Metallic material connector and metallic material connecting method
The use of a thermoplastic resin film for connecting metal materials addresses contamination and repair issues, providing a strong, efficient, and environmentally friendly bonding solution.
Patent Information
- Application Number
- JP2023541817
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-26
- Filing Date
- 2023-07-05
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-07-05
AI Technical Summary
Existing methods for connecting metal materials, such as those using adhesive tapes, welding, liquid adhesives, and caulking, face issues like contamination of production lines, difficulty in repair, long process times, thickness changes at connection points, and environmental hazards, making them unsuitable for certain applications.
A connection method using a film composed mainly of thermoplastic resin, which is melted and solidified at overlapping portions to join metal materials, providing a strong, repairable, and contamination-free bond without chemical reactions.
The method offers a quick connection process with minimal thickness change, excellent repairability, and resistance to contamination, ensuring high bonding strength and compatibility with various metal materials.
Smart Images

Figure 0007563612000002 
Figure 0007563612000003 
Figure 0007563612000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a connected body of metal materials formed by overlapping and connecting an end A of a metal material A with an end B of a metal material B, and a method for connecting metal materials suitable for applications in which an end A of a metal material A and an end B of a metal material B are overlapped and connected. [Background technology]
[0002] A method has been disclosed in which the starting end of a first roll material and the end of a second roll material are overlapped and bonded via a double-sided adhesive tape to connect them (Patent Document 1).
[0003] When connecting using double-sided adhesive tape or single-sided adhesive tape (hereinafter collectively referred to as adhesive tape), there is a problem of contamination of the production line due to the adhesive components such as matrix resin and tackifier, which are the resin compositions that make up the adhesive layer of the adhesive tape, adhering to the transport path and molds in the production line. In particular, if the adhesive tape accidentally peels off, the adhesive layer of the peeled adhesive tape becomes exposed, and the adhesive components adhere to the transport path and molds in the production line, causing contamination of the production line, which can be a major problem. When the metal material is immersed in a chemical bath, the adhesive components such as the tackifier dissolve in the chemical bath, which can cause the chemical bath to become contaminated. In addition, the heat resistance and chemical resistance of the metal material are poor.
[0004] Other possible connection means include connection by welding, connection by liquid adhesive, connection by film-like thermosetting adhesive (hereinafter referred to as thermosetting adhesive film), connection by crimping, etc., but each of these has the following problems.
[0005] In the case of connections by welding, once the welding is done, it is impossible to dismantle it without destroying it. Therefore, there is a problem that it is not easy to reconnect (hereinafter referred to as repair) in case of a mistake such as misalignment of the connection part. In addition, welding generates sparks and scatters metal powder, which can cause problems in the working environment.
[0006] The connection using a liquid adhesive requires a coating process in which a liquid thermosetting resin composition is applied, and a curing process in which the resin composition is polymerized and cured after application. The coating process takes time to apply the resin composition, and the curing process takes time for the polymerization reaction. Thus, the connection using a liquid adhesive has a problem of lack of convenience because the process time for connection is long. In addition, since it is an amorphous liquid, it is difficult to reproducibly control the thickness, amount, and range of application for connection. In addition, in the case of a liquid thermosetting adhesive, repair is impossible or difficult, as in the case of welding.
[0007] When connecting using a thermosetting adhesive film, the coating step is unnecessary and the process time can be shortened, but repairs cannot be made after connecting. When the thermosetting adhesive film is a B-stage film, the polymerization reaction easily proceeds at room temperature, resulting in poor storage stability and making it impossible to store the film for long periods at room temperature. For this reason, when the thermosetting adhesive film is a B-stage film, it must be stored at low temperatures, requiring a low-temperature storage cabinet, and it is difficult to store large quantities for long periods, resulting in a lack of convenience.
[0008] When connecting by crimping, metal materials are stacked together to perform the crimping, and protrusions are created by the crimping. This increases the thickness at the crimped part, which is the connection part, making it difficult to apply to low-profile manufacturing lines. In addition, crimping requires a flat metal space larger than the crimp diameter, which makes it difficult to obtain sufficient connection strength with metal materials of complex shapes or narrow pitches. In addition, when passing through multiple chemical tanks, there is a problem that more chemicals are carried over to the next tank, which causes contamination of the chemicals and shortens the life of the chemicals. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2016-175768 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of the above technical background, and aims to provide a connecting technology that does not involve concerns about contamination of the production line by adhesive components, allows repair, has a short process time, and causes little change in thickness at the connecting parts. [Means for solving the problem]
[0011] In order to achieve the above object, the present invention provides the following means.
[0012] <Metal material connector> [1] A connected body of metal materials having an overlapping portion where end A of metal material A and end B of metal material B are overlapped via a film whose main component is a thermoplastic resin, the film being a film that has been melted and solidified at the overlapping portion. [2] The metal material connection according to [1], wherein the metal material A and the metal material B are at least one selected from the group consisting of a metal plate having a thickness of 1 mm or less and a metal foil having a thickness of 1 mm or less. [3] The metal material connection body of [1] or [2], in which the metal material A and the metal material B are in a strip shape and the metal material A and the metal material B are connected so as to be continuous in the longitudinal direction. [4] The metal material linkage of [3], wherein the metal material A and the metal material B are rolled materials each formed by winding at least one selected from the group consisting of a metal plate and a metal foil into a roll shape. [5] The metal material connection body according to any one of [1] to [4], in which the film is interposed over the entire overlapping surfaces of the end portion A and the end portion B. [6] The metal material linked body according to any one of [1] to [5], wherein the thermoplastic resin is an amorphous thermoplastic resin. [7] The metal connector according to [6], wherein the amorphous thermoplastic resin is at least one selected from the group consisting of thermoplastic epoxy resins and phenoxy resins. [8] The metal connector according to [7], wherein the amorphous thermoplastic resin is an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more, or an amorphous thermoplastic resin not containing an epoxy group. [9] The metal material connected body according to any one of [1] to [8], wherein the film has an adhesive, and the adhesive serves to temporarily fasten the film but does not serve as an adhesive.
[0013] <Metal material connection method>
[10] A method for connecting metal materials, in which end A of metal material A and end B of metal material B are overlapped with a film mainly composed of a thermoplastic resin, and the film is melted and solidified at the overlapping portion to connect metal material A and metal material B.
[11] The method for connecting metal materials according to
[10] , wherein the film has a thickness of 10 μm to 3 mm. Effect of the Invention
[0014] According to the present invention, a joining technique can be provided which is free from the risk of contamination of the production line by adhesive components, allows repairs, requires a short process time, and causes little change in thickness at the joining portion. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a plan view of a connected body of metal materials in one embodiment of the present invention. [Diagram 2] FIG. 2 is a plan view of a connected body of metal materials in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described in detail. In this specification, "connection" means connecting objects to form a continuous piece, and "bonding" is a subordinate concept. In this specification, "bonding" means connecting objects so that they come into contact with each other, and "adhesion" and "welding" are subordinate concepts. "Adhesion" means bonding two adherends (objects to be bonded) together via an organic material such as a tape or adhesive (such as a thermosetting resin or a thermoplastic resin). "Welding" means melting the surface of a thermoplastic resin or the like by heat, and then cooling it to cause entanglement through molecular diffusion, resulting in a bonded state.
[0017] [Metal material connector] The connected body of metal materials has an overlapping portion 4 where an end A:5 of a metal material A:1 and an end B:6 of a metal material B:2 are overlapped with each other via a film 3 (hereinafter, simply referred to as a "film") mainly composed of a thermoplastic resin. The film 3 is a film that has been melted and solidified at the overlapping portion 4. As shown in Figure 1, the connected body of this embodiment has an "overlapped portion 4" in which an end B:6 of a metal material B:2 is placed on an end A:5 of a metal material A:1 with the film 3 interposed therebetween. In this specification, the term "main component" refers to the component that is contained in the largest amount among the resin components in the film. The film preferably contains 50% by mass or more of the resin component, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.
[0018] By melting and solidifying the film 3 at the overlapping portion 4, the film 3 and the end A:5 of the metal material A:1 are joined, and the film 3 and the end B:6 of the metal material B:2 are joined, and the metal material A:1 and the metal material B:2 are connected to form a connected body. The connected body of the present invention obtained by melting and solidifying the film at the overlapping portion 4 exhibits excellent connection strength. Since the strength of the connection is affected by many factors, such as the thickness of the film, the molecular weight and chemical structure of the polymer constituting the film, the mechanical properties, and the viscoelastic properties, in addition to the strength of the interfacial interaction between the film and the metal material, the details of the mechanism by which the connector of the present invention exhibits excellent connection strength are not clear, but it is presumed that the main factor is the formation of chemical bonds or intermolecular forces, such as hydrogen bonds or van der Waals forces, at the interfaces between the film and metal material A and between the film and metal material B. However, since the state or properties of the interface between the film and the metal material in the connector are identified by analyzing the chemical structure of an extremely thin interface on the nanometer level or less, it is impossible or impractical with current technology to identify the connector of the present invention by directly identifying the state or properties of the interface between the film and the metal material.
[0019] The connected body of the present invention is connected by a film 3 that has been melted and solidified at the overlapping portion 4. The film 3 that has been melted and solidified at the overlapping portion 4 can be distinguished from the film before melting and solidification by whether the corners of the film are rounded and whether there is variation in thickness. A film before melting and solidifying has sharp cut surfaces formed during the manufacturing process of the film, but the film 3 that constitutes the metal material connection body of the present invention is a film 3 that has been melted and solidified at the overlapping portion 4, so it does not have sharp cut surfaces formed during the manufacturing process of the film, and it is presumed that the corners of the film are rounded. Since a film is usually manufactured to have a uniform thickness, there is no variation in thickness before melting and solidification, but since the film 3 constituting the metal material joint of the present invention is a film 3 that has undergone melting and solidification at the overlapping portion 4, it is presumed that there is a variation in thickness that inevitably occurs during the melting and solidification process. Any appropriate method can be adopted as a method for measuring the thickness variation, such as measuring the thickness of any multiple points on the surface of the measurement object and performing statistical processing. Examples of such a method for measuring the thickness include a method involving physical contact such as a micrometer, a micro caliper, a dial gauge, etc.; a non-contact method for measuring the transmittance or reflectance of alpha rays, X-rays, infrared rays, electromagnetic waves, etc. for the measurement object; a method for cutting the measurement object at any measurement point and observing it with an optical microscope or an electron microscope; and the like, and a combination of these may be adopted. It is presumed that after melting and solidifying at the overlapping portion 4, the surface texture of end A:5 of metal material A:1 is transferred to the film surface that contacts end A:5, and the surface texture of end B:6 of metal material B:2 is transferred to the film surface that contacts end B:6. Here, surface texture refers to the fine irregularities created on the surface of the metal material during machining or other processes of the metal material.
[0020] The connection of the present invention utilizes the phase change (solid-liquid-solid) of a film mainly composed of a thermoplastic resin, and is a connection that does not involve a chemical reaction such as a polymerization reaction. Since the film is used in a state in which the polymerization reaction is completed, the polymerization reaction does not proceed even at room temperature, and the film can be stored for a long period of time at room temperature. The film can be softened and melted by heat and can be easily peeled off, so it has excellent dismantling properties. In addition, since the film has thermoplastic properties, it can be reversibly softened, melted, and solidified repeatedly, and it also has excellent repairability. The connection using the film utilizes the phase change (solid-liquid-solid) of the film, and has the advantage that it takes a short time compared to a polymerization reaction involving the formation of chemical bonds, and the process time is short. Since the film is not a liquid at room temperature but a solid where the polymerization reaction is completed, and is bonded by a mechanism different from adhesion, it is unnecessary to use an adhesive containing an adhesive component for the purpose of adhesion, and there is no need to worry about contamination of the production line by the adhesive component. Since the polymerization reaction of the film is completed, it also has excellent heat resistance and chemical resistance. In addition, because the connection is made using a thin film, there is an advantage that there is less change in thickness at the connection compared to rivets, etc.
[0021] The connection body is preferably formed by interposing the film 3 over the entire surface of the overlapping surface between the end A:5 of the metal material A:1 and the end B:6 of the metal material B:2.
[0022] <Metal materials> The shapes of the metal material A and the metal material B are not particularly limited as long as they are flat, but the present invention is suitable for connecting at least one selected from the group consisting of metal plates with a thickness of 1 mm or less and metal foils with a thickness of 1 mm or less, and is suitable for applications in which the metal material A and the preceding metal material B are both strip-shaped (long), and end A of the metal material A and end B of the metal material B are overlapped and connected so as to be continuous in the longitudinal direction. Specifically, the present invention is suitable for applications in which the metal foil is wound into a roll, and is particularly suitable for applications in which the end of a preceding roll material being fed into a production line is connected to the start of a following roll material, and for applications in which the end and start of a roll material having a break in the roll are connected. In this specification, the metal foil means a highly ductile metal that is stretched into a thin paper shape.
[0023] The type of metal for metal material A and metal material B is not particularly limited, but is preferably at least one selected from the group consisting of aluminum, iron, copper, magnesium, and alloys thereof. From the viewpoint of the strength of the interfacial adhesion with the film, it is particularly preferable to use at least one selected from the group consisting of aluminum alloys and iron alloys, since this can achieve a strong connection. Furthermore, the surface of at least one selected from the group consisting of metal material A and metal material B may be subjected to a metal plating treatment, or may be coated with a resin. Examples of the resin include polyolefins and acid-modified products thereof, polystyrene, polymethyl methacrylate, AS resin, ABS resin, thermoplastic aromatic polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonate, polyimide, polyamide, polyamideimide, polyetherimide, polyethersulfone, polyphenylene ether and modified products thereof, polyphenylene sulfide, polyoxymethylene, polyarylate, polyether ketone, polyether ether ketone, polyether ketone ketone, thermoplastic epoxy resins, and the like.
[0024] By pretreating the portions of metal material A and metal material B that come into contact with the film, high adhesive strength may be obtained between the film and the metal material. As the pretreatment, a treatment for cleaning the surface of the metal material or a treatment for making the surface uneven is preferable. When the metal material is made of aluminum or iron, at least one pretreatment selected from the group consisting of degreasing treatment, UV ozone treatment, blasting treatment, polishing treatment, plasma treatment, and etching treatment is preferable. The pretreatment may be performed by one type alone or by two or more types. As the specific method for these pretreatments, known methods can be used.
[0025] <Film> In this specification, the term "film" refers to a thin film of a resin whose main component is a thermoplastic resin, or a thin film of a resin composition whose main component is a thermoplastic resin.
[0026] In order to fully impart the properties of a thermoplastic resin to the film, the content of the thermoplastic resin is preferably 60 mass % or more of the resin components in the film, more preferably 70 mass % or more, even more preferably 80 mass % or more, and most preferably 90 mass % or more.
[0027] The thermoplastic resin is preferably an amorphous thermoplastic resin. In this embodiment, the amorphous thermoplastic resin means a resin in which no crystals are present or the content of crystals is very small, specifically, the heat of fusion of the crystals is 15 J / g or less.
[0028] The heat of fusion is calculated from the area of the endothermic peak of DSC (differential scanning calorimeter) and the weight of the thermoplastic resin component. When an inorganic filler or the like is contained in the film, the heat of fusion is calculated from the weight of the thermoplastic resin component excluding the inorganic filler. Specifically, 2-10 mg of a sample is weighed out, placed in an aluminum pan, and heated from 23°C to 200°C or higher at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve, and the heat of fusion can be calculated from the area of the endothermic peak at the time of melting obtained from the DSC curve and the weighed value. More preferably, the heat of fusion is 11 J / g or less, even more preferably 7 J / g or less, even more preferably 4 J / g or less, and most preferably, the melting peak is below the detection limit.
[0029] In a film whose main component is an amorphous thermoplastic resin with a heat of fusion of 15 J / g or less, when heated to melt it, there is no sudden drop in viscosity as seen in conventional hot melt adhesives, and it does not reach a low viscosity state (0.001 to 100 Pa s) even in high temperature ranges exceeding 200°C. Therefore, the film does not melt and flow out, and the thickness after solidification can be maintained within a specified range, making it possible to stably obtain high bonding strength.
[0030] When the amorphous thermoplastic resin, which is the main component of the film, contains a small amount of crystals, the melting point is preferably 50 to 400° C., more preferably 60 to 350° C., and even more preferably 70 to 300° C. By having a melting point in the range of 50 to 400° C., the film efficiently deforms and melts when heated, and effectively wets and spreads over the respective bonding surfaces of the film and metal material A and the film and metal material B, thereby obtaining a high bonding strength. In this specification, the melting point of a thermoplastic resin means the melting peak temperature measured by DSC. If the melting peak is not obtained or the heat of fusion is 15 J / g or less, the melting point is the glass transition point plus 70°C. The glass transition point means the temperature at which the DSC curve starts to drop in the second cycle after heating to 200°C by DSC, cooling to 40°C or less, and further heating to 200°C.
[0031] The amorphous thermoplastic resin is preferably at least one selected from the group consisting of thermoplastic epoxy resins and phenoxy resins. Thermoplastic epoxy resins and phenoxy resins have low cohesive strength within the resin, and therefore have strong interactions with metal materials, and can connect metal materials with a stronger connecting strength than conventional crystalline hot melt adhesives. In addition, thermoplastic epoxy resins and phenoxy resins have excellent flexibility and toughness, and therefore can provide a strong connection.
[0032] The amorphous thermoplastic resin preferably has an epoxy equivalent of 1,600 or more, or does not contain an epoxy group. The epoxy equivalent (weight of the thermoplastic resin containing 1 mole of epoxy groups) is the epoxy equivalent of the thermoplastic resin contained in the film before linking, and is a value (unit: g / eq.) measured by the method specified in JIS-K7236:2001. Specifically, a potentiometric titrator is used to add brominated tetraethylammonium acetate solution, and a 0.1 mol / L perchloric acid-acetic acid solution is used, and the solvent-diluted product (resin varnish) is calculated as a solid content equivalent value from the non-volatile content. In the case of a mixture of two or more resins, it can also be calculated from the content and epoxy equivalent of each resin. The epoxy equivalent of the amorphous thermoplastic resin is more preferably 2,000 or more, even more preferably 5,000 or more, and even more preferably 9,000 or more, and most preferably is equal to or more than the detection limit so that the epoxy group is not substantially detected. Note that the epoxy equivalent being equal to or more than the detection limit means that the epoxy group is not detected when the epoxy equivalent is measured based on JIS K 7236:2001 described later.
[0033] By using a film whose main component is an amorphous thermoplastic resin with an epoxy equivalent of 1,600 or more, the sudden decrease in viscosity can be more effectively suppressed, and a higher bonding strength can be stably obtained.
[0034] <Thermoplastic epoxy resin> The thermoplastic epoxy resin is preferably a polymer of (a) a difunctional epoxy resin monomer or a difunctional epoxy resin oligomer and (b) a difunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxy group, a mercapto group, an isocyanato group, and a cyanate ester group. By using such a compound, the polymerization reaction for forming a linear polymer proceeds preferentially, making it possible to obtain a thermoplastic epoxy resin having the desired properties.
[0035] The (a) difunctional epoxy resin monomer means an epoxy resin monomer having two epoxy groups in the molecule, and the (a) difunctional epoxy resin oligomer means an epoxy resin oligomer having two epoxy groups in the molecule. Specific examples of the (a) include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bifunctional phenol novolac type epoxy resins, bisphenol AD type epoxy resins, biphenyl type epoxy resins, bifunctional naphthalene type epoxy resins, bifunctional alicyclic epoxy resins, bifunctional glycidyl ester type epoxy resins (e.g., diglycidyl phthalate, diglycidyl tetrahydrophthalate, dimer acid diglycidyl ester, etc.), bifunctional glycidyl amine type epoxy resins (e.g., diglycidyl aniline, diglycidyl toluidine, etc.), bifunctional heterocyclic epoxy resins, bifunctional diarylsulfone type epoxy resins, hydroquinone type epoxy resins (e.g., hydroquinone diglycidyl ether, 2,5-di-tert-butyl ether, etc.), t-Butylhydroquinone diglycidyl ether, resorcin diglycidyl ether, etc.), bifunctional alkylene glycidyl ether compounds (e.g. butanediol diglycidyl ether, butenediol diglycidyl ether, butynediol diglycidyl ether, etc.), bifunctional glycidyl group-containing hydantoin compounds (e.g. 1,3-diglycidyl-5,5-dialkylhydantoin, 1-glycidyl-3-(glycidoxyalkyl)-5,5-dialkylhydantoin, etc.), bifunctional glycidyl group-containing siloxanes (e.g. 1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane, α,β-bis(3-glycidoxypropyl)polydimethylsiloxane, etc.) and modified products thereof. Among these, bisphenol A type epoxy resins, bisphenol F type epoxy resins, and biphenyl type epoxy resins are preferred in terms of reactivity and workability. Examples of the (b) bifunctional compound having a phenolic hydroxyl group include mononuclear aromatic dihydroxy compounds having one benzene ring, such as catechol, resorcin, and hydroquinone; bisphenols, such as bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane (bisphenol F), and bis(4-hydroxyphenyl)ethane (bisphenol AD); compounds having a condensed ring, such as dihydroxynaphthalene; bifunctional phenol compounds having an allyl group introduced therein, such as diallyl resorcin, diallyl bisphenol A, and triallyl dihydroxybiphenyl; and dibutyl bisphenol A. Specific examples of the (b) carboxy group-containing compound include adipic acid, succinic acid, malonic acid, cyclohexanedicarboxylic acid, phthalic acid, isophthalic acid, and terephthalic acid. Examples of the (b) bifunctional compound having a mercapto group include ethylene glycol bisthioglycolate and ethylene glycol bisthiopropionate. Specific examples of the (b) isocyanato group-containing bifunctional compound include diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HMDI), and tolylene diisocyanate (TDI). Specific examples of the (b) cyanate ester group-containing bifunctional compound include 2,2-bis(4-cyanatophenyl)propane, 1,1-bis(4-cyanatophenyl)ethane, and bis(4-cyanatophenyl)methane. Among the above (b), a bifunctional compound having a phenolic hydroxyl group is preferred from the viewpoint of obtaining a thermoplastic polymer, a bifunctional compound having two phenolic hydroxyl groups and a bisphenol structure or a biphenyl structure is preferred from the viewpoint of heat resistance and connectability, and at least one selected from the group consisting of bisphenol A, bisphenol F and bisphenol S is preferred from the viewpoint of heat resistance and cost.
[0036] When the (a) is a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, or a biphenyl type epoxy resin, and the (b) is at least one selected from the group consisting of bisphenol A, bisphenol F, and bisphenol S, the polymer obtained by polymerization of the (a) and (b) has a main chain having a paraphenylene structure and an ether bond as a main skeleton, the main chain being linked by an alkylene group, and a structure in which a hydroxyl group generated by polyaddition is arranged in a side chain. The linear structure of the paraphenylene skeleton can increase the mechanical strength of the polymer after polymerization, and the hydroxyl groups arranged in the side chains can improve adhesion to metal materials. As a result, high bond strength can be achieved while maintaining the adhesiveness of the thermosetting resin. Furthermore, in the case of a thermoplastic resin, recycling and repair are possible by softening and melting with heat, improving the recyclability and repairability that are problems with thermosetting resins.
[0037] Phenoxy resin Phenoxy resin is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin, and has thermoplastic properties. For the production of phenoxy resin, a method by direct reaction of dihydric phenols with epichlorohydrin and a method by addition polymerization reaction of diglycidyl ether of dihydric phenols with dihydric phenols are known, but the phenoxy resin used in the present invention may be obtained by either method. In the case of direct reaction of dihydric phenols with epichlorohydrin, examples of dihydric phenols include phenols such as bisphenol A, bisphenol F, bisphenol S, biphenol, biphenylenediol, and fluorenediphenyl; and aliphatic glycols such as ethylene glycol, propylene glycol, and diethylene glycol. Among them, bisphenol A, bisphenol F, and bisphenol S are preferred from the viewpoints of cost, connectivity, viscosity, and heat resistance. These may be used alone or in combination of two or more. Phenoxy resin has a chemical structure similar to that of epoxy resin, with a paraphenylene structure and an ether bond as the main skeleton, a main chain connecting these, and a structure in which hydroxyl groups are arranged in the side chains.
[0038] <Physical properties of thermoplastic epoxy resin and phenoxy resin> The thermoplastic epoxy resin and the phenoxy resin preferably have a weight average molecular weight of 10,000 to 500,000, more preferably 18,000 to 300,000, and even more preferably 20,000 to 200,000, which is a value calculated in terms of polystyrene by GPC (gel permeation chromatography). The weight average molecular weight is calculated from the elution peak position detected by GPC, and each is a value of the molecular weight calculated in terms of standard polystyrene. When the weight average molecular weight is within this range, the balance between thermoplasticity and heat resistance is good, and a linker can be efficiently obtained by melting, and the heat resistance is also high. When the weight average molecular weight is 10,000 or more, the heat resistance is excellent, and when it is 500,000 or less, the viscosity during melting is low and the linkage is high.
[0039] <Components other than the resin component in the film> If necessary, the film may or may not contain fillers and additives as components other than the resin component, provided that the object of the present invention is not impaired.
[0040] The filler includes inorganic fillers and organic fillers (resin powder). Examples of inorganic fillers include spherical fused silica, metal powders such as iron, silica sand, talc, calcium carbonate, mica, acid clay, diatomaceous earth, kaolin, quartz, titanium oxide, silica, phenolic resin microballoons, and glass balloons. When the film contains a filler, the content of the filler in the total amount (100 volume %) of the film is preferably 50 volume % or less, more preferably 30 volume % or less, further preferably 20 volume % or less, and most preferably 10 volume % or less. The volume of the filler can be calculated by dividing the weight of the filler contained in the film by the apparent specific gravity of the filler. The content of the resin component in the total amount (100 volume%) of the film is preferably 10 volume% or more, more preferably 20 volume% or more, even more preferably 30 volume% or more, and even more preferably 50 volume% or more, in one embodiment 80 volume% or more, in another embodiment 90 volume% or more, and in another embodiment 99 volume% or more.
[0041] Examples of the additives include antifoaming agents, coupling agents such as silane coupling agents, pigments, etc., and these may be contained alone or in combination of two or more kinds. The content of the additive in the film is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The content of the resin component in the film is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and still more preferably 50% by mass or more, in one embodiment 80% by mass or more, in another embodiment 90% by mass or more, and in another embodiment 99% by mass or more.
[0042] Film morphology and physical properties The film before bonding preferably has a thickness of 10 μm to 3 mm. By making the film 10 μm to 3 mm thick, it can be efficiently spread by heating or pressing between the bonding surfaces of the film and metal material A and between the film and metal material B, and a high bonding strength can be obtained. From the viewpoint of obtaining a connection body with excellent connectivity in a short process time, the thickness of the film before bonding is more preferably 1 mm or less, even more preferably 0.5 mm or less, even more preferably 0.3 mm or less, particularly preferably 0.2 mm or less, and most preferably 0.1 mm or less. From the viewpoint of handling properties, the thickness of the film before bonding is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more.
[0043] The film may be a single layer or a laminate consisting of multiple layers. From the viewpoint of ease of production and improvement of the connecting strength, the thermoplastic resin layer is preferably a single layer. The film may be a multiple layer in which the thermoplastic resin is laminated on a film substrate composed of a resin having a melting point higher than that of the resin composition. In such a case, the resin film substrate does not melt when heat-welded to the metal substrate, and the thickness of the resin film substrate remains, so that good connecting strength can be maintained.
[0044] The film may also have tackiness to the extent that it does not impair its binding strength or heat resistance. Tackiness may be imparted by mixing a tackifier into the thermoplastic resin, or by applying an adhesive containing an adhesive component such as a tackifier to the film. The adhesive preferably has a function of temporarily fixing the film and does not have an adhesive function. An adhesive that has a function of temporarily fixing the film and does not have an adhesive function is, for example, an adhesive that remains within the surface of the joining surface and is not exposed to the outside of the surface. The adhesive may be applied to the entire surface of the joining surface, or to a part of the joining surface in stripes, dots, grids, tiles (a shape with multiple squares lined up with gaps), etc. The smaller the application area, the weaker the tackiness, but the risk of the adhesive being exposed to the outside from the edge of the film after joining and becoming a cause of contamination can be reduced.
[0045] In conventional adhesive tapes, the adhesive strength between the metal material and the film is provided only by the adhesiveness of the adhesive layer of the adhesive tape, but in the case of the thermoplastic film, the adhesive strength is provided by the adhesion caused by the melting and solidification of the thermoplastic resin as described above, so the tackiness is preferably such that it provides the temporary fixing function as described above. In other words, when the film is placed between the metal materials, it is not necessary for the film to stick to the metal materials, and it is sufficient that the resistance is increased (it becomes less slippery) when a force in the shear direction is applied. For the purpose of imparting tackiness sufficient to provide a temporary fixing function, it is preferable to limit the amount of adhesive applied to the minimum amount necessary to temporarily hold the film (to prevent slipping).
[0046] In conventional adhesive tapes, if there are any areas where the adhesive layer protrudes from the edge of the mating surface, the adhesive components may adhere to the transport path or mold of the production line, causing contamination. Also, if the adhesive tape is peeled off within the line for some reason, the adhesive layer is exposed, and there is a concern that the adhesive components may adhere to the transport path or mold of the production line, causing contamination. In addition, the end faces of strip-shaped metal materials are not necessarily straight, and in such cases, when the metal material and the double-sided adhesive tape are overlapped and bonded to create a connected body, the double-sided adhesive tape, which has a straight shape, cannot be completely overlapped with the strip-shaped metal material, resulting in a connected body with either (a) exposed double-sided adhesive tape or (b) parts of the metal material that are not bonded. In the case of (a) above, the adhesive component may adhere to the conveying path or mold of the production line, causing contamination. In the case of (b) above, the chemical solution is likely to accumulate in the unbonded parts, and when passing through multiple chemical solution layers, the amount of chemical solution carried over increases, and the contamination of the chemical solution layers may progress quickly. According to the present invention, in which bonding strength is achieved by adhesion through melting and solidifying a thermoplastic resin, no adhesive is required for bonding purposes, and even if an adhesive is used for purposes such as positioning, it can be used only to a minimum extent, thereby avoiding all of the above-mentioned problems associated with conventional adhesive tapes.
[0047] The breaking strength of the film in the connected body of the metal material A and the metal material B connected by the film is preferably 20 to 1000 N / 25 mm.
[0048] The breaking strength of the film in the connected body is more preferably 50 to 1000 N / 25 mm, and most preferably 100 to 1000 N / 25 mm.
[0049] The breaking strength when the metal material A and the metal material B are connected using the film is the tensile strength at break per 25 mm film width measured under the conditions described in the Examples section.
[0050] <Film manufacturing method> The method for producing a film mainly composed of a thermoplastic resin is not particularly limited. For example, a resin composition may be obtained by heating and polymerizing a monomer or oligomer of a bifunctional epoxy compound, adding a solvent to the obtained resin composition as necessary, applying the composition to a release film, curing and drying, and applying pressure as necessary to obtain a film. The polymerization reaction may be carried out after application to a release film or after the film is obtained, or a combination of these may be used.
[0051] [Metal material connection method] The method for producing a connected body according to this embodiment includes a step of overlapping end A:5 of metal material A:1 and end B:6 of metal material B:2 via a film mainly composed of a thermoplastic resin at overlapping portion 4, where the film is melted and solidified to connect metal material A and metal material B. By melting and solidifying the film at overlapping portion 4, film 3 and end A:5 of metal material A:1 are joined, and film 3 and end B:6 of metal material B:2 are joined, connecting metal material A and metal material B. The metal material and film are the same as those constituting the above-mentioned connecting body, and therefore a description thereof will be omitted.
[0052] <Melting and solidifying the film> The method for melting the film is not particularly limited as long as it is a means capable of heating and melting the film. Specifically, the film may be melted by at least one method selected from the group consisting of contact heating, hot air heating, heat pressing, impulse heater heating, hot plate welding, infrared heating, ultrasonic welding, vibration welding, and high-frequency induction welding. Among them, melting by at least one method selected from the group consisting of impulse heater and heat pressing is preferred from the viewpoint of ease of production and shortening the process.
[0053] In the case of hot pressing, it is more preferable to carry out the heating and pressing under conditions of 100 to 400° C. and 0.001 to 20 MPaG. The heating conditions are more preferably 100 to 300° C., even more preferably 120 to 250° C., and most preferably 150 to 220° C. By heating at 100 to 400° C., the film efficiently deforms and melts, effectively wetting and spreading over the respective bonding surfaces of the film and metal material A and the film and metal material B, thereby obtaining a high bonding strength. The pressure is preferably from 0.001 to 20 MPaG, more preferably from 0.005 to 10 MPaG, and most preferably from 0.01 to 5 MPaG. By applying a pressure of from 0.001 to 20 MPaG, the film is efficiently deformed and effectively wetted and spread, thereby obtaining a high connecting strength. By melting and solidifying the film, the film and metal material A and the film and metal material B are bonded to each other, and metal material A and metal material B are connected to each other.
[0054] In the case of ultrasonic welding, the transmission frequency is preferably 10 to 70 kHz, and more preferably 15 to 40 kHz. From the viewpoints of adhesion and appearance, the ultrasonic application time is preferably 0.1 to 3 seconds, and more preferably 0.2 to 2 seconds. When pressure is applied during ultrasonic application, the pressure is preferably 0.01 to 20 MPaG, more preferably 0.1 to 10 MPaG, and even more preferably 0.2 to 5 MPaG. Within this pressure range, the film is efficiently deformed and effectively wets and spreads across the adhesive surface, resulting in high adhesive strength. In the case of high-frequency induction welding, the output may be in the range of 100 to 5000 W, and the oscillation time may be adjusted according to the size and type of the resin substrate, and is, for example, preferably 1.0 to 10.0 seconds, and more preferably 1.5 to 8.0 seconds.
[0055] Methods for solidifying the molten film include a method of cooling at room temperature or a method of cooling using a cooling device. Here, "room temperature" means a general room temperature within the range of 5 to 30° C. Among these, the method of cooling at room temperature is preferred from the viewpoint of ease of production.
[0056] In this specification, "solidified" means that the film is solid at room temperature, that is, has no fluidity in the absence of pressure at 23° C. However, the film after solidification may have tackiness. EXAMPLES
[0057] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.
[0058] <Metal material A and metal material B> As metal material A and metal material B, C1100 (tough pitch copper) having a width of 25 mm, a length of 100 mm and a thickness of 0.1 mm was prepared.
[0059] <Weight average molecular weight, heat of fusion and epoxy equivalent of thermoplastic epoxy resin and phenoxy resin> The weight average molecular weight, heat of fusion and epoxy equivalent of the thermoplastic epoxy resin and the phenoxy resin were determined as follows.
[0060] (Weight average molecular weight) Thermoplastic epoxy resin or phenoxy resin was dissolved in tetrahydrofuran, and measurement was performed under the following conditions using Prominence 501 (manufactured by Showa Science Co., Ltd., Detector: Shodex (registered trademark) RI-501 (manufactured by Showa Denko K.K.)). Column: Showa Denko LF-804 x 2 Column temperature: 40℃ Sample: 0.4% by mass of resin in tetrahydrofuran Flow rate: 1ml / min Eluent: Tetrahydrofuran Calibration method: Conversion using standard polystyrene
[0061] (Heat of fusion) 2 to 10 mg of thermoplastic epoxy resin or phenoxy resin was weighed out and placed in an aluminum pan, and the temperature was raised from 23°C to 200°C at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve. The heat of fusion was calculated from the area of the endothermic peak at the time of melting in the DSC curve and the weighed value.
[0062] (epoxy equivalent) The values were measured in accordance with JIS K-7236:2001 and converted into values based on the resin solid content. In the case of simple mixtures that did not involve reactions, the values were calculated from the epoxy equivalent and content of each.
[0063] < Reference example 1> (Film P-1) In a reaction apparatus equipped with a stirrer, reflux condenser, gas inlet tube, and thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged, and the temperature was raised to 100°C while stirring under a nitrogen gas atmosphere. After visually confirming that the mixture had dissolved, the mixture was cooled to 40°C to obtain a resin composition with a solid content of about 20% by mass. The solvent was removed from this to obtain a solid. A non-adhesive fluororesin film (Nitoflon (registered trademark) No. 900UL, manufactured by Nitto Denko Corporation) was placed on the upper and lower plates of a press machine, and the solid was placed on the non-adhesive fluororesin film of the lower plate. The press machine was then heated to 160°C, and the resin composition or phenoxy resin was heat-compressed for 2 hours to obtain a solid adhesive (P-1) in the form of a film having a thickness of 100 μm and a solid content of 100 mass%. The weight-average molecular weight was about 37,000. The epoxy equivalent was above the detection limit (i.e., almost no epoxy groups were present). No heat of fusion peak was detected in DSC, confirming that the material was amorphous. (concatenation) End B of metal material B was overlapped on end A of metal material A via the film P-1 cut to a size of 20 x 25 mm, and placed on a hot plate set at 200 ° C. At the overlapping portion via the film P-1, metal material A was placed on the hot plate, a 3 x 3 cm glass plate was placed on metal material B, and a 2 kg weight was placed on the glass plate to perform welding for 1 minute. After the welding, the glass plate and the weight were removed and the film P-1 was cooled to room temperature.
[0064] <Example 2> (Film P-2) A reactor equipped with a stirrer, reflux condenser, gas inlet tube, and thermometer was charged with 20 g of Phenototo (registered trademark) YP-50S (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 50,000) and 80 g of cyclohexanone, and the mixture was heated to 60°C while stirring, and the mixture was confirmed to have dissolved by visual inspection, and cooled to 40°C to obtain a resin composition with a solid content of 20% by mass. The resin composition was applied onto a release film and dried at 120°C for 30 minutes to obtain a film P-2 with a solid content of 100% by mass and a thickness of 100 μm. The epoxy equivalent was above the detection limit (i.e., almost no epoxy groups were present). No heat of fusion peak was detected in DSC, and it was confirmed to be amorphous. (concatenation) Other than using P-2 as the film Reference example A conjugate was prepared in the same manner as in 1.
[0065] <Example 3> (Film P-3) A reactor equipped with a stirrer, reflux condenser, gas inlet tube, and thermometer was charged with 20 g of Phenototo (registered trademark) YPS-007A (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 42000) and 80 g of cyclohexanone, and the mixture was heated to 60°C while stirring, and the mixture was confirmed to have dissolved by visual inspection, and cooled to 40°C to obtain a resin composition with a solid content of 20% by mass. The resin composition was applied onto a release film and dried at 120°C for 30 minutes to obtain a film P-3 with a solid content of 100% by mass and a thickness of 100 μm. The epoxy equivalent was above the detection limit (i.e., almost no epoxy groups were present). No heat of fusion peak was detected in DSC, and it was confirmed to be amorphous. (concatenation) Other than using P-3 as film Reference example A conjugate was prepared in the same manner as in 1.
[0066] < Reference example 4 > (concatenation) The film used was a crystalline olefin-based hot melt adhesive film (Elfan (registered trademark) NT-120, manufactured by Nihon Matai Co., Ltd., thickness 80 μm before preparation of the connector) and the temperature of the hot plate was set to 150 ° C. Reference example 1 The linker was prepared in the same manner as in Example 1. The heat of fusion peak in DSC was 60 J / g.
[0067] <Comparative Example 1> (concatenation) Two pieces of adhesive tape (Sekisui Cellotape (registered trademark) No. 252, manufactured by Sekisui Chemical Co., Ltd., thickness 50 μm before preparation of the connector) cut to a size of 30 × 25 mm were used to attach end B of metal material B onto end A of metal material A so as to cover both sides of the overlapping portion, which was 25 mm wide × 20 mm long, as shown in Figure 2, to prepare a connector.
[0068] <Comparative Example 2> (concatenation) End B of metal material B was placed on end A of metal material A via double-sided adhesive tape (NITOMS PROSELF, manufactured by Nitoms Inc.) cut to a size of 20 x 25 mm. A 3 x 3 cm glass plate was placed on end B, a 2 kg weight was placed on the glass plate, and after leaving it for 1 minute, the weight was removed to create a connected body.
[0069] <Comparative Example 3> (concatenation) A linked body was prepared in the same manner as in Comparative Example 2, except that a heat-resistant double-sided adhesive tape (polyimide tape PB416-20-30, manufactured by AS ONE Corporation) cut to a size of 20×25 mm was used as the adhesive tape.
[0070] [Breaking strength measurement_tensile test] The tensile strength of the connected bodies obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was measured. The measurement conditions were a gripping distance of 13 cm and a tensile speed of 5 mm / min, using a Shimadzu Corporation universal testing machine Autograph AG-X Plus. The measurement results (breaking strength) are shown in Table 1. The measurements were taken under the conditions of "room temperature: 23°C" and "immersed in ethylene glycol." In Table 1, the measurements under the "immersed in ethylene glycol" condition were taken after immersing the sample in ethylene glycol at 40°C for 5 days, removing the sample, immersing the sample in water for 5 seconds, wiping off the ethylene glycol, photographing the appearance, and then leaving the sample to stand for 20 to 30 minutes before measuring the value at room temperature.
[0071] [Line contamination] The possibility of production line contamination by sticky components was evaluated. As described in the Background section, when adhesive tape is used for connection, contamination of the production line becomes a major problem, especially if the adhesive tape comes off due to an accident on the production line. Therefore, in this evaluation, after the tensile test described above, when the metal materials A and B were separated, the presence or absence of exposure of the layer containing the adhesive component was observed, and the line contamination was evaluated. Specifically, after the tensile test, when the metal materials A and B were separated, those with an exposed layer containing the adhesive component were rated as "X (possibility of line contamination)" and those without an exposed layer containing the adhesive component were rated as "O (possibility of line contamination not occurring)." The evaluation results are shown in Table 1. When adhesive tape is used for connection, peeling due to cohesive failure is generally unlikely to occur. Separation of metal materials A and B is likely to be caused by interfacial peeling, in which case the adhesive surface will be exposed after failure (i.e., after metal materials A and B are separated). In all of Examples 1 to 4, the connector was produced by utilizing the phase change (solid-liquid-solid) of a film whose main component was a thermoplastic resin, and metal materials A and B were bonded together by a mechanism other than adhesion, so the above evaluation for all of them was "Good (no possibility of line contamination)."
[0072] [Table 1] [Industrial Applicability]
[0073] The present invention is suitable for applications such as connecting frame materials in a production line for LED lead frames, and connecting board materials in a production line for flexible printed circuit boards, but is not limited to these exemplary applications. [Explanation of symbols]
[0074] 1 Metal material A 2 Metal material B 3. Film (film that constitutes the connecting body) 4. Overlapped section 5 End A 6 End B 7 Single-sided adhesive tape
Claims
1. A connected body of metal materials having an overlapping portion in which an end A of a metal material A and an end B of a metal material B are overlapped with each other via a film mainly composed of a thermoplastic resin, The film is a film that has been melted and solidified at the overlapping portion, The thermoplastic resin is an amorphous thermoplastic resin, the amorphous thermoplastic resin is at least one selected from the group consisting of a thermoplastic epoxy resin and a phenoxy resin, The thermoplastic epoxy resin is (a) a polymer of a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group (excluding bisphenols and polyhydroxy polyethers synthesized from epichlorohydrin), The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film. A metal connector.
2. 2. The metal material linkage according to claim 1, wherein the metal material A and the metal material B are at least one selected from the group consisting of a metal plate having a thickness of 1 mm or less and a metal foil having a thickness of 1 mm or less.
3. 2. The metal material connection according to claim 1, wherein the metal material A and the metal material B are in a strip shape, and the metal material A and the metal material B are connected so as to be continuous in the longitudinal direction.
4. The connected body of metal materials according to claim 3 , wherein the metal material A and the metal material B are rolled materials each formed by winding at least one selected from the group consisting of a metal plate and a metal foil into a roll shape.
5. 2. The metal material connection according to claim 1, wherein the film is disposed over the entire overlapping surfaces of the end portion A and the end portion B.
6. 2. The metal material linkage according to claim 1, wherein the amorphous thermoplastic resin is an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more, or an amorphous thermoplastic resin containing no epoxy groups.
7. The film has an adhesive, The metal material connector according to claim 1 , wherein the adhesive material functions to temporarily fasten the film but does not function as an adhesive.
8. A method for connecting metal materials, comprising: overlapping an end A of a metal material A and an end B of a metal material B with a film mainly composed of a thermoplastic resin therebetween; and melting and solidifying the film at an overlapping portion to connect the metal material A and the metal material B, The thermoplastic resin is an amorphous thermoplastic resin, the amorphous thermoplastic resin is at least one selected from the group consisting of a thermoplastic epoxy resin and a phenoxy resin, The thermoplastic epoxy resin is (a) a polymer of a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group (excluding bisphenols and polyhydroxy polyethers synthesized from epichlorohydrin), The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film. A method for connecting metal materials.
9. The method for connecting metal materials according to claim 8, wherein the film has a thickness of 10 μm to 3 mm.
Citation Information
Patent Citations
process for joining components
DE102016212622A1
JP1973021724B1
Bonding method of metal plate
JP1981089520A
Base material connecting method and base material connecting device
JP1998157896A
Method of producing sheet joined body, and sheet joined body
JP2009298136A