Manufacturing method of metal joint and joining method of die-cast members

By applying residual stress to die-cast members and using diffusion bonding, the method overcomes the bonding challenges of die-casting, enhancing the strength of metal joints in complex shapes.

JP7564602B2Active Publication Date: 2024-10-09MOLES ACT
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024528180
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-06-22
Publication Date
2024-10-09
Estimated Expiration
2042-06-22

Smart Images

  • Figure 0007564602000001
    Figure 0007564602000001
  • Figure 0007564602000002
    Figure 0007564602000002
  • Figure 0007564602000003
    Figure 0007564602000003
Patent Text Reader

Abstract

Provided is a method for manufacturing a metal joined body, the method including: a metal member preparation step for preparing a first die-cast member 10 that comprises an aluminum-based material and to which a residual stress is applied while leaving a chill layer of a first surface 12 to be joined, and a second die-cast member 20 that comprises an aluminum-based material and to which a residual stress is applied while leaving a chill layer of a second surface 22 to be joined; and a metal joined body formation step for forming a metal joined body 100 by diffusion-joining the first die-cast member 10 and the second die-cast member 20 by pressing the die-cast members against each other. Through this method for manufacturing a metal joined body, there is provided a method for manufacturing a metal joined body whereby it is possible to increase joining strength by promoting the occurrence of lattice defects (dislocations, vacancies, etc.), which are disruptions in atomic arrangement in the first surface to be joined and the second surface to be joined, by residual stress, and activating establishment of metal bonds or diffusion of atoms between the first surface to be joined and the second surface to be joined.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a metal joined body and a method for joining die-cast members. [Background technology]

[0002] Conventionally, a method for manufacturing a metal joined body by joining steel members has been known that includes a steel member preparation step of preparing two steel members (metal members) and a joined body formation step of butting the surfaces to be joined of the two steel members together, pressing the two steel members under prescribed pressure conditions while heating them to a first temperature at which the two steel members can be joined, thereby joining the two steel members to each other to form a metal joined body (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5198458 Summary of the Invention [Problem to be solved by the invention]

[0004] One of the widely used metal forming methods is die casting, which makes it possible to manufacture metal parts with high dimensional accuracy in a short time (high cycle time) by forcing molten metal into a die.

[0005] Metal components manufactured by die casting (hereinafter referred to as die-cast components) are often used as final products either as is or after undergoing simple processing or treatment, taking advantage of their high dimensional accuracy. However, because die casting is also a type of metal mold casting method, there are limitations to the shapes of components that can be manufactured. For example, with current technology, it is impossible to manufacture components with external shapes that cannot be removed from a metal mold or components with complex internal shapes (e.g., heat exchange medium flow paths) using die casting alone.

[0006] For this reason, it is believed that by applying conventional methods for producing metal bonded bodies by joining multiple metal components to die-cast components, it will be possible to produce components (metal bonded bodies) having a variety of external and internal shapes.

[0007] However, joining die-cast components is not common at present. One of the reasons for this is the properties of the metal materials used in die casting. Metal materials with relatively low melting points are used in die casting, and typical materials are aluminum or aluminum alloys (hereinafter collectively referred to as "aluminum-based materials"). Aluminum-based materials are characterized by being softer than steel materials and having a strong oxide film on their surfaces. Although these characteristics are advantages, they are also disadvantages from the viewpoint of performing joining, making it difficult to increase the joining strength.

[0008] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a method for manufacturing a metal joined body and a method for joining die-cast members made of an aluminum-based material, which are capable of increasing the joining strength. [Means for solving the problem]

[0009] The method for producing a metal joined body of the present invention is characterized by comprising: a metal member preparation step of preparing a first die-cast member made of an aluminum-based material and having a first planned joining surface, the first planned joining surface being imparted with residual stress while leaving a chill layer on the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, the second planned joining surface being imparted with residual stress while leaving a chill layer on the second planned joining surface; and a metal joined body formation step of diffusion-bonding the first die-cast member and the second die-cast member to form a metal joined body by pressing the first die-cast member and the second die-cast member relative to each other while the first planned joining surface and the second planned joining surface are in contact with each other so that pressure is applied to the first planned joining surface and the second planned joining surface.

[0010] The method for joining die-cast members of the present invention is characterized in that a first die-cast member made of an aluminum-based material and having a first planned joining surface, the first planned joining surface being imparted with residual stress while leaving a chill layer on the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, the second planned joining surface being imparted with residual stress while leaving a chill layer on the second planned joining surface, are brought into contact with each other, and the first die-cast member and the second die-cast member are pressed relative to each other so that pressure is applied to the first planned joining surface and the second planned joining surface, thereby diffusion-bonding the first die-cast member and the second die-cast member to form a metal joint body. Effect of the Invention

[0011] The method for producing a metal bonded body of the present invention involves preparing a first die-cast member made of an aluminum-based material and having a first planned joining surface, in which a chill layer is left on the first planned joining surface while residual stress is imparted to the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, in which a chill layer is left on the second planned joining surface while residual stress is imparted to the second planned joining surface, and diffusion bonding these members to form a metal bonded body.As will be described later, this method for producing a metal bonded body is capable of increasing the joining strength by promoting the generation of lattice defects (dislocations, vacancies, etc.), which are disturbances in the atomic arrangement, in the first planned joining surface and the second planned joining surface, and activating the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface and the second planned joining surface.

[0012] The method for joining die-cast members of the present invention involves diffusion bonding a first die-cast member made of an aluminum-based material and having a first planned joining surface, in which a chill layer is left on the first planned joining surface while residual stress is imparted to the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, in which a chill layer is left on the second planned joining surface while residual stress is imparted to the second planned joining surface, so that, as will be described later, the residual stress promotes the generation of lattice defects, which are disturbances in the atomic arrangement, in the first planned joining surface and the second planned joining surface, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface and the second planned joining surface, thereby resulting in a method for joining die-cast members that can increase the joining strength. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a diagram for explaining a first die-cast member 10 and a second die-cast member 20 in the first embodiment. [Diagram 2] 1A and 1B are diagrams for explaining the application of residual stress and lattice defects. [Diagram 3] 1 is a view for explaining a metal bonded body formation step S20 in the first embodiment. FIG. [Figure 4] 10 is a diagram for explaining a first die-cast member 30 and a second die-cast member 40 in the second embodiment. FIG. [Diagram 5] 11 is a view for explaining a metal bonded body formation step S21 in the second embodiment. FIG. [Figure 6] 11 is a diagram for explaining a first die-cast member 50 and a second die-cast member 60 in the third embodiment. FIG. [Figure 7] 11 is a view for explaining a metal bonded body formation step S22 in the third embodiment. FIG. [Figure 8] 13 is a diagram for explaining a first deformation suppressing member 200 according to a fourth embodiment. FIG. [Figure 9] 13 is a view for explaining a metal bonded body formation step S23 in embodiment 4. FIG. [Figure 10]13 is a diagram for explaining a second die-cast member 60a and a second deformation suppressing member 300 in the fifth embodiment. FIG. [Figure 11] 13 is a view for explaining a metal bonded body formation step S24 in the fifth embodiment. FIG. [Figure 12] 13 is a view for explaining a second die-cast member 60b in the sixth embodiment. FIG. [Figure 13] 13 is a view for explaining a metal bonded body formation step S25 in the sixth embodiment. FIG. [Figure 14] 13 is a diagram for explaining a first die-cast member 80 and a second die-cast member 90 in the seventh embodiment. FIG. [Figure 15] FIG. 13 is a view for explaining a metal bonded body formation step S26 in the seventh embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The manufacturing method of a metal joined body and the joining method of die-cast members of the present invention will be described below based on the embodiments shown in the drawings. Each drawing is a schematic diagram and does not necessarily strictly reflect the actual structure, configuration, ratio, etc. Each embodiment described below does not limit the invention according to the claims. Furthermore, not all of the elements and combinations thereof described in each embodiment are essential to the present invention. In the following description, the same reference numerals are used across the embodiments for components that can be considered to be substantially equivalent, and repeated description will be omitted.

[0015] [Embodiment 1] Fig. 1 is a diagram for explaining a first die-casting member 10 and a second die-casting member 20 in the first embodiment. Fig. 1(a) is a perspective view (isometric view) of the first die-casting member 10, Fig. 1(b) is a plan view of the first die-casting member 10, Fig. 1(c) is a cross-sectional view taken along line A1-A1 of Fig. 1(b), Fig. 1(d) is an enlarged cross-sectional view showing the state of the surface of the first intended joining surface 12, Fig. 1(e) is a perspective view of the second die-casting member 20, Fig. 1(f) is a plan view of the second die-casting member 20, Fig. 1(g) is a cross-sectional view taken along line A2-A2 of Fig. 1(f), and Fig. 1(h) is an enlarged cross-sectional view showing the state of the surface of the second intended joining surface 22 of Fig. 1(f). FIG. 2 is a diagram for explaining the application of residual stress and lattice defects. FIG. 2(a) is a diagram showing the arrangement of atoms before applying residual stress to the first die-casting member 10 and the first planned joining surface 12, FIG. 2(b) is a diagram showing the arrangement of atoms after applying residual stress to the first planned joining surface 12, FIG. 2(c) is a diagram showing the arrangement of dislocations, which are lattice defects, and FIG. 2(d) is a diagram showing the arrangement of vacancies, which are lattice defects. FIG. 2(a) and FIG. 2(b) are oblique projection diagrams, and the round objects arranged in a cube shape are atoms. FIG. 2(c) is an oblique projection diagram, and FIG. 2(d) is a plan diagram. The white circles in FIG. 2(c) and FIG. 2(d) are atoms. FIG. 2 is merely a schematic diagram, and does not show a specific crystal structure, etc., in the first planned joining surface 12. In particular, while in FIG. 2 the atoms are shown as having a simple cubic lattice structure, this is for the convenience of making the illustration easier to understand and does not indicate that the atoms in the first die-cast member 10 actually have such a structure. Fig. 3 is a diagram for explaining the metal bonded body forming step S20 in the first embodiment. Fig. 3(a) is a cross-sectional view showing a state in which the first die-casting member 10 and the second die-casting member 20 are pressed relative to each other, Fig. 3(b) is an enlarged cross-sectional view showing the state of the first planned joining surface 12 and the second planned joining surface 22 during pressing, Fig. 3(c) is a cross-sectional view showing the metal bonded member 100 formed by diffusion bonding, and Fig. 3(d) is an enlarged cross-sectional view showing the state of the bonding interface after bonding. The reference character P and the thick arrow in Fig. 3(a) indicate that the first die-casting member 10 and the second die-casting member 20 are pressed relative to each other. The reference character P and the thick arrow have the same meanings in the "diagrams shown for explaining the metal bonded body forming step" described later. 3(c) and 3(d) show a bonded interface, but this does not mean that a bonded interface remains in the metal bonded body 100, but is intended to clearly show that the metal bonded body 100 is manufactured from two members. This also applies to the "drawings shown to explain the metal bonded body forming step" described later.

[0016] The manufacturing method of the metal bonded body according to the embodiment 1 includes a metal member preparation step S10 and a metal bonded body formation step S20. The joining method of the die-cast members according to the embodiment 1 corresponds to the metal bonded body formation step S20. Each step will be described below.

[0017] 1. Metal component preparation process S10 The metal member preparation step S10 is a step of preparing a first die-cast member 10 made of an aluminum-based material and having a first planned joining surface 12, and a second die-cast member 20 made of an aluminum-based material and having a second planned joining surface 22 (see FIG. 1). The first die-cast member 10 is a member in which a residual stress is imparted to the first planned joining surface 12 while leaving a chill layer on the first planned joining surface 12. The second die-cast member 20 is a member in which a residual stress is imparted to the second planned joining surface 22 while leaving a chill layer on the second planned joining surface 22. The first die-cast member 10 and the second die-cast member 20 may be made of the same material or different materials as long as they are made of an aluminum-based material.

[0018] Note that "a first die-cast member having a first intended joining surface and a residual stress imparted thereto while leaving a chill layer on the first intended joining surface" can also be rephrased as "a first die-cast member having a chill layer on the first intended joining surface and a residual stress imparted thereto (first die-cast member)." Similarly, "a second die-cast member having a second intended joining surface and a chill layer on the second intended joining surface and a residual stress imparted thereto (second die-cast member)" can also be rephrased as "a second die-cast member having a chill layer on the second intended joining surface and a residual stress imparted thereto (second die-cast member)."

[0019] In this specification, the term "die-cast member" refers to a metal member manufactured by die casting. In this specification, the term "die-cast member" includes a member that has been subjected to post-processing (e.g., deburring or drilling) to the extent that the overall shape is not significantly changed.

[0020] In this specification, the term "chill layer" refers to a characteristic structure of a die-cast member, which is a relatively high-strength structure formed near the surface of the die-cast member. Die-cast members are manufactured by injecting molten metal into a die at high pressure, and the surface of the die-cast member is cooled more rapidly than the internal portion of the die-cast member due to contact with the die, etc. For this reason, a chill layer, which is a high-density structure (with fewer voids) compared to the internal portion, is formed on the surface of the die-cast member. The chill layer does not have a clear boundary, but it is considered appropriate to treat the area of ​​about 0.3 mm from the surface as the chill layer.

[0021] In this specification, "residual stress" refers to stress that exists (remains) within an object. Although stress remains within a component even when it is merely manufactured by die casting, in order to make it "a component with residual stress imparted to the intended joining surface" in this specification, it is necessary to carry out a process to impart residual stress after manufacturing by die casting. In other words, in this specification, "residual stress" refers to residual stress imparted after manufacturing by die casting.

[0022] The first die-casting member 10 is a member in which the surface of the first planned joining surface 12 is plastically deformed by shot blasting to impart residual stress to the first planned joining surface 12. The second die-casting member 20 is a member in which the surface of the second planned joining surface 22 is plastically deformed by shot blasting to impart residual stress to the second planned joining surface 22. The shot blasting process refers to a process in which a projectile (granular material) is collided with a target surface. The conditions of the projectile material, particle size, and projectile colliding speed can be determined arbitrarily according to the type of aluminum-based material constituting the first die-casting member 10 and the second die-casting member 20. However, when setting the conditions, it is necessary to take care not to scrape the surfaces of the first planned joining surface and the second planned joining surface to remove the chill layer. As for the material of the projectile, for example, an aluminum-based material or a steel material can be suitably used. When the shot blasting process is performed, the impact of the blasting material forms fine irregularities on the surfaces of the first intended joining surface 12 and the second intended joining surface 22 (see Fig. 1(d) and Fig. 1(h)). Note that Fig. 1(d) and Fig. 1(h) are schematic views, and therefore the size, ratio, shape, etc. of the irregularities on the surfaces are not limited to those shown in the drawings.

[0023] In addition, the first die-casting member 10 and the second die-casting member 20 may also have surfaces other than the first intended joining surface 12 and the second intended joining surface 22 subjected to shot blasting treatment.

[0024] Here, the application of residual stress will be described by taking the first die-cast member 10 as an example. By applying residual stress to the first planned joining surface 12, the atomic level structure (particularly the metal crystal structure) in the first planned joining surface 12 is affected (see Figs. 2(a) and 2(b)), and the generation of lattice defects, which are disturbances in the atomic arrangement, can be promoted. In particular, by applying residual stress to the first planned joining surface 12 by plastically deforming the surface of the first planned joining surface 12, it becomes possible to generate a large number of dislocations d1 (Fig. 2(c)), which are linear lattice defects in which the atomic arrangement is shifted in rows. In addition, the application of residual stress may also generate vacancies d2 (see Fig. 2(d)), which are point-like lattice defects, and planar lattice defects. The above matters are also the same for the second die-cast member 20.

[0025] In the metal member preparation step S10, the first die-cast member 10 and the second die-cast member 20 are prepared such that the first planned joining surface 12 and the second planned joining surface 22 have a predetermined surface roughness, respectively. In the first embodiment, the first planned joining surface 12 and the second planned joining surface 22 having the predetermined surface roughness can be directly used after being subjected to shot blasting.

[0026] In this specification, the term "predetermined surface roughness" refers to a roughness that is likely to cause changes in the surface microstructure, such as deformation, destruction, or slippage, of the unevenness on the surfaces of the first and second intended joining surfaces when the second die-casting member is pressed relative to the first die-casting member in the metal joined body forming process described below. The appropriate value of the predetermined surface roughness varies depending on the type of material, the required joining strength, etc., but it is generally considered preferable to set the surface roughness to Ra = 0.05 μm or more. In this specification, the term "surface microstructure" refers to an atomic-scale surface structure.

[0027] Various materials can be used as the aluminum-based material constituting the first die-cast member 10 and the second die-cast member 20. A specific example is an ADC-based material (particularly ADC12), which is an alloy for casting. It has been found that the method of the present invention can provide a metal joint having high joint strength for die-cast members made of ADC12.

[0028] 2. Metal bonded body forming process S20 The metal bonded body formation process S20 is a process in which the first die-casting member 10 and the second die-casting member 20 are pressed relative to each other so that pressure is applied to the first intended joining surface 12 and the second intended joining surface 22 while the first intended joining surface 12 and the second intended joining surface 22 are in contact with each other (see Figure 3(a)), thereby diffusion bonding the first die-casting member 10 and the second die-casting member 20 to form a metal bonded body 100 (see Figures 3(c) and 3(d)).

[0029] In the metal bonded body formation process S20, the first die-casting member 10 and the second die-casting member 20 are pressed relative to each other to cause changes in the surface microstructure of the first planned joining surface 12 and the second planned joining surface 22, thereby diffusion bonding the first die-casting member 10 and the second die-casting member 20 to form the metal bonded body 100. The changes in the surface microstructure include uneven deformation, destruction, slippage, etc. (see FIG. 3(b)), and the combination of these changes with the residual stress imparted to the first planned joining surface 12 and the second planned joining surface 22 promotes diffusion bonding.

[0030] The principle by which diffusion bonding is promoted between the first and second planned bonding surfaces to which residual stress has been applied is believed to be as follows. By applying residual stress to the first and second planned bonding surfaces, it is possible to promote the generation of lattice defects in each of the planned bonding surfaces, as described above. As the number of lattice defects increases, the first and second planned bonding surfaces become in a state in which atoms can easily move. As a result, it is possible to activate the diffusion of atoms and the establishment of metallic bonds between the first and second planned bonding surfaces (the bonding interface).

[0031] In this specification, "pressing the first die-cast member and the second die-cast member relative to each other" does not only mean pressing the first die-cast member by fixing the first die-cast member and applying a moving force to the second die-cast member, but also includes pressing the first die-cast member by fixing the second die-cast member and applying a moving force to the second die-cast member, and pressing the first die-cast member and the second die-cast member by applying a moving force to both the first die-cast member and the second die-cast member.

[0032] The metal bonded body forming step S20 is preferably performed by heating the first die-cast member 10 and the second die-cast member 20 to promote diffusion bonding, and maintaining the first die-cast member 10 and the second die-cast member 20 at a certain temperature (however, a temperature below the melting point). That is, in the metal bonded body forming step S20, it is preferable to press the first die-cast member 10 and the second die-cast member 20 relative to each other under temperature conditions that allow diffusion bonding of the first die-cast member 10 and the second die-cast member 20 (preferably under temperature conditions suitable for diffusion bonding).

[0033] The temperature conditions suitable for diffusion bonding vary mainly depending on the type of aluminum-based material constituting the first die-cast member 10 and the second die-cast member 20. For example, when the aluminum-based material is ADC12, the temperature can be about 500 to 550° C. In addition, the optimum pressure to be applied varies greatly depending on the type of aluminum-based material constituting the first die-cast member 10 and the second die-cast member 20, the shapes of the first die-cast member 10 and the second die-cast member 20, the bonding temperature, etc., so it is difficult to give an appropriate value, but it is considered that a pressure of approximately MPa order is required.

[0034] In order to diffusion bond the first die-casting member 10 and the second die-casting member 20 and obtain a high bonding strength, it is necessary to maintain the temperature and pressure to a certain extent. The time varies depending on the type of aluminum-based material constituting the first die-casting member 10 and the second die-casting member 20, the shapes of the first die-casting member 10 and the second die-casting member 20, the bonding temperature, the pressure, etc., but can be, for example, about 10 minutes to 3 hours.

[0035] The metal bonded body forming step S20 is preferably carried out in a vacuum or in an inert gas, although it is considered that the metal bonded body forming step S20 can also be carried out in the presence of air.

[0036] 3. Effects of the manufacturing method of the metal joined body and the joining method of the die-cast members according to the first embodiment The manufacturing method of the metal bonded body of embodiment 1 includes preparing a first die-cast member 10 made of an aluminum-based material and having a first planned joining surface 12, in which a residual stress is imparted to the first planned joining surface 12 while leaving a chill layer on the first planned joining surface 12, and a second die-cast member 20 made of an aluminum-based material and having a second planned joining surface 22, in which a residual stress is imparted to the second planned joining surface 22 while leaving a chill layer on the second planned joining surface 22, and then diffusion bonding these to form the metal bonded body 100.This method for manufacturing a metal bonded body enables the bonding strength to be increased by promoting the generation of lattice defects in the first planned joining surface 12 and the second planned joining surface 22 due to the residual stress, and activating the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 12 and the second planned joining surface 22.

[0037] Furthermore, according to the manufacturing method of the metal joined body of embodiment 1, the first die-casting member 10 imparts residual stress to the first planned joining surface 12 by plastically deforming the surface of the first planned joining surface 12, and the second die-casting member 20 imparts residual stress to the second planned joining surface 22 by plastically deforming the surface of the second planned joining surface 22. Therefore, the increase in residual stress due to plastic deformation promotes the generation of lattice defects, which are disturbances in the atomic arrangement, in the first planned joining surface 12 and the second planned joining surface 22, and makes it possible to activate the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 12 and the second planned joining surface 22.

[0038] Furthermore, according to the manufacturing method of the metal joined body of embodiment 1, the first die-casting member 10 has a residual stress imparted to the first planned joining surface 12 by plastically deforming the surface of the first planned joining surface 12 through shot blasting treatment, and the second die-casting member 20 has a residual stress imparted to the second planned joining surface 22 by plastically deforming the surface of the second planned joining surface 22 through shot blasting treatment. Therefore, by successively colliding the first planned joining surface 12 and the second planned joining surface 22 with a shot material, it is possible to plastically deform the entire surfaces of the first planned joining surface 12 and the second planned joining surface 22 approximately evenly and substantially without directionality, thereby imparting residual stress.

[0039] In addition, according to the manufacturing method of the metal joined body of embodiment 1, in the metal member preparation step S10, a first die-casting member 10 and a second die-casting member 20 are prepared, the first planned joining surface 12 and the second planned joining surface 22 having a predetermined surface roughness, and in the metal joined body formation step S20, the first die-casting member 10 and the second die-casting member 20 are pressed relative to each other to form the metal joined body 100 by diffusion bonding the first die-casting member 10 and the second die-casting member 20 while causing changes in the surface microstructure of the first planned joining surface 12 and the second planned joining surface 22.Therefore, by taking advantage of the unevenness on the surfaces of the first planned joining surface 12 and the second planned joining surface 22 to cause changes in the surface microstructure, it is possible to further increase the joining strength.

[0040] Furthermore, according to the manufacturing method of the metal bonded body of embodiment 1, in the metal bonded body formation process S20, when the first die-cast member 10 and the second die-cast member 20 are pressed relative to each other under temperature conditions that allow diffusion bonding of the first die-cast member 10 and the second die-cast member 20 (preferably under temperature conditions suitable for diffusion bonding), the first die-cast member 10 and the second die-cast member 20 are placed in a state that is conducive to diffusion bonding when pressed, that is, thermal expansion increases lattice defects such as vacancies on the surfaces of the first intended joining surface 12 and the second intended joining surface 22, making it easier for atoms to diffuse, thereby making it possible to further increase the bonding strength.

[0041] The method for joining die-cast members in embodiment 1 involves diffusion bonding a first die-cast member 10 made of an aluminum-based material and having a first planned joining surface 12, in which a chill layer is left on the first planned joining surface 12 while residual stress is imparted to the first planned joining surface 12, and a second die-cast member 20 made of an aluminum-based material and having a second planned joining surface 22, in which a chill layer is left on the second planned joining surface 22 while residual stress is imparted to the second planned joining surface 22. Therefore, the residual stress promotes the generation of lattice defects in the first planned joining surface 12 and the second planned joining surface 22, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 12 and the second planned joining surface 22, thereby resulting in a method for joining die-cast members that can increase the joining strength.

[0042] [Embodiment 2] FIG. 4 is a diagram for explaining the first die-casting member 30 and the second die-casting member 40 in the second embodiment. FIG. 4(a) is a perspective view of the first die-casting member 30, FIG. 4(b) is a plan view of the first die-casting member 30, FIG. 4(c) is a cross-sectional view taken along the line A3-A3 of FIG. 4(b), FIG. 4(d) is a perspective view of the second die-casting member 40, FIG. 4(e) is a plan view of the second die-casting member 40, and FIG. 4(f) is a cross-sectional view taken along the line A4-A4 of FIG. 4(e). In FIG. 4(a), the portion of the shape of the joining recess 32 that is not directly visible is indicated by a broken line. The same applies to the case where a member having a joining recess or space is illustrated in each of the perspective views described later. Fig. 5 is a diagram for explaining the metal bonded body formation step S21 in embodiment 2. Fig. 5(a) is a cross-sectional view showing a state in which the first die-casting member 30 and the second die-casting member 40 are pressed relative to each other, and Fig. 5(b) is a cross-sectional view showing the metal bonded body 110 formed by diffusion bonding.

[0043] The manufacturing method of the metal bonded body according to the embodiment 2 includes a metal member preparation step S11 and a metal bonded body formation step S21. The joining method of the die-cast members according to the embodiment 2 corresponds to the metal bonded body formation step S21. Each step will be described below.

[0044] 1. Metal component preparation process S11 The metal member preparation step S11 is similar to the metal member preparation step S10 in the first embodiment in that it is a step of preparing a first die-cast member made of an aluminum-based material and having a first planned joining surface, in which a chill layer is left on the first planned joining surface and residual stress is applied to the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, in which a chill layer is left on the second planned joining surface and residual stress is applied to the second planned joining surface, but differs from the metal member preparation step S10 in the first embodiment in the following points. That is, in the metal member preparation step S11, a first die-cast member 30 is prepared, in which a joining recess 32 is formed in which at least a part of the inner surface is a first inclined surface angled with respect to the pressing direction in the metal bonded body formation step S21 (see Figs. 4(a) to 4(c)). The joining recess 32 does not have a bottom and is like a through hole. Furthermore, in the metal member preparation process S11, a second die-cast member 40 is prepared, which has a joining protrusion 42 having at least a portion of its side surface which is a second inclined surface angled to correspond to the first inclined surface, and which has a shape in which the first inclined surface and the second inclined surface butt against each other when inserted into the joining recess 32 (see Figures 4(d) to 4(f)).

[0045] It can also be said that the first inclined surface and the second inclined surface in the second embodiment are tapered surfaces. The taper angles of the first inclined surface and the second inclined surface can be any angle depending on the type of aluminum-based material constituting the first die-cast member 30 and the second die-cast member 40, the shape of the metal bonded body 110 to be manufactured (or a product manufactured by processing the metal bonded body 110), and the like.

[0046] At least a part of the first inclined surface is the first planned joining surface 34. At least a part of the second inclined surface is the second planned joining surface 44. In the manufacturing method of the metal bonded body according to the second embodiment, the first and second inclined surfaces are the first and second planned joining surfaces 34 and 44, respectively, which are butted when the joining convex portion 42 is inserted into the joining concave portion 32 and which are brought into contact by pressing in the metal bonded body forming step S21. Note that the first die-casting member 30 is a member in which a residual stress is imparted to the first planned joining surface 34 while leaving a chill layer on the first planned joining surface 34, and the second die-casting member 40 is a member in which a residual stress is imparted to the second planned joining surface 44 while leaving a chill layer on the second planned joining surface 44, as in the first embodiment.

[0047] The reason will be explained later, but the first intended joining surface 34 of the first die-casting member 30 and the second intended joining surface 44 of the second die-casting member 40 do not have to have a specified surface roughness like the first intended joining surface 12 and the second intended joining surface 22 in embodiment 1.

[0048] 2. Metal bonded body forming process S21 The metal bonded body formation process S21 is a process in which the first die-casting member 30 and the second die-casting member 40 are pressed relative to each other with the bonding protrusion 42 inserted into the bonding recess 32 (see Figure 5(a)), thereby diffusion bonding the first die-casting member 30 and the second die-casting member 40 while causing changes in the surface microstructure of the first intended bonding surface 34 and the second intended bonding surface 44 to form a metal bonded body 110 (see Figure 5(b)).

[0049] When the first die-casting member 30 and the second die-casting member 40 are pressed relative to each other with the joining protrusion 42 inserted into the joining recess 32, the first planned joining surface 34 and the second planned joining surface 44 are subjected to not only pressure in the opposing directions but also force due to misalignment. Therefore, more complex forces are applied to the first planned joining surface 34 and the second planned joining surface 44 than in the case of embodiment 1, accelerating changes in the surface microstructure. Therefore, in the metal joined body formation step S21, even if the first planned joining surface 34 and the second planned joining surface 44 do not have a predetermined surface roughness, changes in the surface microstructure are likely to occur.

[0050] In addition, in the metal bonded body formation process S21, as in the metal bonded body formation process S20 in embodiment 1, it is preferable to press the first die-cast member 30 and the second die-cast member 40 relative to each other under temperature conditions at which the first die-cast member 30 and the second die-cast member 40 can be diffusion bonded (preferably under temperature conditions suitable for diffusion bonding).

[0051] 3. Effects of the manufacturing method of the metal joined body and the joining method of the die-cast members according to the second embodiment The manufacturing method of the metal bonded body according to the second embodiment includes preparing a first die-cast member 30 made of an aluminum-based material and having a first planned joining surface 34, in which a residual stress is applied to the first planned joining surface 34 while leaving a chill layer on the first planned joining surface 34, and a second die-cast member 40 made of an aluminum-based material and having a second planned joining surface 44, in which a residual stress is applied to the second planned joining surface 44 while leaving a chill layer on the second planned joining surface 44, and then diffusion-bonding these members to form the metal bonded body 110. Therefore, as with the manufacturing method of the metal bonded body according to the first embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surface 34 and the second planned joining surface 44, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 34 and the second planned joining surface 44, thereby achieving a manufacturing method of a metal bonded body that can increase the bonding strength.

[0052] According to the method for manufacturing a metal bonded body according to the second embodiment, in the metal member preparation step S11, a first die-cast member 30 is prepared, which has a joining recess 32 formed on at least a part of its inner surface which is a first inclined surface angled with respect to the pressing direction in the metal bonded body formation step S21, and a second die-cast member 40 is prepared, which has a joining protrusion 42 formed on at least a part of its side surface which is a second inclined surface angled with respect to the first inclined surface and which has a shape in which the first inclined surface and the second inclined surface butt against each other when the second die-cast member 40 is inserted into the joining recess 32, and at least a part of the first inclined surface is a first intended joining surface 34, and At least a part of the inclined surface is the second intended joining surface 44, and in the metal joined body formation process S21, the first die-casting member 30 and the second die-casting member 40 are pressed relative to each other with the joining protrusion 42 inserted into the joining recess 32, thereby forming the metal joined body 110 by diffusion bonding the first die-casting member 30 and the second die-casting member 40 while causing changes in the surface microstructure of the first intended joining surface 34 and the second intended joining surface 44.Therefore, by utilizing the pressure and shift between the first intended joining surface 34 and the second intended joining surface 44 that occurs during pressing to cause a change in the surface microstructure, it is possible to further increase the joining strength.

[0053] The method for producing a metal bonded body according to the second embodiment also has the same effects as those of the method for producing a metal bonded body according to the first embodiment.

[0054] The method for joining die-cast members according to the second embodiment involves diffusion bonding a first die-cast member 30 made of an aluminum-based material and having a first planned joining surface 34, in which a chill layer is left on the first planned joining surface 34 while residual stress is imparted to the first planned joining surface 34, and a second die-cast member 40 made of an aluminum-based material and having a second planned joining surface 44, in which a chill layer is left on the second planned joining surface 44 while residual stress is imparted to the second planned joining surface 44. Therefore, similar to the method for joining die-cast members according to the first embodiment, this method for joining die-cast members is capable of increasing the joining strength by promoting the generation of lattice defects in the first planned joining surface 34 and the second planned joining surface 44 due to the residual stress, and activating the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 34 and the second planned joining surface 44.

[0055] [Embodiment 3] Figure 6 is a diagram for explaining the first die-casting member 50 and the second die-casting member 60 in embodiment 3. Figure 6(a) is a perspective view of the first die-casting member 50, Figure 6(b) is a plan view of the first die-casting member 50, Figure 6(c) is a cross-sectional view taken along line A5-A5 of Figure 6(b), Figure 6(d) is a perspective view of the second die-casting member 60, Figure 6(e) is a plan view of the second die-casting member 60, and Figure 6(f) is a cross-sectional view taken along line A6-A6 of Figure 6(e). Fig. 7 is a diagram for explaining the metal bonded body formation step S22 in embodiment 3. Fig. 7(a) is a cross-sectional view showing a state in which the first die-casting member 50 and the second die-casting member 60 are pressed relative to each other, Fig. 7(b) is a cross-sectional view showing a state in which the first intended joining surface 58 and the second intended joining surface 68 are in contact with each other due to pressing, and Fig. 7(c) is a cross-sectional view showing the metal bonded body 120 formed by diffusion bonding.

[0056] The manufacturing method of the metal bonded body according to the embodiment 3 includes a metal member preparation step S12 and a metal bonded body formation step S22. The joining method of the die-cast members according to the embodiment 3 corresponds to the metal bonded body formation step S22. Each step will be described below.

[0057] 1. Metal component preparation process S12 The metal member preparation step S12 is similar to the metal member preparation step S10 in the first embodiment and the metal member preparation step S11 in the second embodiment in that it is a step of preparing a first die-cast member made of an aluminum-based material and having a first planned joining surface, the first planned joining surface being given residual stress while leaving a chill layer on the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, the second planned joining surface being given residual stress while leaving a chill layer on the second planned joining surface, but differs from them in the following respects. That is, in the metal member preparation step S12, a first die-cast member 50 is prepared, the first die-cast member 50 having a joining recess 52 formed such that at least a part of the inner surface is a first inclined surface angled with respect to the pressing direction in the metal bonded body formation step S22, and the joining recess 52 has a bottom (see Figs. 6(a) to 6(c)). In the first die-cast member 50 , at least a part of the first inclined surface is the first intended joining surface 54 , and the bottom surface of the joining recess 52 is also the first intended joining surface 58 .

[0058] In the metal member preparation step S12, a second die-cast member 60 is prepared, which has a joining protrusion 62 having a shape in which at least a portion of the side surface is a second inclined surface with an angle corresponding to the first inclined surface, and the first inclined surface and the second inclined surface butt against each other when inserted into the joining recess 52. In the second die-cast member 60, at least a portion of the second inclined surface is a second intended joining surface 64, and the tip surface of the joining protrusion 62 is also a second intended joining surface 68 (see Figures 6(d) to 6(f)).

[0059] The first intended joining surface 54 of the first die-cast member 50 and the second intended joining surface 64 of the second die-cast member 60 do not have to have a specified surface roughness, as in the metal member preparation process S11 in embodiment 2, but the first intended joining surface 58 and the second intended joining surface 68 have a specified surface roughness, as in the first intended joining surface 12 and the second intended joining surface 22 in embodiment 1.

[0060] As in the cases of embodiments 1 and 2, the first die-cast member 50 has residual stress imparted to the first intended joining surfaces 54, 58 while leaving chill layers on the first intended joining surfaces 54, 58, and the second die-cast member 60 has residual stress imparted to the second intended joining surfaces 64, 68 while leaving chill layers on the second intended joining surfaces 64, 68.

[0061] Although not shown, the joining recess 52 of the first die-casting member 50 and the second inclined surface of the second die-casting member 60 may have holes or grooves for venting air, if necessary.

[0062] 2. Metal bonded body forming process S22 The metal bonded body forming step S22 is similar to the metal bonded body forming step S21 in the second embodiment in that it is a step of forming a metal bonded body by diffusion bonding the first die-cast member and the second die-cast member while causing a change in the surface microstructure of the first and second planned bonding surfaces, but differs from the metal bonded body forming step S21 in the second embodiment in the following points. That is, in the metal bonded body forming step S22, the first die-cast member 50 and the second die-cast member 60 are pressed relative to each other in a state in which the bonding protrusion 62 is inserted into the bonding recess 52 (see FIG. 7(a)). As a result, the first planned bonding surface 58 and the second planned bonding surface 68 come into contact with each other (see FIG. 7(b)). Therefore, not only the first planned bonding surface 54 and the second planned bonding surface 64, but also the first planned bonding surface 58 and the second planned bonding surface 68 are diffusion bonded to form a metal bonded body 120 (see FIG. 7(c)). The principle by which the first intended joining surface 58 and the second intended joining surface 68 are diffusion-bonded is the same as in the first embodiment.

[0063] 3. Effects of the manufacturing method of the metal joined body and the joining method of the die-cast members according to the third embodiment The manufacturing method of the metal bonded body according to the third embodiment includes preparing a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress is applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60 made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress is applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68, and then diffusion-bonding these members to form the metal bonded body 120. Therefore, as in the manufacturing methods of the metal bonded bodies according to the first and second embodiments, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby providing a manufacturing method of a metal bonded body capable of increasing the bonding strength.

[0064] In addition, according to the manufacturing method of the metal joined body of embodiment 3, in the metal member preparation step S12, a first die-cast member 50 and a second die-cast member 60 are prepared, in which the first planned joining surface 58 and the second planned joining surface 68 have a predetermined surface roughness, and in the metal joined body formation step S22, the first die-cast member 50 and the second die-cast member 60 are pressed relative to each other to form the metal joined body 120 by diffusion bonding the first die-cast member 50 and the second die-cast member 60 while causing a change in the surface microstructure of the first planned joining surface 58 and the second planned joining surface 68. Therefore, by taking advantage of the unevenness on the surfaces of the first planned joining surface 58 and the second planned joining surface 68 to cause a change in the surface microstructure, it is possible to further increase the joining strength.

[0065] According to the manufacturing method of the metal bonded body of the third embodiment, in the metal member preparation step S12, a first die-cast member 50 is prepared, which has a joining recess 52 formed in which at least a part of the inner surface is a first inclined surface angled with respect to the pressing direction in the metal bonded body formation step S22, and a second die-cast member 60 is prepared, which has a joining protrusion 62 formed in such a shape that the first inclined surface and the second inclined surface butt against each other when the second die-cast member 60 is inserted into the joining recess 52, and at least a part of the first inclined surface is a first intended joining surface 54, and At least a part of the inclined surface is the second intended joining surface 64, and in the metal joined body formation process S22, the first die-casting member 50 and the second die-casting member 60 are pressed relative to each other with the joining protrusion 62 inserted into the joining recess 52, thereby forming the metal joined body 120 by diffusion bonding the first die-casting member 50 and the second die-casting member 60 while causing changes in the surface microstructure of the first intended joining surface 54 and the second intended joining surface 64.Therefore, by utilizing the pressure and shift between the first intended joining surface 54 and the second intended joining surface 64 that occurs during pressing to cause a change in the surface microstructure, it is possible to further increase the joining strength.

[0066] The method for producing a metal bonded body according to the third embodiment also has the corresponding effects among the effects possessed by the methods for producing a metal bonded body according to the first and second embodiments.

[0067] The method for joining die-cast members according to the third embodiment involves diffusion bonding a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a chill layer is left on the first planned joining surfaces 54, 58 while a residual stress is applied to the first planned joining surfaces 54, 58, and a second die-cast member 60 made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a chill layer is left on the second planned joining surfaces 64, 68 while a residual stress is applied to the second planned joining surfaces 64, 68. As a result, similar to the methods for joining die-cast members according to the first and second embodiments, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby making it possible to increase the joining strength.

[0068] [Embodiment 4] Fig. 8 is a diagram for explaining the first deformation suppressing member 200 in embodiment 4. Fig. 8(a) is a perspective view of the first deformation suppressing member 200, Fig. 8(b) is a plan view of the first deformation suppressing member 200, and Fig. 8(c) is a cross-sectional view taken along A7-A7 in Fig. 8(b). Fig. 9 is a diagram for explaining the metal bonded body formation step S23 in embodiment 4. Fig. 9(a) is a cross-sectional view showing a state in which the first die-casting member 50 and the second die-casting member 60 are pressed relative to each other, Fig. 9(b) is a cross-sectional view showing a state in which the first intended joining surface 58 and the second intended joining surface 68 are in contact with each other due to pressing, and Fig. 9(c) is a cross-sectional view showing the metal bonded body 120 formed by diffusion bonding.

[0069] The manufacturing method of the metal bonded body according to the fourth embodiment is basically the same as the manufacturing method of the metal bonded body according to the third embodiment, but differs from the manufacturing method of the metal bonded body according to the third embodiment in that a first deformation suppressing member is used in the metal bonded body forming step. The manufacturing method of the metal bonded body according to the fourth embodiment includes a metal member preparing step S12 and a metal bonded body forming step S23. The joining method of the die-cast members according to the fourth embodiment corresponds to the metal bonded body forming step S23. Since the metal member preparing step S12 in the fourth embodiment is the same as the metal member preparing step S12 in the third embodiment, the metal bonded body forming step S23 will be described below.

[0070] The first deformation suppressing member 200 in the fourth embodiment is a member that suppresses deformation of the first die-casting member 50 at least in a direction (outward) perpendicular to the pressing direction. The first deformation suppressing member 200 can also be expressed as a member that can cover at least the side surface of the first die-casting member 50. The first deformation suppressing member 200 in the fourth embodiment is a member that can also cover the bottom surface of the first die-casting member 50. In the first deformation suppressing member 200, a space corresponding to the outer shape of the side surface and the bottom surface of the first die-casting member 50 is formed (see FIG. 8). The first deformation suppressing member 200 is made of a material that is less likely to deform than the material that constitutes the first die-casting member 50. Examples of such materials include steel, cemented carbide, and ceramics. Although the first deformation suppressing member 200 is illustrated as being a member made of one component as a whole, it may be a member made of multiple components (a member that can be separated and combined).

[0071] In the metal bonded body formation process S23 in the fourth embodiment, the first deformation suppressing member 200 and the first die-casting member 50 are combined (the first die-casting member 50 is fitted into the space in the first deformation suppressing member 200) and the first die-casting member 50 and the second die-casting member 60 are pressed relative to each other (see Figs. 9(a) and 9(b)). The first deformation suppressing member 200 is removed after the metal bonded body 120 is formed by diffusion bonding (see Fig. 9(c)).

[0072] The manufacturing method of the metal bonded body according to the fourth embodiment includes preparing a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress is applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60 made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress is applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68, and then diffusion-bonding these members to form the metal bonded body 120. Therefore, as with the manufacturing method of the metal bonded body according to the third embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby providing a manufacturing method of a metal bonded body capable of increasing the bonding strength.

[0073] Furthermore, according to the manufacturing method of the metal joined body of embodiment 4, in the metal joined body formation process S23, the first deformation suppression member 200 and the first die-cast member 50 are combined and the first die-cast member 50 and the second die-cast member 60 are pressed relative to each other, so that it is possible to suppress deformation of the first die-cast member 50 such as by expanding (being pushed outward) during pressing, and as a result, it is possible to suppress a drop in pressure between the first intended joining surface 54 and the second intended joining surface 64.

[0074] The method for producing a metal bonded body according to the fourth embodiment also has the same effects as those of the method for producing a metal bonded body according to the third embodiment.

[0075] The method for joining die-cast members according to the fourth embodiment involves diffusion bonding a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress has been applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60 made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress has been applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68. Therefore, as with the method for joining die-cast members according to the third embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby providing a method for joining die-cast members that can increase the joining strength.

[0076] [Embodiment 5] Fig. 10 is a diagram for explaining the second die-casting member 60a and the second deformation suppressing member 300 in the fifth embodiment. Fig. 10(a) is a perspective view of the second die-casting member 60a, Fig. 10(b) is a plan view of the second die-casting member 60a, Fig. 10(c) is a cross-sectional view taken along line A8-A8 of Fig. 10(b), Fig. 10(d) is a perspective view of the second deformation suppressing member 300, Fig. 10(e) is a plan view of the second deformation suppressing member 300, and Fig. 10(f) is a cross-sectional view taken along line A9-A9 of Fig. 10(e). Fig. 11 is a diagram for explaining the metal bonded body formation step S24 in embodiment 5. Fig. 11(a) is a cross-sectional view showing a state in which the first die-casting member 50 and the second die-casting member 60a are pressed relative to each other, Fig. 11(b) is a cross-sectional view showing a state in which the first intended joining surface 58 and the second intended joining surface 68 are in contact with each other due to pressing, and Fig. 11(c) is a cross-sectional view showing a metal bonded body 130 formed by diffusion bonding.

[0077] The manufacturing method of the metal joined body according to the fifth embodiment is basically the same as the manufacturing method of the metal joined body according to the fourth embodiment, but differs from the manufacturing method of the metal joined body according to the fourth embodiment in terms of the shape of the second die-cast member and the use of a second deformation suppressing member in the metal joined body forming step. The manufacturing method of the metal joined body according to the fifth embodiment includes a metal member preparation step S14 and a metal joined body forming step S24. The joining method of the die-cast members according to the fifth embodiment corresponds to the metal joined body forming step S24. Each step will be described below.

[0078] In the metal member preparation step S14 in embodiment 5, a second die-cast member 60a having a space 69a formed inside a joining protrusion 62 is prepared (see Figs. 10(a) to 10(c)). The second die-cast member 60a has a similar configuration to the second die-cast member 60 in embodiments 3 and 4, except for the space 69a. In the metal member preparation step S14, a first die-cast member 50 similar to the first die-cast member 50 in embodiments 3 and 4 is prepared.

[0079] The second deformation suppressing member 300 in the fifth embodiment is a member that suppresses deformation of the second die-casting member 60a at least in a direction perpendicular to the pressing direction (inward). Specifically, the second deformation suppressing member 300 is a member having a portion that corresponds to the inner shape (space 69a) of the second die-casting member 60a (see Figs. 10(d) to 10(f)). The second deformation suppressing member 300 is made of a material that is less likely to deform than the material that constitutes the second die-casting member 60a. Examples of such materials include steel, cemented carbide, and ceramics. Although the second deformation suppressing member 300 is illustrated as being a member made of a single component, it may be a member made of multiple components (a member that can be separated and combined).

[0080] In the metal bonded body formation process S24 in the fifth embodiment, the first die-casting member 50 and the second die-casting member 60a are pressed relative to each other with the second deformation suppressing member 300 inserted into the space 69a of the bonding protrusion 62 (see Figs. 11(a) and 11(b)). The second deformation suppressing member 300 is removed, like the first deformation suppressing member 200, after the metal bonded body 130 is formed by diffusion bonding (see Fig. 11(c)).

[0081] The manufacturing method of the metal bonded body according to the fifth embodiment includes preparing a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress is applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60a made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress is applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68, and then diffusion-bonding these members to form the metal bonded body 130. Therefore, as with the manufacturing method of the metal bonded body according to the fourth embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby providing a manufacturing method of a metal bonded body capable of increasing the bonding strength.

[0082] Furthermore, according to the manufacturing method of the metal joined body of embodiment 5, in the metal member preparation step S14, a second die-cast member 60a having a space 69a formed inside the joining convex portion 62 is prepared, and in the metal joined body formation step S24, the first die-cast member 50 and the second die-cast member 60a are pressed relative to each other with the second deformation suppression member 300 inserted into the space 69a of the joining convex portion 62, so that it is possible to suppress deformation of the second die-cast member 60a so as to be crushed during pressing, and as a result, it is possible to suppress a drop in pressure between the first planned joining surface 54 and the second planned joining surface 64.

[0083] The method for producing a metal bonded body according to the fifth embodiment also has the same effects as those of the method for producing a metal bonded body according to the fourth embodiment.

[0084] The method for joining die-cast members according to the fifth embodiment involves diffusion bonding a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress has been applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60a made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress has been applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68. Therefore, as with the method for joining die-cast members according to the fourth embodiment, the method for joining die-cast members is capable of increasing the joining strength by promoting the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68 due to the residual stress, and activating the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68.

[0085] [Embodiment 6] Figure 12 is a diagram for explaining the second die-casting member 60b in embodiment 6. Figure 12(a) is a perspective view of the second die-casting member 60b, Figure 12(b) is a plan view of the second die-casting member 60b, and Figure 12(c) is a cross-sectional view taken along A10-A10 in Figure 12(b). Fig. 13 is a diagram for explaining the metal bonded body formation step S25 in embodiment 6. Fig. 13(a) is a cross-sectional view showing a state in which the first die-casting member 50 and the second die-casting member 60b are pressed relative to each other, Fig. 13(b) is a cross-sectional view showing a state in which the first intended joining surface 58 and the second intended joining surface 68 are in contact with each other due to pressing, and Fig. 13(c) is a cross-sectional view showing a metal bonded body 140 formed by diffusion bonding.

[0086] The manufacturing method of the metal joined body according to the sixth embodiment is basically the same as the manufacturing method of the metal joined body according to the third embodiment, but the shape of the second die-cast member is different from that of the manufacturing method of the metal joined body according to the third embodiment. The manufacturing method of the metal joined body according to the sixth embodiment includes a metal member preparation step S15 and a metal joined body formation step S25. The joining method of the die-cast members according to the sixth embodiment corresponds to the metal joined body formation step S25. Each step will be described below.

[0087] In the metal member preparation step S15 in the sixth embodiment, the second die-cast member 60b has a space-forming recess 69b formed on the second intended joining surface 64, which remains as a space even after the metal bonded body 140 is formed (even after the metal bonded body formation step S25) (see FIG. 12). The space-forming recess 69b in the sixth embodiment has a continuous groove shape. In the metal member preparation step S15, the first die-cast member 50 is prepared to be the same as the first die-cast member 50 in the third embodiment.

[0088] The metal bonded body forming step S25 in the sixth embodiment is basically the same as the metal bonded body forming step S22 in the third embodiment, but uses the above-mentioned second die-casting member 60b as the second die-casting member (see Figs. 13(a) and 13(b)). In the metal bonded body 140 thus formed, a space-forming recess 69b remains as a space (see Fig. 13(c)). Such a space-forming recess 69b can be used, for example, as a flow path for a heat exchange medium.

[0089] The manufacturing method of the metal bonded body according to the sixth embodiment includes preparing a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress is applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60b made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress is applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68, and then diffusion-bonding these members to form the metal bonded body 140. Therefore, as in the manufacturing method of the metal bonded body according to the third embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby providing a manufacturing method of a metal bonded body capable of increasing the bonding strength.

[0090] Furthermore, according to the manufacturing method of the metal bonded body of embodiment 6, the second intended joining surface 64 is formed with the space-forming recess 69b that remains as a space even after the metal bonded body 140 is formed, so that it is possible to manufacture a metal bonded body having a complex internal shape.

[0091] The method for producing a metal bonded body according to the sixth embodiment also has the same effects as those of the method for producing a metal bonded body according to the third embodiment.

[0092] The method for joining die-cast members according to the sixth embodiment involves diffusion bonding a first die-cast member 50 made of an aluminum-based material and having first planned joining surfaces 54, 58, in which a residual stress has been applied to the first planned joining surfaces 54, 58 while leaving a chill layer on the first planned joining surfaces 54, 58, and a second die-cast member 60b made of an aluminum-based material and having second planned joining surfaces 64, 68, in which a residual stress has been applied to the second planned joining surfaces 64, 68 while leaving a chill layer on the second planned joining surfaces 64, 68. Therefore, as with the method for joining die-cast members according to the third embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surfaces 54, 58 and the second planned joining surfaces 64, 68, thereby making it possible to increase the joining strength.

[0093] [Embodiment 7] Figure 14 is a diagram for explaining the first die-casting member 80 and the second die-casting member 90 in embodiment 7. Figure 14(a) is a perspective view of the first die-casting member 80, Figure 14(b) is a plan view of the first die-casting member 80, Figure 14(c) is a cross-sectional view taken along A11-A11 in Figure 14(b), Figure 14(d) is a perspective view of the second die-casting member 90, Figure 14(e) is a plan view of the second die-casting member 90, and Figure 14(f) is a cross-sectional view taken along A12-A12 in Figure 14(e). Fig. 15 is a diagram for explaining the metal bonded body formation step S26 in embodiment 7. Fig. 15(a) is a cross-sectional view showing a state in which the first die-casting member 80 and the second die-casting member 90 are pressed relative to each other, Fig. 15(b) is a cross-sectional view showing a state in which the first intended joining surface 84 and the second intended joining surface 94 are in contact entirely due to pressing, and Fig. 15(c) is a cross-sectional view showing a metal bonded body 150 formed by diffusion bonding.

[0094] The manufacturing method of the metal joined body according to the seventh embodiment is basically the same as the manufacturing method of the metal joined body according to the third embodiment, but the shapes of the first die-cast member and the second die-cast member are different from those of the manufacturing method of the metal joined body according to the third embodiment. The manufacturing method of the metal joined body according to the seventh embodiment includes a metal member preparation step S16 and a metal joined body formation step S26. The joining method of the die-cast members according to the seventh embodiment corresponds to the metal joined body formation step S26. Each step will be described below.

[0095] In the metal member preparation process S16 in embodiment 7, a first die-cast member 80 is prepared having a substantially hemispherical joining recess 82 formed therein (see Figures 14(a) to 14(c)), and a second die-cast member 90 is prepared having a substantially hemispherical joining protrusion 92 (see Figures 14(d) to 14(f)).

[0096] In the joining recess 82 of the first die-casting member 80, the entire inner surface (semispherical portion) becomes the first planned joining surface 84. It can be considered that the vicinity of the apex of the joining recess 82 corresponds to the first planned joining surface 58 (bottom surface) in the third embodiment, and the vicinity of the periphery corresponds to the first planned joining surface 54 (first inclined surface) in the third embodiment. Therefore, at least the vicinity of the apex of the hemisphere of the joining recess 82 has a predetermined surface roughness.

[0097] In the joining protrusion 92 of the second die-cast member 90, the entire outer surface (semispherical portion) becomes the second planned joining surface 94. The vicinity of the apex of the joining protrusion 92 can be considered to correspond to the first planned joining surface 58 (tip surface) in embodiment 3, and the vicinity of the periphery can be considered to correspond to the second planned joining surface 64 (second inclined surface) in embodiment 3. Therefore, at least the vicinity of the apex of the hemisphere of the joining protrusion 92 also has a predetermined surface roughness. Note that the joining protrusion 92 has a slightly larger diameter than the joining recess 82 in order to satisfy the condition that "the joining protrusion 92 is shaped so that the first inclined surface and the second inclined surface butt against each other when inserted into the joining recess 82."

[0098] The metal bonded body forming step S26 in the seventh embodiment is basically the same as the metal bonded body forming step S22 in the third embodiment, except for the difference in the shapes of the first die-cast member 80 and the second die-cast member 90. That is, in the metal bonded body forming step S26, the first die-cast member 80 and the second die-cast member 90 are pressed relative to each other with the bonding protrusion 92 inserted into the bonding recess 82 (see FIG. 15(a)). As a result, the apex of the first planned bonding surface 84 and the apex of the second planned bonding surface 94 come into contact with each other (see FIG. 15(b)). Therefore, the entire surfaces of the first planned bonding surface 84 and the second planned bonding surface 94 are diffusion bonded, and the metal bonded body 150 is formed (see FIG. 15(c)).

[0099] The manufacturing method of the metal bonded body according to the seventh embodiment involves preparing a first die-cast member 80 made of an aluminum-based material and having a first planned joining surface 84, in which a residual stress is imparted to the first planned joining surface 84 while leaving a chill layer on the first planned joining surface 84, and a second die-cast member 90 made of an aluminum-based material and having a second planned joining surface 94, in which a residual stress is imparted to the second planned joining surface 94 while leaving a chill layer on the second planned joining surface 94, and then diffusion-bonding these members to form the metal bonded body 150. Therefore, as with the manufacturing method of the metal bonded body according to the third embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surface 84 and the second planned joining surface 94, and activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 84 and the second planned joining surface 94, thereby achieving a manufacturing method of a metal bonded body capable of increasing the bonding strength.

[0100] The method for producing a metal bonded body according to the seventh embodiment also has the same effects as those of the method for producing a metal bonded body according to the third embodiment.

[0101] The method for joining die-cast members according to the seventh embodiment involves diffusion bonding a first die-cast member 80 made of an aluminum-based material and having a first planned joining surface 84, in which a chill layer is left on the first planned joining surface 84 while residual stress is imparted to the first planned joining surface 84, and a second die-cast member 90 made of an aluminum-based material and having a second planned joining surface 94, in which a chill layer is left on the second planned joining surface 94 while residual stress is imparted to the second planned joining surface 94. As a result, similar to the method for joining die-cast members according to the third embodiment, the residual stress promotes the generation of lattice defects in the first planned joining surface 84 and the second planned joining surface 94, and thereby activates the diffusion of atoms and the establishment of metallic bonds between the first planned joining surface 84 and the second planned joining surface 94, thereby making it possible to increase the joining strength.

[0102] Although the present invention has been described based on the above-mentioned embodiments, the present invention is not limited to the above-mentioned embodiments. The present invention can be embodied in various forms without departing from the spirit of the present invention, and for example, the following modifications are also possible.

[0103] (1) The shapes of the first and second die-cast members in the above embodiments are merely examples, and any shape may be used without departing from the scope of the present invention.

[0104] (2) In the sixth embodiment, the space-forming recess 69b has a continuous groove shape, but the present invention is not limited to this. The space-forming recess may have any shape.

[0105] (3) In the sixth embodiment, the space-forming recess 69b is formed on the second planned joining surface 64, but the present invention is not limited to this. The space-forming recess may be formed on the first planned joining surface, or on both the first planned joining surface and the second planned joining surface.

[0106] (4) The features of the above fourth to seventh embodiments are applicable to the other embodiments as long as there are no prohibitive factors.

[0107] (5) In each of the above embodiments, the first die-casting member has a first intended joining surface imparted with residual stress by plastically deforming the surface of the first intended joining surface, and the second die-casting member has a second intended joining surface imparted with residual stress by plastically deforming the surface of the second intended joining surface, but the present invention is not limited to this. The first die-casting member and the second die-casting member may have a first intended joining surface and a second intended joining surface imparted with residual stress by a means other than plastic deformation (for example, a heat treatment such as quenching).

[0108] (6) In the above embodiments, the first die-cast member has a first intended joining surface imparted with residual stress by shot blasting, and the second die-cast member has a second intended joining surface imparted with residual stress by shot blasting, but the present invention is not limited to this. The first die-cast member and the second die-cast member may have a first intended joining surface and a second intended joining surface imparted with residual stress by plastic deformation by a process other than shot blasting.

[0109] (7) In the above embodiment 1, it is preferable to perform the metal bonded body formation process S20 while heating the first die-cast member 10 and the second die-cast member 20 and maintaining them at a certain temperature (however, below the melting point) in order to promote diffusion bonding, but the present invention is not limited to this. For example, since it is considered that diffusion bonding is likely to proceed in an environment such as outer space, when the metal bonded body formation process of the present invention is performed in such an environment, it is not necessarily necessary to heat the first die-cast member and the second die-cast member. This is also true for the metal bonded body formation processes of the other embodiments. [Explanation of symbols]

[0110] 10,30,50,80...first die-cast member, 12,34,54,58,84...first intended joining surface, 20,40,60,60a,60b,90...second die-cast member, 22,44,64,68,94...second intended joining surface, 32,52,82,92...joining recess, 42,62...joining protrusion, 69a...space, 69b...space-forming recess, 100,110,120,130,140,150...metal joined body, 200...first deformation suppressing member, 300...second deformation suppressing member

Claims

1. a metal member preparation process for preparing a first die-cast member made of an aluminum-based material and having a first planned joining surface, the first die-cast member having a chill layer remaining on the first planned joining surface while imparting residual stress to the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, the second die-cast member having a chill layer remaining on the second planned joining surface while imparting residual stress to the second planned joining surface; and a metal bonded body formation process for forming a metal bonded body by diffusion bonding the first die-cast member and the second die-cast member, by pressing the first die-cast member and the second die-cast member relatively so that pressure is applied to the first and second planned joining surfaces while the first and second planned joining surfaces are in contact with each other.

2. the first die-casting member has a first intended joining surface that is plastically deformed to impart residual stress to the first intended joining surface, The method for manufacturing a metal joined body according to claim 1, characterized in that the second die-cast member has a residual stress imparted to the second intended joining surface by plastically deforming the surface of the second intended joining surface.

3. the first die-cast member is a member in which a residual stress is imparted to the first intended joining surface by plastically deforming the surface of the first intended joining surface through a shot blasting treatment; The method for manufacturing a metal joined body according to claim 2, characterized in that the second die-cast member has a residual stress imparted to the second intended joining surface by plastically deforming the surface of the second intended joining surface through shot blasting treatment.

4. In the metal member preparation step, the first die-cast member and the second die-cast member, each of which has a predetermined surface roughness, are prepared, 4. The method for manufacturing a metal joined body according to any one of claims 1 to 3, characterized in that in the metal joined body formation process, the first die-casting member and the second die-casting member are diffusion-bonded to form a metal joined body while generating changes in the surface microstructure of the first intended joining surface and the second intended joining surface by pressing the first die-casting member and the second die-casting member relative to each other.

5. In the metal member preparation step, the first die-cast member is provided with a joining recess, at least a part of whose inner surface is a first inclined surface angled with respect to the pressing direction in the metal bonded body formation step, and the second die-cast member is provided with a joining protrusion, at least a part of whose side surface is a second inclined surface angled corresponding to the first inclined surface, and the second die-cast member is provided with a joining protrusion, the first inclined surface and the second inclined surface abut against each other when the second die-cast member is inserted into the joining recess. At least a part of the first inclined surface is the first intended joining surface, At least a part of the second inclined surface is the second intended joining surface, The method for manufacturing a metal joined body according to any one of claims 1 to 3, characterized in that in the metal joined body formation process, the first die-cast member and the second die-cast member are pressed relative to each other with the joining convex portion inserted into the joining concave portion, thereby forming a metal joined body by diffusion bonding the first die-cast member and the second die-cast member while generating a change in the surface microstructure of the first intended joining surface and the second intended joining surface.

6. The method for manufacturing a metal joined body as described in claim 5, characterized in that in the metal joined body formation process, the first die-casting member and the second die-casting member are pressed relative to each other in a state in which the first die-casting member is combined with a first deformation suppression member that suppresses deformation of the first die-casting member at least in a direction perpendicular to the pressing direction.

7. In the metal member preparation step, a second die-cast member having a space formed inside the joining protrusion is prepared, The method for manufacturing a metal joined body as described in claim 5, characterized in that in the metal joined body formation process, the first die-cast member and the second die-cast member are pressed relative to each other while a second deformation suppression member that suppresses deformation of the second die-cast member at least in a direction perpendicular to the pressing direction is inserted into the space of the joining convex portion.

8. The method for manufacturing a metal joined body according to any one of claims 1 to 3, characterized in that in the metal joined body formation process, the first die-cast member and the second die-cast member are pressed relative to each other under temperature conditions that enable diffusion bonding of the first die-cast member and the second die-cast member.

9. The method for manufacturing a metal joined body according to any one of claims 1 to 3, characterized in that at least one of the first intended joining surface and the second intended joining surface has a space-forming recess formed therein, which remains as a space even after the metal joined body is formed.

10. a first die-cast member made of an aluminum-based material and having a first planned joining surface, the first planned joining surface being imparted with residual stress while leaving a chill layer on the first planned joining surface, and a second die-cast member made of an aluminum-based material and having a second planned joining surface, the second planned joining surface being imparted with residual stress while leaving a chill layer on the second planned joining surface, the first die-cast member and the second die-cast member being brought into contact with each other, and the first die-cast member and the second die-cast member being pressed relative to each other so that pressure is applied to the first planned joining surface and the second planned joining surface, thereby diffusion-bonding the first die-cast member and the second die-cast member to form a metal joint body.

Citation Information

Patent Citations

  • Doryokudentatsusochi

    JP1976098458A

  • Method of mutually joining metal

    JP1985037281A

  • Method of manufacturing rigid internal tooth gear for wave motive gear