Modified fibrous base material

Coating fibrous materials with a cured polysilazane compound improves water resistance and strength without altering texture, addressing the limitations of traditional coatings and organic resins.

JP7564069B2Active Publication Date: 2024-10-08SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021142081
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-01
Publication Date
2024-10-08
Estimated Expiration
2041-09-01

AI Technical Summary

Technical Problem

Fibrous materials like paper lose strength when wet due to hydrophilic fibers unraveling, leading to issues such as product damage and environmental pollution from non-decomposable organic resin alternatives, while coatings impair texture and do not fundamentally address water resistance.

Method used

Coating fibers with a cured polysilazane compound having a specific structure to enhance water resistance without altering the material's texture, using organic or inorganic fibers in paper, paperboard, or cloth.

Benefits of technology

Maintains sufficient strength and water resistance without changing the material's texture, being environmentally friendly and avoiding the drawbacks of organic resin coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564069000001
    Figure 0007564069000001
  • Figure 0007564069000002
    Figure 0007564069000002
  • Figure 0007564069000003
    Figure 0007564069000003
Patent Text Reader

Abstract

To provide a modified fibrous base material which has improved water resistance without changing texture and can maintain sufficient strength even when wet with water.SOLUTION: A modified fibrous base material is coated with a cured polysilazane compound having a structure represented by the following formula (1), and the fibers are only organic fibers or only inorganic fibers, wherein the fibrous base material is selected from paper, paperboard, or cloth. (Where, R1 and R2 are a group selected from hydrogen atoms, aliphatic hydrocarbon groups having 1-6 carbon atoms, aromatic hydrocarbon groups having 6-12 carbon atoms, or alkoxy groups having 1-6 carbon atoms, and may be identical or different; however, at least one of R1 and R2 is a hydrogen atom bonded to a silicon atom.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to modified fibrous base materials. [Background technology]

[0002] Fiber materials such as paper and cloth are made from fibrous raw materials, and are therefore highly processable and moldable. Depending on how they are made, they can be used for a variety of purposes, making them an indispensable and versatile material in our daily lives. Paper, in particular, is used for a wide variety of purposes, including notebooks and newspapers for writing and printing, daily necessities such as tissue paper and toilet paper, building materials such as shoji screens, and food packaging. There are many products on the market that have the necessary characteristics for each purpose, but they generally have a weakness in that they are weak against water. This is because paper is made by entangling fibers and is not bonded to each other with adhesives, and the fibers in paper are hydrophilic fibers obtained from plants. Therefore, when paper gets wet, the entangled fibers come undone and its strength is greatly reduced. Toilet paper and other products make use of this characteristic, so it is required that its strength be reduced by water. However, on the other hand, if the strength of packaging materials such as cardboard is reduced by rain, the transported items may fall, causing serious problems such as damage to the items and injuries to people around them.

[0003] To solve this problem, organic resin (plastic) products such as polystyrene foam are often used instead of cardboard in fish markets, rivers, and around the sea, where it is assumed that the material will get wet. However, organic resins such as polystyrene foam do not naturally decompose, and if they are not collected in a prescribed manner, they will directly lead to the pollution of forests and oceans. In particular, in recent years, the "Sustainable Development Goals," commonly known as "SDGs," were adopted at the United Nations Summit and have been promoted worldwide. For this reason, there has been a global trend to reduce organic resin products that lead to the pollution of forests and oceans as much as possible. In response to this issue, paper products have once again attracted attention, and there are many products that boast the waterproofing of paper, but most of them are paper surfaces or fibers coated with organic resins (Patent Document 1). These coatings are effective to a certain extent in terms of waterproofing, but they give the paper a glossy or smooth texture that is not found in original paper, which significantly changes the texture, and the workability is reduced, such as repelling ink and preventing duct tape from adhering. In addition, the advantages of the fiber, such as breathability and printability with ink, are lost due to the coating, so this type of modification is not preferred depending on the application. Furthermore, it is bad for the environment because it contains organic resin components when disposed of, and it does not fundamentally solve the problem. Furthermore, these coatings are a method of repelling water to prevent the paper fibers from getting wet, so the fundamental problem of the water resistance of the paper itself is not solved. Therefore, if the coating peels off or cracks for some reason, the strength will decrease just like conventional paper. In addition to this method, a method has been proposed in which paper and organic resin sheets are alternately laminated to achieve water resistance, but for the same reasons as above, this is not a true alternative technology (Patent Document 2 and Patent Document 3).

[0004] For the reasons mentioned above, there is a demand for fibrous materials that can maintain sufficient strength even when wet by improving the water resistance of the fibrous substrates, such as paper, in an environmentally friendly manner without compromising the properties of the substrates. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-180044 A [Patent Document 2] JP 2005-193934 A [Patent Document 3] JP 2013-095058 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a modified fibrous base material that has improved water resistance without changing the texture and can maintain sufficient strength even when wetted with water. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides a modified fibrous substrate, in which fibers are coated with a cured product of a polysilazane compound having a structure represented by the following formula (1), the fibers are composed of only organic fibers or only inorganic fibers, and the fibrous substrate is selected from paper, paperboard, and cloth. [ka] (In the formula, R1 and R2 are each a group selected from a hydrogen atom, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and may be the same or different, provided that at least one of R1 or R2 is a hydrogen atom bonded to a silicon atom.)

[0008] Such a modified fibrous base material has improved water resistance without changing the texture, and is capable of maintaining sufficient strength even when wet.

[0009] In the present invention, the fibrous base material is preferably a cardboard base paper.

[0010] Such a modified fibrous base material is preferable because it allows the effects of the present invention to be fully exhibited.

[0011] In the present invention, the polysilazane compound is preferably perhydropolysilazane.

[0012] Such a polysilazane compound can further improve the effects of the present invention.

[0013] In the present invention, it is preferable that the polysilazane compound further contains a curing catalyst.

[0014] Such a polysilazane compound is preferable because it allows for short-time curing or low-temperature curing.

[0015] In the present invention, the cured product of the polysilazane compound is preferably at least one of an oxide, a nitride, and an oxynitride of the polysilazane compound.

[0016] Such a cured product of the polysilazane compound can be used in the modified fibrous base material of the present invention. Effect of the Invention

[0017] As described above, the modified fibrous substrate of the present invention has a transparent glassy coating that does not affect the texture of the substrate, thereby improving the water resistance without impairing the original properties and texture of the substrate, and providing a modified fibrous substrate that can maintain sufficient strength even when wet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] As described above, there has been a need for the development of a modified fibrous base material that can improve water resistance without changing the texture and that can maintain sufficient strength even when wet.

[0019] As a result of intensive research into the above-mentioned problems, the inventors have discovered that by coating a fibrous substrate with a cured product of a polysilazane compound having a specific structure, it is possible to develop a modified fibrous substrate that has improved water resistance without changing the texture and that can maintain sufficient strength even when wet, and have completed the present invention.

[0020] That is, the present invention relates to a modified fibrous substrate, in which fibers are coated with a cured product of a polysilazane compound having a structure represented by the following formula (1), the fibers are composed of only organic fibers or only inorganic fibers, and the fibrous substrate is selected from paper, paperboard, and cloth. [ka] (In the formula, R1 and R2 are each a group selected from a hydrogen atom, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and may be the same or different, provided that at least one of R1 or R2 is a hydrogen atom bonded to a silicon atom.)

[0021] The present invention will be described in detail below, but the present invention is not limited thereto.

[0022] [Modified fiber base material] The present invention relates to a modified fibrous substrate, in which fibers are coated with a cured product of a polysilazane compound having a structure represented by the following formula (1), the fibers are composed of only organic fibers or only inorganic fibers, and the fibrous substrate is selected from paper, paperboard, and cloth.

[0023] [Polysilazane compounds] The polysilazane compound in the present invention is a polysilazane having a structure represented by the following formula (1). [ka]

[0024] In the formula (1), R1 and R2 are each a group selected from a hydrogen atom, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and may be the same or different. However, at least one of R1 or R2 is a hydrogen atom bonded to a silicon atom. If there is no Si-H bond in the molecule, the film will not become hard even after curing, making it difficult to use for the purpose of improving water resistance.

[0025] Examples of the polysilazane compound in the present invention include perhydropolysilazane and monomethylpolysilazane, with perhydropolysilazane being particularly preferred.

[0026] There is no particular restriction on the curing method as long as the polysilazane compound is cured to such an extent that it does not separate from the fiber, but if sufficient curing is not possible due to restrictions such as the heat resistance temperature of the fibrous substrate to be coated, a curing catalyst may be added. Also, additives such as a solvent or a filler may be added as necessary.

[0027] There are no particular restrictions on the molecular weight, but it is generally preferable that the weight-average molecular weight is within the range of 1 to 1 million in terms of polystyrene. If the weight-average molecular weight is 100 or more, there is little volatilization at room temperature, and a sufficient coating film is formed. Also, if the weight-average molecular weight is 1 million or less, the viscosity is not too high, so it is possible to penetrate into the gaps between fibers and coat each fiber. The weight-average molecular weight was measured using a GPC device using the following method. [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: UV detector Column: TSK Guardcolumn SuperH-L TSKgel SuperMultipore HZ-M (4.6mm I.D. x 15cm x 4) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (0.5 wt% THF solution)

[0028] [Curing catalyst] The polysilazane compound of the present invention may further contain a curing catalyst. The addition of a curing catalyst enables short-time curing or low-temperature curing. There are no particular restrictions on the curing catalyst as long as it promotes the curing of the Si-H group or alkoxy group, which is a binding functional group contained in the polysilazane compound used. Examples of curing catalysts for Si-H groups include platinum group compounds such as nickel, palladium, and platinum, aliphatic amines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, and tetramethylethylenediamine, aliphatic amino alcohols such as methylaminoethanol and dimethylaminoethanol, aromatic amines such as aniline, phenylethylamine, and toluidine, heterocyclic amines such as pyrrolidine, piperidine, piperazine, pyrrole, pyrazole, imidazole, pyridine, pyridazine, and pyrimidine pyrazine, and aminosilanes such as aminopropyltriethoxysilane, aminoethylaminopropyltrimethoxysilane, and aminoethylaminopropylmethyldiethoxysilane. In the case of an alkoxy group, triethoxyaluminum, tributoxyaluminum, dibutoxy(2-oxo-5-oxa-3-hepten-4-yloxy)aluminum, di(ethylacetoacetate)monobutoxyaluminum, ethylacetoacetate di(isopropoxy)aluminum, aluminum trichloride, tetraethoxytitanium, tetraisopropoxytitanium, tetrabutoxytitanium, tetra(2-ethylhexoxide)titanium, titanium tetrachloride, tetrakis(2,4-pentanedionato)titanium, diisopropoxybis(ethylacetoacetate)titanium, zinc chloride, zinc acetate, and other metal compounds, inorganic acids such as hydrochloric acid, nitric acid, and sulfuric acid, organic acids such as formic acid, acetic acid, propionic acid, citric acid, and oxalic acid, inorganic bases such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, and organic bases such as pyridine and triethylamine. Two or more of these catalysts may be added in any ratio.

[0029] Among these, in the case of Si-H groups, amine compounds are preferred because curing is accelerated at room temperature, and aminopropyltriethoxysilane is more preferred from the viewpoint of curing speed and stability. In the case of alkoxy groups, all catalysts sufficiently progress the curing reaction at room temperature, but metal compounds that are effective with smaller amounts are preferred, and among them, aluminum compounds, titanium compounds, and zinc compounds are more preferred from the viewpoint of curing speed.

[0030] These curing catalysts can be added in any ratio to adjust the curing speed and curing temperature, but generally, it is preferable that the amount is within the range of 0.01 to 10% by mass based on the polysilazane compound.

[0031] [Additives] In addition to the curing catalyst, additives may be added to the polysilazane compound of the present invention as necessary.Additives include, for example, metal fillers containing metal elements such as magnesium, aluminum, titanium, vanadium, chromium, manganese, iron, cobalt, zinc, gallium, zirconium, niobium, palladium, platinum, etc., reinforcing inorganic fillers such as fumed silica, fumed titanium dioxide, fumed alumina, etc., non-reinforcing inorganic fillers such as fused silica, alumina, zirconium oxide, calcium carbonate, calcium silicate, titanium dioxide, ferric oxide, zinc oxide, etc., ultraviolet reflectors, ultraviolet absorbers such as benzophenone, benzotriazole, triazine, etc., organosiloxane oligomers containing at least two, preferably two or three, functional groups selected from Si-H group, alkenyl group, alkoxysilyl group, and epoxy group, adhesive assistants such as organooxysilyl modified isocyanurate compounds and their hydrolysis condensates, silicone oils such as dimethyl silicone and phenyl silicone, etc., and can be added at any ratio.

[0032] [fiber] The fibers in the present invention are either only organic fibers or only inorganic fibers. These fibers provide the fibrous base material described below. Examples of organic fibers include regenerated fibers and synthetic fibers, and examples of inorganic fibers include glass fibers and carbon fibers.

[0033] [Fiber base material] The fibrous substrate in the present invention is a material obtained by entangling or weaving the above-mentioned fibers to form a flat shape, and is selected from paper, paperboard, or cloth. Examples of the fibrous substrate include newsprint used for newspapers, printing paper used for notebooks and copy paper, wrapping paper used for envelopes, shopping bags, rice bags, etc., sanitary paper used for tissue paper and toilet paper, Japanese paper such as calligraphy paper and shoji screens, paper such as glass fiber paper, paperboard such as cardboard base paper, paper boxes, and wrap cores, cloth such as cotton, nylon, linen, rayon, acrylic, polyester, and quartz fiber, wood such as cypress, pine, cedar, oak, beech, and zelkova, or molded products such as plywood, cellulose, and carbon nanofiber.

[0034] Among them, paper and paperboard are preferred because they are required to have strength but lose strength significantly when wet, and among them, cardboard base paper, which is mainly used for transporting goods, is particularly preferred.

[0035] [Method of treating fibrous substrate] In the fibrous substrate of the present invention, the fibers are coated (covered) with a cured product of a polysilazane compound. The cured product of the polysilazane compound is preferably at least one of an oxide, a nitride, and an oxynitride of the polysilazane compound. The oxide, the nitride, and the oxynitride of the polysilazane compound can be identified using FT-IR. There is no particular restriction on the method of covering the fibers with the cured product of the polysilazane compound, but it is required that the contact surface between the fibers is covered from the viewpoint of maintaining the strength when wetted with water. During the covering process, the polysilazane compound may be diluted with any solvent as necessary. Examples of the covering method include roll coating methods such as a chamber doctor coater, a single roll kiss coater, a reverse kiss coater, a bar coater, a reverse roll coater, a positive rotation roll coater, a blade coater, and a knife coater, spin coating methods, dispensing methods, dipping methods, spraying methods, transfer methods, and slit coating methods. In addition, when the above-mentioned coating methods cannot be used, a wiping coating method can be used in which the polysilazane compound is soaked into any cloth or paper and then applied to the substrate by hand. Each coating method has its own advantages and disadvantages, but the dip method, which can coat the entire fiber at once, is the most preferable.

[0036] The amount of coating is not particularly limited as long as the properties such as water resistance are exhibited, but generally, it is preferable that the amount is within the range of 0.001 to 0.5 g per 1 g of fibrous base material. If it is 0.001 g or more, the effect of coating on the fibers is exhibited, and if it is within 0.5 g, the texture of the fibrous base material is not impaired.

[0037] After the polysilazane compound is applied to the fibrous substrate in this manner, it is preferable to leave the substrate to harden the polysilazane compound. At this time, the hardening time can be shortened by simultaneously heating the substrate. The purpose of this step is to remove the solvent contained in the coating film and to promote hardening reactions such as hydrolysis, dehydration condensation, dehydrogenation condensation, and deammonia condensation of Si-H groups and alkoxy groups in the polysilazane. When heating, it is preferable to heat the substrate at 50 to 150°C. The time for which the step is left to stand is appropriately optimized depending on the conditions such as temperature and humidity, but it is preferable to leave the substrate to stand at least until the substrate is dry to the touch.

[0038] "Touch-dry" refers to the state in which the fingertip does not become dirty when lightly touched to the center of the coating surface, as described in JIS 5600-1-1:1999. EXAMPLES

[0039] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, parts refer to parts by mass. Room temperature refers to a temperature condition in the range of 5 to 35°C as described in JIS Z 8703:1993.

[0040] The substrates obtained in the following Examples 1 to 5 and Comparative Examples 1 to 6 were subjected to the following evaluations.

[0041] [exterior] The appearance of the coating was evaluated visually.

[0042] [Tensile evaluation] 1 g of water was dropped onto the bottom end of a 100 mm x 100 mm substrate using a dropper. After leaving it to stand for 5 minutes, the top end of the substrate was fixed and a jig measuring 30 mm x 20 mm was attached to the bottom end of the substrate. A weight was attached to the jig and the change in the substrate was observed. The evaluation results were based on the following index. No tears in the base material: 〇 There is some damage to the base material: △ Base material is broken: ×

[0043] [Example 1] One part of perhydropolysilazane with a weight average molecular weight of 4,215 as a polysilazane compound, 0.05 parts of aminopropyltriethoxysilane as a curing catalyst, and 99 parts of dibutyl ether as a dilution solvent were mixed, and a 100 mm x 100 mm x 5 mm thick cardboard base paper was impregnated with the mixture at room temperature for one minute. The cardboard base paper was then held by a clip and left hanging at room temperature for 24 hours. After that, it was confirmed by an optical microscope that the fibers of the cardboard base paper were coated with the cured product of the polysilazane compound (oxide, nitride, oxynitride), and identification was performed by FT-IR. The amount of coating per 1 g of cardboard base paper at this time was 0.01 g. Next, 1 g of water was dropped onto the cardboard base paper, and after 5 minutes the area on which the water had been dropped was pulled with a force of 9.8 N for evaluation; no change in appearance occurred.

[0044] [Example 2] 5 parts of perhydropolysilazane of Example 1 as a polysilazane compound, 0.25 parts of aminopropyltriethoxysilane as a curing catalyst, and 95 parts of dibutyl ether as a dilution solvent were mixed, and a 100 mm x 100 mm x 5 mm thick cardboard base paper was impregnated with the mixture at room temperature for 1 minute. Then, the cardboard base paper was held by a clip and left hanging at room temperature for 24 hours. Then, it was confirmed by an optical microscope that the fibers of the cardboard base paper were covered with the cured product of the polysilazane compound, and identification was performed by FT-IR. The amount of coverage per 1 g of cardboard base paper at this time was 0.05 g. Next, 1 g of water was dropped onto the cardboard base paper, and after 5 minutes the area on which the water had been dropped was pulled with a force of 9.8 N for evaluation; no change in appearance occurred.

[0045] [Example 3] One part of monomethyl polysilazane with a weight average molecular weight of 2,356 as a polysilazane compound, 0.008 parts of palladium propionate as a curing catalyst, 10 parts of anisole as a dilution solvent, and 89 parts of dibutyl ether were mixed, and a 100 mm x 100 mm x 5 mm thick cardboard base paper was impregnated with the mixture at room temperature for one minute. The cardboard base paper was then held by a clip and heated at 100°C for three hours while hanging. An optical microscope was then used to confirm that the fibers of the cardboard base paper were coated with the cured product of the polysilazane compound, and identification was performed using FT-IR. The amount of coating per 1 g of cardboard base paper at this time was 0.02 g. Next, 1 g of water was dropped onto the cardboard base paper, and after 5 minutes the area on which the water had been dropped was pulled with a force of 9.8 N for evaluation; no change in appearance occurred.

[0046] [Example 4] 5 parts of perhydropolysilazane of Example 1 as a polysilazane compound, 0.25 parts of aminopropyltriethoxysilane as a curing catalyst, and 95 parts of dibutyl ether as a dilution solvent were mixed, and a glass fiber paper of 100 mm x 100 mm x 0.05 mm thick was impregnated at room temperature for 1 minute. Then, the glass fiber paper was held by a clip and heated at 100 ° C. for 3 hours while hanging. Then, it was confirmed by an optical microscope that the fibers of the glass fiber paper were covered with the cured product of the polysilazane compound, and identification was performed by FT-IR. In addition, the amount of coverage per 1 g of glass fiber paper at this time was 0.04 g. Next, 1 g of water was dropped onto the glass fiber paper, and after 5 minutes the area on which the water had been dropped was subjected to a pulling test with a force of 0.50 N, but no change occurred in appearance.

[0047] [Example 5] 1 part of perhydropolysilazane of Example 1 as a polysilazane compound, 0.2 parts of silica fine powder dispersion (Nissan Chemical Co., Ltd., TOL-ST), 0.05 parts of aminopropyltriethoxysilane as a curing catalyst, and 99 parts of dibutyl ether as a diluting solvent were mixed, and a 100 mm x 100 mm x 5 mm thick cardboard base paper was impregnated with the mixture at room temperature for 1 minute. Then, the cardboard base paper was held by a clip and left hanging at room temperature for 24 hours. Then, it was confirmed by an optical microscope that the fibers of the cardboard base paper were covered with the cured product of the polysilazane compound, and identification was performed by FT-IR. In addition, the amount of coverage per 1 g of cardboard base paper at this time was 0.01 g. Next, 1 g of water was dropped onto the cardboard base paper, and after 5 minutes the area on which the water had been dropped was pulled with a force of 9.8 N for evaluation; no change in appearance occurred.

[0048] [Comparative Example 1] 1g of water was dropped onto a piece of cardboard paper measuring 100mm x 100mm x 5mm thick. After 5 minutes, the area on which the water had been dropped was pulled with a force of 9.8N, causing the cardboard paper to break.

[0049] [Comparative Example 2] 1 g of water was dropped onto a piece of glass fiber paper measuring 100 mm x 100 mm x 0.05 mm thick. After 5 minutes, the area on which the water was dropped was subjected to a pulling test with a force of 0.50 N, and the glass fiber paper broke.

[0050] [Comparative Example 3] 5 parts of perhydropolysilazane of Example 1 as a polysilazane compound, 0.25 parts of aminopropyltriethoxysilane as a curing catalyst, and 95 parts of dibutyl ether as a dilution solvent were mixed, and a 100 mm×100 mm×5 mm thick cardboard linerboard was impregnated at room temperature for 1 minute. The amount of coating before curing per 1 g of cardboard linerboard was 0.04 g. Afterwards, 1 g of water was dropped onto the cardboard before the polysilazane hardened, and after 5 minutes the area where the water had been dropped was pulled with a force of 9.8 N, resulting in the cardboard rupture. When the fibers of the cardboard were examined using an optical microscope and FT-IR, it was found that the polysilazane compound had adhered, but almost no hardened product of the polysilazane compound had formed.

[0051] [Comparative Example 4] Five parts of dimethyl silicone resin and 95 parts of toluene as a dilution solvent were mixed, and a 100 mm x 100 mm x 5 mm thick cardboard base paper was impregnated at room temperature for one minute. After that, it was confirmed with an optical microscope that the fibers of the cardboard base paper were coated with dimethyl silicone resin. The amount of coating per 1 g of cardboard base paper at this time was 0.07 g. Next, after the solvent had dried, 1 g of water was dropped onto the cardboard base paper. After 5 minutes, the area where the water had been dropped was pulled with a force of 9.8 N and the cardboard base paper broke.

[0052] [Comparative Example 5] Five parts of tetraethoxysilane (TEOS), 0.01 parts of tetra-t-butoxytitanium as a curing catalyst, 50 parts of water as a dilution solvent, and 45 parts of methanol were mixed, and a 100 mm x 100 mm x 5 mm thick cardboard base paper was impregnated with the mixture at room temperature for one minute. The cardboard base paper was then held by a clip and heated at 100°C for three hours while hanging. After that, it was confirmed by an optical microscope that the fibers of the cardboard base paper were coated with oxides formed from TEOS. The amount of coating per 1 g of cardboard base paper at this time was 0.05 g. Next, 1 g of water was dropped onto the cardboard paper, and after 5 minutes the area on which the water had been dropped was subjected to a pulling test with a force of 9.8 N, resulting in the cardboard paper breaking.

[0053] [Comparative Example 6] Epoquick FC (manufactured by Buhler Co., Ltd.) was used as an epoxy resin and impregnated into a 100 mm x 100 mm x 5 mm thick cardboard base paper for 1 minute at room temperature. The cardboard base paper was then held by a clip and left hanging at room temperature for 24 hours. An optical microscope was then used to confirm that the fibers of the cardboard base paper were covered with the cured epoxy resin. At this time, the gaps between the fibers of the cardboard base paper were also filled with the cured epoxy resin, and the amount of coverage per 1 g of cardboard base paper was 0.5 g. Next, 1 g of water was dropped onto the cardboard base paper, and after 5 minutes the area on which the water had been dropped was subjected to a pulling force of 9.8 N for evaluation; no change occurred in the cardboard base paper.

[0054] The results of Examples 1-5 and Comparative Examples 1-6 are shown in Table 1. [Table 1]

[0055] From the results in Table 1, in Examples 1 to 3, 5 and Comparative Example 6, the cardboard paper maintained its original state in the tensile test after water was dropped. However, in Examples 1 to 3 and 5, there was no change in the appearance of the cardboard paper after coating, and the coating agent did not contain any organic resin that could lead to environmental pollution, whereas in Comparative Example 6, the appearance became glossy, and the coating agent itself was an organic resin. Furthermore, in Comparative Example 1 and Comparative Examples 3 to 5, the cardboard paper broke in the tensile test after water was dropped. This is thought to be due to insufficient fiber reinforcement by the coating agent.

[0056] On the other hand, in Comparative Example 2 and Example 4, glass fiber paper was used as the fibrous substrate for verification. Since glass fiber paper does not have glass fibers woven into it like glass cloth, it is very brittle and will break under its own weight just by lifting it, so the load for the tensile evaluation was lowered to 0.50 N. As a result, Comparative Example 2, which was not coated with polysilazane, broke easily during the test, but Example 4, which was coated with polysilazane, did not break.

[0057] These results show that the modified fibrous substrate of the present invention is extremely effective in maintaining the structure of the substrate without causing any change in appearance, and since it does not use organic resin-based materials that have a large environmental impact, it is possible to provide an environmentally friendly substrate.

[0058] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A modified fibrous base material, comprising fibers coated with a cured product of a polysilazane compound having a structure represented by the following formula (1), the fibers being composed only of organic fibers or only of inorganic fibers, and the fibrous base material being a cardboard base paper. 【Chemistry 1】 (In the formula, R 1 and R 2 are each a group selected from a hydrogen atom, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms, and may be the same or different. 1 Or R 2 At least one of the is a hydrogen atom bonded to a silicon atom.)

2. 2. The modified fibrous base material of claim 1, wherein the polysilazane compound is a perhydropolysilazane.

3. The modified fibrous base material according to claim 1 or 2, characterized in that the polysilazane compound further contains a curing catalyst.

4. 4. The modified fibrous base material according to claim 1, wherein the cured product of the polysilazane compound is at least one of an oxide, a nitride, and an oxynitride of the polysilazane compound.

Citation Information

Patent Citations

  • Silicon nitride fiber-reinforced composite material

    JP1989210428A

  • Fiber reinforced metal matrix composite

    JP1992013824A

  • Corrugated fiberboard box for frozen food

    JP2005193934A

  • Antifouling, nonflammable flexible film material

    JP2006272660A

  • Method for manufacturing corrugated cardboard and paper container using the same

    JP2013095058A