Organic solvent dispersion
By controlling the aggregation of titanium oxide particles within specific size ranges, the viscosity stability of dispersions is maintained, addressing the long-term storage issues and improving the consistency of semiconductor films in dye-sensitized solar cells.
Patent Information
- Application Number
- JP2020057533
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-27
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Existing titanium oxide dispersions in organic solvents experience significant changes in viscosity over long-term storage due to sedimentation and agglomeration of particles, affecting the stability and homogeneity of semiconductor films in dye-sensitized solar cells.
Controlled aggregation of titanium oxide particles within specific size ranges, with primary particle diameters between 5 nm and 25 nm and aggregate particle diameters of 150 nm or less, along with a minimal size variation (D90 - D10 ≤ 170 nm), ensuring stable dispersion even after prolonged storage.
The controlled aggregation maintains viscosity stability, preventing sedimentation and ensuring consistent film formation in dye-sensitized solar cells, enhancing the long-term storage and application performance of titanium oxide dispersions.
Smart Images

Figure 0007563889000002 
Figure 0007563889000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an organic solvent dispersion containing aggregated particles of titanium oxide. [Background technology]
[0002] Titanium oxide is widely used as a pigment, cosmetic material, and photocatalyst, and in recent years has also been used in dye-sensitized solar cells.
[0003] A dye-sensitized solar cell is a type of solar cell that uses an organic dye to generate photovoltaic power. Compared to conventional solar cells, dye-sensitized solar cells have the characteristics of being simple in structure, inexpensive in materials and manufacturing processes, and high flexibility in shape. Various structures of this dye-sensitized solar cell have been considered. For example, there is a structure in which an indium / tin-based transparent conductive layer is provided on the inner surface of a glass plate or a transparent plastic sheet. In this structure, the transparent conductive layer has an electrode on which fine particles such as titanium dioxide on which an organic dye such as a ruthenium-based dye is adsorbed is fixed, and a counter electrode such as platinum or carbon. And, it is known that a redox agent such as an iodine solution is filled between the two electrodes. In order to create these structures more simply, the use of a printing method is also being considered.
[0004] Titanium dioxide, which is widely used in dye-sensitized solar cells, is used as a porous semiconductor film formed on the surface of a transparent electrode. The dye adsorbed to this titanium dioxide absorbs light energy. This causes excited electrons to move through the porous semiconductor film to the transparent electrode, generating electricity. Therefore, there has been a demand for titanium dioxide used in dye-sensitized solar cells that is porous and has a large specific surface area so that it can adsorb a larger amount of dye.
[0005] Various titanium dioxide particles for dye-sensitized solar cells have been investigated. For example, Patent Document 1 describes an aggregate of titanium dioxide nanoparticles having an average primary particle diameter of 20 nm or less and an average diameter of 30 to 500 nm. Patent Document 2 describes a coating material for forming a semiconductor film, which contains porous titanium dioxide microparticle aggregates having an average particle diameter in the range of 0.5 to 10 μm and a pore volume in the range of 0.1 to 0.8 mL / g, and non-aggregated titanium dioxide microparticles having an average particle diameter in the range of 5 to 400 nm. With the improvement of titanium dioxide particles for dye-sensitized solar cells, the performance of dye-sensitized solar cells is improving.
[0006] These titanium dioxides are dispersed in water or an organic solvent and used in methods such as coating and screen printing to form a porous semiconductor film. In this case, the viscosity of the paint is a very important factor for forming a homogeneous porous semiconductor film. However, these dispersions have the problem that when stored for a long period of time, particle settling occurs, causing changes in the agglomeration state of titanium dioxide, resulting in a large change in viscosity after long-term storage. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2011-213505 A [Patent Document 2] JP 2009-289669 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide an organic solvent dispersion containing titanium oxide, which exhibits little change in viscosity even when stored for a long period of time. [Means for solving the problem]
[0009] The present inventors have focused on the aggregate particle size of titanium oxide contained in an organic solvent dispersion, and have controlled the aggregate particle size within a specific range and reduced the variation therein, thereby finding that the viscosity is unlikely to change even after long-term storage, making it possible to store the organic solvent dispersion for a long period of time.
[0010] That is, the present invention provides a dispersion in which aggregated particles of titanium oxide are dispersed in an organic solvent, the primary particle diameter of the titanium oxide particles being in the range of 5 nm to 25 nm, and the aggregated particle diameter (D 50 ) is 150 nm or less, and the difference between the 90% cumulative diameter and the 10% cumulative diameter of the aggregated particles (D 90 -D 10 ) is 170 nm or less (hereinafter, also referred to as the organic solvent dispersion of the present invention). Effect of the Invention
[0011] According to the present invention, there can be provided an organic solvent dispersion containing titanium oxide, which exhibits little change in viscosity even when stored for a long period of time. [Brief description of the drawings]
[0012] [Figure 1] 1 is a conceptual diagram of an organic solvent dispersion and a method for producing the same according to the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Summary of the organic solvent dispersion of the present invention] The organic solvent dispersion of the present invention is one in which the aggregated particle size of titanium oxide particles is controlled to a specific range and the variation is reduced. Therefore, the organic solvent dispersion of the present invention does not contain extremely large or small aggregated particles as much as possible. The aggregated particles are dispersed in the organic solvent with a specific surface potential. If the size of the aggregated particles varies, the surface potential also varies, resulting in an imbalanced charge in the organic solvent. If the organic solvent dispersion is in such a state, the aggregated state of the aggregated particles is likely to change. Therefore, the viscosity of the organic solvent dispersion is also likely to change. Therefore, for example, the method shown in FIG. 1 is used to control the aggregated particle size of titanium oxide particles to a specific range and the variation is reduced. Then, by dispersing the aggregated particles in an organic solvent, an organic solvent dispersion in which the viscosity change is small even when stored for a long period of time can be obtained.
[0014] In the present invention, the aggregate particle diameter and its variation of titanium oxide particles are calculated from the particle size distribution obtained by the zeta potential measurement method. 50 ) is the aggregate particle diameter, and the 10% cumulative diameter (D 10 ) and 90% cumulative diameter (D 90 The difference between the dispersion of aggregate particles (D 90 -D 10 ) was decided.
[0015] [Comparison with prior art] The organic solvent dispersion of the present invention is, as compared with Patent Documents 1 and 2, characterized in that "the aggregate particle diameter (D 50 ) is 150 nm or less, and the difference between the 90% cumulative diameter and the 10% cumulative diameter of the aggregated particles (D 90 -D 10 ) is 170 nm or less. In particular, the idea of controlling the agglomerated particle size of titanium oxide contained in an organic solvent dispersion to a specific range and reducing the variation therein is not described in the above patent documents.
[0016] [Organic solvent dispersion of the present invention] The organic solvent dispersion of the present invention will be described in detail below.
[0017] [Titanium oxide] The organic solvent dispersion of the present invention contains titanium oxide particles. In the present invention, titanium oxide does not only refer to titanium dioxide, but also includes titanium dioxide having a composition in which oxygen is partially missing. In addition, the surface of these titanium oxide particles usually contains terminal OH groups, but may be modified with an organic functional group.
[0018] [Primary particle size and aspect ratio of titanium dioxide particles] The organic solvent dispersion of the present invention is a dispersion of titanium oxide aggregate particles in an organic solvent as a dispersion medium, and the size of the primary particles of the titanium oxide constituting the aggregate particles (hereinafter also referred to as "primary particle diameter") is in the range of 5 nm to 25 nm. This primary particle diameter is preferably in the range of 5 nm to 20 nm. The smaller the primary particle diameter, the larger the specific surface area of the titanium oxide particles. For example, when a porous semiconductor film for a dye-sensitized solar cell is formed using the organic solvent dispersion of the present invention, the specific surface area of the titanium oxide particles is large. Therefore, it is preferable because the amount of dye adsorption of the porous semiconductor film increases. The primary particle diameter is calculated by a method of observing the titanium oxide particles extracted from the organic solvent dispersion described above with an electron microscope. In addition, for example, the organic solvent dispersion can be obtained by a method of preparing a titanium oxide slurry as shown in FIG. 1 and then replacing the water with an organic solvent. The primary particle diameter of titanium oxide can also be calculated from this organic solvent dispersion by observing the titanium oxide particles contained in the titanium oxide slurry before the organic solvent replacement with an electron microscope. This calculation method will be described in detail in the Examples below. The aspect ratio (major axis / minor axis) of the titanium oxide particles is preferably in the range of 1 to 3. When a titanium oxide layer is formed using an organic solvent dispersion containing titanium oxide particles having an aspect ratio close to 1, the density of the layer tends to be high.
[0019] [Agglomerated particle size: D 50 ] The titanium oxide particles contained in the organic solvent dispersion of the present invention are present as aggregated particles in the organic solvent dispersion. In the present invention, the size of the aggregated particles is represented by a 50% cumulative diameter calculated from the particle size distribution obtained by measuring the zeta potential. Here, it is important that the aggregated particle diameter contained in the organic solvent dispersion of the present invention is measured in a state in which the aggregated particles are dispersed in a solvent. This is because the state of the aggregated particles in the solvent greatly affects the long-term storage stability of the dispersion. In a measurement method in which the aggregated particles are taken out of the solvent and observed under an electron microscope, the aggregated particles further aggregate when the solvent is removed. In such a state, the boundaries of the aggregated particles become difficult to distinguish, so this is not an appropriate method for measuring the aggregated particle diameter of the organic solvent dispersion of the present invention. The zeta potential measurement used in the present invention is one of the conventionally known measurement methods for measuring the particle size distribution of particles present in a solvent. However, this measurement method can be performed in either an organic solvent or an aqueous solvent, but is more accurate in an aqueous solvent. Therefore, in the present invention, the aggregated particles are taken out under conditions in which the aggregated particles in the organic solvent dispersion do not grow, and then redispersed in an aqueous solvent under specific conditions for measurement. In addition, in the case of an organic solvent dispersion obtained by a method in which a titanium oxide slurry as shown in Figure 1 is prepared and then the water is replaced with an organic solvent, the measurement values of the titanium oxide slurry before solvent replacement can be regarded as the measurement values of the organic solvent dispersion.
[0020] In the present invention, the aggregate particle diameter (D 50 ) is 150 nm or less, preferably in the range of 50 nm or more and 150 nm or less, more preferably in the range of 75 nm or more and 125 nm or less, and particularly preferably in the range of 80 nm or more and 100 nm or less. The organic solvent dispersion of the present invention having the above-mentioned aggregate particle size in this range is unlikely to undergo a change in viscosity or sedimentation of particles even when stored for a long period of time.
[0021] [Agglomerated particle size: D 90 -D 10 ] It is preferable that the variation in size of the aggregated particles contained in the organic solvent dispersion of the present invention is as small as possible. In the present invention, the 10% cumulative diameter (D 10 ) and 90% cumulative diameter (D 90 ) difference (D 90 -D 10 ) was used. In the organic solvent dispersion of the present invention, where this difference is small, the viscosity is unlikely to change even when stored for a long period of time. Specifically, in the organic solvent dispersion of the present invention, this difference is 170 nm or less, preferably 160 nm or less, and particularly preferably 150 nm or less. 50 When the aggregated particle diameter (D) is small, the dispersion state of the aggregated particles is likely to change, and the viscosity of the organic solvent dispersion is also likely to change. 50 If the difference (D 90 -D 10 ) is preferably 50 nm or less.
[0022] [Agglomerated particle size: D 100 ] It is preferable that the organic solvent dispersion of the present invention does not contain coarse particles as much as possible. Specifically, the 100% cumulative diameter (D 100 ) is preferably 1 μm or less, and more preferably 0.5 μm or less. If such coarse particles are contained in the organic solvent dispersion of the present invention, the charge in the organic solvent dispersion becomes more non-uniform.
[0023] [Crystal structure of titanium oxide particles] The crystal structure of the titanium oxide particles contained in the organic solvent dispersion of the present invention can be a conventionally known crystal structure such as anatase type, brookite type, or rutile type. The preferred crystal structure varies depending on the application of the titanium oxide particles. For example, if the titanium oxide particles are for photocatalysis or for use in a semiconductor layer contained in a dye-sensitized solar cell, the anatase type having a large band gap is preferred. In addition, if the titanium oxide particles are used as the negative electrode of a lithium ion secondary battery, the brookite type is preferred. The presence or absence of these crystal structures can be determined by X-ray diffraction measurement.
[0024] [Titanium oxide particle concentration] The concentration of titanium oxide particles contained in the organic solvent dispersion of the present invention is preferably in the range of 5% by mass to 25% by mass, more preferably in the range of 10% by mass to 20% by mass, calculated as TiO2. If the concentration of titanium oxide particles is too high, sedimentation of the particles is likely to occur during long-term storage.
[0025] [Organic solvents] The organic solvent contained in the organic solvent dispersion of the present invention is not particularly limited. As the organic solvent, alcohols, ketones, glycols, ethers, turpentines, etc. are preferred. These can be used alone or in combination of two or more. As the alcohols, for example, methanol, ethanol, isopropyl alcohol, butanol, etc. are preferred. As the ketones, for example, acetone, etc. are preferred. As the glycols, for example, ethylene glycol, propylene glycol, etc. are preferred. As the ethers, for example, butyl carbitol, butyl carbitol acetate, etc. are preferred. As the turpentines, for example, terpineol, dihydroterpineol, terpinolene, etc. are preferred. In particular, butyl carbitol or terpineol is preferred. The concentration of the organic solvent contained in the organic solvent dispersion of the present invention varies depending on the concentration of other components, but is preferably in the range of approximately 50% by mass or more, more preferably in the range of 50% by mass or more and 95% by mass or less.
[0026] [Thickener] The organic solvent dispersion of the present invention may contain a thickener as necessary. Examples of the thickener include compounds such as polyethylene glycol, polyvinylpyrrolidone, hydroxypropyl cellulose, polyacrylic acid, ethyl cellulose, methyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylic resin, ketone resin, and melamine resin. The concentration of the thickener contained in the coating material of the present invention varies depending on the target viscosity, but may be in the range of approximately 1% by mass to 40% by mass, or 4% by mass to 10% by mass.
[0027] [viscosity] The viscosity of the organic solvent dispersion of the present invention is 0.5×10 5 mPa s or more 2.0×10 5 In addition, when the organic solvent dispersion of the present invention is used for forming a semiconductor layer of a dye-sensitized solar cell, the viscosity is preferably in the range of 1.0×10 5 mPa s or more 2.0×10 5 It is more preferable that the viscosity is in the range of not more than mPa·s. When the viscosity is in the above range, it becomes easy to form a porous semiconductor layer by screen printing or the like.
[0028] [Nitrate ion concentration] When the organic solvent dispersion of the present invention is used to form a porous semiconductor layer of a dye-sensitized solar cell, it is preferable that the coating material of the present invention contains nitrate ions. When a porous semiconductor layer is formed using an organic solvent dispersion in which titanium oxide particles and nitrate ions coexist in this way, a change occurs in the band gap of titanium oxide. Such a change in the band gap is preferable because it broadens the range of wavelengths of light that can be absorbed. The inventors speculate that the change in the band gap is due to the reduction of the titanium oxide surface by nitrate ions accompanying the heat treatment. This speculation does not limit the present invention. In particular, it is preferable that nitrate ions are contained in the range of 1 mass % to 10 mass % relative to the total mass of titanium oxide particles contained in the organic solvent dispersion of the present invention.
[0029] [Water content] When the organic solvent dispersion of the present invention contains a polar organic solvent or a thickener, it is preferable that the organic solvent dispersion of the present invention contains a very small amount of moisture. Such a small amount of moisture is introduced through a process of adjusting the moisture so that a certain amount of moisture is contained during the production process, together with the moisture contained in the raw material. By having such a small amount of moisture contained in the organic solvent dispersion of the present invention, the dispersibility of the titanium oxide particle aggregate particles in the organic solvent is improved. This makes it difficult for viscosity changes and particle sedimentation to occur even when stored for a long period of time. The inventors speculate that the presence of a small amount of moisture makes it easier for the polar organic solvent or thickener to be coordinated to the titanium oxide aggregate particles. This speculation does not limit the present invention.
[0030] [Method for producing organic solvent dispersion of the present invention] The dispersion of the present invention can be produced, for example, by a production method including the following steps (A) to (D). (A) Titanium oxide slurry production process (B) Coarse particle removal process (C) Agglomeration state adjustment process (D) Solvent replacement process
[0031] [(A) Titanium oxide slurry production process] This step is a step of producing a titanium oxide slurry. The slurry in the present invention is a suspension in which particles are mixed in a liquid, and includes sol and gel. The titanium oxide slurry can be obtained, for example, by hydrolyzing a titanium compound to produce amorphous orthotitanic acid, adding a crystallizing agent to this, and then subjecting the resultant to hydrothermal treatment.
[0032] Titanium compounds that can be used include titanium halides (titanium tetrachloride, etc.), titanium salts (titanium sulfate, titanyl sulfate, etc.), and titanium alkoxides (titanium tetramethoxide, titanium tetraethoxide, titanium tetraisopropoxide, etc.). These titanium compounds are preferably used as a solution. The solvent in the titanium compound solution may be water, an organic solvent, or a mixture thereof. If necessary, the titanium compound solution may contain a component that promotes hydrolysis, such as an acid or an alkali. In this case, the concentration of the titanium compound is preferably in the range of 1% by mass to 20% by mass, and more preferably in the range of 1% by mass to 10% by mass, calculated as TiO2. When the concentration of the titanium compound is in this range, titanium oxide particles having a uniform primary particle size can be obtained.
[0033] When the solution of these titanium compounds is hydrolyzed in the presence of water, it is preferable to gradually add an acid or alkali to the solution while stirring it, so that the final pH is in the range of 7 to 13. At this time, it is more preferable that the final pH is in the range of 8 to 10. It is also preferable to add the acid or alkali over at least one hour so that the pH is in the above-mentioned range. In this way, by gradually changing the pH of the titanium compound solution to the above-mentioned range, the variation in the primary particle size of the titanium oxide finally obtained is reduced. If the variation in the primary particle size of titanium oxide is reduced, the variation in the aggregated particle size of titanium oxide is also likely to be reduced. The temperature of this solution is preferably in the range of 0°C to 60°C, and more preferably in the range of 30°C to 50°C. By carrying out the hydrolysis in the above-mentioned temperature range, the primary particle size and its variation of the titanium oxide particles are further reduced. The inventor speculates that fine, uniform-sized amorphous orthotitanic acid is produced by hydrolysis under the above-mentioned conditions. The inventor speculates that this is then crystallized by the hydrothermal treatment described below to become titanium oxide particles. These assumptions are not intended to limit the invention.
[0034] A solution containing amorphous orthotitanic acid obtained by the above-mentioned hydrolysis can be hydrothermally treated to obtain a titanium oxide slurry. In this case, it is preferable to hydrothermally treat this solution in an autoclave at a temperature range of 100°C to 250°C. Furthermore, it is preferable that the time for holding the solution in the above-mentioned temperature range is in the range of 2 hours to 48 hours. If this holding time is too short, titanium oxide particles may not be sufficiently generated. If this holding time is too long, it is also not preferable from the viewpoint of economy.
[0035] A crystallizing agent may be added to the solution containing amorphous orthotitanic acid, if necessary. As the crystallizing agent, an alkali metal hydroxide such as NaOH or KOH, a quaternary ammonium hydroxide, or an organic basic compound such as an alcoholamine can be used. In the present invention, it is preferable to use an organic basic compound. In addition, the crystallizing agent is selected from the group consisting of a molar amount (M C ) and the number of moles of amorphous orthotitanic acid converted to TiO2 (M T ) and the ratio (M C / M T ) is preferably added to the solution so that the ratio is in the range of 0.0001 to 0.1. It is more preferably added so that the ratio is in the range of 0.001 to 0.01. The crystallization agent has the function of promoting the crystallization of titanium oxide particles. Therefore, if the amount added is too small, crystallization may be insufficient. Furthermore, the crystallization agent contained in the titanium oxide slurry after the hydrothermal treatment can be removed using an ion exchange method, ultrafiltration method, or the like, as necessary.
[0036] The titanium oxide slurry obtained in this step preferably has a pH in the range of 2 or less. Titanium oxide begins to aggregate when its pH is around 1, so the pH is adjusted to the above range at this stage to create agglomerated titanium oxide particles. In this way, agglomerated titanium oxide particles are created once, and after removing the coarse particles in the step described below, the agglomerated particles are deflocculated and re-aggregated. This makes it possible to obtain agglomerated titanium oxide particles with small size variation. Nitric acid is preferred as the pH adjuster.
[0037] [(B) Coarse particle removal process] This step is a step of removing coarse particles from the titanium oxide slurry obtained in the above-mentioned titanium oxide slurry production step. The coarse particles are composed of excessively grown titanium oxide particles and large aggregated particles contained in the titanium oxide slurry. The coarse particles have an adverse effect when the organic solvent dispersion of the present invention is stored for a long period of time. Therefore, in this step, the titanium oxide slurry is removed from the titanium oxide slurry by removing the coarse particles having a particle size distribution smaller than D 100 The coarse particles are removed by a conventional method until the particle size becomes 1 μm or less.
[0038] In this step, as a conventionally known method for removing coarse particles, a method of passing through a sieve or mesh having a specific mesh size, a centrifugal separation method, etc. can be used. For particularly large coarse particles, a method of passing through a sieve or mesh is effective. For other coarse particles, a centrifugal separation method is effective. These methods can be appropriately used depending on the degree of the particle size distribution described above. In addition, if the particles cannot be completely removed in one go, this step may be repeated multiple times.
[0039] [(C) Aggregation state adjustment process] This step is a step in which the agglomerated particles of titanium oxide contained in the titanium oxide slurry from which the coarse particles have been removed in the above-mentioned coarse particle removal step are deflocculated and re-agglomerated, thereby regulating the size of the agglomerated particles of titanium oxide.
[0040] In this step, as a method for deflocculating the agglomerated particles of titanium oxide contained in the titanium oxide slurry, the pH of the titanium oxide slurry is adjusted to a range of 0.5 to 2 and the zeta potential to a range of 40 mV or more. Then, a method of performing a dispersion treatment such as ultrasonic treatment can be used. By adjusting the pH and zeta potential of the titanium oxide to the above-mentioned ranges, an environment in which the titanium oxide particles are easily dispersed is first created. Next, the titanium oxide particles are dispersed in such an environment in which the titanium oxide particles are easily dispersed, thereby deflocculating the agglomerated titanium oxide particles. As a method for the dispersion treatment, a method using a homogenizer, a bead mill, or the like can be used. For example, a high-pressure homogenizer or an ultrasonic homogenizer can be used.
[0041] In this step, after the above-mentioned dispersion treatment, the deflocculated titanium oxide particles are re-aggregated to form aggregated particles of a certain size. At this time, the pH and zeta potential of the titanium oxide slurry are lowered below the above-mentioned ranges, so that the deflocculated titanium oxide particles can be re-aggregated.
[0042] [(D) Solvent replacement process] In this step, the water contained in the titanium oxide slurry obtained through the above-mentioned aggregation state adjustment step is replaced with an organic solvent.
[0043] The method of replacing the water contained in the titanium oxide slurry with an organic solvent can be a conventional method. For example, a method of centrifuging the titanium oxide slurry, removing the resulting supernatant, and then adding a predetermined organic solvent can be used. In addition, by repeating such an operation, the purity of the organic solvent in the organic solvent dispersion can be further increased. As another method, a method of replacing with a polar organic solvent such as ethanol, adding a predetermined organic solvent, and then removing the polar organic solvent using a rotary evaporator or vacuum emulsifier can be used. In addition, by using such a method, the purity of the organic solvent can be further increased. In addition, when a thickener is added, it is preferable to add it after replacing in the organic solvent. In addition, after replacing with an organic solvent by each method, it is preferable to perform a dispersion treatment such as ultrasonic treatment or homogenizer treatment. However, this dispersion treatment is performed with an intensity to the extent that the aggregated particles are dispersed in the organic solvent. Through such a solvent replacement treatment, an organic solvent dispersion is obtained.
[0044] By adding a very small amount of moisture to the organic solvent dispersion obtained through the above-mentioned process, the change in viscosity when the organic solvent dispersion is stored for a long period of time can be further suppressed. This is not a method of simply adding water droplets to the organic solvent dispersion or spraying moisture using a sprayer, but a method of absorbing moisture using moisture in the atmosphere. The method of using moisture in the atmosphere can add a very small amount of moisture to the organic solvent dispersion. By using such a method, moisture can be uniformly dispersed in the organic solvent dispersion. Specifically, the organic solvent dispersion is kneaded in an exposed state in a thermo-hygrostat. At this time, the amount of moisture absorbed in the organic solvent dispersion is controlled depending on how much the humidity in the tank has decreased. Note that in the above-mentioned method using a sprayer, water segregates in the organic solvent dispersion. For this reason, the change in viscosity becomes large when the organic solvent dispersion is stored for a long period of time. EXAMPLES
[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the scope of these examples.
[0046] [Example 1] [(A) Titanium oxide slurry production process] Pure water was ultrafiltered to obtain UF water. This UF water was heated to 40°C in a reaction vessel. A titanium tetrachloride aqueous solution (manufactured by Osaka Titanium Technologies, TiO2 equivalent concentration: 28.2% by mass) was added to this heated UF water to obtain a titanium tetrachloride aqueous solution with a TiO2 equivalent concentration of about 4% by mass. Ammonia aqueous solution (NH3 concentration 15% by mass) was added to this titanium tetrachloride aqueous solution at a constant rate over 1 hour so that the pH of the finally obtained aqueous solution containing amorphous orthotitanic acid was 8.6, and then the solution was stirred for 1 hour to obtain a solution containing amorphous orthotitanic acid. The cake obtained by centrifuging this solution was washed with UF water heated to 50°C. UF water was added to this washed cake to obtain a solution containing amorphous orthotitanic acid with a TiO2 equivalent concentration of 7% by mass. Tetramethylammonium hydroxide (manufactured by Tama Chemicals, concentration: 25% by mass) was added to this solution to obtain the TiO2 equivalent mole number (M T) and the number of moles of crystallization agent (M C ) molar ratio (M C / M T ) was 0.002. This solution was heated in an autoclave at 150°C for 15 hours, and then at 190°C for 2 hours to obtain a titanium oxide slurry. UF water was added to this titanium oxide slurry to obtain a titanium oxide slurry with a TiO2 equivalent concentration of 2.56% by mass. Nitric acid (concentration: 61% by mass) was added to this titanium oxide slurry to obtain a titanium oxide slurry with a pH of 1.5. This slurry was subjected to ion exchange to remove tetramethylammonium hydroxide. This slurry was concentrated using an ultraconcentration method until the TiO2 equivalent concentration reached 21% by mass. The filtrate generated at this time was stored as a solution for adjusting the concentration in the coarse particle removal process described below.
[0047] [(B) Coarse particle removal process] The titanium oxide slurry obtained in the titanium oxide slurry preparation step was centrifuged at 2800 rpm for 10 minutes. The cake generated by centrifugation was removed from this slurry, and the above-mentioned filtered water was added to the remaining supernatant until the TiO2 equivalent concentration became 20 mass%. Furthermore, this slurry was centrifuged at 6500 rpm for 10 minutes. The cake generated by centrifugation was removed from this slurry. This operation removed coarse particles from the titanium oxide slurry.
[0048] [(C) Aggregation state adjustment process] Hydrochloric acid (concentration: 15% by mass) was added to the titanium oxide slurry obtained in the coarse particle removal process described above. At this time, the pH of this slurry was 1.1, and its zeta potential was 42 mV. This slurry was ultrasonically treated for 5 minutes at an output (300 W, 19.5 kHz). Nitric acid (concentration: 61% by mass) was added to this ultrasonically treated slurry. At this time, the pH of the slurry was 1.0. This slurry was ultrasonically treated for 5 minutes at an output (300 W, 19.5 kHz). The pH of the titanium oxide slurry obtained through this process was 1.0, and its zeta potential was 34 mV.
[0049] [(D) Solvent replacement process] Ethanol was added to the titanium oxide slurry obtained through the above-mentioned flocculation state adjustment process. The titanium oxide slurry to which ethanol was added was centrifuged at 3000 rpm for 10 minutes. The supernatant generated by the centrifugation was removed, and ethanol was added to the remaining cake. Then, this was ultrasonicated for 10 minutes at an output of 300 W and 19.5 kHz. This process (centrifugation, addition of ethanol, ultrasonication) was repeated twice. This was treated with a homomixer at 10000 rpm for 3 minutes to obtain an ethanol dispersion. Ethyl cellulose (manufactured by Sigma-Aldrich Co., Ltd.), terpineol (manufactured by Yasuhara Chemical Co., Ltd.), and butyl carbitol (manufactured by Kanto Chemical Co., Ltd., product name: 2-(2-n-butoxyethoxy)ethanol) were added to this ethanol dispersion. Furthermore, this dispersion was treated with a homomixer at 10000 rpm for 3 minutes, and then ultrasonicated for 10 minutes at an output of 300 W and 19.5 kHz. This homomixer treatment and ultrasonic treatment were repeated a total of three times. Ethanol was removed from this dispersion using an evaporator and a vacuum emulsifier to obtain a paste containing titanium oxide. In a thermo-hygrostat chamber at 25°C and a humidity of 57%, this paste containing titanium oxide was kneaded on a three-roll mill for 30 minutes or more. At this time, the humidity in the thermo-hygrostat chamber was reduced to 35%, and a certain amount of water was added to the paste containing titanium oxide, finally obtaining an organic solvent dispersion.
[0050] [Example 2] An organic solvent dispersion was obtained in the same manner as in Example 1, except that in the coarse particle removal step, the titanium oxide slurry was centrifuged at 13,000 rpm for 10 minutes. The properties of this organic solvent dispersion are shown in Table 1.
[0051] [Example 3] An organic solvent dispersion was obtained in the same manner as in Example 1, except that in the coarse particle removal step, the titanium oxide slurry was centrifuged at 13,000 rpm for 100 minutes. The properties of this organic solvent dispersion are shown in Table 1.
[0052] [Example 4] An organic solvent dispersion was obtained in the same manner as in Example 1, except that in the coarse particle removal step, the titanium oxide slurry was centrifuged at 13,000 rpm for 180 minutes. The properties of this organic solvent dispersion are shown in Table 1.
[0053] [Example 5] An organic solvent dispersion was obtained in the same manner as in Example 1, except that in the coarse particle removal step, the titanium oxide slurry was centrifuged at 13,000 rpm for 240 minutes. The properties of this organic solvent dispersion are shown in Table 1.
[0054] [Comparative Example 1] An organic solvent dispersion was obtained in the same manner as in Example 1, except that hydrochloric acid (concentration: 15% by mass) was not added to the titanium oxide slurry in the aggregation state adjustment step, and a thermo-hygrostat was not used in the solvent replacement step. The properties of this organic solvent dispersion are shown in Table 1.
[0055] [Measurement of primary particle size and aspect ratio of titanium oxide] The titanium oxide slurry obtained through the above-mentioned flocculation adjustment process was used to measure the primary particles of titanium oxide. After the flocculation adjustment process and before the addition of ethanol in the solvent replacement process, 10 mL of the titanium oxide slurry was collected once from the surface of the slurry in the center of the container together with the liquid using a 20 mL dropper. This was dispersed in 20 mL of ethanol. While stirring, 2 mL was collected using another 5 mL dropper and dropped onto the sample stage of a transmission electron microscope, and the solvent was allowed to evaporate naturally. After that, the center of the sample was photographed using a transmission electron microscope (JEOL, JEM1400) at a magnification that allowed the primary particles of titanium oxide to be observed. Then, the major and minor diameters of all 300 primary particles of titanium oxide in the center of the image were measured with a ruler. The total value of all the measured major and minor diameters was divided by 300 to determine the primary particle diameter of titanium oxide. The aspect ratio (major axis / minor axis) of titanium oxide was also determined.
[0056] [Measurement of aggregate particle size] The titanium oxide slurry obtained through the above-mentioned aggregation state adjustment process and before the addition of ethanol in the solvent replacement process was used to measure the aggregate particle size. Specifically, the titanium oxide concentration in the titanium oxide slurry was adjusted to 20 mass % and the zeta potential was adjusted to a range of 40 mV to 45 mV, and the particle size distribution (volume basis) was measured using a zeta potential measuring device (ELSZ-2000, manufactured by Otsuka Electronics Co., Ltd.). From this particle size distribution, the particle size (D 10 ), 50% frequency particle size (D 50 ), 90% frequency particle size (D 90 ) was calculated. The results are shown in Table 1. It is also possible to measure this by a method in which the titanium oxide particles are taken out of the organic solvent dispersion and then redispersed in water. In this case, the solvent is adjusted so that the titanium oxide concentration is 10 mass % and the zeta potential is in the range of 40 mV to 45 mV.
[0057] [Viscosity measurement] The viscosity of the organic solvent dispersion (on the first day) was measured under the following conditions. Note that this viscosity was measured within one day after the preparation of the organic solvent dispersion was completed. Viscometer: Model RheoStress3000 Rotor: Model C35 / 1Ti Constant temperature bath temperature: 30±1℃ Sample size: 1g Shear rate: Change from 0 to 100 (1 / s) Viscosity: Calculated from shear stress at a shear rate of 4.2.
[0058] [Evaluation of viscosity change over time] The organic solvent dispersion was stored in a cool, dark place (10°C) for 90 days. Thereafter, the viscosity of the organic solvent dispersion was measured (after 90 days) under the above-mentioned conditions. Using the viscosity (initial day) and viscosity (after 90 days) values obtained in the above-mentioned viscosity measurement, the viscosity change rate was calculated from the following formula. Viscosity change rate [%] = |Viscosity (first day) - Viscosity (after 90 days)| / Viscosity (first day) x 100
[0059] [Table 1]
Claims
1. A dispersion in which aggregated particles of titanium oxide are dispersed in an organic solvent, The primary particle diameter of the titanium oxide particles is in the range of 5 nm or more and 25 nm or less, The aggregate particle diameter (D 50 ) is 150 nm or less, The difference between the 90% cumulative diameter and the 10% cumulative diameter of the aggregated particles (D 90 -D 10 ) is 170 nm or less; The titanium oxide particles contain nitrate ions in an amount of 1% by mass or more and 10% by mass or less based on the total mass of the titanium oxide particles. An organic solvent dispersion for forming the semiconductor layer of a dye-sensitized solar cell.
2. Viscosity is 1.0 x 10 5 mPa・s or more, 2.0×10 5 2. The organic solvent dispersion according to claim 1, having a viscosity in the range of mPa·s or less.
3. The organic solvent dispersion according to claim 2 , wherein the titanium oxide particles have an aspect ratio in the range of 1 or more and 3 or less.
Citation Information
Patent Citations
New metal oxide particles and application thereof
JP2002110261A
Electrode material for dye-sensitized photocell and its manufacturing method
JP2002343453A
Titanium oxide dispersion and its producing method
JP2006001774A
Titanium oxide dispersion and its producing method
JP2006001775A
Dispersion of metal oxide fine particle and its manufacturing method
JP2007197296A