Method for evaluating delayed fracture characteristics of metal plate for press forming, method for manufacturing press-formed product, and program

By evaluating stress distributions in the thickness direction of sheared end faces, the method addresses inconsistent fracture predictions in high-strength steel plates, enhancing the reliability of press-formed products by accurately determining critical stress for delayed fracture prevention.

JP7563657B1Active Publication Date: 2024-10-08JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024531727
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-07-26
Filing Date
2024-03-28
Publication Date
2024-10-08
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Conventional methods for evaluating delayed fracture in high-strength steel plates after press forming are inadequate as they do not account for the varying critical stress due to different load conditions, particularly between uniaxial tensile deformation and bending deformation, leading to inconsistent evaluation accuracy.

Method used

A method that evaluates delayed fracture characteristics by considering the stress distribution in the thickness direction of the sheared end face, incorporating residual stress and external loads, using tests under multiple loading conditions and converting stress distributions into index values to predict fracture occurrence.

Benefits of technology

Enables accurate prediction and prevention of delayed fracture in press-formed products by determining critical stress based on stress gradients, improving evaluation accuracy and ensuring the reliability of high-strength steel plate applications in automotive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563657000004
    Figure 0007563657000004
  • Figure 0007563657000005
    Figure 0007563657000005
  • Figure 0007563657000006
    Figure 0007563657000006
Patent Text Reader

Abstract

The purpose of the present invention is to evaluate the delayed fracture properties of the sheared end surface, taking into account the load conditions during press forming. The delayed fracture properties evaluation method evaluates the delayed fracture properties of the sheared end surface of a metal plate for press forming used in press working, in which a target metal plate is sheared under the same shear conditions to prepare a plurality of test pieces having the sheared end surface, and tests are performed under a plurality of load conditions in which the stress distribution in the plate thickness direction is the same or similar to each other, in order to apply stress to the sheared end surface of the test piece under load conditions in which the stress distribution in the plate thickness direction is different from each other, and a critical stress, which is a limit value of the load stress at which delayed fracture does not occur, is obtained according to the stress distribution in the plate thickness direction based on the tests for each load condition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technique for evaluating delayed fracture properties at a sheared end surface of a metal sheet for press forming. The present invention also relates to a manufacturing method and program for a press-formed product utilizing the evaluation technique. The present invention is a technique suitable for a metal sheet for press forming made of a high-strength steel sheet. In this specification, a high-strength steel sheet refers to a steel sheet having a tensile strength of 980 MPa or more. [Background technology]

[0002] Currently, automobiles are required to improve fuel efficiency and collision safety by reducing their weight. To achieve both weight reduction and protection of passengers in the event of a collision, there is a trend to use high-strength steel plates in the structural parts of the car body. In particular, ultra-high-strength steel plates with a tensile strength of 1470 MPa or more have been used in car bodies in recent years. One of the issues when using high-strength steel plates in car bodies is delayed fracture that occurs after press forming. In particular, delayed fracture that occurs from the end face after shear processing is a major issue for steel plates with a tensile strength of 980 MPa or more. The end face after shear processing is also called the sheared end face. It is known that a large tensile stress remains at the sheared edge. This raises the concern of delayed fracture at the sheared edge. It is known that this delayed fracture is further accelerated by applying an external stress to the sheared edge.

[0003] Conventionally, methods proposed as methods for evaluating delayed fracture are described in, for example, Patent Documents 1 to 3. That is, Patent Documents 1 and 2 describe a test method in which stress is applied by constant displacement restraint due to bending deformation. Patent Document 3 describes a test in which stress is applied by constant load application due to uniaxial tensile deformation. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-142086 A [Patent Document 2] JP 2014-70927 A [Patent Document 3] JP 2016-57163 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, there has been concern about delayed fracture occurring from the sheared edge of high-strength steel sheet after press forming. The inventors have conducted extensive research into delayed fracture occurring at the sheared edge after press forming. As a result, they have found that even if the same stress load is applied to the sheared edge, the critical stress at which delayed fracture does not occur at the sheared edge may differ if the load conditions are different. For example, when comparing the case of uniaxial tensile deformation with the case of bending deformation, the critical stress at which delayed fracture does not occur at the sheared edge may differ. Specifically, they have found that the above critical stress may be lower in the case of uniaxial tensile deformation than in the case of bending deformation. For this reason, the conventional evaluation methods sometimes had poor evaluation accuracy for delayed fracture.

[0006] The present invention has been made in consideration of the above points, and aims to evaluate the delayed fracture properties of the sheared end surface, taking into account the load conditions during press forming. [Means for solving the problem]

[0007] The inventors conducted extensive research into the fact that the critical stress at which delayed fracture does not occur may differ between uniaxial tensile deformation and bending deformation. As a result, they discovered the following: In bending deformation, there is a stress gradient in the plate thickness direction compared to uniaxial tensile deformation (see Figures 5 and 6). For this reason, they discovered that in bending deformation, the crack propagation of delayed fracture is suppressed. Despite this discovery, conventional methods were unable to evaluate delayed fracture taking into account the stress distribution in the plate thickness direction at the shear end face. The inventors have found the following about actual automobile parts after press forming: in order to predict delayed fracture at the sheared end surface, the critical stress for delayed fracture must be set taking into account the stress distribution in the plate thickness direction.

[0008] Therefore, the inventors considered evaluating the critical stress for delayed fracture by taking into account the stress distribution in the plate thickness direction caused by an external load. Specifically, they assumed a residual stress in the plate width direction introduced at the shear end face. Then, they considered the following process for delayed fracture tests under stress loading conditions due to bending or uniaxial tension. That is, they considered measuring the critical stress for delayed fracture according to the plate thickness distribution of the stress load through the test, and quantifying the plate thickness distribution of the stress load. Note that stress loading conditions are synonymous with load loading conditions. The critical stress for delayed fracture according to the thickness distribution of stress load may be calculated based on the calculated residual stress distribution due to shear in the thickness direction, for example, by X-ray residual stress measurement or CAE analysis.

[0009] The critical stress for delayed fracture thus obtained is compared with the thickness distribution of stress applied under specific load conditions, making it possible to predict whether or not delayed fracture will occur under those load conditions. The load conditions are, for example, the method of applying a load such as bending (deformation) or short-axis tension (deformation) to a plate. Generally, deformation occurs in the plate due to a load such as bending. However, it is not necessary for a clear deformation to occur due to the application of the load. The present invention has been made based on the above considerations.

[0010] That is, in order to solve the problem, one aspect of the present invention is a delayed fracture property evaluation method for evaluating the delayed fracture property of a sheared end surface of a metal plate for press forming used in press working, in which a target metal plate is sheared under the same shearing conditions to prepare a plurality of test pieces having the above-mentioned sheared end surfaces, and tests are performed under a plurality of load conditions in which the stress distribution in the plate thickness direction is the same or similar to each other, thereby applying stress to the sheared end surfaces of the above-mentioned test pieces under load conditions in which the stress distribution in the plate thickness direction is different from each other, and a threshold stress, which is a limit value of the load stress at which delayed fracture does not occur according to the stress distribution in the plate thickness direction, is determined based on the above test for each load condition. Effect of the Invention

[0011] According to the aspect of the present invention, it is possible to evaluate the critical stress for delayed fracture of a metal plate for press forming by taking into account the stress distribution in the plate thickness direction due to an external load. The aspect of the present invention can be used when manufacturing a press-formed product using the evaluated metal plate for press forming. According to the aspect of the present invention, the delayed fracture property at the shear end surface of the plate can be evaluated in advance during the manufacturing process. Therefore, according to the aspect of the present invention, it is possible to select a press-formed shape and a metal plate having effective delayed fracture property and manufacture a press-formed product. Therefore, according to the aspects of the present invention, when a high-strength steel sheet is applied to various parts such as panel parts, structural / skeletal parts, etc. of an automobile, delayed fracture properties can be improved. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing an example of a process flow of evaluation according to an embodiment based on the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a shearing process. [Diagram 3] Schematic diagram of the shape of the sheared end surface on the remaining side, (a) being a cross-sectional view and (b) being a plan view. [Figure 4] FIG. 2 is a schematic diagram showing a residual stress distribution in the stretching direction at a typical sheared end surface. [Diagram 5]1 is a schematic diagram of stress distribution in the plate thickness direction due to bending deformation. [Figure 6] 1 is a schematic diagram of stress distribution in the plate thickness direction due to uniaxial tensile deformation. [Figure 7] This is a schematic diagram of superposition stress during bending deformation (when the shear surface side is the outside of the bend). [Figure 8] Schematic diagram of overlapping stress during bending deformation (when the fractured surface side is the outside of the bend). [Figure 9] FIG. 1 is a schematic diagram of superposition stress in uniaxial tensile deformation. [Figure 10] FIG. 2 is a diagram illustrating an example of a program configuration. [Figure 11] FIG. 13 is a diagram showing the relationship between the residual stress in the extension direction of the sheared end face and the distance from the sheared surface. [Figure 12] FIG. 13 is a diagram showing the relationship between the applied stress and the distance from the sheared surface. [Figure 13] FIG. 13 is a diagram showing the relationship between overlap stress and the distance from the sheared surface. [Figure 14] FIG. 1 is a diagram showing the relationship between the critical stress and the stress gradient τ. [Figure 15] FIG. 2 is a diagram showing a press-molded product shape defined in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Next, an embodiment based on the present invention will be described with reference to the drawings. (Delayed fracture property evaluation method) This embodiment is a method for evaluating a metal sheet for press forming used in press working. Specifically, this is a delayed fracture property evaluation method for evaluating the delayed fracture property of a sheared end surface of the metal sheet. This embodiment is particularly effective when the metal sheet is a high-strength steel sheet. In this embodiment, the delayed fracture property evaluation process for the metal plate to be evaluated includes a test step for performing an actual test and an evaluation step. Specifically, the delayed fracture property evaluation method of this embodiment includes a first step S10, a second step S20, a third step S30, a fourth step S40, and a fifth step S50, as shown in Fig. 1. The first step S10 to the fourth step S40 correspond to the test step. The fifth step S50 corresponds to the evaluation step.

[0014] <First step S10> The first step S10 is a step of shearing a metal plate to be evaluated under set shearing conditions, thereby producing a test piece having a sheared end surface to be evaluated. The shearing conditions are processing conditions during shearing, such as the value of the clearance between the upper blade and the lower blade.

[0015] FIG. 2 is a schematic diagram of shearing. As shown in FIG. 2, in shearing, first, the metal sheet 1 is clamped between the lower blade 2 on the side that is not to be punched and the sheet holder 3. This restrains the metal sheet 1. In this restrained state, the upper blade 4 is moved vertically relative to the sheet. This applies shear deformation to the metal sheet 1. When the metal sheet 1 is sufficiently deformed by this shear deformation, cracks are generated in the metal sheet 1 at the position where the tip 4a of the upper blade 4 and the tip 2a of the lower blade 2 come into contact. The cracks then meet and the metal sheet is separated. As a result, the shearing is completed. The direction of movement of the upper blade 4 is the shear direction. The symbol CR indicates clearance.

[0016] Figure 3 is a schematic diagram of the shape of the sheared edge on the remaining side. Figure 4 shows the residual stress distribution in the elongation direction at a typical sheared edge in the plate thickness direction. Here, the region indicated by the sheared edge is the region within a depth of 1 mm from the edge surface created by shearing. This sheared edge region is the region where strain and residual stress due to shear exist. This sheared edge has two regions in the thickness direction on the remaining side: a sheared surface region and a fractured surface region. The sheared surface side is the side that is scraped by the upper blade to become a smooth edge. The fractured surface side is the side that is separated by the crack propagation from the tips of the upper and lower blades to become a relatively rough edge.

[0017] Usually, the fractured surface side where the crack has propagated has a higher residual stress than the sheared surface side. As shown in Figure 4, there is a point where the cracks from the tips of the upper and lower blades meet. This point is, for example, located about 1 / 4 of the plate thickness from the lower blade side on the fractured surface side. This point is also the point where the material is finally separated. For this reason, this point undergoes the strongest plastic deformation, and the highest tensile stress remains at this point (see Figure 4). As described above, in the first step S10, a plurality of test pieces having the same sheared surface are prepared by shearing under the same shear processing conditions.

[0018] <Second step S20> The second step S20 is a method of applying an external load to the shear end face of the test piece. That is, the second step S20 is a step of selecting a load application condition. In this example, each load application condition is a load application method that results in the same or similar stress distribution in the thickness direction of the shear end face. The methods of applying load to the sheared end face include, for example, bending deformation, uniaxial tension deformation, and tension bending deformation, which is a combination of bending and uniaxial tension elements. Note that the stress distribution in the plate thickness direction also differs depending on the direction of bending deformation.

[0019] In this example, the basic loading conditions are selected from the following three types of deformation: the first deformation, the second bending deformation, and uniaxial tensile deformation. The first bending deformation is a deformation in which the plate is bent so that a peak (tensile side) is formed on the shear surface side. The second bending deformation is a deformation in which the plate is bent so that a peak (tensile side) is formed on the fracture surface side. As described below, under all of these loading conditions, the stress distribution in the plate thickness direction is one in which the stress changes linearly along the plate thickness direction (see Figures 5 and 6).

[0020] <Third step S30> The third step S30 is a step of applying a preset external load stress to the shear end surface of the test piece under the load application condition selected in the second step S20, and restraining the test piece in that loaded state. When the first bending deformation or the second bending deformation is selected as the load condition, for example, a method of applying stress to a test piece having a shear end surface by four-point bending can be exemplified. When the tensile stress application by uniaxial tension is selected as the load condition, a method of grabbing both ends of the test piece with a chuck and applying tensile deformation can be exemplified. However, the bending deformation or uniaxial tensile deformation can be applied by a conventionally known method.

[0021] It is desirable to adjust the stress by checking the value of the applied stress, for example, by using a strain gauge attached to the test piece in advance. In addition, a plurality of test pieces are prepared in which the applied stress is changed in sufficiently small intervals, for example, in increments of 100 MPa. In other words, a plurality of test pieces with different applied stresses are prepared.

[0022] <Fourth step S40> In the third step S30, an external load stress is applied to each test piece and the test piece is restrained in that state. In the fourth step S40, each test piece in the restrained state is placed in a predetermined hydrogen penetration environment for a predetermined time, and the test piece in that state is evaluated for crack occurrence in the fourth step S40. In this case, the hydrogen penetration environment and installation time are preferably set to conditions that obtain an amount of hydrogen penetration equivalent to the amount of hydrogen that is estimated to penetrate in the environment in which the material to be evaluated is actually used.

[0023] The test specimen is placed in a hydrogen penetration environment by immersing it in a bathtub containing an acid such as hydrochloric acid or an aqueous solution of NHSCN. The concentration of the acid and the immersion time are set so that the amount of hydrogen that is preset as the allowable upper limit penetrates into the test specimen. The maximum applied stress that does not cause cracks of a predetermined magnitude or more is defined as the critical stress according to the stress distribution in the plate thickness direction that corresponds to the heavy load condition. Then, for the test piece prepared in the first step S10, the load application conditions selected in the second step S20 are changed, and the processing of the third and fourth steps S30 and S40 is executed. The above tests allow us to determine the critical stress corresponding to the stress distribution in the thickness direction for each load condition. The critical stress is the limit value of the applied stress at which delayed fracture does not occur. Each critical stress can be used as a judgment value to evaluate the limit of the applied stress at which delayed fracture does not occur for each stress distribution in the thickness direction applied to the shear end face.

[0024] <Fifth step S50> In the fifth step S50, a plurality of combination data are obtained. The combination data includes a stress distribution in the plate thickness direction corresponding to a load application condition and a limit value of the applied stress corresponding to the stress distribution. The stress distribution in the thickness direction may be converted into a function, for example, or may be expressed in terms of a corresponding load condition. In this embodiment, the stress distribution in the plate thickness direction corresponding to each load condition is converted into an index value representing the stress distribution in the plate thickness direction, for example, by a preset function. In this embodiment, the index value is expressed, for example, by a stress gradient τ that represents the gradient of the corresponding stress distribution in the plate thickness direction.

[0025] The stress gradient τ is calculated, for example, by the following formula (1). Here, the stress on the fractured surface side is σf, and the stress on the sheared surface side is σb. The stress gradient τ expressed by formula (1) is a non-dimensional value. The stress gradient τ is calculated using the stress distribution when the limit stress is applied. τ =(σf-σb) / |MAX(σf, σb)| ···(1)

[0026] The stress distribution can be calculated, for example, as follows. The first method is to measure the residual stress distribution due to shear in the plate thickness direction by X-ray residual stress measurement. The second method is to calculate the stress distribution from the results of CAE analysis under the target load condition where the limit stress is applied. The stress gradient τ, which is the gradient of the distribution, may be calculated simply by the following formula (2). τ = σf / σb (2)

[0027] Then, in the fifth step S50, information on the correlation between the index value and the corresponding limit value of the applied stress is obtained by referring to a plurality of combination data. The combination data consists of data on (index value, limit stress). The correlation information may be calculated by a known calculation method. For example, the correlation information may be a multiple regression model or a model formula based on machine learning. A plurality of combination data may be used as the correlation information. The correlation information may be expressed, for example, by a function or a table. In this way, by obtaining correlation information in advance, it becomes possible to predict whether or not delayed fracture will occur at the sheared end face when a metal sheet for press forming is press-formed into an actual press-formed product shape or a planned press-formed product shape.

[0028] For example, consider a case where a target press-formed product is manufactured by press-forming a metal plate for press forming. The stress distribution in the plate thickness direction at the shear end surface of the press-formed product and the residual stress due to forming are evaluated with reference to the correlation information obtained above. Here, the stress distribution in the plate thickness direction and the residual stress due to forming can be calculated by forming analysis using normal CAE. The stress distribution in the plate thickness direction obtained by the analysis is converted into, for example, an index value. Then, by referring to previously obtained correlation information, it is determined whether the residual stress due to forming exceeds the limit stress at the obtained index value. Based on this determination, it is evaluated whether delayed fracture will occur at the shear end surface.

[0029] The evaluation points may be selected from multiple representative points on the sheared end face. Also, for example, the load conditions that impart external stress to each part of the sheared end surface in press forming and the residual stress due to forming are obtained.Then, the limit stress under the conditions that are close to the stress distribution in the plate thickness direction that approximates the obtained load conditions is set as the judgment value.Then, based on the judgment value, it may be possible to evaluate whether or not delayed fracture will occur at that part. In addition, in actual press forming, the load conditions on the shear end face may be simple bending and uniaxial tension, as well as a composite load condition in which these are superimposed. For the composite load condition, combined data consisting of the stress distribution in the plate thickness direction and the limit stress may be obtained.

[0030] In this case, for the combined load condition, the limit stress may be obtained by carrying out the above-mentioned test. Alternatively, the limit stress may be obtained as follows. That is, the pressure distributions at each limit stress under the combined load conditions are combined. Then, the stress at the position where the stress is maximum in the plate thickness direction when combined is regarded as the limit stress corresponding to the combined load condition in the plate thickness direction.

[0031] Also, the above steps may be performed by changing the shear processing conditions, and the critical stress corresponding to the stress distribution in the plate thickness direction may be obtained for each shear processing condition. Then, first, the critical stress and correlation information corresponding to the stress distribution in the plate thickness direction, which corresponds to the shear processing conditions used for the metal plate to be used, is determined. Then, using that information, it is possible to evaluate whether or not delayed fracture occurs at the sheared end surface. However, in the manufacture of mass-produced products, shear processing is often performed under the same shear processing conditions. Therefore, there is no problem if only information under those shear processing conditions is available.

[0032] (About the action and other matters) Figures 5 and 6 are examples of stress distribution in the thickness direction caused by applied stress, which is assumed when stress is applied to the sheared end face. That is, Figures 5 and 6 are examples of typical stress distribution in the thickness direction caused by the external load in the sheared end face extension direction. When the load condition is stress loading due to bending deformation, a linearly changing stress is applied from tension to compression from one plate thickness surface to the other plate thickness surface. Therefore, when stress is loaded due to bending deformation, the stress is distributed in the plate thickness direction as shown in Figure 5. Depending on the direction of bending deformation, both the shear surface side and the fracture surface side are expected to be the sides where the stress becomes tensile. The side where the stress becomes tensile is the side that becomes convex due to bending.

[0033] In addition, when the load condition is stress loading due to uniaxial tensile deformation, tensile stress is applied uniformly throughout the entire plate thickness. Therefore, when stress loading due to uniaxial tensile deformation is applied, the stress distribution in the plate thickness direction is as shown in Figure 6. In addition, a load condition that combines elements of bending and uniaxial tension, such as tension bending, is also assumed. When stress is applied to the sheared end face, the stress distribution in the plate thickness direction of the sheared end face is expected to be a combination of the distribution of residual stress due to the shear described above and the distribution of stress load due to applied stress.

[0034] Figures 7 to 9 are schematic diagrams in which stress load distributions under various load conditions are superimposed on the residual stress distribution of the sheared end face shown in Figure 4. Figure 7 is a schematic diagram when a load load condition of bending deformation outside bending is selected on the sheared end face side. Figure 8 is a schematic diagram when a load load condition of bending deformation outside bending is selected on the fractured surface side. Figure 9 is a schematic diagram when a load load condition of uniaxial tensile deformation is selected. As shown in these schematic diagrams (see Figs. 7 to 9), even if the maximum value of the external load stress applied to the sheared end face in the plate thickness is the same, the superimposed stress is different. In other words, the total maximum tensile stress of the sheared end face is different. The total value is the sum of the external load stress and the residual stress of the sheared end face due to shear processing.

[0035] Specifically, the relationship of the maximum tensile stress at the shear end surface as a total is as follows: Uniaxial tension > Bending (tension on fracture surface side) > Bending (tension on shear surface side) In addition, in the case of tensile bending, a combination of uniaxial tension and bending is used, so it is expected that the maximum tensile stress will be intermediate between the two. In addition, if a specimen is placed in a hydrogen intrusion environment with a stress load applied to the sheared edge, cracks may occur as the amount of hydrogen increases, leading to delayed fracture. It is known that this delayed fracture is more likely to occur when the stress at the sheared edge is high.

[0036] From the above, it is considered that there is a limit stress at the sheared end surface at which delayed fracture occurs. Here, it is assumed that delayed fracture occurs when the maximum value of the sum of the overlapping distributions of the shear residual stress and the load stress at the sheared end surface reaches the limit stress. If we make this assumption, the maximum possible stress load within the range in which delayed fracture does not occur has the following relationship depending on the load conditions. Hereinafter, the maximum possible stress load within the range in which delayed fracture does not occur will be referred to simply as the limit stress. Uniaxial tension < bending (tension on fracture surface side) < bending (tension on shear surface side) In addition, in the case of tensile bending, since it is a combination of uniaxial tension and bending, it is expected to be in an intermediate state between the two.

[0037] From the above, by determining the limit stress for each stress distribution in the plate thickness direction, the delayed fracture characteristics of the sheared end surface of a metal plate for press forming can be evaluated. The limit stress is the limit value of the applied stress at which delayed fracture does not occur. For example, the limit stress corresponding to the stress distribution in the plate thickness direction corresponding to the load application conditions is determined for each of a plurality of stress distributions in the plate thickness direction. Then, it is evaluated whether delayed fracture does not occur at a representative position of the sheared end surface when the metal plate for press forming is press formed.

[0038] Here, a simple evaluation method is to design the stress applied to the shear end surface of the press-formed product within a range where the load conditions do not exceed the limit stress of uniaxial tension. However, this does not take into account the stress load due to bending. Therefore, there is a problem that this evaluation is overly strict. From these findings, the inventors have come to the following findings in order to realize a more excellent delayed fracture evaluation of the sheared edge.

[0039] (1) The maximum applied stress (threshold stress) at the delayed fracture limit varies depending on the distribution of shear residual stress at the shear end. Furthermore, the maximum applied stress (threshold stress) at the delayed fracture limit varies depending on the distribution of stress load in the plate thickness. Therefore, it is necessary to apply multiple loads that give different stress distributions in the plate thickness direction, and evaluate each threshold stress according to the different stress distributions.

[0040] (2) In addition, in actual press forming, the load conditions on the shear end face are assumed to be not only simple bending and uniaxial tension, but also superimposed composite load conditions. The evaluation accuracy can be improved by determining the limit stress according to the stress distribution corresponding to the composite load conditions.

[0041] (3) The stress distribution in the plate thickness direction is converted into an index value. In this case, the correlation between the stress distribution in the plate thickness direction and the limit stress can be expressed mathematically. In this case, the correlation information can be expressed more simply. As a result, delayed fracture evaluation at the shear end surface after press forming can be performed more simply.

[0042] (4) When the loading condition is stress loading by uniaxial tension, the delayed fracture critical stress is expected to be the lowest. When the loading condition is stress loading by bending, the delayed fracture critical stress is expected to be lower when tensile stress is applied to the fracture surface side where the shear residual stress is relatively high. Therefore, based on the corresponding stress distribution in the plate thickness direction, the index value can be set as a value that represents the gradient of the stress in the plate thickness direction.

[0043] For example, the stress on the fractured surface side is σf, and the stress on the sheared surface side is σb. In this case, the stress gradient τ as an index value can be defined as equation (1) or a similar equation. (σf-σb) / |MAX(σf, σb)| ···(1) In this case, by changing the critical stress as a function of the stress gradient τ as a variable, it becomes possible to accurately express the critical stress for delayed fracture.

[0044] The above-mentioned delayed fracture evaluation method can use analytical information of press-formed products calculated by CAE to evaluate the occurrence of delayed fracture. For example, from the press forming analysis by CAE, the stress distribution σ(t) in the plate thickness direction of the sheared end surface corresponding to the position t in the plate thickness direction at each point of the sheared end surface is obtained. The obtained stress distribution σ(t) can be used to evaluate the occurrence of delayed fracture. In addition, the stress distribution σ(t) in the thickness direction of the shear end surface is expressed as an index value. As a result, the determination of the limit stress becomes more generalized, and delayed fracture properties can be evaluated more simply. Here, the stress gradient τ as an example of the index value is not limited to the above formula (1). For example, (σf / σb) may be used as the stress gradient τ expressing the gradient of stress in the plate thickness direction.

[0045] In addition, the load conditions themselves may be used as an index expressing the stress distribution σ(t) in the thickness direction of the sheared end face. Then, the presence or absence of delayed fracture may be evaluated based on the limit stress under load conditions that are close to the load conditions applied by press forming to the location of the sheared end face to be evaluated. For example, the stress distribution in the thickness direction due to external stress load (press forming) at the location to be evaluated is obtained by CAE analysis. Then, the load conditions that are close to this stress distribution are identified. After that, it may be evaluated whether delayed fracture will occur based on whether the limit stress under the identified load conditions is exceeded. However, it is easier to evaluate the stress distribution σ(t) in the plate thickness direction at the shear end surface by expressing it as an index value.

[0046] (Method of manufacturing press-molded products) A metal plate for press forming having a sheared end surface is press-formed to produce a target press-formed product. At this time, for the metal sheet for press forming to be used, the correlation between the index value and the critical stress is previously obtained based on the above-mentioned method for evaluating delayed fracture properties of metal sheet for press forming. Then, a computer is used to perform CAE analysis to press-form the metal plate for press forming into a press-formed product. Then, based on the analysis results, the stress distribution in the plate thickness direction at each point on the shear end surface and the correlation, the presence or absence of delayed fracture of the press-formed product is evaluated. If it is evaluated that delayed fracture has occurred, the press-formed shape of the press-formed product is changed, or the material or plate thickness of the metal plate used is changed. Then, an evaluation of delayed fracture is performed again. This is repeated until it is evaluated that delayed fracture will not occur. This makes it possible to manufacture press-formed products that are free from delayed fracture.

[0047] (program) An example of a program used in the above-mentioned delayed fracture property evaluation method will be described below. As shown in Fig. 10, the program is stored in a storage unit 40 such as a RAM or ROM of a computer. The program is executed by the computer. The program of this example obtains in advance information 40A on the correlation between the index value and the critical stress, and stores it in the memory unit 40. The index value is an index value that expresses the stress distribution in the plate thickness direction caused by applying an external load to a metal plate. The critical stress is the critical stress under the load application conditions that result in the stress distribution in the plate thickness direction. The correlation information 40A may be obtained in advance by processing the evaluation method for delayed fracture properties as described above. For example, the index value is calculated using equation (1).

[0048] The program of this example inputs information on stress distribution and outputs a critical stress, which is the limit value of the applied stress at which delayed fracture does not occur. The input information on the stress distribution is obtained by executing a CAE analysis for forming a metal plate into a target press-formed product shape, and substituting the value obtained by the analysis into a formula for obtaining an index value. Reference numeral 20 in Fig. 10 denotes a CAE analysis unit. The program 30 of this example is executed as follows: First, in an index value calculation step 30A, an index value to be evaluated is calculated by substituting the stress values ​​at both ends in the plate thickness direction into formula (1) based on the inputted stress distribution information.

[0049] Next, in a limit stress calculation step 30B, the limit stress corresponding to the calculated index value is found by referring to the correlation information 40A. Then, the program 30 of this embodiment outputs the determined value of the critical stress. Here, when the stress value occurring at the evaluation point is input to the program together with the stress distribution information, the program may be configured to compare the determined critical stress with the input stress value and output information on whether or not delayed fracture will occur.

[0050] (others) The present disclosure may also have the following configuration. (1) Disclosure 1 is a method for evaluating delayed fracture properties of a shear end surface of a metal plate for press forming used in press working, comprising: A plurality of test pieces having the above-mentioned sheared end surface are prepared by shearing the target metal plate under the same shearing conditions; The test is carried out under multiple load conditions that result in the same or similar stress distribution in the thickness direction on the shear end surface of the test piece, and The above test is performed under a plurality of load conditions with different stress distributions in the plate thickness direction, Based on the above tests for each load condition, the critical stress, which is the limit value of the applied stress at which delayed fracture does not occur, is determined according to the stress distribution in the plate thickness direction. A method for evaluating the delayed fracture properties of metal sheets for press forming. (2) Disclosure 2 states that in the above test, a test piece to which stress is applied is placed in a hydrogen penetration environment, and the upper limit of the applied stress at which delayed fracture does not occur in the hydrogen penetration environment is defined as the critical stress. (3) Disclosure 3 states that the multiple load conditions include a load applied by bending convexly in the shear direction, a load applied by bending concavely in the shear direction, and a stress applied by uniaxial tension. (4) Disclosure 4 has a composite load condition in which two or more load conditions having different stress distributions in the plate thickness direction are superimposed, Furthermore, a critical stress corresponding to the stress distribution in the plate thickness direction corresponding to the above-mentioned combined load conditions is obtained. (5) In disclosure 5, the metal plate for press molding is made of a high-strength steel plate. (6) Disclosure 6 converts the stress distribution in the plate thickness direction into an index value expressing the distribution state of the stress distribution, A correlation between the index value and the limit stress is obtained from a plurality of data sets each consisting of the index value and the limit stress. (7) In Disclosure 7, the index value is a value that expresses the gradient of the stress distribution in the plate thickness direction. (8) In Disclosure 8, when the stress on the fractured surface side surface of the plate in the stress distribution is σf and the stress on the sheared surface side surface of the plate is σb, the index value τ is expressed by the following equation (1). τ =(σf-σb) / |MAX(σf, σb)| ···(1) (9) Disclosure 9 is a method for manufacturing a press-molded product by press-molding a metal plate for press molding having a sheared end surface to manufacture a press-molded product, For a target metal sheet, a correlation between the index value and the critical stress is previously obtained based on the method for evaluating delayed fracture properties of a metal sheet for press forming according to the present disclosure; A CAE analysis is performed using a computer to press-form the metal plate for press forming into a press-formed product. Based on the analysis results, the stress distribution in the plate thickness direction at each point on the shear end surface and the correlation are used to evaluate whether or not delayed fracture occurs in the press-formed product. The evaluation is performed by converting the stress distribution in the plate thickness direction at each point of the shear end surface into an index value. A manufacturing method for press-molded products. (10) Disclosure 10 relates to a method for evaluating delayed fracture properties of a metal sheet for press forming according to the present disclosure, and information on the correlation between the index value and the critical stress is stored in a storage unit; A step of calculating the index value from the input information on stress distribution in the plate thickness direction; determining a critical stress, which is a limit value of a load stress at which delayed fracture does not occur, based on the correlation information and the calculated index value; A program for causing a computer to execute the following. EXAMPLES

[0051] Next, examples based on this embodiment will be described. In this example, a test material A, which is a steel having a tensile strength of 1470 MPa and a plate thickness of 1.4 mm, will be described as a metal plate for press forming. However, the present invention is not limited to the test material A. The present invention can be suitably applied to metal materials such as ultra-high tensile steel having a tensile strength of 980 MPa or more, which may cause delayed fracture at the shear end surface. In this example, the clearance during shearing was set to 12% of the plate thickness as a shearing condition. Then, the specimen A was sheared under the shearing conditions to prepare a test piece. The test piece had a linear sheared end surface with a length of 500 mm.

[0052] Figure 11 shows the calculated stress distribution by X-ray in the thickness direction parallel to the sheared end surface of the test piece. Figure 11 also shows the calculated stress distribution by FEM analysis of shear processing by CAE on the sheared end surface of the test piece. As can be seen from Figure 11, the X-ray stress measurement and CAE analysis results showed the same tendency. It was also found that the residual stress on the fractured surface side of the sheared edge was generally higher than that on the sheared surface side. In particular, the maximum tensile residual stress was found at the 1 / 4 plate thickness position on the fractured surface side. Next, stress was applied to the shear end surface of the test piece by bending load by four-point bending. In addition, stress was applied by uniaxial tension by gripping and pulling the rectangular test piece with a chuck. In other words, the load conditions were exemplified as bending deformation and uniaxial tension deformation. Then, external stress was applied to each of the multiple test pieces for each load condition.

[0053] The applied stress was adjusted as follows. A strain gauge was attached near the shear end surface to measure the strain. The measured strain was multiplied by the Young's modulus of 205 GPa to measure the maximum applied stress within the plate thickness under each condition. The external stress applied to each test piece was adjusted with reference to the measurement. The applied stress was then added in increments of 100 MPa, and multiple test pieces with different applied stresses were created for each load condition. However, for the stress applied by bending load due to four-point bending, the following two types of test pieces were prepared. In other words, test pieces with an external load applied were prepared under two load conditions: one in which the shear surface side was tensile (convex) and the other in which the fracture surface side was tensile (convex). Tension (convex) refers to bending deformation such that the tensile side is convex. A schematic diagram of the estimated load stress distribution in the plate thickness under each load condition is shown in Fig. 12. The example shown in Fig. 12 is an example when the maximum load stress is 1000 MPa.

[0054] Next, each test piece in the stressed state was immersed in a hydrochloric acid bath with a constant pH of 2.5 for 100 hours. The presence or absence of cracks penetrating the plate thickness direction at the end of the immersion was determined. This determination was used to investigate the occurrence of delayed fracture. The maximum external stress at which no cracks were generated, i.e., no delayed fracture occurred, was defined as the critical stress. The critical stresses determined for each load condition are shown in Table 1.

[0055] [Table 1]

[0056] As can be seen from Table 1, the limit stress is lowest in uniaxial tension. Next, the limit stress is high in bending (tensile on fracture surface side), and the highest is bending (tensile on shear surface side). Bending (tensile on fracture surface side) refers to the case where the fracture surface side is under tension due to bending deformation. Bending (tensile on shear surface side) refers to the case where the shear surface side is under tension due to bending deformation.

[0057] Figure 13 shows the load stress distributions for uniaxial tension, bending (tensile on the fracture surface side), and bending (tensile on the shear surface side) at each limit stress, added together with the distributions of the X-ray stress measurements shown in Figure 5. The limit stress as the maximum load stress within the plate thickness under each load condition is different. However, as shown in Figure 13, when added together with the shear residual stress, the following relationship was obtained. That is, bending (tensile on the fracture surface side) was 1632 MPa at the outermost surface of the fracture surface side. Bending (tensile on the shear surface side) was 1665 MPa at the outermost surface of the shear surface side. Uniaxial tension was 1613 MPa on the shear surface side. That is, in each case, the maximum stress was almost the same locally.

[0058] This indicates that the following exists due to the distribution of residual stress due to shear within the plate thickness. In other words, it indicates that there are different maximum stresses for the delayed fracture limit load depending on the stress distribution σ(t). The stress distribution σ(t) is the stress distribution in the plate thickness direction of the shear end face depending on the position t in the plate thickness direction at the stress load on the shear end face. It also indicates that this evaluation is possible with the above test. A simple way to consider it would be to design the stress loaded on the shear end face of a press-formed product so that it does not exceed the delayed fracture limit stress in uniaxial tension. However, this does not take into account the stress load due to bending. For this reason, there is a problem that it is overly strict.

[0059] The critical stress for delayed fracture is lowest under uniaxial tension. Even under the same bending load, the critical stress is different between sheared surface side tension and fractured surface side tension. Therefore, it is necessary to distinguish between sheared surface side tension and fractured surface side tension. In this example, the stress gradient τ defined in (1) above is used as an index value. In this case, by changing the critical stress σlim as a function of the stress gradient τ, it is possible to accurately express the critical stress according to the stress distribution in the plate thickness direction.

[0060] Figure 8 plots three pieces of information, the stress gradient τ and the limit stresses for uniaxial tension, bending (tensile on the shear surface side), and bending (tensile on the fracture surface side), from the results in Table 1. Figure 8 also shows the linear interpolation of the states between the plots, which correspond to the tensile bending state. According to this method, the limit stress σlim is expressed by the following equation: σlim = - 550 ×τ + 400(τ≦0) σlim = 200×τ + 400 (τ>0) By using the above formula, it is possible to more accurately express the dependency of the critical stress on the applied stress distribution. Note that a separate test may be conducted on the tensile bending state and the results may be plotted in Figure 14.

[0061] 15 is a schematic diagram of a press-formed product having a sheared end surface in this example. Table 2 shows the evaluation results when the press-formed product shown in FIG. Table 2 shows the maximum load stress within the plate thickness as the residual stress from press forming at an example location of the shear end surface based on CAE analysis, the stress gradient τ, the limit stress depending on τ, and the delayed fracture test results.

[0062] [Table 2]

[0063] As can be seen from Table 2, it was found that for press-formed products having a sheared end surface, delayed fracture can be accurately predicted by evaluating the delayed fracture according to the stress distribution within the plate thickness. Furthermore, Table 3 shows the results when measures were taken to reduce stress at points C, E, and F where delayed fracture occurred.

[0064] [Table 3]

[0065] As can be seen from Table 3, delayed fracture was suppressed by reducing the stress at the position where delayed fracture occurs with reference to the critical stress using the stress gradient τ as an index. In this way, it became possible to manufacture press-formed products with sheared edges that have excellent resistance to delayed fracture.

[0066] The entire contents of Japanese Patent Application No. 2023-121673 (filed on July 26, 2023), from which this application claims priority, are incorporated herein by reference. Although the present invention has been described with reference to a limited number of embodiments, the scope of the invention is not limited thereto, and modifications of each embodiment based on the above disclosure would be obvious to one skilled in the art. [Explanation of symbols]

[0067] 1 metal plate 2 Lower blade 2a tip 4 Upper blade 4a tip 30 Programs 30A Index value calculation steps 30B Limit stress calculation step 40 Storage section 40A Correlation Information S10 First step S20 Second process S30 Third process S40 Fourth step S50 5th step τ Stress gradient (index value)

Claims

1. A method for evaluating delayed fracture properties of a sheared end surface of a metal plate for press forming used in press working, comprising: A plurality of test pieces having the above-mentioned sheared end surface are prepared by shearing the target metal plate under the same shearing conditions; A test is performed in which stress is applied to the shear end surface of the test piece under load conditions that result in the same or similar stress distribution in the thickness direction, and a plurality of load stresses are applied under the same or similar load conditions; The above test is carried out for each of a plurality of load conditions in which the stress distribution in the plate thickness direction is different from each other, Based on the above tests for each load condition, the critical stress, which is the limit value of the applied stress at which delayed fracture does not occur, according to the stress distribution in the plate thickness direction, is determined. The plurality of loading conditions include two or more loading conditions selected from a load applied by bending convex in the shear direction, a load applied by bending concave in the shear direction, and a stress applied by uniaxial tension. A method for evaluating the delayed fracture properties of metal sheets for press forming.

2. In the above test, a test piece to which stress is applied is placed in a hydrogen penetration environment, and the upper limit of the applied stress at which delayed fracture does not occur in the hydrogen penetration environment is defined as the critical stress. A method for evaluating delayed fracture properties of a metal sheet for press forming according to claim 1.

3. The stress distribution in the plate thickness direction is different from that in the plate thickness direction. Furthermore, a critical stress corresponding to the stress distribution in the plate thickness direction corresponding to the above-mentioned combined load conditions is obtained. A method for evaluating delayed fracture properties of a metal sheet for press forming according to claim 1.

4. The metal plate for press molding is made of a high-strength steel plate. A method for evaluating delayed fracture properties of a metal sheet for press forming according to claim 1.

5. The stress distribution in the plate thickness direction is converted into an index value expressing a distribution state of the stress distribution, determining a correlation between the index value and the limit stress from a plurality of data sets each including the index value and the limit stress; A method for evaluating delayed fracture properties of a metal sheet for press forming according to claim 1.

6. The index value is a value representing the stress of the stress distribution in the plate thickness direction. A method for evaluating delayed fracture properties of a metal sheet for press forming according to claim 5.

7. In the stress distribution, when the stress on the fractured surface side surface of the plate is σf and the stress on the sheared surface side surface of the plate is σb, the index value τ is expressed by the following formula (1): A method for evaluating delayed fracture properties of a metal sheet for press forming according to claim 6. τ = (σf-σb) / |MAX(σf, σb)| ...(1)

8. A method for producing a press-molded product by press-molding a metal plate for press molding having a sheared end surface, comprising: For a target metal sheet, a correlation between the index value and the critical stress is previously obtained based on the method for evaluating delayed fracture properties of a metal sheet for press forming according to any one of claims 5 to 7, A CAE analysis is performed using a computer to press-form the metal plate for press forming into a press-formed product; Based on the analysis results, the stress distribution in the plate thickness direction at each point on the shear end surface and the correlation are used to evaluate whether or not delayed fracture occurs in the press-formed product. The above evaluation is performed by converting the stress distribution in the plate thickness direction at each point of the shear end surface into an index value. A manufacturing method for press-molded products.

9. Information on the correlation between the index value and the critical stress obtained based on the method for evaluating delayed fracture properties of a metal sheet for press molding according to any one of claims 5 to 7 is stored in a storage unit, Calculating the index value from the input information on stress distribution in the plate thickness direction; determining a critical stress, which is a critical value of a load stress at which delayed fracture does not occur, based on the correlation information and the calculated index value; A program for causing a computer to execute the following.

Citation Information

Patent Citations

  • Method for evaluating delayed fracture characteristics of metal plate, and method for manufacturing press component

    JP2022024814A

  • Jig for assessing delayed fracture, method for assessing delayed fracture in sheared end surface, and test piece

    JP2023072460A

  • Method for evaluating deformation limit, crack prediction method, and method for designing press die

    WO2019064922A1

  • Test piece and method for delayed fracture characteristic evaluation of ultra-high strength surface treated steel plate

    JP2014070927A

  • Evaluation method of hydrogen embrittlement characteristic of steel material

    JP2016057163A