Transfer foil
By adding a plasticizer to the resin-based protective layer, the transfer foil addresses issues of cracking and blistering during heat-pressure transfer, ensuring the foil's flexibility and maintaining the metal layer's brightness and adhesion.
Patent Information
- Application Number
- JP2023211101
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-12-14
AI Technical Summary
Existing transfer foils suffer from issues such as cracks, breaks, and blisters during and after heat-pressure transfer due to differences in expansion, contraction, and stress between resin and metal layers, leading to reduced brightness and glossiness of the metal vapor deposited layer.
Incorporation of a plasticizer into the resin-based protective layer of the transfer foil to enhance flexibility and synchronization with the transfer process, preventing cracks and blisters by allowing the layers to stretch in unison.
The use of a plasticizer in the resin-based protective layer improves the transfer foil's flexibility, preventing cracks and blisters, maintaining the brightness and glossiness of the metal layer, and enhancing the durability and adhesion of the transfer layer.
Smart Images

Figure 0007563800000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a transfer foil, and more particularly to a transfer foil including a modification laminate consisting of a transfer laminate. [Background technology]
[0002] The transfer foil as a surface modification of a resin-based molded product formed by a thermal pressure transfer method or the like includes a protective layer, a peeling layer, a resin-based protective layer or a colored resin-based protective layer, a metal deposition layer, a resin-based protective layer, and an adhesive layer, which are formed in this order on a substrate film. Each layer is formed selectively, and the resin-based protective layer, the colored resin-based protective layer, and the like are formed by applying them together in layers. According to the thermal pressure transfer method, a film with a transfer lamination is placed on the transferee with the adhesive layer facing, and pressure and heat are applied from above the substrate film by a thermal pressure transfer device, the transfer lamination is transferred, and then the substrate film is peeled off. As a result, the surface of the transferee is transferred by the transfer lamination (modification lamination), and the transferee becomes a modified product decorated by the transfer lamination.
[0003] In the case of resin-based molded products, one method for surface modification is to prepare a transfer foil having a transfer lamination by overlaying a release layer, a resin-based protective layer, a metal vapor deposition layer, and an adhesive layer on a base film, and then to modify the surface of various transfer objects, including resin-based molded products, by heat and pressure transfer means.
[0004] Using a transfer foil having the above-mentioned laminate on a base film, the adhesive layer is placed on the surface layer of a resin-based molded product or other object to be transferred, and the transfer is performed from the base film side using a transfer machine. A rubber-based roll plate, a metal-based flat plate 30, a letterpress 40, or other image-forming heat medium is selected, and a transfer laminate consisting of a release layer, a resin-based protective layer, a metal-deposited layer, and an adhesive layer is transferred onto a resin-based molded product or other object, or onto metals, glass, wood, fibers, paper, or rubber, by pressurizing and heating, and then the base film is removed. This allows the transfer of the surface onto the object to be transferred, such as a resin-based molded product, and the surface of the material to be modified.
[0005] Japanese Patent Application Laid-Open No. 56-53086 (Patent Document 1) discloses a transfer foil for protecting a transferee in transfer painting. This transfer foil includes a release layer formed on a base sheet, a first protective layer formed on the release layer, a second protective layer formed on the first protective layer, a colored layer formed on the second protective layer, and an adhesive layer formed on the colored layer. The colored layer contains a thermoplastic acrylic resin, a synthetic rubber, and a vinyl chloride resin. The first and second protective layers, which are curable, and the colored layer and adhesive layer, which are plastic, are continuously layered. When the transferee and the transfer foil are stretched or contracted at the interface between the second protective layer and the colored layer during transfer or over time, the elasticity of each layer is taken into consideration as a transfer load at the interface between the curable film of the protective layer and the plastic film of the colored layer, and the layer constituting the protective film is set as a curable film against the reversible elasticity and contraction of the synthetic rubber put into the colored layer. Regarding the ability of the curable film of the protective layer to follow the shrinkage of the colored layer, there remains a problem in avoiding the influence of the shrinkage on the film, which may cause breakage.
[0006] Moreover, a general-purpose transfer foil has the following structure. Looking at an example of a transfer foil, in a transfer foil including a peeling layer, a protective layer, a color layer, a metal deposition layer, and an adhesive layer on a base film, various defects exist both during transfer and over time after transfer. Defects that occur during thermal pressure transfer include poor breaking accuracy of the transfer film, cracks, breakage, poor interlayer adhesion, and poor transfer heat resistance. Changes that occur over time after transfer include peeling, cracks, swelling, etc., which occur due to the influence of the temperature, humidity, etc. of the environment under exposure. Fading and deterioration due to light may occur.
[0007] In the case of the thermal pressure transfer method using a transfer machine, a load is generated on the base film, the peeling layer, the resin-based protective layer, the colored resin-based protective layer, the metal deposition layer, the resin-based protective layer, the adhesive layer, etc., due to heating and pressure. The difference in response occurs due to the expansion, contraction, pressure, etc. caused by the thermal pressure during the transfer lamination and transfer of the transferee. The resin-based layer is easy to expand, while the metal layer is difficult to expand. The expansion of the resin-based layer applies a tensile stress to the metal layer, and the metal layer with a high elastic modulus undergoes cohesive failure, resulting in cracks, breaks, swelling, etc. This defect impairs and attenuates the brightness of the metal deposition layer as a light reflective layer. There is a risk of impairing the glossiness that can be modified.
[0008] In terms of peeling the transfer layer from the base film, the layer through the film shows a peeling effect by making the absorbency of heat pressure sensitive and lowering the heat pressure sensitivity when heat pressure is propagated. The adhesive layer is made to function by selectively adopting a resin that is excellent in low-temperature sensitization with heat pressure. In the resin-based protective layer, the resistance of the film is increased to eliminate the physical and chemical effects of the transfer surface layer after transfer. The color-developing resin-based protective film contains a coloring agent, and forms a film configuration that shows a coloring effect and prevents fading and discoloration. The metal vapor deposition layer has a glittering effect as a film reflection of the deposited layer of the used metal, a film formed by dotting the film in a sea-island shape, and a multi-layered film. The peeling layer and adhesive layer are shifted to lower temperatures, while the protective layer, vapor deposition protective layer, and vapor deposition layer are shifted to higher temperatures. As a result, the transfer lamination, including the base film, and the transfer lamination caused by the heat pressure propagation caused by the heat pressure transfer are not uniform in expansion and contraction. This places a heavy load on the highly elastic metal vapor deposition layer, which may result in cracks, breakage, swelling, etc. in the transfer layer, which may progress to a decrease in brightness and a decrease in gloss.
[0009] If the extensibility of the metal in the metal deposition layer is low, the cohesion of the metal layer is destroyed by the extension caused to the transfer lamination that occurs in the transfer layer during transfer. As a result, cracks, breaks, and swelling appear in the transfer layer with the modified lamination. If the extensibility of the resin-based protective layer is high, the effect on the cohesion of the metal deposition layer can be mitigated, but the extension of the protective layer caused by the heating and pressure during transfer causes tensile stress to act on the metal layer, which leads to breakage and acts as a decrease in the gloss and brightness of the modified lamination. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 56-53086 [Patent Document 2] JP 2002-192895 A [Patent Document 3] JP 2016-124289 A Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide a transfer foil capable of preventing the occurrence of cracks, breakage, blistering, and the like. [Means for solving the problem]
[0012] The transfer foil according to the present invention includes a base film and a transfer laminate. The transfer laminate includes a release layer formed on the base film, a first resin-based protective layer formed on the release layer, and an adhesive layer formed on the first resin-based protective layer. The first resin-based protective layer contains a plasticizer. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view showing the structure of the transfer foil according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing the structure of the transfer foil according to the second embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing plate making by a top-bottom type transfer foil stamping machine using a planographic plate. [Figure 4] FIG. 4 is a schematic diagram showing plate making by a top-bottom type transfer foil stamping machine using a relief plate. [Diagram 5] FIG. 5 is a schematic diagram showing plate making using a roll-type heat pressure transfer machine. [Figure 6] FIG. 6 is a schematic diagram showing a gravure printing machine and a type 1 drying oven. [Figure 7] FIG. 7 is a schematic diagram showing a gravure printing machine and a type 2 drying oven. [Figure 8] FIG. 8 is a photograph showing a three-dimensional film of the transfer lamination. [Figure 9] FIG. 9 is a photograph showing a three-dimensional film of the transfer lamination. [Figure 10] FIG. 10 is a photograph showing a three-dimensional film of the transfer lamination. [Figure 11] FIG. 11 is a photograph showing cracks, breaks, and blisters that occurred in the flat film of the transfer laminate. [Figure 12] FIG. 12 is a photograph showing cracks that occurred in the three-dimensional film of the transfer object. [Figure 13] FIG. 13 is a magnified photograph showing the opening of a crack that occurred in the transfer laminate. [Figure 14] FIG. 14 is a 5000-times enlarged photograph of the enlarged photograph shown in FIG. [Figure 15] FIG. 15 is a photograph showing the transferred appearance of the transfer laminate. [Figure 16] FIG. 16 is a photograph showing a metallic transfer relief plate. [Figure 17] FIG. 17 is a photograph showing an aluminum surface on which a film was formed by vacuum deposition. [Figure 18] FIG. 18 is a photograph showing the surface of an indium film formed by vacuum deposition. [Figure 19] FIG. 19 is a graph showing the transfer residence times in Table 9. [Figure 20] FIG. 20 is a graph showing the aperture widths of the transfer stacks in Table 9. [Figure 21]FIG. 21 is a graph showing the elongation percentage of the vinyl chloride sheets in Table 9. [Figure 22] FIG. 22 is a graph combining the graphs of FIGS. [Figure 23] FIG. 23 is a photograph showing a three-dimensional film of the transfer lamination. [Figure 24] FIG. 24 is a photograph showing a three-dimensional film of the transfer lamination. [Diagram 25] FIG. 25 is a photograph showing a three-dimensional film of the transfer lamination. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] [Overview of the embodiment] A transfer foil according to an embodiment of the present invention includes a base film and a transfer laminate. The transfer laminate includes a release layer formed on the base film, a first resin-based protective layer formed on the release layer, and an adhesive layer formed on the first resin-based protective layer. The first resin-based protective layer contains a plasticizer.
[0015] According to this transfer foil, since the first resin-based protective layer contains a plasticizer, the release layer, the first resin-based protective layer, and the adhesive layer can expand in synchronization with the transfer, which makes it possible to prevent the occurrence of cracks, breakage, blistering, etc.
[0016] The transfer laminate may further include a metallic layer formed between the first resinous protective layer and the adhesive layer.
[0017] The transfer laminate may further include a second resin-based protective layer formed between the metal layer and the adhesive layer.
[0018] The transfer foil may further include a film protective layer formed between the base film and the release layer.
[0019] In this case, the second resin-based protective layer functions as a compounding agent layer that increases the resistance of the metal layer.
[0020] Examples of the plasticizer include chlorinated paraffin, butyl adipate, 2-ethylhexyl adipate, dioctyl adipate, 2-ethylhexyl azelaate, phthalate esters, dibutyl phthalate, diheptyl phthalate, di-2-ethylhexyl phthalate, diisononyl phthalate, diisodecyl phthalate, citric acid esters, esters of succinic acid and triethylene glycol monomethyl ether, esters of adipic acid and diethylene glycol monomethyl ether, tricarboxylate esters such as trioctyl trimellitate, esters of 1,3,6-hexatricarboxylic acid and butyl diglycol, tricresyl phosphate, triphenyl phosphate, tri-2-ethylhexyl phosphate, trixylenyl phosphate, triethyl phosphate, low molecular weight polyesters, epoxidized soybean oil, epoxidized linseed oil, epoxidized linseed oil, ethylene glycol monomethyl ether ... The carboxylic acid esters include at least one selected from the group consisting of epoxidized octyl stearate, epoxidized fatty butyl, epoxidized linseed oil fatty acid butyl, trimellitic acid ester, pyromellitic acid ester, sebacic acid ester, azelaic ester, maleic acid ester, benzoic acid ester, methyl adeticate, butyl oleate, oxy acid ester, dihydric alcohol ester, aliphatic dibasic acid ester, triphenyl phosphate, dinonylnaphthalene, tributyl acetyl citrate, P-toluenesulfonamide, toluenesulfonamide, toluenesulfoneethylamide, aminobenzenesulfonamide compounds, aminotoluenesulfonamide compounds, N-butylbenzenesulfonamide, N-ethyl-ortho-toluenesulfonamide, dinonylnalene, tributyl acetyl citrate, and ethylene olefin oligomers.
[0021] The plasticizer preferably includes one or more selected from the group consisting of P-toluenesulfonamide, toluenesulfonamide, toluenesulfoneethylamide, aminotoluenesulfonamide compounds, and N-ethyl-o-toluenesulfonamide.
[0022] The content of the plasticizer in the first resin-based protective layer is, for example, 0.01 to 20% by weight. The lower limit of the content is preferably 0.1% by weight, and more preferably 1% by weight. On the other hand, the upper limit of the content is preferably 10% by weight, and more preferably 5% by weight.
[0023] The first resin-based protective layer has a thickness of, for example, 1 to 20 μm.
[0024] The first resin-based protective layer may contain one or more types of acrylic resins.
[0025] The first resin-based protective layer may contain a curing agent.
[0026] The first resin-based protective layer may contain a color developer.
[0027] The color developer may contain a pigment having a particle size of 10 to 120 nm, where the particle size is the geometric mean particle size obtained by averaging the major axis diameter and the minor axis diameter.
[0028] The first resin-based protective layer may contain a light stabilizer.
[0029] The first resin-based protective layer may contain an ultraviolet absorbing agent.
[0030] [Details of the embodiment] Hereinafter, embodiments will be described in detail with reference to the accompanying drawings. In the drawings, the same or corresponding parts are denoted by the same reference characters and description thereof will not be repeated.
[0031] [Embodiment 1] 1, the transfer foil 10 according to the first embodiment includes a base film 11 and a transfer laminate (hereinafter, may be referred to as a "modified laminate") 12. The transfer laminate 12 includes a release layer 13 formed on the base film 11, a resin-based protective layer (hereinafter, may be simply referred to as a "protective layer") 14 formed on the release layer 13, a metal layer 15 formed on the resin-based protective layer 14, and an adhesive layer 16 formed on the metal layer 15. The protective layer 14 contains a plasticizer.
[0032] [Embodiment 2] As shown in Fig. 2, the transfer foil 20 according to the second embodiment includes a base film 11 and a transfer laminate 21. The transfer laminate 21 includes a film protective layer 22 formed on the base film 11, a release layer 13 formed on the film protective layer 22, a resin-based protective layer 14 formed on the release layer 13, a metal layer 15 formed on the resin-based protective layer 14, a resin-based protective layer 23 formed on the metal layer 15, and an adhesive layer 16 formed on the resin-based protective layer 23. The transfer foil 20 according to the second embodiment includes, in addition to the configuration of the transfer foil 10 according to the first embodiment, a film protective layer 22 formed between the base film 11 and the release layer 13, and another resin-based protective layer 23 formed between the metal layer 15 and the adhesive layer 16.
[0033] [Other embodiments] Although the above-mentioned transfer foils 10 and 20 have the metal layer 15, the metal layer 15 may be omitted.
[0034] The transfer foil 10 according to the first embodiment will be taken as an example and described in detail below, but unless otherwise specified, the description can also be applied to the transfer foil 20 according to the second embodiment.
[0035] The plasticizer is not particularly limited, but examples thereof include chlorinated paraffin, butyl adipate, 2-ethylhexyl adipate, dioctyl adipate, 2-ethylhexyl azelaate, phthalate esters, dibutyl phthalate, diheptyl phthalate, di-2-ethylhexyl phthalate, diisononyl phthalate, diisodecyl phthalate, citric acid esters, esters of succinic acid and triethylene glycol monomethyl ether, esters of adipic acid and diethylene glycol monomethyl ether, tricarboxylic acid esters such as trioctyl trimellitate, esters of 1,3,6-hexatricarboxylic acid and butyl diglycol, tricresyl phosphate, triphenyl phosphate, tri-2-ethylhexyl phosphate, trixylenyl phosphate, triethyl phosphate, low molecular weight polyesters, epoxidized soybean oil, epoxidized linseed oil, The esters include at least one selected from the group consisting of epoxidized octyl stearate, epoxidized fatty butyl, epoxidized linseed oil fatty acid butyl, trimellitic acid esters, pyromellitic acid esters, sebacic acid esters, azelaic esters, maleic acid esters, benzoic acid esters, methyl adeticate, butyl oleate, oxyacid esters, dihydric alcohol esters, aliphatic dibasic acid esters, triphenyl phosphate, dinonylnaphthalene, tributyl acetyl citrate, p-toluenesulfonamide, toluenesulfonamide, toluenesulfoneethylamide, aminobenzenesulfonamide compounds, aminotoluenesulfonamide compounds, N-butylbenzenesulfonamide, N-ethyl-o(ortho)-toluenesulfonamide, dinonylnalene, tributyl acetyl citrate, and ethylene olefin oligomers.
[0036] The content of the plasticizer in the resin-based protective layer 14 is, but is not limited to, 1 to 20% by weight. The thickness of the resin-based protective layer 14 is, but is not limited to, 1 to 20 μm. The resin-based protective layer 14 contains, but is not limited to, one or more kinds of acrylic resins. The resin-based protective layer 14 contains, but is not limited to, a curing agent. The resin-based protective layer 14 contains, but is not limited to, a coloring agent. Hereinafter, a resin-based protective layer containing a coloring agent may be particularly referred to as a "coloring resin-based protective layer". The resin-based protective layer 14 contains, but is not limited to, a light stabilizer. The resin-based protective layer 14 contains, but is not limited to, an ultraviolet absorbing agent.
[0037] The above-mentioned transfer foil 10 is transferred to a transferee using a transfer device shown in FIG. 3, FIG. 4 or FIG. 5. FIG. 3 is a schematic diagram showing plate making by an up-down transfer foil stamping machine 31 using a flat plate 30. The foil stamping machine 31 transfers the transfer laminate 12 to a transferee 32 such as a soft vinyl chloride sheet by pressing the transfer foil 10 with the flat plate 30. FIG. 4 is a schematic diagram showing plate making by an up-down transfer foil stamping machine 41 using a relief plate 40. The foil stamping machine 41 transfers the transfer laminate 12 to a transferee 32 such as a soft vinyl chloride sheet by pressing the transfer foil 10 with the relief plate 40. FIG. 5 is a schematic diagram showing plate making by a heat pressure transfer machine (hereinafter sometimes referred to as a "roll type transfer machine") 51 using a roll plate 50. The heat pressure transfer machine 51 transfers the transfer laminate 12 to a transferee 32 such as a resin-based molded product by pressing the transfer foil 10 with the roll plate 50.
[0038] The transfer foil 10 described above is manufactured using a gravure printing machine and a drying oven shown in Fig. 6 or Fig. 7. Fig. 6 is a schematic diagram showing a gravure printing machine 60 and a first type drying oven 61. Fig. 7 is a schematic diagram showing a gravure printing machine 60 and a second type drying oven 62.
[0039] As shown in FIG. 6 and FIG. 7, the gravure printing machine 60 includes a film unwinding section 63, a film control roll 64, and a gravure coating head section 65. A first type drying oven 61 is provided downstream of the gravure printing machine 60 shown in FIG. 6. The first type drying oven 61 includes a driving metal roll 66, a far-infrared heater 67, an exhaust device 68, and a hot air device 69. A film control roll 70, a pressure device 71, a cooling device 72, and a film winding section 73 are provided downstream of the first type drying oven 61. A second type drying oven 62 is provided downstream of the gravure printing machine 60 shown in FIG. 7. The second type drying oven 62 includes an ultraviolet irradiation device 74 in addition to the configuration of the first type drying oven 61 described above. A film control roll 70, a pressure device 71, a cooling device 72, and a film winding section 73 are provided downstream of the second type drying oven 62.
[0040] In this embodiment, a transfer laminate 12 including a release layer 13, a resin-based protective layer 14, a metal layer 15, and an adhesive layer 16 is formed on the surface of a base film 11, to provide a transfer foil 10 for thermal and pressure-sensitive transfer that can prevent cracks, breaks, and blistering and reduce fading in the thermal and pressure-sensitive transfer film that modifies the shape of the transferred object 32.
[0041] The release layer 13, the resin-based protective layer 14, and the adhesive layer 16 are formed using a gravure printer 60. The metal layer 15 is formed using a two-chamber semi-continuous vacuum deposition apparatus. For example, the apparatus shown in FIG. 4 of JP 2002-192895 A (Patent Document 2) can be used as the vacuum deposition apparatus. The resin-based protective layer 14 containing a plasticizer is heated and dried with hot air by the gravure printer 60 to form a film on the release layer 13, and the metal layer 15 and the adhesive layer 16 are formed. The resin-based protective layer 14 contains a plasticizer, so that it has flexibility. The dry film of the resin-based protective layer 14 formed on the release layer 13 is heated in the drying furnaces 61 and 62 of the gravure printer 60, annealed with hot air, and then pressurized and cooled by passing through the connected pressurizing device 71 and cooling device 72, whereby the film quality is modified from hard to soft. Thereafter, a metal layer 15 and an adhesive layer 16 are deposited.
[0042] Instead of the above-mentioned method, the transfer foil 10 can also be manufactured by the following method. After forming the metal layer 15 on the resin-based protective layer 14 containing a plasticizer, the superposed peel layer 13, protective layer 14 and metal layer 15 are heated by the hot air device 69 of the drying furnaces 61 and 62, and an annealing process is performed to heat and bake the superposed dry film, and the resin-based protective layer 14 and metal layer 15 are made flexible from their hard films by passing through a pressure device 71 and a cooling device 72 installed outside the furnaces and connected to the drying furnaces 61 and 62, and the interface between the resin-based protective layer 14 and the metal layer 15 becomes more bonded and extensible.
[0043] The transfer laminate 12 has a flat membrane structure, but can also be produced to have a three-dimensional structure by coating through heating, hot air, pressure, and cooling using a gravure printing machine 60 or the like.
[0044] In the transfer laminate 12, 21, the release of residual stress during film formation during thermal pressure transfer, and the influence of the transfer laminate 12 due to the substrate film 11, the transfer laminate 12, the transferred surface, structure, material, shape, etc. during transfer, peeling, and fixing during thermal pressure transfer affect the metal formation film with low elasticity. Regardless of the metal cohesive structure of the metal deposition structure layer or metal island structure layer, which is the metal layer 15, the influence on the cohesiveness of the metal layer 15 is expressed by the propagation of heat pressure during transfer. The cohesive failure of the metal layer 15 is generated and appears in the form of cracks, breaks, bulges, etc. If it occurs in the metal layer 15 or the adjacent protective layer 14, it will affect the modification, reduce the brightness, and promote film deterioration.
[0045] The purpose of this embodiment is to avoid the above-mentioned problems and improve the transfer ability of the transfer laminate 12, 21. In this embodiment, a plasticizer is added to the resin-based protective layer 14, and heat treatment, hot air treatment, pressure treatment, and cooling treatment are performed using a gravure printing machine 60 or the like, and a drying oven type 1 oven 61 or type 2 oven 62 of the gravure printing machine 60 is used. Since the resin-based protective layer 14 contains a plasticizer, the flexibility of the protective layer 14 exhibits affinity for the metal layer 15, and in the process of bonding the protective layer 14 and the metal layer 15, the flexibility of the plasticizer promotes integration of the protective layer 14 and the metal layer 15, and the stretch resistance and shrink resistance of the protective layer 14 and the metal layer 15 are improved.
[0046] Eliminating the above-mentioned problems also leads to the attenuation of luminance deterioration. In addition, by making the particulate coloring agent fine and incorporating it into the resin-based protective layer 14, it is possible to improve the coloring effect and the reflectance of the metal layer 15 while maintaining the transparency of the protective layer 14. By selecting the particles, it is possible to obtain light resistance as well as coloring, transparency, and a metallic feel accompanied by metallic reflectivity.
[0047] The adhesive for forming the adhesive layer 16 is appropriately selected from various materials, taking into consideration the adhesiveness, film rupture property, and film stability.
[0048] Examples of adhesives include polyacrylic ester-based resins, polyvinyl acetate-based resins, vinyl chloride-vinyl acetate copolymers, ethylene-vinyl acetate copolymers, polyester-based resins, polystyrene-based resins, polyamide-based resins, ethylene-propylene-based resins, polypropylene-based resins, ethylene-vinyl acetate-based resins, vinyl chloride-vinyl acetate-based resins, polyvinyl chloride, polyvinylidene chloride, cellulose-based resins, rosin-based resins, organic pigments, and inorganic pigments.
[0049] In terms of adhesiveness, it is preferable to select from polypropylene, polyester, vinyl, etc. In order to ensure the stability of the film formation, cellulose is preferable. In terms of the film rupture property of the adhesive layer 16, it is preferable to select from rosin, or organic, inorganic, or filler pigments.
[0050] The resin-based protective layer 14 preferably contains one or more acrylic resins and has weather resistance. Deterioration by ultraviolet light due to natural light causes a decrease in physical properties and a change in appearance. Direct and scattered solar radiation breaks hydrogen atoms in the polymer and coloring agent of the transfer laminate 12, generating radicals. The radicals combine with oxygen in the air to generate peroxy radicals. The peroxy radicals remove hydrogen atoms from the polymer to generate radicals and hydroperoxides. The hydroperoxides accelerate the deterioration of the polymer. To improve the resistance of the protective layer 14, acrylic resins that are expected to have a long-term shielding effect, ultraviolet shielding agents such as inorganic pigments, ultraviolet absorbers (UVA) that convert ultraviolet light into heat energy, etc., light stabilizers (HALS) that capture radicals, phenol-based antioxidants that capture peroxy radicals generated by the combination of radicals and oxygen, and phosphorus-based antioxidants that decompose the hydroperoxides by removing hydrogen atoms from the polymer with the peroxy radicals. One of the acrylic resins contained in the mixture for the protective layer 14 contains ultraviolet absorbing groups and ultraviolet stable groups (HALS) in the resin skeleton, and radicals are generated by light in the surface peel layer 13 and the resin-based protective layer 14 after transfer, and a long-term ultraviolet shielding effect is expected to be achieved by inactivating active oxygen. The other acrylic resin is a silicone acrylic resin that contains ultraviolet absorbing groups and ultraviolet stable groups (HALS) and has silyl groups, and contains alkyl silicate, forming a coating that is hard and highly resistant to ultraviolet rays. The third acrylic resin has reactive functional groups attached, and is crosslinked with an amino resin by a catalyst to form a hard film.
[0051] The resin-based protective layer 14 is a thermosetting resin having an amino-based resin, a hardener, and an acrylic-based resin. The amino-based resin is selected from melamine-based resins. The hardener is selected from organic acids or inorganic acids. The acrylic refers to acrylic or methacrylic. The acrylic resin is selected from those having ultraviolet stable groups (HALS) added thereto, those having functional groups such as silyl groups, amino groups, methylol groups, hydroxyl groups, oxadrine groups, cyclocarbonate groups, and cyclocarbonate groups, copolymers with trialkoxyvinylsilanes, etc., isocyanate groups, addition reactions with unsaturated groups, reactions with amines, and materials having epoxy groups, etc.
[0052] A peeling layer 13 and a resin-based protective layer 14 containing a coloring agent are formed on a substrate film 11 by a gravure printing machine 60, a metal layer 15 is formed by a two-chamber semi-continuous vacuum deposition apparatus, and an adhesive layer 16 is formed thereon by a gravure printing machine 60 to produce a transfer foil 10 including a pressure-sensitive heat-sensitive thermo-pressure transfer laminate 12. In this transfer foil 10, a pigment is used as a coloring agent for the resin-based protective layer 14. When the pigment content is low, there is transparency but no coloring effect. When the pigment content is high, there is a coloring effect but the reflectivity of the metal layer 15 is concealed. A pigment is selected as a coloring agent for the protective layer 14. The protective layer 14 is refined to a thickness of 1 to 10 μm, a liquid preparation solvent of 60 to 80 wt%, a solute of 20 to 40 wt%, a pigment content of 5 to 15 wt%, and a pigment particle size of 10 to 120 nm. The pigment is further sized to a particle size of 10 to 80 nm. By using this finely divided pigment in the formulation of the protective layer 14, a coloring effect similar to that of a dye is produced, transparency of the protective layer 14 is produced, and reflectivity of the metal layer 15 is produced, resulting in light resistance. This not only provides reflectivity to the metal layer 15, but also allows the use of the pigment to produce a metallic feel due to the metallizing effect as a coloring effect. The resin-based protective layer 14 obtains light resistance by using a coloring agent such as an organic pigment.
[0053] As the coloring agent, inorganic pigments such as titanium white, carbon black, red iron oxide, yellow lead, ultramarine, etc., organic pigments such as aniline black, quinacridone red, isoindolinone yellow, phthalocyanine blue, etc. are selected, and the pigments are sized to about 10 to 80 nm using a bead mill type disperser. The coloring agent can improve the transparency of the pigment and the visibility as a coloring effect. Furthermore, the resistance can be increased by selecting a pigment with excellent light resistance. For example, fine oxides such as TiO2, SO2, Al2O3, Fe2O3, etc. Furthermore, by additionally containing a light stabilizer, an ultraviolet absorbing agent, and a light shielding agent, the fading of the protective layer 14 can be suppressed. Furthermore, the resistance can be promoted and improved by adopting a polymerization material that combines a light stabilizer, silicon, silicate, etc. with the skeleton of an acrylic resin.
[0054] In the resin-based protective layer 14, a light stabilizer is added to the formulation. It contributes to light stability by capturing and detoxifying radicals generated by ultraviolet light. A non-basic neutral type hindered amine-based light stabilizer is selected. This prevents the formation of a thermosetting film of the protective layer 14 from going wrong.
[0055] An ultraviolet absorbing agent is added to the resin-based protective layer 14. The ultraviolet absorbing agent is selected from ultraviolet absorbing agents capable of suppressing photoinduced reactions that lead to photodegradation of the protective layer 14. Hydroxyphenyltriazine-based materials with ultraviolet absorbing wavelengths of 280 to 350 nm, 310 to 330 nm are selected in order to stabilize the protective layer 14 by absorbing ultraviolet rays, converting them into low thermal energy, and releasing them.
[0056] In order to suppress chemical reactions caused by light in the transfer laminate 12, which causes discoloration and film deterioration, the transfer laminate 12 absorbs light and becomes in a high energy state due to the absorbed energy, some of which undergoes photosensitization and becomes light energy again. Some of it leads to chemical reactions. In addition, the excess energy is transferred to other molecules and reacts with polymers. The ultraviolet wavelength range of 200 to 300 nm has a significant chemical effect. As a countermeasure for the resin-based protective layer 14 containing a color retaining agent, in addition to preparations that obtain transparent fine pigments, acrylic resins, polymers with hindered amines bonded to the structure of acrylic resins, hindered amine-based light stabilizers, and hydroxyphenyl triazine-based ultraviolet absorbers, a photoreaction inhibitor is selected from salicylic acid esters, 4-t-butylphenyl-salicylate, phenyl salicylate, etc., and phenyl salicylate, which is an ultraviolet blocking agent, is selected and added as a photoreaction inhibitor.
[0057] As a means for forming the metal layer 15, there are vapor phase deposition methods such as PVD (physical vapor deposition) such as vacuum deposition and sputtering, chemical vapor deposition methods such as thermal CVD, atomic layer deposition (ALD), plasma CVD, metal organic chemical vapor deposition, two-flow MOCVD, catalytic chemical vapor deposition (Cat-CVD), etc., and liquid phase deposition methods such as melt methods such as liquid phase epitaxy, plating methods such as wet plating, chemical plating, and sol-gel, and coating methods such as spin coating, printing, and inkjet. The metals used are selected from Au, Ag, Cu, Sn, Al, Ni, Pt, Rh, Pd, Zn, Cr, Si, as well as oxides such as In2O3, CdO, CdIn2O4, Cd2SnO4, TiO2, SnO2, ZnO, SiO2, ZrO2, sulfides such as ZnS, and fluorides such as MgF2. Alloys can also be used. Multilayers are also possible. The film shape of the metal layer 15 includes a sea-island film structure in which the metal layer 15 is in an isolated island state, and a deposited film structure showing the deposited state of metal. In any structure, regardless of the metal used or the deposited state of the metal, it is possible to suppress the expansion and contraction that the transfer laminate 12 receives during thermocompression transfer, and cracks, breaks, swelling, etc. caused by pressure.
[0058] The thickness of the metal layer 15 is 10 to 30 nm in the case of isolated islands, and 20 to 60 nm in the case of a continuous film deposition. In either case, the metallic color can be kept uniformly shiny. It enhances the decorativeness and designability of the thermal pressure transfer figurative display.
[0059] [Method 1] As the base film 11, any film may be used as long as there is no abnormality in heat resistance during production, resistance to solute solvents, transfer heat resistance during use, and pressure resistance. For example, there are polyester-based films such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-isophthalate copolymer, terephthalic acid-cyclohexane dimethanol-ethylene glycol copolymer, polyethylene terephthalate-polyethylene naphthalate co-extrusion film, polyamide-based films, polyolefin-based films, acrylic-based films, imide-based films, various engineering-based films, styrene-based films, cellulose-based films, etc. Among them, in order to maintain physical and chemical strength, biaxially stretched films are preferable. Among these, polyethylene terephthalate films are preferable. Taking into consideration heat and pressure transfer, if the film is thick, both heat conduction and pressure transmission are insufficient. On the other hand, if the film is thin, the mechanical strength is insufficient, and it becomes difficult to clearly display the transferred image due to deviation from the control of the transfer heat pressure. It is preferable to use a film having a thickness in the range of 12 to 75 μm according to the shape and material of the transferee 32.
[0060] Similarly, the release layer 13, the resin-based protective layer 14, and the adhesive layer 16 are formed by the gravure method. A far-infrared heater 67 and a hot air device 69 are used as drying means. FIG. 6 shows an outline of the gravure printing machine 60 and the first type drying oven 61. The first type drying oven 61 is used, and the plate is run and stayed in the oven atmosphere at 90 to 210° C. for 20 to 50 seconds to produce each film with a thickness of 0.1 to 20 μm. In addition, a two-chamber semi-continuous vacuum deposition device is used to form the metal layer 15 with a thickness of 30 to 60 nm. Then, the adhesive layer 16 is formed.
[0061] [Method 2] After the release layer 13 and the resin-based protective layer 14 are formed, the sheet is printed on a 2.64 m 3 sheet of paper in a gravure printing machine 60 shown in FIG. 3 The second type drying furnace 62 is used, and the dry film is baked by running and staying in an atmosphere of 100 to 210° C. for 20 to 50 seconds, followed by an annealing process. Thereafter, the metal layer 15 and the adhesive layer 16 are formed.
[0062] [Method 3] The drying means for the release layer 13 and the resin-based protective layer 14 is a type 1 drying oven 61 shown in Fig. 6 using a far-infrared heater 67 and a hot air device 69 in the oven, and the film is run and stayed in an atmosphere of 90 to 210°C for 20 to 50 seconds to produce a flat film with a thickness of 0.1 to 20 μm. Next, after forming the metal layer 15 with a deposition machine, a type 2 drying oven 62 in a gravure printing machine 60 shown in Fig. 7 is used, and the film is run and stayed in an atmosphere of 150 to 210°C for 20 to 50 seconds to perform an annealing treatment for baking the dry film consisting of the release layer 13, the resin-based protective layer 14, and the metal layer 15 laminated on the base film 11. Then, the adhesive layer 16 is formed.
[0063] [Method 4] The resin-based protective layer was dried using a far-infrared heater 67 and a hot air device 69. A first-type drying oven 61 shown in FIG. 6 was used, and the film was run and stayed in an atmosphere of 90 to 210° C. for 20 to 50 seconds to produce a flat film with a thickness of 0.1 to 20 μm. Next, after the metal layer 15 was formed using a deposition machine, a gravure printing machine 60 having a second-type drying oven 62 shown in FIG. 7 was used, and the film was run and stayed in an atmosphere of 150 to 210° C. for 20 to 50 seconds to be heated in the oven. A pressurizing treatment was performed using a pressurizing device 71 directly connected to the outside of the oven, followed by a cooling treatment using a cooling device 72 installed thereon. Then, an adhesive layer 16 was formed.
[0064] [Recipe 5] A first type drying furnace 61 shown in Fig. 6 is used, and the film is left in an atmosphere of 90 to 210°C for 20 to 50 seconds to produce a flat film with a thickness of 0.1 to 20 μm. Next, after forming a metal layer 15 with a deposition machine, a second type drying furnace 62 shown in Fig. 7 is used, and the film is left in a heated atmosphere of 150 to 210°C for 20 to 50 seconds to perform an annealing process for baking the dry film. After heating in the furnace, continuous pressurization and cooling processes are performed by an external pressurizing device 71 and a cooling device 72 connected to the furnace, and a three-dimensional structure film including a peeling layer 13, a resin-based protective layer 14, and a metal layer 15 is completed. Then, an adhesive layer 16 is formed.
[0065] [Recipe 6] A first type drying oven 61 shown in FIG. 6 is used, and the film is run and stayed in an atmosphere of 100 to 210°C for 20 to 50 seconds to produce a flat membrane with a thickness of 0.1 to 20 μm. Next, after forming a metal layer 15 with a vacuum deposition machine, a second type drying oven 62 shown in FIG. 7 is used, and the film is run and stayed in an atmosphere of 150 to 210°C for 20 to 50 seconds. After heating, continuous pressure treatment and cooling treatment are performed to complete a flat membrane or a three-dimensional membrane. The production of a flat membrane or a three-dimensional membrane can be distinguished by changing the level of heating, hot air, pressure, and cooling treatment. Then, an adhesive layer 16 is formed.
[0066] The transfer foil 10 according to the present embodiment includes a base film 11 and a transfer laminate 12 composed of a peeling layer 13, a protective layer 14, a metal layer 15, and an adhesive layer 16. The transfer laminate 12 is peeled from the base film 11 and transferred to a transferee 32 through the heat pressure time of a transfer machine. During the transfer operation, the transfer laminate 12 peeled from the base film 11 is transferred to the transferee 32 by the transfer action, requiring a heat source, pressure, and transfer residence time supplied from the transfer machine. Depending on the shape and hardness of the material of the transferee 32, the effects of heat and pressure are not uniform. Compared to the base film 11 and the transferee 32, the transfer laminate 12 is a thin film with peelability and has breakability during transfer peeling. The film peelability is a peel resistance value of 1 to 100 g / cm. 2 (Using a peel resistance tester manufactured by Asahi Sokki Co., Ltd.) This is the starting point of film peeling. The film rupture resistance is 500g~10Kg / cm 2This is the starting point of film rupture due to transfer pressure at 0.5 seconds (using an Ikeda-type transfer device). The transfer laminate 12 is easy to peel off and has a breakability. The transferee 32 has a variety of shapes, including two-dimensional and three-dimensional, and is made of various materials, including leather, paper, paper containers, printing paper, special paper, wood, fiber, resin sheet, resin molding, metal, and glass. Considering the transfer laminate 12, which is stretched over the base film 11, with the transferee 32, the transfer laminate 12 is more likely to develop cracks, breaks, and swelling due to the stretchability and breakability of the transfer laminate 12 in response to the supply of heat and pressure during transfer, compared to the base film 11 and the transferee 32. Here, flexibility can be imparted by adding a plasticizer to the protective layer 14. Furthermore, the adhesion between the protective layer 14 and the metal layer 15 is enhanced to a bond by going through the process using the gravure printing machine 60. The combined effects of heating, hot air, pressure, and cooling by the gravure printing machine 60 are that the flexibility provided by the addition of plasticizer to the protective layer 14 becomes extensible, the heat resistance of 380°C maintains resistance to the occurrence of cracks, breakage, and swelling, and the structural transformation of the resistance that results in the expression of the ability of the protective layer 14 and the metal layer 15 to coexist brings about a change in the ability of the transfer laminate 12.
[0067] When the transfer laminate 12 is formed by the gravure printing machine 60, the following film-forming environment can be newly established. (1) Adhesion: Bonding by overlapping the resin-based protective layer 14 and the metal layer 15 (2) Extensibility: Extensibility of the resin-based protective layer 14 and the metal layer 15 (3) Durability: Avoidance of cracks, breaks, and swelling during transfer and after aging of the transfer laminate 12 (4) Metal reflectance: Reflectance of Al metal layer 15 is 82.15% (spectral reflectance %) When a pigment is used in the protective layer 14, the luster is excellent. In the base film 11, the peeling layer 13, the protective layer 14, the Al metal layer 15, and the adhesive layer 16, the Al film reflectance of the color layer using a fine pigment in the protective layer 14 is (5) Morphology of the deposited film: The protective layer 14 and the metal layer 15 maintain their bond and exhibit extensibility, regardless of whether the metal layer 15 has a sea-island film structure or a deposited film structure. This makes it possible to prevent cracks, breaks, and swelling of the transferred laminate 12 caused by cohesive failure of the metal. (6) Heat resistance: In a heat resistance test after transfer of the transfer laminate 12, the transfer laminate 12 has excellent resistance to cracks, breakage, and swelling at 380°C. (7) Resin-based protective layer 14: Thermoplastic resin, thermosetting resin, ultraviolet curing resin, or a multilayer of ultraviolet curing resin and thermosetting resin can be used. All of them contain the above-mentioned plasticizer, and by the above-mentioned manufacturing process, a film that shows heat resistance and extensibility and has adhesiveness with the metal layer 15 can be formed. (8) Resin-based protective layer 14: A curable type can be used as an ultraviolet-curable resin. (9) Resin-based protective layer 14: An after-cure type ultraviolet-curing resin can be used. (10) Resin-based protective layer 14: When an ultraviolet-curable resin is used, hot stamping and cold stamping can be used as a transfer method. (11) Resin-based protective layer 14: When a multilayer of ultraviolet-curable resin and thermosetting resin is used, the ultraviolet-curable resin increases the strength of the film, while the thermosetting resin increases the film breakability. Both resins contain a plasticizer. (12) Extensibility: There is a three-dimensional transfer target 32 as a resin-based processed product produced by a resin-based molding machine or the like. In this case, when forming a molded product, the transfer laminate film is shaped in the mold of the molding machine, and is bonded by the heat and pressure of the molten resin. When the excess film is then peeled off, the transfer laminate 12 can maintain resistance to the stretching that it receives.
[0068] The surface modification of the molded product may be performed by transferring and peeling the modified laminate consisting of the transfer laminate 12 peeled off from the base film 11 using a transfer machine, or by transfer transfer in a molding machine. After adhering the plasticizer-containing resin-based protective layer 14 or the colored resin-based protective layer 14 or the image-formed colored resin-based protective layer 14 to the base film 11, the metal layer 15, the resin-based protective layer 23, and the adhesive layer 16 are formed on the resin-based protective layer 14, and the adhesive layer 16 is brought into contact with the transferee 32 via a transfer device, and is bonded by heat and pressure supplied from above the base film 11, and can be bridged to the transferee 32 together with the base film 11. This manufacturing method enables a multi-layered structure with excellent heat resistance and extensibility. According to such a multi-layered structure, the transfer laminate 12 using the base film 11 and the modifying image-formed film integrated with the base film 11 can be applied regardless of heat and pressure transfer, out-molding, or in-molding.
[0069] Molding methods using thermoplastic resins and thermosetting resins for producing two-dimensional and three-dimensional molded products using a molding machine using resin-based materials include injection molding, blow molding (hollow molding, suction molding), extrusion molding, cast molding, vacuum forming, air pressure molding, compression molding, press molding, hand lay-up, T-die method, inflation method, calendar molding, co-extrusion multi-layer T-die method, biaxial stretching method, lamination method, profile extrusion, extrusion coating, co-extrusion, etc., and after formation into a molded product, there are means for transferring transfer lamination 12 as a modified lamination by post-application, means for peeling and transferring an image from base film 11 during in-mold to the molded product as a primary processing method in the mold of the molding machine, and means for laminating the molded product together with base film 11, etc. The object 32 to be transferred by simultaneous transfer onto a molded product, simultaneous attachment onto a molded product, or post-transfer can be a modified laminated structure film that has been given a shaped color by selecting from a wide variety of molding methods and modification means, including leather, as described above.
[0070] When the selected plasticizer is added to the protective layer 14 and the above-mentioned manufacturing process is carried out, the produced transfer laminate 12 and the film lamination that is laminated together with the base film 11 will have the functionality of stretchability, heat resistance, interlayer adhesion, maintenance of the reflectance of the metal layer 15, light resistance, and prevention of cracks, breakage, and swelling, which indicates improved quality.
[0071] The three-dimensional structure of the transfer laminate 12 including the resin-based protective layer 14 is a substrate film 11, a peeling layer 13, a resin-based protective layer 14, a metal layer 15, and an adhesive layer 16. In the transfer laminate 12, a flat film and a three-dimensional film can be formed by heating and drying the coating film using a heat source of a far-infrared heater 67 and a hot air device 69 at a temperature in the range of 150 to 210 ° C., pressurizing, and cooling by a drying means using a first type drying oven 61 of a gravure printing machine 60 and a second type drying oven 62 of a gravure printing machine 60. At this time, the transfer laminate 12 is completed by sequentially forming the peeling layer 13, the resin-based protective layer 14, the metal layer 15, and the adhesive layer 16 on the substrate film 11, but when the resin-based protective layer 14 is treated, the first type drying oven 61 of the gravure printing machine 60 is used to continuously perform heating and drying, hot air treatment, pressurization treatment, and cooling treatment. The protective layer 14 is hardened by heating and drying using a mixture of an amino resin material containing a plasticizer and a hardener, while the resin material is hardened by successive operations of heating, hot air, pressure, and cooling. The protective layer 14 containing a plasticizer exhibits flexibility. After the protective layer 14 is formed, the metal layer 15 is formed, and the peeling layer 13, the protective layer 14, and the metal layer 15 are layered together, and the dry film is baked using a gravure printing machine 60 having a two-type drying oven 62. This allows the protective layer 14 to exhibit flexibility. When the interface between the protective layer 14 and the metal layer 15 is heated, pressurized, and cooled, the heating and pressurizing operations create affinity between the protective layer 14 and the metal layer 15, and the cooling operation ensures fixation between the layers to form the transfer laminate 12. The metal layer 15 may have an isolated island structure in which the metal is in a sea-island shape, or a sedimentary structure in which the metal is in a sedimentary shape.
[0072] During the drying process of gravure coating, heating in the second type drying oven 62, applying pressure outside the oven, and cooling outside the oven are successively performed, so that the resin-based protective layer 14 becomes sticky through this process of the protective layer 14 and the metal layer 15. Compatibility is created between the resin in the protective layer 14 and some of the metal particles in the metal layer 15. The effects of accumulation of residual stress due to film shrinkage when the protective layer 14 hardens are reduced by the inclusion of a plasticizer in the formulation. The shear stress on the metal layer 15 is reduced, and the load on the destruction of the cohesiveness of the metal layer 15 is attenuated.
[0073] The peeling layer 13 and the resin-based protective layer 14 are treated in a first drying oven 61 of a gravure printing machine 60, the metal layer 15 is overlaid, heated in a second drying oven 62 of the gravure printing machine 60, and then pressurized and cooled outside the oven in succession. This is a necessary process for the flexible film quality of the resin-based protective layer 14 to be propagated to the interface with the metal layer 15 and fixed. Both the protective layer 14 and the metal layer 15 become hard and sticky film quality by heating, pressurizing, and cooling. Furthermore, the flexible film quality of the protective layer 14 is transferred to the metal layer 15, and both layers have the hardened film and toughness of the protective layer 14 and the extensibility due to the flexibility of the protective layer 14 containing a plasticizer. The film rupture caused by the cohesive failure of the metal layer 15 due to the residual stress of the protective layer 14 begins to shear the transfer laminate 12, which is a factor in the occurrence of cracks, breakage, swelling, etc. In order to suppress this, the film quality is modified to improve the heat resistance, flexibility, adhesion, and extensibility between the two layers. In order to improve the adhesion between the protective layer 14 and the metal layer 15, a film quality containing a heat-resistant plasticizer and an interface migration-inducing plasticizer is transferred and bonded to the metal layer 15, and annealing treatment such as heating, pressure treatment, and cooling treatment are performed. It is confirmed whether the correlation between the protective layer 14 and the metal layer 15 is expressed in the heat resistance, flexibility, adhesion, and extensibility in the relationship with the bonding of the two layers.
[0074] In the examples described later, when the surface of the transfer laminate 12 after transfer was observed, the three-dimensional structure formed was a cross section of a radial arcuate shape with a chord of 1 μm, a height of 13 μm, and an arc of 26 μm, as shown in FIG. 8. It appeared as a three-dimensional structure film of concave-convex ridge-like adjacent layers. Further investigation was performed to enlarge the changes in the surface of the surface layer after the thermal pressure transfer, and no phenomena such as cracks, breaks, or swelling were observed.
[0075] Figures 8 to 10 are photographs showing the three-dimensional structure film, and Figures 11 to 14 are photographs showing cracks, breaks, and blisters on the flat membrane structure film of the transferred laminate 12.
[0076] A peeling layer 13 is formed on the base film 11, and a plasticizer-containing resin-based protective layer 14 is coated using a gravure printer 60 having a type 1 drying oven 61 to produce a flat film. Next, a metal layer 15 is formed by overlapping, and while still in the laminated state, a gravure printer 60 having a type 2 drying oven 62 is used to bake the dry film, and heating, pressing, and cooling are performed using a far-infrared heater 67 and hot air. The transfer laminate 12 was stretched and raised together, and a continuous three-dimensional structure band with a ridge-like wrinkle shape was observed. Next, an adhesive layer 16 was formed to complete the transfer laminate 12. This transfer laminate 12 was transferred onto a soft vinyl chloride sheet, and the surface layer of the transfer laminate 12 was confirmed. The heat and pressure transfer conditions were as follows: a top-bottom transfer foil stamping machine was used, the temperature was 160°C, and the pressure was 5Kg / cm. 2 When the transfer dwell time was 0.5 seconds and relief plate 40 was used, no cracks, breaks, or blistering occurred, and no change was observed in the metallizing effect. The plasticizer-containing resin-based protective layer 14 and the metal layer 15 are both in tune with the film extension, and the metal layer 15 with low cohesive force and the protective layer 14 released from residual stress by the heating, pressurizing, and cooling processes induce plastic deformation in the thin metal film and provide plasticity through the in-furnace and out-furnace processes of the gravure printing machine 60. The metal layer 15 has a structure of a deposited particle film or an isolated island particle film, and propagates its film quality to the protective layer 14. As a result, both the protective layer 14 and the metal layer 15 exhibit bonding properties, and the interface between the two layers is fixed.
[0077] The photograph in Figure 10 shows an enlarged three-dimensional structured image of the surface of the transfer foil 10 after it was transferred using a top-bottom transfer foil stamper in an experiment based on Manufacturing Method 5. The metal layer 15 was made of aluminum and had a film thickness of 40 nm, a valley width of 1.4 to 1.76 μm, a peak width of 0.99 to 1.2 μm, and a height of 11 to 14 μm.
[0078] This embodiment aims to improve defects that occur in the transfer laminate 12 during the thermal pressure transfer of the transfer foil 10 and over time after transfer. The transfer laminate 12 and the transferee 32 are deformed by external and internal forces such as cracks, breaks, swelling, and fading due to the thermal pressure load on the transfer laminate 12, breaks, bulging, and fading. The deformation of the transferee 32 and the transfer laminate 12 during transfer caused by this derived phenomenon reduces the modifiability of the transferee 32. It becomes necessary to obtain a maintenance method that can deal with this deformation individually as a burden that the transfer laminate 12 can bear.
[0079] The functions of the transfer laminate 12 include peeling, breaking, adhesion, heat resistance, glitter resistance, coloring, shape display, and decorativeness. In addition, in order to deal with the above-mentioned morphological changes that occur during transfer and after aging, it is necessary to add the following as a means for the transfer laminate 12. By adding a material that functions by expressing extensibility due to flexibility using heat resistance, flexibility, and migration inductivity to the protective layer 14 from among plasticizers, the function of the protective layer 14 can be improved and the function can be propagated to the metal layer 15. Furthermore, by passing the drying means of the gravure printing machine 60 through heating treatment, hot air treatment, pressure treatment, and cooling treatment, the functions of heat resistance and flexibility, along with the material with migration inductivity of the protective layer 14 to the metal layer 15, become a function propagated due to affinity to the interface of the metal layer 15, and are bonded and fixed. This creates extensibility in both the resin-based protective layer 14 and the metal layer 15. The protective layer 14 and the metal layer 15 share transfer breakability, extensibility, and heat resistance. The transfer laminate 12 becomes a modified laminate that is resistant to cracks, breaks, and blistering during transfer and after aging.
[0080] Among the plasticizers, a flexibility transfer inducer is set. A specific amount is set within a range that does not lead to delamination at the interface of the protective layer 14. The plasticizer-containing preparation has the function of transferring and inducing the flexibility property up to the vicinity of the interface of the thermosetting resin-based protective layer 14. The interface with flexibility due to the plasticizer of the thermosetting resin-based protective layer 14 is not sealed in the hardening film structure, but is dispersed in the film, and a small amount is fixed to the interface. When the protective layer 14 is formed by the gravure method, the affinity between the protective layer 14 and the metal layer 15 is enhanced by successively passing the film formation through the means of heating, hot air, pressure, and cooling.
[0081] For the plasticizer, materials with heat resistance, flexibility, and migration inductivity are identified and added to the protective layer 14. The identification of each material and the amount of each material are determined through experiments, and the heat resistance, flexibility, and migration inductivity are maintained, leading to the creation of affinity for the film that is layered on the interface of the protective layer 14. The plasticizer that can create these functions can be selected from one or more of the plasticizers listed above.
[0082] After forming a film of release agent on the base film 11 by the gravure method, the protective layer 14 is formed by heating the first type drying furnace 61 using a far-infrared heater 67, hot air treatment, and a film-forming method using an external furnace pressure device 71 and an external furnace cooling device 72 directly connected thereto. Alternatively, a flat film structure or a three-dimensional structure of the transfer laminate 12 can be formed by heating using a type 2 drying furnace 62, performing a film formation operation using an external pressure device 71 and an external cooling device 72 directly connected to hot air treatment, or performing an annealing process to bake the dry film of the protective layer 14 using a type 1 furnace 61 and a type 2 furnace 62, a film modification process of the protective layer 14 using an external pressure device 71 and an external cooling device 72, a modification process by superposing both the protective layer 14 and the metal layer 15, and by appropriately combining the modification process for each layer with the selection of a plasticizer in the formulation of the protective layer 14, the setting of the amount of plasticizer added and the effect, and the interfacial modification process of the superposed film of the protective layer 14 and the metal layer 15, etc.
[0083] In each of the heating, hot air, pressurizing, and cooling devices, the resin-based protective layer 14 can be cured and hardened by heating and hot air treatments. The pressurizing treatment releases the compressive residual stress of the resin film, and the cooling treatment softens and fixes the resin film, thereby enabling the fixing of the protective layer 14 and the metal layer 15. In the heating, hot air, pressurizing, and cooling treatments of the resin-based protective layer 14, and the annealing treatment of baking the dry film in the heating, hot air, pressurizing, and cooling treatments after the resin-based protective layer 14 and the metal layer 15 are layered, the affinity between the protective layer 14 and the metal layer 15 is improved, resulting in a softer, more viscous film quality.
[0084] The transfer foil 10 is composed of a film as a base material and a modified laminate to be transferred and peeled off. It is formed by laminating a film protective layer 22, a peeling layer 13, a resin-based protective layer 14, a metal layer 15, a resin-based protective layer 23, and an adhesive layer 16 in this order on a base material film 11 selected from chemical films. The film protective layer 22 and the metal layer 15 are not necessary. The resin-based protective layer 14 can be laminated. One or more of the plasticizers listed above are added to the resin-based protective layer 14. The metal layer 15 can be excluded, and the colored resin-based protective layer 14 can be a colored layer using a coloring agent such as a dye or pigment.
[0085] The film protective layer 22, the peeling layer 13, the resin-based protective layer 14, the adhesive layer 16, etc. are formed by the gravure method. The metal layer 15 is formed as a deposition layer using a two-chamber semi-continuous vacuum deposition apparatus. The drying equipment used in gravure coating has a far-infrared heater 67 installed in the oven, and can be heated and dried together with a hot air device 69. The transfer laminate 12 in the heating and warming vortex can be pressurized together with the base film 11 by a pressure device 71 installed just outside the drying ovens 61 and 62. Furthermore, the film can be rapidly cooled by passing through a cooling device 72 installed continuously to form a film. In addition, only the heating process can be performed by the far-infrared heater 67 and the hot air device 69. The gravure printing machine 60 is equipped with a first type drying oven 61 shown in FIG. 6 or a second type drying oven 62 shown in FIG. 7. The drying equipment can perform dry film formation through a drying means from a wet state of the prepared solution. In addition, an annealing process can be performed in which the dry film formed is heated and baked through a hot air treatment. Furthermore, the film that has been softened by swelling due to heat treatment can be compressed by the pressurizing device 71. The film can be rapidly cooled by the subsequent cooling device 72, thereby enhancing the fixation between the layers. Each of the means and the device for film formation can be carried out independently. They can also be used in conjunction with each other to form multiple layers. They can be selected and combined.
[0086] In addition to blending a plasticizer into the resin-based protective layer 14, the heat treatment using the gravure method, which involves heating, hot air, pressure, and cooling, tends to result in a noticeable tendency for the protective layer 14 to have a flexible state and affinity at each interface between the protective layer 14 and the metal layer 15 to have bonding properties after heat treatment. The compatibility of the resin-based layer and the metal-based layer is forced and bonding properties are enhanced by the processes using each device, such as heating, hot air, pressure, and cooling, using the gravure printing machine 60. The transfer laminate 12 is affected by the heating and pressure from the transfer device during thermo-press transfer, and the transfer laminate 12 and the transferee 32 are subjected to a load of expansion and contraction caused by the shape of the transfer laminate 12 including the base film 11, and the transferee 32. As a result, the transfer laminate 12 is prevented from cracking, breaking, swelling, etc.
[0087] The resin-based protective layer 14 is composed of acrylic resin, amino resin, hardener, ketone resin, coloring agent, light stabilizer, light blocking agent, ultraviolet absorber, plasticizer, solvent, etc. These are formed into a film by a gravure printing machine 60 as a transfer laminate 12. During transfer, the transfer laminate 12 is subjected to loads of expansion, contraction, compression, and heat. In order for the transfer laminate 12 to withstand the formation of cracks, breaks, blistering, etc., flexibility is imparted to the cured film by selecting a plasticizer, and the affinity of the interface between the protective layer 14 and the metal layer 15 is enhanced by incorporating heating, pressure, and cooling by the gravure method. As a result, the transfer laminate 12 can be produced by selecting a flat film structure or a three-dimensional film structure that is highly extensible. EXAMPLES
[0088] Of the modified laminates, in the three-dimensional structure film, the surface layer of the transferred laminate 12 forms a continuous film with a three-dimensional structure with ridge-like unevenness. As shown in the photograph in Figure 8. It has a continuous three-dimensional shape with a parabolic arch cross section with a chord of 22.30 μm, a height of 13.87 μm, and an arc of 37.25 μm, and has a continuous three-dimensional film structure with a valley width of 1.1 to 1.14 μm in the concave parts and a peak width of 0.7 to 0.9 μm in the convex parts.
[0089] 8 to 10 show the three-dimensional shape of the modified laminate after transfer. Regarding the flat membrane structure of the modified laminate, in a heat resistance test after transfer, the temperature was gradually increased from room temperature to 380°C, and then the temperature was decreased to room temperature. As a result of the test in a cycle, no cracks, breaks, blistering, etc. occurred, there was no change in the reflectance of the metal layer 15, and no abnormalities such as peeling between layers of the laminate were observed.
[0090] As described above, the deposition of the three-dimensional structure film forms a continuous coating with fine irregularities on the surface layer by the transfer lamination 12. Light incident on the metal layer 15 in the film is reflected by the metal layer 15 and reaches the surface layer. The diffracted light returns to the surface layer, where optical interference occurs, producing the coherent metallizing effect. In addition, the light received by the fine three-dimensional layer on the surface layer produces optical interference on the surface layer.
[0091] The surface layer of the fine three-dimensional structure of the transfer laminate 12 is subjected to a pressure of 5 to 10 kg / cm during thermal transfer. 2The transfer peel resistance and film rupture properties were checked under conditions of a temperature of 150 to 200° C. and a transfer residence time of 0.5 seconds, and no change was observed. There was also no change in the luster.
[0092] The color-changing resin-based protective layer 14 contains a light stabilizer, a light blocking agent, an ultraviolet absorbing agent, etc., and prevents the fading of the dye, pigment, resin, etc.
[0093] The resin-based protective layer 14 has film strength as a cured film, contains a plasticizer, and is flexible. By applying heat, hot air, pressure, and cooling by the drying means of the gravure method, the transfer laminate 12 exhibits film toughness and stickiness. In the film production in which the flat film structure or three-dimensional structure shape of the transfer laminate 12 can be stretched while including the metal layer 15, the transfer breakability is maintained by the ketone-based material added to the formulation. When the base film 11 is peeled off from the transferee 32 after transfer, the transfer laminate 12 clearly displays the break end surface of the contour of the transfer image and has shear properties. The transfer breakability of the transfer laminate 12 was measured using a top-bottom transfer foil stamping machine using a metal transfer relief plate 40 shown in the photograph of Figure 16, at a temperature of 120 to 150°C, a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2 The transfer was performed using a 1 mm thick PP sheet as the transferee 32. The breakability after transfer is shown in the photograph in Figure 15. The transfer laminate 12 transferred onto the PP sheet was precisely broken and transferred into the shape of the metal plate, as shown in the photograph in Figure 16.
[0094] The transfer laminate 21 is formed by laminating the film protective layer 22, the peeling layer 13, the resin-based protective layer 14, the metal layer 15, the resin-based protective layer 23, and the adhesive layer 16 on the base film 11 in this order. The film protective layer 22 contains at least one selected from the group consisting of phenolic resin, epoxy resin, urea resin, unsaturated polyester resin, silicone resin, melamine resin, aniline resin, sulfonamide resin, alkyd resin, polyurethane resin, diallyl phthalate resin, and thermosetting polyimide resin. The film protective layer 22 is smoothly coated and adhered to the base film 11 with a thickness of 0.3 to 1 μm by a gravure printing machine 60. The film protective layer 22 has a function of providing uniformity of peeling to the peeling layer 13 during thermal pressure transfer. In addition, it maintains uniformity of thermal pressure propagation to the base film 11 and the transfer laminate 21 caused by the thermal pressure during transfer. Furthermore, it is possible to suppress the influence of the expansion and contraction action caused by the thermal pressure during transfer that the base film 11 receives. These features make it possible to maintain uniformity in the peeling of the transfer laminate 12 and to maintain stability in the thermal pressure transfer.
[0095] Since the resin-based protective layer 14 contains a plasticizer, even if the transfer laminate 12 expands and contracts due to thermocompression transfer, the metal layer 15 does not suffer from cohesive failure, and therefore the transfer laminate 12 does not crack, break, or bulge.
[0096] The transfer foil 10 is heated and pressurized on the transfer film with the transfer laminate 12 passed between the transfer foil 10 and the transferee 32, and the transfer laminate 12 is peeled off and broken from the base film 11, and transferred onto the transferee 32 as the selected image. This results in modification of the surface layer of the transferee 32. The modified laminate, which is the transfer laminate 12, is provided on the base film 11 with a resin-based protective layer 14 having adhesiveness for protecting the base film 11 and modifying the interface. By adhering the modified laminate to the base film 11 and forming a cured film, this serves as a measure to prevent the expansion and contraction of the base film 11 during the thermal transfer, and prevents the expansion and contraction from being transmitted to the transfer laminate 12. The transfer laminate 12 also provides peel stability during peeling. The film is formed to a thickness of 0.3 to 5 μm using a known thermosetting resin. Next, a peeling layer 13 is provided. Materials can be selected from known materials, such as methyl methacrylate, ethyl methacrylate, butyl acrylate, vinyl chloride resin, vinyl chloride-vinyl acetate copolymer, vinyl butyral, polyester resin, urethane resin, epoxy amino resin, amino alkyd resin, silicon wax, silicon resin, silicon modified resin, fluororesin, fluoromodified resin, polyvinyl alcohol, cellulose materials such as nitrocellulose, silica as a hardener, various waxes such as polyethylene wax, etc., and can be formed by mixing one or more selected materials. As a result of peeling with a release material, a heat transfer material, a hardening material, a breaking material, an interlayer bonding material, a pressure-resistant material, a lubricating material, a heat-resistant material, a gloss material, a substrate film 11 or a film protective layer 22 in the form of interfacial peeling or destructive peeling due to cohesive failure in the peeling layer 13 due to transfer heat pressure, the release agent cover formation on the next layer of the resin protective layer 14 and the assistance of physical and chemical resistance after transfer are necessary elements as well as the peeling ability. For this purpose, the release layer 13 may be multi-layered. Also, it may be multi-layered with differentiated functions. The release layer 13 is formed by drying a prepared solution prepared using a known film forming machine such as a gravure printing machine 60. The film thickness is 0.1 to 20 μm, preferably 0.1 to 10 μm.
[0097] Following the base film 11, a film protective layer 22, a peeling layer 13, a resin-based protective layer 14 containing a plasticizer or a color-changing resin-based protective layer 14 containing a plasticizer, a metal layer 15, a resin-based protective layer 23 containing a plasticizer, and an adhesive layer 16 are laminated in this order to form the transfer laminate 12 of the transfer foil 10. Each layer can be selectively adopted and combined to form the transfer foil 10. For example, it is possible to sequentially form a base film 11, a peeling layer 13, a selection of either a resin-based protective layer 14 containing a plasticizer or a color-forming resin-based protective layer 14 containing a plasticizer, a metal layer 15, and an adhesive layer 16, a base film 11, a film protective layer 22, a peeling layer 13, a resin-based protective layer 14 containing a plasticizer or a color-forming resin-based protective layer 14 containing a plasticizer, a metal layer 15, and an adhesive layer 16, or a base film 11, a peeling layer 13, a resin-based protective layer 14 containing a plasticizer or a color-forming resin-based protective layer 14 containing a plasticizer, a metal layer 15, a resin-based protective layer 14 containing a plasticizer, and an adhesive layer 16. These means reflect the effect of each resin-based protective layer 14 containing a plasticizer together with the metal layer 15 in adapting to the load of expansion and contraction and pressure that arise during thermal and pressure transfer.
[0098] The film protective layer 22 shown in Fig. 2 is formed under the following conditions. During heat and pressure transfer, the base film 11 expands or contracts due to the transmission of heat pressure. To suppress this, a hard film protective layer 22 is formed. To achieve stable and uniform peeling of the release layer 13 during transfer, a hard and smooth film protective layer 22 is formed between the base film 11 and the release layer 13. This allows pressure and heat to be transmitted equally during transfer, improving transfer peeling, transfer fixation, and breakability during image transfer and the like during transfer.
[0099] During thermal pressure transfer, the base film 11, the resin-based protective layer 14, the color resin-based protective layer 14, and the adhesive layer 16 all undergo film stretching. When a tensile stress is applied to the metal layer 15, causing the resin-based protective layer 14 and the adhesive layer 16 to stretch, cracks, breaks, bulges, etc. occur in the metal layer 15 or between the metal layer 15 and the resin-based protective layer 14. This results in a decrease in the brightness of the transferred laminate 12 due to a decrease in the brilliance of the metal layer 15 and bulging of the resin-based protective layer 14 due to heat yield during transfer, etc.
[0100] In the transfer lamination 21 in which the film protective layer 22, the peeling layer 13, the resin-based protective layer 14, the metal layer 15, the resin-based protective layer 23, and the adhesive layer 16 are laminated in sequence on the base film 11 to form a thermo-pressure transfer layer, a plasticizer is added to the resin-based protective layer 14 to prepare a liquid. The film protective layer 22 and the adhesive layer 16 are formed by coating using a gravure printer 60. Each process is dried by a far-infrared heater 67 and a hot air device 69 in the drying ovens 61 and 62 of the gravure printer 60. The protective layer 14 shrinks during heat treatment. The stress of the shrinkage is accumulated inside the film. A plasticizer is mixed into the protective layer 14. The plasticizer in the network structure film of the film formation is provided with flexibility in the hardening film. The protective layer 14 is provided with a buffering property against the generation of stress from external and internal forces. Therefore, the deformation of the protective layer 14 due to the expansion and contraction it receives can be reduced. The influence of breakage or shear on the metal layer 15 caused by the expansion and contraction of the interface between the protective layer 14 and the metal layer 15 or the protective layer 14 can be reduced or avoided.
[0101] The color resin protective layer 14 is a light-resistant layer, and dyes, inorganic pigments, organic pigments, etc. can be used as coloring materials. In addition, one or more types of acrylic resins containing hindered amine-based materials, which are light stabilizers, are added as weather-resistant materials. One or more types of hydroxyphenyl triazine-based materials, which are ultraviolet absorbing agents, are added. By containing phenyl salicylate as a light blocking agent, fading of the transfer laminate 21 can be suppressed, and the resistance can be extended.
[0102] The transfer shape of the transferee 32 ranges from a flat shape to a three-dimensional shape, and its material ranges from hard to soft, and when heating and pressing during transfer, an elongation and compression stress due to heating and pressing is applied between the transferee 32 and the transfer laminate 12. At the same time, the deposition layer, which is a metal granular deposition layer, in the metal layer 15 is stretched, and a force that inhibits the cohesion of the metal is generated, and as a result of the load being concentrated on the cohesion of the metal deposition layer or the metal island layer against the tensile stress of the protective layer 14, cohesion failure progresses, and from this point on, the transfer laminate 12 may progress to cracks, breaks, bulges, fissures, peeling, poor interlayer adhesion, foil removal due to poor interlayer adhesion, poor heat resistance, poor luster, poor weather resistance, etc.
[0103] In order to improve this situation, various experiments were conducted and it was found that by selectively adding a plasticizer to the liquid formulation of the resin-based protective layer 14, affinity is expressed in the correlation between the resin-based protective layer 14 and the metal layer 15. The interface fixation of the protective layer 14 and the metal layer 15, which contributes to suppressing the occurrence of cracks, breakage, blistering, etc., is enhanced, and a means is obtained that shows resistance to the occurrence of extension of the transfer laminate 12 during transfer. By incorporating into the process the addition of a plasticizer to the protective layer 14, a method of heat treatment of the protective layer, and a heat treatment, hot air treatment, pressure treatment, cooling treatment, annealing treatment, etc., in the state in which the protective layer 14 and the metal layer 15 are combined, the transfer laminate 12 comes to have heat resistance, flexibility, and extensibility, and can face and suppress the stress during transfer by thermal pressure transfer.
[0104] [Recipe 7] After forming the release layer 13 coated on the base film 11 by the gravure printing machine 60, the plasticizer-containing resin-based protective layer 14 becomes a thermosetting resin layer formed by amino resin, hardener, and acrylic resin. The addition of the plasticizer results in a flexible film. The preparation is heated by an infrared heater and a hot air device 69 in the first drying oven 61 of the gravure printing machine 60, and a film is formed. Next, a metal layer 15 is formed by a vacuum deposition device, and an adhesive is added.
[0105] [Recipe 8] After forming the release layer 13 coated on the base film 11 by the gravure printing machine 60, the plasticizer-containing resin-based protective layer 14 becomes a thermosetting resin layer formed by amino resin, hardener, and acrylic resin. The addition of the plasticizer results in a flexible film. The preparation is heated by an infrared heater and a hot air device 69 in the first drying oven 61 of the gravure printing machine 60, and a film is formed. Next, in the gravure printing machine 60 having a second drying oven 62, a dry film in which the release layer 13 and the protective layer 14 containing the plasticizer are laminated on the base film 11 is formed in a gravure printing machine 60 having a volume of 2.64 m. 3 An annealing treatment constituting baking is performed by operating at a temperature of 100 to 210°C and a residence time in the furnace of 20 to 50 seconds. Thereafter, a metal layer 15 and an adhesive layer 16 are formed. A transfer foil 10 including a transfer laminate 12 that decorates the surface layer of a transfer-receiving body 32 having a flat film layer structure is obtained.
[0106] [Recipe 9] After forming a release layer 13 coated on the base film 11 by a gravure printer 60, the plasticizer-containing resin-based protective layer 14 becomes a thermosetting resin layer formed by amino resin, hardener, and acrylic resin. Because a plasticizer is added, the film is flexible. Then, a metal layer 15 is formed. Then, a baking process is performed in a gravure printer 60 having a type 2 drying oven 62, similar to the above heat treatment. Then, an adhesive layer 16 is added. A transfer foil 10 is obtained, including a transfer laminate 12 that modifies the surface layer of a transferee 32 having a flat film layer structure.
[0107] [Recipe 10] After forming the peeling layer 13 coated on the base film 11 by the gravure printing machine 60, the resin-based protective layer 14 containing the plasticizer becomes a thermosetting resin layer formed by amino resin, hardener, and acrylic resin. Since the plasticizer is added, the film is flexible. Then, the metal layer 15 is formed. Then, the gravure printing machine 60 having the two-type drying furnace 62 performs baking treatment in the same manner as the above heat treatment. Through the outside furnace pressure device 71 and the outside furnace cooling device 72 directly connected to the drying furnaces 61 and 62, heat treatment, pressure treatment, and cooling treatment are performed, and the protective layer 14 becomes a hard, tough thermosetting film, and a flat film structure is formed in which the film quality having viscosity, flexibility, and extensibility is propagated to the metal layer 15. Then, the adhesive layer 16 is added. A transfer foil 10 including the transfer laminate 12 that modifies the surface layer of the transferee 32 is obtained.
[0108] [Recipe 11] After forming the peeling layer 13 coated on the base film 11 by the gravure printing machine 60, the resin-based protective layer 14 containing the plasticizer becomes a thermosetting resin layer formed by amino resin, hardener, and acrylic resin. Since the plasticizer is added, the film is flexible. Then, the metal layer 15 is formed. After this, the gravure printing machine 60 equipped with the drying furnace type 2 furnace 62 performs heating in the furnace and hot air treatment, pressurizes with the connected external furnace pressurizing device 71, and cools with the external furnace cooling device 72. An annealing treatment is performed to bake the dry film of the multilayer body including the base film 11, the peeling layer 13, the protective layer 14, and the metal layer 15. At this time, the heating of the drying furnaces 61 and 62 and the heat treatment with hot air are made in a high temperature region, and the peeling layer 13, the protective layer 14, and the metal layer 15 form a continuous three-dimensional structure layer having a fine uneven ridge-like wrinkled shape through pressurization and cooling. Then, the adhesive layer 16 is added. A transfer foil 10 is obtained, which includes a transfer laminate 12 that modifies the surface layer of a recipient 32 .
[0109] [Recipe 12] After forming the peeling layer 13 coated by the gravure printer 60 on the base film 11, the resin-based protective layer 14 containing the plasticizer becomes a thermosetting resin layer formed by amino resin, hardener, and acrylic resin. Since the plasticizer is added, the film is flexible. In the first type drying oven 61 of the gravure printer 60, the far-infrared heater 67 and hot air treatment are performed in the high temperature range. Then, the metal layer 15 is formed. Furthermore, in the second type drying oven 62 of the gravure printer 60, the far-infrared heater 67 and hot air treatment are performed in the high temperature range, followed by pressure treatment and cooling treatment, thereby forming a continuous three-dimensional structure layer in the form of fine ridges. Then, the adhesive layer 16 is added. A transfer foil 10 including a transfer laminate 12 that modifies the surface layer of the transferee 32 is obtained.
[0110] By controlling the temperature of the first furnace 61 and the second furnace 62 to a low temperature range of 100-160°C and a high temperature range of 140-210°C, a flat membrane structure is produced in the low temperature range and a three-dimensional membrane structure is produced in the high temperature range. The membrane structures can be produced separately as flat membrane structures and three-dimensional structures. The resin-based protective layer 14 is formed by processing with the gravure printing machine 60. Drying of the prepared solution, annealing, membrane modification, and membrane bonding can be performed through processing with the first drying furnace 61 and the second drying furnace 62, processing with the far-infrared heater 67, hot air processing, pressurization processing, and cooling processing.
[0111] [Recipe 13] The three-dimensional structure is a continuous membrane structure with a ridged shape. It is a continuous three-dimensional membrane with an arch-shaped cross section. It is a continuous three-dimensional structure with a cross section of a chord length of 10 to 70 μm, a height of 10 to 270 μm, and an arc length of 40 to 550 μm.
[0112] The photograph shown in Fig. 8 shows the surface of the transferred transfer laminate 12. The photograph on the right in Fig. 9 shows the surface of the transfer laminate 12 including a resin-based protective layer 14 that contains a plasticizer. The photograph on the left in Fig. 9 shows the surface of the transfer laminate 12 including a resin-based protective layer 14 that does not contain a plasticizer. The photograph in Fig. 10 shows an enlarged view of the uneven portion of the surface shown in Fig. 9.
[0113] The formation is carried out as follows. The peeling layer 13 is heated and dried on the base film 11 in the drying oven type 1 furnace 61 of the gravure printing machine 60 to form a film, then the resin-based protective layer 14 containing a plasticizer is heated and dried in the drying oven type 1 furnace 61 to form a film, then the metal layer 15 is formed using a two-chamber semi-continuous vacuum deposition machine via a high-frequency excitation plasma activation reactive device, and then the peeling layer 13, the protective layer 14, and the deposition film are formed on the base film 11 in the drying oven type 2 furnace 62 of the gravure printing machine 60, and the annealing treatment is performed in a high temperature range of 150 to 210 ° C., followed by continuous hot air treatment, outside furnace pressurization treatment, and outside furnace cooling treatment. In this machine, the peeling layer 13, the protective layer 14, and the deposition layer are integrated and stretched and raised to present a fine three-dimensional structure without damage. Next, the adhesive layer 16 is heated and dried using the drying oven type 1 furnace 61 of the gravure printing machine 60 to complete the three-dimensional film of the transfer laminate 12.
[0114] In the formation of the three-dimensional film, the interface between the protective layer 14 and the metal layer 15 is a film having excellent adhesion and affinity for interface fixation. In the above example, it has a continuous three-dimensional structure with a bow-shaped, arc-shaped cross section of 20 to 550 μm. The area of the film formed after the deposition film formation and the area after the process in the second type of drying oven 62 were compared and measured with the film included, and were found to be the same area. After the operations of heat treatment, hot air treatment, pressure treatment, and cooling treatment of the resin-based protective layer 14 containing a plasticizer and the metal layer 15 were performed, a three-dimensional film was formed, and the cross section of the bow-shaped arc showed 20 to 550 μm, which represents the stretching ratio. No cracks, breaks, bulges, etc. were observed in either the protective layer 14 or the metal layer 15 after stretching. There was no change in brightness after transfer.
[0115] The resin-based protective layer 14 containing the plasticizer is heated, heated air, pressurized, and cooled by the drying ovens 61 and 62 of the gravure printing machine 60, and becomes a thermosetting resin film with the amino resin, hardener, and acrylic resin, and the film is hardened. The plasticizer in the network structure film gives flexibility to the film. Furthermore, by using a plasticizer that induces migration into the film within a limit, multiple plasticizers with flexibility and migration inductivity are mixed and attached into the hardened film of the protective layer 14. This gives the protective layer 14 a film quality that changes from a hard and tough film quality to a film quality with flexibility and interface inductivity. The hard and tough protective layer 14 in the film becomes sticky, and the flexibility becomes elastic. The interface inductivity of the plasticizer leads to the interface of the protective layer 14 having affinity to the grain boundaries of the metal deposit layer and the isolated island layer of the metal layer 15. The plasticizer needs to maintain the heat resistance of the transfer laminate 12 in addition to its flexibility. During thermal transfer, the transfer laminate 12 must withstand the thermal load of transfer, prioritizing the generation of flexibility in the protective layer 14. The flexibility of the protective layer 14 is made apparent when pressure is applied outside the furnace, and affinity for the metal layer 15 is promoted together with a migration-inducing agent, and the adhesion at the interface between the protective layer 14 and the metal layer 15 is improved by cooling outside the furnace. At least one type of plasticizer must be added to the resin-based protective layer 14 to establish its function.
[0116] Furthermore, through the continuous operations of heating, hot air, pressure, and cooling by the gravure printing machine 60, the resin-based protective layer 14 containing a plasticizer is provided with heat resistance as a thermosetting resin film, and stress is removed by the annealing process and pressure for baking the dry film, and the plasticizer also generates flexibility, and the interface-inducing plasticizer in the film is guided to the interface of the metal layer 15 together with the flexible plasticizer. The heat-resistant, flexible, and extensible protective layer 14 is further enhanced by the generation of affinity at the interface and fixation of adhesion by forced pressure and forced cooling. The protective layer 14 and the metal layer 15 have heat resistance, flexibility, and extensibility in addition to being a hard and tough film quality, and are formed into a film that maintains adhesion between the layers.
[0117] Between the resin-based protective layer 14 containing a plasticizer and the metal layer 15, a plasticizer that imparts flexibility to the protective layer 14 and a plasticizer that acts on migration are selected. Furthermore, the plasticizer maintains heat resistance during transfer. By combining with the prevention of loss of affinity with the interface of the metal layer 15, the metal layer 15 undergoes metal plasticity modification through the operations of heating, hot air, pressure, and cooling, and affinity is increased due to the inductive effect of migration induction by the plasticizer in the formulation of the protective layer 14 along the metal deposit structure or metal island structure, and further intervenes with the metal layer 15, progressing to bonding, and further progressing the fixation between the layers.
[0118] Defects of the transfer foil 10 include insufficient peelability, poor film breaking accuracy, cracks, cracks, peeling, swelling, poor interlayer adhesion, defoiling due to poor interlayer adhesion, poor transfer heat resistance, poor luster, poor weather resistance, defoiling due to poor adhesion, insufficient slipperiness of the foil surface, discoloration, and poor film permeability that reduces the metallic effect. Of these, cracks, cracks, and swelling are phenomena that occur during transfer, leading to a drop in luster and defoiling factors over time, and damage to the aesthetic appearance. The transferred body 32 also undergoes dimensional changes over time due to humidity, temperature, and climate. These effects also impair the decorativeness of the transfer laminate 12, causing damage and defoiling.
[0119] 11 to 14 are photographs showing cracks, breaks, and bulges in the transferred laminate 12. FIG.
[0120] The transfer laminate 12 has layers with different functions, and is formed by selecting and applying materials. Each layer obtains the transfer conditions of heat sensitivity, pressure sensitivity, and time as the transfer foil 10, and the transfer laminate 12 is peeled off from the base film 11, and all layers have the same film breakability, accurately transferring the shape of the image of the plate-making material. In addition, the transfer object 32 includes general printing, paper containers, bookbinding, film sheets, electric wire tubes, resin processing molding, leather, textiles, wood, glass products, metal products, etc., and has a wide variety of shapes. The transfer shape ranges from a flat shape to a three-dimensional shape, and during transfer, the stress response and cohesive force between the transfer object 32 and the transfer foil 10 are affected, and are concentrated as expansion and contraction in the transfer laminate 12. This leads to the above-mentioned defects in the transfer foil 10.
[0121] In view of the above, this embodiment suppresses cracks, breaks, blistering, etc. in the transfer foil 10, and improves heat resistance, light resistance, etc. by selecting materials for the transfer laminate 12, improving the adhesion strength between layers, improving stretch resistance, and controlling the stress in each film.Extensive experiments were conducted to find countermeasures to problems that occur when the transfer laminate 12 is placed between the transfer equipment and the transferred body 32, and details are given below.
[0122] [Experiment 1] A polyester film having a thickness of 12 μm was used as the base film 11. A release layer 13 was formed on the base film 11. Specifically, a release agent consisting of 71.1% by weight of toluene (Idemitsu Kosan Co., Ltd.), 25% by weight of MIBK (methyl isobutyl ketone) (Mitsubishi Holdings Co., Ltd.), 0.03% by weight of ethylene glycol (Wako Pure Chemical Industries, Kyoto Co., Ltd.), 1.04% by weight of Fischer Trophic Wax (Sador Co., Ltd.; A859), and 0.9% by weight of acrylic resin (Nippon Shokubai Co., Ltd.; UV-G301) was prepared, and the release agent was applied and dried by a gravure printing machine 60 to form a release layer 13 having a thickness of 0.5 μm. A first furnace 61 of the gravure printing machine 60 was used, and the film was allowed to stay in a heating temperature of 100 to 120° C. for 20 to 50 seconds to produce a flat film (release layer 13) having a thickness of 0.5 μm.
[0123] Next, a resin-based protective layer 14 was formed on the release layer 13, prepared, and coated and dried by a gravure printing machine 60 to form a resin-based protective layer 14 having a thickness of 1 μm. The resin-based protective layer 14 was composed of 26.9% by weight of toluene (Idemitsu Kosan Co., Ltd.), 16.7% by weight of MEK (methyl ethyl ketone) (Idemitsu Kosan Co., Ltd.), 14.9% by weight of MIBK (methyl isobutyl ketone) (Mitsubishi Chemical Holdings Corporation), 0.04% by weight of ethylene glycol (Wako Pure Chemical Industries, Kyoto Co., Ltd.), 20.6% by weight of acrylic resin (Nippon Shokubai Co., Ltd.; UV-G301), 11.7% by weight of acrylic resin (Alpha Kaken Co., Ltd.; silicon acrylic silicate UVHA), 1.19% by weight of acrylic resin (Wilbur-Ellis; Paraloid AT740), and methyl ethyl ketone (Mitsubishi Chemical Holdings Corporation). A thermosetting resin-based protective layer 14 was prepared using 1.49 weight% lamin resin (MS-001, Nippon Carbide Corporation), 4.4 weight% ketone resin (Polyton K-97, Wally Corporation), 0.08 weight% UV absorber (Tinuvin 1600, BASF), 0.08 weight% UV absorber (Tinuvin 479, BASF), 0.08 weight% light stabilizer (Tinuvin 249, BASF), 0.08 weight% light blocking agent (phenyl salicylate, Tokyo Chemical Industry Co., Ltd.), and 0.03 weight% hardener (p-toluenesulfonic acid, Tokyo Chemical Industry Co., Ltd.).
[0124] The thermoplastic resin-based protective layer 14 was composed of the above-mentioned melamine resin and hardener excluded. Volume: 5.28 m 3 The first furnace 61 was used, and the material was left in a heating temperature range of 150 to 210° C. for 20 to 50 seconds to produce a flat film (thermoplastic resin-based protective layer 14) having a thickness of 1 μm.
[0125] Next, a metal layer 15 was formed using aluminum as the metal, with a coating thickness of 30 to 80 nm using a two-chamber semi-continuous vacuum deposition apparatus and a high-frequency induction heating metal melting heat source.
[0126] Next, an adhesive layer 16 was formed on the metal layer 15. 50.0% by weight of toluene (Idemitsu Kosan Co., Ltd.), 37.7% by weight of ethyl acetate (Showa Denko K.K.), 1.5% by weight of butyl acetate (Standard Oil Co., Ltd.), 0.07% by weight of ethyl silicate (Colcoat Co., Ltd.; Ethyl Silicate 100), 2.7% by weight of acrylic resin (Mitsubishi Chemical Co., Ltd.; Coponyl N2147), 2.7% by weight of ethylene vinyl acetate (Mitsubishi Chemical Co., Ltd.; Soarnol D2908), and 3.0% by weight of ketone resin (Wally Co., Ltd.; Polyton K-97) were used to prepare films with thicknesses of 1 μm and 2 μm by a gravure coater. Volume 5.28 m 3 The first furnace 61 was used, and the material was allowed to stand at a heating temperature of 100 to 120° C. for 20 to 50 seconds to produce flat films (adhesive layers 16) having thicknesses of 1 μm and 2 μm.
[0127] As described above, a transfer foil 10 including a thermosetting resin-based protective layer 14 and a transfer foil 10 including a thermoplastic resin-based protective layer 14 were produced. In addition, a transfer foil 10 including an adhesive layer 16 having a thickness of 1 μm and a transfer foil 10 including an adhesive layer 16 having a thickness of 2 μm were produced. Using a thermal pressure transfer machine 51, the occurrence of cracks in the transfer foil 10 was evaluated.
[0128] The resin-based protective layer 14 was thermosetting or thermoplastic, and the adhesive layer 16 was 1 μm or 2 μm thick. In addition, a top-bottom type transfer foil stamping machine 31 using a brass flat plate 30 or a top-bottom type transfer foil stamping machine 41 using a brass relief plate 40 was used, and a soft vinyl chloride sheet with a thickness of 0.9 mm was used as the transfer target 32, and the occurrence of cracks after transfer was confirmed. The photograph shown in FIG. 11 shows cracks, breaks, and swelling of the transfer foil 10. The photograph shown in FIG. 12 shows cracks in the transfer foil 10 on the transfer target 32 with unevenness. The photographs shown in FIG. 13 and FIG. 14 are enlarged views of the opening of the crack in the transfer foil 10.
[0129] The thermosetting and thermoplastic transfer laminate 12 is applied using the up-down transfer foil stamping machine 31 or 41, respectively, at a transfer temperature of 120°C or 160°C and a transfer pressure of 5 kg / cm 2The transfer was performed under the conditions of a transfer residence time of 0.5 seconds. The plasticizer content was 3.0% in both the thermosetting and thermoplastic resin-based protective layers 14. As a result, no cracks were observed on any of the transfer foils 10. No stretching of the soft vinyl chloride sheet was observed. The results are shown in Table 1. In the table, "◯" indicates good and "×" indicates poor. This is the same for the following tables.
[0130] [Table 1]
[0131] [Experiment 2] In addition, the change in the extension of the transferred body 32 and the effect on the transfer foil 10 by changing the transfer residence time were confirmed by setting them as follows. The transfer residence time was divided into three stages: 0.5 seconds, 0.75 seconds, and 1.00 seconds. The transfer temperature was 160°C, and the transfer pressure was 5 kg / cm. 2 The transfer machine was a top-bottom type transfer foil stamping machine 41 using a relief plate 40 (length 3 mm × width 6.75 mm × height 2 mm). The thickness of the adhesive layer 16 was 1 μm. The transfer laminate 12 was composed of a peeling layer 13, a resin-based protective layer 14, a metal layer 15, and an adhesive layer 16. However, the resin-based protective layer 14 was a thermosetting or thermoplastic resin. The preparation was the same as in the above experiment 1. After the transfer, the extension of the soft vinyl chloride sheet was confirmed, and when the transfer residence time was 0.5 seconds, there was no extension of the soft vinyl chloride sheet. When the transfer residence time was 0.75 seconds, the extension of the soft vinyl chloride sheet was 2% of the original transfer size. When the transfer residence time was 1.00 seconds, the extension was 8.2%. When the transfer foil 10 was checked for cracks, no cracks were confirmed for 0.5 seconds. Cracks were confirmed for 0.75 seconds and 1.00 seconds. The state of cracks in the transfer foil 10 is shown in Table 2. Here, the protective layer 14 was divided into a thermosetting layer and a thermoplastic layer, and the transfer residence time was divided into 0.5 seconds, 0.75 seconds, and 1.00 seconds.
[0132] Additionally, regarding the stretching of the soft polyvinyl chloride sheet during transfer, the stretched portion of the soft polyvinyl chloride sheet was measured from the transfer plate and the edge of the transfer plate, and the crack opening width (μm) was measured, and these are shown in Table 2. When the transfer dwell time was 0.5 seconds, no cracks occurred. When the transfer dwell time was 0.75 seconds, the soft polyvinyl chloride sheet stretched by 2%, and the opening width was 7μm. When the transfer dwell time was 1.00 seconds, the soft polyvinyl chloride sheet stretched by 8.2%, and the opening width was 282μm. From these results, it was found that when the transfer conditions of heating, pressure, and time are applied to the soft vinyl chloride sheet, which is the transfer object 32, and the cycle of releasing the pressure and returning to room temperature causes the metal layer 15 of the transfer laminate 12 to be affected by the tensile stress and compressive stress caused by the expansion and contraction of the soft vinyl chloride sheet, cohesive failure progresses to the metal layer 15, which has weak cohesive strength, and the stress of fracture progresses from the fracture of the metal layer 15 to the interface of the protective layer 14 and to the protective layer 14, resulting in the generation of cracks. In both the thermosetting and thermoplastic resin-based protective layer 14, and in both the transfer residence time of 0.75 seconds and 1.00 seconds, cracks occurred. The results are shown in Table 2. When the protective layer 14 did not contain a plasticizer, both the crack opening width and the elongation rate were extremely large.
[0133] [Table 2]
[0134] [Experiment 3] From the results of the above experiment 2, it was found that cracks occurred when the transfer residence time was 0.75 to 1.00 seconds. In order to improve this, it is necessary to equip the transfer foil 10 with a means for responding to the expansion and contraction of the transferee 32. The transferee 32 has a wide variety of materials and shapes, including flat surfaces, three-dimensional surfaces, hard materials, soft materials, organic materials, and inorganic materials. It is necessary to respond to deformations such as distortion, expansion, contraction, deviation, twisting, bending, and inclination caused by various stresses such as external and internal forces that are generated during transfer between the transferee 32 and the transfer stack 12. The transfer stack 12 cannot withstand the interference deformation and expansion that occurs between the transfer operation and the transferee 32, leading to film rupture and shear. The transfer stack 12 is a film with transfer rupture properties, and it is difficult to maintain the film properties due to the effects of the expansion and contraction of the transferee 32 and the action of various stresses caused by transfer. Here, a study was conducted on a form that could withstand cracks and maintain stretchability while maintaining the fracture shear strength of the transfer laminate 12.
[0135] Among the plasticizers mentioned above, additive materials that can maintain resistance to the effect of the deformation of the transfer laminate 12 caused by the transfer stretching of the soft vinyl chloride sheet on the occurrence of cracks in the transfer foil 10 were selected for use in the preparation of the resin-based protective layer 14. Functions that can be obtained when added as additives to the resin-based protective layer 14, color-changing resin-based protective layer 14, etc. include flexibility, extensibility, transparency, and compatibility with other materials, no interlayer adhesion inhibition, no whitening phenomenon or interface deterioration after component transfer, no change over time, no change in heat resistance, and no effect on the breakability of the film. In order to select these, each layer was laminated in order on the base film 11 to prepare the transfer foil 10.
[0136] The base film 11 is laminated with a release layer 13, a resin-based protective layer 14, a metal layer 15, an adhesive layer 16, etc., and at the interface of the metal layer 15, which has weak cohesion, there is the resin-based protective layer 14 and the adhesive layer 16. By improving the extensibility of the resin-based protective layer 14, it is possible to prevent deformation of the transfer laminate 12. A thermosetting film is used as an inhibitor of cracks caused by plastic deformation of the film, and a plasticizer is added to obtain flexibility and extensibility as well as to prevent a drop in the softening point and shearing of the film.
[0137] A release layer 13 was formed on a 12 μm thick polyester base film 11 in the same manner as in Experiment 1 above, and then a resin-based protective layer 14 was formed thereon. The resin-based protective layer 14 contained 26.9% by weight of toluene (Idemitsu Kosan Co., Ltd.), 17.2% by weight of MEK (Idemitsu Kosan Co., Ltd.), 14.9% by weight of MIBK (methyl isobutyl ketone) (Mitsubishi Chemical Holdings Corporation), 0.04% by weight of ethylene glycol (Wako Pure Chemical Industries, Ltd.), 20.6% by weight of acrylic resin (Nippon Shokubai; UV-G301), 11.7% by weight of acrylic resin (Alpha Kaken; UVHA), 1.19% by weight of acrylic resin (Wilbur-Ellis; Paraloid AT-740), and 1.49% by weight of melamine resin. % by weight (Nippon Carbide Corporation; MS001), 4.4 wt % by weight of ketone resin (Wally Corporation; Polyton K97), 0.08 wt % by weight of UV absorber (BASF; Tinuvin 1600), 0.08 wt % by weight of UV absorber (BASF; Tinuvin 479), 0.08 wt % by weight of light stabilizer (BASF; Tinuvin 249), 0.08 wt % by weight of light blocking agent (Tokyo Chemical Industry Co., Ltd.; phenyl salicylate), 0.03 wt % by weight of hardener (Tokyo Chemical Industry Co., Ltd.; p-toluenesulfonic acid), and 1.0 wt % by weight of plasticizer were added.
[0138] As the plasticizer, the following (1) to (5) were selected. (1) Paraffins (Nippon Seiro Co., Ltd.; ParaffinWax 115) (2) Low molecular weight polyesters (Mitsubishi Chemical Corporation; adipic acid polyester D620) (3) Phosphate esters (Tokyo Chemical Industry Co., Ltd.; Phosphate ester PO271) (4) Sulfonamides (Fujifilm Wako Pure Chemical Industries, Ltd.; benzenesulfonamide) (5) Ethylene olefins (Idemitsu Kosan Co., Ltd.; Linearene 6)
[0139] The coating agent is a type 1 furnace 61 (volume 5.28 m) for a gravure printing machine 60. 3) was used, and the film was formed by passing it through an atmosphere of 150 to 210°C for 20 to 50 seconds. The film thickness was set to 1 μm. Next, similarly to the above-mentioned experiment 1, a metal layer 15 and an adhesive layer 16 were formed, and a transfer foil 10 having a flat film structure was produced. Next, a top-bottom transfer foil stamping machine 41 equipped with a relief plate 40 was used to perform heat and pressure transfer onto a soft vinyl chloride sheet, and the base film 11 was peeled off to confirm the transferred appearance.
[0140] The following functions were evaluated as the evaluation items of the plasticizer. 1: Compatibility with other ingredients when mixing 2: Transparency of the film (transparency of the coating film during coating) 3: Flexibility of film formation (cracks in foil caused by transfer device letterpress printing, soft vinyl chloride sheet transfer material) 4: Flexibility of the transfer laminate 12 (cracks in the foil caused by the transfer device letterpress printing, soft vinyl chloride sheet transfer material) 5: Heat resistance of the transfer laminate 12 (transfer device letterpress plate making, temperature 160°C, transfer residence time 0.5 seconds, transfer pressure 5 kg / cm 2 , transfer material, soft vinyl chloride sheet, attenuation of brilliance) 6: Breakability of the transfer laminate 12 (breakage of the transfer film of the image during transfer, state of shear shape) 7: Compatibility at both interfaces of the protective layer 14 (affinity at the interface of adjacent layers, by peeling with adhesive tape) 8: Elasticity of the transfer laminate 12 (transfer device letterpress plate making, temperature 160°C, transfer residence time 0.75 seconds, transfer pressure 5 kg / cm 2 , whether or not cracks appear on the image on the soft vinyl chloride sheet 9: Interlayer adhesion at both interfaces of the protective layer 14 (confirmed by placing upper and lower adhesive tapes inside the transfer layer and peeling the interface state by a 180°C peel test) 10: Migration of plasticizer (Put two transfers on a soft vinyl chloride sheet together, apply a 500g load, place in a thermo-hygrostat at 160℃ for 48 hours, then return to room temperature and check for peeling)
[0141] Table 3 shows the judgment contents and results.
[0142] [Table 3]
[0143] (a) Paraffin-based and (b) low molecular weight polyester-based are particularly poor in flexibility, so they may be excluded from the selection. (c) Phosphate-based is poor in flexibility, so they may be excluded from the selection. (d) Toluenesulfonamide-based showed no abnormalities in all evaluation items. Specifically, characteristics were observed in flexibility and heat resistance, but no abnormalities were observed in extensibility, elasticity, interlayer adhesion, and migration. (e) Ethylene olefin-based showed abnormalities in extensibility, elasticity, interlayer adhesion, and migration, but the characteristic of interface induction was observed in migration. The amount of this material added was determined so that the affinity of the protective layer 14 to the metal layer 15 was improved, and the effect was confirmed. As a result, (d) Toluenesulfonamide-based was good in all evaluation items. (e) Ethylene olefin-based was selected to reconfirm interface induction. As mentioned above, it is preferable to select (d) Toluenesulfonamide-based and (e) Ethylene olefin-based.
[0144] [Experiment 4]
[0145] We selected protective layers 14 containing (d) toluenesulfonamide-based and (e) ethylene olefin-based plasticizers. In order to confirm the changes in the transfer laminate 12 affected by heat in these two respects, we produced a transfer laminate 12 with a flat membrane structure and conducted a heat resistance test. The test contents included evaluation of the transfer pressure, transparency, heat resistance, elasticity, interlayer adhesion, migration, etc., to see whether the results would lead to cracks, breaks, blistering, etc. of the transfer foil 10.
[0146] The heat resistance was evaluated as follows: An acrylic binder film 10 cm long, 3 cm wide, and 1 μm thick was printed and coated by silk screen onto a transparent glass plate 10 cm long, 10 cm wide, and 0.5 cm thick, and the dried resin film was used as the transfer target 32.
[0147] A transfer foil 10 was prepared by providing a release layer 13 on a base film 11 and including a thermosetting protective layer 14 containing a toluenesulfonamide-based plasticizer (d) in the protective layer 14. Furthermore, a transfer foil 10 was also prepared by including a protective layer 14 containing an ethylene olefin-based plasticizer (e) in the protective layer 14.
[0148] The above two types of transfer foils 10 were thermally and pressure-transferred using a roll-type thermal transfer machine 51 shown in Fig. 5. The transfer machine 51 uses a silicone rubber roller as a heating and pressurizing medium, and applies a transfer line pressure of 0.5 kg / cm to the acrylic resin layer formed on the glass. 2 The transfer was performed under the conditions of a foil feed speed of 2.5 m / sec and a roller heat temperature of 200°C. Two hours after the transfer, five samples of each of the above two types of samples transferred onto the glass substrate were stored in a thermostatic chamber. The temperature was raised from room temperature to 380°C over 200 minutes, and then the samples were allowed to stay there for five minutes and then cooled to room temperature over 150 minutes. After 12 hours had passed since the temperature was lowered, the samples were removed and the transfer laminate 12 on the samples was checked. The effects of the added plasticizer were identified and evaluated from the visual results in terms of gloss attenuation due to changes in transparency, effects on the metallizing effect, inhibition of adhesion due to migration of the plasticizer within the protective layer 14, cracks occurring in the transfer laminate 12, cracks occurring between the transferee 32 and the transfer laminate 12, and swelling occurring in the transfer laminate 12.
[0149] For (d) toluenesulfonamide-based plasticizers, no defects were observed in terms of brightness, adhesion, cracking, breakage, blistering, etc. For (e) ethylene olefin-based plasticizers, in terms of adhesion, a cellophane tape peeling test showed partial interlayer peeling between the release layer 13 and the protective layer 14, and between the protective layer 14 and the metal layer 15. (d) toluenesulfonamide-based plasticizers remained within the protective layer 14, while (e) ethylene olefin-based plasticizers showed migration within the thermoset film of the protective layer 14.
[0150] The above evaluation results are shown in Table 4.
[0151] [Table 4]
[0152] Five samples were prepared for each test. The evaluation results are shown in Table 4.
[0153] [Evaluation method] Heat resistance: Using a thermal transfer machine 51, temperature 160℃, transfer line pressure 0.5Kg / cm 2 The transfer was performed with a transfer residence time of 0.5 seconds. Glitter: Temperature 160℃, transfer line pressure 0.5Kg / cm 2 After the transfer was performed with a transfer residence time of 0.5 seconds, the transfer was visually confirmed. Adhesion: Confirmed by a 180-degree peel test using 15 mm wide adhesive tape. Crack occurrence: The specimen was visually inspected at 500x magnification. Crack occurrence: The specimen was visually inspected at 500x magnification. Blistering: The specimen was visually inspected at 500x magnification.
[0154] [Evaluation Results] (d) Toluenesulfonamide type: No problems were observed during heat treatment. (e) Ethylene olefin type: Problems with adhesion such as delamination occurred.
[0155] [Experiment 5] As for the results of the above-mentioned Experiment 4, for the (e) ethylene olefin-based plasticizer, a phenomenon of partial interlayer peeling occurred at both interfaces of the protective layer 14. The protective layer 14 in which the plasticizer was dispensed was a thermosetting film, and it was shown that the (e) ethylene olefin-based plasticizer migrated and reached both interfaces of the release layer 13 and the metal layer 15 without being blocked by the aggregated resin chains in this film.
[0156] The amount of additive was specified to complement the film structure by reducing the elasticity of the protective layer 14, maintaining its breakability, increasing its extensibility, imparting flexibility while maintaining migration inductivity, and maintaining interfacial adhesion.
[0157] The amounts of (e) ethylene olefin plasticizer added to the protective layer 14 were set to 0.075 wt %, 0.05 wt %, and 0.025 wt % and prepared to form the transfer laminate 12, thereby producing the transfer foil 10 with a flat membrane structure.
[0158] As described above, the glass substrate was resin-processed, roll-transferred, and placed in a thermostatic chamber, then removed and the performance was confirmed in the same manner as described above. The results are shown in Table 5. In the table, "△" indicates that the product is not defective but contains defects.
[0159] (e) It was found that an ethylene olefin-based plasticizer is effective without causing any change in adhesion when the upper limit of its amount is set to 0.025% by weight. It can be used as an interlayer flexibility propagation agent for the resin-based protective layer 14 together with other plasticizers as a flexibility propagation agent for the migration induction of materials, etc.
[0160] The above evaluation results are shown in Table 5.
[0161] [Table 5]
[0162] [Evaluation method] Heat resistance: confirmed by visual inspection. Adhesion: After removing from the thermostatic chamber, a 180-degree peel test was performed using 15 mm wide adhesive tape. Crack occurrence: The specimen was visually inspected at 500x magnification. Crack occurrence: The specimen was visually inspected at 500x magnification. Blistering: The specimen was visually inspected at 500x magnification.
[0163] [Evaluation Results] Heat resistance: There was no change in brilliance, and all showed good results. Interlayer adhesion: poor when added at 0.075% by weight, defective when added at 0.05% by weight, and good when added at 0.025% by weight. (e) When the ethylene olefin plasticizer was added in an amount of 0.025% by weight, adhesion, cracking, breakage, and blistering were visually checked after the heat resistance test, and it was confirmed that the resistance could be maintained without causing any deterioration of the film.
[0164] [Experiment 6] Through the above process, a phenomenon occurred in which the (e) ethylene olefin plasticizer migrated to the layer interface in the thermosetting resin film in the protective layer 14 of the thermosetting resin film. This led to interfacial peeling of the protective layer 14. Furthermore, as a result of trying to adjust the amount of addition, with the upper limit of the amount added being 0.025 wt %, no abnormal peeling of the interlayer adhesion occurred, and it became possible for the plasticizer to be involved in migration induction in the protective layer 14.
[0165] It has been confirmed in Experiment 3 that, as the plasticizer contained in the protective layer 14, a phosphoric acid ester-based, toluenesulfonamide-based, or ethylene olefin-based plasticizer can be used in terms of heat resistance.
[0166] The effect of adding a plasticizer is to generate flexibility in the protective layer 14, and to induce the transfer of flexibility to the interface of the protective layer 14, thereby raising the affinity of the interface of the protective layer 14 with the metal layer 15 in terms of bonding. By adding a plasticizer to modify the interface of the protective layer 14 through heat treatment by the gravure printing machine 60, miscibility, transparency, breakability, compatibility, flexibility, heat resistance, and migration inductivity are created in the thermosetting film. The expansion of the temperature range of the protective layer 14 containing the plasticizer reaches the interface in the curable film of the protective layer 14. When the tough thermosetting film of the protective layer 14 is modified to a flexible film by maintaining its heat resistance, migration inductivity is a necessary condition for the plasticizer to be contained.
[0167] By adding 1 wt% of the plasticizer benzenesulfonamide (Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.025 wt% of the plasticizer ethylene olefin resin (Idemitsu Kosan Co., Ltd.; Linearene 6) to the preparation of the thermosetting resin-based protective layer 14 in Experiment 1, flexibility, heat resistance, and migration inductivity were imparted, and a peel layer 13, protective layer 14, metal layer 15, and adhesive layer 16 were formed, producing a transfer laminate 12 with a flat membrane structure.
[0168] The processing on the glass substrate was carried out in accordance with the processing described in Experiment 4, and a thermal transfer was performed using a roll-type transfer device, a heat resistance test was performed by placing the sample in a thermostatic chamber, and the sample was removed and checked. No cracks, breaks, or swelling were observed. The results are shown in Table 8. The coating film formed using the first type drying oven 61 of the gravure printing machine 60 was made by adding (d) a toluenesulfonamide plasticizer and (e) an ethylene olefin plasticizer to the tough thermosetting resin film, which gave it flexibility, heat resistance, and flexibility migration inductivity.
[0169] The above evaluation results are shown in Table 6.
[0170] [Table 6]
[0171] [Evaluation method] A resin coating was applied to a glass substrate, which was then transferred using a roll transfer method. The substrate was then placed in a thermostatic chamber, heated from room temperature to 380°C, and left there for 5 minutes. After cooling to room temperature, the resistance was confirmed. The rest of the experiment was carried out in the same manner as in Experiment 2 above. Interface adhesion after heat resistance test: A 180-degree peel test was performed using a 15 mm wide adhesive tape. Crack occurrence: The specimen was visually inspected at 500x magnification. Crack occurrence: The specimen was visually inspected at 500x magnification. Blistering: The specimen was visually inspected at 500x magnification.
[0172] [Evaluation Results] As shown in Table 6, the results of the heat resistance test showed that no defects were observed in the interfacial adhesion between the protective layer 14 and the release layer 13 or the metal layer 15. No deterioration such as cracks, breakage, or blistering was observed.
[0173] [Experiment 7] A protective layer 14 was prepared by adding 1% by weight of a benzenesulfonamide-based plasticizer and 0.025% by weight of an ethylene olefin-based plasticizer. This was used to form a resin-based protective layer 14. A transfer laminate 12 having a flat membrane structure consisting of a release layer 13, a protective layer 14, a metal layer 15, and an adhesive layer 16 was formed on a base film 11 to prepare a specimen. This specimen was used to perform heat and pressure transfer onto a soft vinyl chloride sheet using a top-bottom transfer foil stamping machine 41 with a relief plate 40 (3 mm long x 6.75 mm wide x 2 mm high). The transfer temperature was 160°C, and the transfer pressure was 5 kg / cm. 2 The transfer residence time was varied according to the procedure. The ability of the transfer laminate 12 to conform to the stretching of the soft vinyl chloride sheet was confirmed. Table 7 shows the results of the stretching during transfer to the soft vinyl chloride sheet and the occurrence of cracks.
[0174] At a dwell time of 0.5 seconds, no stretching of the soft polyvinyl chloride sheet was observed, no openings appeared, and no cracks or breakage was observed. At a dwell time of 0.75 seconds, there was a 2.4% stretch and the crack opening width was 8.4μm. At a dwell time of 1.00 seconds, there was a 11.48% stretch and the crack opening width was 394μm.
[0175] Furthermore, in order to confirm the expansion of the soft vinyl chloride sheet and the occurrence of openings and cracks in the transfer laminate 12 during thermal pressure transfer, the transfer residence time was set to 0.58 seconds, 0.66 seconds, and 0.74 seconds between 0.5 seconds and 0.75 seconds. As a result, at a transfer residence time of 0.58 seconds, the sheet expanded 0.8% and the opening width was 0 μm. At a transfer residence time of 0.66 seconds, the sheet expanded 1.6% and the opening width was 5.6 μm. At a transfer residence time of 0.74 seconds, the sheet expanded 2.4% and the opening width was 8.4 μm. It was found that the transfer laminate 12 of the flat membrane structure including the protective layer 14 containing a plasticizer can withstand up to 0.8% of the expansion that occurs in the soft vinyl chloride sheet at a transfer residence time of 0.58 seconds in terms of the followability of the transfer laminate 12 to the expansion of the soft vinyl chloride sheet.
[0176] The above evaluation results are shown in Tables 7 to 9.
[0177] [Table 7]
[0178] [Table 8]
[0179] [Table 9]
[0180] For the protective layer 14, one or more selected plasticizers were added during preparation. The protective layer 14 and metal layer 15 had good adhesion with each other, and the elongation of both layers was observed during the course of experiment 7, as shown in Table 7. At a transfer residence time of 0.58 seconds, the elongation rate of the polychlorinated soft vinyl sheet was 0.8%, and no cracks were observed in the transfer foil 10 to which two types of plasticizers were added. This was due to the effect of the plasticizer on the resin-based protective layer 14, and it was found that it followed the elongation of the transfer target 32.
[0181] The flexibility of the protective layer 14 containing a plasticizer can weaken the internal stress applied during film formation, thereby simultaneously weakening film rupture and film shear stress on the metal layer 15. It can mitigate cracks, breaks, bulges, etc. of the transfer laminate 12 that occur due to cohesive failure in the metal layer 15 caused by elongation that occurs in the transferee 32 and elongation that occurs in the transfer laminate 12 during transfer. If the transferee 32 shows an elongation of 0.8% or more, the internal stress and rupture shear stress applied to the protective layer 14 and metal layer 15 cannot be weakened, and there is a risk of loss of luster and removal of foil from the transferee 32 over time.
[0182] 11 to 14 are photographs of cracks, breaks, blisters, etc.
[0183] Examples of the base film 11 include polyesters such as polyethylene terephthalates, polypropylene, polycarbonate, vinyl chloride, polystyrene, polyethylene, and polyimide. The thickness of the film is selected from the range of 12 to 75 μm. A release layer 13 is provided between the base film 11 and the protective layer 14. It is a layer made of resins and waxes, and polyethylene resins, polypropylene resins, polystyrene resins, vinyl chloride resins, polyester resins, acrylic resins, urethane resins, melamine resins, epoxy resins, fluorine resins, waxes, etc. can be used, and may be a single material or a mixture of one or more types. The thickness of the release layer 13 is preferably 0.1 to 10 μm. The protective layer 14 is a preparation using one or more types of acrylic resins, melamine resins, ketone resins, hardeners, ultraviolet absorbers, light stabilizers, light blocking agents, dyes, pigments, inorganic agents, and plasticizers. The thickness is preferably 1 to 20 μm. The metal layer 15 may be an alloy using one or more metals such as Ag, Cu, Sn, In, Al, Ni, Cr, Si, Zn, In2O3, CdO, CdIn2O4, Cd2SnO4, TiO2, SnO2, ZnO, SiO2, ZrO2, ZnS, MgF2, etc. The thickness of the metal layer 15 is preferably 20 to 60 nm. The metal layer 15 can be formed by wet plating, dry plating, or chemical plating. Taking into consideration the fixation between the resin-based protective layer 14 and the metal layer 15, dry plating is selected. Specifically, examples of the method include deposition such as vacuum deposition, electron beam deposition, and chemical deposition, and sputtering. The adhesive layer 16 has a function of adhering the transferred body 32 and the transfer laminate 12 (modified laminate), and examples of the adhesive include acrylic resins, chlorinated polypropylene resins, vinyl chloride acetate resins, and polyester resins. A mixture of one or more types of preparations may be used, and the thickness of the adhesive layer 16 is preferably between 1 and 10 μm. The transfer object 32 may be resin, metal, wood, leather, fiber, etc. A gravure printing machine 60 is used for the release layer 13, protective layer 14, and adhesive layer 16. A two-chamber semi-continuous vacuum deposition device is used for the metal layer 15.
[0184] Transfer lamination (modified lamination) 12 A film protective layer 22 may be provided between the base film 11 and the release layer 13. It is applied using a gravure printing machine 60 using a melamine resin and a sulfonic acid hardener selected from among amino resins and hardeners. It is used to ensure the smoothness of the surface of the base film 11 and the uniformity of the release properties. The film is adhered to the base film 11. The thickness is preferably between 0.5 and 5 μm.
[0185] A resin-based protective layer 14 can be provided between the metal layer 15 and the adhesive layer 16. In a structure of a base film 11, a release layer 13, a resin-based protective layer 14, a metal layer 15, a resin-based protective layer 14, and an adhesive layer 16, cohesive failure of the metal layer 15 can be further avoided by using the same protective layer 14 for both layers. A color-developing resin-based protective layer 14 using a coloring agent can be provided between the release layer 13 and the metal layer 15. Furthermore, the resin-based protective layer 14 can be laminated. The metal layer 15 can also be removed to form a transfer laminate 12.
[0186] [Experiment 8] A polyester base film having a thickness of 12 μm was used as the substrate film 11, and a release layer 13 was formed thereon. 3 The gravure printing machine 60, which had a capacity of 100 to 140°C, was used to form a film having a thickness of 0.5 to 0.8 μm by using a far-infrared heater 67 and a hot air device 69, with the running residence time in the oven being within a range of 20 to 50 seconds. The liquid preparation was the same as in Experiment 1. The protective layer 14 was formed in a drying oven type 1 oven 61 (volume 5.28 m 3A gravure printing machine 60 having a 1000-2000°C oven was used, and the machine was run for 20-50 seconds in a furnace with a temperature of 150-210°C using a far-infrared heater 67 and a hot air device 69 to produce a flat film with a thickness of 1-2 μm. The liquid preparation for the protective layer 14 was a thermosetting resin film, as in Experiment 1. As a plasticizer, 1% by weight of benzenesulfonamide (Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.025% by weight of ethylene olefin resin (Idemitsu Kosan Co., Ltd. Linearene 6) were added. Then, the metal layer 15 was formed. Using a two-chamber semi-continuous vacuum deposition device and a high-frequency induction heating metal melting heat source, the protective layer 14 was covered with aluminum with a thickness of 40-60 nm. Next, the adhesive layer 16 was formed. The formulation was the same as in Experiment 1. A film was formed to a thickness of 1 μm in the drying furnace type 1 furnace 61 of the gravure printing machine 60 at a furnace temperature of 80-110°C for a residence time of 20-50 seconds.
[0187] Using this flat film structure transfer foil 10, ten glass test pieces as described in Experiment 4 were prepared and transferred using a roll-type transfer machine 51. The test pieces were then placed in a thermostatic chamber and subjected to a heat resistance test. The temperature was raised from room temperature to 380°C over 200 minutes, after which the test pieces were allowed to stay there for five minutes, and then cooled to room temperature over 150 minutes. After 12 hours at a constant temperature, the test pieces were removed and the transfer laminate 12 on the test pieces was checked. Visual inspection was performed to check for cracks, breaks, swelling, and gloss loss, and no abnormalities were found.
[0188] [Experiment 9] A polyester base film having a thickness of 12 μm was used as the substrate film 11, and a release layer 13 was formed thereon. 3 The gravure printing machine 60, which had a capacity of 100 to 140°C, was used to form a film with a thickness of 0.5 μm to 0.8 μm by using a far-infrared heater 67 and a hot air device 69, with a running residence time in the oven of 20 to 50 seconds. The liquid preparation was the same as in Experiment 1. The protective layer 14 was formed in a drying oven type 1 oven 61 (volume 5.28 m 3) was used, and the machine was run for 20 to 50 seconds in a furnace temperature of 150 to 210°C using a far-infrared heater 67 and a hot air device 69 to produce a flat film with a thickness of 1 to 2 μm. The liquid preparation for the protective layer 14 was a thermosetting resin film, as in Experiment 1. As a plasticizer, 1% by weight of benzenesulfonamide (Fuji Film Wako Pure Chemical Industries, Ltd.) and 0.025% by weight of ethylene olefin resin (Linearene 6, Idemitsu Kosan Co., Ltd.) were added. Then, using a gravure printing machine 60 with a drying furnace type 2 furnace 62, an annealing treatment was performed to bake the dry film, which required a residence time in the furnace of 20 to 50 seconds in a furnace temperature of 100 to 210°C. Then, a metal layer 15 was formed. The protective layer 14 was covered with aluminum with a thickness of 40 to 60 nm using a two-chamber semi-continuous vacuum deposition device and a high-frequency induction heating metal melting heat source. Next, an adhesive layer 16 was formed. The formulation was the same as in Experiment 1. A film was formed to a thickness of 1 μm in a type 1 drying furnace 61 of a gravure printing machine 60 at an internal temperature of 80 to 110° C. with a residence time of 20 to 50 seconds.
[0189] Using this flat film structure transfer foil 10, ten glass test pieces shown in Table 2 were prepared and transferred using a roll-type transfer machine 51. The test pieces were then placed in a thermostatic chamber and subjected to a heat resistance test. The temperature was raised from room temperature to 380°C over 200 minutes, after which the test pieces were allowed to stay there for five minutes, and then cooled to room temperature over 150 minutes. After 12 hours at a constant temperature, the test pieces were removed and the transfer laminate 12 on the test pieces was checked. Visual inspection was performed to check for cracks, breaks, swelling, and gloss loss, and no abnormalities were found in any of the cases.
[0190] [Experiment 10] A polyester base film having a thickness of 12 μm was used as the substrate film 11, and a release layer 13 was formed thereon. A resin-based protective layer 14 was formed using a gravure printing machine 60 having a drying oven type 1 furnace 61. Then, a metal layer 15 was formed using aluminum. Then, using a drying oven type 2 furnace 62 of the gravure printing machine 60, the substrate film 11, the release layer 13, the protective layer 14, and the metal layer 15 were heated and annealed under the conditions of an in-furnace temperature of 150 to 210° C. and a running residence time in the furnace of 20 to 50 seconds. Then, an adhesive layer 16 was formed in the same manner as above. A transfer laminate 12 having a flat membrane structure was obtained. A heat resistance test was performed in the same manner as above. Visual inspection was performed for cracks, breaks, swelling, and gloss attenuation, and no abnormalities were observed in any of them.
[0191] [Experiment 11] A polyester base film having a thickness of 12 μm was used as the substrate film 11, and a release layer 13 was formed thereon. A resin-based protective layer 14 was formed using a gravure printing machine 60 having a first-type drying oven 61. Then, a metal layer 15 was formed using aluminum. Then, using a second-type drying oven 62 of the gravure printing machine 60, the substrate film 11, the release layer 13, the protective layer 14, and the metal layer 15 were heated and baked under the conditions of an oven temperature of 150 to 210° C. and a running residence time in the oven of 20 to 50 seconds. In addition to the heating treatment using the far-infrared heater 67 in the oven, hot air of 100 to 140° C. was blown into the oven by a hot air device 69. Furthermore, an external pressure device 71 directly connected to the oven was used to apply a transfer line pressure of 10 to 50 kg / cm. 2 The substrate film 11, the release layer 13, the protective layer 14, and the metal layer 15 were passed between the metal rolls that were kept at 5 to 15°C and the EPDM rolls that were pressed against each other. Next, using an external furnace cooling device 72, the substrate film 11, the release layer 13, the protective layer 14, and the metal layer 15 were passed between the metal rolls that were kept at 5 to 15°C and the Si rolls that were pressed against each other. Thereafter, the adhesive layer 16 was formed in the same manner as above. A transfer laminate 12 having a flat membrane structure was obtained. A heat resistance test was performed in the same manner as above. Visual inspection was performed for cracks, breaks, swelling, and gloss reduction, and no abnormalities were observed in any of the results.
[0192] [Experiment 12] In the film-forming operation similar to that of Experiment 11, the heating temperature of the drying oven 2 type 62 of the gravure printing machine 60 was set to 180 to 210°C, and the hot air was set to 120 to 140°C. By performing annealing, pressurization, and cooling, a continuous three-dimensional structure with uneven ridges and wrinkles was obtained. A heat resistance test was performed similar to the above. The visual results were examined for cracks, breaks, swelling, and gloss reduction, and no abnormalities were observed.
[0193] 23 to 25 are enlarged photographs of the surface of the three-dimensionally structured transferred laminate 12 after transfer. The parabolic arched cross section was as follows. That is, in FIG. 23, the chord length was 22.30 μm, the height was 13.87 μm, and the arc length was 37.25 μm. In FIG. 24, the chord length was 21.96 μm, the height was 35.98 μm, and the arc length was 66.29 μm. In FIG. 25, the chord length was 66.29 μm, the height was 267.30 μm, and the arc length was 542.70 μm.
[0194] The films formed by the peel layer 13, protective layer 14, metal layer 15, and adhesive layer 16 undergo processes of adding a plasticizer, heating with a gravure printing machine 60, applying hot air, pressure, and cooling, which causes the layers to be denatured and bonded together, so that no defects occur even when the film is subjected to a load of stretching.
[0195] [Experiment 13] In a film-forming operation similar to that in Experiment 11, a transfer laminate 12 exhibiting a flat film was obtained by annealing, pressing, and cooling using the second type drying furnace 62 of the gravure printing machine 60 with a heating temperature of 120-160°C and hot air of 80-100°C. The treatment in Experiment 12 produced a three-dimensional structure, but the treatment in Experiment 13 produced a flat film structure. A heat resistance test was performed similar to that described above. Visual inspection was performed for cracks, breaks, blisters, and gloss decay, and no abnormalities were observed in either the flat film structure or the three-dimensional structure.
[0196] The evaluation results for cracks, breakage, swelling, and gloss in the heat resistance tests of Experiments 8 to 13 are shown in Table 10.
[0197] [Table 10]
[0198] It is possible to deal with cracks, breaks, and bulges in the transfer laminate 12 by using any of the manufacturing methods in Experiments 8 to 13. In the manufacturing method of Experiment 8, as shown in Table 9, a flat film transfer laminate 12 is shown that follows the elongation of the transferee 32 up to 0.8%. In the manufacturing method of Experiment 12, as described above, the elongation of the three-dimensional film transfer laminate 12 shows a cross-sectional length of a bow-shaped parabola arc of 40 to 550 μm. As described above, the means for obtaining this extensibility allows the production of flat film and three-dimensional film structures. By using the first drying furnace 61 of the gravure printing machine 60 and the second drying furnace 62 of the gravure printing machine 60 to heat, dry the prepared solution with hot air, anneal the dry film of the protective layer 14, and process with the pressure device 71 and cooling device 72, the protective layer 14 and the metal layer 15 are hardened, softened, and stress-modified, thereby making it possible to achieve the expansion compliance of the transfer laminate 12 of the flat film and the three-dimensional film without losing the metallic luster. According to Experiments 8 to 12, (1) peeling layer 13, protective layer 14 drying in a first furnace 61, annealing drying in a second furnace 62, metal layer 15, adhesive layer 16, (2) peeling layer 13, protective layer 14 drying in a first furnace 61, metal layer 15, annealing treatment in a second furnace 62, adhesive layer 16, or (3) peeling layer 13, protective layer 14 drying in a first furnace 61, metal layer 15, annealing treatment including hot air treatment in a second furnace 62, pressure treatment, cooling treatment, adhesive layer 16, up to this point, the film can be formed flat by controlling each treatment. Furthermore, in the high-temperature drying in a first furnace 61 of peeling layer 13, protective layer 14, high-temperature annealing treatment including hot air treatment in a second furnace 62, pressure treatment, cooling treatment, adhesive layer 16, protective layer 14 and metal layer 15 high-temperature treatment, the film can be formed three-dimensionally.
[0199] Tables 11 to 13 show the processing, processing order, resistance, and elongation of the resin-based protective layer 14 and the metal layer 15.
[0200] [Table 11]
[0201] [Table 12]
[0202] In the table, ◯ indicates good, and × indicates bad.
[0203] [Table 13]
[0204] [Experiment 14] After forming a release layer 13 and a resin-based protective layer 14 on the base film 11, a metal layer 15 was formed using a two-chamber semi-continuous vacuum deposition machine. Specifically, metal layers 15 of Al, Cr, and Sn were formed in thicknesses ranging from 20 to 65 nm. Thereafter, an adhesive layer 16 was formed, thereby producing a transfer laminate 12. Next, using a heat and pressure transfer machine 51, the transfer was applied to a calendared glossy cardboard at a transfer temperature of 100 to 140°C, a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2 After the transfer laminate 12 was transferred, the reflectance of the surface layer of the metal layer 15 was measured using a spectrocalorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The spectral reflectance of Al was L=89.44, the spectral reflectance of Cr was L=62.36, and the spectral reflectance of Sn was L=68.31.
[0205] [Experiment 15] A transfer laminate 12 was produced by forming a release layer 13, a color-changing resin-based protective layer 14 containing a metal-containing dye, an Al metal layer 15 having a thickness of 20 to 65 nm, and a pressure-sensitive heat-sensitive adhesive layer 16 having a thickness of 1 μm on a base film 11. Next, using a heat and pressure transfer machine 51, a transfer was performed on a calendared glossy cardboard at a transfer temperature of 100 to 140°C, a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2After the transfer laminate 12 was transferred, the reflectance of the metal layer 15 was measured on the surface through the colored resin-based protective layer 14 using a spectrocalorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The spectral reflectance of Al was L=80.21. The spatial chromaticity L*a*b* according to JIS Z8781-4 was measured using a colorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The lightness chromaticity was L=80.21, a=3.86, and b=28.54. The transfer laminate 12 has a flat film structure that reflects the metal layer 15 and exhibits a transparent metallized gold color.
[0206] [Experiment 16] A transfer laminate 12 was produced by forming a release layer 13, a color resin-based protective layer 14 containing finely divided transparent pigments, an Al metal layer 15 having a thickness of 20 to 65 nm, and a pressure-sensitive heat-sensitive adhesive layer 16 having a thickness of 1 μm on a base film 11. Next, using a heat and pressure transfer machine 51, a transfer was performed on a calendared glossy cardboard at a transfer temperature of 100 to 140°C, a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2 After the transfer laminate 12 was transferred, the reflectance of the metal layer 15 was measured on the surface through the colored resin-based protective layer 14 using a spectrocalorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The spectral reflectance of Al was L=82.15. The spatial chromaticity L*a*b* according to JIS Z8781-4 was measured using a colorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The lightness chromaticity was L=82.15, a=-0.04, and b=24.49. The transfer laminate 12 has a flat film structure that reflects the metal layer 15 and exhibits a transparent metallized gold color.
[0207] [Experiment 17] A transfer laminate 12 was produced by forming a release layer 13, a color resin-based protective layer 14 containing a general-purpose pigment, an Al metal layer 15 having a thickness of 20 to 65 nm, and a pressure-sensitive heat-sensitive adhesive layer 16 having a thickness of 1 μm on a substrate film 11. Next, using a heat and pressure transfer machine 51, a transfer was performed on a calendared glossy cardboard at a transfer temperature of 100 to 140° C., a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2After the transfer laminate 12 was transferred, the reflectance of the metal layer 15 was measured through the colored resin-based protective layer 14 using a spectrocalorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90) for the surface layer. The lightness chromaticity was measured using a color difference meter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90) to measure the spatial chromaticity L*a*b* according to JIS Z8781-4. The colored resin-based protective layer 14 containing a pigment had a low reflectance of Al due to its hiding property. The spectral reflectance L of Al was L=43.99 when it contained a blue pigment, L=61.28 when it contained a pink pigment, L=45.84 when it contained a red pigment, L=81.85 when it contained a yellow pigment, and L=31.63 when it contained a black pigment.
[0208] [Experiment 18] On the base film 11, a release layer 13, a colored resin-based protective layer 14 containing a metal-containing dye, and an Al metal layer 15 having a thickness of 20 to 65 nm were formed, and then, using a two-type drying furnace 62 of a gravure printing machine 60, heat treatment by annealing, hot air treatment, pressure treatment, and cooling treatment were performed to make the laminate up to the metal layer 15 into a three-dimensional film. An adhesive layer 16 was further formed on top of that to produce a transfer laminate 12. Next, using a heat and pressure transfer machine 51, the transfer laminate was transferred onto calendared glossy cardboard at a transfer temperature of 100 to 140°C, a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2 After the transfer laminate 12 was transferred, the reflectance of the metal layer 15 was measured on the surface through the colored resin-based protective layer 14 using a spectrocalorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The spectral reflectance of Al was L=75.40. The spatial chromaticity L*a*b* according to JIS Z8781-4 was measured using a colorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The lightness chromaticity was L=75.40, a=3.06, and b=28.67. The transfer laminate 12 has a three-dimensional structure that reflects the metal layer 15 and exhibits a transparent metallized gold color.
[0209] [Experiment 19] On the substrate film 11, a release layer 13, a transparent resin-based protective layer 14, and an Al metal layer 15 having a thickness of 20 to 65 nm were formed, and then, using a two-type drying furnace 62 of a gravure printing machine 60, heat treatment by annealing, hot air treatment, pressure treatment, and cooling treatment were performed to make the laminate up to the metal layer 15 into a three-dimensional film. An adhesive layer 16 was further formed on top of that to produce a transfer laminate 12. Next, using a heat and pressure transfer machine 51, the laminate was transferred onto calendared glossy cardboard at a transfer temperature of 100 to 140°C, a transfer residence time of 0.5 seconds, and a pressure of 5 kg / cm. 2 After the transfer laminate 12 was transferred, the reflectance of the metal layer 15 on the surface was measured through the transparent resin-based protective layer 14 using a spectrocalorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The spectral reflectance of Al was L=87.74. The spatial chromaticity L*a*b* according to JIS Z8781-4 was measured using a colorimeter (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90). The lightness chromaticity was L=87.74, a=-0.17, and b=0.76. The transfer laminate 12 has a three-dimensional structure that reflects the metal layer 15 and exhibits a transparent metallized silver color.
[0210] [Table 14]
[0211] The attenuation of the reflectance of the protective layer 14 was confirmed from the spectral reflectance of the metal layer 15. In experiment 16, it was found that the finely divided pigment provided good transparency. In experiment 19, it was found that the reflectance of the Al metal layer 15 did not change even when a three-dimensional structure was formed. In experiment 16, it was found that the pigment in the protective layer 14 exhibited coloration and transparency equivalent to that of the metal-containing dye. In experiment 17, all of the general-purpose pigments blocked the reflection of the Al metal layer 15. In experiments 18 and 19, no attenuation of the spectral reflectance due to the three-dimensional structure was observed.
[0212] [Experiment 20] A transfer laminate 12 was formed using a base film 11 as a frame support, and consisting of a release layer 13, a colored resin-based protective layer 14 using a transparent pigment, an Al metal layer 15, and an adhesive layer 16. The release layer 13 was set as follows. That is, 72.2% by weight of toluene (Idemitsu Kosan Co., Ltd.), 25.4% by weight of MIBK (Mitsubishi Chemical Holdings Corporation), and 0.03% by weight of ethylene glycol (Kyoto Wako Pure Chemical Industries, Ltd.) were used as the solvent, and 1.07% by weight of Fischer Trophic Wax (Sador Co., Ltd.; A859), 0.04% by weight of fatty acid ester (NOF Corporation; WEP), and 0.9% by weight of acrylic resin (Nippon Shokubai Co., Ltd.; UV-G301) were used as the solute, and these were mixed together. A film was formed using a gravure printing machine 60 under the conditions of an oven drying temperature of 90 to 140°C, a residence time in the drying ovens 61 and 62 of 20 to 60 seconds, and a thickness of 0.1 to 20 μm. The resin-based protective layer 14 uses a pigment as a coloring agent. Specifically, the resin-based protective layer 14 contains 14.6% by weight of toluene (Idemitsu Kosan Co., Ltd.), 8.7% by weight of butyl acetate (Standard Oil Co., Ltd.), 17.0% by weight of MEK (Idemitsu Kosan Co., Ltd.), 17.0% by weight of MIBK (Mitsubishi Chemical Holdings Corporation), 0.004% by weight of ethylene glycol (Kyoto Wako Pure Chemical Industries, Ltd.), 20.5% by weight of acrylic resin (Nippon Shokubai Co., Ltd.; UV-G301), 1.1% by weight of acrylic resin (Wilbur Ellis; AT740), 1.3% by weight of melamine resin ( A mixed solution was prepared by disposing the following: 4.3% by weight of ketone resin (K-95 by Wally Co., Ltd.; Nippon Carbide Co., Ltd.), 4.3% by weight of ketone resin (K-95 by Wally Co., Ltd.; Tokyo Chemical Industry Co., Ltd.; p-toluenesulfonic acid) of hardener (p ...The particle size of the pigment is required to be in the range of 10 to 80 nm in order to obtain coloration, transparency, and reflectivity from the metal layer 15 to give a metallic appearance, and is necessary for using the pigment as a coloring material. The pigments were sized to be finely dispersed using a bead mill type pigment disperser KD-5 manufactured by DYNO-MIL. The metal layer 15 was formed by vapor deposition of aluminum with a thickness of 40 to 60 nm. The thickness of the adhesive layer 16 was 1 to 10 μm, the drying temperature was 80 to 140° C., and the residence time in the furnace was 10 to 40 seconds. The formulation used was 51.7 wt% toluene (Idemitsu Kosan Co., Ltd.), 37.7 wt% ethyl acetate (Showa Denko K.K.), 1.5 wt% butyl acetate (Standard Oil Corporation), 0.7 wt% ethyl silicate (Colcoat Co., Ltd.; HAS-10), 2.7 wt% acrylic resin (Mitsubishi Chemical Corporation; N2147), 2.7 wt% ethylene vinyl acetate resin (Mitsubishi Chemical Corporation; D2908), and 3.0 wt% ketone resin (Wally Chemicals; K-95).
[0213] The color of the resin-based protective layer 14 of the completed transfer foil 10 was highly transparent, even though a pigment was used. A specimen (transferred transfer laminate 12) was prepared by transferring the color using a top-bottom type heat-pressure transfer machine 51 onto a piece of cardboard that had been smoothly calendered and had its surface coated with resin. A xenon arc type lightfastness tester (Suga Test Instruments Co., Ltd.; XT1500) was used to remove the specimen after 800 hours, and a spectrophotometer (Nippon Denshoku Industries Co., Ltd.; SZS-Σ90) was used to measure the color displacement ΔE. The results of the presence or absence of exposure are shown in Table 15. The transfer laminate 12, which had a resin-based protective layer 14 containing fine pigment and was a metallic layer with a transparent gold color and metallic reflection, had excellent lightfastness.
[0214] [Table 15]
[0215] [Experiment 21] In experiment 20, the transfer laminate 12 using finely divided transparent pigment had a metallic layer 15, and thus exhibited metallic coloring and light resistance. In experiment 22, a known material was further used to promote light resistance.
[0216] The objective of the present invention is to improve the light resistance of the transfer laminate 12, which has a finely processed, transparent pigment that exhibits color development and provides a metallized reflection of the metal layer 15. In the transfer laminate 12, which is formed by forming a release layer 13, a color resin-based protective layer 14, a metal layer 15, and an adhesive layer 16 on a base film 11, the following was added to the release layer 13 and the color resin-based protective layer 14 in an attempt to improve the light resistance.
[0217] When exposed to ultraviolet light, the hydrogen atoms of the polymer in the color-changing resin-based protective layer 14 are broken, turning into hydroperoxides, which accelerates the deterioration of the polymer. To prevent this, a hindered amine-based material is used. Polymer deterioration occurs as a chain reaction of radical generation due to photolysis, but this is suppressed. An acrylic resin that barely absorbs ultraviolet light was selected, as well as an acrylic polymerized material in which silicone with good light resistance, a silicate-based material with light shielding properties, and hindered amine as a light stabilizer are polymerized. For the acrylic resin, we selected HALTH HYBRID UV-G301 made by Nippon Shokubai Co., Ltd., in which hindered amine is polymerized, and for the acrylic resin, we selected UVH made by Alpha Kaken Co., Ltd., in which silicone, silicate, and hindered amine are polymerized. In addition, we selected Tinuvin 249 made by BASF, which is a neutral monomer hindered amine, as a stabilizer against the photodecomposition of the resin by ultraviolet light. We selected a hydroxyphenyl triazine-based material as an ultraviolet absorber. Specifically, Tinuvin 479 and 1600 were selected by selecting the wavelength range from among the Tinuvin types manufactured by BASF. As light shielding agents, iron oxides, titanium oxide, and organic pigments with good light resistance and fine particle size of 10 to 80 nm were selected. As a photo-action inhibitor, phenyl salicylate was selected, which does not transfer ultraviolet light quantum with a blocking effect to a polymer chain. In the peeling layer 13, titanium oxide, iron oxide, and phenyl salicylate were used as ultraviolet shielding agents, and an acrylic resin with hindered amine as a polymerization agent was selected as a binder. The release layer 13 was formulated as follows: 72.2 wt% toluene (Idemitsu Kosan Co., Ltd.), 25.4 wt% MIBK (Mitsubishi Chemical Holdings Corporation), 0.03 wt% ethylene glycol (Kyoto Wako Pure Chemical Industries, Ltd.), 1.07 wt% Fischer Trophic Wax (Sador A859), 0.04 wt% fatty acid ester (NOF Corporation; WEP), 0.91 wt% acrylic resin (Nippon Shokubai Co., Ltd.), HALS Hybrid UV-G301 polymerized with hindered amine, 0.05 wt% iron oxide (Mikoku Pigment Co., Ltd.; 8197M), 0.062 wt% titanium oxide (Ishihara Techno Co., Ltd.; TTO-55D), and 0.081 wt% phenyl salicylate (Tokyo Chemical Industry Co., Ltd.).The color-changing resin-based protective layer 14 was formulated as follows: 14.65% by weight of toluene (Idemitsu Kosan Co., Ltd.), 8.57% by weight of butyl acetate (Standard Oil Co., Ltd.), 17% by weight of MEK (Idemitsu Kosan Co., Ltd.), 17% by weight of MIBK (Mitsubishi Chemical Holdings Corporation), 0.0039% by weight of ethylene glycol (Kyoto Wako Pure Chemical Industries, Ltd.), 1.08% by weight of acrylic resin (Wilbur-Ellis Co., Ltd.; AT740), 1.37% by weight of amino resin (Nippon Carbide Corporation; MS-001), 4.32% by weight of ketone resin (Wally Co., Ltd.; K95), 20.5% by weight of acrylic resin (Nippon Shokubai Co., Ltd.; UV-G301), 11.7% by weight of acrylic resin (Alpha The pigments were 0.9836 wt% (Mikuni Color Co., Ltd. 8196M), red pigment 0.9836 wt% (DuPont; Shinshaka Red B), yellow pigment 0.934 wt% (BASF; Paliotol Yellow 1070), and phenyl salicylate 0.078 wt% (Tokyo Chemical Industry Co., Ltd.). The particle size ranges of cerium oxide, titanium oxide, iron oxide, and color pigment are 10 to 30 nm, 10 to 40 nm, 40 to 100 nm, and 60 to 100 nm, respectively, which lead to transparency and are good for coloring effects. The metal layer 15 and adhesive layer 16 were formed in the same manner as above. The peel layer 13, colored resin-based protective layer 14, and adhesive layer 16 were formed using a gravure printing machine 60, with a drying temperature of 90 to 180°C, a residence time in the drying ovens 61 and 62 of 20 to 60 seconds, a thickness of 0.1 to 20 μm, and a drying oven type 1 oven 61 (volume 5.28 m). 3 ) was used for film formation.
[0218] [Experiment 22] The light fastness test described in Experiment 21 was carried out based on the specifications described in Experiment 20. In this Experiment 22, the transfer laminate 12 from Experiment 21 was used as the specimen. The results of the light fastness test are shown in Table 16.
[0219] [Table 16]
[0220] Regarding the coloring effect of the resin-based protective layer 14, the reflectance of the original Al metal layer 15 was 81.33%, which was highly transparent. Even after 1400 hours, the reflectance of the metal layer 15 was 81.53%, which was the same level as the original. Regarding the change in spatial chromaticity Lab value after 1400 hours, ΔE was 1.23, which was the same coloring as the original. The reflectance of the metal layer 15 containing a finely processed pigment with highly transparent coloring was high. The release layer 13 was prepared by adding an acrylic resin containing a hindered amine, finely processed iron oxide, titanium oxide, and phenyl salicylate, which is a light shielding agent. For the preparation of the color resin protective layer 14, acrylic resin polymerized with hindered amine, hindered amine, silicon, silicate, acrylic resin polymerized with hindered amine, ultraviolet absorber, cerium oxide, titanium oxide, phenyl salicylate, iron oxides as coloring materials, and organic pigments with excellent light resistance were selected and arranged to improve the light resistance of the continuous layers of the peelable layer 13 and protective layer 14. In the light resistance test, it was confirmed after 1400 hours that the spatial chromaticity L*a*b* was ΔE=1.23, and the light resistance of the organic pigment used for the preparation of the protective layer 14 in experiment 20 was maintained. [Explanation of symbols]
[0221] 10: Transfer foil 11: Base film 12, 21: Transfer lamination 13: Release layer 14,23: Resin-based protective layer 15: Metal layer 16: Adhesive layer 22: Film protection layer
Claims
1. A base film; and a transfer lamination. The transfer lamination is A release layer formed on the substrate film; a first resin-based protective layer formed on the release layer; a metal layer formed on the first resin-based protective layer; an adhesion layer formed on the metal layer; The first resin-based protective layer contains a plasticizer and includes a multilayer of an ultraviolet curable resin and a thermosetting resin, The transfer laminate is a transfer foil having a three-dimensional structure with uneven ridges.
2. The transfer foil according to claim 1, The transfer lamination further comprises: A transfer foil comprising a second resin-based protective layer formed between the metal layer and the adhesive layer.
3. The transfer foil according to claim 1, further comprising: A transfer foil comprising a film protective layer formed between the base film and the release layer.
4. The transfer foil according to claim 1, The transfer foil, wherein the plasticizer comprises a toluenesulfonamide-based plasticizer and an ethylene olefin-based plasticizer.
5. The transfer foil according to claim 1, A transfer foil, wherein the content of the toluenesulfonamide-based plasticizer in the first resin-based protective layer is 0.01 to 20% by weight, and the content of the ethylene olefin-based plasticizer in the first resin-based protective layer is 0.01 to 0.025% by weight.
6. The transfer foil according to claim 1, The transfer foil, wherein the first resin-based protective layer has a thickness of 1 to 20 μm.
7. The transfer foil according to claim 1, A transfer foil, wherein the first resin-based protective layer contains one or more acrylic resins.
8. The transfer foil according to claim 1, The transfer foil, wherein the first resin-based protective layer contains a curing agent.
9. The transfer foil according to claim 1, The first resin-based protective layer comprises a color developer.
10. The transfer foil according to claim 9, The color developer comprises a pigment having a particle size of 10 to 120 nm.
11. The transfer foil according to claim 10, The first resin-based protective layer comprises a light stabilizer.
12. The transfer foil according to claim 10, The first resin-based protective layer comprises an ultraviolet absorbing agent.
Citation Information
Patent Citations
Transfer foil
JP1981053086A
Manufacture of heat-sensitive image recording body
JP1999115325A
Electro-magnetic wave transmittable metalized hologram transfer material and its manufacturing method
JP2002192895A
In-mold transfer foil and three-dimensional molded article obtained by using the same
JP2010137495A
Decorative product and laminate for thermal transfer
JP2016124289A