Temporary Fixation Adhesive Sheet

A temporarily fixed adhesive sheet with a recessed pressure-sensitive adhesive layer facilitates solvent-assisted peeling, addressing the need for quick and damage-free removal in manufacturing processes.

JP7564625B2Active Publication Date: 2024-10-09LINTEC CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020015271
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-31
Publication Date
2024-10-09
Estimated Expiration
2040-01-31

AI Technical Summary

Technical Problem

Existing adhesive sheets used in manufacturing processes, such as those for semiconductor devices, require improved methods for easy and quick peeling without applying excessive force, to prevent contamination, deformation, and damage to adherends.

Method used

A temporarily fixed adhesive sheet with a pressure-sensitive adhesive layer featuring recesses on at least one surface, allowing for solvent contact releasability, enabling easy peeling by immersion in solvents like organic solvents or water within 25 minutes.

Benefits of technology

The adhesive sheet can be easily peeled off from adherends upon contact with solvents, reducing peeling time and minimizing damage to the adherend, thus enhancing productivity and workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564625000003
    Figure 0007564625000003
  • Figure 0007564625000004
    Figure 0007564625000004
  • Figure 0007564625000005
    Figure 0007564625000005
Patent Text Reader

Abstract

To provide a temporarily fixing pressure-sensitive adhesive sheet easily peelable from an adherend through contact with a solvent.SOLUTION: A temporarily fixing pressure-sensitive adhesive sheet 10 has an adhesive layer (X)2 in which recesses 1 having a difference of elevation of 0.5 μm or more are present on at least one surface, and a solvent contact peelability. In the temporarily fixing pressure-sensitive adhesive sheet 10, the recesses 1 continuously connected from one site of an outline of the surface of the adhesive layer (X)2 to the other site are present. In the temporarily fixing pressure sensitive adhesive sheet 10, an adhesive force of the surface on which the recesses 1 of the adhesive layer (X)2 are present is 0.01-12.00 N / 25 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a temporary fixing pressure-sensitive adhesive sheet, more specifically to a temporary fixing pressure-sensitive adhesive sheet that exhibits self-releasability upon contact with a solvent. [Background technology]

[0002] Adhesive sheets are not only used to semi-permanently fix components, but may also be used to temporarily fix components such as building materials, interior materials, and electronic components when processing or inspecting them. As an example, in the manufacturing process of a semiconductor device, when processing a semiconductor wafer or using materials for electronic devices such as semiconductor chips, a pressure-sensitive adhesive sheet is used as a temporary fixing sheet. In this way, when the pressure-sensitive adhesive sheet is attached to an adherend such as an electronic device material and then peeled off after use, it is desirable to be able to do so without applying an excessive load to the adherend. Similarly, the pressure-sensitive adhesive sheet can also be used as, for example, a protective material such as a protective film, wallpaper, various label applications, etc. If it becomes possible to peel the pressure-sensitive adhesive sheet attached to the adherend from the adherend without applying a load to the adherend, it is expected that defects such as contamination, deformation, and breakage of the adherend caused by the pressure-sensitive adhesive sheet can be reduced and prevented. In this way, when a pressure-sensitive adhesive sheet is used by temporarily attaching it to an adherend, the pressure-sensitive adhesive sheet is required to exhibit sufficient adhesive strength when attached and to have excellent releasability when removed. As described above, in this specification, pressure-sensitive adhesive sheets that are used not only for semi-permanent fixing of various components to which the pressure-sensitive adhesive sheet is attached, but also for temporary fixing, are also referred to as "temporary fixing pressure-sensitive adhesive sheets."

[0003] For example, Patent Document 1 discloses a temporary fixing adhesive composition that contains a (meth)acrylate and an alicyclic (meth)acrylate, each of which has a homopolymer glass transition temperature that falls within a specific range, and a photopolymerization initiator; and a method for temporarily fixing a member, which comprises using the temporary fixing adhesive composition to temporarily fix a member, immersing the processed member in an organic solvent, and removing the cured body of the composition. Furthermore, for example, Patent Document 2 discloses a processing method for brittle materials that includes a step of forming a unit in which a brittle material is fixed to a hard plate via a double-sided adhesive sheet having adhesive layers on both sides, and peeling the brittle material from the hard plate, characterized in that the unit is immersed in a liquid that is insoluble or poorly soluble in the adhesive, allowing the liquid to penetrate into the interface between the double-sided adhesive sheet and the brittle material, or the interface between the double-sided adhesive sheet and the hard plate, and then peeling the brittle material from an end of the unit. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-108044 A [Patent Document 2] JP 2003-338475 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in recent years, when adhesive sheets such as those disclosed in Patent Documents 1 and 2 are used in the manufacturing processes of various products, there has been a demand, from the standpoint of improving productivity, for shortening the time required for the adhesive sheet to be peeled off from the adherend after being immersed in a solvent or the like. Furthermore, even in the case of pressure-sensitive adhesive sheets used in processes other than the production process as described above, there is a demand for shortening the peeling process time from the viewpoint of improving workability during peeling. From this perspective, an object of the present invention is to provide a temporary fixing pressure-sensitive adhesive sheet that can be easily peeled off from an adherend by contacting it with a solvent. [Means for solving the problem]

[0006] The present inventors have found that a temporary fixing pressure-sensitive adhesive sheet having a specific pressure-sensitive adhesive layer (X) having recesses on at least one surface thereof can solve the above problems, and have completed the present invention. That is, the present invention provides the following [1] to [9]. [1] A temporary fixing pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer (X) having recesses on at least one surface, and having solvent contact releasability. [2] The temporary fixing pressure-sensitive adhesive sheet according to [1], wherein the height difference of the recesses is 0.5 μm or more. [3] The temporary fixing pressure-sensitive adhesive sheet according to [1] or [2], wherein when the pressure-sensitive adhesive layer (X) is viewed in a plane, the recesses are present and are continuously connected from one point to another point on the contour of the surface of the pressure-sensitive adhesive layer (X). [4] The temporary fixing pressure-sensitive adhesive sheet according to any one of [1] to [3] above, wherein the adhesive strength of the surface of the pressure-sensitive adhesive layer (X) on which the recesses are present before the pressure-sensitive adhesive layer (X) is 0.01 to 12.00 N / 25 mm before the pressure-sensitive adhesive layer (X) is immersed in a solvent. [5] The temporary fixing pressure-sensitive adhesive sheet according to any one of the above [1] to [4], wherein the pressure-sensitive adhesive layer (X) is formed from an acrylic pressure-sensitive adhesive composition. [6] The temporary fixing pressure-sensitive adhesive sheet according to any one of the above [1] to [5], which has a substrate. [7] The temporary fixing pressure-sensitive adhesive sheet according to any one of the above [1] to [6], which is used for temporarily fixing a material for an electronic device to a support. [8] The temporary fixing pressure-sensitive adhesive sheet according to [7], wherein the material for an electronic device is a wafer for an electronic device. [9] The temporary fixing pressure-sensitive adhesive sheet according to any one of the above [1] to [8], which is used in processing and / or inspecting materials for electronic devices. Effect of the Invention

[0007] According to the present invention, it is possible to provide a temporary fixing pressure-sensitive adhesive sheet that can be easily peeled off from an adherend by contacting it with a solvent. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view showing one example of the configuration of the temporary fixing pressure-sensitive adhesive sheet of the present invention, taken along a plane that allows the depressions present on the surface of the pressure-sensitive adhesive layer (X) to be discerned. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing one example of the configuration of the temporary fixing pressure-sensitive adhesive sheet of the present invention, taken along a plane that allows the depressions present on the surface of the pressure-sensitive adhesive layer (X) to be discerned. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing one example of the configuration of the temporary fixing pressure-sensitive adhesive sheet of the present invention, taken along a plane that allows the depressions present on the surface of the pressure-sensitive adhesive layer (X) to be discerned. [Figure 4] FIG. 2 is a schematic cross-sectional view showing one example of the configuration of the temporary fixing pressure-sensitive adhesive sheet of the present invention, taken along a plane that allows the depressions present on the surface of the pressure-sensitive adhesive layer (X) to be discerned. [Diagram 5] This is a schematic cross-sectional view of a sample for evaluating the solvent (organic solvent or water) contact peelability of a temporary fixing pressure-sensitive adhesive sheet in an embodiment, which is a schematic cross-sectional view cut at a plane that allows the depressions present on the surface of the pressure-sensitive adhesive layer (X) to be identified. [Figure 6] 1 is a plan view schematic diagram illustrating an example of the temporary fixing pressure-sensitive adhesive sheet of the present invention. [Figure 7] 1 is a plan view schematic diagram illustrating an example of the temporary fixing pressure-sensitive adhesive sheet of the present invention. [Figure 8] This is a schematic cross-sectional view showing an example of the configuration of a release material that may be possessed by the temporary fixing adhesive sheet of the present invention, and is a schematic cross-sectional view of a release material cut on a plane such that the convex portions present on the surface of the release material can be identified. [Figure 9] 1 is an example of a scanning electron microscope (SEM) image when checking the height difference and width of recesses of the temporary fixing pressure-sensitive adhesive sheet produced in Example 1, which is an example of this embodiment. [Figure 10] This is an example of a scanning electron microscope (SEM) image when confirming the height difference and width of the convex portions of the release material 1 used in producing the temporary fixing adhesive sheets produced in Examples 1 and 13, which are examples of this embodiment. [Figure 11]1 is an example of a scanning electron microscope (SEM) image when confirming the pattern shape of recesses of the temporary fixing pressure-sensitive adhesive sheet produced in Example 1, which is an example of this embodiment. [Figure 12] FIG. 1 is an example of a scanning electron microscope (SEM) image for confirming the pattern shape of the convex portions of the release material 1 used in producing the temporary fixing adhesive sheets produced in Examples 1 and 13, which are examples of this embodiment. [Figure 13] 1 is an example of a scanning electron microscope (SEM) image when checking the height difference and width of the recesses of the temporary fixing pressure-sensitive adhesive sheet produced in Example 13, which is an example of this embodiment. [Figure 14] 1 is an example of a scanning electron microscope (SEM) image when confirming the pattern shape of the recesses of the temporary fixing pressure-sensitive adhesive sheet produced in Example 13, which is an example of this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Temporary fixing adhesive sheet] The temporary fixing pressure-sensitive adhesive sheet of the present invention has a pressure-sensitive adhesive layer (X) having recesses on at least one surface, and has solvent contact releasability. In this specification, the self-peeling that occurs when a temporary fixing adhesive sheet (hereinafter also simply referred to as "adhesive sheet") comes into contact with a solvent is referred to as "solvent contact peeling," and such a property is referred to as "solvent contact releasability." In one embodiment of the present invention, whether or not a pressure-sensitive adhesive sheet has "solvent contact releasability" is determined, for example, by judging whether or not the temporary fixing pressure-sensitive adhesive sheet is capable of self-peeling from the adherend in less than 25 minutes when the pressure-sensitive adhesive layer (X) of the pressure-sensitive adhesive sheet is immersed in a solvent at 25°C when peeling from the adherend, and if the temporary fixing pressure-sensitive adhesive sheet self-peels from the adherend in less than 25 minutes, the pressure-sensitive adhesive sheet is deemed to have "solvent contact releasability". In this specification, the term "self-peeling" refers to the state in which the adhesive sheet is peeled off or falls off from the adherend without the application of a force to pull the adhesive sheet off, and such a property is referred to as "self-peeling properties." In one embodiment of the present invention, for example, when the PSA sheet has "organic solvent contact releasability" or "water contact releasability" as described below, the PSA sheet is considered to have "solvent contact releasability".

[0010] The "solvent" can be appropriately selected depending on the application of the pressure-sensitive adhesive sheet, and examples thereof include organic solvents and water.

[0011] Here, the "organic solvent" can be appropriately selected depending on the application of the pressure-sensitive adhesive sheet, and for example, methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, isopropanol, etc. can be preferably used. Among these, one or more selected from the group consisting of methyl ethyl ketone, methyl isobutyl ketone, toluene, and ethyl acetate can be more preferably used. In addition, in this specification, the "solvent contact releasability" that is exhibited by the pressure-sensitive adhesive sheet due to contact with an organic solvent is referred to as "organic solvent contact releasability". In one embodiment of the present invention, whether or not a pressure-sensitive adhesive sheet has "organic solvent contact releasability" is determined, for example, by judging whether or not the temporary fixing pressure-sensitive adhesive sheet is capable of self-peeling from the adherend in less than 25 minutes when the pressure-sensitive adhesive layer (X) of the pressure-sensitive adhesive sheet is immersed in the organic solvent at 25°C when peeling from the adherend, and if the temporary fixing pressure-sensitive adhesive sheet self-peels from the adherend in less than 25 minutes, the pressure-sensitive adhesive sheet is deemed to have "organic solvent contact releasability". In one embodiment of the present invention, whether or not a pressure-sensitive adhesive sheet has "organic solvent contact releasability" is determined, for example, by judging whether or not the temporary fixing pressure-sensitive adhesive sheet is capable of self-peeling from the adherend in less than 25 minutes when the pressure-sensitive adhesive layer (X) of the pressure-sensitive adhesive sheet is immersed in methyl ethyl ketone at 25°C when peeling from the adherend, and if the temporary fixing pressure-sensitive adhesive sheet self-peels from the adherend in less than 25 minutes, the pressure-sensitive adhesive sheet is deemed to have "organic solvent contact releasability". In one embodiment of the present invention, for example, a more specific method for determining whether or not a pressure-sensitive adhesive sheet has "organic solvent contact releasability" is, for example, evaluation of organic solvent contact releasability by the method described in the Examples. Here, in an embodiment in which the pressure-sensitive adhesive sheet to be evaluated is a double-sided pressure-sensitive adhesive sheet, one pressure-sensitive adhesive layer having organic solvent contact releasability and the other pressure-sensitive adhesive layer having no organic solvent contact releasability, if the layer having organic solvent contact releasability self-detaches from the adherend by the above-mentioned evaluation, the pressure-sensitive adhesive sheet can be determined to have organic solvent contact releasability.

[0012] The "water" also includes the form of an "aqueous solution" in which a liquid or solid other than water is dissolved, so long as the effects of the present application are achieved. The "water" can be appropriately selected depending on the application of the pressure-sensitive adhesive sheet, and preferably includes tap water, pure water such as ion-exchanged water, RO water, and distilled water, and ultrapure water, and more preferably includes one or more selected from the group consisting of pure water and ultrapure water. In this specification, the self-peeling that occurs when the pressure-sensitive adhesive sheet comes into contact with water is referred to as "peeling upon contact with water," and such a property is referred to as "peeling properties upon contact with water." In one embodiment of the present invention, whether or not a pressure-sensitive adhesive sheet has "water-contact releasability" is determined, for example, by judging whether or not the temporary-fixing pressure-sensitive adhesive sheet is capable of self-peeling from the adherend in less than 25 minutes when the pressure-sensitive adhesive layer (X) of the pressure-sensitive adhesive sheet is immersed in the water at 25°C when peeling from the adherend, and if the temporary-fixing pressure-sensitive adhesive sheet self-peels from the adherend in less than 25 minutes, the pressure-sensitive adhesive sheet is deemed to have "water-contact releasability". Furthermore, in one embodiment of the present invention, whether or not an adhesive sheet has "water contact releasability" is determined, for example, by judging whether or not the temporary fixing adhesive sheet is capable of self-peeling from the adherend in less than 25 minutes when the surface having the recesses of the adhesive layer (X) of the adhesive sheet is attached to an adherend having a smooth surface and then the adhesive layer (X) is immersed in pure water at 25°C when peeling from the adherend, and if the temporary fixing adhesive sheet self-peels from the adherend in less than 25 minutes, the adhesive sheet is deemed to have "water contact releasability". In one embodiment of the present invention, a more specific method for determining whether or not a PSA sheet has "water contact releasability" is, for example, evaluating water contact releasability by the method described in the Examples. Here, in an embodiment in which the PSA sheet to be evaluated is a double-sided PSA sheet, one PSA layer has water contact releasability and the other PSA layer does not have water contact releasability, if the layer having water contact releasability self-detaches from the adherend according to the above-mentioned evaluation, the PSA sheet can be determined to have water contact releasability.

[0013] Furthermore, the term "adherend having a smooth surface" merely defines an adherend used when determining whether or not the pressure-sensitive adhesive sheet has solvent contact releasability, and does not define an adherend to which the temporary fixing pressure-sensitive adhesive sheet of the present invention is attached. Furthermore, the "adherend having a smooth surface" is not a part that constitutes the temporary fixing pressure-sensitive adhesive sheet of the present invention. Furthermore, the adherend to which the temporary fixing pressure-sensitive adhesive sheet of the present invention is attached is not particularly limited as to whether it has a smooth surface or not, and may be, for example, a light-transmitting adherend having a curved surface. The "smooth surface" of the "adherend having a smooth surface" is defined as the center line average roughness (Ra 75 The material of the adherend is not particularly limited, but glass is preferred from the viewpoints that it is easy to obtain an adherend having the above-specified smooth surface and that the interface with the pressure-sensitive adhesive layer can be easily observed with the naked eye or with a digital microscope.

[0014] In addition, in this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum, and examples thereof include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated by using, for example, an electrodeless lamp, a high-pressure mercury lamp, a metal halide lamp, a UV-LED, or the like as an ultraviolet ray source. Electron beams can be irradiated by generating them using an electron beam accelerator, or the like. Among these, ultraviolet rays can be preferably used.

[0015] When the pressure-sensitive adhesive layer (X) used in the present invention (hereinafter also simply referred to as "layer (X)") comes into contact with a solvent, it is believed that self-peeling occurs due to a combined effect of: the effect of the solvent penetrating into the interface between layer (X) and the adherend due to the affinity between layer (X) and the solvent; and the effect of layer (X) itself taking up the solvent and swelling, which causes the solvent to penetrate into the interface between layer (X) and the adherend. Since the layer (X) used in the present invention has the recesses, the solvent penetrates along the recesses, and when the pressure-sensitive adhesive sheet is viewed in plan, the solvent can easily penetrate into the interface between the layer (X) and the adherend not only from the outer edge of the pressure-sensitive adhesive sheet but also from the location where the recesses are present. In addition, the penetration of the solvent from the recesses also shortens the time it takes for the layer (X) to swell with the solvent. As a result, the time it takes for the solvent to penetrate into the interface between the layer (X) and the adherend to the extent that the pressure-sensitive adhesive sheet can be self-peeled from the adherend is significantly shortened, and it is considered that the solvent contact peelability is significantly improved. From this viewpoint, the method of contacting the layer (X) with the solvent is preferably to immerse the layer (X) in the solvent so that the interface between the layer (X) and the adherend is located below the liquid level of the solvent, more preferably to immerse the layer (X) in the solvent so that at least the recesses located on the outer periphery of the layer (X) when viewed in a plan view are immersed in the solvent, and further preferably to immerse the layer (X) in the solvent so that the entire layer (X) is immersed in the solvent.

[0016] The temperature of the solvent is not particularly limited as long as it does not impair the effects of the present invention, but is preferably more than 0° C. and less than 100° C., more preferably 4° C. or more and less than 50° C., and even more preferably 5° C. or more and 40° C. or less. The pressure-sensitive adhesive sheet according to one embodiment of the present invention can achieve sufficient effects even when treated with a solvent at room temperature (25° C.). That is, even when the solvent that is brought into contact with the pressure-sensitive adhesive sheet is not subjected to treatment such as heating or cooling, the pressure-sensitive adhesive sheet can exhibit solvent contact releasability, and therefore the pressure-sensitive adhesive sheet is excellent in workability and economy when used (during the peeling treatment).

[0017] Furthermore, in a pressure-sensitive adhesive sheet which is one embodiment of the present invention, in a solvent (organic solvent or water) contact peelability evaluation performed by the method described in the Examples section below, the time required for the pressure-sensitive adhesive sheet to self-peel from an adherend when immersed in a solvent is preferably 20 minutes or less, more preferably 10 minutes or less, even more preferably 5 minutes or less, still more preferably 1 minute or less, and even more preferably less than 1 minute.

[0018] In addition, in this specification, the lower limit and the upper limit described in stages for the preferred numerical range (for example, the range of the content, etc.) can be combined independently. For example, from the description "preferably 10 or more, more preferably 30 or more, and preferably 90 or less, more preferably 60 or less", the "preferable lower limit (10)" and the "more preferable upper limit (60)" can be combined to make the preferred range "10 or more, 60 or less". Similarly, from the description "preferably 10 to 90, more preferably 30 to 60", it can be made "10 to 60". In addition, unless otherwise specified, when the preferred numerical range is simply described as "10 to 90", it represents a range of 10 to 90. In addition, in this specification, for example, "(meth)acrylic acid" refers to both "acrylic acid" and "methacrylic acid," "(meth)acrylate" refers to both "acrylate" and "methacrylate," "(meth)acryloyl group" refers to both "acryloyl group" and "methacryloyl group," and the same applies to other similar terms. In addition, in this specification, the "active ingredient" in the pressure-sensitive adhesive composition refers to, among the components contained in the pressure-sensitive adhesive composition, components that are liquid at room temperature (25°C) excluding solvents (water and organic solvents) that are not directly involved in the reaction, and components that are solid at room temperature (25°C).

[0019] An example of a pressure-sensitive adhesive sheet according to an embodiment of the present invention will be described below with reference to the accompanying drawings. However, the pressure-sensitive adhesive sheet of the present invention is not limited to the following example as long as the effects of the present invention are exhibited. Figures 1 to 4 are schematic cross-sectional views of adhesive sheets 10, 20, 30 and 40, respectively, showing an example of the configuration of the adhesive sheet of the present invention, and are schematic cross-sectional views of layer (X) 2, which has a recess 1 present on at least one surface, cut along a plane such that the recess 1 can be identified. For example, when adhesive sheet 70, which is one example of the configuration of the adhesive sheet of the present invention shown in the schematic plan view of FIG. 7, is cut along line AA, schematic cross-sectional views such as those shown in FIGS. 1 to 4 are obtained.

[0020] One embodiment of the pressure-sensitive adhesive sheet of the present invention is, for example, a pressure-sensitive adhesive sheet consisting of a single layer of layer (X) 2, such as pressure-sensitive adhesive sheet 10 shown in Fig. 1. In the case of the pressure-sensitive adhesive sheet shown in Fig. 1, an adherend to be peeled off when layer (X) 2 is brought into contact with a solvent can be attached to the surface on which recesses 1 exist. In addition, the pressure-sensitive adhesive sheet 10 shown in Fig. 1 may be a pressure-sensitive adhesive sheet in which recesses 1 exist on both surfaces of layer (X) 2 (not shown), or a release material may be provided on one exposed surface and both exposed surfaces of layer (X) 2 (not shown).

[0021] One embodiment of the pressure-sensitive adhesive sheet of the present invention includes a structure in which a base material 3 and a layer (X) 2 are laminated in this order, such as the pressure-sensitive adhesive sheet 20 shown in Fig. 2. Providing the layer (X) 2 on the base material 3 can improve the shape stability of the pressure-sensitive adhesive sheet and impart stiffness to the pressure-sensitive adhesive sheet, which is preferable from the viewpoint of improving the workability when removing the release material from the layer (X) 2 and when peeling the pressure-sensitive adhesive sheet from the adherend. In the adhesive sheet 20 shown in FIG. 2, the adhesive sheet may have a recess 1 on the surface side of the layer (X) 2 that contacts the substrate 3 (not shown), or the adhesive sheet may have a recess 1 on both the surface of the layer (X) 2 facing the substrate 3 and the surface opposite the substrate 3 (not shown), or a release material may be provided on the surface of the layer (X) 2 opposite the substrate 3 and / or the surface of the substrate 3 opposite the layer (X) 2 (not shown).

[0022] One embodiment of the pressure-sensitive adhesive sheet of the present invention is, for example, a double-sided pressure-sensitive adhesive sheet having a multilayer structure in which layers (X) 2 are laminated on both sides of a substrate 3, as in the pressure-sensitive adhesive sheet 30 shown in Fig. 3. In the pressure-sensitive adhesive sheet 30 shown in Fig. 3, the two layers (X) 2 may be the same layer (X) 2 or different layers (X) 2. Also, the pressure-sensitive adhesive sheet 30 shown in Fig. 3 may be a pressure-sensitive adhesive sheet in which a recess 1 is present on the surface of the layer (X) 2 that contacts the substrate 3 (not shown), or a pressure-sensitive adhesive sheet in which a recess 1 is present on both the surface of the layer (X) 2 on the substrate 3 side and the surface opposite to the substrate 3 (not shown). In addition, in the adhesive sheet 30 shown in FIG. 3, one of the two layers (X) 2 may be an adhesive layer other than the layer (X) 2 that does not have recesses 1 on its surface (not shown).

[0023] In addition, as one embodiment of the adhesive sheet of the present invention, for example, as in adhesive sheet 40 shown in FIG. 4, in adhesive sheet 30 shown in FIG. 3, release material 4-1 and release material 4-2 may be provided on the surface (exposed surface) of layer (X) 2 opposite to substrate 3. In FIG. 4, the release material 4-1 is a release material having a convex portion 4a that pairs with the concave portion 1 of the layer (X) 2, and the release material 4-2 is a release material having no convex portion. In the adhesive sheet 40 shown in FIG. 4, the release material 4-1 may be used for both of the release materials, or the release material 4-2 may be used for both of the release materials. However, from the viewpoint of easily maintaining the shape of the concave portion 1 on the layer (X) 2 during storage and / or transportation of the adhesive sheet 40, and also from the viewpoint of easily forming the concave portion 1 as described later in the manufacturing method of the adhesive sheet, which is one embodiment of the present invention, it is preferable to provide the release material 4-1 having the convex portion 4a that pairs with the concave portion 1 of the layer (X) 2 on the surface having the concave portion 1 of the layer (X) 2. The same applies when the release material 4 is provided in the adhesive sheets 10, 20, and 30 shown in FIG. 1 to FIG. 3.

[0024] Fig. 5 shows a schematic cross-sectional view of a sample 100 for evaluating the solvent (organic solvent or water) contact peelability of a pressure-sensitive adhesive sheet in an example of the present application. The pressure-sensitive adhesive sheet 50 shown in Fig. 5 is a double-sided pressure-sensitive adhesive sheet having a multilayer structure in which a pressure-sensitive adhesive layer (X) 2, a substrate 3, and a pressure-sensitive adhesive layer (Z) (hereinafter also simply referred to as "layer (Z)") 5 which is a pressure-sensitive adhesive layer other than the pressure-sensitive adhesive layer (X) are laminated in this order. In the adhesive sheet 50 shown in FIG. 5, the recess 1 of the layer (X) 2 does not come into contact with the adherend (glass plate) 101 even when it comes into contact with the adherend 101, and the solvent penetrates along the inside of the recess 1. Therefore, it is considered that the time for the solvent to penetrate into the interface between the layer (X) 2 and the adherend 101 and the time for the layer (X) 2 to swell with the solvent can be shortened, compared to, for example, layer (Z) 5 which does not have the recess 1.

[0025] In addition, in the pressure-sensitive adhesive sheet 20 shown in Fig. 2, the base material 3 and the layer (X) 2 may be directly laminated as shown in Fig. 2, or another layer may be interposed between the base material 3 and the layer (X) 2. Here, "directly laminated" refers to a configuration in which, for example, in the case of the pressure-sensitive adhesive sheet 20 shown in Fig. 2, the base material 3 and the layer (X) 2 are in direct contact with each other without there being another layer between them. In the pressure-sensitive adhesive sheets 30 and 40 shown in Figures 3 and 4, the base material 3 and the layer (X) 2 may be laminated directly to each other as three layers as shown in each figure, or another layer may be laminated between the base material 3 and either one of the layers (X) 2, or between the base material 3 and both layers (X) 2, via another layer. In addition, in the adhesive sheet 50 shown in FIG. 5, the layer (X) 2, the base material 3, and the layer (Z) 5 may be laminated directly as shown in FIG. 5, or another layer may be interposed between the layer (X) 2 and the base material 3, and / or between the base material 3 and the layer (Z) 5. Furthermore, for example, as shown in FIGS. 1 to 5, a portion where no recess 1 exists relative to the recess 1 of the layer (X) 2 may be referred to as a protrusion 2a of the layer (X) 2.

[0026] <Adhesive layer (X)> The pressure-sensitive adhesive layer (X) is a pressure-sensitive adhesive layer having recesses on at least one surface, and is preferably a layer formed from a pressure-sensitive adhesive composition containing a pressure-sensitive adhesive resin, and more preferably a layer formed from an acrylic pressure-sensitive adhesive composition. Examples of the adhesive resin include rubber-based resins such as polyisobutylene-based resins, acrylic-based resins, urethane-based resins, polyester-based resins, olefin-based resins, silicone-based resins, and polyvinyl ether-based resins. Of these, acrylic-based resins are preferred. Furthermore, when these adhesive resins are copolymers having two or more types of constitutional units, the copolymer may be in the form of any one of a block copolymer, a random copolymer, and a graft copolymer. These adhesive resins may be used alone or in combination of two or more kinds.

[0027] (recess) The "recesses" of the layer (X) refer to depressions that are intentionally provided so that the layer (X) does not come into contact with an adherend when the surface of the layer (X) having the recesses is attached to the adherend. The shape of the recesses when the layer (X) is viewed from above can be appropriately selected depending on the application of the pressure-sensitive adhesive sheet, and may be either regular or irregular. When the shape of the recess in the plan view of the layer (X) is a fixed shape, examples of the shape include polygons such as triangles, quadrilaterals (including rectangles, squares, and trapezoids), pentagons, and hexagons; shapes in which some or all of the corners of the polygon are slightly rounded (also referred to as "rounded corners (R)"); circles such as perfect circles and ellipses; semicircles such as semicircles, semiellipses, and U-shapes; and shapes represented by closed areas surrounded by at least three lines (including straight lines and curves), as well as one or more shapes selected from figures combining these (hereinafter also referred to as "independent recess shapes").

[0028] Furthermore, the shape of the recesses when the layer (X) is viewed in a plane is preferably such that the recesses are in contact with the contour of the surface of the layer (X) having the recesses, more preferably such that the recesses are continuously connected from any one point on the contour of the surface of the layer (X) having the recesses to other points (not limited to the contour, any point on the plane where the recesses of the layer (X) exist) (hereinafter also referred to as a "continuous recess shape"), further preferably such that the recesses are continuously connected from any one point on the contour of the surface of the layer (X) having the recesses to other points on the contour, and still further preferably such that the recesses are continuously connected from any one side of the surface of the layer (X) having the recesses to another side. When the recesses have a continuous recess shape, the solvent can more easily penetrate from the outer edge (contour) of the layer (X) toward the center when the layer (X) is viewed in a plane, which is preferable because it further improves the solvent contact peelability of the pressure-sensitive adhesive sheet.

[0029] For this reason, for example, when the layer (X) is viewed in a plane, it is preferable that at least a part of the continuous recesses is present on the line segment (including the center of gravity) on the center of gravity side when the shortest straight line (hereinafter also referred to as the "shortest distance to the center of gravity") connecting the center of gravity of a figure drawn by the contour of the surface having the recesses of the layer (X) is bisected, it is more preferable that at least a part of the continuous recesses is present on the line segment (including the center of gravity) closest to the center of gravity side when the shortest distance to the center of gravity is divided into thirds, and it is even more preferable that at least a part of the continuous recesses is present on the line segment (including the center of gravity) closest to the center of gravity side when the shortest distance to the center of gravity is divided into fifths. Furthermore, when the layer (X) is viewed in a plane, it is preferable that at least a part of the continuous recesses is present on the line segment (including the center of gravity) on the center of gravity side when the longest straight line (hereinafter also referred to as the "longest distance to the center of gravity") connecting the center of gravity of a figure drawn by the contour of the surface having the recesses of the layer (X) and any one point on the contour is divided into two equal parts; it is more preferable that at least a part of the continuous recesses is present on the line segment (including the center of gravity) closest to the center of gravity side when the longest distance to the center of gravity is divided into thirds; and it is even more preferable that at least a part of the continuous recesses is present on the line segment (including the center of gravity) closest to the center of gravity side when the longest distance to the center of gravity is divided into fifths.

[0030] Further, it is more preferable that the layer (X) has both continuous recesses at least a part of which is present at a preferred position on the shortest distance to the center of gravity, and continuous recesses at least a part of which is present at a preferred position on the longest distance to the center of gravity. In this case, the preferred position where the part of the continuous recesses is present on the shortest distance to the center of gravity and the preferred position where the part of the continuous recesses is present on the longest distance to the center of gravity can be combined independently. For example, the continuous recesses may have at least a part of the recesses present on the line segment (including the center of gravity) closest to the center of gravity when the shortest distance to the center of gravity is divided into two equal parts, and the continuous recesses may have at least a part of the recesses present on the line segment (including the center of gravity) closest to the center of gravity when the longest distance to the center of gravity is divided into five equal parts. Among them, it is more preferable to combine the above-mentioned recesses in the more preferable modes. That is, it is more preferable to combine the modes in which at least a part of the continuous recesses is present at a position closer to the center of gravity.

[0031] Examples of the continuous recess shape include linear shapes such as straight lines, curved lines, zigzags, and wavy lines connecting any one point on the surface of the layer (X) having recesses to one or more other points. Among these, a shape composed of straight lines is preferable, and examples of such shapes include striped and lattice-shaped recesses described below. On the layer (X), at least one selected from these continuous recess shapes can be arranged at a predetermined interval so as not to intersect, or to intersect with each other, to provide recesses in the form of, for example, striped shapes as shown in FIG. 6, lattice shapes as shown in FIG. 7, or other geometric patterns. In this case, a region 6 surrounded by recesses 1 may be formed, as in the lattice shape shown in FIG. 7, and examples of the shape of the region 6 include shapes similar to those described for the independent recess shapes described above. The region 6 is also the protrusion 2a. On the surface of the layer (X), a discontinuous shape may exist due to a part of the continuous recessed shape being missing, or a continuous recessed shape and an independent recessed shape may exist together. Each shape that can be taken by the recesses when the layer (X) is viewed in a plane may be present regularly or irregularly, but it is preferable that they are present regularly in a pattern as shown in Figure 6 or 7. In the case of a lattice pattern as shown in FIG. 7, identical recess shapes (straight lines) intersect with each other to form one recess, and since there are no discontinuous portions, the recess shapes can be regarded as a single recess shape.

[0032] In addition, the cross-sectional shape of the recess when the layer (X) is cut in the thickness direction may vary depending on the cut surface and cannot be generally specified, but examples thereof include polygons such as triangles, quadrilaterals (including rectangles, squares, and trapezoids), pentagons, and hexagons; shapes in which some or all of the corners of the polygons are slightly rounded (also referred to as "rounded corners (R)"); semicircular shapes such as semicircles, semiellipses, and U-shapes; and the like.

[0033] The height difference of the recesses is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 3.0 μm or more, and is preferably 50.0 μm or less, more preferably 30.0 μm or less, even more preferably 25.0 μm or less, and even more preferably 20.0 μm or less. The width of the recess is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 75.0 μm or less, still more preferably 50.0 μm or less, and still more preferably 35.0 μm or less. There is no particular lower limit to the width of the recess, but it is preferably 1.0 μm, more preferably 3.0 μm, and still more preferably 5.0 μm. The height difference and width of the recess are values ​​measured using the method described in the Examples. Regarding the values ​​described as the preferred ranges, for example, when "the height difference of the recess is 0.5 μm or more," it is sufficient that a portion having a height difference of 0.5 μm or more exists in any portion of the recess, and it is not necessary that the entire region of the recess has a height difference of 0.5 μm or more. Similarly, even if there are multiple recesses with different shapes on layer (X), it is sufficient that any of the recesses has a portion having a height difference of 0.5 μm or more, and it is not necessary that all of the recesses have a height difference of 0.5 μm or more. The height difference and width of the recess are values ​​measured using the method described in the Examples. For example, the distance 1h shown in FIG. 1 corresponds to the height difference of the recess. Also, the distance 1w shown in FIG. 1, FIG. 6, and FIG. 7 corresponds to the width of the recess. Note that, as an example, if we use the cross-sectional images of the recess shown in FIG. 9 and FIG. 13, which are images of a scanning electron microscope (SEM) taken using the method described in the Examples, the distance 1h in FIG. 9 and FIG. 13 corresponds to the height difference of the recess, and the distance 1w corresponds to the width of the recess.

[0034] The shape of the recesses can be formed, for example, by applying the pressure-sensitive adhesive composition onto a release material having protrusions that correspond to the recesses, as described below, and drying the composition to transfer the shape of the protrusions on the surface of the release material to the surface of layer (X).

[0035] When a plurality of recesses are present on the layer (X), the shapes of the plurality of recesses may be the same or different, and in that case, the height difference and width of the recesses may be independently the same or different.

[0036] The distance between the edges of the recesses is preferably 50.0 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, and even more preferably 200 μm or more. And, it is preferably 2,000 μm or less, more preferably 1,500 μm or less, and even more preferably 1,000 μm or less. For example, in the case of Figure 6 where there are multiple recesses, the distance between the edges of the recesses refers to the shortest distance between the edge of any one recess and the edge of the other recess that is closest to that recess, which refers to distance 7f in Figure 6. Furthermore, for example, in the case of the lattice-shaped recess shown in FIG. 7, the edge-to-edge distance of the recess refers to the shortest distance between the edge of any one side of the recess forming the lattice and the edge of the side opposite to that side, and refers to distance 7f in FIG. 7. The shortest pitch between the recesses is preferably 50.0 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, and even more preferably 200 μm or more, and is preferably 2,000 μm or less, more preferably 1,500 μm or less, and even more preferably 1,000 μm or less. For example, in the case of Figure 6 where there are multiple recesses, the shortest pitch of the recesses refers to the shortest distance from the midpoint of the shortest distance between the edges of any one recess to the midpoint of the shortest distance between the edges of another recess that is closest to the recess in question, and refers to distance 7p in Figure 6. Also, for example, in the case of the lattice-shaped recesses shown in Figure 7, the shortest pitch of the recesses refers to the shortest distance from the midpoint of the shortest distance between the edges of a recess portion forming one side of the lattice to the midpoint of the shortest distance between the edges of another recess portion forming a side opposite to the one side, and refers to distance 7p in Figure 7.

[0037] The adhesive strength of the surface of layer (X) on which the recesses are present is appropriately set depending on the application of the adhesive sheet, but is preferably 0.01 to 12.00 N / 25 mm, more preferably 0.05 to 6.00 N / 25 mm, and even more preferably 0.08 to 3.00 N / 25 mm, before layer (X) is immersed in a solvent. In this specification, the adhesive strength of the pressure-sensitive adhesive layer refers to the adhesive strength before the layer (X) is immersed in a solvent, and specifically refers to the value measured by the method described in the Examples.

[0038] The thickness of the layer (X) is preferably 5 to 150 μm, more preferably 8 to 100 μm, even more preferably 12 to 70 μm, and even more preferably 15 to 50 μm, although the thickness of the layer (X) is preferably thicker than the height difference of the recesses. When the thickness of the layer (X) is 5 μm or more, sufficient adhesive strength is easily obtained, and unintended peeling from the adherend during temporary fixing, displacement of the adherend, etc. are easily suppressed. On the other hand, when the thickness of the layer (X) is 150 μm or less, the adhesive sheet is easily handled.

[0039] (Acrylic adhesive composition) The pressure-sensitive adhesive composition that can be used in the pressure-sensitive adhesive sheet of one embodiment of the present invention is not particularly limited as long as it does not impair the effects of the present invention, but is preferably an acrylic pressure-sensitive adhesive composition containing an acrylic polymer (A) (hereinafter also referred to as "component (A)") and a crosslinking agent (B) (hereinafter also referred to as "component (B)").

[0040] When an organic solvent is used as the solvent, the acrylic pressure-sensitive adhesive composition is preferably an acrylic pressure-sensitive adhesive composition (R1) (hereinafter also referred to as "composition (R1)") containing an acrylic polymer (A1) (hereinafter also referred to as "component (A1)"), which is component (A), having a concentration of a group containing a carbon-carbon double bond exceeding 0 mmol / g, and a crosslinking agent (B1) (hereinafter also referred to as "component (B1)"), which is component (B), that crosslinks component (A1), and composition (R1) preferably further contains a photopolymerization initiator (C) (hereinafter also referred to as "component (C)"). Each component contained in the composition (R1) will be described below.

[0041] [Component (A1): Acrylic polymer (A1) having a concentration of groups containing carbon-carbon double bonds exceeding 0 mmol / g] Component (A1) is an acrylic polymer having a group containing a carbon-carbon double bond in the side chain. When the composition (R1) contains an acrylic polymer (A1) having a concentration of groups containing a carbon-carbon double bond exceeding 0 mmol / g, the organic solvent contact peelability of the resulting pressure-sensitive adhesive sheet is improved. This is believed to be because, when component (A1) has a group containing a carbon-carbon double bond, the interfacial adhesive strength at the interface between the layer (X) containing component (A1) and the adherend does not become too high, and the penetration of the organic solvent into the interface between the layer (X) and the adherend, which is caused by the penetration of the organic solvent from the outer edge or recesses of the pressure-sensitive adhesive sheet, easily proceeds sufficiently. On the other hand, when the concentration of the group containing a carbon-carbon double bond is 1.80 mmol / g or less, the swelling of the layer (X) due to the organic solvent is less likely to be suppressed, and the penetration of the organic solvent into the interface between the layer (X) and the adherend due to the swelling of the layer (X) due to the organic solvent proceeds sufficiently and is therefore preferable. From such a viewpoint, the concentration of the group containing the carbon-carbon double bond in component (A) is preferably 0.05 mmol / g or more, more preferably 0.10 mmol / g or more, even more preferably 0.20 mmol / g or more, and preferably 1.80 mmol / g or less, more preferably 1.50 mmol / g or less, even more preferably 1.30 mmol / g or less.

[0042] Examples of the group containing a carbon-carbon double bond include a (meth)acryloyl group, a vinyl group, and an allyl group, with a (meth)acryloyl group being preferred. Hereinafter, in this specification, a "group containing a carbon-carbon double bond" may also be simply referred to as a "carbon-carbon double bond group".

[0043] Component (A1) has a structural unit (a1) (hereinafter also referred to as "structural unit (a1)") derived from an alkyl (meth)acrylate (am1) (hereinafter also referred to as "monomer (am1)"). Component (A1) is preferably an acrylic polymer having a group containing a carbon-carbon double bond in the side chain, and more preferably an acrylic polymer that is a reaction product obtained by reacting an acrylic copolymer (P) having a structural unit (a1) and a structural unit (a2) (hereinafter also referred to as "structural unit (a2)") derived from a monomer (am2) (hereinafter also referred to as "monomer (am2)") containing a functional group, with a polymerizable compound (Q) having a carbon-carbon double bond group. The acrylic copolymer (P) can be produced by a known polymerization method such as bulk polymerization, solution polymerization, emulsion polymerization, etc. The acrylic copolymer (P) may be in the form of a block copolymer, a random copolymer, or a graft copolymer. In this specification, unless otherwise specified, the polymerizable compound (Q) having a carbon-carbon double bond group is not included in the "monomer".

[0044] {Alkyl(meth)acrylate (am1)} The number of carbon atoms in the alkyl group of the monomer (am1) is preferably 1 to 24, more preferably 1 to 12, even more preferably 2 to 10, and still more preferably 2 to 8, from the viewpoint of improving adhesive properties. The alkyl group contained in the monomer (am1) may be a linear alkyl group or a branched alkyl group.

[0045] Examples of the monomer (am1) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate. The monomer (am1) is preferably at least one selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate. These monomers (am1) may be used alone or in combination of two or more kinds.

[0046] The content of the structural unit (a1) in the acrylic copolymer (P) is preferably 60 to 99 mass%, more preferably 65 to 98 mass%, and even more preferably 70 to 96 mass%, based on 100 mass% of all structural units constituting the acrylic copolymer (P). The content of the structural unit (a1) in the acrylic copolymer (P) can also be calculated as the content of the monomer (am1) in 100% by mass of all the monomers used in polymerizing the acrylic copolymer (P). Furthermore, the content of the structural unit (a1) in component (A1) is preferably 40 to 99 mass%, more preferably 50 to 98 mass%, and even more preferably 60 to 96 mass%, based on 100 mass% of all structural units constituting component (A1). The content of the structural unit (a1) in the component (A1) can also be calculated as the content of the monomer (am1) in the total of 100 mass% of all monomers and polymerizable compound (Q) used in synthesizing the component (A1).

[0047] Moreover, the monomer (am1) that can be used in one embodiment of the present invention preferably contains at least an alkyl (meth)acrylate having two or more carbon atoms. The alkyl(meth)acrylate having 2 or more carbon atoms is more preferably an alkyl(meth)acrylate having an alkyl group with 4 to 8 carbon atoms, and further preferably n-butyl(meth)acrylate. In the component (A1) that can be used in one embodiment of the present invention, the content of the structural units derived from alkyl (meth)acrylates having 2 or more carbon atoms in the acrylic copolymer (P) is preferably 45 to 99 mass%, more preferably 55 to 98 mass%, and even more preferably 65 to 96 mass%, based on 100 mass% of all structural units constituting the acrylic copolymer (P). The content of the structural units derived from alkyl (meth)acrylates having 2 or more carbon atoms in the acrylic copolymer (P) can also be calculated as the content of the alkyl (meth)acrylates having 2 or more carbon atoms in 100% by mass of all monomers used in polymerizing the acrylic copolymer (P). Furthermore, in component (A1) that can be used in one embodiment of the present invention, the content of the structural units derived from alkyl (meth)acrylates having 2 or more carbon atoms in component (A1) is, in 100% by mass of all structural units constituting component (A1), preferably 35% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, still more preferably 50% by mass or more, and is preferably 99% by mass or less, even more preferably 98% by mass or less, and even more preferably 96% by mass or less. The content of structural units derived from alkyl(meth)acrylates having 2 or more carbon atoms in component (A1) can also be calculated as the content of alkyl(meth)acrylates having 2 or more carbon atoms in 100% by mass of the total of all monomers and polymerizable compound (Q) used in synthesizing component (A1).

[0048] {Functional group-containing monomer (am2)} The monomer (am2) may be a monomer having a functional group such as a hydroxy group, a carboxy group, an epoxy group, an amino group, a cyano group, a nitrogen atom-containing ring group, an alkoxysilyl group, etc. Among these, one or more selected from a hydroxy group-containing monomer, a carboxy group-containing monomer, and an epoxy group-containing monomer are preferred, one or more selected from a hydroxy group-containing monomer and a carboxy group-containing monomer are more preferred, and a hydroxy group-containing monomer is even more preferred.

[0049] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol. The hydroxyl group-containing monomer is preferably a hydroxyalkyl (meth)acrylate, more preferably one or more selected from 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, and even more preferably 2-hydroxyethyl (meth)acrylate.

[0050] Examples of the carboxy group-containing monomer include ethylenically unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids and anhydrides thereof such as fumaric acid, itaconic acid, maleic acid and citraconic acid; 2-(acryloyloxy)ethyl succinate, 2-carboxyethyl (meth)acrylate, and the like. The carboxyl group-containing monomer also includes the anhydrides of the ethylenically unsaturated dicarboxylic acids and derivatives of the ethylenically unsaturated dicarboxylic acids. This is because the carboxyl group can also be generated by hydrolyzing the groups derived from the unsaturated carboxylic anhydrides in component (A). Examples of the unsaturated carboxylic anhydrides include the anhydrides of the above-mentioned unsaturated polyvalent carboxylic acids, such as maleic anhydride, citraconic anhydride, and nadic anhydride. The carboxy group-containing monomer is preferably one or more selected from an ethylenically unsaturated monocarboxylic acid and an ethylenically unsaturated dicarboxylic acid, more preferably an ethylenically unsaturated monocarboxylic acid, even more preferably one or more selected from the group consisting of (meth)acrylic acid, and even more preferably acrylic acid.

[0051] Examples of epoxy-containing monomers include epoxy group-containing (meth)acrylic acid esters and non-acrylic epoxy group-containing monomers. Examples of epoxy group-containing (meth)acrylic acid esters include glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, 3-epoxycyclo-2-hydroxypropyl (meth)acrylate, etc. Examples of non-acrylic epoxy group-containing monomers include glycidyl crotonate, allyl glycidyl ether, etc. These monomers (am2) may be used alone or in combination of two or more kinds.

[0052] The content of the structural unit (a2) in the acrylic copolymer (P) is preferably 1 to 40 mass % in 100 mass % of all structural units constituting the acrylic copolymer (P). The inclusion of the structural unit (a2) in an amount of 1% by mass or more of the total structural units constituting the acrylic copolymer (P) constituting component (A1) is preferred because it improves the organic solvent contact peelability of the resulting pressure-sensitive adhesive sheet.The inclusion of the structural unit (a2) in an amount of 40% by mass or less of the total structural units constituting the acrylic copolymer (P) is preferred because it allows the glass transition temperature to be set low and improves the adhesive strength. From this viewpoint, the content of the structural unit (a2) in the acrylic copolymer (P) is more preferably from 2 to 35 mass %, even more preferably from 3 to 30 mass %, and even more preferably from 4 to 20 mass %. The content of the structural unit (a2) in the acrylic copolymer (P) can also be calculated as the content of the monomer (am2) in 100% by mass of all the monomers used in polymerizing the acrylic copolymer (P). From the same viewpoint, the content of the structural unit (a2) in component (A1) is preferably 1 to 30 mass%, more preferably 2 to 25 mass%, even more preferably 3 to 20 mass%, and still more preferably 4 to 15 mass%, of 100 mass% of all structural units constituting component (A1). The content of the structural unit (a2) in the component (A1) can also be calculated as the content of the monomer (am2) in the total of 100 mass% of all monomers and polymerizable compound (Q) used in the synthesis of component (A1).

[0053] The acrylic copolymer (P) may also have a structural unit (a3) ​​(hereinafter also referred to as "structural unit (a3)") derived from a monomer (am3) (hereinafter also referred to as "monomer (am3)") other than the monomers (am1) and (am2).

[0054] Examples of the monomer (am3) include functional group-containing monomers other than the monomers (am1) and (am2); olefins such as ethylene, propylene, and isobutylene; halogenated olefins such as vinyl chloride and vinylidene chloride; diene monomers such as butadiene, isoprene, and chloroprene; (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and imide (meth)acrylate; styrene, α-methylstyrene, vinyl toluene, vinyl formate, vinyl acetate, acrylonitrile, (meth)acrylamide, (meth)acrylonitrile, (meth)acryloylmorpholine, and N-vinylpyrrolidone. When these monomers (am3) are used, they may be used alone or in combination of two or more kinds.

[0055] The total content of the structural units (a1) and (a2) in the acrylic copolymer (P) is preferably 80 to 100 mass%, more preferably 85 to 100 mass%, even more preferably 90 to 100 mass%, and still more preferably 95 to 100 mass%, based on 100 mass% of all structural units constituting the acrylic copolymer (P). The total content of the structural units (a1) and (a2) can also be calculated as the total content of the monomers (am1) and (am2) in 100% by mass of all the monomers used in polymerizing the acrylic copolymer (P).

[0056] {Polymerizable compound (Q) having a carbon-carbon double bond group} The polymerizable compound (Q) having a carbon-carbon double bond group (hereinafter also simply referred to as "polymerizable compound (Q)") is a compound having a carbon-carbon double bond group and a substituent (hereinafter also simply referred to as "reactive substituent") that can react with a functional group in the structural unit (a2) derived from the (am2) component of the acrylic copolymer (P). As the carbon-carbon double bond group, a (meth)acryloyl group is preferable as described above. Also, the polymerizable compound (Q) is preferably a compound having 1 to 5 carbon-carbon double bond groups per molecule. The reactive substituent in the polymerizable compound (Q) may be appropriately changed depending on the functional group possessed by the monomer (am2), and may be, for example, an isocyanate group, a carboxy group, an epoxy group, etc., with an isocyanate group being preferred from the viewpoint of reactivity, etc. If the polymerizable compound (Q) has an isocyanate group, for example, when the functional group of the monomer (am2) is a hydroxy group, it becomes possible for the polymerizable compound (Q) to easily react with the acrylic copolymer (P).

[0057] Examples of the polymerizable compound (Q) include (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate, (meth)acrylic acid, etc. These polymerizable compounds (Q) may be used alone or in combination of two or more. Among these, (meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of being a compound having a suitable isocyanate group as the reactive substituent and having an appropriate distance between the main chain and the carbon-carbon double bond group. The polymerizable compound (Q) is reacted with the functional group in an amount of preferably 0.15 to 0.95 equivalents, more preferably 0.20 to 0.90 equivalents, even more preferably 0.25 to 0.80 equivalents, and even more preferably 0.30 to 0.60 equivalents, of the total amount (1 equivalent) of functional groups derived from the monomer (am2) in the acrylic copolymer (P).

[0058] The mass average molecular weight (Mw) of component (A1) is not particularly limited as long as the effects of the present invention are manifested, but from the viewpoint of making it easier for the obtained pressure-sensitive adhesive sheet to manifest sufficient adhesion before contact with an organic solvent and better releasability upon contact with an organic solvent, it is preferably from 100,000 to 3,000,000, more preferably from 200,000 to 2,000,000, and even more preferably from 300,000 to 1,000,000. The value of the weight average molecular weight (Mw) is a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC), specifically, a value measured based on the method described in the examples.

[0059] The glass transition temperature (Tg) of component (A1) is not particularly limited as long as the effects of the present invention are manifested, but from the viewpoint of making it easier for the obtained pressure-sensitive adhesive sheet to manifest sufficient adhesiveness before contact with an organic solvent and better releasability upon contact with an organic solvent, the glass transition temperature (Tg) is preferably −20° C. or lower, more preferably −25° C. or lower, even more preferably −35° C. or lower, and still more preferably −40° C. or lower. The glass transition temperature (Tg) is calculated using the Fox formula.

[0060] From the viewpoint of making it easier for the resulting pressure-sensitive adhesive sheet to exhibit sufficient adhesion before contact with an organic solvent and better releasability upon contact with an organic solvent, the content of component (A1) in composition (R1) is preferably 80 to 99.8 mass%, more preferably 85 to 99 mass%, and even more preferably 90 to 98 mass%, of the total amount of the acrylic pressure-sensitive adhesive composition (100 mass% of active ingredient). The content of the component (A1) can also be calculated as the amount of the component (A1) in 100% by mass of all the components mixed when preparing the composition (R1). The same applies to the contents of the component (B1) contained in the composition (R1), and the component (C) and other components contained as necessary.

[0061] [Component (B1): Crosslinking agent] Component (B1) is a crosslinking agent that crosslinks component (A1). Component (B1) may be, for example, an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an aziridine-based crosslinking agent, or a metal chelate-based crosslinking agent. Among these, an isocyanate-based crosslinking agent is preferred. When an isocyanate-based crosslinking agent is used, for example, when component (A1) has a hydroxyl group, the crosslinking agent preferentially crosslinks component (A1). The acrylic pressure-sensitive adhesive composition is crosslinked by the component (B1), for example, by heating after application.

[0062] The isocyanate-based crosslinking agent that can be used as component (B1) includes a polyisocyanate compound. Specific examples of polyisocyanate compounds include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and the like. In addition, biuret bodies, isocyanurate bodies, and further adduct bodies which are reaction products with low molecular weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil are also included. Among these, adduct bodies of aromatic polyisocyanates such as tolylene diisocyanate and polyhydric alcohols (e.g., trimethylolpropane, etc.) are preferred. These may be used alone or in combination of two or more.

[0063] Examples of epoxy crosslinking agents that can be used as component (B1) include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. These may be used alone or in combination of two or more. Examples of metal chelate crosslinking agents that can be used as component (B1) include metal chelate compounds in which acetylacetone, ethyl acetoacetate, tris(2,4-pentanedionate), etc. are coordinated to polyvalent metals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, zirconium, etc. These may be used alone or in combination of two or more. Examples of aziridine crosslinking agents that can be used as component (B1) include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), tris-1-(2-methylaziridine)phosphine, trimethylolpropane tri-β-(2-methylaziridine)propionate, hexa[1-(2-methyl)-aziridinyl]triphosphatriazine, etc. These may be used alone or in combination of two or more.

[0064] The content of component (B1) in composition (R1) is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, even more preferably 1 to 8 parts by mass, and even more preferably 3 to 7 parts by mass, relative to the total amount of component (A1) (100 parts by mass of active ingredient), from the viewpoint of enabling the obtained pressure-sensitive adhesive sheet to easily exhibit sufficient adhesion before contact with an organic solvent and better releasability upon contact with an organic solvent.

[0065] [Component (C): Photopolymerization initiator] The composition (R1) preferably contains a photopolymerization initiator (hereinafter, also referred to as "component (C)"). By containing the photopolymerization initiator, the composition (R1) is easily cured by irradiation with energy rays such as ultraviolet rays. Examples of component (C) include acetophenone, 2,2-diethoxybenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, Michler's ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, benzyl dimethyl ketal, dibenzyl, diacetyl, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-ethylanthraquinone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1- Examples of such initiators include low molecular weight initiators such as hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropanone-1,2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-hydroxy-2-methyl-1-phenyl-propan-1-one, diethylthioxanthone, isopropylthioxanthone, and 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide, and oligomerized initiators such as oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}. Among these, 1-hydroxycyclohexyl phenyl ketone is preferred. These may be used alone or in combination of two or more.

[0066] The content of component (C) in composition (R1) is preferably 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 2 to 6 parts by mass relative to the total amount of component (A1) (100 parts by mass of active ingredient), from the viewpoint of making it easier for the resulting pressure-sensitive adhesive sheet to exhibit sufficient adhesion before contact with an organic solvent and better organic solvent contact releasability after irradiation with energy rays.

[0067] [Other Additives in the Composition (R1)] The composition (R1) may contain other additives in addition to the above-mentioned components (A1), (B1) and (C) as long as the effects of the present invention are not impaired. Examples of other additives include resin components other than component (A1), surfactants, antioxidants, ultraviolet absorbers, light stabilizers, flame retardants, conductive agents, antistatic agents, slip agents, antiblocking agents, colorants, and plasticizers. When the composition (R1) contains other additives, the content of each of them is preferably 0.01 to 20 mass%, more preferably 0.01 to 10 mass%, even more preferably 0.01 to 5 mass%, and still more preferably 0.01 to 2 mass%, relative to 100 mass% of the composition (R1). Examples of resin components other than the component (A1) include polyolefin resins such as polyethylene and polypropylene; polyester resins; and the like.

[0068] When water is used as the solvent, the acrylic pressure-sensitive adhesive composition is preferably an acrylic pressure-sensitive adhesive composition (R2) (hereinafter also referred to as "composition (R2)") comprising: component (A), an acrylic polymer (A2) having a carboxy group (hereinafter also referred to as "component (A2)"); component (B), a crosslinking agent (B2) (hereinafter also referred to as "component (B2)") that crosslinks component (A2); and a neutralizing agent (D) (hereinafter also referred to as "component (D)"). Each component contained in the composition (R2) will be described below.

[0069] [Component (A2): Acrylic polymer having a carboxy group (A2)] Component (A2) is an acrylic polymer having a carboxy group. The inclusion of the carboxyl-containing acrylic polymer (A2) in the composition (R2) improves the water contact peelability of the resulting PSA sheet. This is believed to be because the hydrophilicity of the layer (X) improves the effect of water infiltration into the interface between the layer (X) and the adherend, and the effect of the layer (X) itself taking up water and swelling (hereinafter also referred to as "water swelling") improves, facilitating the sufficient penetration of water into the interface between the layer (X) and the adherend.

[0070] {Alkyl(meth)acrylate (am1)} Component (A2) has a structural unit (a1) (hereinafter also referred to as "structural unit (a1)") derived from an alkyl (meth)acrylate (am1) (hereinafter also referred to as "monomer (am1)"). The number of carbon atoms in the alkyl group of the monomer (am1) that can be used as a raw material for component (A2) is preferably 1 to 24, more preferably 1 to 12, even more preferably 2 to 10, and even more preferably 4 to 8, from the viewpoint of improving adhesive properties. The alkyl group contained in the monomer (am1) may be a linear alkyl group or a branched alkyl group.

[0071] Examples of the monomer (am1) that can be used as a raw material for component (A2) include the various alkyl (meth)acrylates described above for the monomer (am1) related to component (A1). Among them, one or more selected from the group consisting of ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate are preferred, one or more selected from the group consisting of n-butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are more preferred, and n-butyl (meth)acrylate is even more preferred. These monomers (am1) may be used alone or in combination of two or more kinds.

[0072] The content of structural unit (a1) in component (A2) is preferably 45 to 99 mass%, more preferably 55 to 98 mass%, even more preferably 65 to 96 mass%, still more preferably 75 to 94 mass%, and even more preferably 80 to 90 mass%, of all structural units constituting component (A2) (100 mass%). The content of the structural unit (a1) can also be calculated as the content of the monomer (am1) in 100% by mass of all the monomers used when polymerizing component (A2).

[0073] {Carboxy group-containing monomer (am4)} Furthermore, component (A2) is preferably an acrylic polymer having a structural unit (a4) (hereinafter also referred to as "structural unit (a4)") derived from a carboxy group-containing monomer (am4) (hereinafter also referred to as "monomer (am4)").

[0074] Examples of the monomer (am4) include the various carboxy group-containing monomers mentioned above as the monomer (am2) related to the component (A1). As the monomer (am4), one or more selected from an ethylenically unsaturated monocarboxylic acid and an ethylenically unsaturated dicarboxylic acid are preferable, an ethylenically unsaturated monocarboxylic acid is more preferable, one or more selected from the group consisting of (meth)acrylic acid is even more preferable, and acrylic acid is even more preferable. These monomers (am4) may be used alone or in combination of two or more kinds.

[0075] It is more preferable that component (A2) contains the structural unit (a4) in an amount of 0.1 to 20 mass % relative to 100 mass % of all monomers constituting component (A2). The content of the structural unit (a4) in 100% by mass of all structural units constituting component (A2) is preferably 0.1% by mass or more, since the resulting pressure-sensitive adhesive sheet has improved water contact peelability. The content of the structural unit (a4) in 100% by mass of all structural units constituting component (A2) is preferably 20% by mass or less, since the glass transition temperature can be set low and the adhesive strength can be improved. From this viewpoint, the content of the structural unit (a4) in 100% by mass of all structural units constituting component (A2) is more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and more preferably 15% by mass or less, even more preferably 10% by mass or less, and even more preferably 5% by mass or less. The content of the structural unit (a4) can also be calculated as the content of the monomer (am4) in 100% by mass of all the monomers used when polymerizing component (A2).

[0076] {Hydroxy group-containing monomer (am5)} Furthermore, component (A2) is preferably an acrylic polymer having a structural unit (a5) (hereinafter also referred to as "structural unit (a5)") derived from a monomer (am5) (hereinafter also referred to as "monomer (am5)") that contains a hydroxy group. Examples of the monomer (am5) include the various hydroxy group-containing monomers mentioned above as the monomer (am2) related to the component (A1). The monomer (am5) is preferably a hydroxyalkyl (meth)acrylate, more preferably one or more selected from the group consisting of 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, and further preferably 2-hydroxyethyl (meth)acrylate. These monomers (am5) may be used alone or in combination of two or more kinds.

[0077] It is more preferable that component (A2) contains the structural unit (a5) in an amount of 1 to 30 mass % relative to 100 mass % of all monomers constituting component (A2). The content of the structural unit (a5) in 100% by mass of all structural units constituting component (A2) is preferably 1% by mass or more, since the resulting pressure-sensitive adhesive sheet has improved water contact peelability. The content of the structural unit (a5) in 100% by mass of all structural units constituting component (A2) is preferably 30% by mass or less, since the glass transition temperature can be set low and the adhesive strength can be improved. From this viewpoint, the content of the structural unit (a5) in 100% by mass of all structural units constituting component (A2) is more preferably 3% by mass or more, even more preferably 6% by mass or more, even more preferably 9% by mass or more, and more preferably 25% by mass or less, even more preferably 20% by mass or less, and even more preferably 15% by mass or less. The content of the structural unit (a5) can also be calculated as the content of the monomer (am5) in 100% by mass of all the monomers used when polymerizing component (A2).

[0078] In component (A2), the total content of the structural units (a1), (a4), and (a5) is preferably 80 to 100 mass%, more preferably 85 to 100 mass%, even more preferably 90 to 100 mass%, still more preferably 95 to 100 mass%, and even more preferably 98 to 100 mass%, based on 100 mass% of all structural units constituting component (A2). The total content of the structural units (a1), (a4), and (a5) can also be calculated as the total content of the monomers (am1), (am4), and (am5) in 100% by mass of all the monomers used when polymerizing component (A2).

[0079] Component (A2) may have a structural unit (a6) (hereinafter also referred to as "structural unit (a6)") derived from a monomer (am6) (hereinafter also referred to as "monomer (am6)") other than the monomers (am1), (am4), and (am5).

[0080] Examples of the monomer (am6) include functional group-containing monomers other than the monomers (am4) and (am5), such as amino group-containing monomers, substituted amino group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, and alkoxysilyl group-containing monomers; olefins such as ethylene, propylene, and isobutylene; halogenated olefins such as vinyl chloride and vinylidene chloride; diene monomers such as butadiene, isoprene, and chloroprene; cyclohexyl (meth)acrylate, benzyl (meth)acrylate, Examples of the monomer (am6) include isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, imide (meth)acrylate, and other (meth)acrylates having a cyclic structure; styrene, α-methylstyrene, vinyltoluene, vinyl formate, vinyl acetate, acrylonitrile, (meth)acrylamide, (meth)acrylonitrile, (meth)acryloylmorpholine, and N-vinylpyrrolidone. When these monomers (am6) are used, they may be used alone or in combination of two or more.

[0081] Examples of the amino group or substituted amino group-containing monomer include 2-aminoethyl(meth)acrylate, 2-aminoethyl(meth)acrylamide, N-methylaminoethyl(meth)acrylate, and N-methylaminoethyl(meth)acrylamide. Examples of the epoxy group-containing monomer include the various epoxy group-containing monomers described above as the monomer (am2) related to component (A1).

[0082] As a method for introducing a carboxy group into component (A2) other than the method using the monomer (am4), a method can be used in which a homopolymer of the monomer (am1) or a copolymer with a monomer other than the monomer (am1) is polymerized, and then the homopolymer or copolymer is partially saponified to introduce a carboxy group into component (A2). In this case, it is preferable to adjust the content of the structural unit (a1) that remains unsaponified in component (A2) to the content of the structural unit (a1) in component (A2) described above, and the preferred content is also the same.

[0083] The component (A2) can be produced by using a known polymerization method such as bulk polymerization, solution polymerization, or emulsion polymerization. Furthermore, when these components (A2) are copolymers having two or more types of structural units, the copolymer may be in the form of a block copolymer, a random copolymer, or a graft copolymer.

[0084] The mass average molecular weight (Mw) of component (A2) is not particularly limited as long as the effects of the present invention are manifested, but from the viewpoint of making it easier for the obtained pressure-sensitive adhesive sheet to manifest sufficient adhesion before contact with water and better releasability upon contact with water, it is preferably from 100,000 to 3,000,000, more preferably from 200,000 to 2,000,000, and even more preferably from 300,000 to 1,000,000. The value of the weight average molecular weight (Mw) is a value calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC), specifically, a value measured based on the method described in the examples.

[0085] From the viewpoint of making it easier for the resulting pressure-sensitive adhesive sheet to exhibit sufficient adhesion before contact with water and better releasability upon contact with water, the content of component (A2) in composition (R2) is preferably 75 to 95 mass%, more preferably 80 to 92 mass%, and even more preferably 85 to 90 mass%, of the total amount of composition (100 mass% active ingredient). The content of the component (A2) can also be calculated as the amount of the component (A2) in 100% by mass of all the components mixed when preparing the composition (R2). The same applies to the contents of the components (B2), (D) and other components contained in the composition (R2).

[0086] [Component (B2): Crosslinking agent] Component (B2) is a compound that reacts with component (A2) to form a crosslinked structure, and is preferably a compound that reacts with some or all of the carboxy groups in component (A2) to crosslink component (A2). If the composition (R2) does not contain the component (B2), the water-swellability of the layer (X) will not be sufficient. As described below, the pressure-sensitive adhesive layer (X) is a layer having a crosslinked structure derived from component (A2) and component (B2) and a salt-like moiety derived from component (A2) and component (C), and is therefore considered to be able to exhibit excellent water-contact peelability.

[0087] Examples of the component (B2) include epoxy-based crosslinking agents, methylol-based crosslinking agents, metal chelate-based crosslinking agents, aziridine-based crosslinking agents, etc. Among these, one or more types selected from epoxy-based crosslinking agents and metal chelate-based crosslinking agents are preferred, and epoxy-based crosslinking agents are more preferred.

[0088] Examples of epoxy crosslinking agents that can be used as component (B2) include neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, phthalic acid diglycidyl ester, dimer acid diglycidyl ether, diglycerol triglycidyl ether, sorbitol tetraglycidyl ether, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, N,N,N',N'-tetraglycidyldiaminodiphenylmethane, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidyl aniline, and diglycidylamine. Examples of the metal chelate crosslinking agent that can be used as component (B2) include the various metal chelate compounds described above in the description of the crosslinking agent (B1). These components (B2) may be used alone or in combination of two or more.

[0089] The content of component (B2) in composition (R2) is, from the viewpoint of making it easier for the obtained pressure-sensitive adhesive sheet to exhibit sufficient adhesion before contact with water and better releasability upon contact with water, preferably 0.05 to 10 parts by mass, more preferably 0.1 to 9 parts by mass, even more preferably 1 to 8 parts by mass, still more preferably 4 to 8 parts by mass, and even more preferably 6 to 8 parts by mass, relative to the total amount of component (A2) (100 parts by mass of active ingredient).

[0090] [Component (D): Neutralizer] When the composition (R2) contains the neutralizing agent (D), the water-swellability of the layer (X) is improved, and the water-contact peelability of the resulting pressure-sensitive adhesive sheet is improved. It is believed that the neutralizing agent (D) reacts with some or all of the carboxy groups of the component (A2), and the reaction sites partially form salt-like sites (hereinafter also referred to as "salt sites").The salt sites formed by the carboxy groups of the component (A2) and the component (D), and the crosslinked structure formed by the component (A2) and the above-mentioned crosslinking agent (B2), improve the hydrophilicity and water swelling of the layer (X), and the layer (X) exhibits excellent water-contact peelability.

[0091] As the component (D), various basic compounds can be used as long as the effects of the present invention are exhibited, and preferred examples include amine compounds. Examples of the amine compound include organic amino compounds exhibiting alkalinity, such as ammonia, ammonium salts exhibiting alkalinity, primary amine compounds such as monoethylamine and monoethanolamine, secondary amine compounds such as diethylamine and diethanolamine, tertiary amine compounds such as triethylamine, triethanolamine, N,N-dimethylformamide diethylacetal, N,N,N-trimethylethylenediamine, N-methyldiethanolamine, N,N-diethylhydroxylamine and N,N-diethylethanolamine, amino compounds having multiple nitrogen atoms in one molecule such as diamine and polyethyleneimine, and cyclic amino compounds such as pyridine. The amine compound is preferably a tertiary amine compound.

[0092] In addition, as described above, it is considered that the component (D) can provide better hydrophilicity when it forms a salt moiety with the carboxyl group in the component (A2), so among the amine compounds, a hydroxyl group-containing amine compound is more preferred. When the component (D) is a hydroxyl group-containing amine compound, it is considered that the hydroxyl group derived from the component (D) makes the layer (X) more likely to take up water, and the water swelling property of the layer (X) is further improved. From this viewpoint, the component (D) is more preferably a hydroxyl group-containing tertiary amine compound, and even more preferably triethanolamine. These neutralizing agents (D) may be used alone or in combination of two or more kinds.

[0093] From the viewpoint of making it easier for the resulting pressure-sensitive adhesive sheet to exhibit good water-contact peelability, the content of component (D) in composition (R2) is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 9 parts by mass, even more preferably 1 to 8 parts by mass, still more preferably 4 to 8 parts by mass, and even more preferably 6 to 8 parts by mass, relative to the total amount of component (A2) (100 parts by mass of active ingredient).

[0094] [Other Additives in the Composition (R2)] The composition (R2) may contain other additives in addition to the above-mentioned components (A2), (B2) and (D) as long as the effects of the present invention are not impaired. Examples of other additives include resin components other than component (A2), surfactants, antioxidants, ultraviolet absorbers, light stabilizers, flame retardants, conductive agents, antistatic agents, slip agents, antiblocking agents, colorants, and plasticizers. When these additives are contained, the content of each is preferably 0.01 to 20 mass%, more preferably 0.01 to 10 mass%, even more preferably 0.01 to 5 mass%, and still more preferably 0.01 to 2 mass%, relative to 100 mass% of the composition (R2). Examples of resin components other than component (A2) include polyolefin resins such as polyethylene and polypropylene; polyester resins; and the like.

[0095] <Base material> Examples of materials for forming the substrate that can be used in one embodiment of the present invention include resins, metals, and paper materials, and can be appropriately selected depending on the application of the pressure-sensitive adhesive sheet.

[0096] Examples of resins used for the substrate include polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polystyrene; acrylonitrile-butadiene-styrene copolymer; cellulose triacetate; polycarbonate; urethane resins such as polyurethane and acrylic-modified polyurethane; polymethylpentene; polysulfone; polyether ether ketone; polyether sulfone; polyphenylene sulfide; polyimide resins such as polyetherimide and polyimide; polyamide resins; acrylic resins; and fluorine-based resins. Among these, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate are preferred. Examples of the substrate using the resin as a forming material include a resin film or a resin sheet containing the resin. Examples of the metal include aluminum, tin, chromium, and titanium. Examples of the paper material include thin paper, medium-quality paper, fine paper, impregnated paper, coated paper, art paper, parchment paper, glassine paper, and dust-free paper.

[0097] These forming materials may be used alone or in combination of two or more kinds. Examples of substrates that combine two or more forming materials include paper laminated with a thermoplastic resin such as polyethylene, and resin-containing resin films or sheets having a metal layer formed on the surface thereof. Examples of methods for forming the metal layer include a method of depositing a metal by a PVD method such as vacuum deposition, sputtering, or ion plating, and a method of attaching a metal foil with a general adhesive.

[0098] Among these substrates, a resin film or sheet is preferred, a film or sheet made of a polyester-based resin is more preferred, and a film or sheet made of polyethylene terephthalate (PET) is even more preferred.

[0099] In addition, from the viewpoint of improving interlayer adhesion with other layers laminated on the substrate, one or both surfaces of the substrate may be subjected to a surface treatment such as an oxidation method or a roughening method. Examples of the oxidation method include corona discharge treatment, plasma treatment, chromic acid oxidation (wet), flame treatment, hot air treatment, ozone irradiation treatment, ultraviolet irradiation treatment, ultraviolet-ozone treatment, etc. Examples of the roughening method include sandblasting, solvent treatment, etc.

[0100] Furthermore, a primer layer, a filling layer, etc. may be provided on one or both surfaces of the substrate, if necessary. Examples of components constituting the primer layer include polyester-based resins, urethane-based resins, polyester urethane-based resins, acrylic resins, etc., and these resins may be used alone or in combination of two or more kinds. The filling layer is provided to further improve the adhesion between the substrate and a layer adjacent to the substrate, or to impart rigidity to the substrate when the substrate is too soft, such as a paper substrate. The filling layer is not particularly limited, and examples thereof include layers composed of a styrene-butadiene copolymer, an acrylic resin, a polyester resin, a polyurethane resin, a polystyrene resin, or the like as the main component, to which a filler such as clay, silica, calcium carbonate, titanium oxide, or zinc oxide is added as necessary. When these other layers are present, their thicknesses are each independently preferably 0.05 to 30 μm, more preferably 0.1 to 5 μm, even more preferably 0.1 to 1 μm, and still more preferably 0.1 to 0.5 μm. The substrate that can be used in the present invention may contain, as desired, additives for the substrate, such as an ultraviolet absorber, a light stabilizer, an antioxidant, an antistatic agent, a slip agent, an antiblocking agent, a colorant, etc., within the scope that does not impair the effects of the present invention.

[0101] The thickness of the substrate is appropriately set depending on the application of the pressure-sensitive adhesive sheet, but from the standpoint of ease of handling and economic efficiency, it is preferably 5 to 250 μm, more preferably 10 to 200 μm, and even more preferably 25 to 150 μm.

[0102] <Removal material> Examples of the release material that can be used in one embodiment of the present invention include a release sheet that has been treated for release on both sides and a release sheet that has been treated for release on one side, and examples of such a release material include a release agent applied to a substrate for the release material. Examples of the substrate for the release material include plastic films such as polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin, and polyolefin resin films such as polypropylene resin and polyethylene resin. Examples of the release agent include rubber-based elastomers such as silicone-based resins, olefin-based resins, isoprene-based resins, and butadiene-based resins, long-chain alkyl-based resins, alkyd-based resins, and fluorine-based resins.

[0103] As described above, for the purpose of forming recesses on the pressure-sensitive adhesive layer (X), a release material in which a convex shape is formed on the release treatment surface (hereinafter also referred to as a "release material having convex portions") is preferred, and from the viewpoint of making it easier to maintain the recess shape of the layer (X) during storage of the pressure-sensitive adhesive sheet, a release material in which convex portions that pair with the recesses of the layer (X) are formed on the release treatment surface is more preferred. In addition, the term "protrusion" as defined in this specification refers to a protruding portion having a difference in height. The shape of the convex portions can be formed, for example, by transferring a shape engraved on the peripheral surface of an embossing roll onto the release surface by embossing. Moreover, for example, the convex portions can be formed by utilizing a printing technique such as a screen printing method.

[0104] In addition, examples of the shape of the convex portion include a shape that pairs with a concave portion of the layer (X). A preferred embodiment of the convex portion is a shape that pairs with the concave portion described as a preferred embodiment in the description of the concave portion of the layer (X), and therefore detailed description thereof will be omitted here. Furthermore, for example, preferred aspects of “the cross-sectional shape of the recess when the layer (X) is cut in the thickness direction” and “the shape of the recess when the layer (X) is viewed in plan” are similar to preferred aspects of “the cross-sectional shape of the convex portion when the release material is cut in the thickness direction” and “the shape of the convex portion when the release material is viewed in plan”.

[0105] Furthermore, the preferred range of the "height difference and width of convex portions" present on the surface of the release material can also be referred to as the height difference and width of convex portions that can form the "height difference and width of concave portions" present on the surface of the layer (X) described above. Similarly, the preferred range of the "base-to-base distance and shortest pitch of convex portions" present on the surface of the release material can also be referred to as the base-to-base distance and shortest pitch of convex portions that can form the "edge-to-edge distance and shortest pitch of concave portions" present on the surface of the layer (X) described above. Therefore, the preferred ranges of the "height difference and width of the convex portion" and the "distance between the bases of the convex portions and the shortest pitch" are not particularly limited as long as they do not impair the effects of the present invention, and may be, for example, the ranges shown below.

[0106] The height difference of the convex portions is preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 3.0 μm or more, and is preferably 50.0 μm or less, more preferably 30.0 μm or less, even more preferably 25.0 μm or less, and even more preferably 20.0 μm or less. Similarly, the width of the convex portion is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 75.0 μm or less, still more preferably 50.0 μm or less, still more preferably 35.0 μm or less, and still more preferably 30.0 μm or less. There is no particular lower limit to the width of the concave portion, but it is preferably 1.0 μm, more preferably 3.0 μm, and still more preferably 5.0 μm. The height difference and width of the convex portion are values ​​measured using the method described in the Examples. For example, distance 4h shown in Fig. 8 corresponds to the height difference of convex portion 4a. Distance 4w shown in Fig. 8 corresponds to the width of the convex portion. As an example, if we use the cross-sectional image of convex portion 4a shown in Fig. 10, which is a scanning electron microscope (SEM) image taken using the method described in the Examples, distance 4h in Fig. 10 corresponds to the height difference of the convex portion, and distance 4w corresponds to the width of the convex portion.

[0107] The distance between the bases of the convex portions is preferably 50.0 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, and even more preferably 200 μm or more. It is preferably 2,000 μm or less, more preferably 1,500 μm or less, and even more preferably 1,000 μm or less. For example, if the concave portions in Figure 6 are replaced with convex portions (assuming that Figure 6 is a surface having convex portions of a release material), the distance between the bases of the convex portions refers to the shortest distance between the base of any convex portion and the base of the convex portion closest to that convex portion, which refers to distance 7f in Figure 6. Furthermore, for example, if the lattice-like concave portions shown in Figure 7 are replaced with convex portions (assuming Figure 7 is a surface having convex portions of a release material), the distance between the bases of the convex portions refers to the shortest distance between the base of any one side of the convex portions forming the lattice and the base of the side opposite that side, and refers to distance 7f in Figure 7. The shortest pitch between the convex portions is preferably 50.0 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, and even more preferably 200 μm or more, and is preferably 2,000 μm or less, more preferably 1,500 μm or less, and even more preferably 1,000 μm or less. For example, if the concave portions in Figure 6 are replaced with convex portions (if Figure 6 is assumed to be a surface having convex portions of a release material), the shortest pitch of the convex portions refers to the shortest distance from the midpoint of the shortest distance between the bases of any one convex portion to the midpoint of the shortest distance between the bases of another convex portion that is closest to the convex portion in question, and refers to distance 7p in Figure 6. Furthermore, for example, if the lattice-like concave portions shown in Figure 7 are replaced with convex portions (assuming Figure 7 is a surface having convex portions of a release material), the shortest pitch of the convex portions refers to the shortest distance from the midpoint of the shortest distance between the bases of convex portions forming one side of the lattice to the midpoint of the shortest distance between the bases of other convex portions forming the side opposite to the one side, and refers to distance 7p in Figure 7. As an example, if we use a planar image of the convex portion 4a shown in Figure 12, which is a scanning electron microscope (SEM) image taken using the method described in the examples, the distance 4p in Figure 12 corresponds to the shortest pitch of the convex portions, and the distance 4w corresponds to the width of the convex portions.

[0108] The thickness of the release material is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 5 to 250 μm, more preferably 30 to 200 μm, and even more preferably 50 to 150 μm.

[0109] The total thickness of the adhesive sheet (the total thickness of each layer, excluding the release material) is set appropriately depending on the application of the adhesive sheet, but is preferably 30 μm or more, more preferably 70 μm or more, even more preferably 95 μm or more, and is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 170 μm or less, and even more preferably 150 μm or less.

[0110] <Other adhesive layers (Z)> The pressure-sensitive adhesive sheet according to one embodiment of the present invention may have a pressure-sensitive adhesive layer (Z) other than the above-mentioned layer (X) as long as the effects of the present invention are not impaired. An example of the pressure-sensitive adhesive sheet is, as described above, a pressure-sensitive adhesive sheet 30 shown in Fig. 3 in which one of the two layers (X) 2 is a pressure-sensitive adhesive layer (Z) other than the layer (X) 2 that does not have a recess 1 on its surface. Another example is a pressure-sensitive adhesive sheet 50 shown in Fig. 5. The other adhesive layer (Z) other than the layer (X) can be appropriately selected depending on the application of the adhesive sheet, and is not particularly limited as long as it does not impair the effects of the present invention. Examples of the adhesive resin contained in the other adhesive layer (Z) include rubber-based resins such as acrylic resins, urethane resins, and polyisobutylene resins, polyester resins, olefin resins, silicone resins, and polyvinyl ether resins. These adhesive resins may be used alone or in combination of two or more kinds. Furthermore, when these adhesive resins are copolymers having two or more types of constitutional units, the copolymer may be in the form of any one of a block copolymer, a random copolymer, and a graft copolymer. Furthermore, when the pressure-sensitive adhesive sheet according to one embodiment of the present invention has a pressure-sensitive adhesive layer (Z), the aforementioned release material may be provided on the exposed surface of the pressure-sensitive adhesive layer (Z).

[0111] [Method of manufacturing temporary fixing adhesive sheet] The method for producing the temporary fixing pressure-sensitive adhesive sheet is not particularly limited as long as it is possible to form a pressure-sensitive adhesive layer (X) having a recess on at least one surface. Preferably, the method includes a production method having at least the following steps (1) and (2): Step (1): A step of applying a pressure-sensitive adhesive composition onto the surface of a release material having convex portions, on which the convex portions are present, to form a coating film. Step (2): A step of drying the coating film formed in step (1) to form a pressure-sensitive adhesive layer (X) having recesses on the surface on the release material side, thereby obtaining a temporary fixing pressure-sensitive adhesive sheet.

[0112] In the following explanation, the aspects of the pressure-sensitive adhesive layer (X), the release material and the substrate, the aspect of the pressure-sensitive adhesive composition forming the layer (X) and the aspect of the acrylic pressure-sensitive adhesive composition which is a preferred aspect thereof, as well as the aspect of the obtained temporary fixing pressure-sensitive adhesive sheet are the same as those explained in the section on the temporary fixing pressure-sensitive adhesive sheet, and their preferred aspects are also the same, so detailed explanations will be omitted.

[0113] By using a release material having convex portions in step (1), the shape of the convex portions can be transferred onto the surface of layer (X) to form concave portions in layer (X) during the process in step (2) in which the coating film made of the pressure-sensitive adhesive composition is dried to form the pressure-sensitive adhesive layer (X). When the pressure-sensitive adhesive composition is applied onto a release material having convex portions, the pressure-sensitive adhesive composition may be used in the form of a solution by further blending an organic solvent with the pressure-sensitive adhesive composition. Examples of the organic solvent to be used include methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol. As for these organic solvents, the organic solvents used in producing each component contained in the pressure-sensitive adhesive composition may be used as they are, or one or more other organic solvents may be added thereto.

[0114] The solution of the pressure-sensitive adhesive composition can be applied onto the release material by a known application method to form a coating film. Examples of the coating method include spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, and gravure coating.

[0115] In step (2), the coating film formed in step (1) is dried. As described above, the coating film is dried to form the pressure-sensitive adhesive layer (X), and recesses in the layer (X) are formed. The drying temperature in step (2) is not particularly limited as long as the layer (X) can be formed, but is preferably 80 to 150° C., more preferably 90 to 140° C., and even more preferably 95 to 130° C. The drying time is not particularly limited as long as the layer (X) can be formed, but is preferably 30 seconds to 5 minutes, and more preferably 1 minute to 3 minutes.

[0116] [Applications of temporary fixing adhesive sheets] The temporary fixing adhesive sheet of one embodiment of the present invention has solvent contact releasability, and while it has sufficient adhesive strength when affixed to an adherend, when it is to be removed from the adherend it can be self-detached in a short time by contacting it with a solvent, and therefore can be applied to any application as long as an adherend that can come into contact with a solvent is used. The adherend is not particularly limited, but from the viewpoint that the temporary fixing adhesive sheet has solvent contact releasability and can reduce the load on the adherend, a preferred embodiment of the adherend is a brittle material, and preferred examples of the brittle material include wafers for electronic devices, which will be described later. In addition, from the viewpoint that the temporary fixing adhesive sheet has solvent contact peelability and is expected to suppress or prevent defects such as contamination, deformation, and damage of the adherend caused by the temporary fixing adhesive sheet, an example of a suitable embodiment of the adherend is a material for electronic devices. Examples of the electronic device material include chips for electronic devices such as semiconductor chips, wafers for electronic devices such as semiconductor wafers, compound semiconductors, packages for electronic devices such as semiconductor packages, electronic components, sapphire substrates, displays, substrates for panels, etc. Among these, wafers for electronic devices are more preferred.

[0117] Similarly, the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention can be suitably used in, for example, the manufacturing process of electronic device materials as described above.Specific examples of the pressure-sensitive adhesive sheet in such a usage mode include, for example, a dicing sheet used when dicing an adherend such as an electronic device wafer, a backgrind sheet used in the process of grinding an adherend such as an electronic device wafer, a temporary fixing sheet used to temporarily fix a support for supporting a backgrind sheet to which an adherend such as an electronic device wafer is attached, an expand tape used to expand the distance between adherends such as electronic device chips that have been singulated by dicing, a transfer tape used to invert the front and back of an adherend such as an electronic device chip, and a temporary fixing sheet for inspecting an object to be inspected. Therefore, the temporary fixing pressure-sensitive adhesive sheet of one embodiment of the present invention can be suitably used in the processing and / or inspection of materials for electronic devices.

[0118] In addition, as described above, the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention has self-peeling properties, and is expected to suppress and prevent defects such as contamination, deformation, and damage of the adherend caused by the pressure-sensitive adhesive sheet. Therefore, the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention can be used in a variety of applications other than electronic device materials, such as protective film applications such as window films, protective and design-imparting applications such as wallpaper and wrapping films, various label applications such as returnable labels, and use in attaching temporary notices and the like. Furthermore, when the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention is a pressure-sensitive adhesive sheet having the layer (X) having the above-mentioned continuous recessed shape, it can be suitably used in applications requiring air release properties and appearance when attached to an adherend, such as identification, decoration, paint masking, and surface protection of metal plates, etc. More specifically, it can be suitably used, for example, as a paint replacement tape; a marking film; and a tape for attaching to a vehicle (for example, a decorative tape for decorating the exterior and interior of an automobile, a blackout tape, etc.).

[0119] In addition, when the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention is used as a double-sided pressure-sensitive adhesive sheet, for example, when the pressure-sensitive adhesive sheet is composed of only a single pressure-sensitive adhesive layer and the recess is present only on one surface of the layer (X), or when the pressure-sensitive adhesive sheet has two pressure-sensitive adhesive layers and the layer (X) has a recess only on one surface, it is possible to appropriately select which of the adherends the surface having the recess is to be attached to. For example, the layer (X) may be attached to the side of the adherend that is desired to be peeled off with a lower load, or, for example, when the other pressure-sensitive adhesive layer is another pressure-sensitive adhesive layer provided for a purpose other than the layer (X) (for example, when it is a pressure-sensitive adhesive layer with lower staining properties, etc.), the attachment surface for each adherend may be selected according to the effect of each layer.

[0120] For example, when the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention is used as a double-sided pressure-sensitive adhesive sheet for processing and inspection of an adherend, from the viewpoint of improving the processability and inspectability of the adherend, the adherend can be attached to either one of the pressure-sensitive adhesive layers on both sides, and a support can be attached to either one of the pressure-sensitive adhesive layers. In this case, as described above, it is sufficient to use layer (X) as either one of the pressure-sensitive adhesive layers, and both pressure-sensitive adhesive layers may be layers (X). Fixing the adherend to the support via the adhesive sheet is preferable because it suppresses vibration and displacement of the adherend, and damage when the adherend is a fragile material such as a brittle material, when the adherend is subjected to one or more of processing and inspection, thereby improving processing accuracy and processing speed as well as inspection accuracy and inspection speed. In this case, when using a double-sided pressure-sensitive adhesive sheet having only one of the pressure-sensitive adhesive layers as layer (X), depending on the type of adherend to be processed and / or inspected and the type of processing and / or inspection method, the adherend to be processed and / or inspected may be affixed to the layer (X) side and the support may be affixed to the other pressure-sensitive adhesive layer, or the support may be affixed to the layer (X) side and the adherend to be processed and / or inspected may be affixed to the other pressure-sensitive adhesive layer. Similarly, when using a double-sided pressure-sensitive adhesive sheet having different layers (X) on both sides, either layer (X) may be attached to an adherend that is to be processed and / or inspected.

[0121] The adherend to be processed and / or inspected is preferably a material for electronic devices, as described above. Therefore, for example, when the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention is used as a double-sided pressure-sensitive adhesive sheet for processing and / or inspecting the material for electronic devices, it can be suitably used for temporarily fixing the material for electronic devices to a support. The material of the support may be appropriately selected taking into consideration the required properties such as mechanical strength and heat resistance depending on the type of adherend to be processed and / or inspected, the type of processing and / or inspection method, etc. For example, when the temporary fixing pressure-sensitive adhesive sheet of one embodiment of the present invention is used as a double-sided pressure-sensitive adhesive sheet for processing and / or inspecting the electronic device material, examples of the material for the support include metal materials such as SUS; non-metallic inorganic materials such as glass and silicon wafers; resin materials such as epoxy resins, ABS resins, acrylic resins, engineering plastics, super engineering plastics, polyimide resins, and polyamideimide resins; and composite materials such as glass epoxy resins, and among these, SUS, glass, and silicon wafers are preferred. Examples of the engineering plastics include nylon, polycarbonate (PC), and polyethylene terephthalate (PET). Examples of the super engineering plastics include polyphenylene sulfide (PPS), polyethersulfone (PES), and polyetheretherketone (PEEK).

[0122] In addition, when the temporary fixing pressure-sensitive adhesive sheet according to one embodiment of the present invention is used as a double-sided pressure-sensitive adhesive sheet for processing and / or inspecting the electronic device material, the support is preferably attached to the entire adhesive surface of the adhesive layer to be attached. Therefore, the surface area of ​​the support on the side attached to the adhesive surface of the adhesive layer is preferably equal to or larger than the surface area of ​​the adhesive surface of the adhesive layer. In addition, the surface of the support on the side attached to the adhesive surface of the adhesive layer is preferably flat. The shape of the support is not particularly limited, but is preferably a plate shape. The thickness of the support may be appropriately selected in consideration of the required characteristics, but is preferably from 20 μm to 50 mm, more preferably from 60 μm to 20 mm. EXAMPLES

[0123] The present invention will be described in detail with reference to the following examples, but the present invention is not limited to the following examples. Note that the physical properties in the following examples were measured by the following methods.

[0124] <Mass average molecular weight (Mw)> Measurements were carried out using a gel permeation chromatograph (manufactured by Tosoh Corporation, product name "HLC-8020") under the conditions below, and values ​​measured in terms of standard polystyrene were used. (Measurement conditions) Column: "TSK guard column HXL-L", "TSK gel G2500HXL", "TSK gel G2000HXL", and "TSK gel G1000HXL" (all manufactured by Tosoh Corporation) connected in series Column temperature: 40℃ Developing solvent: Tetrahydrofuran ·Flow rate: 1.0mL / min

[0125] <Glass transition temperature (Tg)> The glass transition temperature (Tg) of component (A) was calculated using the Fox formula.

[0126] <Thickness of the base layer and release layer> The measurements were made using a constant pressure thickness gauge (manufactured by Techclock Corporation, model number: "PG-02J", standard specifications: compliant with JIS K6783-1994, Z1702-1994, Z1709-1995). The thickness of the embossed release material is the distance from the smooth surface of the release material to the point where the protrusions on the embossed surface are formed. For example, the distance 4t shown in Figure 8 corresponds to the thickness of the release material.

[0127] <Thickness of each layer in the adhesive sheet> Cross sections in the thickness direction of the adhesive layer (X1) and the adhesive layer (X2) of the adhesive sheets produced in the Examples and Comparative Examples, cut perpendicularly to a plane parallel to the surface of the base layer (corresponding to a portion where no recesses are formed), were observed using a scanning electron microscope (manufactured by Hitachi, Ltd., product name "S-4700"), and the thicknesses of the adhesive layer (X1) and the adhesive layer (X2) were measured. The thickness of the pressure-sensitive adhesive layer (X) was determined as the distance from the surface of the pressure-sensitive adhesive layer in contact with the substrate to a location on the surface opposite the substrate where no recesses were formed. For example, the distance 2t shown in FIG. 1 corresponds to the thickness of the layer (X). The thickness of the pressure-sensitive adhesive layer (Z), which will be described later, was also measured in the same manner.

[0128] <Height difference, width and minimum pitch of recesses in layer (X)> The height difference and width of the recesses present on the surface opposite the substrate of the pressure-sensitive adhesive layer (X) (layer (X1) and layer (X2)) of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples were measured by observing the cross-section of the pressure-sensitive adhesive sheet using a scanning electron microscope (manufactured by Hitachi, Ltd., product name "S-4700") and utilizing the measurement function of image analysis software for scanning electron microscopes. 9 and 13 show SEM images of the measurements of the height difference of the recesses on the layer (X1) in Examples 1 and 13, respectively. In the case of Example 1, the height difference and width values ​​correspond to the distances 1h and 1w shown in FIG. 9. In the case of Example 13, the height difference and width values ​​correspond to the distances 1h and 1w shown in FIG. 11 and 14 show SEM images of the shortest pitch of the recesses on the layer (X1) in Examples 1 and 13, respectively. In the cases of Examples 1 and 13, the shortest pitch corresponds to the distance 7p shown in Figures 11 and 14. Note that 1w shown in Figures 11 and 14 corresponds to the width of the recesses.

[0129] <Height difference, width and minimum pitch of the convex parts of the release material> The height difference and width of the convex portions present on the adhesive layer side of the release material used in the examples were measured by observing the cross section using a scanning electron microscope (manufactured by Hitachi, Ltd., product name "S-4700") and utilizing the measurement function of image analysis software for scanning electron microscopes. 10 shows an SEM image obtained when measuring the height difference and the like of the convex portions of the release material 1. The height difference and width values ​​of the convex portions of the release material 1 correspond to the distances 4h and 4w shown in FIG. Moreover, Fig. 12 shows an SEM image obtained when measuring the shortest pitch of the convex portions of the release material 1. The value of the shortest pitch of the convex portions of the release material 1 corresponds to the distance 4p shown in Fig. 12. Note that 4w shown in Fig. 12 corresponds to the width of the convex portions.

[0130] <Evaluation of peelability of adhesive sheets after contact with organic solvents> Double-sided pressure-sensitive adhesive sheets for evaluating organic solvent contact peelability were produced in the pressure-sensitive adhesive sheets produced in Examples 1 to 12 and Comparative Examples 1 to 5 described below, in which the pressure-sensitive adhesive layer (X2) was replaced with a pressure-sensitive adhesive layer (Z) having no recesses formed as follows. Specifically, an acrylic copolymer (Tg = -33°C, mass average molecular weight = 500,000) obtained by copolymerizing 77 parts by mass of n-butyl acrylate, 20 parts by mass of methyl methacrylate, and 3 parts by mass of 2-hydroxyethyl acrylate was prepared as the acrylic polymer for the adhesive layer (Z). Next, 5 parts by mass (active ingredient ratio) of trimethylolpropane adduct tolylene diisocyanate (manufactured by Tosoh Corporation, product name "Coronate (registered trademark) L") as a crosslinking agent was added to 100 parts by mass of the acrylic copolymer to prepare an acrylic pressure-sensitive adhesive composition, which was then diluted with toluene and stirred for 30 minutes to prepare a solution of the acrylic pressure-sensitive adhesive composition. Next, the solution of the acrylic adhesive composition was applied onto the release-treated surface of the release material 4 described below using an applicator, and dried at a drying temperature of 100°C for 2 minutes to form an adhesive layer (Z) having no recesses to a thickness of 20 μm. Then, the exposed surface of the pressure-sensitive adhesive layer (Z) was bonded to the exposed surface of the PET substrate of a laminate consisting of a pressure-sensitive adhesive layer (X1) and a PET substrate prepared in the same manner as in Examples 1 to 12 and Comparative Examples 1 to 5 described below, to prepare a double-sided pressure-sensitive adhesive sheet for evaluating organic solvent contact peelability. Each of the prepared double-sided PSA sheets for evaluating the organic solvent contact peelability was cut into test pieces measuring 50 mm in length (MD) × 50 mm in width (TD). In addition, two glass plates (manufactured by Corning Corporation, product name "Eagle XG (registered trademark)", size: length 50 mm × width 50 mm × thickness 2 mm) were prepared. Then, only the release material on the adhesive layer (X1) side was removed, and one of the glass plates was bonded to the exposed surface of the adhesive layer (X1) by pressure bonding using a tabletop laminator (manufactured by Fujipla Inc., product name "LPD3212") at 23°C and a lamination speed of 300 mm / min. Next, the release material 4 on the adhesive layer (Z) side was also removed, and the remaining glass plate was bonded to the exposed surface of the adhesive layer (Z) by pressing it using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., product name "V-130") under conditions of 60°C, 0.2 MPa, and 30 seconds. After that, an ultraviolet irradiation device (manufactured by Lintec Corporation, product name "RAD-2000m / 12") was used to irradiate the sample with an illuminance of 180 mW / cm 2 , cumulative light intensity 300mJ / cm 2Under the above conditions, the layer (X1) was irradiated with ultraviolet light through the glass plate from the front side of the pressure-sensitive adhesive layer (X1) to cure the layer (X1), thereby preparing a sample for evaluating the peelability from contact with an organic solvent. The obtained organic solvent contact peelability evaluation sample was immersed in methyl ethyl ketone (MEK) at 25°C with the layer (X1) facing upward, and the time until the entire surface of the glass plate attached to the layer (X1) side peeled off by itself was measured. Note that even if the evaluation sample was placed flat in a transparent container containing methyl ethyl ketone, the organic solvent penetrated between the peeled glass plate and the layer (X1), causing a difference in refractive index between the peeled and unpeeled parts of the evaluation sample, so that it was possible to visually check whether or not peeling had occurred even from outside the transparent container. Here, MD in MD direction is an abbreviation of Machine Direction, and MD direction means the longitudinal direction when the pressure-sensitive adhesive sheet is molded. Also, TD in TD direction is an abbreviation of Transverse Direction, and TD direction means the width direction when the pressure-sensitive adhesive sheet is molded. Here, the "MD direction" of the pressure-sensitive adhesive sheet refers to the direction in which the pressure-sensitive adhesive composition is applied when forming the pressure-sensitive adhesive layer (X1). The results obtained are shown in Table 1 below.

[0131] <Evaluation of water contact peelability of adhesive sheets> Using the same method as described above for the preparation of double-sided PSA sheets for evaluating organic solvent contact peelability, double-sided PSA sheets for evaluating water contact peelability were prepared by replacing the PSA layer (X2) with the PSA layer (Z) (thickness 20 μm) not having the recesses described above in the PSA sheets prepared in Examples 13 to 15 and Comparative Examples 6 to 7 described below. Each of the prepared double-sided PSA sheets for evaluating water contact peelability was cut into test pieces measuring 50 mm in length (MD) × 50 mm in width (TD). In addition, two glass plates (manufactured by Corning Corporation, product name "Eagle XG (registered trademark)", size: length 50 mm × width 50 mm × thickness 2 mm) were prepared. Then, only the release material on the adhesive layer (X1) side was removed, and one of the glass plates was bonded to the exposed surface of the adhesive layer (X1) by pressure bonding using a tabletop laminator (manufactured by Fujipla Inc., product name "LPD3212") at 23°C and a lamination speed of 300 mm / min. Next, the release material 4 on the adhesive layer (Z) side was also removed, and the remaining glass plate was bonded to the exposed surface of the adhesive layer (Z) by pressure bonding using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., product name "V-130") under conditions of 60°C, 0.2 MPa, and 30 seconds, to prepare a sample for evaluating water contact peelability. The obtained water contact peelability evaluation sample was immersed in a water tank of pure water at 25°C with the layer (X1) side facing up, and the time until the entire surface of the glass plate attached to the layer (X1) side peeled off by itself was measured. Even if the evaluation sample was placed flat in the water tank, water penetrated between the peeled glass plate and the layer (X1), causing a difference in refractive index between the peeled and unpeeled parts of the evaluation sample, so that it was possible to visually check whether or not peeling had occurred even from outside the water tank. Here, the "MD direction" of the pressure-sensitive adhesive sheet in this evaluation method refers to the direction in which the pressure-sensitive adhesive composition is applied when forming the pressure-sensitive adhesive layer (X1). The results obtained are shown in Table 2 below.

[0132] <Adhesive strength of adhesive layer (X1)> In the same manner as the pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples, single-sided pressure-sensitive adhesive sheets not forming a pressure-sensitive adhesive layer (X2) were prepared as samples for evaluating adhesive strength. Each evaluation sample was cut into test pieces measuring 300 mm in length (MD) × 25 mm in width (TD). Then, the release material on the adhesive layer (X1) was removed, and the exposed surface of the adhesive layer (X1) was attached to the mirror surface of a silicon mirror wafer using a 2 kg rubber roller in accordance with JIS Z0237:2000. After that, after leaving it to stand for 20 minutes in an environment of 23°C and 50% RH (relative humidity), the adhesive layer (X1) was peeled off from the silicon mirror wafer at a tensile speed of 300 mm / min by the 180° peeling method based on JIS Z0237:2000, and the adhesive strength of the adhesive layer (X1) was measured. The adhesive strength of the adhesive sheets produced in Examples 1 to 12 and Comparative Examples 1 to 5 indicates the adhesive strength before irradiation with ultraviolet light in Table 1 below. (Adhesive strength after UV exposure) For the pressure-sensitive adhesive sheets produced in Examples 1 to 12 and Comparative Examples 1 and 2, the adhesive strength after irradiating the pressure-sensitive adhesive layer (X1) with ultraviolet light was also measured by the following method. A test piece was prepared in the same manner as the test piece before ultraviolet irradiation, and the surface of the adhesive layer (X1) was attached to the mirror surface of the silicon mirror wafer under the same conditions. After leaving it for 20 minutes in an environment of 23°C and 50% RH (relative humidity), it was irradiated with ultraviolet light at an illuminance of 180mW / cm using an ultraviolet irradiator (manufactured by Lintec Corporation, product name "RAD-2000m / 12"). 2 , cumulative light intensity 300mJ / cm 2 Under the above conditions, the pressure-sensitive adhesive layer (X1) was irradiated with ultraviolet light from the PET substrate side. After that, after leaving it to stand for 20 minutes in an environment of 23°C and 50% RH (relative humidity), the adhesive layer (X1) was peeled off from the silicon mirror wafer at a tensile speed of 300 mm / min by the 180° peeling method based on JIS Z0237:2000, and the adhesive strength of the adhesive layer (X1) after ultraviolet irradiation was measured.

[0133] [Manufacturing of adhesive sheets]

[0134] <Substrate and release material> The abbreviations shown below respectively represent the following materials. PET substrate: polyethylene terephthalate film, manufactured by Toyobo Co., Ltd., product name "Cosmoshine (registered trademark)", product number "A4300", thickness 50 μm Release material 1: Film with silicone release treatment on the embossed surface, thickness 139μm (including convex height), embossed pattern diagonal lattice, minimum pattern pitch 250μm, convex cross-sectional shape V-shaped, convex height 9μm, convex width 20μm Release material 2: Release paper having a resin layer with a silicone release treatment on the embossed surface, thickness 143 μm (including the height of the convex part), embossing pattern parallel oblique lines, minimum pattern pitch 700 μm, cross-sectional shape of the convex part U-shaped, convex part height 23 μm, convex part width 71 μm Release material 3: Release paper having a resin layer with a silicone release treatment on the embossed surface, thickness 142 μm (including the height of the convex part), embossing pattern wavy line, cross-sectional shape of the convex part U-shaped, convex part height 22 μm, convex part width 98 μm Release material 4: Polyethylene terephthalate film with silicone release treatment on one side, product name "SP-PET381031", thickness 38μm, not embossed.

[0135] <Production and evaluation of adhesive sheet with organic solvent peelability> Example 1 An acrylic copolymer (A1) was prepared by adding methacryloyloxyethyl isocyanate (hereinafter also abbreviated as "MOI") to an acrylic copolymer (P) obtained by copolymerizing 95.5 parts by mass of n-butyl acrylate (hereinafter also abbreviated as "BA") and 4.5 parts by mass of 2-hydroxyethyl acrylate (hereinafter also abbreviated as "2HEA") at an addition rate of 0.33 equivalents relative to the hydroxyl group of 2HEA (1 equivalent) (carbon-carbon double bond group concentration = 0.13 mmol / g, Tg = -52°C, mass average molecular weight = 500,000). The concentration of the carbon-carbon double bond group was calculated as follows. First, the molecular weight of BA is 128 g / mol, the molecular weight of 2HEA is 116 g / mol, and the molecular weight of MOI is 155 g / mol. The number of moles of MOI added to 100 g of acrylic copolymer (P) consisting of BA and 2HEA is calculated as 0.039 (mol) x 33% = 0.013 (mol) because the number of moles of 2HEA is 4.5 (g) / 116 (g / mol) = 0.039 (mol), and the addition rate to the hydroxyl group of the 2HEA is 0.33 equivalents. The mass of MOI at this number of moles is 0.013 (mol) x 155 (g / mol) = 2.0 (g). That is, 2.0 g of MOI is added to 100 g of acrylic copolymer (P) consisting of BA and 2HEA, and the mass of the obtained acrylic polymer (A1) is 102.0 g. As a result, since the MOI contained in the acrylic polymer (A1) is 0.013 (mol), the concentration of the carbon-carbon double bond group in the acrylic polymer (A1) is 0.013 (mol) / 102.0 (g)=0.13×10 -3 (mol / g)=0.13 (mmol / g). The same calculation was performed in the following examples from Example 2 onwards. Next, 5 parts by mass (effective ingredient ratio) of trimethylolpropane adduct tolylene diisocyanate (manufactured by Tosoh Corporation, product name "Coronate (registered trademark) L") as a crosslinking agent and 3 parts by mass (effective ingredient ratio) of 1-hydroxycyclohexyl phenyl ketone (manufactured by IGM Resins, product name "Omnirad (registered trademark) 184") as a photopolymerization initiator were added to 100 parts by mass of the acrylic polymer (A1) to prepare an acrylic pressure-sensitive adhesive composition, which was then diluted with toluene and stirred for 30 minutes to prepare a solution of the acrylic pressure-sensitive adhesive composition. Next, the solution of the acrylic adhesive composition was applied onto the embossed surface of the release material 1 using an applicator and dried for 2 minutes at a drying temperature of 100° C. to form a first adhesive layer (X1). Furthermore, the PET substrate was laminated onto the exposed surface of the adhesive layer (X1). Separately, a second pressure-sensitive adhesive layer (X2) was formed on the embossed surface of the release material 1 prepared above, using the solution of the acrylic pressure-sensitive adhesive composition in the same manner as above. Then, the exposed surface of the pressure-sensitive adhesive layer (X2) was laminated onto the exposed surface of the PET substrate laminated to the pressure-sensitive adhesive layer (X1), to obtain a pressure-sensitive adhesive sheet having pressure-sensitive adhesive layers (X) on both sides.

[0136] Examples 2 to 12 and Comparative Examples 1 to 5 Each pressure-sensitive adhesive sheet shown in Table 1 was obtained in the same manner as in Example 1, except that the acrylic polymer was changed to an acrylic polymer having the composition shown in Table 1, and the type of release material and the thickness of the pressure-sensitive adhesive layer were changed to those shown in Table 1. However, for the preparation of the acrylic pressure-sensitive adhesive compositions of Comparative Examples 1 and 2, a solution of the acrylic pressure-sensitive adhesive composition was prepared in the same manner as in Example 1, except that an acrylic polymer having the composition shown in Table 1 was used and the photopolymerization initiator was not added. In addition, "MMA" in Table 1 is an abbreviation for methyl methacrylate.

[0137] The pressure-sensitive adhesive sheets obtained in Examples 1 to 12 and Comparative Examples 1 to 5 were evaluated using the above-mentioned evaluation methods. The results are shown in Table 1 below.

[0138] [Table 1]

[0139] It was confirmed from Table 1 that the pressure-sensitive adhesive sheets of Examples 1 to 12 had excellent organic solvent contact peelability, and the time it took for the pressure-sensitive adhesive sheets to self-peel from the adherend after immersion in an organic solvent was significantly shorter than that of the pressure-sensitive adhesive sheets of Comparative Examples 1 to 5. It was also confirmed that the pressure-sensitive adhesive sheets of Examples 1 to 12 had sufficient adhesive strength to hold the adherend even before immersion in an organic solvent (after UV irradiation). In the pressure-sensitive adhesive sheets of Examples 1 to 12, the acrylic pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer (X) (layer (X1) and layer (X2)) contains an acrylic polymer (A) having a carbon-carbon double bond group concentration of more than 0 mmol / g. This makes it easier for each pressure-sensitive adhesive layer (X) to swell with an organic solvent, and easier for the organic solvent to penetrate into the interface between each pressure-sensitive adhesive layer (X) and the adherend, presumably improving the organic solvent contact peelability. Furthermore, the pressure-sensitive adhesive sheets of Examples 1 to 12 have recesses on the attachment surface of the pressure-sensitive adhesive layer (X) (layer (X1) and layer (X2)) to the adherend. When the pressure-sensitive adhesive sheets are viewed in a plan view, therefore, when immersed in an organic solvent, the organic solvent can easily penetrate from the outer edge of the pressure-sensitive adhesive sheet to the center of the pressure-sensitive adhesive sheet along the recesses. It is believed that for these reasons, the pressure-sensitive adhesive sheets of Examples 1-12 exhibited a significantly shorter time until they were peeled off upon contact with an organic solvent than the pressure-sensitive adhesive sheets of Comparative Examples 1-5. On the other hand, in the pressure-sensitive adhesive sheets of Comparative Examples 1 and 2, recesses are present on the application surface of the pressure-sensitive adhesive layer (X) (layer (X1) and layer (X2)). However, since the acrylic pressure-sensitive adhesive composition forming each pressure-sensitive adhesive layer (X) does not contain an acrylic polymer (A) having a carbon-carbon double bond group concentration of more than 0 mmol / g, it is believed that this results in the layer (X) being less likely to swell in an organic solvent and therefore longer times until peeling occurs upon contact with an organic solvent. Furthermore, since the pressure-sensitive adhesive sheets of Comparative Examples 3 to 5 have no recesses on the attachment surfaces of the pressure-sensitive adhesive layers (layers (X1) and (X2)), after the pressure-sensitive adhesive sheets are immersed in an organic solvent, the organic solvent can only penetrate into the interface between each pressure-sensitive adhesive layer and the adherend from the outer edge of the pressure-sensitive adhesive sheet. Therefore, it is considered that it took time for the organic solvent to penetrate into the interface between each pressure-sensitive adhesive layer and the adherend to an extent that the pressure-sensitive adhesive sheet could be self-peeled from the adherend. In addition, for the pressure-sensitive adhesive sheets of Examples 1 to 12, the surfaces of the pressure-sensitive adhesive layers (X1) and (X2) were observed in plan (magnification: 100 times) using an optical digital microscope (manufactured by Keyence Corporation, product name "Digital Microscope VHX-5000") before immersing the evaluation samples in the organic solvent contact peelability evaluation in MEK. As a result, it was confirmed that both the pressure-sensitive adhesive layers (X1) and (X2) of the pressure-sensitive adhesive sheets of Examples 1 to 12 had a plurality of the recesses continuously bonded from any one point of the contour of the surface to another point of the contour. It was also confirmed that the continuously bonded recesses formed a recess continuously bonded from any one side to any other side of the surface of the pressure-sensitive adhesive layer (X). It was also confirmed that the shortest pitch of the recesses formed on the surface of the adhesive layer (X) of the adhesive sheet of Example 1 was 250 μm, and the shortest pitch of the recesses formed on the surface of the adhesive layer (X) of the adhesive sheet of Example 11 was 700 μm.

[0140] <Preparation and evaluation of adhesive sheets with water contact peelability> (Preparation of Acrylic Pressure-Sensitive Adhesive Composition) Manufacturing Example 1 An acrylic pressure-sensitive adhesive composition was prepared by blending 100 parts by mass (effective component ratio) of an acrylic copolymer (an acrylic copolymer having structural units derived from raw material monomers consisting of n-butyl acrylate (BA) / 2-hydroxyethyl acrylate (2HEA) / acrylic acid (AAc) = 85 / 12 / 3 (mass ratio), mass average molecular weight (Mw): 400,000) which is an acrylic polymer (A2) having a carboxy group with 7 parts by mass of triethanolamine as a neutralizing agent (B2) and 7 parts by mass (effective component ratio) of an epoxy crosslinking agent (manufactured by Nagase ChemteX Corporation, product name "Denacol (registered trademark) EX-810") as a crosslinking agent (D). The mixture was further diluted with toluene and stirred uniformly to prepare a solution of the acrylic pressure-sensitive adhesive composition.

[0141] Manufacturing Example 2 A solution of an acrylic pressure-sensitive adhesive composition was prepared in the same manner as in Production Example 1, except that triethanolamine was not added.

[0142] Example 13 The solution of the acrylic adhesive composition prepared in Production Example 1 was applied onto the embossed surface of the release material 1 using an applicator, and dried for 2 minutes at a drying temperature of 100° C. to form a first adhesive layer (X1). Furthermore, the PET substrate was laminated onto the exposed surface of the adhesive layer (X1). Separately, a second pressure-sensitive adhesive layer (X2) was formed on the embossed surface of the release material 1 prepared above in the same manner as above, using the solution of the acrylic pressure-sensitive adhesive composition prepared in Production Example 1. Then, the exposed surface of the pressure-sensitive adhesive layer (X2) was laminated onto the exposed surface of the PET substrate laminated to the pressure-sensitive adhesive layer (X1), to obtain a pressure-sensitive adhesive sheet having pressure-sensitive adhesive layers (X) on both sides.

[0143] Examples 14 and 15, and Comparative Example 6 Each adhesive sheet shown in Table 2 below was obtained in the same manner as in Example 13, except that the release material shown in Table 2 below was used as the release material and the thickness of each of the adhesive layers (X1) and (X2) was changed.

[0144] Comparative Example 7 An adhesive sheet was obtained in the same manner as in Example 13, except that the adhesive composition prepared in Production Example 2 was used as the adhesive composition forming the adhesive layers (X1) and (X2).

[0145] The pressure-sensitive adhesive sheets obtained in Examples 13 to 15 and Comparative Examples 6 and 7 were evaluated using the above-mentioned evaluation methods. The results are shown in Table 2 below.

[0146] [Table 2]

[0147] It was confirmed from Table 2 that the pressure-sensitive adhesive sheets of Examples 13 to 15 had excellent releasability when contacted with water, and the time it took for the pressure-sensitive adhesive sheets to self-peel from the adherend after immersion in water was significantly shorter than that of the pressure-sensitive adhesive sheets of Comparative Examples 6 and 7. It was also confirmed that the pressure-sensitive adhesive sheets had sufficient adhesive strength to hold the adherend in place before immersion in water. The pressure-sensitive adhesive sheets of Examples 13 to 15 have recesses on the surface of the pressure-sensitive adhesive layer (X) (layer (X1) and layer (X2)) that is attached to the adherend, and therefore when the pressure-sensitive adhesive sheet is viewed in plan, water can easily penetrate from the outer edge of the pressure-sensitive adhesive sheet to the center of the pressure-sensitive adhesive sheet along the recesses when immersed in water. As a result, it is believed that the time until water-contact peeling is significantly shortened. On the other hand, in Comparative Example 6, since there are no recesses on the attachment surfaces of the pressure-sensitive adhesive layers (layer (X1) and layer (X2)), after the pressure-sensitive adhesive sheet is immersed in water, water can only penetrate into the interface between each pressure-sensitive adhesive layer and the adherend from the outer edge of the pressure-sensitive adhesive sheet. Therefore, it is considered that a long time was required for water to penetrate into the interface between the pressure-sensitive adhesive layer and the adherend to the extent that the pressure-sensitive adhesive sheet became self-peelable from the adherend. In addition, in Comparative Example 7, recesses were present on the application surface of the pressure-sensitive adhesive layer (X) (layer (X1) and layer (X2)), but the pressure-sensitive adhesive composition forming each pressure-sensitive adhesive layer (X) did not contain neutralizing agent (D), resulting in a longer time until water-contact peeling compared to the pressure-sensitive adhesive sheets of Examples 13 to 15. This result is considered to indicate that, since the pressure-sensitive adhesive layer (X) of the pressure-sensitive adhesive sheets of Examples 13 to 15 is a layer formed from a pressure-sensitive adhesive composition containing components (A2), (B2) and (D), the water-swellability of layer (X) is improved, making it easier for water to penetrate into the interface between the pressure-sensitive adhesive layer (X) and the adherend, and improving the water-contact peelability. It was also confirmed that the shortest pitch of the recesses formed on the surface of the adhesive layer (X) of the adhesive sheet of Example 13 was 250 μm, and the shortest pitch of the recesses formed on the surface of the adhesive layer (X) of the adhesive sheet of Example 14 was 700 μm. In addition, for the pressure-sensitive adhesive sheets of Examples 13 to 15, before the evaluation samples prepared in the water contact peelability evaluation were immersed in a water tank, the surfaces of the pressure-sensitive adhesive layers (X1) and (X2) were viewed in plan (magnification: 100 times) using an optical digital microscope (manufactured by Keyence Corporation, product name "Digital Microscope VHX-5000"). As a result, it was confirmed that both of the pressure-sensitive adhesive layers (X1) and (X2) of the pressure-sensitive adhesive sheets of Examples 13 to 15 had a plurality of the recesses continuously bonded from any one point of the contour of the surface to another point of the contour. It was also confirmed that the continuously bonded recesses formed a recess continuously bonded from any one side to any other side of the surface of the pressure-sensitive adhesive layer (X). [Industrial Applicability]

[0148] The temporary fixing adhesive sheet of one embodiment of the present invention has sufficient adhesive strength when attached to an adherend, but when peeled off from the adherend, it can be self-peeled in a short time by contacting it with a solvent, and is therefore applicable to any application as long as the adherend used is one that can come into contact with the solvent used during peeling. For example, the adhesive sheet can be suitably used as various types of temporary fixing pressure-sensitive adhesive sheets used in the manufacturing process of materials for electronic devices, as described above. In addition to electronic device applications, the temporary fixation pressure-sensitive adhesive sheet of one embodiment of the present invention can be used in a variety of applications, including, for example, protective film applications such as the above-mentioned window films, protective and decorative applications such as wallpapers and wrapping films, various label applications such as returnable labels, and use for attaching temporary notices and the like. Furthermore, when the temporary fixing pressure-sensitive adhesive sheet of one embodiment of the present invention is a temporary fixing pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer (X) having the above-mentioned continuous recessed shape, it can also be suitably used for, for example, the above-mentioned identification, decoration, paint masking, surface protection of metal plates, etc. [Explanation of symbols]

[0149] 10, 20, 30, 40, 50, 60, 70 Temporary adhesive sheet 100 Solvent contact peelability evaluation samples of temporary fixing pressure sensitive adhesive sheets in the examples 101 Adherend (glass plate) 1. A recess on the surface of the adhesive layer (X) 1h Height difference of depressions on the surface of the adhesive layer (X) 1w: Width of the recess on the surface of the adhesive layer (X) 2 Adhesive layer (X) 2a Convex portion of adhesive layer (X) 2t Thickness of adhesive layer (X) 3 Base material 4. Release material 4-1 First release material 4-2 Second release material 4a: A convex portion of the release material that is paired with a concave portion of the adhesive layer (X) 4h Height difference of the convex part of the release material 4w Width of the convex part of the release material 4t Thickness of the peeling material 4p The shortest pitch of the convex parts of the release material 5. Adhesive layer (Z) other than adhesive layer (X) 6 Area surrounded by recess 1 7f Distance between edges of recess 1 7p Shortest pitch of recess 1

Claims

1. A temporary fixing pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer (X) having recesses on at least one surface, the recesses being regularly shaped in a pattern when the pressure-sensitive adhesive layer (X) is viewed in plan, and having solvent contact releasability, the pressure-sensitive adhesive layer (X) is formed from an acrylic pressure-sensitive adhesive composition, The height difference of the recess is 0.5 μm or more and 50.0 μm or less, The width of the recess is 1.0 μm or more and 150 μm or less, The solvent contact peelability of the temporary fixing adhesive sheet is evaluated using glass having a smooth surface, and in the evaluation, when the adhesive sheet attached to the glass is immersed in methyl ethyl ketone or water at 25°C, the temporary fixing adhesive sheet has the property of self-peeling from the glass in less than 25 minutes.

2. The temporary fixing pressure-sensitive adhesive sheet according to claim 1 , wherein the height difference of the recesses is 1.0 μm or more and 30.0 μm or less.

3. The temporary fixing pressure-sensitive adhesive sheet according to claim 1 or 2, wherein when the pressure-sensitive adhesive layer (X) is viewed in plan, the recesses are present and are continuously connected from one point to another point on the contour of the surface of the pressure-sensitive adhesive layer (X).

4. The temporary fixing pressure-sensitive adhesive sheet according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive layer (X) has an adhesive strength of a surface on which recesses are present, before the pressure-sensitive adhesive layer (X) is immersed in a solvent, of 0.01 to 12.00 N / 25 mm.

5. The temporary fixing pressure-sensitive adhesive sheet according to any one of claims 1 to 4, wherein the thickness of the pressure-sensitive adhesive layer (X) is greater than the height difference of the recesses.

6. The temporary fixing pressure-sensitive adhesive sheet according to any one of claims 1 to 5, which has a substrate.

7. The temporary fixing pressure-sensitive adhesive sheet according to any one of claims 1 to 6, comprising a release material on a surface having recesses of the pressure-sensitive adhesive layer (X), the release material having protrusions that form pairs with the recesses of the pressure-sensitive adhesive layer (X).

8. The temporary fixing pressure-sensitive adhesive sheet according to any one of claims 1 to 7, which is used for temporarily fixing a material for an electronic device to a support.

9. The temporary fixing pressure-sensitive adhesive sheet according to claim 8 , wherein the material for an electronic device is a wafer for an electronic device.

10. The temporary fixing pressure-sensitive adhesive sheet according to any one of claims 1 to 9, which is used in processing and / or inspection of materials for electronic devices.

Citation Information

Patent Citations

  • Adhesive sheet and object separation method using adhesive sheet

    JP1998289888A

  • Adhesive sheet for thermal recording

    JP2003011526A

  • Method for manufacturing thinned wafer

    JP2003037155A

  • Machining method of brittle material

    JP2003338475A

  • Adhesive composition and adhesive tape having active energy ray-eliminating tackiness

    JP2009035618A