Laser Marker Label

The laser marker label with a white layer of acrylic urethane copolymer maintains print distinguishability under harsh conditions by using crosslinking points to prevent peeling, addressing the challenge of visibility in high temperature and humidity environments.

JP7564610B2Active Publication Date: 2024-10-09LINTEC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2018229918
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-12-07
Publication Date
2024-10-09
Estimated Expiration
2038-12-07

AI Technical Summary

Technical Problem

Laser marker labels used for vehicle identification and hull numbers need to maintain print distinguishability under harsh environments, including high temperature and high humidity conditions, as well as outdoor exposure, to ensure long-term visibility of printed information.

Method used

The laser marker label consists of a black layer and a white layer, where the white layer is made of an acrylic urethane copolymer with ethylenically unsaturated groups at both ends, formed by polymerizing a (meth)acrylic acid ester, which provides crosslinking points to maintain structural integrity under extreme conditions.

Benefits of technology

The label maintains excellent print distinguishability after exposure to high temperature and high humidity environments and outdoor conditions, preventing peeling and ensuring clear visibility of printed information.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564610000002
    Figure 0007564610000002
  • Figure 0007564610000003
    Figure 0007564610000003
  • Figure 0007564610000001
    Figure 0007564610000001
Patent Text Reader

Abstract

To provide a laser marker label excellent in print discriminability both after exposure to high temperature and high humidity environment and exposure to outdoor environment.SOLUTION: A laser marker label has a black layer 14 and a white layer 13, in which a resin constituting the white layer contains an acrylic urethane copolymer in which a resin constituting the white layer is obtained by polymerizing (meth)acrylate with an urethane prepolymer having ethylenically unsaturated groups at both ends.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laser marker label. [Background technology]

[0002] A laser marker label has a surface layer that absorbs laser light, generates heat, is destroyed, and can be removed, and a lower layer that is adjacent to the surface layer and has a brightness difference that is easily visible from the surface layer, and is a label that can be printed clearly due to the color difference between the surface layer and the lower layer by irradiating the surface with laser light to cut away characters and the like in a pattern. For example, a laser marker label has a black layer that is placed on the surface layer, and a white layer that is placed under the black layer, and records information by cutting away the black layer with laser light to expose the white layer, which is the lower layer, and making the white color in the black layer visible (for example, Patent Document 1).

[0003] Laser marker labels are widely used for labels that display the vehicle identification number (VIN) of an automobile, labels that display the hull identification number of a vessel such as a motorboat, and anti-theft labels. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-90063 A Summary of the Invention [Problem to be solved by the invention]

[0005] In particular, a label that displays the vehicle identification number of an automobile or the hull identification number of a ship is required to have durability in a harsh environment. Specifically, when a label that displays the vehicle identification number of an automobile is transported by ship, the label may be placed in a high-temperature and high-humidity environment (e.g., 70°C, 90% RH) that deviates from the normal environment. In addition, a label that displays the hull identification number of a ship may be immersed in water or exposed to high temperatures depending on the location where it is attached. Therefore, the laser marker label used for the above-mentioned purpose is required to be able to identify the printed information even after being exposed to a high-temperature and high-humidity environment for a long period of time (printing identifiability after exposure to a high-temperature and high-humidity environment). In addition, the laser marker label used for the above-mentioned purpose is required to be able to identify the printed information even after being exposed to an outdoor environment for a long period of time (printing identifiability after exposure to an outdoor environment) because it may be left outdoors for a long period of time depending on the usage conditions.

[0006] Therefore, an object of the present invention is to provide a laser marker label that has excellent print identification properties both after exposure to a high-temperature, high-humidity environment and after exposure to an outdoor environment. [Means for solving the problem]

[0007] In order to achieve the above-mentioned object, the laser marker label of the present invention is a laser marker label having a black layer and a white layer, in which the resin constituting the white layer contains an acrylic urethane copolymer obtained by polymerizing a (meth)acrylic acid ester with a urethane prepolymer having ethylenically unsaturated groups at both ends. Effect of the Invention

[0008] According to the present invention, a laser marker label that has excellent print identification properties both after exposure to a high-temperature, high-humidity environment and after exposure to an outdoor environment can be obtained. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic cross-sectional view showing how laser marking is performed on a laser marker label according to this embodiment. FIG. [Diagram 2] 2 is a schematic plan view of the laser marker label of FIG. 1(C) viewed from above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the attached drawings. In the description of the drawings, the same elements are given the same reference numerals, and duplicated description will be omitted. In addition, the dimensional ratios of the drawings are exaggerated for the convenience of explanation, and may differ from the actual ratios.

[0011] In this specification, the range "X to Y" means "X or more and Y or less." Unless otherwise specified, the operations and physical properties are measured under the conditions of room temperature (20 to 25°C) and relative humidity of 45 to 55% RH. In this specification, "(meth)acrylic" refers to "acrylic or methacrylic."

[0012] A laser marker label according to one embodiment of the present invention has a black layer and a white layer, and the resin constituting the white layer contains an acrylic urethane copolymer obtained by polymerizing a (meth)acrylic acid ester with a urethane prepolymer having ethylenically unsaturated groups at both ends. The laser marker label has excellent print identification properties both after exposure to a high-temperature and high-humidity environment and after exposure to an outdoor environment.

[0013] The present inventors have conducted extensive research into the resin that constitutes the white layer of the laser marker label. As a result, they have found that by using an acrylic urethane copolymer (hereinafter also simply referred to as "acrylic urethane copolymer") obtained by polymerizing a (meth)acrylic acid ester with a urethane prepolymer having ethylenically unsaturated groups at both ends for the white layer, it is possible to achieve both print identification properties of the laser marker label after exposure to a high-temperature, high-humidity environment and print identification properties after exposure to an outdoor environment. It is believed that the acrylic urethane copolymer has a structure in which a polymer of a (meth)acrylic acid ester is crosslinked at multiple points via a urethane prepolymer. Therefore, even if the urethane portion is damaged by water or the acrylic portion is damaged by ultraviolet light or heat, the crosslinked points remain and the crosslinked structure can be maintained. As a result, the white layer is less likely to generate gas even when exposed to water, ultraviolet light, or heat. Therefore, the laser marker label according to one embodiment of the present invention is less likely to float at the interface between the white layer and the black layer even when stored for a long period of time in a high-temperature, high-humidity environment and outdoors, and the black layer is prevented from peeling off and exposing the white layer. Therefore, it is believed that the printed information can be identified (that is, the print identification properties are excellent both after exposure to a high temperature and high humidity environment and after exposure to an outdoor environment).

[0014] It should be noted that the above mechanism is merely speculation, and the present invention is not limited to the above mechanism.

[0015] In the following description, the laser marker label may be simply referred to as a "label." The concept of a "label" includes things called tapes, films, sheets, etc.

[0016] 1(A) is a schematic cross-sectional view of a laser marker label 10 according to this embodiment. The laser marker label 10 has a release liner 11, an adhesive layer 12, a white layer 13, and a black layer 14, in this order.

[0017] The release liner 11 prevents adhesion of dirt and other foreign matter to the adhesive layer 12 until the adhesive layer 12 is attached to an adherend (e.g., an automobile, a ship, etc.). Therefore, the release liner 11 is peeled off when the label 10 is attached to the adherend. For this reason, the laser marker label 10 also includes those that do not have a release liner 11.

[0018] The white layer 13 and the black layer 14 are disposed adjacent to each other. With this configuration, visible information can be imparted to the label due to the color difference between the two layers.

[0019] The black layer 14 is brittle and breaks when the white layer 13 breaks.

[0020] The laser marker label 10 may further have a coating layer on the black layer 14. By providing a coating layer so as to cover the black layer 14, it is possible to prevent the white layer 13 from being exposed even if the black layer 14 is unintentionally scratched.

[0021] The method of forming each layer of the laser marker label 10, the materials, etc. will be described below.

[0022] <Release liner 11> The release liner 11 is not particularly limited, but examples thereof include paper such as fine paper, glassine paper, and kraft paper; polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; and plastic films such as polyolefin films such as polypropylene and polyethylene.

[0023] The thickness of release liner 11 is usually about 10 to 400 μm. A layer made of a release agent such as silicone may be provided on the surface of release liner 11 in order to improve the releasability of pressure-sensitive adhesive layer 12. When such a layer is provided, the thickness of the layer is usually about 0.01 to 5 μm.

[0024] <Adhesive layer 12> The adhesive used in the adhesive layer 12 is not particularly limited, and may be an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyester adhesive, a styrene-diene block copolymer adhesive, or the like. Among them, from the viewpoint of adhesive reliability, an acrylic adhesive is particularly preferred. The above adhesives may be used alone or in combination of two or more kinds.

[0025] The pressure-sensitive adhesive preferably further contains a crosslinking agent, such as an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, or a metal chelate-based crosslinking agent.

[0026] If necessary, the adhesive layer 12 may appropriately contain colorants, fillers, antistatic agents, tackifiers, wetting agents, leveling agents, thickeners, antifoaming agents, preservatives, and the like.

[0027] The thickness of the adhesive layer 12 is not particularly limited, but from the viewpoint of adhesiveness, it is preferably 10 to 100 μm.

[0028] The method for forming the adhesive layer 12 is not particularly limited, but a method of applying an adhesive onto the release liner 11 is adopted. The application method is not particularly limited, and for example, application can be performed using a known application device such as a roll coater, a knife coater, an air knife coater, a bar coater, a blade coater, a slot die coater, a lip coater, or a gravure coater. The thickness of the applied adhesive is usually 10 to 100 μm, preferably 15 to 50 μm. After the adhesive is applied onto the release liner 11, a drying treatment is performed to form the adhesive layer 12. The drying conditions at this time are not particularly limited, and the drying is usually performed at 60 to 150° C. for 10 to 60 seconds.

[0029] <White layer 13> The white layer 13 contains an acrylic urethane copolymer as a constituent resin, and preferably further contains a white colorant.

[0030] [Acrylic urethane copolymer] The acrylic urethane copolymer is prepared by polymerizing a (meth)acrylic acid ester with a urethane prepolymer having ethylenically unsaturated groups at both ends (hereinafter, also simply referred to as "urethane prepolymer"). Here, the ethylenically unsaturated groups refer to acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, etc.

[0031] The acrylic urethane copolymer may be a polymer obtained by polymerizing a urethane prepolymer with a (meth)acrylic acid ester (hereinafter also referred to as "polymer X"), or a crosslinked body obtained by crosslinking polymer X with a crosslinking agent.

[0032] The molecular weight of the polymer X is not particularly limited, but in order to further enhance the effects of the present invention, the weight average molecular weight (Mw) is preferably 15,000 to 100,000, and more preferably 30,000 to 100,000. The weight average molecular weight is a value calculated in terms of polystyrene measured by gel permeation chromatography (GPC).

[0033] The viscosity of the polymer X is preferably 1,000 to 10,000 mPa·s (25° C.).

[0034] The raw materials and production method of polymer X will be described below.

[0035] (Urethane prepolymer) In order to further enhance the effects of the present invention, the weight average molecular weight of the urethane prepolymer is preferably 10,000 to 100,000. The weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0036] The urethane prepolymer may be either linear or branched.

[0037] The urethane prepolymer may be either a synthetic product or a commercially available product.

[0038] When synthesizing a urethane prepolymer, the synthesis method is not particularly limited, but for example, a method of adding a diisocyanate compound to the hydroxyl groups at both ends of a high molecular weight diol compound to obtain a urethane prepolymer having isocyanate groups at both ends (hereinafter also referred to as a "urethane prepolymer precursor") (step 1), and then adding an ethylenically unsaturated monomer having a hydroxyl group to the isocyanate groups at both ends of the urethane prepolymer precursor to convert both ends into ethylenically unsaturated groups (step 2) can be mentioned. Hereinafter, this method will be described.

[0039] <Step 1: Synthesis of urethane prepolymer precursor> Examples of the high molecular weight diol compound used in step 1 include polyether diol, polycarbonate diol, polyester diol, and the like.

[0040] Examples of polyether diols include polyoxyethylene glycol (hereinafter abbreviated as PEG), polyoxyethyleneoxypropylene block copolymer diol, polyoxyethyleneoxytetramethylene block copolymer diol; ethylene oxide adducts of low molecular weight glycols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexamethylene glycol, neopentyl glycol, bis(hydroxymethyl)cyclohexane, and 4,4'-bis(2-hydroxyethoxy)-diphenylpropane; condensed polyether ester diols obtained by reacting PEG having a number average molecular weight of 2,000 or less with one or more dicarboxylic acids [aliphatic dicarboxylic acids having 4 to 10 carbon atoms (e.g., succinic acid, adipic acid, sebacic acid, etc.), aromatic dicarboxylic acids having 8 to 15 carbon atoms (e.g., terephthalic acid, isophthalic acid, etc.)]; and mixtures of two or more of these.

[0041] An example of the polycarbonate diol is polyhexamethylene carbonate diol.

[0042] Examples of polyester diols include condensed polyester diols obtained by reacting low molecular weight diols and / or polyether diols having a number average molecular weight of 1,000 or less with one or more of the above-mentioned dicarboxylic acids, and polylactone diols obtained by ring-opening polymerization of lactones having 4 to 12 carbon atoms. Examples of the low molecular weight diols include low molecular weight glycols exemplified in the above polyether diol section. Examples of the polyether diols having a number average molecular weight of 1,000 or less include polyoxypropylene glycol and PTMG. Examples of the lactones include ε-caprolactone and γ-valerolactone. Specific examples of the polyester diols include polyethylene adipate diol, polybutylene adipate diol, polyneopentylene adipate diol, poly(3-methyl-1,5-pentylene adipate) diol, polyhexamethylene adipate diol, polycaprolactone diol, and mixtures of two or more of these.

[0043] Among these, polycarbonate diols are preferred from the viewpoint of further improving print identifiability after exposure to a high-temperature and high-humidity environment and / or outdoor environment.

[0044] The weight average molecular weight of the high molecular weight diol compound is preferably 500 to 200,000. The weight average molecular weight is a value measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0045] The high molecular weight diol compound may be either a synthetic product or a commercially available product, such as Nipporan (registered trademark) 981, 980R, 982R, 976, 965, 963, 964, and 968 manufactured by Tosoh Corporation.

[0046] The high molecular weight diol compounds may be used alone or in combination of two or more kinds.

[0047] The diisocyanate compound used in step 1 includes trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 2,6-diisocyanate, 1,2-dimethylphenyl di ... Aliphatic diisocyanates such as socyanate methyl caprate, lysine diisocyanate, lysine ester triisocyanate, 1,6,11-undecane triisocyanate, 1,3,6-hexamethylene triisocyanate, trimethylhexamethylene diisocyanate, decamethylene diisocyanate, etc.; aromatic diisocyanates such as tolylene diisocyanate, xylene diisocyanate, etc.; and alicyclic diisocyanates such as isophorone diisocyanate, etc. The diisocyanate compounds may be used alone or in combination of two or more.

[0048] In step 1, the high molecular weight diol compound and the diisocyanate compound are preferably reacted in a molar ratio of 1:1.5 to 1:4.0. By allowing the latter to exist in excess, the urethane prepolymer precursor can be obtained with high efficiency.

[0049] A solvent may be used in step 1. The solvent is not particularly limited as long as it can dissolve the above components and does not interfere with the reaction between the high molecular weight diol compound and the diisocyanate compound, and examples of the solvent include toluene and methyl ethyl ketone.

[0050] In step 1, known additives such as a catalyst and a chain extender may be further used.

[0051] The reaction conditions in step 1 can be appropriately selected, and are, for example, under a nitrogen atmosphere, at a temperature of 60 to 90° C., and for 3 to 10 hours.

[0052] <Step 2: Synthesis of urethane prepolymer> In step 2, an ethylenically unsaturated monomer having a hydroxyl group is added to the isocyanate groups at both ends of the urethane prepolymer precursor obtained in step 1 to convert both ends into ethylenically unsaturated groups, thereby obtaining a urethane prepolymer.

[0053] Examples of the ethylenically unsaturated monomer having a hydroxyl group used in step 2 include (meth)acrylic monomers containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. The above compounds may be used alone or in combination of two or more.

[0054] In step 2, the urethane prepolymer precursor and the ethylenically unsaturated monomer having a hydroxyl group are preferably reacted in a molar ratio of 1:1.5 to 1:4.0. By making the latter exist in excess, the urethane prepolymer can be obtained with high efficiency.

[0055] A solvent may be used in step 2. As the solvent, the same solvent as described in step 1 can be used.

[0056] In step 2, known additives such as a catalyst and a chain extender may be further used.

[0057] The reaction conditions in step 2 can be appropriately selected, and are, for example, under a nitrogen atmosphere, at a temperature of 60 to 90° C., and for 3 to 10 hours.

[0058] ((Meth)acrylic acid ester) Examples of (meth)acrylic acid esters to be polymerized with the urethane prepolymer to obtain the polymer X include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate; and (meth)acrylic acid esters having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate. The (meth)acrylic acid esters may be used alone or in combination of two or more.

[0059] When a (meth)acrylic acid ester having a reactive group such as a hydroxyl group is polymerized with a urethane prepolymer, a polymer X having the reactive group is obtained, which can be crosslinked with a crosslinking agent described later. Therefore, a white layer having a higher crosslink density is obtained, and the print identifiability of the laser marker label after exposure to a high temperature and high humidity environment and / or the print identifiability after exposure to an outdoor environment is further improved. Among them, a combination of a polymer X having a hydroxyl group and an isocyanate-based crosslinking agent is more preferable because a highly crosslinked white layer can be formed in a short time. Therefore, it is preferable to polymerize a (meth)acrylic acid ester having a hydroxyl group with a urethane prepolymer. That is, in one embodiment of the present invention, the (meth)acrylic acid ester includes a (meth)acrylic acid ester having a hydroxyl group.

[0060] In step 2, the amount of the (meth)acrylic acid ester having a hydroxyl group used is preferably 1 to 20 mass %, more preferably 2 to 10 mass %, based on the total amount of the (meth)acrylic acid esters used.

[0061] (Production method of polymer X) The method for producing the polymer X is not particularly limited, and conventionally known methods such as solution polymerization, emulsion polymerization, suspension polymerization, reversed-phase suspension polymerization, thin film polymerization, and spray polymerization using a polymerization initiator can be used. In addition to the method of initiating polymerization using a polymerization initiator, a method of initiating polymerization by irradiation with radiation, electron beams, ultraviolet rays, etc. can also be adopted. Among them, the solution polymerization method using a polymerization initiator is preferred because it is easy to adjust the molecular weight and can reduce impurities. For example, the polymer X can be obtained by using ethyl acetate, toluene, methyl ethyl ketone, etc. as a solvent, adding preferably 0.01 to 0.50 parts by mass of the polymerization initiator relative to 100 parts by mass of the total amount of the monomers, and reacting in a nitrogen atmosphere at a reaction temperature of, for example, 60 to 110° C. for 3 to 112 hours.

[0062] Examples of the polymerization initiator include azo compounds such as azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylbutyronitrile), and azobiscyanovaleric acid; organic peroxides such as tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butylperoxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; and inorganic peroxides such as hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate. These may be used alone or in combination of two or more. The amount of the polymerization initiator used is preferably 0.1 to 10% by mass based on the total amount of all monomers used in the production of the polymer X.

[0063] In producing the polymer X, in addition to the above-mentioned urethane prepolymer and (meth)acrylic acid ester, a monomer copolymerizable therewith (hereinafter also referred to as "other monomer") may be used. Examples of the other monomer include carboxyl group-containing monomers such as (meth)acrylic acid, itaconic acid, and maleic acid; aromatic vinyl compounds such as styrene and substituted styrene; vinyl esters such as vinyl acetate; amide group-containing monomers such as acrylamide, methacrylamide, N-vinylpyrrolidone, and N,N-dimethylacrylamide; and amino group-containing monomers such as aminoethyl (meth)acrylate and (meth)acryloylmorpholine. The reactive groups contained in these monomers can also be crosslinked with the crosslinking agent described below to form a crosslinked structure. The amount of the other monomer used is preferably 5% by mass or less (lower limit: 0% by mass) based on the total amount of all monomers used in the production of the polymer X.

[0064] In addition, a chain transfer agent may be added to the monomer solution for the purpose of appropriately controlling the molecular weight of the polymer X. Examples of the chain transfer agent include thiol compounds such as n-dodecyl mercaptan, 2-mercaptoethanol, β-mercaptopropionic acid, octyl β-mercaptopropionate, methoxybutyl β-mercaptopropionate, trimethylolpropane tris(β-thiopropionate), butyl thioglycolate, thioglycerol, propanethiols, butanethiols, and thiophosphites, and halogen compounds such as carbon tetrachloride. These may be used alone or in combination of two or more. From the viewpoint of appropriately controlling the molecular weight and not impairing the effects of the present invention, the amount of the chain transfer agent used is preferably 10 to 80% by mass relative to the amount of the polymerization initiator used.

[0065] (Crosslinking agent) The acrylic urethane copolymer may be a crosslinked body obtained by crosslinking polymer X with a crosslinking agent. By including an acrylic urethane copolymer having such a form, the crosslink density of the white layer becomes higher. Therefore, the print identifiability of the laser marker label after exposure to a high-temperature and high-humidity environment and / or the print identifiability after exposure to an outdoor environment is further improved. That is, in one embodiment of the present invention, the acrylic urethane copolymer is obtained by crosslinking a polymer (polymer X) obtained by polymerizing a (meth)acrylic acid ester with a urethane prepolymer having ethylenically unsaturated groups at both ends with a crosslinking agent.

[0066] As the crosslinking agent, a known crosslinking agent can be appropriately used depending on the type of reactive group to be introduced into the polymer X, and examples thereof include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a metal chelate-based crosslinking agent, etc. Among them, when the reactive group to be introduced into the polymer X is a hydroxyl group, an isocyanate-based crosslinking agent is preferred from the viewpoint of forming a highly crosslinked white layer in a short period of time.

[0067] Examples of the isocyanate crosslinking agent include the above diisocyanate compounds, adducts of the above diisocyanate compounds with polyol compounds such as trimethylolpropane, and isocyanate derivatives such as biuret and isocyanurate of the above diisocyanate compounds.

[0068] Examples of epoxy crosslinking agents include polyglycidylamine type epoxy resins, bisphenol A type epoxy resins, novolac type epoxy resins, alicyclic type epoxy resins, aliphatic epoxy resins, brominated epoxy resins, and alcohol type epoxy resins.

[0069] Examples of the metal chelate crosslinking agent include acetylacetonate complexes of metals such as aluminum, titanium, nickel, chromium, iron, zinc, cobalt, manganese, and zirconium.

[0070] The crosslinking agent may be used alone or in combination of two or more kinds.

[0071] [White colorants] The white colorant is preferably an inorganic pigment, such as titanium dioxide, alumina white, zinc oxide, zinc sulfide, calcium carbonate, clay, barium sulfate, silica, and white mica. Among them, from the viewpoint of providing whiteness, the colorant is preferably titanium dioxide. These white colorants may be used alone or in combination of two or more.

[0072] The amount of the white colorant in the white layer is preferably 1 to 50 mass % (solid content equivalent), and more preferably 5 to 30 mass % (solid content equivalent).

[0073] [Additives] In addition to the above components, the white layer may contain additives within the range that does not impair the effects of the present invention. Examples of the additives include fillers, resins, plasticizers, antioxidants, UV absorbers, light stabilizers, antistatic agents, flame retardants, dispersants, etc.

[0074] [Physical properties of the white layer] The thickness of the white layer 13 is preferably 50 μm or more, more preferably 60 μm or more, from the viewpoint of preventing the laser L from penetrating the white layer 13 during laser marking. Also, from the viewpoint of increasing the brittleness of the laser marker label and imparting a tamper-proof function, the thickness is preferably 200 μm or less, more preferably 100 μm or less.

[0075] [Manufacturing method of white layer] The white layer 13 can be formed, for example, by preparing a dispersion (hereinafter, white layer-forming dispersion) in which the polymer X and, if necessary, a white colorant, a crosslinking agent, and an additive are dispersed in a solvent, casting the dispersion onto a processing film to a predetermined dry thickness, and drying by heating (solvent casting method). The white layer 13 may also be formed by other manufacturing methods (calender method, melting method).

[0076] The solvent used in the solvent casting method can be appropriately selected, and examples of the solvent that can be used include halogenated hydrocarbons such as methylene chloride, chloroform, and tetrachloroethane, ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, esters such as ethyl acetate, ethyl lactate, butyl acetate, and methyl 2-hydroxyisobutyrate, aromatic hydrocarbons such as benzene, toluene, and xylene, ethers such as diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, and dioxane, ether alcohols such as propylene glycol monomethyl ether, ethyl cellosolve, and butyl cellosolve, ether esters such as butyl cellosolve monoacetate and propylene glycol monomethyl ether monoacetate, amides such as dimethylformamide and dimethylacetamide, and sulfoxides such as dimethyl sulfoxide. These solvents may be used alone or in combination of two or more.

[0077] The amount of the solvent used is usually 100 to 400 parts by mass, and preferably 150 to 350 parts by mass, based on 100 parts by mass of the polymer X.

[0078] The coating device for casting the white layer-forming dispersion onto the process film is not particularly limited, and examples thereof include coaters such as knife coaters, lip coaters, die coaters, doctor blade coaters, bar coaters, and roll coaters. Next, the solvent is removed by heating to form a film. The heating conditions are not particularly limited as long as the solvent can be removed, and are appropriately set. For example, from the viewpoint of promoting the crosslinking reaction between the polymer X and the crosslinking agent, the heating temperature is preferably about 80 to 180°C.

[0079] Examples of materials for the casting film include synthetic resin films such as polyethylene terephthalate, polyethylene naphthalate, polyimide, and polypropylene. The casting film may have a release layer of alkyd resin, silicone, or the like on the synthetic resin film. In this case, a white layer 13 is formed on the surface on which the release layer is formed. The thickness of the casting film is preferably 5 to 200 μm, and more preferably 15 to 100 μm.

[0080] <Black Layer 14> The black layer 14 preferably contains a black-based colorant and a resin.

[0081] [Black colorants] Examples of black colorants include carbon black, iron black, cobalt oxide pigments, aniline black, and perylene black. Among them, carbon black is preferably used as a black colorant because of its good laser light absorption. The preferred average primary particle size of carbon black is in the range of 10 to 500 nm, more preferably in the range of 10 to 150 nm. Here, the average primary particle size of carbon black is the arithmetic mean diameter obtained by observing 1000 carbon black particles with an electron microscope. Carbon black includes channel black, furnace black, acetylene black, thermal black, and the like, depending on the production method, and any of them can be used. The black colorant may be used alone or in combination of two or more kinds.

[0082] From the viewpoints of coloring property and mechanical strength, the content of the colorant in the black layer 14 is preferably 1 to 50 mass % relative to the solid content of the black layer, and more preferably 5 to 20 mass %.

[0083] [resin] The resin may be a thermosetting resin or an ultraviolet curing resin.

[0084] From the viewpoint of laser processability, it is preferable to use a urethane resin, an acrylic resin, the above-mentioned acrylic urethane copolymer, a polyester resin, or the like as the resin. Among them, it is preferable to use the above-mentioned acrylic urethane copolymer from the viewpoint of further improving print identification after both exposure to a high-temperature and high-humidity environment and exposure to an outdoor environment. Therefore, in a preferred embodiment of the present invention, the resin constituting the black layer contains the above-mentioned acrylic urethane copolymer. In this case, the acrylic urethane copolymer may be polymer X or a crosslinked product of polymer X.

[0085] [Additives] The black layer 14 may contain additives as long as the effects of the present invention are not impaired.

[0086] For example, when the black colorant does not have the property of absorbing laser light, a compound for converting laser light into heat may be required. Examples of the compound for converting laser light into heat include infrared absorbents such as cyanine and phthalocyanine.

[0087] Examples of other additives include mica, aluminum powder, antioxidants, ultraviolet absorbers, light stabilizers, antistatic agents, flame retardants, dispersants, etc. Examples of crosslinking agents that can be used include known crosslinking agents such as isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and metal chelate-based crosslinking agents.

[0088] [Physical properties of the black layer] Considering the brittleness of the black layer 14, the thickness of the black layer 14 is preferably 30 μm or less, more preferably 1 to 15 μm, and even more preferably 1 μm or more and less than 5 μm. By making the thickness of the black layer 14 1 μm or more and less than 5 μm, the time from irradiation with the laser L until the white layer 13 is exposed can be reduced, improving the printing efficiency on the laser marker label.

[0089] [Manufacturing method of black layer] The black layer 14 is formed, for example, by dispersing a dispersion liquid (hereinafter referred to as a dispersion liquid for forming a black layer) in a solvent containing a black colorant, a resin, an additive, etc., and applying the dispersion liquid to the white layer 13 through film formation or printing using a solvent casting method, a T-die method, or the like.

[0090] When the black layer 14 is formed by printing, the layer thickness can be made thinner than when it is formed by film formation such as the solvent casting method or the T-die method. Therefore, the black layer 14 is also damaged when the white layer 13 is damaged, and the irradiation time of the laser L can be relatively shortened. Therefore, the printing efficiency on the laser marker label 10 is improved. In addition, when the black layer 14 is formed by printing, the variation in thickness of the black layer 14 is reduced compared to the black layer formed by film formation. Therefore, by removing the black layer 14 to the desired depth, the white layer 13 can be more reliably exposed. Therefore, in one embodiment of the present invention, the black layer is preferably a black printed layer.

[0091] When the black layer is formed by printing, examples of the printing method include screen printing, flexographic printing, gravure printing, etc. In any case, the surface of the white layer 13 on which the black layer 14 is to be formed may be subjected to a corona discharge treatment or coated with an anchor agent in advance in order to improve the adhesion of the ink.

[0092] Examples of the solvent used in the production of the black layer include those exemplified in the section [Production method of the white layer] above.

[0093] The amount of solvent used in printing may be appropriately set taking into consideration the thickness and final viscosity.

[0094] <Laser marker label manufacturing method> The manufacturing method of the laser marker label 10 according to this embodiment is not particularly limited, but may be, for example, a method in which a laminate (laminate A) of a white layer 13 and a black layer 14, and a laminate (laminate B) of a release liner 11 and an adhesive layer 12 are prepared, and the white layer 13 surface of the laminate A and the adhesive layer 12 surface of the laminate B are bonded together. The laminate A is obtained by forming the white layer 13 on a processing film, forming the black layer 14 on the white layer 13, and removing the processing film. The laminate B is obtained by applying an adhesive to the release liner 11 to form the adhesive layer 12 on the release liner 11. The processing film may be removed after the laminate A and the laminate B are bonded together.

[0095] Alternatively, the laser marker label 10 may be produced by forming the adhesive layer 12, the white layer 13 and the black layer 14 in this order on the release liner 11.

[0096] The method for forming each layer is as described above, and therefore the description thereof will be omitted.

[0097] <How to use laser marker labels> By irradiating a laser L onto the laser marker label 10 according to this embodiment, desired information can be printed.

[0098] 1(B) and (C), a laser L is irradiated from the black layer 14 side of the laser marker label 10 to form an exposed portion 15. This allows the desired information (e.g., a vehicle identification number) to be visually recognized due to the contrast between the black layer 14 and the white layer 13.

[0099] Examples of the laser L include a CO2 laser, a Nd:YAG laser, an excimer laser, a semiconductor laser, a semiconductor-pumped solid-state laser, an Ar laser, a N2 / Dye laser, and a HeCd laser. In general, it is preferable to use a CO2 laser or a Nd:YAG laser, which require inexpensive equipment and are relatively easy to handle. The irradiation conditions of the laser L may be appropriately set so that the laser penetrates the black layer 14 but does not penetrate the white layer 13.

[0100] Fig. 2 is a top view of the laser marker label of Fig. 1(C). In Fig. 2, the exposed portion 15 shows the numbers "12345", but may be in the form of any characters, symbols, figures, etc., and may also be information such as product information, manufacturing date, manufacturing location, etc.

[0101] The laser marker label on which information is printed in this manner has excellent print identification both after exposure to a high-temperature, high-humidity environment and after exposure to an outdoor environment, and can therefore be suitably used as a label attached to a moving object that is placed in a high-temperature, high-humidity environment or outdoors. Examples of moving objects include, but are not limited to, automobiles, aircraft, ships, and the like. Examples of automobiles include four-wheeled automobiles (passenger cars, trucks, buses, and the like), two-wheeled motorcycles, bulldozers, excavators, truck cranes, forklifts, and the like. Examples of ships include motorboats, and the like. Therefore, the laser marker label according to the embodiment of the present invention can be suitably used as a label that displays, for example, the identification number of a moving object (for example, the vehicle identification number of an automobile, or the hull identification number of a ship). EXAMPLES

[0102] The effects of the present invention will be described using the following examples and comparative examples. In the examples, the terms "parts" and "%" may be used, but unless otherwise specified, they represent "parts by mass" or "% by mass". Furthermore, unless otherwise specified, each operation is carried out at room temperature (25°C).

[0103] <Laser marker label production> [Example 1] (1) Synthesis of polymer X In a reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen gas inlet tube, 100 parts of polycarbonate diol (Nipporan (registered trademark) 981 manufactured by Tosoh Corporation, hydroxyl value 107 to 117 mg KOH / g), 23 parts by mass of a diisocyanate compound (manufactured by Tosoh Corporation, trade name "Coronate (registered trademark) HL", 150 parts of toluene, and 0.02 parts by mass of a tin-based catalyst were charged, and reacted at 80 ° C. under a nitrogen atmosphere for 6 hours or more to synthesize a urethane prepolymer having isocyanate groups at both ends (hereinafter, urethane prepolymer precursor). When the isocyanate group concentration in the system reached the theoretical amount, 2 parts of 2-hydroxyethyl methacrylate and 30 parts of toluene were added, and the mixture was further reacted at 80 ° C. for 6 hours until the isocyanate group of the urethane prepolymer precursor disappeared, and a solution of a urethane prepolymer having methacryloyl groups at both ends (hereinafter, urethane prepolymer) was obtained. The weight average molecular weight of the urethane prepolymer was 34,000. The weight average molecular weight is a value calculated in terms of polystyrene measured by gel permeation chromatography (GPC).

[0104] Next, 145 parts of methyl methacrylate, 6 parts of 2-hydroxyethyl methacrylate, 1.4 parts of thioglycerol, and 65 parts of toluene were added to this urethane prepolymer solution, and the temperature was raised to 105°C while stirring. A mixed liquid consisting of 2.7 parts of 2,2'-azobis(2-methylbutyronitrile) and 260 parts of toluene was added dropwise thereto over a period of 4 hours. After the completion of the dropwise addition, the mixture was reacted at the same temperature for 6 hours to obtain a polymer X solution. The polymer X had a viscosity of 4000 mPa·s (25°C) and a weight average molecular weight of 84,000. The weight average molecular weight was a value calculated in terms of polystyrene measured by gel permeation chromatography (GPC).

[0105] (2) Preparation of dispersion for forming white layer As a dispersion for forming a white layer, 100 parts by mass (solid content) of the polymer X solution synthesized above, 30 parts by mass of titanium oxide (Typique CR-57, manufactured by Ishihara Sangyo Kaisha, Ltd., average particle size 0.25 μm) and a solvent were mixed, and thoroughly stirred to disperse and dissolve, thereby preparing a dispersion with a solid content concentration of 35% by mass.

[0106] (3) Preparation of Laminate A The dispersion obtained in (2) above was cast onto a peelable casting film, and heated and dried at 150°C to form a white layer with a thickness of 75 μm. Next, black ink (manufactured by T&K TOKA Corporation, product name "UV Flexo Ink 500") was printed on the white layer as a dispersion for forming a black layer by flexographic printing, and cured with ultraviolet light to form a black layer with a thickness of 3 μm. The casting film was then peeled off to produce a laminate A consisting of a white layer and a black layer.

[0107] (4) Preparation of adhesive layer A reaction apparatus equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen gas inlet tube was charged with 90 parts by mass of butyl acrylate monomer and 10 parts by mass of acrylic acid monomer, and 0.3 parts by mass of azobisisobutyronitrile was added. Polymerization was carried out for 8 hours at 80°C under a nitrogen gas atmosphere, thereby obtaining an acrylic polymer solution having a weight average molecular weight of 500,000.

[0108] To 100 parts by mass of the solid content of this acrylic polymer solution, 2 parts by mass of an isocyanate crosslinking agent (Coronate (registered trademark) L manufactured by Tosoh Corporation) was added in terms of solid content, and the solution was further diluted with toluene to prepare a pressure-sensitive adhesive solution.

[0109] The adhesive solution was applied to the release-treated surface of a release liner using a knife coater and dried at 80° C. for 1 minute to form a laminate B consisting of a release liner and an adhesive layer (thickness 20 μm).

[0110] Next, the adhesive layer surface of the laminate B was attached to the white layer surface of the laminate A to prepare a laser marker label.

[0111] [Example 2] A laser marker label was prepared in the same manner as in Example 1, except that 5 parts by mass of an isocyanate-based crosslinking agent [Coronate (registered trademark) HL, manufactured by Tosoh Corporation] was further added to prepare a dispersion liquid for forming a white layer.

[0112] [Comparative Example 1] A laser marker label was produced in the same manner as in Example 1, except that in Example 1, 100 parts by mass of polyester-based polyurethane resin was used instead of 100 parts by mass of Polymer X to prepare a white layer-forming dispersion liquid.

[0113] [Comparative Example 2] A laser marker label was produced in the same manner as in Example 1, except that in Example 1, 100 parts by mass of an acrylic resin (a mixture of 60 parts by mass of a methyl methacrylate / methyl acrylate copolymer [manufactured by Mitsubishi Rayon Co., Ltd., "ACRYPET (registered trademark) MD"] and 40 parts by mass of a methyl methacrylate / styrene / butyl acrylate copolymer [manufactured by Mitsubishi Rayon Co., Ltd., "ACRYPET (registered trademark) RF065"]) was used instead of 100 parts by mass of Polymer X to prepare a white layer-forming dispersion liquid.

[0114] [Comparative Example 3] A laser marker label was produced in the same manner as in Example 1, except that a white layer-forming dispersion was prepared using 50 parts by mass of polyester-based polyurethane resin and 50 parts by mass of acrylic resin (a mixture of 60 parts by mass of methyl methacrylate / methyl acrylate copolymer [manufactured by Mitsubishi Rayon Co., Ltd., "ACRYPET (registered trademark) MD"] and 40 parts by mass of methyl methacrylate / styrene / butyl acrylate copolymer [manufactured by Mitsubishi Rayon Co., Ltd., "ACRYPET (registered trademark) RF065"]) instead of 100 parts by mass of Polymer X in Example 1.

[0115] <Performance evaluation of laser marker labels> [Printing Identification (Initial)] The laser-marked labels of the examples and comparative examples were irradiated with a Panasonic CO2 laser marker LP-400 so that the laser penetrated the black layer and reached the white layer to mark characters. The identifiability of the printed characters was visually observed.

[0116] ○: The printed characters were visible ×: The printed characters were not visible.

[0117] [Print distinguishability (after exposure to high temperature and high humidity environment)] Characters were marked on the laser marker labels of the examples and comparative examples by the method described above in [Printing identifiability]. Next, the release liner was removed from the laser marker label, and the adhesive layer surface was attached to a glass substrate, and then stored in a high temperature and high humidity environment (70°C, 90% RH) for 30 days. After storage, the identifiability of the characters printed on the label was visually observed and evaluated according to the following evaluation criteria (good or better was considered to be pass).

[0118] ◎: Characters were extremely easy to distinguish ○: Characters were easily distinguishable △: There are some problems with the legibility of characters, but this does not pose a problem in practical use. ×: Swelling occurred to the extent that it was difficult to distinguish characters.

[0119] [Print distinguishability (after exposure to outdoor environment)] Characters were marked on the laser marker labels of the examples and comparative examples by the method described above in [Printing identifiability]. Next, the release liner was removed from the laser marker label, and the adhesive layer surface was attached to a glass substrate. After 24 hours, an accelerated weather resistance test was performed. The accelerated weather resistance test was performed using a xenon weather meter at an illuminance of 60 W / m 2 The laser was irradiated for 2000 hours under the conditions of a black panel temperature of 63°C and a humidity of 40 to 60% RH. After the weather resistance test, the legibility of the characters printed on the laser marker label was visually observed and evaluated according to the following evaluation criteria (above was considered to be a pass).

[0120] ◎: Characters were extremely easy to distinguish ○: Characters were easily distinguishable △: There are some problems with the legibility of characters, but this does not pose a problem in practical use. ×: Cracks were generated to the extent that it was difficult to distinguish the characters.

[0121] [Table 1]

[0122] As shown in Table 1, it was found that the laser marker labels of the examples had superior print identification properties both after exposure to a high temperature and high humidity environment and after exposure to an outdoor environment, compared to the laser marker labels of the comparative examples.

[0123] The above describes the laser marker label of the present invention through embodiments, but the present invention is not limited to the configurations described in the embodiments and can be modified as appropriate based on the description of the claims. [Explanation of symbols]

[0124] 10 Laser Marker Labels, 11 release liner, 12 adhesive layer, 13 white layer, 14 Black layer, 15 Exposed parts.

Claims

1. A laser marker label having a black layer disposed on a surface layer onto which a laser is irradiated, and a white layer disposed adjacent to the black layer and below the black layer, a resin constituting the white layer and a resin constituting the black layer each contain an acrylic urethane copolymer, A laser marker label, in which the acrylic urethane copolymer is a polymer obtained by polymerizing a urethane prepolymer having ethylenically unsaturated groups at both ends with a (meth)acrylic acid ester including a (meth)acrylic acid ester having a hydroxyl group, and further crosslinking the polymer with a crosslinking agent capable of crosslinking with the hydroxyl group.

2. 2. The laser marker label according to claim 1, wherein the white layer has a thickness of 50 μm or more.

3. 3. The laser marker label according to claim 1, wherein the crosslinking agent is an isocyanate-based crosslinking agent.

Citation Information

Patent Citations

  • Adhesive sheet and decorative adhesive sheet

    JP2006002143A

  • Laser marking label and article with label

    JP2008090063A

  • Laser marking label

    JP2009034905A

  • Alteration prevention label

    JP2011020374A

  • Method of manufacturing brittle laser marker label

    JP2017111344A