Metal oxide particles coated with rare earth oxides and method for their preparation by flame spray pyrolysis - Patents.com
Metal oxide particles with a core/shell structure, prepared via flame spray pyrolysis, address the instability issue by maintaining UV protection and water resistance, ensuring long-term effectiveness in aqueous compositions.
Patent Information
- Application Number
- JP2022539239
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-27
- Filing Date
- 2020-12-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Metal oxides used in applications such as cosmetics and electronics suffer from instability over time, particularly when exposed to water, leading to degradation and loss of UV protection properties.
Metal oxide particles with a core/shell structure are prepared using flame spray pyrolysis, where the core is composed of metals like titanium or iron oxides, and the shell is made of rare earth oxides such as cerium or yttrium oxides, providing a stable coating that covers at least 90% of the core surface.
The coated particles maintain good optical properties for UV protection and water resistance, preventing degradation and ensuring long-term effectiveness in aqueous compositions.
Smart Images

Figure 0007564215000004 
Figure 0007564215000001 
Figure 0007564215000002
Abstract
Description
[Technical field]
[0001] The present invention relates to coated metal oxide particles, a process for the preparation of such coated particles by a flame spray pyrolysis technique, metal oxide particles obtainable by such a process, compositions comprising such particles, and uses thereof. [Background technology]
[0002] Metal oxides are used in many applications (cosmetics, paints, stains, electronics, rubber, etc.) especially for their optical properties, and especially for their light absorbing and / or scattering properties to protect surfaces from UV radiation and / or to convert ambient light into electricity.
[0003] However, metal oxides have the disadvantage of being particularly unstable over time. For example, zinc oxide can convert to zinc hydroxide and even to Zn in the presence of water, either from the composition containing it or from atmospheric moisture. 2+ Such decomposition has the effect of partially or even completely dissolving zinc oxide in water and significantly reducing or even eliminating the desirable properties of zinc oxide.
[0004] This instability is particularly problematic when metal oxides are used in photoprotective cosmetic compositions: as the metal oxide decomposes, UV protection actually decreases.
[0005] It has been considered to coat metal oxides with silica, especially using a sol-gel process, or to graft fluoro compounds onto metal oxides. However, these solutions are not entirely satisfactory. Metal oxides coated with silica by a sol-gel process generally have worse optical properties than uncoated particles. As for the grafting techniques, the use of fluoro compounds is harmful to the environment and can be dangerous to the user.
[0006] It is also known to use flame spray pyrolysis (FSP) to prepare metal oxide particles.
[0007] Flame spray pyrolysis or FSP is a currently well-known method that has been essentially developed to synthesize ultrafine powders of single or mixed oxides of various metals (e.g. SiO2, Al2O3, BO, ZrO2, GeO2, WO3, Nb2O5, SnO2, MgO, ZnO) with controlled morphology and / or to deposit them on various substrates by starting from various metal precursors, usually in the form of organic or inorganic, preferably non-flammable, sprayable liquids. The liquid sprayed into the flame releases nanoparticles of metal oxides that are sprayed onto these various substrates by combustion, and in particular by the flame itself. The principle of this method is recalled, for example, in a recent (2011) publication by Johnson Matthey (J. Appl. Phys. 1999, 143:1311-1323, 2001). Numerous variants of FSP processes and reactors are also described, for example, in the following patents or patent applications: WO 2005 / 023636, WO 2005 / 023636, WO 2005 / 023637, WO 2005 / 023638, WO 2005 / 023639 ...
[0008] However, this method utilized for the preparation of metal oxides still leaves room for perfection, in particular to improve the stability of the metal oxide particles over time and, more particularly, their resistance to water.
[0009] Furthermore, a scientific paper by Han Gao et al. describes particles that include a layer of CeO2 disposed on the TiO2 particles in order to reduce the formation of radicals resulting from the interaction between TiO2, light and the external environment. However, this type of particle is coated with a very thin layer of cerium oxide, which does not completely cover the TiO2 core (Non-Patent Document 2). These particles are not suitable because the cerium oxide layer does not cover the TiO2 core and cannot prevent the titanium oxide from coming into contact with the external environment, and in particular cannot prevent the release of titanium atoms found in the particle core. Another scientific paper concerns particles that combine an iron oxide core with a coating formed from cerium oxide and an acrylate polymer as a therapeutic material for inflammatory diseases (Non-Patent Document 3). The coating layer on top of the iron oxide core is a cluster of cerium oxide nanoparticles connected to each other by a polymer matrix based on acrylic monomers. This type of coating layer is not very stable, especially in water, because the acrylic polymer is solubilized and the cerium oxide nanoparticles peel off from the surface of the core, after which water has free access to the iron oxide.
[0010] There is therefore a real need to develop metal oxide particles that have good stability over time, in particular good water resistance, while maintaining good optical properties in terms of absorption and / or scattering of light, more particularly ultraviolet light; and to develop methods that allow the preparation of such particles. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] U.S. Pat. No. 5,958,361 [Patent Document 2] U.S. Patent No. 2,268,337 [Patent Document 3] International Publication No. 01 / 36332 Brochure [Patent Document 4] U.S. Patent No. 6,887,566 [Patent Document 5] International Publication No. 2004 / 005184 Brochure [Patent Document 6] U.S. Patent No. 7,211,236 [Patent Document 7] International Publication No. 2004 / 056927 Brochure [Patent Document 8] International Publication No. 2005 / 103900 Brochure [Patent Document 9] International Publication No. 2007 / 028267 Brochure [Patent Document 10] U.S. Patent No. 8,182,573 [Patent Document 11] International Publication No. 2008 / 049954 Brochure [Patent Document 12] U.S. Patent No. 8,231,369 [Patent Document 13] International Publication No. 2008 / 019905 Brochure [Patent Document 14] US Patent Application Publication No. 2009 / 0123357 [Patent Document 15] U.S. Patent Application Publication No. 2009 / 0126604 [Patent Document 16] US Patent Application Publication No. 2010 / 0055340 [Patent Document 17] International Publication No. 2011 / 020204 Brochure [Non-patent literature]
[0012] [Non-Patent Document 1] “Flame Spray Pyrolysis: a Unique Facility for the Production of Nanopowders”, Platinum Metals Rev.,2011,55,(2),149-151 [Non-Patent Document 2] Ind.Eng.Chem.Res.2014,53(1),189-197 [Non-Patent Document 3] Y.Wu et al.Journal of Materials Chemistry B.2018,6,pp 4937-4951 Summary of the Invention [Means for solving the problem]
[0013] These objects are achieved by the present invention, one subject of which is in particular metal oxide particles, in particular core / shell structured metal oxide particles of the M1-M2 oxide type, comprising a core 1 and one or more upper coating layers 2 covering said core 1, (i) the core 1 is composed of an oxide of at least one metal M1, preferably in a crystalline state; (ii) said upper coating layer 2 covers at least 90% of the surface of the core 1, preferably the entire surface of the core 1, and comprises one or more inorganic compounds containing one or more elements M2 and one or more oxygen atoms; (iii) said element M2 is different from the metal M1 and is selected from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and mixtures thereof; however, - if the core 1 consists of titanium oxide and the upper coating layer 2 consists of cerium oxide, the upper coating layer 2 is present in an amount greater than 1% by weight relative to the total weight of the particle; - the particles are different from particles comprising a core 1 made of iron oxide Fe3O4 and an upper coating layer 2 made of cerium oxide CeO2; It is understood that.
[0014] It has been observed that the coated metal oxide particles according to the present invention do not degrade appreciably over time in the presence of water when they are formulated in an aqueous composition.
[0015] It has also been observed that the metal oxide particles according to the invention have good optical properties with respect to light absorption and / or light scattering. More specifically, they have high UV absorption and low or high visible light scattering, thus allowing applications such as sun protection and / or visual appearance modification, while benefiting from resistance in the presence of water.
[0016] Furthermore, the compositions containing the coated metal oxide particles according to the invention showed good screening power, especially with regard to long and short UV-A radiation.
[0017] Furthermore, compositions comprising the coated metal oxide particles of the present invention have a particularly high transparency, which can prove advantageous when the composition is applied and then dried onto a coating, especially onto the skin.
[0018] In addition, the coated metal oxide particles according to the invention do not require a hydrophobic coating, which allows them to be used across a broad formulation spectrum (e.g. in fully aqueous and / or surfactant-free formulations), further reducing the risk of inappropriate deposition (on the edges of the sink, on the walls of the plumbing, or on rocks) when the formulations thus obtained end up in water (in sink drains, lakes, or the sea).
[0019] Another subject of the invention is a method for producing a composition comprising at least a. preparing a composition (A) by adding precursors of one or more metals M1 to a flammable solvent or mixture of flammable solvents; thereafter b. forming a flame in a flame spray pyrolysis device by injecting composition (A) and an oxygen-containing gas until an aggregate of oxides of metal M1 is obtained; and c. injecting a composition (B) comprising precursors of one or more elements M2 into the flame until a coating layer comprising one or more elements M2 and one or more oxygen atoms is obtained on the surface of the aggregates of oxides of the metal M1, said element M2 being selected from scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof, preferably from cerium, yttrium, lanthanum, and mixtures thereof; The present invention relates to a method for preparing such metal oxide particles, in particular metal oxide grains of core / shell structure of the M1-M2 oxide type, comprising:
[0020] The method according to the invention makes it possible to obtain metal oxide particles coated with a layer of inorganic material based on element M2, which have been observed to be particularly stable over time and have good water resistance.
[0021] Moreover, unlike conventional coating methods, the method according to the invention has the advantage of preserving good intrinsic properties of the core despite the presence of the coating: in fact, due to the particular nature of the coating layer, at a given particle mass it is possible to reduce the proportion of metal oxide without degrading and / or adversely affecting the properties of said metal oxide.
[0022] Thus, the method of the present invention makes it possible to produce stable metal oxide particles while avoiding the disadvantages of the increased amounts of particles traditionally required to maintain the good optical properties of metal oxides.
[0023] The accompanying drawings are schematic diagrams, not necessarily to scale, and are intended to particularly illustrate the principles of the invention. [Brief description of the drawings]
[0024] [Figure 1] 1 depicts a cross-sectional view of a metal oxide particle according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Other objects, features, aspects and advantages of the present invention will become more apparent from reading the following description and examples.
[0026] Unless otherwise specified herein, - the term "at least one" is equivalent to and may be replaced by the term "one or more"; - the use of the word "between" is equivalent to and can be substituted for the word "in the range of" and indicates an inclusive limit; - the expression "keratinous materials" denotes in particular human keratinous fibres, such as the skin and hair; - The core (1) is also called the "center"; - the upper coating layer (2), also called the "outer layer", "shell" or "coating"; - "Alkyl" means an "alkyl group", i.e., C1-C 10 in particular C1-C8, more particularly C1-C6 and preferentially C1-C4, linear or branched hydrocarbon-based radicals, such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl or tert-butyl; - an "aryl" group is understood to mean a monocyclic or fused or non-fused polycyclic carbon-based group containing 6 to 22 carbon atoms, at least one ring of which is aromatic, preferentially an aryl group is phenyl, biphenyl, naphthyl, indenyl, anthracenyl or tetrahydronaphthyl, preferably phenyl; - An "arylate" group is one or more -C(O)O groups, such as naphthalate or naphthenate. - is understood to mean an aryl group containing a carboxylate group; - "complexed metal" is understood to mean that a metal atom forms a "metal complex" or "coordination compound" in which the metal ion corresponding to the central atom, i.e. M1, is chemically bound to one or more electron donors (ligands); - "ligand" is understood to mean a coordinating organic chemical group or compound, i.e. which contains at least one carbon atom, is capable of coordinating to the metal M1 and which, once coordinated or complexed, results in a metal compound (unique complex or chelate) that corresponds to the principle of a coordination sphere with a given number of electrons - see Ullmann's Encyclopedia of Industrial Chemistry, "Metal complex dyes", 2005, p. 1-42. More specifically, the ligand is an organic group that contains at least one group that is electron donating due to the inductive and / or mesomeric effect, more specifically having at least one electron donating group that is amino, phosphino, hydroxy or thiol, or the ligand is a persistent carbene, in particular of the "argengo" type (imidazol-2-ylidene), or contains at least one carbonyl group.The ligands may more specifically be: i) those containing at least one phosphorus atom -P<, i.e. phosphines such as triphenylphosphine; ii) bidentate ligands of the formula RC(X)-CR'R''-C(X)-R''', such as acetylacetone or β-diketones, where R and R'''' are the same or different and represent a linear or branched (C1-C6) alkyl group, R' and R'' are the same or different and represent a hydrogen atom or a linear or branched (C1-C6) alkyl group, preferentially R' and R'' represent a hydrogen atom, and X represents an oxygen atom, a sulfur atom or an N(R) group, where R represents a hydrogen atom or a linear or branched (C1-C6) alkyl group; iii) bidentate ligands of the formula [[HO-C(X)-R''', such as lactic acid, glycolic acid, tartaric acid, citric acid and maleic acid, as well as arylates (naphthalates, etc.). (Poly)hydroxycarboxylic acid ligands of the formula: AC(O)-OH (O)] (wherein A represents a monovalent group if the value of n is zero or a polyvalent group if n is 1 or more, which is saturated or unsaturated, cyclic or acyclic, aromatic or non-aromatic, based on a hydrocarbon containing 1 to 20 carbon atoms, optionally interrupted by one or more heteroatoms and / or optionally substituted, in particular substituted by one or more hydroxyl groups; preferably A represents a monovalent (C1-C6) alkyl group or a polyvalent (C1-C6) alkylene group, optionally substituted by one or more hydroxyl groups; n represents an integer between 0 and 10 (inclusive); preferably n is between 0 and 5, e.g. between 0, 1 or 2); and iv) C2-C alkyl groups containing 2 to 5 hydroxyl groups. 10 Polyol ligands, in particular ethylene glycol, glycerol, more particularly ligands further comprising carboxy, carboxylate or amino groups, in particular those selected from acetate, (C1-C6)alkoxylate, (di)(C1-C6)alkylamino, and arylate (such as naphthalate or naphthenate) groups.
[0027] The term "fuel" is understood to mean a liquid compound that burns in a chemical reaction using dioxygen and energy to produce heat: combustion. In particular, liquid fuels are selected from aprotic solvents, in particular alcohols such as methanol, ethanol, isopropanol, n-butanol, esters such as those derived from methyl esters and acetates (such as 2-ethylhexyl acetate), acids (such as 2-ethylhexanoic acid (EHA)), acyclic ethers (such as ethyl ether, methyl tert-butyl ether (MTBE), methyl tert-amyl ether (TAME), methyl tert-hexyl ether (THEME), ethyl tert-butyl ether (ETBE), ether tert-amyl ether (TAEE), diisopropyl ether (DIPE)), cyclic ethers (such as tetrahydrofuran (THF)), aromatic hydrocarbons or arenes (such as xylene), non-aromatic hydrocarbons, and mixtures thereof. The fuel may optionally be selected from liquefied hydrocarbons such as acetylene, methane, propane, or butane; and mixtures thereof.
[0028] metal oxide particles The metal oxide particles according to the invention, in particular metal oxide particles with a core / shell structure of the M1-M2 oxide type, comprise a core 1 composed of an oxide of at least one metal M1, preferably in the crystalline state.
[0029] Preferably, the metal M1 is selected from the elements of the second row of the Periodic Table of the Elements, titanium, zinc, copper, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium; more preferentially from magnesium, calcium, titanium, zinc, copper, cerium and yttrium.
[0030] According to the invention, the metal M1 is different from the element M2.
[0031] The crystalline state of Core 1 and its composition can be determined, for example, by conventional X-ray diffraction methods.
[0032] Advantageously, the core 1 of the particle according to the invention is composed of one or more aggregates of crystalline primary particles of an oxide of at least one metal M1, in other words, the core 1 is composed of a plurality of crystallites of an oxide of at least one metal M1.
[0033] The metal oxide particles according to FIG. 1 are composed of an oxide of at least one metal M1 in a crystalline state and contain one or more aggregates of primary particles of the oxide of at least one metal M1 and have a mean diameter D m Includes Core 1.
[0034] The metal oxide particles according to FIG. 1 completely cover the surface of the core 1 and have an average thickness d m It also includes a top coating layer 2 having
[0035] Number average diameter of core 1 D m can be determined, for example, by transmission electron microscopy (abbreviated as TEM). Preferably, the number-average diameter D m is in the range of 3 to 1000 nm, more preferentially 6 to 50 nm, and even more preferentially 10 to 30 nm.
[0036] The metal oxide particles according to the invention comprise one or more upper coating layers 2 covering at least 90% of the surface of the core 1 .
[0037] The degree of coverage of the core by the upper coating layer can be determined, for example, by visual analysis of the TEM-BF or STEM-HAADF type combined with a STEM-EDX analysis.
[0038] Each analysis is carried out on a statistical number of particles, in particular at least 20 particles. The particles are deposited on a metal grid made of a metal different from the metal that forms part of the particle, whether in the core or in the upper coating layer. For example, the grid is made of copper (unless it is desired to use copper in the manufacture of the particles).
[0039] Visual analysis of the TEM-BF and STEM-HAADF images allows one to infer, based on contrast, whether the coating completely surrounds the core of the particle. The average coverage can be determined by analyzing each of 20 (or more) images to estimate the coverage of the core, and then averaging.
[0040] By STEM-EDX analysis it is possible to verify that the coating indeed contains mainly or only the element M2. To do this it is necessary to carry out measurements at the edge of the grains (for at least 20 grains). These measurements then reveal the element M2.
[0041] STEM-EDX analysis also makes it possible to verify that the core is indeed free of metal M1. To do this, measurements must be made in the center of the particles (for at least 20 particles). These measurements then reveal metal M1 and element M2.
[0042] Preferably, the top coating layer 2 completely covers the surface of the core 1 .
[0043] The upper coating layer 2 comprises one or more inorganic compounds containing one or more elements M2 and one or more oxygen atoms.
[0044] Said element M2 is different from the metal M1.
[0045] The element M2 belongs to the group of rare earth elements in the +III oxidation state, which is selected from the group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof.
[0046] Preferably, element M2 is selected from cerium, yttrium, lanthanum, and mixtures thereof.
[0047] According to a first particular embodiment of the invention, element M2 is preferably cerium.
[0048] According to another particular embodiment of the invention, the element M2 is preferably yttrium.
[0049] According to yet another particular embodiment of the invention, the element M2 is lanthanum.
[0050] According to yet another particular embodiment of the invention, the metal oxide particle comprises a core 1 composed of yttrium oxide and an upper coating layer 2 comprising cerium oxide.
[0051] Number average thickness of the upper coating layer d m can also be determined by transmission electron microscopy.
[0052] Preferably, the number average thickness d m is in the range of 1 to 30 nm, more preferentially 1 to 15 nm, and even more preferentially 1 to 6 nm.
[0053] Advantageously, the upper coating layer 2 is amorphous.
[0054] Preferably, the upper coating layer 2 is composed of one or more oxides of at least one element M2; said oxide of at least one element M2 is different from said oxide of at least one metal M1.
[0055] More preferentially, the upper coating layer 2 is composed of cerium oxide CeO2, yttrium oxide Y2O3 and / or lanthanum oxide La2O3, and mixtures of these oxides.
[0056] Particularly preferably, the particles according to the invention comprise an upper coating layer 2 consisting of an oxide of an element M2 selected from cerium oxide CeO2, yttrium oxide Y2O3 and / or lanthanum oxide La2O3.
[0057] Advantageously, the metal oxide particles according to the invention have a specific (M1 / M2) 粒子 It contains metal M1 and element M2 in a molar atomic ratio.
[0058] This ratio corresponds to the molar amount of metal M1 atoms present in one particle according to the invention relative to the molar amount of element M2 present in the other particle according to the invention.
[0059] This ratio can be determined by spectroscopic analysis according to one of two methods: according to the first method, the powder is spread and an X-ray fluorescence measurement study is carried out with an X-ray spectrometer, from which the metal ratio is deduced; according to the other method, the particles of the invention are dissolved beforehand in acid; then, on the material obtained, an elemental analysis is carried out by ICP-MS (Inductively Coupled Plasma Mass Spectroscopy), from which the metal ratio is deduced.
[0060] Preferably, (M1 / M2) 粒子 The molar atomic ratio is 0.25 or more, more preferentially in the range of 0.25-99, even more preferentially in the range of 1-80, even more preferentially in the range of 3-20.
[0061] Preferably, the sum of the content of the oxide of metal M1 and the content of the oxide of element M2 is at least 99% by weight, based on the total weight of core 1 and upper coating layer 2.
[0062] The number average diameter of the particles according to the invention can also be determined by transmission electron microscopy. Preferably, the number average diameter of the particles according to the invention is in the range of 3 to 5000 nm, more preferentially 4 to 3000 nm, even more preferentially 5 to 1000 nm.
[0063] Preferably, the particles according to the invention have a BET specific surface area of 1 m 2 / g~350m 2 / g; preferentially 1m 2 / g~200m 2 / g; more preferentially 30-100m 2 / g.
[0064] According to a particular embodiment of the invention, the metal oxide particles according to the invention may optionally further comprise an additional coating layer covering the upper coating layer 2 and comprising at least one hydrophobic organic compound.
[0065] The hydrophobic organic compound contained in the additional coating layer is more preferentially selected from silicones, in particular silicones containing at least one fatty chain; carbon-based derivatives containing at least 6 carbon atoms, in particular fatty acid esters; and mixtures thereof.
[0066] The additional coating layer can be produced by liquid or solid methods. By liquid methods, hydroxyl functional groups react with reactive functional groups of the compound forming the coating (typically silanol functional groups of silicones or acid functional groups of carbon-based fatty materials). By solid methods, the particles are contacted with a liquid or pasty compound containing a hydrophobic material.
[0067] Preferably, the metal oxide particles according to the invention are obtained by the inventive preparation process described below.
[0068] Method for preparing coated metal oxide particles Another subject of the invention relates to a method for the preparation of metal oxide particles, in particular core / shell structured metal oxide particles of the M1-M2 oxide type, comprising at least one step a. of preparing a composition (A), followed by step b. of forming a flame and step c. of spraying composition (B).
[0069] Step a. of the method according to the invention consists of preparing a composition (A) by adding one or more precursors of the metal M1 to a flammable solvent or a mixture of flammable solvents.
[0070] Preferably, the metal M1 is selected from the elements of the second row of the Periodic Table of the Elements, titanium, zinc, copper, scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium; more preferentially from magnesium, calcium, titanium, zinc, copper, cerium and yttrium.
[0071] According to the invention, the metal M1 is different from the element M2.
[0072] The metal M1 precursors and flammable solvents that can be used according to the invention can be selected from the metal M1 precursors and flammable solvents conventionally used in flame spray pyrolysis.
[0073] Preferably, the metal M1 precursor contained in composition (A) comprises one or more metal M1 atoms optionally complexed with one or more ligands comprising at least one carbon atom.
[0074] More preferentially, the ligand is an acetate, a (C1-C6) alkoxylate, a (C2-C 10 )alkyl carboxylate, (di)(C1-C6)alkylamino, and arylate (such as naphthalate or naphthenate) groups.
[0075] Preferably, the flammable solvent is selected from protic flammable solvents, aprotic flammable solvents, and mixtures thereof; more preferentially, from alcohols, esters, acids, acyclic ethers, cyclic ethers, aromatic hydrocarbons or arenes, non-aromatic hydrocarbons, and mixtures thereof; and even more preferably, from 2-ethylhexyl acetate, 2-ethylhexanoic acid (EHA), ethyl ether, methyl tert-butyl ether (MTBE), methyl tert-amyl ether (TAME), methyl tert-hexyl ether (THEME), ethyl tert-butyl ether (ETBE), ether tert-amyl ether (TAEE), diisopropyl ether (DIPE), tetrahydrofuran (THF), xylene, and mixtures thereof.
[0076] Particularly preferably, the flammable solvent is selected from aprotic flammable solvents containing at least 3 carbon atoms and mixtures thereof; more preferably, from xylene, tetrahydrofuran, 2-ethylhexyl acetate, 2-ethylhexanoic acid (EHA), and mixtures thereof.
[0077] Advantageously, the content of precursor of metal M1 in composition (A) ranges from 1% to 60% by weight, preferably from 15% to 30% by weight, relative to the total weight of composition (A).
[0078] The preparation method according to the present invention further comprises step b. of injecting composition (A) and an oxygen-containing gas into a flame spray pyrolysis (FSP) device to form a flame.
[0079] During this step b., the composition (A) and the oxygen-containing gas are advantageously injected into the flame spray pyrolysis device by two jets separated from each other, in other words, the composition (A) and the oxygen-containing gas are injected separately, i.e., the composition (A) and the oxygen-containing gas are not injected by a single nozzle.
[0080] More specifically, composition (A) is transported through one tube, while an oxygen-containing gas (also called "dispersed oxygen") is transported through another tube. The inlets of the two tubes are positioned such that the oxygen-containing gas creates a negative pressure that draws up composition (A) and converts it into droplets by the Venturi effect.
[0081] Step b. may optionally further comprise the injection of an additional "premix" mixture comprising oxygen and one or more combustible gases. This "premix" mixture (also called "support flame oxygen") allows the generation of a support flame intended to ignite and sustain the flame arising from composition A and the oxygen-containing gas (i.e., "dispersed oxygen").
[0082] Preferably, during step b., composition (A), the oxygen-containing gas and the optional "premix" mixture, if present, are injected into a reaction tube (also called "filled tube"). Preferably, this reaction tube is made of metal or quartz. Advantageously, the reaction tube has a height of at least 30 cm, preferably at least 40 cm and more preferentially at least 50 cm. Preferentially, the length of said reaction tube is between 30 cm and 300 cm, in particular between 40 cm and 200 cm, more particularly between 45 cm and 100 cm, for example 50 cm.
[0083] The mass ratio between the mass of the solvent present in the composition (A), on the one hand, and the mass of the oxygen-containing gas, on the other hand, is defined as follows: First, the amount of oxygen-containing gas (also called oxidizer compound) is calculated for the assembly formed by composition (A) (i.e. combustible solvent and precursor of metal M1 on the one hand, and oxygen-containing gas on the other hand) so that they can react together in a combustion reaction in a stoichiometric ratio (and therefore without too much or too little oxidizer compound). Starting from this calculated amount of oxygen-containing gas (also called "calculated oxidizer"), a new calculation is carried out to derive from this the amount of oxygen-containing gas injected (also called "injected oxidizer") according to the following formula: Injected oxidizer = calculated oxidizer / φ (φ is preferably 0.3 to 0.9, more preferentially 0.4 to 0.65).
[0084] This method is defined inter alia by Turns, S. R. in An Introduction to Combustion: Concepts and Applications, 3rd ed.; McGraw-Hill: New York, 2012.
[0085] The preparation method according to the invention further comprises a step c. which comprises injecting into the flame formed during step b. a composition (B) comprising one or more element M2 precursors.
[0086] The injection of composition (A) and the injection of composition (B) are preferably simultaneous, in other words the method of the invention is continuous and the flame formed in step b. is maintained.
[0087] Preferably, the flame formed during step (b) is at a temperature of 2000° C. or greater in at least a part of the flame.
[0088] At the point of injection of composition (B) into the flame formed in step b. and maintained in step c., i.e. during step c., the temperature is preferably between 200°C and 800°C, more preferentially between 400°C and 500°C.
[0089] Advantageously, during step c., composition (B) is injected from the above-mentioned atomizing ring placed above the reaction tube, where the injection of composition (A) is particularly performed. More preferentially, an additional tube is placed in the series of reaction tube and atomizing ring, which in turn is placed above the atomizing ring, which is itself placed above the reaction tube.
[0090] According to this preferred embodiment, this additional tube is made of metal or quartz. Advantageously, this additional tube has the same diameter as the reaction tube and a height of at least 30 cm, preferably at least 40 cm and more preferentially at least 50 cm. Preferentially, the length of said additional tube is between 30 cm and 300 cm, in particular between 40 cm and 200 cm, more particularly between 45 cm and 100 cm, for example 50 cm.
[0091] As indicated above, the element M2 belongs to the group of rare earth elements in the +III oxidation state, which is selected from the group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and mixtures thereof.
[0092] Preferably, element M2 is selected from cerium, yttrium, lanthanum, and mixtures thereof.
[0093] According to a first particular embodiment of the invention, element M2 is preferably cerium.
[0094] According to another particular embodiment of the invention, the element M2 is preferably yttrium.
[0095] According to yet another particular embodiment of the invention, the element M2 is lanthanum.
[0096] Preferably, the precursor of element M2 comprises one or more atoms of element M2, optionally complexed with one or more ligands.
[0097] Preferably, the ligand is an acetate, a nitrate, a (C1-C6) alkoxylate, a (C2-C 10 )alkyl carboxylate, (di)(C1-C6)alkylamino, and arylate (such as naphthalate or naphthenate) groups.
[0098] The precursor of element M2 may be selected from halides of element M2.
[0099] During the method according to the invention, (M1 / M2) 噴射 A molar atomic ratio can be calculated, which corresponds to the molar amount of metal M1 atoms injected during step b. on the one hand relative to the molar amount of element M2 injected during step c. on the other hand.
[0100] Preferably, (M1 / M2) 噴射 The molar atomic ratio is 0.25 or more; more preferentially in the range of 0.25-120; even more preferentially in the range of 0.25-99; even more preferentially in the range of 1-80; even more preferentially in the range of 3-20.
[0101] Preferably, nitrogen (N2) is bubbled into the above-mentioned composition (B) before the injection during step c. In this case, the injection rate of the composition (B) can be controlled by controlling the temperature and the flow rate of the bubbler.
[0102] According to one particular embodiment of the invention, said composition (B) is brought to a temperature ranging from 25° C. to 70° C., more preferentially from 30° C. to 60° C., before its injection during step c.
[0103] Preferably, the content of element M2 precursor in composition (B) injected during step c. of the method according to the invention is between 1% and 60% by weight, more preferentially between 5% and 30% by weight, relative to the total weight of composition (B).
[0104] Advantageously, composition (B) may also comprise one or more solvents. Preferably, the solvent present in composition (B) is chosen from polar protic solvents other than water, and more preferentially from (C1-C8) alkanols. More preferentially, composition (B) comprises ethanol.
[0105] According to a preferred embodiment of the present invention, the solvent present in composition (B) is selected from solvents which are flammable at the flame temperature of step c., and which are preferably flammable at temperatures between 200° C. and 800° C., and more preferentially between 400° C. and 500° C. More preferably, the solvent present in composition (B) has a boiling point above room temperature (25° C.), even in the range of 50° C. to 120° C.
[0106] Preferably, the content of solvent present in composition (B) sprayed during step c. of the method according to the invention is between 40% and 99% by weight, more preferentially between 50% and 98% by weight and even more preferentially between 70% and 95% by weight, relative to the total weight of composition (B).
[0107] According to a preferred embodiment of the present invention, the preparation method may further comprise a step d. of calcining the metal oxide particles obtained after step c.
[0108] According to this embodiment, during the firing step d. (i) the calcination lasts preferably for 60 to 400 minutes, more preferentially for 60 to 180 minutes; and / or (ii) The temperature range is preferably from 100°C to 600°C, more preferentially from 300°C to 600°C.
[0109] According to one particular embodiment of the invention, the particles obtained by the preparation method according to the invention are doped. According to this embodiment, composition (A) further comprises one or more precursors of an element D different from the metal M1 and from the element M2, D being selected from fluorine, vanadium, zirconium, hafnium, iron and tungsten.
[0110] Another subject of the present invention relates to a composition, preferably a cosmetic composition, comprising one or more metal oxide particles as defined above and / or preferably obtained by a process according to the invention.
[0111] The composition of the invention may be in various galenic forms: it may thus be in the form of a powder (pulverulent) composition, or a liquid composition, or in the form of a milk, cream, paste or aerosol composition.
[0112] The composition according to the invention is in particular a cosmetic composition, i.e. the material according to the invention is a cosmetic medium. The term "cosmetic medium" means a medium suitable for application to keratinous materials, in particular human keratinous materials such as the skin, said cosmetic medium generally consisting of water or a mixture of water and one or more organic solvents or a mixture of organic solvents.
[0113] The composition according to the invention is advantageously an aqueous composition.
[0114] Preferably, the composition comprises water in a content ranging from 5% to 95%, inclusive, in particular relative to the total weight of the composition.
[0115] The term "organic solvent" means an organic substance that can dissolve another substance without being chemically altered.
[0116] Examples of organic solvents include lower C2-C6 alkanols, such as ethanol and isopropanol; polyols and polyol ethers, such as 2-butoxyethanol, propylene glycol, propylene glycol monomethyl ether, and diethylene glycol monoethyl ether and monomethyl ether, as well as aromatic alcohols, such as benzyl alcohol or phenoxyethanol, and mixtures thereof.
[0117] Preferably, the organic solvent is present in the composition according to the invention in a content of from about 0.1% to 40% by weight (inclusive) relative to the total weight of the composition, more preferentially from about 1% to 30% by weight and even more particularly from 5% to 25% by weight (inclusive) relative to the total weight of the composition.
[0118] The compositions of the invention may comprise a fatty phase and may be in the form of a direct or inverse emulsion.
[0119] The compositions according to the invention may be prepared in the form of simple or multiple emulsions (abbreviated as oil-in-water or O / W, water-in-oil or W / O, oil-in-water-in-oil or O / W / O, or water-in-oil-in-water or W / O / W), such as creams, milky or creamy gels, according to techniques well known to those skilled in the art.
[0120] According to a particular embodiment of the present invention, the composition according to the present invention may be in the form of an anhydrous composition, for example in the form of an oil.The term "anhydrous composition" is intended to mean a composition that contains less than 2% by weight of water, preferably less than 1% by weight of water, and even more preferentially less than 0.5% by weight of water, relative to the total weight of the composition, or even a composition that does not contain water.In this type of composition, the water that may be present corresponds to the residual water that is not added during the preparation of the composition, but is brought about by the mixed components.
[0121] The metal oxide particles according to the invention may be in dry form (powder, flakes, plates), as a dispersion, or as a liquid suspension, or as an aerosol. The metal oxide particles according to the invention may be used as such or in admixture with other components.
[0122] Preferably, the composition of the invention comprises from 0.1% to 40% by weight, more preferentially from 0.5% to 20% by weight, even more preferentially from 1% to 10% by weight, even more preferentially from 1.5% to 5% by weight of metal oxide particles relative to the total weight of the composition.
[0123] Another subject of the invention is a composition according to the invention, preferably a cosmetic composition, for use in protecting the skin, in particular human skin, against visible light (i.e. wavelengths between 400 nm and 800 nm) and / or ultraviolet light (i.e. wavelengths between 100 nm and 400 nm), UV-A radiation (i.e. wavelengths between 320 nm and 400 nm) and / or UV-B radiation (i.e. wavelengths between 280 nm and 320 nm). The compositions according to the invention make it possible to efficiently screen solar radiation, which are broad-spectrum, in particular for UV-A radiation (including long-wave UV-A radiation), whilst being particularly stable over time under UV exposure.
[0124] The composition according to the invention may optionally contain, besides the metal oxide particles according to the invention, one or more additional UV filters chosen from hydrophilic, lipophilic or insoluble organic UV filters and / or one or more inorganic pigments, which will preferentially consist of at least one hydrophilic, lipophilic or insoluble organic UV filter.
[0125] The composition of the invention can be used in a single application or in multiple applications. When the composition of the invention is intended for multiple applications, the content of particles of oxide of element M of the invention is usually lower than in compositions intended for single applications.
[0126] For the purposes of the present invention, the term "single application" means a single application of the composition, which application is optionally repeated several times a day, each application being separated from the next by one or more hours, if desired, or a single application per day.
[0127] For purposes of the present invention, the term "multiple applications" refers to multiple repeated applications of the composition, usually 2 to 5 times, with each application separated by a few seconds to a few minutes from the next application. Each multiple application can be repeated multiple times a day, separated by an hour or more from the next application, or once a day, as needed.
[0128] Apply process The metal oxide particles of the present invention are agents for protection against UVA and UVB radiation. They particularly improve the overall blocking of UV radiation while maintaining good overall transmission in the visible range and excellent transparency in the visible range (400-780 nm).
[0129] The metal oxide particles of the invention are used in particular in cosmetic compositions intended for application to keratinous materials, in particular human keratinous materials such as the skin, preferably in a concentration of 0.1% to 40% by weight relative to the total weight of the composition containing them, and more preferentially 0.5% to 20% by weight relative to the total weight of the composition containing them.
[0130] The composition may be in any galenic form.
[0131] The metal oxide particles of the present invention may be applied to the keratinous material as a single application or as multiple applications. For example, a cosmetic composition comprising the metal oxide particles of the present invention may be applied in one application.
[0132] According to another variant, the application process comprises several successive applications of a cosmetic composition comprising one or more metal oxide particles according to the invention onto the keratin materials.
[0133] They may be a saturated single application, i.e. a single application of a cosmetic composition comprising a high concentration of metal oxide particles according to the invention, or connected application methods such as multiple applications of (lower concentrations) cosmetic compositions comprising one or more metal oxide particles of the invention, in which case multiple successive applications of the cosmetic composition comprising one or more metal oxide particles of the invention may be repeated with or without a delay between applications.
[0134] Another subject of the invention is a process for treating keratinous materials, and in particular human keratinous materials such as the skin, by applying a composition as defined above to the material, preferably by 1 to 5 successive applications, with drying between the layers, the application being by spraying or in other manner.
[0135] According to one embodiment of the present invention, multiple applications are performed on the keratinous material with a drying step between successive applications of the cosmetic composition comprising the metal oxide particles of the present invention. The drying step between successive applications of the cosmetic composition comprising one or more metal oxide particles of the present invention can be performed outdoors or artificially, for example using a hot air drying system such as a hair dryer.
[0136] Another subject of the invention is the use of metal oxide particles as defined above and / or obtainable by the preparation process defined above, for formulating a cosmetic or pharmaceutical composition, in particular having an antiperspirant or pH-regulating effect on the skin or intended to protect the skin against visible and / or ultraviolet light or to modify the appearance of the skin.
[0137] Another subject of the invention is the use of one or more metal oxide particles according to the invention as defined above as UV-A and UV-B screening agents for protecting keratinous materials, and in particular the skin.
[0138] The following examples serve to illustrate the invention without being limiting in nature. EXAMPLES
[0139] Example 1: 1.1 First, a composition (A) of zinc naphthenate (550 mM) in xylene was prepared.
[0140] The previously prepared composition (A) was then used to prepare uncoated zinc oxide particles P1 (outside the invention) using a conventional FSP preparation process Prep1.
[0141] Next, using the same composition (A) and a composition (B) containing cerium(III) nitrate hexahydrate (500 mM) and ethanol, zinc oxide particles P2 coated with cerium dioxide were prepared using the preparation process Prep2 according to the present invention (present invention).
[0142] The parameters for the Prep1 process are as follows: - Ratio (composition (A) / O2) = 5 mL / min of composition (A) and 7 L / min of gas (O2). To adjust the oxygen flow rate, use φ=0.45.
[0143] The parameters of the Prep2 process are as follows: - Ratio (composition (A) / O2) = 5 mL / min of composition (A) and 7 L / min of gas (O2). To adjust the oxygen flow rate, use φ=0.45.
[0144] In this Prep2 process, a quartz tube with a height of 40 cm is used to spray composition (A). A spray ring is placed above the quartz tube to spray composition (B). The diameter of the quartz tube and the spray ring is 10 cm.
[0145] Furthermore, nitrogen is first blown into composition (B). When composition (B) is sprayed, it allows evaporation of cerium (III) nitrate hexahydrate, (Zn / Ce) 噴射 The flow of nitrogen heated to 30-40 °C is adjusted so that the molar atomic ratio is 5.7.
[0146] 1.2 After the particles were prepared, it was observed that the resulting zinc oxide particles were crystalline.
[0147] Furthermore, the particles obtained according to the process Prep2 according to the invention are coated with cerium dioxide, (Zn / Ce) 粒子 The molar atomic ratio of is 5.7.
[0148] The BET specific surface area of the particles produced by process Prep2 is 50m 2 / g. The particles from process Prep2 have a number average diameter of 22 nm.
[0149] 1.3 Water resistance rating: A first aqueous suspension S1 (pH=8 by addition of sodium hydroxide) was prepared from particles P1 and water with a content of 1 g of P1 per liter of water. Similarly, a second aqueous suspension S2 (pH=8 by addition of sodium hydroxide) was prepared from particles P2 and water with a content of 1 g of P2 per liter of water.
[0150] Each suspension S1 and S2 was then placed in an ultrasonic bath for 10 minutes at a power of 20 W.
[0151] Then, the Zn present in the suspension as a function of time 2+ The ionic content is determined for each suspension by conventional anodic stripping voltammetry.
[0152] The results are listed in the table below:
[0153] [Table 1]
[0154] It is noted that the coated zinc oxide particles P2 obtained according to the preparation process Prep2 according to the invention have a much better water resistance than the uncoated zinc oxide particles P1 obtained according to the comparative preparation process Prep1.
[0155] In particular, no preferential precipitation (Ce vs. Zn) or preferential dissolution was observed for coated zinc oxide particles P2 (invention) in suspension S2.
[0156] Example 2: 2.1 First, composition (A) of zinc naphthenate (550 mM) in xylene was prepared.
[0157] The previously prepared composition (A) was then used to prepare cerium dioxide coated zinc oxide particles P3 (invention) using the FSP preparation process Prep3.
[0158] The parameters for the Prep3 process are as follows: - Ratio (composition (A) / O2) = 5 mL / min of composition (A) and 7 L / min of gas (O2). To adjust the oxygen flow rate, use φ=0.45.
[0159] In the Prep3 process, a quartz tube with a height of 40 cm is used to spray composition (A). A spray ring is placed above the quartz tube to spray composition (B). In addition, an additional metal tube with a height of 30 cm is placed above the spray ring. The quartz tube, the additional metal tube, and the spray ring are all 10 cm in diameter.
[0160] Furthermore, nitrogen is first blown into composition (B). When composition (B) is sprayed, it allows evaporation of cerium (III) nitrate hexahydrate, (Zn / Ce) 噴射 The flow of nitrogen heated to 30-40 °C is adjusted so that the molar atomic ratio is 5.7.
[0161] Next, a part of the prepared particles P3 was taken out and subjected to an additional calcination step at 500° C. for 1 hour to obtain zinc oxide particles P4 coated with cerium dioxide (the present invention).
[0162] 2.2 After the particles were prepared, it was observed that the resulting zinc oxide particles P3 and P4 were crystalline.
[0163] Furthermore, the particles P3 and P4 according to the invention are coated with cerium dioxide (Zn / Ce) 粒子 The molar atomic ratio of is 5.7. The BET specific surface area of particle P3 is 44m 2 / g. The BET specific surface area of particle P4 is 40m 2 / g. The number average diameter of particles P3 is 23 nm. The number average diameter of particles P4 is 26 nm.
[0164] 2.3 Evaluation of water resistance A third aqueous suspension S3 (pH=8 by addition of sodium hydroxide) was prepared from particles P3 and water with a content of 1 g of particles P3 per liter of water.
[0165] Similarly, a fourth aqueous suspension S4 (pH=8 by addition of sodium hydroxide) was prepared from particles P4 and water with a content of 1 g of particles P4 per liter of water.
[0166] Each suspension S3 and S4 was then placed in an ultrasonic bath for 10 minutes at a power of 20 W.
[0167] Thereafter, the Z present in suspension S1 of Example 1 and in suspensions S3 and S4 2+ The content of ions as a function of time and compared to the amount of zinc introduced was measured by conventional anodic stripping voltammetry for each suspension.
[0168] The results are listed in the table below.
[0169] [Table 2]
[0170] It is noted that the coated zinc oxide particles P3 and P4 according to the invention have better water resistance than the comparative uncoated zinc oxide particles P1.
[0171] In particular, no preferential precipitation (Ce vs. Zn) or preferential dissolution was observed for coated zinc oxide particles P3 and P4 (invention) in suspensions S3 and S4, respectively.
[0172] Example 3 Particles P1, P2, P3, and P4 from the previous two examples are used.
[0173] 200 mg of one type of particles P1-P4 was placed in 1 L of water to produce formulations F1 (based on particles P1), F2 (based on particles P2), F3 (based on particles P3), and F4 (based on particles P4). Spectra were then generated in the UV and visible ranges for these formulations F1-F4.
[0174] The following absorbances are noted:
[0175] [Table 3]
[0176] It is noted that formulations F2 and F3 according to the invention absorb less UV radiation than formulation F1 (comparative).
[0177] It is observed that formulation F4 according to the invention absorbs more UV radiation than formulation F1 (comparative).
[0178] A RAMAN investigation was performed on particles P1-P4. The Raman peaks of ZnO in particle P4 are much stronger (about three times stronger) than the Raman peaks of the reference ZnO.
[0179] The Raman peaks of ZnO in particles P2 and P3 are also observed.
[0180] Thus, the invention makes it possible in all cases to tailor the hiding power of the composition whilst having good stability in water.
Claims
1. A metal oxide particle comprising a core (1) and one or more upper coating layers (2) covering said core (1), (i) the core (1) is made of zinc oxide; (ii) the upper coating layer (2) covers at least 90% of the surface of the core (1) and comprises one or more inorganic compounds containing cerium and one or more oxygen atoms; The BET specific surface area of the metal oxide particles is 30 m 2 / g to 200m 2 / g, The number average diameter Dm of the core (1), as determined by transmission electron microscopy (TEM), is in the range of 3 to 1000 nm; Particles, wherein the number average thickness d m of said upper coating layer (2), as determined by transmission electron microscopy (TEM), is in the range of 1 to 30 nm.
2. 2. Particles according to claim 1, characterized in that the upper coating layer (2) consists of one or more oxides of cerium.
3. 3. Particle according to claim 2, characterized in that the sum of the zinc oxide content and the cerium oxide content is at least 99% by weight, based on the total weight of the core (1) and the upper coating layer (2).
4. Particles according to any one of claims 1 to 3, characterized in that the number average diameter Dm of the core (1), determined by transmission electron microscopy (TEM), is in the range of 6 to 50 nm.
5. The number average thickness d of the upper coating layer (2) determined by transmission electron microscopy (TEM) m Particles according to any one of claims 1 to 4, characterized in that the diameter of the particles is in the range of 1 to 15 nm.
6. Particles according to any one of claims 1 to 5, characterized in that the number average diameter of the particles, determined by transmission electron microscopy (TEM), is in the range of 3 to 5000 nm.
7. a. preparing a composition (A) by adding one or more zinc precursors to a flammable solvent or mixture of flammable solvents; thereafter b. forming a flame in a flame spray pyrolysis device by injecting the composition (A) and an oxygen-containing gas until zinc oxide aggregates are obtained; and c) injecting a composition (B) comprising one or more precursors of cerium into the flame until a coating layer comprising cerium and one or more oxygen atoms is obtained on the surface of the zinc oxide aggregates; The method for preparing metal oxide particles according to any one of claims 1 to 6, comprising at least
8. 8. The method of claim 7, wherein the zinc precursor comprises one or more zinc atoms complexed with one or more ligands containing at least one carbon atom.
9. 9. The method according to claim 7 or 8, characterized in that the flammable solvent is selected from protic flammable solvents, aprotic flammable solvents and mixtures thereof.
10. A method according to any one of claims 7 to 9, characterized in that the cerium precursor comprises one or more cerium atoms complexed with one or more ligands.
11. 11. The method according to any one of claims 7 to 10, characterized in that the composition (B) contains one or more solvents, said solvents being selected from polar protic solvents other than water.
12. The method according to any one of claims 7 to 11, further comprising a step (d) of calcination at a temperature in the range of 100°C to 600°C after step (c).
13. A composition comprising one or more metal oxide particles according to any one of claims 1 to 6.
14. 14. The composition according to claim 13, for use in protecting the skin against visible light and / or UV-A and / or UV-B ultraviolet radiation.
Citation Information
Patent Citations
Nanometer doped zinc oxide and its prepn and application in photocatalysis to degrade organic matter and kill bacteria
CN1772375A
Composite particle of zinc oxide-cerium oxide
JP2007161578A
Method for coating core ceramic particle by emulsion flame spray pyrolysis method
JP2010053019A
Method for making silica nanoparticles by flame spray pyrolysis adopting two-fluid nozzle
US20090123357A1
Gas phase production of coated titania
US20090126604A1