 62 on the surface S2 side of the substrate 20 and forming a cap film 70 that closes the end of the through electrode 40 on the surface S2 side of the substrate 20 (FIG. 3H).
[0032] The dummy wiring 62 is covered with an insulating film made of an insulator such as SiO2 that constitutes the insulator layer 92 (FIG. 3I). Next, a contact hole 95 is formed from the surface of the insulator layer 92 to the cap film 70 by, for example, reactive ion etching (FIG. 3J).
[0033] Next, the same high-melting point metal (e.g., Ta) as that of the wiring 60, the outer portion 41 of the through electrode 40, the cap film 70, and the dummy wiring 62 is deposited on the surface S2 side of the substrate 20 by, for example, a sputtering method, and the high-melting point metal is patterned to form the base film 80. The base film 80 is connected to the cap film 70 at the bottom surface of the contact hole 95 (FIG. 3K).
[0034] Next, a solder resist 55 is formed on the surface of the insulator layer 92. The solder resist 55 has an opening that exposes the base film 80. Next, the same low-melting point metal (e.g., Sn) as that of the inner portion 42 of the through electrode 40 is deposited on the base film 80 by plating. This forms the bonding electrode 50 (FIG. 3L). Finally, the solder resist 55 is removed (FIG. 3M).
[0035] In the above description, a manufacturing method in which through holes 45 for forming through electrodes 40 are formed from the surface S2 side of substrate 20 has been exemplified, but it is also possible to form through holes 45 from the surface S1 side of substrate 20. Hereinafter, a manufacturing method in which through holes 45 are formed from the surface S1 side of substrate 20 will be described with reference to FIGS. 4A to 4K.
[0036] For example, by reactive ion etching using the Bosch process, through-hole 45 is formed from surface S1 of substrate 20 on which superconducting quantum bit element 30 and insulator layer 90 are formed. Etching is stopped before reaching surface S2 of through-hole 45 (FIG. 4A).
[0037] Next, an insulating film 93 made of an insulator such as SiO2 is formed on the side and bottom of the through hole 45 by, for example, a CVD method. Next, a high-melting point metal M1 (e.g., Ta) that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature is deposited on the surface S1 side of the substrate 20 by, for example, a sputtering method. The surface of the insulator layer 90 and the side and bottom of the through hole 45 are covered with the high-melting point metal M1. The portion of the high-melting point metal M1 covering the side and bottom of the through hole 45 becomes the outer portion 41 of the through electrode 40 (FIG. 4B).
[0038] Next, a seed layer (not shown) is formed on the surface of the high melting point metal M1 by, for example, a sputtering method, and then a low melting point metal M2 (for example, Sn) that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature is deposited on the high melting point metal M1 by a plating method. The low melting point metal M2 fills the through hole 45, thereby forming the inner portion 42 of the through electrode 40 (FIG. 4C).
[0039] Next, the excess low-melting-point metal M2 deposited on the insulator layer 90 is removed by, for example, CMP. Thereafter, the same high-melting-point metal M1 (for example, Ta) as that of the outer portion 41 of the through electrode 40 is further deposited on the surface S1 side of the substrate 20 by, for example, a sputtering method (FIG. 4D).
[0040] Next, the high melting point metal M1 is patterned, thereby forming a cap film 70 that closes the end of the through electrode 40 on the surface S1 side of the substrate 20 (FIG. 4E).
[0041] Next, after forming vias 61 connected to the superconducting quantum bit elements 30, the same high-melting point metal (e.g., Ta) as the outer portion 41 of the through electrode 40 and the cap film 70 is deposited on the surface S1 side of the substrate 20 by, for example, a sputtering method, and then the high-melting point metal is patterned. This forms wiring 60 electrically connected to the superconducting quantum bit elements 30 and the through electrode 40 (FIG. 4F).
[0042] The wiring 60 is covered with an insulating film made of an insulator such as SiO2 that constitutes the insulator layer 90. Next, the surface S2 side of the substrate 20 is ground to thin the substrate 20 until the through electrodes 40 are exposed. As a finishing touch to the thinning process of the substrate 20, CMP and chemical treatment are performed. Next, an insulator layer 92 made of an insulator such as SiO2 is formed on the surface S2 of the substrate 20 by, for example, a CVD method (FIG. 4G).
[0043] Next, a contact hole 95 is formed from the surface of the insulator layer 92 to reach the through electrode 40, for example, by reactive ion etching (FIG. 4H). Next, the same high-melting point metal (for example, Ta) as the wiring 60, the outer portion 41 of the through electrode 40, and the cap film 70 is deposited on the surface S2 side of the substrate 20, for example, by sputtering, and this high-melting point metal is patterned to form an undercoat film 80. The undercoat film 80 is connected to the through electrode 40 at the bottom of the contact hole 95 (FIG. 4I).
[0044] Next, a solder resist 55 is formed on the surface of the insulator layer 92. The solder resist 55 has an opening that exposes the base film 80. Next, the same low-melting point metal (e.g., Sn) as that of the inner portion 42 of the through electrode 40 is deposited on the base film 80 by plating. This forms the bonding electrode 50 (FIG. 4J). Finally, the solder resist 55 is removed (FIG. 4K).
[0045] As described above, the superconducting device 10 according to this embodiment has the through electrode 40 penetrating the substrate 20, so that the superconducting device 10 can be three-dimensionally mounted by stacking the superconducting device 10 and other devices. The superconducting device 10 is bonded to other devices via the bonding electrode 50. In bonding the superconducting device 10 to other devices, a reflow process is performed to melt the bonding electrode 50. The heating in the reflow process can cause the volumes of the bonding electrode 50 and the through electrode 40 to vary. In the superconducting device 10 according to this embodiment, the bonding electrode 50 is disposed directly below the through electrode 40, and the volume of the structure in which the bonding electrode 50 and the through electrode 40 are integrated tends to become large, and stress due to the volume variation becomes a problem. However, in the superconducting device 10 according to this embodiment, the cap film 70 and the base film 80 made of a high melting point metal function as a partition wall that separates the through electrode 40 and the bonding electrode 50. Generally, high melting point metals have a smaller thermal expansion coefficient than low melting point metals, so by separating the through electrode 40 and the bonding electrode 50 with a partition portion made of a high melting point metal, it is possible to separate the volumetric fluctuation in the through electrode 40 from the volumetric fluctuation in the bonding electrode 50. This makes it possible to suppress stress accompanying the volumetric fluctuation of the through electrode 40 and the bonding electrode 50.
[0046] In addition, the low melting point metal constituting the inner portion 42 of the through electrode 40 is completely surrounded (sealed) by the high melting point metal constituting the outer portion of the through electrode 40 and the high melting point metal constituting the cap film 70. Since the volume change accompanying the temperature change of the inner portion 42 of the through electrode 40 is limited by the high melting point metal surrounding the inner portion 42 of the through electrode 40, it is possible to suppress the volume change accompanying the temperature change of the through electrode 40. In addition, although the low melting point metal constituting the inner portion 42 of the through electrode 40 may melt in the reflow process, the high melting point metal constituting the outer portion 41 of the through electrode 40 does not melt, so that the diffusion of the molten low melting point metal constituting the inner portion 42 into the substrate 20 can be suppressed.
[0047] In the superconducting device 10 according to this embodiment, the wiring 60, the outer portion 41 of the through electrode 40, the cap film 70, and the undercoat film 80 are all made of the same high-melting-point metal. This prevents alloy formation when different metals are used. If an alloy is formed, the decoherence effect increases, and it may become difficult to maintain the quantum mechanical superposition state.
[0048] In the above description, the inner portion 42 of the through electrode 40 is made of a low-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature, but is not limited thereto. For example, the inner portion 42 of the through electrode 40 may be made of the same material as the substrate 20 or an oxide of the material that constitutes the substrate 20. That is, the inside of the through electrode 40 may be filled with the same material as the substrate 20 or an oxide of the material that constitutes the substrate 20. For example, when the substrate 20 is a Si substrate, the inner portion 42 of the through electrode 40 may be made of polysilicon or SiO2. The oxide of the same material as the substrate 20 or the material that constitutes the substrate 20 that constitutes the inner portion 42 of the through electrode 40 is surrounded by a high-melting-point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. By constructing the inner portion 42 of the through electrode 40 from the same material as the substrate 20 or an oxide of the material that constitutes the substrate 20, the volumetric changes associated with temperature changes in the through electrode 40 and the substrate 20 occur at approximately the same rate (i.e., the thermal expansion coefficients of the through electrode 40 and the substrate 20 are approximately the same), thereby suppressing stress associated with temperature changes.
[0049] The inner portion 42 of the through electrode 40 may be made of an insulator. The inner portion 42 of the through electrode 40 may be made of the same high-melting point metal as the outer portion 41 of the through electrode 40. This makes it possible to suppress volume fluctuations of the through electrode 40 caused by temperature changes, compared to when the inner portion 42 of the through electrode 40 is made of a low-melting point metal. Generally, high-melting point metals are difficult to form a film by plating, so sputtering or CVD is used as a film formation method for charging the inside of the through electrode 40.
[0050] 5, the inner portion 42 of the through electrode 40 may be hollow. This makes it possible to suppress the volume change of the through electrode 40 caused by the temperature change, compared to the case where the inner portion 42 of the through electrode 40 is made of a low melting point metal. When the inner portion 42 of the through electrode 40 is hollow, it is preferable that the joining electrode 50 is provided at a position shifted from the through electrode 40 in the main surface direction of the substrate 20 from the viewpoint of ensuring mechanical strength. Note that the through electrode 40 exhibits superconductivity, so that electrical resistance does not become a problem. Therefore, it is possible to form the through electrode 40 only from the thin film of high melting point metal that forms the outer portion 41.
[0051] [Second embodiment] 6 is a cross-sectional view showing an example of the configuration of a superconducting device 10A according to a second embodiment of the disclosed technique. The superconducting device 10A according to this embodiment has the form of an interposer that mediates signal transmission between devices, and differs from the superconducting device 10 according to the first embodiment in that it does not include a superconducting quantum bit element. The superconducting device 10A includes a substrate 20, a through electrode 40, and a joining electrode 50.
[0052] The substrate 20 is made of an insulator or a semiconductor. By using a semiconductor such as silicon as the substrate 20, it becomes easy to apply existing semiconductor processing techniques.
[0053] One end of the through electrode 40 is connected to the bonding electrode 50 via a cap film 70 provided on the surface S1 side of the substrate 20, and the other end is connected to the bonding electrode 50 via a cap film 70 provided on the surface S2 side of the substrate 20.
[0054] The outer portion 41 of the through electrode 40 is made of a high-melting point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature, and surrounds the inner portion 42. The inner portion 42 of the through electrode 40 is made of a low-melting point metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature. Both ends of the through electrode 40 are blocked by a cap film 70. The cap film 70 is made of the same high-melting point metal as the outer portion 41 of the through electrode 40. The cap film 70 functions as a partition wall that separates the through electrode 40 and the joining electrode 50. The low-melting point metal that constitutes the inner portion 42 of the through electrode 40 is completely surrounded (sealed) by the high-melting point metal that constitutes the outer portion 41 of the through electrode 40 and the high-melting point metal that constitutes the cap film 70.
[0055] The bonding electrode 50 is provided on both the surface S1 side and the surface S2 side of the substrate 20. The bonding electrode 50 is made of the same low melting point metal as the inner portion 42 of the through electrode 40. The base film 80 is interposed between the bonding electrode 50 and the insulator layers 90, 92. The base film 80 functions as a so-called under-bump metal, and has a function of suppressing the diffusion of the low melting point metal constituting the bonding electrode 50 into the insulator layers 90, 92 and a function of increasing the adhesion between the bonding electrode 50 and the insulator layers 90, 92. The base film 80 also functions as a partition wall that separates the through electrode 40 and the bonding electrode 50. The base film 80 is made of the same high melting point metal as the outer portion 41 of the through electrode 40 and the cap film 70.
[0056] The bonding electrode 50 on the surface S1 side of the substrate 20 is bonded to a first device (not shown), and the bonding electrode 50 on the surface S2 side of the substrate 20 is bonded to a second device (not shown). Signal transmission is possible between the first device and the second device via the through electrode 40. Note that a method for manufacturing the superconducting device 10A according to this embodiment can be implemented using various processes for manufacturing the superconducting device 10 according to the first embodiment, and therefore a description thereof will be omitted.
[0057] According to the superconducting device 10A of this embodiment, similar to the superconducting device 10 of the first embodiment, the through electrode 40 and the joining electrode 50 are separated by a partition portion, so that it is possible to suppress stress associated with temperature changes.
[0058] The inner portion 42 of the through electrode 40 may be made of the same material as the substrate 20 or an oxide of the material constituting the substrate 20. The inner portion 42 of the through electrode 40 may be made of an insulator. The inner portion 42 of the through electrode 40 may be made of the same high melting point metal as the outer portion 41 of the through electrode 40. As shown in FIG. 7, the inner portion 42 of the through electrode 40 may be hollow. When the inner portion 42 of the through electrode 40 is hollow, it is preferable that the bonding electrode 50 is provided at a position shifted from the through electrode 40 in the main surface direction of the substrate 20 from the viewpoint of ensuring mechanical strength.
[0059] [Third embodiment] 8 is a cross-sectional view showing an example of the configuration of a laminate 100 according to the third embodiment of the disclosed technique. The laminate 100 is configured by stacking the superconducting device 10 according to the first embodiment described above and another device 11. The other device 11 may be, for example, a readout device having a function of reading out a quantum bit output from the superconducting device 10. A bonding electrode 50 of the superconducting device 10 is bonded to a pad 25 provided on a surface of a substrate 21 of the other device 11.
[0060] When the superconducting device 10 is joined to the other device 11, a reflow process is performed to melt the joining electrode 50. In the superconducting device 10, the cap film 70 and the base film 80 made of a high melting point metal function as a partition wall separating the through electrode 40 and the joining electrode 50, so that the volumetric fluctuation in the through electrode 40 and the volumetric fluctuation in the joining electrode 50 can be separated. This makes it possible to suppress stress accompanying the volumetric fluctuation of the through electrode 40 and the joining electrode 50.
[0061] 9, in the superconducting device 10, bonding electrodes 50 may be provided on both the surface S1 side and the surface S2 side of the substrate 20, and other devices 11, 12 may be stacked on both the surface S1 side and the surface S2 side of the substrate 20. The bonding electrode 50 on the surface S2 side of the superconducting device 10 is bonded to a pad 25 provided on the surface of the substrate 21 of the other device 11, and the bonding electrode 50 on the surface S1 side of the superconducting device 10 is bonded to a pad 26 provided on the surface of the substrate 22 of the other device 12.
[0062] As shown in FIG. 10, the superconducting device 10 and the other device 11 may be bonded to each other by room-temperature bonding or bonding with an adhesive, instead of bonding via a bonding electrode 50. In the laminate 100 shown in FIG. 10, an insulator layer 92 provided on the surface S2 of the substrate 20 of the superconducting device 10 and an insulator layer 98 provided on the surface S3 of the substrate 21 of the other device 11 are bonded to each other by room-temperature bonding or bonding with an adhesive, and then a through electrode 40 is formed. The through electrode 40 is connected to a pad 25 provided on the surface of the substrate 21 of the other device 11. The superconducting device 10 has a bonding electrode 50 provided on the surface S1 of the substrate 20. Another device (not shown) can be bonded to the superconducting device 10 via the bonding electrode 50.
[0063] 11 is a cross-sectional view showing an example of the configuration of a laminate including the superconducting device 10A according to the second embodiment and the other devices 11 and 12. The superconducting device 10A is an interposer that mediates signal transmission between the other devices 11 and 12. For example, the other device 12 may have a function of outputting a quantum bit, and the other device 11 may have a function of reading out the quantum bit. A bonding electrode 50 on the surface S2 side of the superconducting device 10A is bonded to a pad 25 provided on the surface of the substrate 21 of the other device 11, and a bonding electrode 50 on the surface S1 side of the superconducting device 10 is bonded to a pad 26 provided on the surface of the substrate 22 of the other device 12. [Explanation of symbols]
[0064] 10, 10A superconducting device 11, 12 Other devices 20, 21, 22 Substrate 30 Superconducting quantum bit device 40 Through electrode 41 Outer part 42 Inner part 45 Through hole 50 Junction electrode 60 Wiring 61 Via 62 Dummy wiring 70 Cap membrane 80 Base film 90, 92 Insulator layer 100 Laminate
Claims
1. A substrate; A through hole provided in the substrate; a through-hole electrode provided within the through-hole, the through-hole electrode having a first portion and a second portion provided between the first portion and an inner wall surface of the through-hole, the second portion being made of a material containing a first metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature; a joining electrode electrically connected to the through electrode, at least a portion of which is provided outside the through hole and made of a material containing a second metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature; a partition portion provided between the through electrode and the bonding electrode and made of a material containing the first metal; Including, The melting point of the first metal is higher than the melting point of the second metal. Superconducting devices.
2. a superconducting quantum bit element provided on the substrate; a wiring electrically connected to the superconducting quantum bit element and the through electrode, the wiring being made of a material containing the first metal; The superconducting device of claim 1 further comprising:
3. The substrate further includes a dummy wiring provided on a surface opposite to the surface on which the wiring is provided, the dummy wiring being not connected to the superconducting quantum bit element. The superconducting device according to claim 2 .
4. The bonding electrode has a portion provided within an insulator layer, The bonding electrode further includes a base film formed between the bonding electrode and the insulating layer and made of a material containing the first metal. The superconducting device according to any one of claims 1 to 3.
5. The second portion and the partition wall surround the first portion. The superconducting device according to any one of claims 1 to 4.
6. forming a through hole penetrating the substrate in the substrate; forming a through-hole in the through-hole, the through-hole having a first portion disposed in the through-hole and a second portion provided between the first portion and an inner wall surface of the through-hole, the second portion being made of a material containing a first metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature; forming a partition wall portion made of the first metal on a bottom surface of the through electrode; forming a joining electrode that is in contact with the partition portion, electrically connected to the through electrode, and made of a material containing a second metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature; Including, The melting point of the first metal is higher than the melting point of the second metal. A method for manufacturing a superconducting device.
7. The method further includes forming wiring that is made of a material containing the first metal and electrically connects the superconducting quantum bit element provided on the substrate and the through electrode. The method according to claim 6.
8. A laminate in which a superconducting device and another device are laminated, The superconducting device comprises: A substrate; A through hole provided in the substrate; a through-hole electrode having a first portion and a second portion provided between the first portion and an inner wall surface of the through-hole, the through-hole electrode being made of a material containing a first metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature; a joining electrode that is electrically connected to the through electrode, at least a portion of which is provided outside the through hole and is made of a material containing a second metal that exhibits superconductivity at a temperature equal to or lower than a predetermined temperature; a partition portion provided between the through electrode and the bonding electrode and made of a material containing the first metal; Including, The melting point of the first metal is higher than the melting point of the second metal. Laminate.
Citation Information
Patent Citations
Superconductive compound wire and production of the same
JP1978097798A
Ceramic superconductive multilayer wiring board and manufacture of the same
JP1990069994A
Cuperconducting integrated circuit structure and its manufacture
JP1999177157A
Superconducting Bump Bond
JP2019504511A
Method and semiconductor structure for fabricating a semiconductor device including through-substrate vias with self-aligned solder bumps
JP2020520090A